Emulsion particle-containing aqueous dispersion
The formulation of an aqueous dispersion with alkyl (meth)acrylates, styrene, and emulsifiers, combined with controlled heating and cooling, addresses poor dispersion stability in existing methods, achieving stable monomer and colorant dispersion for paints and coatings.
Patent Information
- Application Number
- JP2023137683
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-21
- Filing Date
- 2023-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-08-04
AI Technical Summary
Existing methods for producing colored resin fine particles with water resistance, weather resistance, and scratch resistance suffer from poor dispersion stability of polymerizable unsaturated monomers in aqueous media, leading to rapid precipitation of colorants and inefficient polymerization.
An aqueous dispersion containing monomer emulsion particles is formulated using alkyl (meth)acrylates, styrene monomers, nonionic emulsifiers, aliphatic organic acid esters, and lipophilic active ingredients, heated above the phase inversion temperature and cooled below it to stabilize the dispersion, followed by polymerization to form polymer emulsion particles with a resin layer.
The method achieves excellent dispersion stability of monomer and colorant components, preventing separation and ensuring long-term stability of the aqueous dispersion, while maintaining particle sizes suitable for applications like paints and coating agents.
Smart Images

Figure 0007595717000001 
Figure 0007595717000002 
Figure 0007595717000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an emulsion particle-containing aqueous dispersion. More specifically, the present invention relates to a monomer emulsion particle-containing aqueous dispersion useful for applications such as paints and coating agents, a method for producing the same, and a polymer emulsion particle-containing aqueous dispersion obtained by polymerizing a monomer component contained in the monomer emulsion particles of the monomer emulsion particle-containing aqueous dispersion. [Background technology]
[0002] As a method for producing colored resin microparticles that give images having water resistance, weather resistance, and abrasion resistance, a method has been proposed in which a polymerizable unsaturated monomer, a colorant, an emulsifier, and a polymerization initiator are phase-inverted emulsified in an aqueous medium using a mixer for high-viscosity paints, and then the polymerizable unsaturated monomer is polymerized (see, for example, Patent Document 1).
[0003] However, the above-mentioned method not only requires a mixer for high-viscosity paints, but also has poor dispersion stability of the polymerizable unsaturated monomer in the aqueous medium, so that the polymerizable unsaturated monomer and the aqueous medium separate in a short time and the colorant settles in a short time. Therefore, after the polymerizable unsaturated monomer, colorant, emulsifier and polymerization initiator are phase-inverted emulsified in the aqueous medium, the polymerizable unsaturated monomer must be polymerized immediately.
[0004] Therefore, in recent years, there has been a demand for the development of an aqueous dispersion containing monomer emulsion particles, which contains an active ingredient such as a colorant and a monomer, and has excellent dispersion stability of the monomer component. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-12709 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in view of the above-mentioned prior art, and is a method for producing a coloring agent containing an active ingredient such as a colorant and a monomer. Monomer-containing components (hereinafter, Monomer Components (That is, The present invention aims to provide a monomer emulsion particle-containing aqueous dispersion having excellent dispersion stability, a method for producing the same, and a polymer emulsion particle-containing aqueous dispersion obtained by polymerizing monomer components contained in the monomer emulsion particles of the monomer emulsion particle-containing aqueous dispersion. [Means for solving the problem]
[0007] The present invention relates to (1) An aqueous dispersion containing monomer emulsion particles containing a monomer component, the monomer component containing (A) at least one monomer X selected from the group consisting of alkyl (meth)acrylates and styrene-based monomers, the alkyl group of which has 4 to 12 carbon atoms, (B) a nonionic emulsifier, (C) an aliphatic organic acid (alkyl ester) having 15 or more carbon atoms, and (D) a lipophilic active ingredient, the monomer emulsion particles having an average particle size of 10 to 200 nm; (2) A method for producing an aqueous dispersion containing monomer emulsion particles containing a monomer component, the method comprising: mixing a monomer component containing (A) at least one monomer X selected from the group consisting of alkyl (meth)acrylates and styrene-based monomers, the alkyl group of which has 4 to 12 carbon atoms; (B) a nonionic emulsifier; (C) an aliphatic organic acid (alkyl ester) having 15 or more carbon atoms; and (D) a lipophilic active ingredient with an aqueous medium; heating the resulting mixture under stirring to a temperature equal to or higher than the phase inversion starting temperature of the mixture and lower than the boiling point of the aqueous medium; and then cooling the mixture to a temperature lower than the phase inversion starting temperature of the mixture. (3) An aqueous dispersion containing polymer emulsion particles, the polymer emulsion particles being obtained by polymerizing a monomer component contained in the monomer emulsion particles described in (1) above, and the average particle size of the polymer emulsion particles being 10 to 200 nm; and (4) An aqueous dispersion containing polymer emulsion particles having a resin layer on the surface thereof, the aqueous dispersion containing the polymer emulsion particles having a resin layer formed by polymerizing a monomer component for forming the resin layer on the surface of the polymer emulsion particles described in (3) above. Regarding. Effect of the Invention
[0008] According to the present invention, there are provided a monomer emulsion particle-containing aqueous dispersion having excellent dispersion stability of a monomer component containing an active ingredient such as a colorant and a monomer, a method for producing the same, and a polymer emulsion particle-containing aqueous dispersion obtained by polymerizing a monomer component contained in the monomer emulsion particles of the monomer emulsion particle-containing aqueous dispersion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The monomer emulsion particle-containing aqueous dispersion of the present invention is an aqueous dispersion containing monomer emulsion particles containing a monomer component, as described above. The monomer component contains (A) at least one monomer X selected from the group consisting of alkyl (meth)acrylates and styrene monomers, each having an alkyl group with 4 to 12 carbon atoms, (B) a nonionic emulsifier, (C) an aliphatic organic acid (alkyl ester) having 15 or more carbon atoms, and (D) a lipophilic active ingredient. The average particle size of the monomer emulsion particles is 10 to 200 nm.
[0010] Since the monomer emulsion particle-containing aqueous dispersion of the present invention has the above-mentioned constituent requirements, it has excellent dispersion stability of a monomer component containing an active ingredient such as a colorant and a monomer, more specifically, excellent dispersion stability of the monomer emulsion particles containing a monomer component in the monomer emulsion particle-containing aqueous dispersion (hereinafter referred to as "dispersion stability of the monomer emulsion particle-containing aqueous dispersion").
[0011] The monomer emulsion particle-containing aqueous dispersion of the present invention can be prepared, for example, by mixing a monomer component containing (A) at least one monomer X selected from the group consisting of alkyl (meth)acrylates and styrene-based monomers, each having an alkyl group with 4 to 12 carbon atoms, (B) a nonionic emulsifier, (C) an aliphatic organic acid (alkyl ester) having 15 or more carbon atoms, and (D) a lipophilic active ingredient with an aqueous medium, heating the resulting mixture under stirring to a temperature that is equal to or higher than the phase inversion onset temperature of the mixture and lower than the boiling point of the aqueous medium, and then cooling the mixture to a temperature lower than the phase inversion onset temperature of the mixture.
[0012] In the present invention, "(meth)acrylate" means "acrylate" or "methacrylate". "(meth)acrylic" means "acrylic" or "methacrylic". "Aliphatic organic acid (alkyl ester) having 15 or more carbon atoms" means "at least one compound selected from the group consisting of aliphatic organic acids having 15 or more carbon atoms and aliphatic organic acid alkyl esters having 15 or more carbon atoms, more specifically "aliphatic organic acids having 15 or more carbon atoms and / or aliphatic organic acid alkyl esters having 15 or more carbon atoms".
[0013] [(A) Monomer X] Monomer X is at least one monomer selected from the group consisting of alkyl(meth)acrylates having an alkyl group with a carbon number of 4 to 12 and styrene-based monomers. Therefore, the alkyl(meth)acrylates having an alkyl group with a carbon number of 4 to 12 and the styrene-based monomers may be used alone or in combination.
[0014] Examples of alkyl(meth)acrylates having an alkyl group with 4 to 12 carbon atoms include n-butyl(meth)acrylate, isobutyl(meth)acrylate, tert-butyl(meth)acrylate, sec-butyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, and n-octyl(meth)acrylate. , S Examples of the alkyl (meth)acrylate include cyclohexyl (meth)acrylate, n-lauryl (meth)acrylate, dodecyl (meth)acrylate, isononyl (meth)acrylate, and isobornyl (meth)acrylate, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more. In the present invention, the alkyl (meth)acrylate is a concept that includes (meth)acrylates having an alicyclic structure.
[0015] Among the alkyl (meth)acrylates, n-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate and cyclohexyl (meth)acrylate are preferred from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion. These monomers may be used alone or in combination of two or more.
[0016] Examples of styrene-based monomers include alkylstyrenes having an alkyl group with 1 to 4 carbon atoms, such as styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, tert-methylstyrene, o-tert-butylstyrene, m-tert-butylstyrene, and p-tert-butylstyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-ethoxystyrene, m-ethoxystyrene, p-ethoxystyrene, and o-tert-butoxystyrene. Examples of the styrene monomer include styrene having an alkoxy group with 1 to 4 carbon atoms, such as m-tert-butoxystyrene and p-tert-butoxystyrene, halogen atom-containing styrene such as o-fluorostyrene, m-fluorostyrene, p-fluorostyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, o-bromostyrene, m-bromostyrene, and p-bromostyrene, acetoxystyrene such as o-acetoxystyrene, m-acetoxystyrene, and p-acetoxystyrene, and vinyl toluene, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more. Among the styrene monomers, from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion, styrene and alkyl styrene having an alkyl group with 1 to 4 carbon atoms are preferred, and styrene is more preferred.
[0017] The styrene-based monomer may have a substituent such as a nitro group, a nitrile group, an alkoxyl group, an acyl group, a sulfone group, a hydroxyl group, or a halogen atom on the benzene ring.
[0018] From the above, among the monomers X, from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion, at least one monomer selected from the group consisting of n-butyl(meth)acrylate, isobutyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, cyclohexyl(meth)acrylate and styrene is preferred, and from the viewpoint of obtaining a monomer emulsion particle-containing aqueous dispersion containing monomer emulsion particles having a fine particle size, at least one monomer selected from the group consisting of n-butyl(meth)acrylate, isobutyl(meth)acrylate, 2-ethylhexyl(meth)acrylate and cyclohexyl(meth)acrylate is more preferred, and it is even more preferred that cyclohexyl(meth)acrylate and / or 2-ethylhexyl(meth)acrylate is used as an essential component and at least one monomer selected from the group consisting of n-butyl(meth)acrylate and isobutyl(meth)acrylate is optionally used.
[0019] The total content of cyclohexyl (meth)acrylate and 2-ethylhexyl (meth)acrylate in monomer X is preferably 50 to 100% by mass, more preferably 60 to 100% by mass, from the viewpoint of obtaining a monomer emulsion particle-containing aqueous dispersion containing monomer emulsion particles having a fine particle size. The total content of n-butyl (meth)acrylate and isobutyl (meth)acrylate in monomer X is preferably 0 to 50% by mass, more preferably 0 to 10% by mass, from the viewpoint of obtaining a monomer emulsion particle-containing aqueous dispersion containing monomer emulsion particles having a fine particle size.
[0020] The content of monomer X in the monomer component is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and even more preferably 25% by mass or more from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion. In addition, the content of monomer X in the monomer component is preferably 45% by mass or less from the viewpoint of finer monomer emulsion particles. Therefore, the content of monomer X in the monomer component is preferably 10 to 80% by mass, more preferably 15 to 70% by mass, even more preferably 20 to 60% by mass, and even more preferably 25 to 60% by mass.
[0021] [(B) Nonionic emulsifier] The HLB (hydrophilic-lipophilic balance) of the nonionic emulsifier is preferably 8 or more, more preferably 9 or more, and even more preferably 10 or more from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion, and is preferably 17 or less, more preferably 16 or less, and even more preferably 15 or less from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion. In addition, the HLB of the nonionic emulsifier is preferably 14 or less, more preferably 13.5 or less, and even more preferably 13 or less from the viewpoint of obtaining a monomer emulsion particle-containing aqueous dispersion containing monomer emulsion particles having a fine particle size. Therefore, the HLB of the nonionic emulsifier is preferably 8 to 17, more preferably 9 to 16, even more preferably 9 to 15, even more preferably 10 to 14, even more preferably 10 to 13.5, and particularly preferably 10 to 13. The HLB of the nonionic emulsifier is calculated based on the Griffin method by the formula: [HLB of nonionic emulsifier] = 20 × [(molecular weight of hydrophilic part) / (molecular weight of emulsifier)] This is the value calculated by
[0022] Examples of nonionic emulsifiers include ester-type nonionic emulsifiers such as polyglycerin fatty acid esters and sucrose fatty acid esters, ethylene-propylene block copolymer-type nonionic emulsifiers, alkyl ether-type nonionic emulsifiers, phenol-type nonionic emulsifiers, and amide-type nonionic emulsifiers, but the present invention is not limited to these examples. These emulsifiers may be used alone or in combination of two or more.
[0023] The nonionic emulsifier is commercially available and easily available. Examples of commercially available nonionic emulsifiers include Kao Corporation's product name: Latemul PD-420 (HLB: 12.6), Nippon Shokubai Co., Ltd.'s product name: Softanol 120 (HLB: 14.5), and ADEKA Corporation's product name: Adeka Reasoap ER-10 (HLB: 12.1), but the present invention is not limited to these examples.
[0024] Among the nonionic emulsifiers, it is preferable to use a reactive nonionic emulsifier from the viewpoint of incorporating the nonionic emulsifier into the monomer emulsion particles. The reactive nonionic emulsifier can be easily obtained commercially. Examples of the reactive nonionic emulsifier that can be easily obtained commercially include ADEKA Corporation, product name: ADEKA REASOAP ER-10 (HLB: 12.1), Kao Corporation, product name: LATEMURU PD-420 (HLB: 12.6), etc., but the present invention is not limited to only these examples.
[0025] The content of the nonionic emulsifier in the monomer component is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, and even more preferably 10% by mass or more from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion, and is preferably 60% by mass or less, more preferably 50% by mass or less from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion. Therefore, the content of the nonionic emulsifier in the monomer component is preferably 1 to 60% by mass, more preferably 3 to 60% by mass, even more preferably 5 to 60% by mass, even more preferably 10 to 60% by mass, and even more preferably 10 to 50% by mass.
[0026] The nonionic emulsifier may contain other emulsifiers, such as anionic emulsifiers, cationic emulsifiers, and amphoteric emulsifiers, within the scope that does not impair the object of the present invention.
[0027] [(C) Aliphatic organic acids (alkyl esters) having 15 or more carbon atoms] An aliphatic organic acid (alkyl ester) having 15 or more carbon atoms means an aliphatic organic acid having a total carbon number of 15 or more in the compound, or an aliphatic organic acid alkyl ester having a total carbon number of 15 or more in the compound. The aliphatic organic acid having 15 or more carbon atoms and the aliphatic organic acid alkyl ester having 15 or more carbon atoms may be used alone or in combination.
[0028] The lower limit of the carbon number of the aliphatic organic acid (alkyl ester) having 15 or more carbon atoms is 15 or more, preferably 18 or more, more preferably 22 or more, from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion, and the upper limit is not particularly limited, but from the viewpoint of easy availability of raw materials, it is preferably 60 or less, more preferably 50 or less, and even more preferably 40 or less. Therefore, the carbon number of the aliphatic organic acid (alkyl ester) is 15 or more, preferably 15 to 60, more preferably 15 to 50, even more preferably 18 to 40, and even more preferably 22 to 40.
[0029] The aliphatic organic acid (alkyl ester) having 15 or more carbon atoms may have a polymerizable unsaturated double bond. The aliphatic organic acid (alkyl ester) having 15 or more carbon atoms and having a polymerizable unsaturated double bond has a polymerizable unsaturated double bond, but is not included in the monomer X.
[0030] Examples of aliphatic organic acids (alkyl esters) having 15 or more carbon atoms include organic acid alkyl esters having an alkyl ester moiety having a polymerizable unsaturated double bond with 14 or more carbon atoms, such as tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate, eicosyl (meth)acrylate, and 2-decyltetradecyl (meth)acrylate; aliphatic organic acid alkyl esters having an alkyl ester moiety with 14 or more carbon atoms, such as hexadecyl 2-ethylhexanoate, myristyl myristate, stearyl myristate, stearyl 2-ethylhexanoate, and stearyl stearate; and aliphatic organic acid alkyl esters having an alkyl group with 14 or more carbon atoms, such as ethyl myristate, isopropyl myristate, butyl myristate, ethyl palmitate, ethyl stearate, and 2-ethylhexyl stearate; however, the present invention is not limited to these examples. These aliphatic organic acids (alkyl esters) may be used alone or in combination of two or more. Among the aliphatic organic acids (alkyl esters) having 15 or more carbon atoms, from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion, organic acid alkyl esters having 14 or more carbon atoms in the alkyl ester portion and having a polymerizable unsaturated double bond, and aliphatic organic acid alkyl esters having 14 or more carbon atoms in the ester portion and having a polymerizable unsaturated double bond are preferred.
[0031] The content of the aliphatic organic acid (alkyl ester) having 15 or more carbon atoms in the monomer component is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion, and is preferably 50% by mass or less, more preferably 45% by mass or less, even more preferably 40% by mass or less, and even more preferably 35% by mass or less from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion. Therefore, the content of the aliphatic organic acid (alkyl ester) in the monomer component is preferably 1 to 50% by mass, more preferably 3 to 50% by mass, even more preferably 5 to 50% by mass, even more preferably 5 to 45% by mass, even more preferably 5 to 40% by mass, and particularly preferably 5 to 35% by mass.
[0032] [Other Monomers] In addition, within the scope of the present invention, other monomers may be contained in addition to (A) the monomer X, (B) the nonionic emulsifier, and (C) the aliphatic organic acid (alkyl ester). Examples of the other monomers include monofunctional monomers and polyfunctional monomers.
[0033] Examples of monofunctional monomers include alkyl (meth)acrylates having an alkyl group with 1 to 3 carbon atoms, acid group-containing monomers, hydroxyl group-containing (meth)acrylates, piperidyl group-containing monomers, oxo group-containing monomers, fluorine atom-containing monomers, nitrogen atom-containing monomers, epoxy group-containing monomers, alkoxyalkyl (meth)acrylates, silane group-containing monomers, carbonyl group-containing monomers, aziridinyl group-containing monomers, and aralkyl (meth)acrylates, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more.
[0034] Examples of alkyl (meth)acrylates having an alkyl group with 1 to 3 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, and isopropyl (meth)acrylate, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more. Among these monomers, those having excellent solubility in the (D) lipophilic active ingredient described in detail below are preferred. In addition, when the solubility of (A) monomer X, (B) nonionic emulsifier, and (C) aliphatic organic acid (alkyl ester) in the (D) lipophilic active ingredient is low, methyl (meth)acrylate is preferred from the viewpoint of improving the solubility and controlling the phase inversion temperature.
[0035] Examples of the acid group-containing monomer include carboxyl group-containing aliphatic monomers such as acrylic acid, methacrylic acid, maleic acid, fumaric acid, crotonic acid, itaconic acid, citraconic acid, maleic anhydride, maleic acid monomethyl ester, maleic acid monobutyl ester, itaconic acid monomethyl ester, itaconic acid monobutyl ester, and vinylbenzoic acid, but the present invention is not limited to these examples. These acid group-containing monomers may be used alone or in combination of two or more kinds.
[0036] Examples of hydroxyl group-containing (meth)acrylates include hydroxyl group-containing (meth)acrylates having an ester moiety with 1 to 18 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate, but the present invention is not limited to these examples. These hydroxyl group-containing (meth)acrylates may be used alone or in combination of two or more kinds.
[0037] Examples of piperidyl group-containing monomers include 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 4-(meth)acryloyl-1-methoxy-2,2,6,6-tetramethylpiperidine, 4-cyano-4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotono Examples of the monomers include acryloylamino-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-1,2,2,6,6-pentamethylpiperidine, 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, but the present invention is not limited to these examples. Each of these monomers may be used alone, or two or more types may be used in combination.
[0038] Examples of oxo group-containing monomers include (di)ethylene glycol (methoxy) (meth) acrylates such as ethylene glycol (meth) acrylate, ethylene glycol methoxy (meth) acrylate, diethylene glycol (meth) acrylate, and diethylene glycol methoxy (meth) acrylate, but the present invention is not limited to these examples. These oxo group-containing monomers may be used alone or in combination of two or more kinds.
[0039] Examples of fluorine atom-containing monomers include fluorine atom-containing alkyl (meth)acrylates having an ester moiety with 2 to 6 carbon atoms, such as trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, and octafluoropentyl (meth)acrylate, but the present invention is not limited to these examples. These fluorine atom-containing monomers may be used alone or in combination of two or more kinds.
[0040] Examples of the nitrogen atom-containing monomer include (meth)acrylamide, N-monomethyl(meth)acrylamide, N-monoethyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, Nn-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, methylenebis(meth)acrylamide, N-methylol(meth)acrylamide, N-butoxymethyl(meth)acrylamide, dimethylaminoethyl(meth)acrylamide, N,N-dimethylaminopropylacrylamide, and acrylamide compounds such as diacetoneacrylamide, nitrogen atom-containing (meth)acrylate compounds such as dimethylaminoethyl(meth)acrylate and diethylaminoethyl(meth)acrylate, N-vinylpyrrolidone, and (meth)acrylonitrile, but the present invention is not limited to these examples. These nitrogen atom-containing monomers may be used alone or in combination of two or more.
[0041] Examples of epoxy group-containing monomers include epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate, α-methylglycidyl (meth)acrylate, and glycidyl allyl ether, but the present invention is not limited to these examples. These epoxy group-containing monomers may be used alone or in combination of two or more kinds.
[0042] Examples of alkoxyalkyl (meth)acrylates include methoxyethyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxybutyl (meth)acrylate, trimethylolpropane tripropoxy (meth)acrylate, etc., but the present invention is not limited to these examples. These alkoxyalkyl (meth)acrylates may be used alone or in combination of two or more kinds.
[0043] Examples of silane group-containing monomers include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(methoxyethoxy)silane, γ-(meth)acryloyloxypropyltrimethoxysilane, 2-styrylethyltrimethoxysilane, vinyltrichlorosilane, γ-(meth)acryloyloxypropylhydroxysilane, γ-(meth)acryloyloxypropylmethylhydroxysilane, etc., but the present invention is not limited to these examples. These silane group-containing monomers may be used alone or in combination of two or more kinds.
[0044] Examples of the carbonyl group-containing monomer include acrolein, fomunilstyrol, vinyl ethyl ketone, (meth)acryloxyalkyl propenal, acetonyl (meth)acrylate, diacetone (meth)acrylate, 2-hydroxypropyl (meth)acrylate acetylacetate, butanediol-1,4-(meth)acrylate acetylacetate, and 2-(acetoacetoxy)ethyl (meth)acrylate, but the present invention is not limited to these examples. These carbonyl group-containing monomers may be used alone or in combination of two or more kinds.
[0045] Examples of the aziridinyl group-containing monomer include (meth)acryloylaziridine, 2-aziridinylethyl (meth)acrylate, etc., but the present invention is not limited to these examples. These aziridinyl group-containing monomers may be used alone or in combination of two or more kinds.
[0046] Examples of the aralkyl (meth)acrylate include aralkyl (meth)acrylates having an aralkyl group having a carbon number of 7 to 18, such as benzyl (meth)acrylate, phenylethyl (meth)acrylate, methylbenzyl (meth)acrylate, and naphthylmethyl (meth)acrylate, but the present invention is not limited to these examples. These aralkyl (meth)acrylates may be used alone or in combination of two or more kinds.
[0047] Examples of the polyfunctional monomer include triallyl compounds having 9 to 20 carbon atoms, such as triallyl cyanurate (triallyl cyanurate), triallyl isocyanurate, triallyl phosphate, and triallylamine; ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, ethylene oxide-modified 1,6-hexanediol di(meth)acrylate, and 1,2-dimethylphenyl di(meth)acrylate. di(meth)acrylates of polyhydric alcohols having 1 to 10 carbon atoms, such as 9-nonanediol di(meth)acrylate, propylene oxide modified neopentyl glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate; di(meth)acrylates of alkylene oxide groups having 2 to 4 carbon atoms, such as polyethylene glycol di(meth)acrylate having 2 to 50 moles of ethylene oxide added, polypropylene glycol di(meth)acrylate having 2 to 50 moles of propylene oxide added, and tripropylene glycol di(meth)acrylate Alkyl di(meth)acrylates having an added mole number of 2 to 50; tri(meth)acrylates of polyhydric alcohols having 1 to 10 carbon atoms, such as ethoxylated glycerin tri(meth)acrylate, propylene oxide modified glycerol tri(meth)acrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol monohydroxy tri(meth)acrylate, and trimethylolpropane triethoxy tri(meth)acrylate; pentaerythritol tetra tetra(meth)acrylates of polyhydric alcohols having 1 to 10 carbon atoms, such as pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and ditrimethylolpropane tetra(meth)acrylate; penta(meth)acrylates of polyhydric alcohols having 1 to 10 carbon atoms, such as pentaerythritol penta(meth)acrylate and dipentaerythritol (monohydroxy)penta(meth)acrylate; hexa(meth)acrylates of polyhydric alcohols having 1 to 10 carbon atoms, such as pentaerythritol hexa(meth)acrylate;Examples of the polyfunctional monomer include epoxy group-containing (meth)acrylates such as bisphenol A di(meth)acrylate, 2-(2'-vinyloxyethoxyethyl)(meth)acrylate, and epoxy(meth)acrylate; and polyfunctional (meth)acrylates such as urethane(meth)acrylate, but the present invention is not limited to these examples. These polyfunctional monomers may be used alone or in combination of two or more kinds.
[0048] [(D) Lipophilic active ingredient] The lipophilic active ingredient is a component for imparting desired properties to the monomer emulsion particle-containing aqueous dispersion, and is a component that has lipophilicity or oil-solubility with respect to the oily component.
[0049] In the present invention, a lipophilic active ingredient means, in the case of a solid ingredient, a component that dissolves in methyl methacrylate when 1000 g of the solid ingredient is mixed with 2 g or more of the solid ingredient at room temperature (23° C.), and, in the case of a liquid ingredient, a component that does not separate when 1000 g of methyl methacrylate is mixed with 30 g or more of the liquid ingredient and the resulting mixture is allowed to stand at room temperature (23° C.) for 12 hours.
[0050] Among the lipophilic active ingredients, from the viewpoint of fully expressing the properties of the active ingredient, in the case of a solid ingredient, it is preferable that the solid ingredient dissolves in an amount of 10 g or more, more preferably 20 g or more, and even more preferably 50 g or more in 1000 g of methyl methacrylate at room temperature (23°C).
[0051] Furthermore, from the viewpoint of improving the dispersion stability of the lipophilic active ingredient, it is preferable that the solid ingredient does not dissolve in an amount of 10 g or more per 1000 g of water at room temperature (23° C.).
[0052] The type of lipophilic active ingredient varies depending on the application of the monomer emulsion particle-containing aqueous dispersion, and therefore it is preferable to appropriately select the type of lipophilic active ingredient depending on the application. The lipophilic active ingredient may be a polymerizable monomer.
[0053] Examples of lipophilic active ingredients include oil-soluble colorants such as oil-soluble dyes, such as oil-soluble phthalocyanine near-infrared absorbing dyes, oil-soluble azo red dyes, oil-soluble chromium complex dyes, and oil-soluble anthraquinone dyes; BASF products (trade names: Tinuvin 400, Tinuvin 900, Tinuvin 928, Tinuvin 405, Tinuvin 460, Tinuvin 479, and Tinuvin 970); Otsuka Chemical Co., Ltd. product name: RUVA-93; ADEKA Corporation product name: Adeka STAB LA-F70; and SHUANG BANG INDUSTRIAL Examples of the oil-soluble active ingredient include oil-soluble ultraviolet absorbers such as SB-UVA650 (trade name, manufactured by ADEKA Corp.), hindered amine light stabilizers (e.g., Adeka STAB LA-87 (trade name, manufactured by ADEKA Corp.), oil-soluble crosslinking agents, oil-soluble antioxidants, oil-soluble fragrances, oil-soluble insecticides, oil-soluble anti-inflammatory analgesics, oil-soluble fresheners, and oil-soluble deodorants, but the present invention is not limited to these examples. These lipophilic active ingredients may be used alone or in combination of two or more kinds.
[0054] The content of the lipophilic active ingredient in the monomer component cannot be determined in general because it varies depending on the type of the lipophilic active ingredient, but from the viewpoint of fully expressing the properties of the lipophilic active ingredient, it is preferably 0.03% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, and from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion, it is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and even more preferably 25% by mass or less. Therefore, the content of the lipophilic active ingredient in the monomer component is preferably 0.03 to 50% by mass, more preferably 0.1 to 50% by mass, even more preferably 0.3 to 40% by mass, even more preferably 0.5 to 30% by mass, and even more preferably 0.5 to 25% by mass.
[0055] [Preparation of Monomer Emulsion Particle-Containing Aqueous Dispersion] As described above, the monomer emulsion particle-containing aqueous dispersion can be prepared by mixing the monomer components with an aqueous medium, heating the resulting mixture under stirring to a temperature between the phase inversion temperature of the mixture and the boiling point of the aqueous medium, and then cooling the mixture to a temperature lower than the phase inversion temperature of the mixture.
[0056] When preparing the monomer emulsion particle-containing aqueous dispersion of the present invention, the monomer components are first mixed with an aqueous medium.
[0057] Examples of the aqueous medium include water and a mixed solvent of water and a water-soluble organic solvent. Examples of the water-soluble organic solvent include lower alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, and tert-butyl alcohol; polyhydric alcohols such as ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, and diethylene glycol; and ketones such as acetone and methyl ethyl ketone, but the present invention is not limited to these examples. Each of these organic solvents may be used alone, or two or more types may be used in combination. The content of water in the aqueous medium is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and even more preferably 80% by mass or more, from the viewpoint of improving the dispersion stability of the aqueous dispersion containing the monomer emulsion particles, and the upper limit of the content is 100% by mass. Among the aqueous media, water is preferred.
[0058] From the viewpoint of uniformly dispersing the monomer component and the aqueous medium, the mass ratio of the monomer component to the aqueous medium (monomer component / aqueous medium) is preferably 20 / 80 to 50 / 50, more preferably 25 / 75 to 45 / 55, and further preferably 30 / 70 to 40 / 60.
[0059] The temperature at which the monomer component and the aqueous medium are mixed varies depending on the phase inversion temperature described below and cannot be generally determined, but is usually preferably 5 to 45°C, more preferably 5 to 40°C, and even more preferably 5 to 35°C. When mixing the monomer component and the aqueous medium, it is preferable to add the monomer component to the aqueous medium under stirring in order to uniformly disperse the monomer component in the aqueous medium. As a means for stirring the aqueous medium, there is no need to use special devices such as a mixer for high viscosity paints or a high-pressure homogenizer that have been used conventionally, and the monomer component can be uniformly dispersed in the aqueous medium with a simple stirring device such as a stirring rod or a magnetic stirrer.
[0060] Next, the monomer component and the aqueous medium are mixed, and the resulting mixture is heated under stirring to a temperature equal to or higher than the phase inversion temperature of the mixture and lower than the boiling point of the aqueous medium, and then cooled under stirring to a temperature lower than the phase inversion temperature. Since this operation is adopted in the present invention, an aqueous dispersion containing monomer emulsion particles having excellent dispersion stability of the monomer component containing the monomer X and the lipophilic active ingredient can be obtained.
[0061] The phase inversion temperature of the mixture is a value measured according to the method described in Example 1 below. In the present invention, the lowest phase inversion temperature is the phase inversion start temperature, and the highest phase inversion temperature is the phase inversion end temperature. The phase inversion temperature is not particularly limited. The phase inversion start temperature is preferably 35°C or higher, more preferably 45°C or higher, and even more preferably 50°C or higher, from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion. The phase inversion end temperature is preferably 98°C or lower, more preferably 97°C or lower, and even more preferably 96°C or lower, from the viewpoint of improving the stability of the monomer emulsion.
[0062] The atmosphere in which the mixture is heated is not particularly limited, but from the viewpoint of avoiding the influence of oxygen contained in the air, it is preferable to use an inert gas such as nitrogen gas or argon gas.
[0063] The lower limit of the heating temperature (maximum temperature when heated) of the mixture is a temperature equal to or higher than the phase inversion start temperature of the mixture from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion, but is preferably a temperature 0.5° C. or higher than the phase inversion start temperature of the mixture, and more preferably a temperature 1° C. or higher than the phase inversion start temperature of the mixture. In addition, the lower limit of the heating temperature (maximum temperature when heated) of the mixture is preferably a temperature equal to or higher than the phase inversion end temperature of the mixture, and more preferably 0.5° C. or higher than the phase inversion end temperature of the mixture, from the viewpoint of improving the dispersion stability of the monomer emulsion particle-containing aqueous dispersion.
[0064] The upper limit of the heating temperature (maximum temperature when heated) of the mixture is usually a temperature lower than the boiling point of the aqueous medium, preferably a temperature 3°C or more lower than the boiling point of the aqueous medium, and more preferably a temperature 5°C or more lower than the boiling point of the aqueous medium.
[0065] Next, after the temperature of the mixture reaches a temperature equal to or higher than the phase inversion starting temperature of the mixture and lower than the boiling point of the aqueous medium, the mixture is cooled to a temperature equal to or lower than the phase inversion temperature of the mixture.
[0066] There is no particular limitation on the means for cooling the mixture. For example, the mixture may be cooled by standing to cool or by air cooling. The mixture is cooled to a temperature equal to or lower than the phase inversion starting temperature of the mixture. The mixture is cooled to a temperature preferably 10°C or more lower than the phase inversion starting temperature of the mixture, more preferably 20°C or more lower than the phase inversion starting temperature of the mixture, even more preferably 25°C or more lower than the phase inversion starting temperature of the mixture, and even more preferably 30°C or more lower than the phase inversion starting temperature of the mixture.
[0067] The above-mentioned operation provides the monomer emulsion particle-containing aqueous dispersion of the present invention. The content of the monomer component in the monomer emulsion particle-containing aqueous dispersion of the present invention varies depending on the application of the monomer emulsion particle-containing aqueous dispersion, and therefore cannot be determined in general. Therefore, it is preferable that the content of the monomer component in the monomer emulsion particle-containing aqueous dispersion of the present invention is appropriately adjusted depending on the application of the monomer emulsion particle-containing aqueous dispersion, and the upper limit is usually 100% by mass.
[0068] The average particle size of the monomer emulsion particles contained in the monomer emulsion particle-containing aqueous dispersion of the present invention is usually 10 to 200 nm, preferably 10 to 150 nm. However, according to the method for producing the monomer emulsion particle-containing aqueous dispersion of the present invention, an aqueous dispersion containing very small monomer emulsion particles having an average particle size of 10 to 100 nm can be obtained. The average particle size of the monomer emulsion particles is a value measured based on the method described in Example 1 below.
[0069] In the monomer emulsion particle-containing aqueous dispersion of the present invention, the monomer component is contained in the monomer emulsion particle, but the monomer component may be unavoidably present in the aqueous dispersion without being completely contained in the monomer emulsion particle. Therefore, the monomer component may be suspended or dissolved in the monomer emulsion particle-containing aqueous dispersion of the present invention within a range that does not impair the object of the present invention.
[0070] The monomer emulsion particle-containing aqueous dispersion of the present invention may contain, for example, additives, etc., within the scope of not impairing the purpose of the present invention. Examples of the additives include colorants such as pigments, leveling agents, ultraviolet absorbers, ultraviolet stabilizers, antioxidants, polymerization inhibitors, fillers, coupling agents, rust inhibitors, antibacterial agents, metal deactivators, wetting agents, defoamers, surfactants, reinforcing agents, plasticizers, lubricants, antifogging agents, anticorrosive agents, pigment dispersants, flow regulators, peroxide decomposers, mold decolorizers, fluorescent brighteners, organic flame retardants, inorganic flame retardants, drip prevention agents, melt flow modifiers, antistatic agents, algae inhibitors, fungicides, flame retardants, slip agents, metal chelating agents, antiblocking agents, heat stabilizers, processing stabilizers, dispersants, thickeners, rheology control agents, foaming agents, antiaging agents, preservatives, antistatic agents, silane coupling agents, antioxidants, film-forming assistants, etc., but the present invention is not limited to only these examples. These additives may be used alone or in combination of two or more kinds. The amount of these additives varies depending on the type of the additive, so it cannot be determined in general, and it is preferable to determine the amount appropriately depending on the type of the additive.
[0071] As described above, the monomer emulsion particle-containing aqueous dispersion of the present invention is excellent in the dispersion stability of the monomer emulsion particles containing the monomer component. Therefore, the monomer emulsion particle-containing aqueous dispersion of the present invention does not separate from the aqueous medium in a short time or the active ingredient does not settle in a short time as in the conventional aqueous dispersion, and the monomer component can be stably dispersed in the aqueous medium for a long period of time.
[0072] [Polymer Emulsion Particle-Containing Aqueous Dispersion] The polymer emulsion particle-containing aqueous dispersion can be prepared by using the monomer emulsion particle-containing aqueous dispersion and polymerizing the monomer components contained in the monomer emulsion particles. The monomer components contained in the monomer emulsion particles can usually be polymerized by emulsion polymerization.
[0073] Examples of a method for emulsion polymerizing the monomer components contained in the monomer emulsion particle-containing aqueous dispersion include a method in which an emulsifier is dissolved in the monomer emulsion particle-containing aqueous dispersion and a polymerization initiator is added to the obtained solution, but the present invention is not limited to only such a method.
[0074] Examples of the emulsifier include anionic emulsifiers, nonionic emulsifiers, cationic emulsifiers, amphoteric emulsifiers, and polymeric emulsifiers. These emulsifiers may be used alone or in combination of two or more kinds.
[0075] Examples of the anionic emulsifier include alkyl sulfate salts such as ammonium dodecyl sulfate and sodium dodecyl sulfate; alkyl sulfonate salts such as ammonium dodecyl sulfonate, sodium dodecyl sulfonate and sodium alkyl diphenyl ether disulfonate; alkyl aryl sulfonate salts such as ammonium dodecyl benzene sulfonate and sodium dodecyl naphthalene sulfonate; polyoxyethylene alkyl sulfonate salts; polyoxyethylene alkyl sulfate salts; polyoxyethylene alkyl aryl sulfate salts; dialkyl sulfosuccinate salts; aryl sulfonic acid-formalin condensates; an Examples of suitable amines include fatty acid salts such as ammonium laurate and sodium stearylate; sulfates having an allyl group or salts thereof such as bis(polyoxyethylene polycyclic phenyl ether) methacrylate sulfonate salts, propenyl-alkyl sulfosuccinate salts, polyoxyethylene (meth)acrylate sulfonate salts, polyoxyethylene (meth)acrylate phosphonate salts, and sulfonate salts of allyloxymethylalkyloxypolyoxyethylene; sulfate salts of allyloxymethylalkoxyethylpolyoxyethylene, and ammonium polyoxyalkylene alkenyl ether sulfate, but the present invention is not limited to these examples.
[0076] Examples of nonionic emulsifiers include polyoxyethylene alkyl ethers, polyoxyethylene alkylaryl ethers, condensates of polyethylene glycol and polypropylene glycol, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid monoglycerides, condensations of ethylene oxide and aliphatic amines, allyloxymethylalkoxyethylhydroxypolyoxyethylene, polyoxyalkylene alkenyl ethers, and the like; however, the present invention is not limited to these examples.
[0077] Examples of cationic emulsifiers include alkyl ammonium salts such as dodecyl ammonium chloride, but the present invention is not limited to these examples.
[0078] Examples of amphoteric emulsifiers include betaine ester emulsifiers, but the present invention is not limited to these examples.
[0079] Examples of polymeric emulsifiers include poly(meth)acrylates such as sodium polyacrylate; polyvinyl alcohol; polyvinylpyrrolidone; polyhydroxyalkyl(meth)acrylates such as polyhydroxyethyl acrylate; and copolymers in which one or more of the monomers constituting these polymers are copolymerized components, but the present invention is not limited to these examples.
[0080] Among the above emulsifiers, emulsifiers having a polymerizable group, that is, so-called reactive emulsifiers, are preferred from the viewpoint of improving weather resistance, and non-nonylphenyl type emulsifiers are preferred from the viewpoint of environmental protection.
[0081] Examples of reactive emulsifiers include propenyl-alkyl sulfosuccinate salts, (meth)acrylic acid polyoxyethylene sulfonate salts, (meth)acrylic acid polyoxyethylene phosphonate salts (e.g., Sanyo Chemical Industries, Ltd., product name: Eleminol RS-30, etc.), polyoxyethylene alkylpropenyl phenyl ether sulfonate salts (e.g., Daiichi Kogyo Seiyaku Co., Ltd., product names: Aqualon BC-10, Aqualon HS-10, etc.), sulfonate salts of allyloxymethyl alkyloxy polyoxyethylene (e.g., Daiichi Kogyo Seiyaku Co., Ltd., product name: Aqualon KH-10, etc.), sulfonate salts of allyloxymethyl nonyl phenoxyethyl hydroxy polyoxyethylene (e.g., ADEKA Corporation, product name: Adeka Reasoap SE-10, etc.), and allyloxymethyl alkoxyethyl Examples of such hydroxypolyoxyethylene sulfate ester salts include ADEKA Corporation's trade names ADEKA REASOAP SR-10 and SR-30, bis(polyoxyethylene polycyclic phenyl ether) methacrylated sulfonate salts include ADEKA Corporation's trade name ANTOX MS-60, and the like, allyloxymethylalkoxyethylhydroxypolyoxyethylenes include ADEKA Corporation's trade name ADEKA REASOAP ER-20, polyoxyethylene alkylpropenylphenyl ethers include Daiichi Kogyo Seiyaku Co., Ltd.'s trade name AQUALON RN-20, and allyloxymethylnonylphenoxyethylhydroxypolyoxyethylenes include ADEKA Corporation's trade name ADEKA REASOAP NE-10, and the like, but the present invention is not limited to these examples.
[0082] The amount of emulsifier (non-volatile content) is preferably 0.3 parts by mass or more, more preferably 0.5 parts by mass or more, per 100 parts by mass of the aqueous dispersion containing the monomer emulsion particles, from the viewpoint of improving polymerization stability, and is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 1 part by mass or less, from the viewpoint of improving weather resistance.
[0083] Examples of the polymerization initiator include azo compounds such as azobisisobutyronitrile, 2,2-azobis(2-methylbutyronitrile), 2,2-azobis(2,4-dimethylvaleronitrile), 2,2-azobis(2-diaminopropane) hydrochloride, 4,4-azobis(4-cyanovaleric acid), and 2,2-azobis(2-methylpropionamidine); persulfates such as ammonium persulfate and potassium persulfate; and peroxides such as hydrogen peroxide, benzoyl peroxide, parachlorobenzoyl peroxide, lauroyl peroxide, and ammonium peroxide, but the present invention is not limited to these examples. These polymerization initiators may be used alone or in combination of two or more.
[0084] The amount of the polymerization initiator is preferably 0.03 parts by mass or more, more preferably 0.04 parts by mass or more, per 100 parts by mass of the monomer emulsion particle-containing aqueous dispersion, from the viewpoints of increasing the polymerization rate and reducing the amount of unreacted monomer components remaining, and is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, from the viewpoint of improving weather resistance.
[0085] The method of adding the polymerization initiator is not particularly limited, and examples of the method of addition include batch addition, divided addition, and continuous dropwise addition.
[0086] In order to promote the decomposition of the polymerization initiator, a suitable amount of a decomposer for the polymerization initiator, for example, a reducing agent such as sodium hydrogen sulfite or a transition metal salt such as ferrous sulfate, may be added to the reaction system.
[0087] In addition, a chain transfer agent can be used to adjust the weight average molecular weight of the polymer. Examples of the chain transfer agent include 2-ethylhexyl thioglycolate, tert-dodecyl mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, mercaptoacetic acid, mercaptopropionic acid, 2-mercaptoethanol, α-methylstyrene, and α-methylstyrene dimer, but the present invention is not limited to these examples. These chain transfer agents may be used alone or in combination of two or more. The amount of the chain transfer agent per 100 parts by mass of the monomer component is preferably 0.01 to 10 parts by mass from the viewpoint of adjusting the weight average molecular weight of the polymer contained in the polymer emulsion particles.
[0088] In addition, when the monomer component is emulsion-polymerized, from the viewpoint of improving weather resistance, a suitable amount of silane coupling agent may be used. Examples of the silane coupling agent include silane coupling agents having polymerizable unsaturated bonds such as (meth)acryloyl group, vinyl group, allyl group, propenyl group, etc., but the present invention is not limited to only these examples.
[0089] When the monomer components are emulsion-polymerized, additives such as a chelating agent, a film-forming agent, a pH buffering agent, etc. may be added in appropriate amounts to the reaction system, if necessary.
[0090] The atmosphere in which the monomer components are emulsion-polymerized is not particularly limited, but from the viewpoint of increasing the efficiency of the polymerization initiator, it is preferable that the atmosphere be an inert gas such as nitrogen gas or argon gas.
[0091] The polymerization temperature when emulsion-polymerizing the monomer components is not particularly limited, but is usually preferably 50 to 100° C., more preferably 60 to 85° C. The polymerization temperature may be constant or may be changed during the polymerization reaction.
[0092] The polymerization time of the monomer components is not particularly limited and may be appropriately set depending on the progress of the polymerization reaction, but is usually about 2 to 9 hours.
[0093] By emulsion-polymerizing the monomer components as described above, the polymer emulsion particle-containing aqueous dispersion of the present invention can be obtained.
[0094] The content of the polymer emulsion particles in the polymer emulsion particle-containing aqueous dispersion of the present invention cannot be determined in general because it varies depending on the application of the polymer emulsion particle-containing aqueous dispersion, etc. Therefore, it is preferable that the content of the polymer emulsion particles in the polymer emulsion particle-containing aqueous dispersion of the present invention is appropriately adjusted depending on the application of the polymer emulsion particle-containing aqueous dispersion, etc.
[0095] The average particle size of the polymer emulsion particles contained in the polymer emulsion particle-containing aqueous dispersion of the present invention is approximately the same as the average particle size of the monomer emulsion particles used as a raw material for the polymer emulsion particle-containing aqueous dispersion, and therefore the average particle size of the monomer emulsion particles is maintained.
[0096] The average particle size of the polymer emulsion particles contained in the polymer emulsion particle-containing aqueous dispersion of the present invention is usually 10 to 200 nm, preferably 10 to 150 nm. According to the method for producing the monomer emulsion particle-containing aqueous dispersion of the present invention, as described above, an aqueous dispersion containing monomer emulsion particles having a very small particle size of 10 to 100 nm can be obtained, and therefore, an aqueous dispersion containing polymer emulsion particles having a very small particle size of 10 to 100 nm can be obtained. The average particle size of the polymer emulsion particles is a value measured based on the method described in Example 1 below.
[0097] [Aqueous dispersion containing polymer emulsion particles having a resin layer on the surface] The aqueous dispersion containing polymer emulsion particles having a resin layer on the surface thereof according to the present invention has a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particles. By forming a resin layer on the surface of the polymer emulsion particles, it is expected that the film-forming property of the aqueous dispersion containing polymer emulsion particles can be improved.
[0098] The polymer emulsion particle-containing aqueous dispersion having a resin layer on the surface of the present invention can be prepared by, for example, adding a polymerization initiator and, if necessary, an aqueous medium to the polymer emulsion particle-containing aqueous dispersion, then adding a component in which the monomer component for forming a resin layer has been emulsified in advance using an emulsifier and water, dissolving an emulsifier in the polymer emulsion particle-containing aqueous dispersion, dropping a monomer component for forming a resin layer and a polymerization initiator under stirring, or dropping a component in which the monomer component for forming a resin layer has been emulsified in advance using an emulsifier and water to the polymer emulsion particle-containing aqueous dispersion, but the present invention is not limited to only such a method.The amount of the aqueous medium may be appropriately set in consideration of the amount of non-volatile matter contained in the obtained polymer emulsion particle-containing aqueous dispersion.
[0099] The resin layer-forming monomer component is a component for forming a resin layer on the surface of the polymer emulsion particle.
[0100] The monomer component for forming the resin layer includes a monofunctional monomer and a polyfunctional monomer. The monofunctional monomer and the polyfunctional monomer may be used alone or in combination.
[0101] Examples of monofunctional monomers include ethylenically unsaturated double bond-containing monomers, but the present invention is not limited to these examples.
[0102] Examples of ethylenically unsaturated double bond-containing monomers include alkyl (meth)acrylates, acid group-containing monomers, hydroxyl group-containing (meth)acrylates, piperidyl group-containing monomers, oxo group-containing monomers, fluorine atom-containing monomers, nitrogen atom-containing monomers, epoxy group-containing monomers, alkoxyalkyl (meth)acrylates, silane group-containing monomers, carbonyl group-containing monomers, aziridinyl group-containing monomers, styrene-based monomers, and aralkyl (meth)acrylates, but the present invention is not limited to these examples. These ethylenically unsaturated double bond-containing monomers may be used alone or in combination of two or more.
[0103] Examples of alkyl (meth)acrylates include alkyl (meth)acrylates having an ester moiety of 1 to 18 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, sec-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, tridecyl (meth)acrylate, cyclohexyl (meth)acrylate, n-lauryl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and isobornyl methacrylate, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more.
[0104] Examples of the acid group-containing monomer, the hydroxyl group-containing (meth)acrylate, the piperidyl group-containing monomer, the oxo group-containing monomer, the fluorine atom-containing monomer, the nitrogen atom-containing monomer, the epoxy group-containing monomer, the alkoxyalkyl (meth)acrylate, the silane group-containing monomer, the carbonyl group-containing monomer, the aziridinyl group-containing monomer, the styrene-based monomer, the aralkyl (meth)acrylate and the polyfunctional monomer include those exemplified as the monomer X. Each of these monomers may be used alone, or two or more of them may be used in combination.
[0105] In addition, from the viewpoint of imparting ultraviolet stability or ultraviolet absorption to the emulsion particles, it is preferable to contain an ultraviolet stable monomer or an ultraviolet absorbing monomer in the monomer component for forming the resin layer, within the range in which the object of the present invention is not hindered. By imparting ultraviolet absorption to the resin layer, it is possible to obtain an aqueous dispersion containing polymer emulsion particles having excellent film-forming properties and weather resistance.
[0106] Examples of ultraviolet-stable monomers include 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 4-(meth)acryloyl-1-methoxy-2,2,6,6-tetramethylpiperidine, 4-cyano-4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotonoyl Examples of the monomers include acryloylamino-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-1,2,2,6,6-pentamethylpiperidine, 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, but the present invention is not limited to these examples. Each of these monomers may be used alone, or two or more types may be used in combination. Among these ultraviolet-stable monomers, piperidyl group-containing (meth)acrylates such as 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, and 4-cyano-4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine are preferred.
[0107] Examples of ultraviolet absorbing monomers include benzotriazole-based ultraviolet absorbing monomers, benzophenone-based ultraviolet absorbing monomers, etc., but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more kinds.
[0108] Examples of benzotriazole-based ultraviolet absorbing monomers include 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-5-tert-butyl-2H-benzotriazole, and 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-5-tert-butyl-2H-benzotriazole. ) acryloylaminomethyl-5'-tert-octylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxypropylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyhexylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-3'-tert-butyl-5'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole , 2-[2'-hydroxy-3'-tert-butyl-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, 2-[2'-hydroxy-5'-tert-butyl-3'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, Examples of the monomers include 2-[2'-hydroxy-5'-(β-(meth)acryloyloxyethoxy)-3'-tert-butylphenyl]-5-cyano-2H-benzotriazole, 2-[2'-hydroxy-5'-(β-(meth)acryloyloxyethoxy)-3'-tert-butylphenyl]-4-tert-butyl-2H-benzotriazole, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more kinds.
[0109] Benzophenone-based ultraviolet absorbing monomers include, for example, 2-hydroxy-4-(meth)acryloyloxybenzophenone, 2-hydroxy-4-[2-hydroxy-3-(meth)acryloyloxy]propoxybenzophenone, 2-hydroxy-4-[2-(meth)acryloyloxy]ethoxybenzophenone, 2-hydroxy-4-[3-(meth)acryloyloxy-2-hydroxypropoxy]benzophenone, and 2-hydroxy-3-tert-butyl-4-[2-(meth)acryloyloxy]butoxybenzophenone, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more kinds.
[0110] The content of the ultraviolet stable monomer in the monomer component for forming the resin layer is preferably 1 to 5 mass % from the viewpoint of improving the ultraviolet stability and the dispersion stability of the aqueous dispersion containing the polymer emulsion particles. The content of the ultraviolet absorbing monomer in the monomer component for forming the resin layer is preferably 1 to 5 mass % from the viewpoint of improving the ultraviolet stability and the dispersion stability of the aqueous dispersion containing the polymer emulsion particles.
[0111] Examples of the emulsifier include the anionic emulsifiers, the nonionic emulsifiers, the cationic emulsifiers, the amphoteric emulsifiers, and the polymer emulsifiers. These emulsifiers may be used alone or in combination of two or more kinds.
[0112] The amount of emulsifier per 100 parts by mass of the monomer component for forming the resin layer is, from the viewpoint of improving polymerization stability, preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, and from the viewpoint of improving weather resistance, is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, even more preferably 5 parts by mass or less, and even more preferably 4 parts by mass or less.
[0113] Examples of the polymerization initiator include azo compounds such as azobisisobutyronitrile, 2,2-azobis(2-methylbutyronitrile), 2,2-azobis(2,4-dimethylvaleronitrile), 2,2-azobis(2-diaminopropane) hydrochloride, 4,4-azobis(4-cyanovaleric acid), and 2,2-azobis(2-methylpropionamidine); persulfates such as ammonium persulfate and potassium persulfate; and peroxides such as hydrogen peroxide, benzoyl peroxide, parachlorobenzoyl peroxide, lauroyl peroxide, and ammonium peroxide, but the present invention is not limited to these examples. These polymerization initiators may be used alone or in combination of two or more.
[0114] The amount of polymerization initiator per 100 parts by mass of the monomer component for forming the resin layer is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, from the viewpoint of increasing the polymerization rate and reducing the amount of remaining unreacted monomer, and is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, from the viewpoint of improving weather resistance.
[0115] The method of adding the polymerization initiator is not particularly limited. Examples of the method of addition include batch charging, divided charging, continuous dropwise addition, etc. In addition, in order to hasten the end of the polymerization reaction, a part of the polymerization initiator may be added before or after the end of adding the monomer component for forming the resin layer into the reaction system.
[0116] In order to promote the decomposition of the polymerization initiator, a suitable amount of a decomposer for the polymerization initiator, for example, a reducing agent such as sodium hydrogen sulfite or a transition metal salt such as ferrous sulfate, may be added to the reaction system.
[0117] In order to adjust the weight average molecular weight of the polymer, the chain transfer agent can be used. The amount of the chain transfer agent per 100 parts by mass of the monomer component for forming the resin layer is preferably 0.01 to 10 parts by mass from the viewpoint of adjusting the weight average molecular weight of the polymer emulsion particles.
[0118] When the monomer component for forming the resin layer is emulsion-polymerized, from the viewpoint of improving the weather resistance of the polymer emulsion particle, a suitable amount of silane coupling agent may be used. Examples of the silane coupling agent include the silane coupling agent having a polymerizable unsaturated bond such as (meth)acryloyl group, vinyl group, allyl group, propenyl group, etc., but the present invention is not limited to only these examples.
[0119] When the monomer components for forming the resin layer are emulsion-polymerized, additives such as a chelating agent, a film-forming aid, a pH buffer, etc. may be added to the reaction system as necessary. The amount of the additive varies depending on the type and cannot be determined in general, but is usually preferably about 0.01 to 5 parts by mass, more preferably about 0.1 to 3 parts by mass, per 100 parts by mass of the monomer components for forming the resin layer.
[0120] The atmosphere in which the monomer components for forming the resin layer are emulsion-polymerized is not particularly limited, but from the viewpoint of increasing the efficiency of the polymerization initiator, it is preferable that the atmosphere be an inert gas such as nitrogen gas.
[0121] The polymerization temperature of the monomer components for forming the resin layer is not particularly limited, but is usually preferably 50 to 100° C., more preferably 60 to 85° C. The polymerization temperature may be constant or may be changed during the polymerization reaction.
[0122] The polymerization time for emulsion-polymerizing the monomer components for forming the resin layer is not particularly limited and may be appropriately set depending on the progress of the polymerization reaction, but is usually about 2 to 9 hours.
[0123] By emulsion-polymerizing the monomer components for forming the resin layer as described above, it is possible to obtain an aqueous dispersion containing polymer emulsion particles having a resin layer on the surface. The thickness of the resin layer formed on the polymer emulsion particles having a resin layer on the surface varies depending on the application of the aqueous dispersion containing polymer emulsion particles having a resin layer on the surface, and therefore cannot be determined in general, but is usually about 2 to 50 nm.
[0124] The mass ratio of the inner layer to the surface resin layer of the polymer emulsion particle having a resin layer on its surface [polymer constituting the inner layer / polymer constituting the surface resin layer] is usually preferably 5 / 95 to 80 / 20, more preferably 10 / 90 to 75 / 25.
[0125] The polymer emulsion particle-containing aqueous dispersion of the present invention may contain, for example, additives, etc., within the scope of not impairing the object of the present invention. Examples of additives include those mentioned above. The amount of additive varies depending on the type of additive, so it cannot be determined in general, and it is preferable to appropriately determine the amount depending on the type of additive.
[0126] From the viewpoint of improving weather resistance, it is preferable to use a black pigment or a black dye as an additive and to include the black pigment or black dye in the resin layer.
[0127] The nonvolatile content in the polymer emulsion particle-containing aqueous dispersion is preferably 20% by mass or more, more preferably 25% by mass or more, from the viewpoint of improving productivity, and is preferably 70% by mass or less, more preferably 60% by mass or less, from the viewpoint of improving handleability. Therefore, the nonvolatile content in the polymer emulsion particle-containing aqueous dispersion is preferably 20 to 70% by mass, more preferably 25 to 60% by mass.
[0128] In this specification, the amount of nonvolatile content in the aqueous resin dispersion is calculated by weighing 1 g of the aqueous resin dispersion, drying it at 110° C. for 1 hour in a hot air dryer, and taking the resulting residue as the nonvolatile content, and is calculated by the formula: [Non-volatile content (mass%) in aqueous resin dispersion] = ([mass of residue] ÷ [1 g of aqueous resin dispersion]) × 100 This means the value calculated based on
[0129] 〔others〕 The polymer emulsion particle-containing aqueous dispersion of the present invention and the polymer emulsion particle-containing aqueous dispersion having a resin layer on the surface thereof can be provided with crosslinking properties by adding a crosslinking agent. The crosslinking agent may be one that initiates a crosslinking reaction at room temperature or one that initiates a crosslinking reaction by heat. Examples of the crosslinking agent include oxazoline group-containing compounds, isocyanate group-containing compounds, and aminoplast resins. These crosslinking agents may be used alone or in combination of two or more.
[0130] In addition to the above-mentioned crosslinking agents, crosslinking agents such as carbodiimide compounds, polyvalent metal compounds represented by zirconium compounds, zinc compounds, titanium compounds, and aluminum compounds can be used in the present invention within the scope that does not impair the object of the present invention.
[0131] Furthermore, the polymer emulsion particle-containing aqueous dispersion of the present invention and the polymer emulsion particle-containing aqueous dispersion having a resin layer on the surface thereof may contain additives in appropriate amounts, such as film-forming aids, plasticizers, foam inhibitors, pigments, thickeners, matting agents, dispersants, wetting agents, UV absorbers, UV stabilizers, fillers, leveling agents, stabilizers, pigments, dyes, and antioxidants, within the scope that does not impair the object of the present invention.
[0132] The polymer emulsion particle-containing aqueous dispersion of the present invention and the polymer emulsion particle-containing aqueous dispersion having a resin layer on the surface thereof can both be suitably used, for example, in aqueous paints. The aqueous paint contains the aqueous resin dispersion.
[0133] The water-based paint may be composed only of the water-based resin dispersion, and may contain, within the scope of the object of the present invention, one or more of, for example, a film-forming assistant, a plasticizer, a foam inhibitor, a pigment, a thickener, a matting agent, a dispersant, a wetting agent, an ultraviolet absorber, an ultraviolet stabilizer, a filler, a leveling agent, a stabilizer, a pigment, a dye, an antioxidant, etc. Examples of water-based paints include enamel paints and clear paints.
[0134] The water-based paint may be applied in one layer by itself, or may be applied by overcoating two or more layers. When applying two or more layers by overcoating, only some of the layers may be formed by the water-based paint, or all of the layers may be formed by the water-based paint. Examples of overcoating include a method in which a paint for a first layer (e.g., undercoat layer) is applied to a substrate that has been subjected to a primer treatment or a sealer treatment, and then dried, and a paint for a second layer (e.g., topcoat layer) is applied on top and dried, but the present invention is not limited to such a method.
[0135] Methods for applying the water-based paint include, for example, application methods using a brush, a bar coater, an applicator, an air spray, an airless spray, a roll coater, a flow coater, etc., but the present invention is not limited to only these examples.
[0136] The water-based paint can be suitably used, for example, when painting the exterior walls of buildings and the bodies of automobiles, and can also be suitably used for inorganic building materials such as ceramic building materials. Examples of ceramic building materials include roof tiles and exterior wall materials. Ceramic building materials are obtained by adding inorganic fillers, fibrous materials, etc. to a hydraulic adhesive material that is the raw material of an inorganic hardened body, molding the resulting mixture, and curing and hardening the resulting molded body. Examples of inorganic building materials that constitute the exterior of buildings include flexible boards, calcium silicate boards, gypsum slag perlite boards, wood chip cement boards, precast concrete boards, ALC boards, and gypsum boards. EXAMPLES
[0137] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0138] In the following examples and comparative examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0139] In the following Examples and Comparative Examples, the abbreviations of the respective compounds mean the following compounds. MMA: Methyl methacrylate BMA: n-Butyl methacrylate IBMA: Isobutyl methacrylate ·EHA: 2-Ethylhexyl acrylate EHMA: 2-Ethylhexyl methacrylate CHMA: Cyclohexyl methacrylate St: styrene · LMA: Lauryl methacrylate CTA: Triallyl cyanurate 1,6HXA: 1,6-Hexanediol diacrylate ·KBM-503: Methacryloxypropyltrimethoxysilane SMA: Stearyl methacrylate ·C22MA: Behenyl methacrylate ·C22A: Behenyl acrylate ·DTDMA: Decyltetradecyl methacrylate EHC: 2-Ethylhexanoate hexadecyl ·SS: Stearyl stearate CS-12: 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate HEMA: 2-hydroxyethyl methacrylate
[0140] Example 1 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 12.5 parts of CHMA, 4.5 parts of EHC and 3 parts of an ultraviolet absorber [BASF, trade name: Tinuvin (registered trademark) 400] were charged, a part of the mixture obtained was taken out, and the phase inversion temperature of the mixture was measured based on the following method. As a result, the phase inversion temperature was 75 ° C (the lower limit temperature is the phase inversion start temperature, the same below) to 88 ° C (the upper limit temperature is the phase inversion end temperature, the same below).
[0141] [Method of measuring phase inversion temperature] A 2 L (liter) reaction vessel was equipped with a stirring device and a temperature sensor, and 1000 g of the mixture was placed in the reaction vessel and stirred.
[0142] While the reaction vessel was heated in a water bath, the electrical conductivity was measured with a conductivity meter (manufactured by EUTECH, trade name: Lacom Tester PC450) every time the temperature of the mixture in the reaction vessel increased by 1°C.
[0143] The electrical conductivity was plotted for each temperature increase, and the temperature at which the electrical conductivity began to decrease continuously with increasing temperature was taken as the phase inversion start temperature, and the temperature at which the electrical conductivity became 1.00 μS or less was taken as the phase inversion end temperature.
[0144] In addition, in the case where the electrical conductivity did not become 1.00 μS or less even when the upper limit of the measurable temperature of the conductivity meter was exceeded, the temperature at which the appearance of the mixture did not change even after 3 minutes or more had elapsed since the mixture reached a temperature higher than the phase inversion starting temperature under stirring was regarded as the end point of the phase inversion temperature.
[0145] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0146] After the temperature of the mixture in the reaction vessel reached 90°C, the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40°C or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0147] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined by the following methods. The results are shown in Table 1.
[0148] (1) Dispersion stability The dispersion state of the monomer emulsion particles after the aqueous dispersion containing the monomer emulsion particles was allowed to stand at room temperature (about 25°C) for 12 hours, and the dispersion state of the monomer emulsion particles after the aqueous dispersion containing the monomer emulsion particles was allowed to stand at room temperature (about 25°C) for 14 days were each visually observed, and the dispersion stability of the aqueous dispersion containing the monomer emulsion particles was evaluated based on the following evaluation criteria. [Evaluation Criteria] ◯: No precipitation of monomer emulsion particles and no separation of monomer components from the aqueous medium were observed. ×: At least one of precipitation of monomer emulsion particles and separation of the monomer component from the aqueous medium is observed.
[0149] (2) Average particle size Using a multi-sample nanoparticle size measurement system (manufactured by Otsuka Electronics Co., Ltd., product name: nanoSAQRA), which is a particle size measurement device using a dynamic light scattering method, the average particle size obtained by cumulant analysis of the monomer emulsion particles immediately after production (hereinafter simply referred to as the average particle size) and the average particle size of the monomer emulsion particles after being left to stand for 14 days after production were measured.
[0150] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.4 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reaction vessel, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 80°C.
[0151] Thereafter, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated at 80°C for 6 hours with stirring, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0152] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 62 nm.
[0153] Example 2 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 70 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 12 parts of CHMA, 5 parts of SMA, and 3 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 80 to 92°C.
[0154] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0155] After the internal temperature of the reaction vessel reached 95° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0156] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0157] Example 3 A monomer emulsion particle-containing aqueous dispersion was obtained by carrying out the same operation as in Example 2, except that the amount of CHMA was changed to 9 parts, the amount of SMA was changed to 9 parts, and the amount of the ultraviolet absorber was changed to 2 parts. The phase inversion temperature of the mixture charged in the reaction apparatus was measured in the same manner as in Example 1, and was found to be 80 to 94°C.
[0158] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0159] Example 4 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 67.2 parts of deionized water, 9.6 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 14.4 parts of CHMA, 4.8 parts of EHC and 4 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 78 to 90 ° C.
[0160] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0161] After the internal temperature of the reaction vessel reached 92° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0162] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0163] Example 5 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 65 parts of deionized water, 7.5 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 17 parts of CHMA, 7.5 parts of C22MA and 3 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, and a part of the resulting mixture was taken out and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 75 to 88 ° C.
[0164] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0165] After the internal temperature of the reaction vessel reached 90° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0166] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0167] Example 6 A monomer emulsion particle-containing aqueous dispersion was obtained by carrying out the same operation as in Example 5, except that the amount of deionized water was changed to 60.0 parts, the amount of nonionic emulsifier was changed to 13.3 parts, the amount of CHMA was changed to 16.6 parts, and the amount of C22MA was changed to 7.1 parts in Example 5. The phase inversion temperature of the mixture charged in the reaction apparatus was measured in the same manner as in Example 1, and the phase inversion temperature was 75 to 88°C.
[0168] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0169] Example 7 A monomer emulsion particle-containing aqueous dispersion was obtained by carrying out the same operation as in Example 5, except that the amount of the nonionic emulsifier was changed to 10 parts, the amount of CHMA was changed to 15 parts, and the amount of C22MA was changed to 7 parts in Example 5. The phase inversion temperature of the mixture charged in the reaction apparatus was measured in the same manner as in Example 1, and the phase inversion temperature was 75 to 88°C.
[0170] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0171] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.8 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reaction vessel, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 80°C.
[0172] Thereafter, 1.1 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated at 80°C for 6 hours with stirring, thereby polymerizing the monomers contained in the monomer emulsion particles to obtain an aqueous dispersion containing polymer emulsion particles.
[0173] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 74 nm.
[0174] Example 8 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 7.5 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 13 parts of CHMA, 2.5 parts of EHMA, 4 parts of EHC and 3 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, and a part of the resulting mixture was taken out and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 78 to 90 ° C.
[0175] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0176] After the internal temperature of the reaction vessel reached 92° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0177] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0178] Example 9 Into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 65 parts of deionized water, 10 parts of a polyoxyalkylene alkenyl ether as a nonionic emulsifier (manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6), 16.1 parts of CHMA, 5.4 parts of EHC, 1.5 parts of an ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 400), 1.5 parts of a hindered amine light stabilizer (manufactured by ADEKA Corporation, trade name: Adeka STAB LA-87), and a tert-butyl ether having the formula (I):
[0179] [ka]
[0180] (In the formula, R is each represented by the formula:
[0181] [ka]
[0182] (representing a group represented by A part of the mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 78 to 90°C.
[0183] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0184] After the internal temperature of the reaction vessel reached 92° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0185] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0186] Example 10 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 65 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 14.7 parts of CHMA, 6.8 parts of C22MA, 1.4 parts of ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400], 1.4 parts of hindered amine light stabilizer [manufactured by ADEKA Corporation, trade name: Adeka STAB LA-87] and 0.7 parts of phthalocyanine near infrared absorbing dye represented by formula (I) were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 78 to 90 ° C.
[0187] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0188] After the internal temperature of the reaction vessel reached 92° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0189] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0190] Example 11 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 70 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 14.8 parts of CHMA, 5 parts of EHC, and 0.2 parts of a phthalocyanine near infrared absorbing dye represented by formula (I) were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 75 to 88°C.
[0191] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0192] After the internal temperature of the reaction vessel reached 92° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0193] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0194] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.4 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reaction vessel, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 80°C.
[0195] Thereafter, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated at 80°C for 6 hours with stirring, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0196] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 59 nm.
[0197] Example 12 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 67 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 14 parts of CHMA, 6 parts of C22A, and 3 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 78 to 90 ° C.
[0198] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0199] After the internal temperature of the reaction vessel reached 92° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0200] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0201] Example 13 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 70 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 12 parts of CHMA, 5 parts of DTDMA, and 3 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 78 to 90 ° C.
[0202] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0203] After the internal temperature of the reaction vessel reached 92° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0204] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0205] Example 14 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 70 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 13 parts of CHMA, 4 parts of SS, and 3 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 80 to 94 ° C.
[0206] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0207] After the internal temperature of the reaction vessel reached 95° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0208] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0209] Example 15 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 67 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 3.99 parts of BMA, 12 parts of CHMA, 5 parts of EHC, 2 parts of an ultraviolet absorber [BASF, trade name: Tinuvin (registered trademark) 400] and 0.01 parts of a red dye [Sumika Chemtex Co., Ltd., trade name: Sumiplast Red HL2B] were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 75 to 88 ° C.
[0210] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0211] After the internal temperature of the reaction vessel reached 90° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0212] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0213] Example 16 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 4 parts of IBMA, 8 parts of CHMA, 5 parts of EHC and 3 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, and a part of the resulting mixture was taken out and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 75 to 88 ° C.
[0214] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0215] After the internal temperature of the reaction vessel reached 90° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0216] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0217] Example 17 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 70 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 12 parts of EHMA, 4 parts of EHC, and 4 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 80 to 94 ° C.
[0218] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0219] After the internal temperature of the reaction vessel reached 95° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0220] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0221] Example 18 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 3 parts of MMA, 9 parts of CHMA, 7 parts of EHC and 1 part of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, and a part of the resulting mixture was taken out and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 80 to 91 ° C.
[0222] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0223] After the internal temperature of the reaction vessel reached 93° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0224] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0225] Example 19 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 69 parts of deionized water, 9.9 parts of secondary alcohol ethoxylate as a nonionic emulsifier [manufactured by Nippon Shokubai Co., Ltd., trade name: Softanol 120, HLB: 14.5], 9.9 parts of St, 9.9 parts of SMA and 1.3 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 50 to 56 ° C.
[0226] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0227] After the internal temperature of the reaction vessel reached 57°C, the reaction vessel was removed from the water bath, immersed in an ice water bath, and cooled with stirring until the internal temperature reached 10°C or below, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0228] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0229] Example 20 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 70 parts of deionized water, 10 parts of a nonionic emulsifier (manufactured by ADEKA Corporation, trade name: Adeka Reasoap ER-10, HLB: 12.1), 15.5 parts of CHMA, 1.5 parts of EHC, and 3 parts of an ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 400) were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 52 to 63°C.
[0230] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0231] After the internal temperature of the reaction vessel reached 65°C, the reaction vessel was removed from the water bath and immersed in an ice water bath to cool with stirring. When the internal temperature reached 10°C, 2.4 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added, and the mixture was stirred for 20 minutes while cooling to 10°C to obtain an aqueous dispersion containing monomer emulsion particles.
[0232] The dispersion stability of the thus obtained aqueous dispersion containing monomer emulsion particles and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 1.
[0233] Example 21 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 10.9 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 3.0 parts of MMA, 7.0 parts of CHMA, 4.1 parts of EHC and 8.0 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 84 to 89 ° C.
[0234] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0235] After the internal temperature of the reaction vessel reached 90° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0236] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0237] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.6 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reaction vessel, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 80°C.
[0238] Thereafter, 1.0 part of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated at 80°C for 6 hours with stirring, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0239] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 57 nm.
[0240] Example 22 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 12.3 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 3.5 parts of MMA, 13.8 parts of CHMA, 5.0 parts of EHC, 0.8 parts of oil-soluble ultraviolet absorber [manufactured by Otsuka Chemical Co., Ltd., trade name: RUVA-93] and 1.6 parts of oil-soluble azo-based red dye [manufactured by Chuo Synthetic Chemical Co., Ltd., trade name: Oil Color Red TR-71] were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 75 to 83 ° C.
[0241] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0242] After the internal temperature of the reaction vessel reached 85° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0243] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0244] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 3.0 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reaction vessel, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 80°C.
[0245] Thereafter, 1.1 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated at 80°C for 6 hours with stirring, thereby polymerizing the monomers contained in the monomer emulsion particles to obtain an aqueous dispersion containing polymer emulsion particles.
[0246] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 47 nm.
[0247] Example 23 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 11.5 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 3.1 parts of MMA, 5.5 parts of EHA, 5.8 parts of CHMA, 2.0 parts of CTA, 0.5 parts of KBM-503, 4.4 parts of EHC, 0.7 parts of an oil-soluble ultraviolet absorber [Otsuka Chemical Co., Ltd., trade name: RUVA-93] and 1.5 parts of an oil-soluble azo-based red dye [Chuo Synthetic Chemical Co., Ltd., trade name: Oil Color Red TR-71] were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 79 to 81 ° C.
[0248] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0249] After the internal temperature of the reaction vessel reached 83° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0250] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0251] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.8 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reaction vessel, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 80°C.
[0252] Thereafter, 1.1 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated at 80°C for 6 hours with stirring, thereby polymerizing the monomers contained in the monomer emulsion particles to obtain an aqueous dispersion containing polymer emulsion particles.
[0253] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 42 nm.
[0254] Example 24 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 12.3 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 3.5 parts of MMA, 13.8 parts of CHMA, 5.0 parts of EHC, 0.8 parts of an oil-soluble ultraviolet absorber [manufactured by Otsuka Chemical Co., Ltd., trade name: RUVA-93] and 1.6 parts of an oil-soluble chromium complex salt-based red dye were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 79 to 85 ° C.
[0255] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0256] After the internal temperature of the reaction vessel reached 87° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0257] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0258] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 3.0 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reaction vessel, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 80°C.
[0259] Thereafter, 1.1 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated at 80°C for 6 hours with stirring, thereby polymerizing the monomers contained in the monomer emulsion particles to obtain an aqueous dispersion containing polymer emulsion particles.
[0260] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 50 nm.
[0261] Example 25 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 11.5 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 3.1 parts of MMA, 5.5 parts of EHA, 5.8 parts of CHMA, 2.0 parts of CTA, 4.4 parts of EHC, 0.7 parts of an oil-soluble ultraviolet absorber [manufactured by Otsuka Chemical Co., Ltd., trade name: RUVA-93] and 1.5 parts of an oil-soluble chromium complex red dye were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 79 to 81 ° C.
[0262] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0263] After the internal temperature of the reaction vessel reached 83° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0264] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0265] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.8 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reaction vessel, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 80°C.
[0266] Thereafter, 1.1 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated at 80°C for 6 hours with stirring, thereby polymerizing the monomers contained in the monomer emulsion particles to obtain an aqueous dispersion containing polymer emulsion particles.
[0267] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 41 nm.
[0268] Example 26 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 12.3 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 3.5 parts of MMA, 11.8 parts of CHMA, 7.0 parts of EHC, 0.8 parts of an oil-soluble ultraviolet absorber [manufactured by Otsuka Chemical Co., Ltd., trade name: RUVA-93] and 1.6 parts of an oil-soluble chromium complex red dye were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 86 to 91 ° C.
[0269] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0270] After the internal temperature of the reaction vessel reached 93° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0271] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0272] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 3.0 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reaction vessel, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 80°C.
[0273] Thereafter, 1.1 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated at 80°C for 6 hours with stirring, thereby polymerizing the monomers contained in the monomer emulsion particles to obtain an aqueous dispersion containing polymer emulsion particles.
[0274] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 48 nm.
[0275] Example 27 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 70 parts of deionized water, 10 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 1 part of MMA, 6.8 parts of CHMA, 4.2 parts of EHC and 8 parts of an ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 400] were charged, a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 80 to 94 ° C.
[0276] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0277] After the internal temperature of the reaction vessel reached 95° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0278] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0279] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.4 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 80°C.
[0280] Thereafter, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated at 80°C for 6 hours with stirring, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0281] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 80 nm.
[0282] Example 28 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 67 parts of deionized water, 10.9 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier (manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6), 3.0 parts of MMA, 7.0 parts of CHMA, 0.4 parts of St, 0.3 parts of 1,6HXA, 4.1 parts of EHC, 3.0 parts of an ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 400), 3.0 parts of an ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 479), 0.3 parts of a hindered amine light stabilizer (manufactured by ADEKA Corporation, trade name: Adeka STAB LA-87), and 1.0 part of an oil-soluble chromium complex red dye were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was found to be 76 to 83°C.
[0283] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0284] After the internal temperature of the reaction vessel reached 86° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0285] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0286] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.6 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 72°C.
[0287] Then, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated with stirring at an internal temperature of 72°C for 1 hour, and then at an internal temperature of 80°C for 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0288] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 51 nm.
[0289] Example 29 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 67 parts of deionized water, 10.8 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 3.0 parts of MMA, 10.4 parts of CHMA, 0.6 parts of 1,6HXA, 0.7 parts of KBM-503, 3.5 parts of EHC, 2.6 parts of an ultraviolet absorber [BASF, trade name: Tinuvin (registered trademark) 400], 1.3 parts of an oil-soluble azo-based red dye and 0.1 parts of an oil-soluble chromium complex salt-based black dye [Orient Chemical Industry Co., Ltd., trade name: VALIFAST BLACK 3810] were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 75 to 79 ° C.
[0290] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0291] After the internal temperature of the reaction vessel reached 83° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0292] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0293] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.6 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 72°C.
[0294] Then, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the mixture was allowed to react at an internal temperature of 72°C for 1 hour. The contents of the reaction vessel were then heated with stirring at an internal temperature of 80°C for an additional 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0295] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 53 nm.
[0296] Example 30 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 67 parts of deionized water, 10.8 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 3.0 parts of MMA, 11.6 parts of CHMA, 0.3 parts of 1,6HXA, 1.1 parts of C22A, 3.3 parts of CS-12, 1.6 parts of ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 479], 0.3 parts of hindered amine light stabilizer [manufactured by ADEKA Corporation, trade name: Adeka STAB LA-87] and 1.0 parts of oil-soluble chromium complex red dye were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 67 to 84 ° C.
[0297] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0298] After the internal temperature of the reaction vessel reached 86° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0299] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0300] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.6 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 70°C.
[0301] Then, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated with stirring at an internal temperature of 70°C for 1 hour, and then at an internal temperature of 80°C for 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0302] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 41 nm.
[0303] Example 31 Into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 64 parts of deionized water, 10.8 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier (manufactured by Kao Corporation, product name: LATEMURU PD-420, HLB: 12.6), 3.0 parts of MMA, 9.9 parts of CHMA, 1.5 parts of St, 0.3 parts of 1,6HXA, 4.2 parts of EHC, 2.0 parts of an ultraviolet absorber (manufactured by BASF, product name: Tinuvin (registered trademark) 400), and 2.0 parts of Tinuvin (registered trademark) 479, 0.5 parts of UV absorber (manufactured by BASF, product name: Tinuvin (registered trademark) 970), 0.4 parts of oil-soluble UV absorber (manufactured by ADEKA Corporation, product name: Adeka STAB LA-F70), 0.3 parts of hindered amine light stabilizer (manufactured by ADEKA Corporation, product name: Adeka STAB LA-87), and 1.0 parts of oil-soluble chromium complex red dye were charged, and a part of the resulting mixture was taken out and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 72 to 81°C.
[0304] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0305] After the internal temperature of the reaction vessel reached 85° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0306] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0307] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.9 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 72°C.
[0308] Then, 1.0 part of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated with stirring at an internal temperature of 72°C for 1 hour and then at an internal temperature of 80°C for 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0309] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 49 nm.
[0310] Example 32 Into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 67 parts of deionized water, 9.5 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier (manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6), 3.0 parts of MMA, 12.0 parts of CHMA, 0.9 parts of St, 0.3 parts of 1,6HXA, 1.1 parts of C22A, 3.3 parts of CS-12, ultraviolet light, 1.0 part of absorbent (manufactured by BASF, trade name: Tinuvin (registered trademark) 479), 0.3 parts of oil-soluble ultraviolet absorber (manufactured by Otsuka Chemical Co., Ltd., trade name: RUVA-93), 0.3 parts of hindered amine light stabilizer (manufactured by ADEKA Corporation, trade name: Adeka STAB LA-87), 1.0 part of oil-soluble chromium complex salt red dye, and 0.3 parts of oil-soluble chromium complex salt black dye (manufactured by Orient Chemical Industry Co., Ltd., trade name: VALIFAST BLACK 3810) were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 82 to 88 ° C.
[0311] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0312] After the internal temperature of the reaction vessel reached 85° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0313] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0314] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.9 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 72°C.
[0315] Then, 1.0 part of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated with stirring at an internal temperature of 72°C for 1 hour and then at an internal temperature of 80°C for 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0316] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 56 nm.
[0317] Example 33 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube and a dropping funnel, 67 parts of deionized water, 10.8 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier [Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6], 1.0 parts of MMA, 10.2 parts of CHMA, 3.8 parts of St, 0.3 parts of 1,6HXA, 4.5 parts of EHC, 1.5 parts of ultraviolet absorber [BASF, trade name: Tinuvin (registered trademark) 479], 0.4 parts of hindered amine light stabilizer [ADEKA Corporation, trade name: Adeka STAB LA-87] and 0.5 parts of oil-soluble blue dye [Kiwa Chemical Industry Co., Ltd., trade name: KP Plast Blue R] were charged, and a part of the obtained mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 73 to 82 ° C.
[0318] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0319] After the internal temperature of the reaction vessel reached 85° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0320] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0321] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.6 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 72°C.
[0322] Then, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated with stirring at an internal temperature of 72°C for 1 hour, and then at an internal temperature of 80°C for 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0323] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 53 nm.
[0324] Example 34 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 66 parts of deionized water, 9.9 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier (manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6), 2.0 parts of MMA, 10.2 parts of CHMA, 3.8 parts of St, 0.3 parts of 1,6HXA, 5.0 parts of C22A, 1.5 parts of an ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 479), 0.4 parts of a hindered amine light stabilizer (manufactured by ADEKA Corporation, trade name: Adeka STAB LA-87), 0.5 parts of an oil-soluble blue dye (manufactured by Kiwa Chemical Industry Co., Ltd., trade name: KP Plast Blue R), and 0.5 parts of an oil-soluble chromium complex black dye (manufactured by Orient Chemical Industry Co., Ltd., trade name: VALIFAST) were added. A portion of the resulting mixture was taken out and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 77 to 88°C.
[0325] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0326] After the internal temperature of the reaction vessel reached 90° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0327] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0328] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.9 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 72°C.
[0329] Then, 1.0 part of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated with stirring at an internal temperature of 72°C for 1 hour and then at an internal temperature of 80°C for 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0330] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 64 nm.
[0331] Example 35 Into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 66 parts of deionized water, 10.9 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier (manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6), 3.0 parts of MMA, 9.0 parts of CHMA, 0.4 parts of St, 0.3 parts of 1,6HXA, 4.1 parts of EHC, 3.0 parts of ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 479), 1.0 part of ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 970), 0.3 parts of hindered amine light stabilizer (manufactured by ADEKA Corporation, trade name: Adeka STAB LA-87), and oil-soluble yellow dye (manufactured by SHIRADO CHEMICAL CO., LTD., Oil Yellow 5GS) were added. A part of the resulting mixture was taken out and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 74 to 83°C.
[0332] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0333] After the internal temperature of the reaction vessel reached 87° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0334] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0335] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.6 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 72°C.
[0336] Then, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated with stirring at an internal temperature of 72°C for 1 hour, and then at an internal temperature of 80°C for 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0337] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 49 nm.
[0338] Example 36 Into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel were added 67 parts of deionized water, 10.8 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier (manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6), 2.8 parts of MMA, 11.8 parts of CHMA, 0.3 parts of 1,6HXA, 4.4 parts of EHC, 1.0 part of ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 400), 0.3 parts of oil-soluble ultraviolet absorber (manufactured by ADEKA Corporation, trade name: Adeka STAB LA-F70), 0.6 parts of hindered amine light stabilizer (manufactured by ADEKA Corporation, trade name: Adeka STAB LA-87), and oil-soluble chromium complex black dye (manufactured by Orient Chemical Industries Co., Ltd., trade name: VALIFAST). A portion of the resulting mixture was taken out and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 82 to 91°C.
[0339] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0340] After the internal temperature of the reaction vessel reached 92° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0341] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0342] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.6 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 75°C.
[0343] Then, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated with stirring at an internal temperature of 75°C for 1 hour, and then at an internal temperature of 80°C for 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0344] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 57 nm.
[0345] Example 37 Into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 67 parts of deionized water, 10.0 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier (manufactured by Kao Corporation, product name: LATEMURU PD-420, HLB: 12.6), 2.9 parts of MMA, 8.1 parts of CHMA, 1.0 part of St, 0.3 parts of 1,6HXA, 4.4 parts of EHC, 2.5 parts of ultraviolet absorber (manufactured by BASF, product name: Tinuvin (registered trademark) 400), 0.5 parts of ultraviolet absorber (manufactured by BASF, product name: Tinuvin (registered trademark) 479), and oil-soluble ultraviolet absorber (SHUANG BANG INDUSTRIAL 2.0 parts of a UV-UVA650 (manufactured by ADEKA CORPORATION, product name: SB-UVA650), 1.0 part of a hindered amine light stabilizer (manufactured by ADEKA CORPORATION, product name: Adeka STAB LA-87), and 0.3 parts of an oil-soluble chromium complex black dye (manufactured by Orient Chemical Industries Co., Ltd., product name: VALIFAST BLACK 3810) were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 86 to 91°C.
[0346] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0347] After the internal temperature of the reaction vessel reached 92° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0348] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0349] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.6 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 75°C.
[0350] Then, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated with stirring at an internal temperature of 75°C for 1 hour, and then at an internal temperature of 80°C for 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0351] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 55 nm.
[0352] Example 38 Into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 67 parts of deionized water, 10.4 parts of polyoxyalkylene alkenyl ether as a nonionic emulsifier (manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6), 2.9 parts of MMA, 7.7 parts of CHMA, 0.8 parts of St, 0.3 parts of 1,6HXA, 4.4 parts of EHC, an ultraviolet absorber (manufactured by BASF, trade name: Tinuv In (registered trademark) 400] 2.0 parts, ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 479] 2.0 parts, ultraviolet absorber [manufactured by BASF, trade name: Tinuvin (registered trademark) 970] 1.0 parts, hindered amine light stabilizer [manufactured by ADEKA Corporation, trade name: Adeka STAB LA-87] 1.0 parts, and oil-soluble chromium complex black dye [manufactured by Orient Chemical Industry Co., Ltd., trade name: VALIFAST BLACK 3810] 0.5 parts were charged, and a part of the obtained mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 80 to 88 ° C.
[0353] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0354] After the internal temperature of the reaction vessel reached 90° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0355] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0356] Next, 100 parts of the monomer emulsion particle-containing aqueous dispersion obtained above was placed in a reaction vessel, and 2.6 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20) was added to the reaction vessel. The mixture was stirred at room temperature for 30 minutes while introducing nitrogen gas into the reactor, and then the reaction vessel was placed in a water bath and heated in the water bath while stirring until the internal temperature of the reaction vessel reached 75°C.
[0357] Then, 0.9 parts of a 5% aqueous potassium persulfate solution was added to the reaction vessel, and the contents of the reaction vessel were heated with stirring at an internal temperature of 75°C for 1 hour, and then at an internal temperature of 80°C for 5 hours, thereby polymerizing the monomers contained in the monomer emulsion particles and obtaining an aqueous dispersion containing polymer emulsion particles.
[0358] The average particle size of the polymer emulsion particles contained in the aqueous dispersion containing the polymer emulsion particles obtained above was measured in the same manner as above, and the average particle size of the polymer emulsion particles was found to be 50 nm.
[0359] Comparative Example 1 In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 70 parts of deionized water, 9 parts of polyoxyalkylene alkenyl ether (manufactured by Kao Corporation, trade name: LATEMURU PD-420, HLB: 12.6) as a nonionic emulsifier, 9 parts of CHMA, 9 parts of LMA, and 3 parts of an ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 400) were charged, and a part of the resulting mixture was taken out, and the phase inversion temperature of the mixture was measured in the same manner as in Example 1. As a result, the phase inversion temperature was 80 to 92°C.
[0360] After measuring the phase inversion temperature of the mixture, the reaction vessel was heated in a water bath under stirring while nitrogen gas was introduced into the reaction vessel.
[0361] After the internal temperature of the reaction vessel reached 94° C., the reaction vessel was removed from the water bath and air-cooled with stirring until the internal temperature reached 40° C. or lower, thereby obtaining an aqueous dispersion containing monomer emulsion particles.
[0362] The dispersion stability of the monomer emulsion particle-containing aqueous dispersion obtained above and the average particle size of the monomer emulsion particles were examined in the same manner as in Example 1. The results are shown in Table 2.
[0363] Next, the obtained aqueous dispersion containing the monomer emulsion particles was allowed to stand at room temperature for 12 hours, and it was confirmed that the monomer emulsion particles and the aqueous medium were separated.
[0364] Comparative Example 2 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 70 parts of deionized water, 10 parts of a polyoxyalkylene alkenyl ether (manufactured by Kao Corporation, product name: LATEMULU PD-420, HLB: 12.6) as a nonionic emulsifier, 17 parts of CHMA, and 3 parts of an ultraviolet absorber (manufactured by BASF, product name: Tinuvin (registered trademark) 400), and the reaction vessel was heated using a water bath with stirring while introducing nitrogen gas into the reaction vessel.
[0365] After the internal temperature of the reaction vessel reached 90° C., the reaction vessel was removed from the water bath and air-cooled under stirring until the internal temperature reached 30° C. or less, thereby obtaining an aqueous dispersion containing monomer emulsion particles, but the monomer emulsion particles and the aqueous medium had already separated when the internal temperature reached 30° C. This shows that the aqueous dispersion containing monomer emulsion particles obtained as described above has significantly poor dispersion stability.
[0366] Even when the temperature of the aqueous dispersion containing the monomer emulsion particles obtained above was raised to 100° C., the phase inversion temperature could not be confirmed.
[0367] Comparative Example 3 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 77 parts of deionized water, 1.8 parts of an anionic emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20), 20 parts of MMA, 1 part of hexadecane, and 0.2 parts of the phthalocyanine near-infrared absorbing dye represented by formula (I), and the reaction vessel was heated using a water bath with stirring while introducing nitrogen gas into the reaction vessel.
[0368] After the internal temperature of the reaction vessel reached 90° C., the reaction vessel was removed from the water bath and air-cooled under stirring until the internal temperature reached 30° C. or less, thereby obtaining an aqueous dispersion containing monomer emulsion particles, but the monomer emulsion particles and the aqueous medium had already separated when the internal temperature reached 30° C. This shows that the aqueous dispersion containing monomer emulsion particles obtained as described above has significantly poor dispersion stability.
[0369] Even when the temperature of the aqueous dispersion containing the monomer emulsion particles obtained above was raised to 100° C., the phase inversion temperature could not be confirmed.
[0370] [Table 1]
[0371] [Table 2]
[0372] The results shown in Tables 1 and 2 show that, according to each Example, an aqueous dispersion containing monomer emulsion particles in which monomer emulsion particles having a small average particle size are stably dispersed for a long period of time can be obtained without using equipment such as a mixer for high-viscosity paints or a high-pressure homogenizer.
[0373] Furthermore, in Examples 21 to 38, the average particle size of the polymer emulsion particles obtained using the monomer emulsion particle-containing aqueous dispersion was almost the same as the average particle size of the monomer emulsion particles used as the raw material, which shows that the average particle size of the monomer emulsion particles can be maintained.
[0374] Example 39 Into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel, 13.3 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 11 and 26 parts of deionized water were charged, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0375] While maintaining the internal temperature at 80° C., 2.28 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel and stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 16 parts of deionized water, 5.76 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20), 14 parts of MMA, 12.6 parts of EHA, 8 parts of CHMA, 0.8 parts of a hindered amine light stabilizer (manufactured by ADEKA Corporation, product name: Adeka STAB LA-87), and 0.6 parts of HEMA was added dropwise to the reaction vessel over a period of 90 minutes while stirring.
[0376] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 11. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 41.8% by mass.
[0377] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 104 nm.
[0378] Example 40 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 26.4 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 11 and 44.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0379] While maintaining the internal temperature at 80° C., 1.43 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel and stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 5.8 parts of deionized water, 3.76 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20), 8.5 parts of MMA, 4.8 parts of EHA, 4.1 parts of CHMA, 0.5 parts of a hindered amine light stabilizer (manufactured by ADEKA Corporation, product name: Adeka STAB LA-87), and 0.3 parts of HEMA was added dropwise to the reaction vessel over a period of 90 minutes while stirring.
[0380] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 11. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 26.7% by mass.
[0381] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 75 nm.
[0382] Example 41 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 24 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 27 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0383] While maintaining the internal temperature at 80° C., 1.43 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel and stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 7.51 parts of deionized water, 3.76 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20), 8.9 parts of MMA, 8 parts of EHA, 5.1 parts of CHMA, 0.5 parts of a hindered amine light stabilizer (manufactured by ADEKA Corporation, product name: Adeka STAB LA-87), and 0.4 parts of HEMA was added dropwise to the reaction vessel over a period of 90 minutes while stirring.
[0384] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 27. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 30.9% by mass.
[0385] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 96 nm.
[0386] Example 42 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 24.0 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 1 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0387] While maintaining the internal temperature at 80° C., 1.43 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel and stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 7.51 parts of deionized water, 3.76 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20), 8.9 parts of MMA, 8 parts of EHA, 5.1 parts of CHMA, 0.5 parts of a hindered amine light stabilizer (manufactured by ADEKA Corporation, product name: Adeka STAB LA-87), and 0.4 parts of HEMA was added dropwise to the reaction vessel over a period of 90 minutes while stirring.
[0388] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 1. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 30.9% by mass.
[0389] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 87 nm.
[0390] Example 43 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 12.3 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 21 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0391] While maintaining the internal temperature at 80° C., 2.28 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel and stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 7.51 parts of deionized water, 5.68 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20), 13.8 parts of MMA, 12.5 parts of EHA, 7.9 parts of CHMA, 0.6 parts of a hindered amine light stabilizer (manufactured by ADEKA Corporation, product name: Adeka STAB LA-87), and 0.8 parts of HEMA was added dropwise to the reaction vessel over a period of 90 minutes while stirring.
[0392] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 21. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 40.0% by mass.
[0393] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 96 nm.
[0394] Example 44 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 12.3 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 27 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0395] While maintaining the internal temperature at 80° C., 2.28 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel and stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 7.51 parts of deionized water, 5.68 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20), 13.8 parts of MMA, 12.5 parts of EHA, 7.9 parts of CHMA, 0.6 parts of a hindered amine light stabilizer (manufactured by ADEKA Corporation, product name: Adeka STAB LA-87), and 0.8 parts of HEMA was added dropwise to the reaction vessel over a period of 90 minutes while stirring.
[0396] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 21. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 39.7% by mass.
[0397] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 118 nm.
[0398] Example 45 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 21.0 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 22 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0399] While maintaining the internal temperature at 80° C., 1.43 parts of 3.5% ammonium persulfate aqueous solution was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 7.51 parts of deionized water, 3.6 parts of a 25% aqueous solution of an anionic emulsifier [ADEKA Corporation, trade name: Adeka Reasoap SR-20], 6.8 parts of MMA, 6.0 parts of EHA, 3.8 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer [ADEKA Corporation, trade name: Adeka STAB LA-87], 0.3 parts of HEMA, 0.2 parts of an ultraviolet absorbing monomer [Otsuka Chemical Co., Ltd., trade name: RUVA-93], and 0.1 parts of methacryloyloxypropyltrimethoxysilane [Shin-Etsu Chemical Co., Ltd., product number: KMB-503] was added dropwise to the reaction vessel over 90 minutes under stirring.
[0400] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 22. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 26.0% by mass.
[0401] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 60 nm.
[0402] Example 46 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 22.9 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 23 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0403] While maintaining the internal temperature at 80° C., 1.43 parts of 3.5% ammonium persulfate aqueous solution was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 7.51 parts of deionized water, 3.12 parts of a 25% aqueous solution of an anionic emulsifier [ADEKA Corporation, trade name: Adeka Reasoap SR-20], 5.7 parts of MMA, 5.7 parts of EHA, 3.8 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer [ADEKA Corporation, trade name: Adeka STAB LA-87], 0.3 parts of HEMA, 0.2 parts of an ultraviolet absorbing monomer [Otsuka Chemical Co., Ltd., trade name: RUVA-93], and 1.3 parts of methacryloyloxypropyltrimethoxysilane [Shin-Etsu Chemical Co., Ltd., product number: KMB-503] was added dropwise to the reaction vessel over 90 minutes under stirring.
[0404] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 23. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 26.0% by mass.
[0405] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 62 nm.
[0406] Example 47 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 21.0 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 24 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0407] While maintaining the internal temperature at 80° C., 1.43 parts of 3.5% ammonium persulfate aqueous solution was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 7.51 parts of deionized water, 3.6 parts of a 25% aqueous solution of an anionic emulsifier [ADEKA Corporation, trade name: Adeka Reasoap SR-20], 6.8 parts of MMA, 6.0 parts of EHA, 3.8 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer [ADEKA Corporation, trade name: Adeka STAB LA-87], 0.3 parts of HEMA, 0.2 parts of an ultraviolet absorbing monomer [Otsuka Chemical Co., Ltd., trade name: RUVA-93], and 0.1 parts of methacryloyloxypropyltrimethoxysilane [Shin-Etsu Chemical Co., Ltd., product number: KMB-503] was added dropwise to the reaction vessel over 90 minutes under stirring.
[0408] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 24. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 26.0% by mass.
[0409] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 72 nm.
[0410] Example 48 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 22.9 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 25 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0411] While maintaining the internal temperature at 80° C., 1.43 parts of 3.5% ammonium persulfate aqueous solution was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 7.51 parts of deionized water, 3.12 parts of a 25% aqueous solution of an anionic emulsifier [ADEKA Corporation, trade name: Adeka Reasoap SR-20], 5.7 parts of MMA, 5.7 parts of EHA, 3.8 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer [ADEKA Corporation, trade name: Adeka STAB LA-87], 0.3 parts of HEMA, 0.2 parts of an ultraviolet absorbing monomer [Otsuka Chemical Co., Ltd., trade name: RUVA-93], and 1.3 parts of methacryloyloxypropyltrimethoxysilane [Shin-Etsu Chemical Co., Ltd., product number: KMB-503] was added dropwise to the reaction vessel over 90 minutes under stirring.
[0412] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 25. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 26.0% by mass.
[0413] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 61 nm.
[0414] Example 49 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 21.0 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 26 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0415] While maintaining the internal temperature at 80° C., 1.43 parts of 3.5% ammonium persulfate aqueous solution was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 7.51 parts of deionized water, 3.6 parts of a 25% aqueous solution of an anionic emulsifier [ADEKA Corporation, trade name: Adeka Reasoap SR-20], 6.8 parts of MMA, 6.0 parts of EHA, 3.8 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer [ADEKA Corporation, trade name: Adeka STAB LA-87], 0.3 parts of HEMA, 0.2 parts of an ultraviolet absorbing monomer [Otsuka Chemical Co., Ltd., trade name: RUVA-93], and 0.1 parts of methacryloyloxypropyltrimethoxysilane [Shin-Etsu Chemical Co., Ltd., product number: KMB-503] was added dropwise to the reaction vessel over 90 minutes under stirring.
[0416] Sixty minutes after the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. Thirty minutes after the end of the neutralization, the reaction vessel was removed from the water bath, and the internal temperature of the reaction vessel was cooled to 40°C or less, thereby obtaining an aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing the monomer component for forming a resin layer on the surface of the polymer emulsion particles obtained in Example 26. The non-volatile content of the aqueous dispersion containing polymer emulsion particles having a resin layer obtained above was 26.0% by mass.
[0417] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 63 nm.
[0418] Example 50 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 27.9 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 28 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0419] While maintaining the internal temperature at 80° C., 2.6 parts of 3.5% ammonium persulfate aqueous solution was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 9.1 parts of deionized water, 2.5 parts of a 25% aqueous solution of an anionic emulsifier [ADEKA Corporation, trade name: Adeka Reasoap SR-20], 6.0 parts of MMA, 6.2 parts of EHA, 3.7 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer [ADEKA Corporation, trade name: Adeka STAB LA-87], 0.3 parts of HEMA, 0.6 parts of an ultraviolet absorbing monomer [Otsuka Chemical Co., Ltd., trade name: RUVA-93], and 0.1 parts of methacryloyloxypropyltrimethoxysilane [Shin-Etsu Chemical Co., Ltd., product number: KMB-503] was added dropwise to the reaction vessel over 90 minutes under stirring.
[0420] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle obtained in Example 28. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 26.0% by mass.
[0421] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 68 nm.
[0422] Example 51 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 27.9 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 28 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0423] While maintaining the internal temperature at 80° C., 2.6 parts of 3.5% ammonium persulfate aqueous solution was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 9.1 parts of deionized water, 2.5 parts of a 25% aqueous solution of an anionic emulsifier [ADEKA Corporation, trade name: Adeka Reasoap SR-20], 6.0 parts of MMA, 6.1 parts of EHA, 3.7 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer [ADEKA Corporation, trade name: Adeka STAB LA-87], 0.3 parts of HEMA, 0.6 parts of an ultraviolet absorbing monomer [Otsuka Chemical Co., Ltd., trade name: RUVA-93], 0.1 parts of methacryloyloxypropyltrimethoxysilane [Shin-Etsu Chemical Co., Ltd., product number: KMB-503], and 0.1 parts of an oil-soluble chromium complex red dye was added dropwise to the reaction vessel over 90 minutes under stirring.
[0424] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle obtained in Example 28. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 26.0% by mass.
[0425] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 70 nm.
[0426] Example 52 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 27.9 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 28 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0427] While maintaining the internal temperature at 80°C, 2.6 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80°C, 9.1 parts of deionized water, 2.5 parts of a 25% aqueous solution of an anionic emulsifier [manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20], 5.8 parts of MMA, 5.9 parts of EHA, 3.7 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer [manufactured by ADEKA Corporation, product name: Adeka STAB LA-87], 0.3 parts of HEMA, and an ultraviolet absorbing monomer [manufactured by Otsuka Chemical Co., Ltd., product name: RUVA- A mixture of 0.6 parts of methacryloyloxypropyltrimethoxysilane [manufactured by Shin-Etsu Chemical Co., Ltd., product number: KMB-503], 0.2 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 479], 0.2 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 970], and 0.1 parts of an oil-soluble chromium complex black dye was added dropwise to a reaction vessel over a period of 90 minutes with stirring.
[0428] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle obtained in Example 28. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 26.0% by mass.
[0429] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 75 nm.
[0430] Example 53 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 27.9 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 29 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0431] While maintaining the internal temperature at 80° C., 2.6 parts of 3.5% ammonium persulfate aqueous solution was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80° C., a mixture of 9.1 parts of deionized water, 2.5 parts of a 25% aqueous solution of an anionic emulsifier [ADEKA Corporation, trade name: Adeka Reasoap SR-20], 6.0 parts of MMA, 6.1 parts of EHA, 3.7 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer [ADEKA Corporation, trade name: Adeka STAB LA-87], 0.3 parts of HEMA, 0.6 parts of an ultraviolet absorbing monomer [Otsuka Chemical Co., Ltd., trade name: RUVA-93], 0.1 parts of methacryloyloxypropyltrimethoxysilane [Shin-Etsu Chemical Co., Ltd., product number: KMB-503], and 0.1 parts of an oil-soluble chromium complex black dye was added dropwise to the reaction vessel over 90 minutes under stirring.
[0432] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer obtained in Example 29 by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 26.0% by mass.
[0433] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 63 nm.
[0434] Example 54 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 41.1 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 31 and 35.1 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0435] While maintaining the internal temperature at 80°C, 1.4 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel, and the mixture was stirred for 10 minutes. Thereafter, while maintaining the internal temperature at 80°C, 7.1 parts of deionized water, 1.6 parts of a 25% aqueous solution of an anionic emulsifier [manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20], 4.5 parts of MMA, 4.7 parts of EHA, 2.8 parts of CHMA, 0.6 parts of a hindered amine-based light stabilizer [manufactured by ADEKA Corporation, product name: Adeka STAB LA-87], 0.2 parts of HEMA, 0.4 parts of an ultraviolet absorbing monomer [manufactured by Otsuka Chemical Co., Ltd., product name: RUVA-93], and methacryloyloxypropyltrimethoxysilane were added. A mixture of 0.1 part of orthoquinone (manufactured by Shin-Etsu Chemical Co., Ltd., product number: KMB-503), 0.2 parts of an ultraviolet absorber (manufactured by BASF, product name: Tinuvin (registered trademark) 479), 0.1 part of an ultraviolet absorber (manufactured by BASF, product name: Tinuvin (registered trademark) 970), 0.1 part of an oil-soluble ultraviolet absorber (manufactured by ADEKA Corporation, product name: Adeka STAB LA-F70), 0.1 part of an oil-soluble chromium complex salt red dye, and 0.1 part of an oil-soluble chromium complex salt black dye was added dropwise to a reaction vessel over a period of 90 minutes with stirring.
[0436] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle obtained in Example 31. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 26.0% by mass.
[0437] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 55 nm.
[0438] Example 55 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 27.9 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 32 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0439] While maintaining the internal temperature at 80°C, 2.6 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80°C, 9.1 parts of deionized water, 2.5 parts of a 25% aqueous solution of an anionic emulsifier [manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20], 5.8 parts of MMA, 5.9 parts of EHA, 3.7 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer [manufactured by ADEKA Corporation, product name: Adeka STAB LA-87], 0.3 parts of HEMA, and an ultraviolet absorbing monomer [manufactured by Otsuka Chemical Co., Ltd., product name: RUVA- A mixture of 0.6 parts of methacryloyloxypropyltrimethoxysilane [manufactured by Shin-Etsu Chemical Co., Ltd., product number: KMB-503], 0.2 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 479], 0.1 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 970], and 0.1 parts of an oil-soluble chromium complex black dye was added dropwise to a reaction vessel over a period of 90 minutes with stirring.
[0440] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle obtained in Example 32. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 26.0% by mass.
[0441] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 71 nm.
[0442] Example 56 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 30.6 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 33 and 31.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0443] While maintaining the internal temperature at 80°C, 1.7 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel, and the mixture was stirred for 10 minutes. Then, while maintaining the internal temperature at 80°C, 13.9 parts of deionized water, 2.9 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20), 6.7 parts of MMA, 6.9 parts of EHA, 4.1 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer (manufactured by ADEKA Corporation, product name: Adeka STAB LA-87), 0.3 parts of HEMA, and an ultraviolet absorbing monomer (manufactured by Otsuka Chemical Co., Ltd., product name: RUVA-9 A mixture of 0.6 parts of methyl methacrylate crosslinker [manufactured by Shin-Etsu Chemical Co., Ltd., product number: KMB-503], 0.2 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 479], 0.2 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 970], and 0.1 parts of an oil-soluble chromium complex black dye was added dropwise to a reaction vessel over a period of 90 minutes with stirring.
[0444] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle obtained in Example 33. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 30.0% by mass.
[0445] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 67 nm.
[0446] Example 57 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 30.6 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 34 and 31.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0447] While maintaining the internal temperature at 80° C., 1.7 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel, and the mixture was stirred for 10 minutes. Thereafter, while maintaining the internal temperature at 80° C., 13.9 parts of deionized water, 2.9 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20), 6.7 parts of MMA, 6.9 parts of EHA, 4.1 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer (manufactured by ADEKA Corporation, product name: Adeka STAB LA-87), 0.3 parts of HEMA, and an ultraviolet absorbing monomer (manufactured by Otsuka Chemical Co., Ltd., product name: RUV A mixture of 0.6 parts of methacryloyloxypropyltrimethoxysilane [manufactured by Shin-Etsu Chemical Co., Ltd., product number: KMB-503], 0.2 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 479], 0.2 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 970], and 0.1 parts of an oil-soluble blue dye was added dropwise to a reaction vessel over a period of 90 minutes with stirring.
[0448] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle obtained in Example 34. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 30.0% by mass.
[0449] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 78 nm.
[0450] Example 58 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 27.9 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 36 and 40.4 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0451] While maintaining the internal temperature at 80° C., 2.6 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel, and the mixture was stirred for 10 minutes. Thereafter, while maintaining the internal temperature at 80°C, a mixture of 9.1 parts of deionized water, 2.5 parts of a 25% aqueous solution of an anionic emulsifier (manufactured by ADEKA CORPORATION, trade name: Adeka Reasoap SR-20), 5.8 parts of MMA, 5.9 parts of EHA, 3.7 parts of CHMA, 0.4 parts of a hindered amine-based light stabilizer (manufactured by ADEKA CORPORATION, trade name: Adeka STAB LA-87), 0.3 parts of HEMA, 0.6 parts of an ultraviolet absorbing monomer (manufactured by Otsuka Chemical Co., Ltd., trade name: RUVA-93), 0.1 parts of methacryloyloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product number: KMB-503), 0.2 parts of an ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 479), and 0.2 parts of an ultraviolet absorber (manufactured by BASF, trade name: Tinuvin (registered trademark) 970) was added dropwise to the reaction vessel over a period of 90 minutes under stirring.
[0452] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle obtained in Example 36. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 26.0% by mass.
[0453] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 70 nm.
[0454] Example 59 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 32.6 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 37 and 28.0 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0455] While maintaining the internal temperature at 80°C, 1.8 parts of 3.5% ammonium persulfate aqueous solution was added to the reaction vessel, and the mixture was stirred for 10 minutes. Thereafter, while maintaining the internal temperature at 80°C, 13.2 parts of deionized water, 3.0 parts of a 25% aqueous solution of an anionic emulsifier [ADEKA CORPORATION, product name: Adeka Reasoap SR-20], 7.3 parts of MMA, 7.5 parts of EHA, 4.5 parts of CHMA, 0.5 parts of a hindered amine light stabilizer [ADEKA CORPORATION, product name: Adeka STAB LA-87], 0.3 parts of HEMA, 0.7 parts of an ultraviolet absorbing monomer [Otsuka Chemical Co., Ltd., product name: RUVA-93], and methacrylate were added. A mixture of 0.1 part of diethyloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product number: KMB-503), 0.1 part of an ultraviolet absorber (manufactured by BASF, product name: Tinuvin 400) (manufactured by BASF, product name: Tinuvin (registered trademark) 479) 0.1 parts of an ultraviolet absorber (manufactured by BASF, product name: Tinuvin (registered trademark) 970) and 0.1 part of an oil-soluble chromium complex black dye was added dropwise to a reaction vessel over a period of 90 minutes with stirring.
[0456] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle obtained in Example 37. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 32.0% by mass.
[0457] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 69 nm.
[0458] Example 60 A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping funnel was charged with 32.6 parts of the aqueous dispersion containing the polymer emulsion particles obtained in Example 38 and 28.0 parts of deionized water, and the reaction vessel was heated with stirring using a water bath until the internal temperature reached 80°C.
[0459] While maintaining the internal temperature at 80°C, 1.8 parts of a 3.5% aqueous solution of ammonium persulfate was added to the reaction vessel, and the mixture was stirred for 10 minutes. Thereafter, while maintaining the internal temperature at 80°C, 13.2 parts of deionized water, 3.0 parts of a 25% aqueous solution of an anionic emulsifier [manufactured by ADEKA Corporation, product name: Adeka Reasoap SR-20], 7.6 parts of MMA, 7.6 parts of EHA, 4.7 parts of CHMA, 0.5 parts of a hindered amine light stabilizer [manufactured by ADEKA Corporation, product name: Adeka STAB LA-87], 0.8 parts of an ultraviolet absorbing monomer [manufactured by Otsuka Chemical Co., Ltd., product name: RUVA-93], and methacryloyloxypropyltrimethoxysilane [manufactured by Shin-Etsu Chemical Co., Ltd.] were added. A mixture of 0.1 parts of an ultraviolet absorber [manufactured by BASF, product number: KMB-503], 0.1 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 400], 0.1 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 479], 0.1 parts of an ultraviolet absorber [manufactured by BASF, product name: Tinuvin (registered trademark) 970], and 0.1 parts of an oil-soluble ultraviolet absorber [manufactured by ADEKA Corporation, product name: Adeka STAB LA-F70] was added dropwise to a reaction vessel over a period of 90 minutes while stirring.
[0460] After 60 minutes from the end of the dropping, 0.1 parts of 25% aqueous ammonia solution was added to the reaction vessel to neutralize the contents of the reaction vessel. After 30 minutes from the end of the neutralization, the reaction vessel was removed from the water bath, the internal temperature of the reaction vessel was cooled to 40°C or less, and 0.1 parts of a preservative (manufactured by DuPont, product name: KORDEK MLX) was added to the reaction vessel to obtain a polymer emulsion particle-containing aqueous dispersion having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particle obtained in Example 38. The non-volatile content of the polymer emulsion particle-containing aqueous dispersion having a resin layer obtained above was 32.0% by mass.
[0461] The average particle size of the polymer emulsion particles contained in the obtained aqueous dispersion containing polymer emulsion particles having a resin layer was measured immediately after production in the same manner as above, and was found to be 67 nm.
[0462] Experimental Example 1 The weather resistance of each of the polymer emulsion particle-containing aqueous dispersions obtained in Example 41, Example 42, Example 43, and Example 44 was evaluated based on the weather resistance evaluation method described below.
[0463] In addition, a polymer emulsion particle-containing aqueous dispersion prepared by mixing 100 parts of an acrylic resin emulsion (manufactured by Nippon Shokubai Co., Ltd., product name: U-DOUBLE EF-015) and 4 parts of an ultraviolet absorber (manufactured by BASF, product name: Tinuvin (registered trademark) 400DW) was used as a conventional polymer emulsion particle-containing aqueous dispersion, and the weather resistance of the polymer emulsion particle-containing aqueous dispersion was evaluated in the same manner as described above.
[0464] [Weather resistance evaluation method 1] A sample was used in which 10 parts of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate (JNC Corporation, product number: CS-12) was added to 100 parts of an acrylic polymer emulsion particle-containing aqueous dispersion (manufactured by Nippon Shokubai Co., Ltd., product name: Acryset EF-005). The sample was applied to a white acrylic resin plate with an applicator so that the coating thickness after drying was 60 μm, and the plate was dried in air at 23 ° C. to obtain a test plate on which a coating film was formed. Each acrylic polymer emulsion particle-containing aqueous dispersion was overcoated with an applicator on the test plate obtained above so that the coating thickness after drying was 20 μm, and the plate was dried in air at 23 ° C. to obtain a test plate on which a coating film was formed. The color difference (L0, a0, b0) of the coating surface of the test plate obtained above was measured with a color difference meter (manufactured by Nippon Denshoku Kogyo Co., Ltd., product name: Spectroscopic color difference meter SE-2000).
[0465] Next, after carrying out an ultraviolet irradiation test for 1200 hours under the following ultraviolet irradiation conditions, the color difference (L1, a1, b1) of the coating surface of the test plate was measured, and the color change (ΔE) before and after the test was calculated using the formula: ΔE = [(L1 - L0) 2 +(a1-a0)2 +(b1-b0) 2 ] 1 / 2 It was obtained based on. As a result, when the polymer emulsion particle-containing aqueous dispersion obtained in Example 41 was used, the color change (ΔE) before and after the test was 0.15, when the polymer emulsion particle-containing aqueous dispersion obtained in Example 42 was used, the color change (ΔE) before and after the test was 0.32, when the polymer emulsion particle-containing aqueous dispersion obtained in Example 43 was used, the color change (ΔE) before and after the test was 0.27, when the polymer emulsion particle-containing aqueous dispersion obtained in Example 44 was used, the color change (ΔE) before and after the test was 0.31, whereas when the conventional polymer emulsion particle-containing aqueous dispersion was used, the color change (ΔE) before and after the test was 0.84. From this, it was confirmed that the polymer emulsion particle-containing aqueous dispersion obtained in each Example was excellent in weather resistance compared to the conventional polymer emulsion particle-containing aqueous dispersion.
[0466] [Ultraviolet irradiation conditions] Ultraviolet rays were irradiated using a super xenon weather meter (manufactured by Suga Test Instruments Co., Ltd., product number: SX2D-75) under test conditions conforming to JIS A6909.
[0467] Experimental Example 2 The polymer emulsion particle-containing aqueous dispersion obtained in Example 45, the polymer emulsion particle-containing aqueous dispersion obtained in Example 46, the polymer emulsion particle-containing aqueous dispersion obtained in Example 47, the polymer emulsion particle-containing aqueous dispersion obtained in Example 48, the polymer emulsion particle-containing aqueous dispersion obtained in Example 49, the polymer emulsion particle-containing aqueous dispersion obtained in Example 50, the polymer emulsion particle-containing aqueous dispersion obtained in Example 51, the polymer emulsion particle-containing aqueous dispersion obtained in Example 52, the polymer emulsion particle-containing aqueous dispersion obtained in Example 53, the polymer emulsion particle-containing aqueous dispersion obtained in Example 54, the polymer emulsion particle-containing aqueous dispersion obtained in Example 55, the polymer emulsion particle-containing aqueous dispersion obtained in Example 56, the polymer emulsion particle-containing aqueous dispersion obtained in Example 57, the polymer emulsion particle-containing aqueous dispersion obtained in Example 58, and the polymer emulsion particle-containing aqueous dispersion obtained in Example 60, were measured for haze based on the following haze measurement method.
[0468] To compare with the polymer emulsion particle-containing aqueous dispersions obtained in each Example, a polymer emulsion particle-containing aqueous dispersion was prepared by adding 1.35 parts of an oil-soluble azo red dye (manufactured by Chuo Synthetic Chemical Industry Co., Ltd., product name: U-DOUBLE EF-015) or 1.35 parts of an oil-soluble chromium complex salt red dye to 100 parts of an acrylic resin emulsion (manufactured by Nippon Shokubai Co., Ltd., product name: U-DOUBLE EF-015). However, in all of the polymer emulsion particle-containing aqueous dispersions, the dye precipitated and did not disperse.
[0469] In addition, a conventional polymer emulsion particle-containing aqueous dispersion was prepared by mixing 3.7 parts of a red pigment aqueous dispersion (manufactured by Sanyo Dye Co., Ltd., product name: EMACOL RED3303) with 100 parts of an acrylic resin emulsion (manufactured by Nippon Shokubai Co., Ltd., product name: U-DOUBLE EF-015). Using the conventional polymer emulsion particle-containing aqueous dispersion obtained above, the haze was measured in the same manner as described above.
[0470] The haze was measured using each polymer emulsion particle-containing aqueous dispersion. As a result, the haze value was 2.1 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 45 was used, 4.3 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 46 was used, 2.3 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 47 was used, 4.7 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 48 was used, and 2.2 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 49 was used. The haze value was 0.4 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 50 was used, 0.8 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 51 was used, 1.2 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 52 was used, 0.7 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 53 was used, 0.9 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 54 was used, 1.3 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 55 was used, 0.6 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 56 was used, 0.9 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 57 was used, 1.2 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 58 was used, and 1.4 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 50 and the polymer emulsion particle-containing aqueous dispersion obtained in Example 60 were used. In contrast, when a conventional aqueous dispersion containing polymer emulsion particles was used, the haze value was 66.7.
[0471] From the above results, it is evident that the polymer emulsion particle-containing aqueous dispersions obtained in the respective Examples have a significantly smaller degree of turbidity than conventional polymer emulsion particle-containing aqueous dispersions.
[0472] [Method of measuring haze] Each aqueous dispersion containing acrylic polymer emulsion particles was applied to a glass plate with an applicator so that the coating thickness after drying would be 60 μm, and then dried in a dryer at 80° C. for 2 hours to form a coating, thereby obtaining a test plate.
[0473] In addition, with regard to Example 60, the acrylic polymer emulsion particle-containing aqueous dispersion of Example 50 was applied to a glass plate with an applicator so that the coating thickness after drying would be 60 μm, and then dried in a dryer at 80° C. for 2 hours, and then the acrylic polymer emulsion particle-containing aqueous dispersion of Example 60 was applied on the coating with an applicator so that the coating thickness after drying would be 60 μm, and then dried in a dryer at 80° C. for 2 hours to form a coating, thereby obtaining a test plate with a multilayer coating film.
[0474] The haze of the coating surface of the test plate obtained above was measured using a spectrophotometer (manufactured by Konica Minolta, Inc., product number: CM-3700A) in accordance with the conditions specified in ASTM-D-1003-97-C.
[0475] Experimental Example 3 Weather resistance was evaluated based on the following weather resistance evaluation method using the polymer emulsion particle-containing aqueous dispersion obtained in Example 50, the polymer emulsion particle-containing aqueous dispersion obtained in Example 52, the polymer emulsion particle-containing aqueous dispersion obtained in Example 56, the polymer emulsion particle-containing aqueous dispersion obtained in Example 57, the polymer emulsion particle-containing aqueous dispersion obtained in Example 58, and the polymer emulsion particle-containing aqueous dispersion obtained in Example 60.
[0476] In addition, a solution of 1.3 parts of oil-soluble chromium complex red dye dissolved in 20 parts of methyl ethyl ketone was added to 100 parts of a conventional solvent-based acrylic resin (manufactured by Nippon Shokubai Co., Ltd., product name: U-DOUBLE S-5115), to obtain an acrylic resin solution in which the red dye was dissolved. In addition, a solution of 0.5 parts of oil-soluble blue dye (manufactured by Kiwa Chemical Industry Co., Ltd., product name: KP Plast Blue R) dissolved in 20 parts of toluene was added to 100 parts of a solvent-based acrylic resin (manufactured by Nippon Shokubai Co., Ltd., product name: U-DOUBLE S-5115), to obtain an acrylic resin solution in which the blue dye was dissolved. These acrylic resin solutions were used to evaluate the weather resistance in the same manner as described above.
[0477] [Weather resistance evaluation method 2] The polymer emulsion particle-containing aqueous dispersion obtained in Example 52, the polymer emulsion particle-containing aqueous dispersion obtained in Example 57, or the acrylic resin solution having a dissolved dye was applied to an aluminum plate (manufactured by Nippon Testpanel Co., Ltd., length: 150 mm, width: 70 mm, thickness: 0.8 mm) with an applicator so that the thickness of the coating film after drying would be 40 μm. The coating film was then dried in a dryer at 80° C. for 2 hours, and an ultraviolet-cut coating agent (manufactured by Nippon Testpanel Co., Ltd.) was applied to each coating film. ) 10 parts of a mixture of HALS Hybrid UV-G101 (manufactured by Nippon Shokubai), 6 parts of toluene, and 2 parts of 6-isocyanatohexylcarbamate 6-[3-(6-isocyanatohexyl)-2,4-dioxo-1,3-diazetidin-1-yl]hexyl were mixed, and within 1 hour of starting mixing, each mixture was applied with an applicator so that the thickness of the coating film after drying would be 40 μm, and the mixture was dried in air at 23°C for 24 hours to form a coating, and a test panel was obtained. Note that in the acrylic resin solution in which the red dye was dissolved, the dye was confirmed to aggregate when dried.
[0478] The polymer emulsion particle-containing aqueous dispersion obtained in Example 56 was applied to an aluminum plate (manufactured by Nippon Test Panel Co., Ltd., length: 150 mm, width: 70 mm, thickness: 0.8 mm) with an applicator so that the coating thickness after drying would be 40 μm, and dried in a dryer at 80° C. for 2 hours to form a coating film, and then the acrylic polymer emulsion particle-containing aqueous dispersion of Example 60 was applied on the coating film with an applicator so that the coating thickness after drying would be 40 μm, and dried in a dryer at 80° C. for 2 hours. After drying, a mixture of 10 parts of an ultraviolet-cutting coating agent (manufactured by Nippon Shokubai Co., Ltd., product name: HALS Hybrid UV-G101), 6 parts of toluene, and 2 parts of 6-isocyanatohexylcarbamate 6-[3-(6-isocyanatohexyl)-2,4-dioxo-1,3-diazetidin-1-yl]hexyl was applied onto the coating with an applicator within 1 hour from the start of mixing so that the coating thickness after drying would be 40 μm, and the coating was dried in air at 23°C for 24 hours to form a coating, and a test panel was obtained.
[0479] The color difference (L0, a0, b0) of the coating surface of the test plate obtained above was measured with a color difference meter (manufactured by Nippon Denshoku Industries Co., Ltd., trade name: Spectroscopic Color Difference Meter SE-2000).
[0480] Next, after irradiating the test plate with ultraviolet light for 504 hours under the following ultraviolet irradiation conditions, the color difference (L1, a1, b1) of the coating surface of the test plate was measured, and the color change (ΔE) due to ultraviolet light irradiation was calculated using the following formula: ΔE = [(L1 - L0) 2 +(a1-a0) 2 +(b1-b0) 2 ] 1 / 2 It was calculated based on the above.
[0481] As a result, the color change (ΔE) was 9.8 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 52 was used, 8.8 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 57 was used, 6.9 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 50 and the polymer emulsion particle-containing aqueous dispersion obtained in Example 58 were used, and 7.2 when the polymer emulsion particle-containing aqueous dispersion obtained in Example 56 and the polymer emulsion particle-containing aqueous dispersion obtained in Example 60 were used. On the other hand, the color change (ΔE) due to irradiation with ultraviolet light was 37.5 when an acrylic resin solution in which a red dye was dissolved was used, and 29 when an acrylic resin solution in which a blue dye was dissolved was used.
[0482] From the above results, it was confirmed that the aqueous dispersions containing polymer emulsion particles obtained in the respective Examples had superior weather resistance compared to the case where a conventional acrylic resin solution was used.
[0483] [Ultraviolet irradiation conditions] Ultraviolet rays were irradiated under the following conditions using a Metaling Weather Meter M6T (trade name) manufactured by Suga Test Instruments Co., Ltd. Cycle: 16 hours light, 6 hours dark Irradiation intensity: 0.50kWh BPT temperature: 63℃ during irradiation Relative humidity: 50% when illuminated, 98% when dark [Industrial Applicability]
[0484] Both the monomer emulsion particle-containing aqueous dispersion and the polymer emulsion particle-containing aqueous dispersion of the present invention are useful for applications such as paints, coatings, inks, pressure sensitive adhesives, adhesives, electronic materials, cosmetics, medicines, heat storage materials, fibers, and civil engineering.
Claims
1. An aqueous dispersion containing monomer emulsion particles comprising a monomer-containing component, the monomer-containing component comprising (A) at least one monomer X selected from the group consisting of n-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate; (B) a nonionic emulsifier, (C) at least one aliphatic organic acid (alkyl ester) selected from the group consisting of aliphatic organic acids having 15 or more carbon atoms and aliphatic organic acid alkyl esters having 18 or more carbon atoms; and (D) at least one lipophilic active ingredient selected from the group consisting of oil-soluble colorants, oil-soluble ultraviolet absorbers, oil-soluble light stabilizers, oil-soluble crosslinking agents, oil-soluble antioxidants, oil-soluble fragrances, oil-soluble insecticides, oil-soluble freshening agents, and oil-soluble deodorants; the aliphatic organic acid (alkyl ester) is at least one selected from the group consisting of organic acid alkyl esters having an alkyl ester moiety with a polymerizable unsaturated double bond and a carbon number of 14 or more, aliphatic organic acid alkyl esters having an alkyl ester moiety with a carbon number of 14 or more, and aliphatic organic acid alkyl esters having an alkyl group with a carbon number of 14 or more, the monomer X contains cyclohexyl (meth)acrylate and / or 2-ethylhexyl (meth)acrylate as an essential component, and the content of monomer X in the monomer-containing component is is 10% by mass or more and 80% by mass or less, the HLB of the nonionic emulsifier is 10 or more and 15 or less, the content of the nonionic emulsifier in the monomer-containing component is 5% by mass or more and 60% by mass or less, the content of the aliphatic organic acid (alkyl ester) in the monomer-containing component is 1% by mass or more and 35% by mass or less, the content of the lipophilic active ingredient in the monomer-containing component is 0.03% by mass or more and 40% by mass or less, and the average particle size of the monomer emulsion particles is 10 to 200 nm.
2. 2. An aqueous dispersion containing polymer emulsion particles, the polymer emulsion particles being obtained by polymerizing a monomer-containing component contained in the monomer emulsion particles according to claim 1, and the polymer emulsion particles having an average particle size of 10 to 200 nm.
3. 3. An aqueous dispersion containing polymer emulsion particles having a resin layer on the surface thereof, the aqueous dispersion containing polymer emulsion particles having a resin layer formed by polymerizing a monomer component for forming a resin layer on the surface of the polymer emulsion particles according to claim 2.
4. The polymer emulsion particle-containing aqueous dispersion according to claim 1, wherein the total content of cyclohexyl (meth)acrylate and 2-ethylhexyl (meth)acrylate in monomer X is 50 to 100 mass %.
5. The polymer emulsion particle-containing aqueous dispersion according to claim 1, which is a polymer emulsion particle-containing aqueous dispersion for use in an aqueous paint.
6. A method for producing an aqueous dispersion containing monomer emulsion particles containing a monomer-containing component, comprising: (A) at least one monomer X selected from the group consisting of alkyl (meth)acrylates having an alkyl group with 4 to 12 carbon atoms and styrene-based monomers; (B) a nonionic emulsifier, (C) at least one aliphatic organic acid (alkyl ester) selected from the group consisting of aliphatic organic acids having 15 or more carbon atoms and aliphatic organic acid alkyl esters having 18 or more carbon atoms; and (D) At least one lipophilic active ingredient selected from the group consisting of an oil-soluble colorant, an oil-soluble ultraviolet absorber, an oil-soluble light stabilizer, an oil-soluble crosslinking agent, an oil-soluble antioxidant, an oil-soluble fragrance, an oil-soluble insecticide, an oil-soluble freshening agent, and an oil-soluble deodorant, wherein cyclohexyl (meth)acrylate and / or 2-ethylhexyl (meth)acrylate is used as an essential component in the monomer X, the content of monomer X in the monomer-containing component is 10% by mass or more and 80% by mass or less, the HLB of the nonionic emulsifier is 10 or more and 15 or less, and the nonionic emulsifier in the monomer-containing component is 0.01 to 0.01% by mass. a content of the aliphatic organic acid (alkyl ester) in the monomer-containing component being 5% by mass or more and 60% by mass or less, a content of the aliphatic organic acid (alkyl ester) in the monomer-containing component being 1% by mass or more and 35% by mass or less, and a content of the lipophilic active ingredient in the monomer-containing component being 0.03% by mass or more and 40% by mass or less, mixing the monomer-containing component with an aqueous medium, heating the resulting mixture under stirring to a temperature that is equal to or higher than the phase inversion onset temperature of the mixture and lower than the boiling point of the aqueous medium, and then cooling the mixture to a temperature that is lower than the phase inversion onset temperature of the mixture.
7. The method for producing an aqueous dispersion containing monomer emulsion particles according to claim 6, wherein monomer X is at least one monomer selected from the group consisting of n-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate.
8. The method for producing an aqueous dispersion containing monomer emulsion particles according to claim 6, wherein the total content of cyclohexyl (meth)acrylate and 2-ethylhexyl (meth)acrylate in monomer X is 50 to 100 mass %.
9. A method for producing a polymer emulsion particle-containing aqueous dispersion as described in claim 6, wherein the polymer emulsion particle-containing aqueous dispersion is a polymer emulsion particle-containing aqueous dispersion for use in an aqueous paint.
Citation Information
Patent Citations
Aqueous dispersion-type resin composition and its production
JP1999116850A
Method for producing a dye-containing aqueous polymer dispersion
JP2002502893A
Aqueous colored fine resin particle dispersion, method for producing the same, colored fine resin particle, method for producing the same, ink, recording unit, ink cartridge, ink-jet recording device and ink-jet recording method
JP2003012709A
Curable water-base resin composition
JP2006045452A
Emulsion, process for its production and water-based paint composition using the emulsion
JP2007270017A