Toner for developing electrostatic images
The electrostatic image developing toner, composed of an amorphous polyester resin and quaternary ammonium salt compound, addresses charging stability issues by enhancing compatibility and dispersibility, resulting in improved charging stability and low-temperature fixability.
Patent Information
- Application Number
- JP2024070851
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-04-24
AI Technical Summary
Toner containing quaternary ammonium salt compounds experiences poor charging stability due to poor compatibility with amorphous polyester resins, leading to dispersion issues.
An electrostatic image developing toner is formulated with an amorphous polyester resin A, which is a polycondensation product of an alcohol component, a carboxylic acid component, and polyethylene terephthalate (PET), and a quaternary ammonium salt compound, with a specific content range of 3 to 30 parts by mass, to enhance compatibility and stability.
The toner exhibits improved charging stability and low-temperature fixability, with reduced conductive paths and enhanced dispersibility of the quaternary ammonium salt compound within the resin.
Smart Images

Figure 0007595798000001 
Figure 0007595798000002 
Figure 0007595798000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a toner for developing electrostatic images used in developing latent images formed in electrophotography, electrostatic recording, electrostatic printing, and the like. [Background technology]
[0002] Toner containing a polyester resin using highly reactive polyethylene terephthalate as a binder resin for the toner has been investigated.
[0003] Patent Document 1 discloses a toner for developing electrostatic images, which comprises a binder resin and a colorant, wherein the binder resin comprises two types of resins whose softening points differ by 10°C or more, and the resin with the lower softening point is a polyester obtained by reacting polyethylene terephthalate or modified polyethylene terephthalate with an alcohol component and a carboxylic acid component, or a hybrid resin having the polyester as one of its resin components. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2004-280085 Summary of the Invention [Problem to be solved by the invention]
[0005] On the other hand, quaternary ammonium salt compounds have high positive charging properties, but have a problem with charging stability.
[0006] The present invention relates to a toner for developing electrostatic images, which has excellent charging stability. [Means for solving the problem]
[0007] The present invention relates to a toner for developing electrostatic images, which contains an amorphous polyester resin A and a quaternary ammonium salt compound X, wherein the amorphous polyester resin A is a polycondensate of an alcohol component, a carboxylic acid component, and polyethylene terephthalate, and the content of the quaternary ammonium salt compound X is 3 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the amorphous polyester resin A. [Effects of the Invention]
[0008] The toner for developing electrostatic images of the present invention exhibits excellent effects in terms of charge stability. DETAILED DESCRIPTION OF THE INVENTION
[0009] The electrostatic image developing toner of the present invention is significantly characterized in that it contains an amorphous polyester resin A, which is a polycondensate of an alcohol component, a carboxylic acid component, and polyethylene terephthalate (PET), and a quaternary ammonium salt compound X. The reason why the electrostatic image developing toner of the present invention has excellent charge stability is not clear, but is presumed to be as follows.
[0010] Because quaternary ammonium salt compounds are cationic, they are incompatible with amorphous polyester resins, making them difficult to disperse in the resin, resulting in problems with charge stability. In response to this, the present invention has discovered that the use of a polycondensation product (amorphous polyester resin A) of an alcohol component, a carboxylic acid component, and PET improves the charge stability of toners. This is believed to be due to the fact that the ester groups sandwiching the PET-derived ethylene glycol moiety in amorphous polyester resin A readily interact with the cationic moiety of the quaternary ammonium salt compound. Furthermore, during the polycondensation reaction of the alcohol component, the carboxylic acid component, and polyethylene phthalate, PET undergoes depolymerization and is incorporated into the polyester resin chain via a transesterification reaction, but is not completely randomized. It exists in amorphous polyester resin A as a unit of a certain length that can be called a polyethylene terephthalate component. This enhances the interaction with the quaternary ammonium salt compound, improving the dispersibility of the quaternary ammonium salt compound in the amorphous polyester resin, thereby reducing the number of conductive paths and improving charge stability.
[0011] Amorphous polyester resin A is a polycondensation product of an alcohol component, a carboxylic acid component, and PET.
[0012] As the alcohol component, from the viewpoint of low temperature fixability, a compound represented by the formula (I):
[0013] [ka]
[0014] (In the formula, OR 1 and R 1 O is an oxyalkylene group, and R 1 is an ethylene group and / or a propylene group, x and y are each a positive number and represent the average number of moles of alkylene oxide added, and the sum of x and y is 1 or more, preferably 1.5 or more, and 16 or less, preferably 8 or less, more preferably 6 or less, and even more preferably 4 or less. Preferred are compounds represented by the following formula (I): Examples of alkylene oxide adducts of bisphenol A represented by formula (I) include polyoxypropylene adducts of 2,2-bis(4-hydroxyphenyl)propane, polyoxyethylene adducts of 2,2-bis(4-hydroxyphenyl)propane, etc. It is preferred to use one or more of these.
[0015] The content of the alkylene oxide adduct of bisphenol A represented by formula (I) in the alcohol component is preferably 80 mol % or more, more preferably 90 mol % or more, even more preferably 95 mol % or more, and still more preferably 100 mol %.
[0016] Examples of other alcohol components include aliphatic diols and trihydric or higher alcohols.
[0017] Examples of the aliphatic diol include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-butenediol, 1,3-butanediol, and neopentyl glycol.
[0018] Examples of the trihydric or higher alcohol include glycerin, trimethylolpropane, and pentaerythritol.
[0019] From the viewpoint of charging stability, the carboxylic acid component preferably contains an aromatic dicarboxylic acid compound.
[0020] Examples of aromatic dicarboxylic acid compounds include phthalic acid, isophthalic acid, terephthalic acid, anhydrides of these acids, and alkyl esters of these acids having 1 to 3 carbon atoms.
[0021] The content of the aromatic dicarboxylic acid compound in the carboxylic acid component is preferably 60 mol % or more, more preferably 70 mol % or more, and even more preferably 80 mol % or more. The carboxylic acid component also includes terephthalic acid units contained in PET.
[0022] Examples of other carboxylic acid components include aliphatic dicarboxylic acid compounds and trivalent or higher carboxylic acid compounds.
[0023] Examples of the aliphatic dicarboxylic acid compound include fumaric acid, maleic acid, succinic acid, succinic acid derivatives substituted with a hydrocarbon group, glutaric acid, adipic acid, sebacic acid, anhydrides of these acids, and alkyl esters of these acids having 1 to 3 carbon atoms.
[0024] Specific examples of succinic acid derivatives substituted with a hydrocarbon group include dodecylsuccinic acid, dodecenylsuccinic acid, tetrapropenylsuccinic acid, decenylsuccinic acid, acid anhydrides thereof, and alkyl esters thereof having 1 to 3 carbon atoms. Among these, from the viewpoint of low-temperature fixability, dodecenylsuccinic acid, tetrapropenylsuccinic acid, and acid anhydrides thereof are preferred, and dodecenylsuccinic anhydride is more preferred.
[0025] From the viewpoint of hydrophobicity, the number of carbon atoms in the hydrocarbon group in the succinic acid derivative is preferably 8 or more, more preferably 10 or more, even more preferably 12 or more, and preferably 20 or less, more preferably 18 or less, even more preferably 16 or less.
[0026] Examples of trivalent or higher carboxylic acid compounds include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, pyromellitic acid, anhydrides of these acids, and alkyl esters in which the alkyl group has 1 to 3 carbon atoms, and among these, trimellitic acid compounds are preferred.
[0027] The raw material monomers may contain trivalent or higher valent monomers (trivalent or higher valent alcohols and / or trivalent or higher carboxylic acid compounds) from the viewpoint of adjusting the softening point.
[0028] The content of trivalent or higher polyvalent monomers is preferably 1 mol% or more, more preferably 3 mol% or more, and preferably 20 mol% or less, more preferably 15 mol% or less, of the total amount of alcohol components and carboxylic acid components. The alcohol components and carboxylic acid components also include ethylene glycol units and terephthalic acid units contained in PET.
[0029] The alcohol component may contain a monohydric alcohol, and the carboxylic acid component may contain a monocarboxylic acid compound, as appropriate.
[0030] In this specification, macromonomers and hydroxycarboxylic acids are not included in the alcohol component and carboxylic acid component.
[0031] PET is produced by the polycondensation reaction of an alcohol component and a carboxylic acid component, and / or by the depolymerization of a portion of PET. The resulting ethylene glycol and terephthalic acid are then used as raw monomers in the polycondensation reaction and incorporated into polyester resin. PET is an equimolar polycondensation product of ethylene glycol and terephthalic acid, with the ethylene glycol and terephthalic acid constituting PET considered to be the alcohol component and the carboxylic acid component, respectively.
[0032] The PET may be new virgin PET or recycled PET. Recycled PET is made by collecting used PET, washing it as necessary, separating it from other materials, and then crushing it. The crushed material is then depolymerized to break it down into monomer units, which are then used as raw materials for resynthesis.
[0033] In the present invention, the PET preferably has a relatively low IV value, i.e., a low molecular weight, compared to conventionally used PET. By introducing a low IV value (low molecular weight) PET into the polyester resin, depolymerization of the PET proceeds more uniformly.
[0034] From the above viewpoints, the IV value of PET is preferably 0.40 or more, more preferably 0.45 or more, even more preferably 0.50 or more, and even more preferably 0.55 or more. From the viewpoints of low-temperature fixability and uniform depolymerization, it is preferably 0.85 or less, more preferably 0.80 or less, even more preferably 0.75 or less, even more preferably 0.70 or less, and even more preferably 0.65 or less. The IV value is an intrinsic viscosity and serves as an index of molecular weight. The IV value of PET can be adjusted by the polycondensation time, etc.
[0035] Commercially available PET products with an IV value of 0.40 or more and 0.85 or less include RAMAPET L1 (manufactured by Indorama Ventures, IV value: 0.60), RAMAPET BF3067 (manufactured by Indorama Ventures, IV value: 0.65), RAMAPET N2G (manufactured by Indorama Ventures, IV value: 0.75), TRN-NTJ (manufactured by Teijin Limited, IV value: 0.53), TRN-RTJC (manufactured by Teijin Limited, IV value: 0.64), RAMAPET S1 (manufactured by Indorama Ventures, IV value: 0.84), and UK-31 (manufactured by Utsumi Recycle Systems Co., Ltd., IV value: 0.67).
[0036] The content of the low IV PET in the total amount of PET used in polycondensation is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and still more preferably 100% by mass.
[0037] From the viewpoint of fixability, the PET content is preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 20 mol% or more, and is preferably 75 mol% or less, more preferably 50 mol% or less, and even more preferably 40 mol% or less, of the total amount of the alcohol component, the carboxylic acid component, and the PET. When the amorphous polyester resin A is composed of two or more resins, the weighted average of the PET contents of the respective resins is taken as the PET content of the amorphous polyester resin A. Since PET is an equimolar polycondensation product of ethylene glycol, terephthalic acid, dimethyl terephthalate, etc., the terephthalic acid-ethylene glycol unit (Mw: 192) is considered to be 1 mole. Therefore, the number of moles of PET = the number of moles of ethylene glycol units = the number of moles of terephthalic acid units.
[0038] The equivalent ratio (COOH groups / OH groups) of the carboxylic acid component (including the terephthalic acid units in the PET) to the alcohol component (including the ethylene glycol units in the PET) is preferably 0.6 or more, more preferably 0.7 or more, even more preferably 0.75 or more, and is preferably 1.2 or less, more preferably 1.15 or less.
[0039] The amorphous polyester resin A can be produced, for example, by polycondensing an alcohol component and a carboxylic acid component in an inert gas atmosphere, preferably in the presence of an esterification catalyst, and optionally in the presence of an esterification promoter, a polymerization inhibitor, etc., at a temperature of preferably 160°C or higher, more preferably 200°C or higher, and preferably 250°C or lower, more preferably 240°C or lower.
[0040] Examples of esterification catalysts include tin compounds such as dibutyltin oxide and tin(II) 2-ethylhexanoate, and titanium compounds such as titanium diisopropoxybis(triethanolaminate) and titanium dihydroxybis(triethanolaminate). The amount of the esterification catalyst used is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and preferably 1.5 parts by mass or less, more preferably 1 part by mass or less, per 100 parts by mass of the alcohol component and the carboxylic acid component combined. Examples of esterification promoters include gallic acid. The amount of the esterification promoter used is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, and preferably 0.5 parts by mass or less, more preferably 0.1 parts by mass or less, per 100 parts by mass of the alcohol component and the carboxylic acid component combined. Examples of polymerization inhibitors include tert-butylcatechol. The amount of the polymerization inhibitor used is preferably 0.001 part by mass or more, more preferably 0.01 part by mass or more, and preferably 0.5 part by mass or less, more preferably 0.1 part by mass or less, per 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component.
[0041] In the present invention, the polyester resin may be modified to such an extent that its properties are not substantially impaired. Examples of modified polyester resins include polyester resins grafted or blocked with phenol, urethane, epoxy, or the like, by the methods described in JP-A Nos. 11-133668, 10-239903, and 8-20636. Among the modified polyester resins, urethane-modified polyester resins in which polyester resins are urethane-extended with a polyisocyanate compound are preferred.
[0042] The softening point of the amorphous polyester resin A is preferably 70°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher from the viewpoint of charging stability, and is preferably 170°C or lower, more preferably 160°C or lower, and even more preferably 150°C or lower from the viewpoint of low-temperature fixability.
[0043] The crystallinity of a resin is expressed by a crystallinity index defined as the ratio of the softening point to the maximum endothermic peak temperature measured by a differential scanning calorimeter, that is, the value of [softening point / maximum endothermic peak temperature]. An amorphous resin is a resin in which no endothermic peak is observed, or if an endothermic peak is observed, the crystallinity index is greater than 1.4, preferably greater than 1.5, more preferably 1.6 or greater, or less than 0.6, preferably 0.5 or less. On the other hand, the crystalline resin is a resin having a crystallinity index of 0.6 or more, preferably 0.7 or more, more preferably 0.9 or more, and 1.4 or less, preferably 1.2 or less, more preferably 1.1 or less. The crystallinity of a resin can be adjusted by the types and ratios of raw material monomers, and production conditions (e.g., reaction temperature, reaction time, cooling rate), etc. The maximum endothermic peak temperature refers to the temperature of the peak with the largest peak area among the observed endothermic peaks. For crystalline resins, the maximum endothermic peak temperature is the melting point.
[0044] From the viewpoint of low-temperature fixability and fixation width, the amorphous polyester resin A may be composed of resins with different softening points. The difference in softening point between the two resins is preferably 10°C or more, more preferably 20°C or more, and is preferably 60°C or less, more preferably 40°C or less.
[0045] The softening point of the amorphous resin with the higher softening point (resin AH) is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 120°C or higher, from the viewpoint of fixing width, and is preferably 170°C or lower, more preferably 160°C or lower, and even more preferably 150°C or lower, from the viewpoint of low-temperature fixability.
[0046] Furthermore, the softening point of the amorphous resin having the lower softening point (resin AL) is preferably 70°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher, from the viewpoint of charging stability, and is preferably 130°C or lower, more preferably 125°C or lower, and even more preferably 120°C or lower, from the viewpoint of low-temperature fixability.
[0047] The mass ratio of resin AH to resin AL (resin AH / resin AL) is preferably 10 / 90 or more, more preferably 20 / 80 or more, even more preferably 30 / 70 or more, and is preferably 90 / 10 or less, more preferably 80 / 20 or less, even more preferably 75 / 25 or less.
[0048] The glass transition temperature of the amorphous polyester resin A is preferably 40°C or higher, more preferably 50°C or higher, from the viewpoint of charging stability, and is preferably 80°C or lower, more preferably 70°C or lower, from the viewpoint of low-temperature fixability.
[0049] The acid value of the amorphous polyester resin A is preferably 1 mgKOH / g or more, more preferably 3 mgKOH / g or more, from the viewpoint of low-temperature fixability, and is preferably 20 mgKOH / g or less, more preferably 18 mgKOH / g or less, from the viewpoint of charging stability.
[0050] In the toner, the amorphous polyester resin A is contained as a binder resin.
[0051] The content of the amorphous polyester resin A in the binder resin is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 100% by mass.
[0052] The content of the binder resin in the toner is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and is preferably less than 100% by mass, more preferably 98% by mass or less, even more preferably 95% by mass or less.
[0053] As the quaternary ammonium salt compound X, from the viewpoint of charging stability, a quaternary ammonium salt-containing resin, which is a polymeric quaternary ammonium salt compound, is preferred, and a quaternary ammonium salt-containing styrene-based resin is more preferred.
[0054] The quaternary ammonium salt-containing styrene-based resin is not particularly limited, but is preferably, for example, a copolymer of a styrene monomer (M1) and / or a (meth)acrylic acid alkyl ester monomer (M2) and a quaternary ammonium salt of a dialkylaminoalkyl (meth)acrylate monomer (M3).
[0055] The styrene monomer (M1) is styrene, and does not include derivatives of styrene such as α-methylstyrene, p-methylstyrene, and p-chlorostyrene.
[0056] Examples of the (meth)acrylic acid alkyl ester monomer (M2) include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, propyl (meth)acrylate, amyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate. The alkyl group preferably has 4 or more and 12 or less carbon atoms. Of these, butyl (meth)acrylate or 2-ethylhexyl (meth)acrylate is preferred, with butyl (meth)acrylate being more preferred.
[0057] Examples of the quaternary ammonium salt of a dialkylaminoalkyl (meth)acrylate monomer (M3) include those represented by the formula (II):
[0058] [ka]
[0059] (In the formula, R 2 is a hydrogen atom or a methyl group, R 3 is an alkylene group having 1 to 5 carbon atoms, R 4 ~R 6 each independently represents an alkyl group having 1 to 5 carbon atoms. A compound represented by the following formula is preferred.
[0060] In formula (II), R 2 As R, a methyl group is preferred.3 Examples of R include a methylene group, an ethylene group, a propylene group, and a butylene group, and among these, an ethylene group is preferred. 4 ~R 6 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an n-butyl group, a tert-butyl group, and the like, and among these, a methyl group or an ethyl group is preferred.
[0061] Examples of dialkylaminoalkyl (meth)acrylates include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dipropylaminoethyl (meth)acrylate, and dibutylaminoethyl (meth)acrylate. Among these, diethylaminoethyl (meth)acrylate is preferred because it is inexpensive.
[0062] Examples of methods for producing a quaternary ammonium salt-containing styrene-based resin include a method in which a dialkylaminoalkyl (meth)acrylate is quaternized using a paratoluenesulfonic acid alkyl ester in a conventional manner to form a quaternary ammonium salt of a dialkylaminoalkyl (meth)acrylate monomer (M3), which is then mixed with a styrene monomer (M1) and / or a (meth)acrylic acid alkyl ester monomer (M2), and copolymerized in the presence of a polymerization initiator.
[0063] Examples of alkyl paratoluenesulfonate include methyl paratoluenesulfonate, ethyl paratoluenesulfonate, and propyl paratoluenesulfonate. Among these, methyl paratoluenesulfonate is preferred because it can be easily quaternized.
[0064] The amount of the alkyl paratoluenesulfonate used is preferably 0.8 moles or more, more preferably 1 mole or more, and preferably 1.5 moles or less, more preferably 1.2 moles or less, per mole of the dialkylaminoalkyl (meth)acrylate to be reacted with it.
[0065] As the copolymerization method, any method such as solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. may be used, but solution polymerization is preferred because it is relatively easy to control the molecular weight of the resulting copolymer and the reaction operation is easy.
[0066] Examples of the solvent used in the solution polymerization include ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone, alcohol solvents such as normal butanol and isobutanol, ester solvents such as ethyl acetate and isobutyl acetate, and aromatic hydrocarbon solvents such as toluene and xylene. Among these, ketone solvents or alcohol solvents are preferred from the viewpoint of the solubility of the copolymer.
[0067] As the polymerization initiator, peroxide initiators such as tert-butylperoxy-2-ethylhexanoate, tert-amylperoxy-2-ethylhexanoate, 1,1-di(tert-butylperoxy)cyclohexane and dibenzoyl peroxide, and azo initiators such as 2,2'-azobis(2-methylbutyronitrile) can be used.
[0068] The amount of the polymerization initiator used is preferably 0.5 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the total of the monomers.
[0069] In the quaternary ammonium salt-containing styrene-based resin, the content of styrene monomer (M1) units in the total amount of styrene monomer (M1) units, (meth)acrylic acid alkyl ester monomer (M2) units, and dialkylaminoalkyl (meth)acrylate quaternary ammonium salt (M3) units is preferably 40 mass% or more, more preferably 50 mass% or more, and preferably 80 mass% or less, more preferably 75 mass% or less.
[0070] In the quaternary ammonium salt-containing styrene-based resin, the content of (meth)acrylic acid alkyl ester monomer (M2) units in the total amount of styrene monomer (M1) units, (meth)acrylic acid alkyl ester monomer (M2) units, and dialkylaminoalkyl (meth)acrylate quaternary ammonium salt (M3) units is preferably 5 mass% or more, more preferably 10 mass% or more, and preferably 40 mass% or less, more preferably 35 mass% or less.
[0071] In the quaternary ammonium salt-containing styrene-based resin, the content of the quaternary ammonium salt (M3) units of dialkylaminoalkyl (meth)acrylate in the total amount of the styrene monomer (M1) units, the (meth)acrylic acid alkyl ester monomer (M2) units, and the quaternary ammonium salt (M3) units of dialkylaminoalkyl (meth)acrylate is preferably 0.5 mass% or more, more preferably 1 mass% or more, and is preferably 35 mass% or less, more preferably 30 mass% or less.
[0072] Commercially available products of the quaternary ammonium salt group-containing styrene resin include, for example, "FCA-201-PS" and "FCA-701-PT" (both manufactured by Fujikura Kasei Co., Ltd.).
[0073] The softening point of the quaternary ammonium salt-containing styrene resin is preferably 140°C or lower, more preferably 135°C or lower, and even more preferably 130°C or lower, from the viewpoint of improving the grindability of the toner to obtain small toner particles and from the viewpoint of low-temperature fixability, and is preferably 90°C or higher, more preferably 95°C or higher, and even more preferably 100°C or higher, from the viewpoint of storage stability.
[0074] The glass transition temperature of the quaternary ammonium salt-containing styrene resin is preferably 90°C or lower, more preferably 85°C or lower, and even more preferably 80°C or lower, from the viewpoint of improving the grindability of the toner to obtain small toner particles and from the viewpoint of low-temperature fixability, and is preferably 35°C or higher, more preferably 40°C or higher, and even more preferably 45°C or higher, from the viewpoint of storage stability.
[0075] Other quaternary ammonium salt compounds X include, for example, compounds of the formula (III):
[0076] [ka]
[0077] (In the formula, R 7 ~R 9 are each independently an alkyl group having 1 to 5 carbon atoms, R 10 represents an alkylene group having 1 to 5 carbon atoms. Examples of commercially available quaternary ammonium salt compounds represented by formula (III) include "Bontron P-51" (manufactured by Orient Chemical Industries, Ltd., R 7 ~R 9 : butyl group, R 10 : methylene group).
[0078] The content of the quaternary ammonium salt compound X is 3 parts by mass or more, preferably 5 parts by mass or more, and more preferably 8 parts by mass or more, relative to 100 parts by mass of the amorphous polyester resin A, from the viewpoint of charging stability, and 30 parts by mass or less, preferably 25 parts by mass or less, and more preferably 20 parts by mass or less, from the viewpoint of dispersibility in the binder resin.
[0079] The toner of the present invention may contain other charge control agents within the range that does not impair the effects of the present invention.
[0080] The toner of the present invention may contain additives such as a colorant, a release agent, a charge control agent, a magnetic powder, a flowability improver, a conductivity adjuster, a reinforcing filler such as a fibrous substance, an antioxidant, and a cleaning property improver, in addition to the binder resin and the quaternary ammonium salt compound X.
[0081] As the colorant, dyes, pigments, magnetic materials, etc. used as toner colorants can be used. Examples include carbon black, phthalocyanine blue, permanent brown FG, brilliant fast scarlet, pigment red 122, pigment green B, rhodamine-B base, solvent red 49, solvent red 146, solvent blue 35, quinacridone, carmine 6B, isoindoline, disazo yellow, etc. In the present invention, the toner may be either a black toner or a color toner.
[0082] From the viewpoint of improving the image density and low-temperature fixability of the toner, the content of the colorant is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and preferably 40 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the binder resin.
[0083] Examples of the release agent include hydrocarbon waxes such as polypropylene wax, polyethylene wax, ethylene-propylene copolymer wax, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax, and oxides thereof; ester waxes such as carnauba wax, montan wax, and deacidified waxes thereof, and fatty acid ester wax; fatty acid amides, fatty acids, higher alcohols, and fatty acid metal salts, and these may be used alone or in combination of two or more.
[0084] The melting point of the release agent is preferably 60°C or higher, more preferably 70°C or higher, from the viewpoint of charge stability, and is preferably 160°C or lower, more preferably 140°C or lower, even more preferably 120°C or lower, and even more preferably 110°C or lower, from the viewpoint of low-temperature fixability.
[0085] The content of the release agent is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 1.5 parts by mass or more, relative to 100 parts by mass of the binder resin, from the viewpoints of the low-temperature fixability and charge stability of the toner and the dispersibility in the binder resin, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 7 parts by mass or less.
[0086] The toner may be a toner obtained by any conventionally known method such as a melt-kneading method, an emulsion aggregation method, or a suspension polymerization method, and may also be a toner having a core-shell structure, but from the viewpoint of charge stability, a pulverized toner obtained by a melt-kneading method is preferred. In the case of a pulverized toner obtained by a melt-kneading method, for example, raw materials such as a binder resin containing an amorphous polyester resin A, a quaternary ammonium salt compound X, and, if necessary, a colorant, a release agent, and a charge control agent are uniformly mixed in a mixer such as a Henschel mixer, and then melt-kneaded in an internal kneader, a single-screw or twin-screw extruder, an open-roll kneader, or the like, followed by cooling, pulverization, and classification to produce the toner.
[0087] In order to improve the transferability of the toner of the present invention, it is preferable to use an external additive. Examples of the external additive include inorganic fine particles such as silica, alumina, titania, zirconia, tin oxide, and zinc oxide, and organic fine particles such as melamine-based resin fine particles and polytetrafluoroethylene resin fine particles, and two or more of these may be used in combination. Among these, silica is preferred, and from the viewpoint of the transferability of the toner, hydrophobic silica that has been subjected to a hydrophobic treatment is more preferred.
[0088] Examples of hydrophobic treatment agents for hydrophobizing the surfaces of silica particles include hexamethyldisilazane (HMDS), dimethyldichlorosilane (DMDS), cyclic silazanes, silicone oils, aminosilanes, octyltriethoxysilane (OTES), and methyltriethoxysilane.
[0089] From the viewpoint of the chargeability, fluidity, and transferability of the toner, the average particle diameter of the external additive is preferably 5 nm or more, more preferably 10 nm or more, and even more preferably 15 nm or more, and is preferably 250 nm or less, more preferably 200 nm or less, and even more preferably 90 nm or less.
[0090] The external addition treatment by mixing the toner particles with the external additives can be carried out in accordance with a conventional method, and a mixer such as a Henschel mixer can be used.
[0091] From the viewpoint of the chargeability, fluidity, and transferability of the toner, the content of the external additive is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.3 parts by mass or more, relative to 100 parts by mass of the toner particles before treatment with the external additive, and is preferably 5 parts by mass or less, and more preferably 3 parts by mass or less.
[0092] The volume median particle size (D 50 ) is preferably 3 μm or more, more preferably 4 μm or more, and is preferably 15 μm or less, more preferably 10 μm or less. 50 ) means the particle size at which the cumulative volume frequency calculated by volume fraction is 50% starting from the smallest particle size. In addition, when the toner is treated with an external additive, the volume median particle size of the toner particles before treatment with the external additive is taken as the volume median particle size of the toner.
[0093] The toner of the present invention can be used as a toner for one-component development as it is, or as a toner for two-component development mixed with a carrier, in an image forming apparatus of a one-component development system or a two-component development system, respectively. [Example]
[0094] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Physical properties of resins and the like can be measured by the following methods.
[0095] [PET IV value] The sample is dissolved in a mixed solvent of phenol / tetrachloroethane (mass ratio) 60 / 40 at a concentration of 4 g / L, and the viscosity is measured using an Ubbelohde viscometer, and calculated using the following formula. IV=(-1+√(1+4kη)) / (2kC) (where k = 0.33, C = 0.004 g / mL, and η = (t1 / t0)-1 (t0: number of seconds it takes for the solvent alone to fall, t1: number of seconds it takes for the sample solution to fall).)
[0096] [Softening point of resin] Using a flow tester "CFT-500D" (Shimadzu Corporation), 1 g of sample is heated at a temperature increase rate of 6°C / min while applying a load of 1.96 MPa with the plunger, and extruding it from a nozzle 1 mm in diameter and 1 mm in length. The plunger depression distance of the flow tester is plotted against the temperature, and the temperature at which half of the sample flows out is taken as the softening point.
[0097] [Maximum endothermic peak temperature of resin] Using a differential scanning calorimeter "Q-100" (TA Instruments Japan Co., Ltd.), weigh 0.01-0.02 g of sample into an aluminum pan, cool from room temperature (25°C) to 0°C at a rate of 10°C / min, and maintain at 0°C for 1 minute. Then, measure at a rate of 10°C / min. The temperature of the peak with the largest peak area among the observed endothermic peaks is taken as the maximum endothermic peak temperature. For crystalline resins, the maximum endothermic peak temperature is taken as the melting point.
[0098] [Glass transition temperature of resin] Using a differential scanning calorimeter "Q-100" (TA Instruments Japan), 0.01-0.02 g of sample is weighed into an aluminum pan, heated to 200°C, and cooled to 0°C at a rate of 10°C / min. The sample is then heated at a rate of 10°C / min, and the endothermic peak is measured. The glass transition temperature is the temperature at the intersection of an extension of the baseline below the maximum endothermic peak temperature and a tangent line showing the maximum slope from the rising part of the peak to the peak apex.
[0099] [Acid value of resin] Measurement is performed based on the method of JIS K 0070:1992, except that the measurement solvent is changed from the ethanol and ether mixture specified in JIS K 0070 to a mixture of acetone and toluene (acetone:toluene = 1:1 (volume ratio)).
[0100] [Melting point of release agent] Using a differential scanning calorimeter "Q-100" (TA Instruments Japan), 0.02 g of sample is weighed into an aluminum pan, heated to 200°C, and then cooled from 200°C to 0°C at a rate of 10°C / min. The sample is then heated at a rate of 10°C / min, the calorific value is measured, and the maximum endothermic peak temperature is taken as the melting point.
[0101] [Volume Median Particle Size and CV Value of Resin Particles, Quaternary Ammonium Salt Compound Particles, Colorant Particles, and Release Agent Particles] (1) Measuring device: Laser diffraction particle size measuring instrument "LA-920" (manufactured by Horiba, Ltd.) (2) Measurement conditions: Put the sample dispersion in a measurement cell, add distilled water, and measure the volume median particle size (D 50 ) and volume average particle diameter are measured. The CV value is calculated according to the following formula. CV value (%) = (standard deviation of particle size distribution / volume average particle size) x 100
[0102] [Solid Content Concentration of Resin Particle Dispersion, Quaternary Ammonium Salt Compound Particle Dispersion, Colorant Particle Dispersion, and Release Agent Particle Dispersion] Using an infrared moisture meter "FD-230" (Kett Electric Laboratory Co., Ltd.), 5 g of the measurement sample is dried at a drying temperature of 150°C and measurement mode 96 (monitoring time 2.5 minutes, fluctuation range 0.05%), and the moisture content (mass%) of the dispersion is measured. The solid content concentration is calculated according to the following formula. Solid concentration (mass%) = 100-moisture (mass%)
[0103] [Volume Median Particle Diameter of Agglomerated Particles] Measuring instrument: "Coulter Multisizer (registered trademark) III" (manufactured by Beckman Coulter, Inc.) Aperture diameter: 50 μm Analysis software: "Multisizer (registered trademark) III version 3.51" (Beckman Coulter, Inc.) Electrolyte: "Isoton (registered trademark) II" (manufactured by Beckman Coulter, Inc.) Measurement conditions: The sample dispersion is added to 100 mL of the electrolyte to adjust the concentration so that the particle size of 30,000 particles can be measured in 20 seconds. Then, 30,000 particles are measured, and the volume median particle size (D 50 ) is found.
[0104] [Average particle size of external additives] The average particle size refers to the number-average particle size, and is calculated by measuring the particle sizes (average values of major and minor axes) of 500 particles in a scanning electron microscope (SEM) photograph and averaging these values by number.
[0105] [Volume median particle size of toner (D 50 ) Measuring instrument: "Coulter Multisizer (registered trademark) III" (manufactured by Beckman Coulter, Inc.) Aperture diameter: 50 μm Analysis software: "Multisizer (registered trademark) III Version 3.51" (Beckman Coulter, Inc.) Electrolyte: "Isoton (registered trademark) II" (manufactured by Beckman Coulter, Inc.) Dispersion: Polyoxyethylene lauryl ether "Emulgen (registered trademark) 109P" (manufactured by Kao Corporation, HLB (Griffin) = 13.6) dissolved in the electrolyte to adjust the concentration to 5% by mass Dispersion conditions: 10 mg of the measurement sample was added to 5 mL of the dispersion, and the mixture was dispersed for 1 minute using an ultrasonic disperser (machine name: US-1 manufactured by SND Corporation, output: 80 W). 25 mL of electrolyte was then added, and the mixture was further dispersed for 1 minute using the ultrasonic disperser to prepare a sample dispersion. Measurement conditions: The sample dispersion was added to 100 mL of the electrolyte to adjust the concentration so that the particle size of 30,000 particles could be measured in 20 seconds. Then, 30,000 particles were measured, and the volume median particle size (D 50 ) is found.
[0106] [Circularity of Toner] The circularity of the toner particles is measured under the following conditions. Measurement equipment: Flow particle image analyzer "FPIA-3000" (Sysmex Corporation) Preparation of dispersion: A dispersion of toner particles is prepared by diluting it with deionized water so that the solid content concentration is 0.001 to 0.05% by mass. Measurement mode: HPF measurement mode
[0107] Preparation Example 1 of Alkenyl Succinic Anhydride (1) Propylene tetramer (manufactured by Nippon Oil Corporation, trade name: "Light Tetramer") was fractionally distilled at a heating condition of 183 to 208°C to obtain an alkylene compound (a). The obtained alkylene compound (a) had 40 peaks in gas chromatography mass spectrometry, which will be described later. The distribution of the alkylene compound was measured according to the analysis of alkylene compound A by mass spectrometry gas chromatography in JP 2014-013384 A, and the C9H 18 :0.5% by mass, C 10 H 20 :4% by mass, C 11 H 22 :20% by mass, C 12 H 24 :66% by mass, C 13 H 26 :9% by mass, C 14 H 28 : 0.5% by mass (6 peaks corresponding to alkylene compounds having 9 to 14 carbon atoms).
[0108] (2) A 1-liter autoclave manufactured by Nitto Koatsu Co., Ltd. was charged with 542.4 g of alkylene compound (a), 157.2 g of maleic anhydride, 0.4 g of the antioxidant "Cherex-O" (triisooctyl phosphite manufactured by SC Organic Chemical Co., Ltd.), and 0.1 g of butylhydroquinone as a polymerization inhibitor. Pressure and nitrogen substitution (0.2 MPaG) were repeated three times. After stirring was initiated at 60°C, the mixture was heated to 230°C over one hour and reacted for six hours. The pressure at the time the reaction temperature was reached was 0.3 MPaG. After the reaction was completed, the mixture was cooled to 80°C, returned to atmospheric pressure (101.3 kPa), and transferred to a 1-liter four-neck flask. The mixture was heated to 180°C with stirring, and the remaining alkylene compound was distilled off at 1.3 kPa over one hour. Subsequently, the mixture was cooled to room temperature (25°C) and then returned to normal pressure (101.3 kPa) to obtain 406.1 g of the target product, alkenyl succinic anhydride A. The average molecular weight of alkenyl succinic anhydride A calculated from the acid value was 268.
[0109] Resin manufacturing example 1 The alcohol component, carboxylic acid component other than trimellitic anhydride, PET, esterification catalyst, and esterification promoter shown in Tables 1 to 3 were placed in a 10-liter four-neck flask equipped with a nitrogen inlet tube, stirrer, and thermocouple. The mixture was heated to 235°C under a nitrogen atmosphere and then subjected to polycondensation at 235°C for 6 hours. The temperature was then lowered to 210°C, and trimellitic anhydride shown in Tables 1 to 3 was added. The mixture was reacted at 210°C for 1 hour, and then further reacted at 210°C under a reduced pressure of 10 kPa until the softening point shown in Tables 1 to 3 was reached, yielding amorphous polyester resins (resins AH1 to AH5, AH8, and AH11 to AH14). The physical properties are shown in Tables 1 to 3.
[0110] Resin manufacturing example 2 The alcohol component, carboxylic acid component, PET, esterification catalyst, and esterification cocatalyst shown in Tables 2 and 5 were placed in a 10-liter four-neck flask equipped with a nitrogen inlet tube, stirrer, and thermocouple. The mixture was maintained at 180°C for 1 hour under a nitrogen atmosphere, then heated from 180°C to 235°C at a rate of 10°C / h. Polycondensation was then carried out at 235°C for 5 hours. The temperature was then lowered to 210°C, and the reaction was continued under a reduced pressure of 10 kPa until the softening points shown in Tables 2 and 5 were reached, yielding amorphous polyester resins (Resins AH6, AH7, AL6, and AL7). Their physical properties are shown in Tables 2 and 5.
[0111] Resin manufacturing example 3 The alcohol component, carboxylic acid component other than trimellitic anhydride and fumaric acid, PET, esterification catalyst, and esterification co-catalyst shown in Table 2 were placed in a 10-liter four-neck flask equipped with a nitrogen inlet tube, stirrer, and thermocouple. The mixture was heated to 235°C under a nitrogen atmosphere and then polycondensed at 235°C for 6 hours. The temperature was then lowered to 180°C, and trimellitic anhydride, fumaric acid, and polymerization inhibitor shown in Table 2 were added. The mixture was reacted at 180°C for 1 hour. The temperature was then increased from 180°C to 210°C at a rate of 10°C / h, and polycondensed at 210°C for 1 hour. The reaction was then continued at 210°C under a reduced pressure of 10 kPa until the softening point shown in Table 2 was reached, yielding an amorphous polyester resin (Resin AH9). The physical properties are shown in Table 2.
[0112] Resin manufacturing example 4 The alcohol component, carboxylic acid component other than trimellitic anhydride, esterification catalyst, and esterification co-catalyst shown in Table 2 were placed in a 10-liter four-neck flask equipped with a nitrogen inlet tube, stirrer, and thermocouple. The mixture was heated to 235°C under a nitrogen atmosphere and then polycondensed at 235°C for 6 hours. The temperature was then lowered to 210°C, and trimellitic anhydride shown in Table 2 was added. The mixture was reacted at 210°C for 1 hour, and then further reacted at 210°C under a reduced pressure of 10 kPa until the softening point shown in Table 2 was reached, yielding an amorphous polyester resin (Resin AH10). The physical properties are shown in Table 2.
[0113] Resin manufacturing example 5 The alcohol component, carboxylic acid component, PET, esterification catalyst, and esterification co-catalyst shown in Tables 4 to 6 were placed in a 10-liter four-neck flask equipped with a nitrogen inlet tube, stirrer, and thermocouple, and the temperature was raised to 235°C under a nitrogen atmosphere, followed by polycondensation at 235°C for 6 hours. The temperature was then lowered to 210°C, and the reaction was continued under a reduced pressure of 10 kPa until the softening points shown in Tables 4 to 6 were reached, yielding amorphous polyester resins (resins AL1 to AL5, AL8, AL11 to AL14). The physical properties are shown in Tables 4 to 6.
[0114] Resin manufacturing example 6 The alcohol component, carboxylic acid component other than fumaric acid, PET, esterification catalyst, and esterification co-catalyst shown in Table 5 were placed in a 10-liter four-neck flask equipped with a nitrogen inlet tube, stirrer, and thermocouple. The mixture was heated to 235°C under a nitrogen atmosphere and then polycondensed at 235°C for 6 hours. The temperature was then lowered to 180°C, and fumaric acid and a polymerization inhibitor shown in Table 5 were added. The mixture was reacted at 180°C for 1 hour. The temperature was then increased from 180°C to 210°C at a rate of 10°C / h, and polycondensed at 210°C for 1 hour. The reaction was then continued at 210°C under a reduced pressure of 10 kPa until the softening point shown in Table 5 was reached, yielding an amorphous polyester resin (Resin AL9). The physical properties are shown in Table 5.
[0115] Resin manufacturing example 7 The alcohol component, carboxylic acid component, esterification catalyst, and esterification co-catalyst shown in Table 5 were placed in a 10-liter four-neck flask equipped with a nitrogen inlet tube, a stirrer, and a thermocouple, and the temperature was raised to 235°C under a nitrogen atmosphere, followed by polycondensation at 235°C for 6 hours. The temperature was then lowered to 210°C, and the reaction was continued under a reduced pressure of 10 kPa until the softening point shown in Table 5 was reached, yielding an amorphous polyester resin (resin AL10). The physical properties are shown in Table 5.
[0116] [Table 1]
[0117] [Table 2]
[0118] [Table 3]
[0119] [Table 4]
[0120] [Table 5]
[0121] [Table 6]
[0122] Example 1, Examples 5 to 12, Examples 16 to 19, Comparative Example 2 [Melt-kneading method] 100 parts by mass of the binder resin shown in Table 7, 5 parts by mass of colorant "ECB-301" (manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., phthalocyanine blue (PB15:3)), 3 parts by mass of release agent "Carnauba Wax C1" (manufactured by Kato Yoko Co., Ltd., melting point: 83°C), and 10 parts by mass of positively chargeable charge control agent "FCA-201-PS" (manufactured by Fujikura Kasei Co., Ltd., softening point: 119°C, glass transition temperature: 65°C), which is a quaternary ammonium salt-containing styrene-based resin, were mixed in a Henschel mixer.
[0123] The resulting mixture was melt-kneaded using a co-rotating twin-screw extruder with a kneading section total length of 1560 mm, a screw diameter of 42 mm, and a barrel inner diameter of 43 mm at a screw rotation speed of 200 r / min and a barrel temperature setting of 100°C to obtain a melt-kneaded product. The mixture was fed at a rate of 20 kg / h and had an average residence time of approximately 18 seconds.
[0124] The resulting melt-kneaded product was cooled and coarsely crushed, then crushed in a jet mill, and classified using an air classifier (manufactured by Nippon Pneumatic Mfg. Co., Ltd.) to obtain the volume median particle diameter (D 50 ) toner particles of 7.0 μm were obtained.
[0125] 100 parts by mass of the obtained toner particles and 0.5 parts by mass of hydrophobic silica "TG820F" (manufactured by Cabot Corporation, hydrophobic treatment agent: HMDS and cyclic silazane, average particle diameter 8 nm) and 1.0 part by mass of hydrophobic silica "NA50Y" (manufactured by Nippon Aerosil Co., Ltd., hydrophobic treatment agent: silicone oil and aminosilane, average particle diameter 40 nm) as external additives were mixed in a Henschel mixer (manufactured by Nippon Coke and Engineering Co., Ltd.) at a rotation speed of 3000 r / min (circumferential speed 32 m / sec) for 3 minutes to obtain a toner.
[0126] Examples 2 to 4, Comparative Example 1 A toner was obtained in the same manner as in Example 1, except that the amount of the positively chargeable charge control agent ("FCA-201-PS") used was changed to the number of parts shown in Table 7.
[0127] Example 13 A toner was obtained in the same manner as in Example 1, except that 10 parts by mass of "BONTRON P-51" (manufactured by Orient Chemical Industries Co., Ltd.) was used instead of "FCA-201-PS" as the positively charged charge control agent.
[0128] Example 14 A toner was obtained in the same manner as in Example 1, except that a continuous open-roll twin-screw kneader "Kneedex" (manufactured by Nippon Coke and Engineering Co., Ltd.) was used for melt-kneading instead of a co-rotating twin-screw extruder. The continuous open-roll twin-screw kneader had a roll outer diameter of 0.14 m and an effective roll length of 0.8 m. The operating conditions were a rotation speed of the high-speed roll (front roll) of 75 r / min (circumferential speed 33 m / min), a rotation speed of the low-speed roll (rear roll) of 50 r / min (circumferential speed 22 m / min), and a roll gap of 0.1 mm. The heating and cooling medium temperatures within the rolls were set as follows: the temperature on the raw material inlet side of the high-speed roll was 140°C, and the temperature on the kneaded material outlet side was 110°C; and the temperature on the raw material inlet side of the low-speed roll was 65°C, and the temperature on the kneaded material outlet side was 30°C. The raw material mixture was supplied at a rate of 10 kg / h, and the average residence time was approximately 5 minutes.
[0129] Example 15 [Emulsion aggregation method] <Preparation of aqueous dispersion of core resin particles> 600 g of methyl ethyl ketone was placed in a 5-liter vessel equipped with a stirrer, reflux condenser, dropping funnel, thermometer, and nitrogen inlet tube, and 150 g of resin AH1 was added and dissolved at 60°C. A 5% by mass aqueous solution of sodium hydroxide was added to the resulting solution to achieve a neutralization degree of 60 mol% relative to the acid value of the resin, and the mixture was stirred for 30 minutes to obtain a mixture. Subsequently, 675 g of deionized water was added over 77 minutes. Next, while stirring at 250 r / min, methyl ethyl ketone and a portion of the water were distilled off under reduced pressure at a temperature of 50°C or less. The solids concentration of the aqueous dispersion was measured, and the solids concentration of the aqueous dispersion was adjusted to 20% by mass with deionized water to obtain a core resin dispersion. The volume median particle diameter (D 50 ) was 200 nm and the CV value was 24%.
[0130] <Preparation of aqueous dispersion of shell resin particles> 600 g of methyl ethyl ketone was placed in a 5-liter vessel equipped with a stirrer, reflux condenser, dropping funnel, thermometer, and nitrogen inlet tube, and 150 g of resin AL1 was added and dissolved at 60°C. A 5% by mass aqueous solution of sodium hydroxide was added to the resulting solution to achieve a neutralization degree of 60 mol% relative to the acid value of the resin, and the mixture was stirred for 30 minutes to obtain a mixture. Subsequently, 675 g of deionized water was added over 77 minutes. Next, while stirring at 250 r / min, methyl ethyl ketone and a portion of the water were distilled off under reduced pressure at a temperature of 50°C or less. The solids concentration of the aqueous dispersion was measured, and the solids concentration of the aqueous dispersion was adjusted to 20% by mass with deionized water to obtain a shell resin dispersion. The volume median particle diameter (D 50 ) was 110 nm and the CV value was 20%.
[0131] <Preparation of Quaternary Ammonium Salt Compound Dispersion> In a 1-liter beaker, 100.0 g of a positively charged charge control agent (FCA-201-PS, manufactured by Fujikura Kasei Co., Ltd.), a quaternary ammonium salt-containing styrene-based resin, 133.3 g of an anionic surfactant (Neopelex® G-15, manufactured by Kao Corporation, 15% by weight sodium dodecylbenzenesulfonate aqueous solution), and 268.5 g of deionized water were mixed and dispersed at room temperature for 1 hour using a homogenizer (TKAGI HOMOMIXER 2M-03, manufactured by Primix Corporation) at a stirring blade rotation speed of 8000 r / min. The mixture was then passed through a homogenizer (Microfluidizer M-110EH, manufactured by Microfluidics) at a pressure of 150 MPa for 12 passes. The mixture was then passed through a 200-mesh filter, and deionized water was added to obtain a quaternary ammonium salt compound dispersion, with the solids concentration adjusted to 12% by weight. The volume median particle size (D 50 ) was 150 nm and the CV value was 30%.
[0132] <Preparation of Colorant Dispersion> In a 1-liter beaker, 116.2 g of colorant "ECB-301" (Dainichiseika Color & Chemicals Mfg. Co., Ltd., Phthalocyanine Blue (PB15:3)), 154.9 g of anionic surfactant "Neopelex (registered trademark) G-15" (Kao Corporation, 15% by mass sodium dodecylbenzenesulfonate aqueous solution), and 260 g of deionized water were mixed and dispersed using a homogenizer at room temperature for 3 hours, and then deionized water was added to obtain a colorant dispersion so that the solids concentration was 24% by mass. The volume median particle diameter (D 50 ) was 118 nm and the CV value was 27%.
[0133] <Preparation of release agent dispersion> 50 g of Fischer-Tropsch wax (manufactured by Nippon Seiro Co., Ltd., trade name: FNP0090, melting point: 90°C), 5 g of a cationic surfactant (manufactured by Kao Corporation, trade name: Sanisol B50), and 200 g of deionized water were heated to 95°C, and the paraffin wax was dispersed using a homogenizer. The mixture was then dispersed using a pressure discharge homogenizer, and deionized water was added to obtain a release agent dispersion with a solids concentration of 20 mass%. The volume median particle diameter (D 50 ) was measured at 550 nm, and the CV value was 26%.
[0134] <Preparation of Toner Particles> 500 g of the core resin dispersion, 143 g of the quaternary ammonium salt compound dispersion, 36 g of the colorant dispersion, 33 g of the release agent dispersion, and 3.3 g of a 15% by mass aqueous solution of sodium dodecylbenzenesulfonate "Neopelex G-15" (Kao Corporation, an anionic surfactant) were mixed at 25° C. in a 3-liter four-neck flask equipped with a dehydration tube, a stirrer, and a thermocouple. Next, while stirring the resulting mixture, a solution prepared by dissolving 40 g of ammonium sulfate in 570 g of deionized water and adding a 4.8% by mass aqueous solution of potassium hydroxide to adjust the pH to 8.2 was added dropwise over 10 minutes at 25° C., and the temperature was then raised to 62° C. over 2 hours to measure the volume median particle diameter (D 50 The temperature was maintained at 62°C until the particle size reached 6.9 µm, thereby obtaining a dispersion of aggregated particles (I).
[0135] While maintaining the temperature of the resulting dispersion of aggregated particles (I) at 62°C, 215 g of the shell resin dispersion was added dropwise at a rate of 0.6 mL / min (0.6 g / min) to obtain a dispersion of aggregated particles (II). 50 ) was 7.0 μm.
[0136] To the resulting dispersion of aggregated particles (II), an aqueous solution containing 20 g of sodium polyoxyethylene lauryl ether sulfate "EMAL E-27C" (Kao Corporation, an anionic surfactant, effective concentration 27% by mass), 280 g of deionized water, and 40 g of 0.1 mol / L aqueous sulfuric acid solution was added. The mixture was then heated to 80°C over 1 hour and maintained at 80°C for 30 minutes. After that, 10 g of 0.1 mol / L aqueous sulfuric acid solution was added, and the mixture was further maintained at 80°C for 15 minutes. Another 15 g of 0.1 mol / L aqueous sulfuric acid solution was then added, and the mixture was maintained at 80°C until the circularity reached 0.970, thereby obtaining a dispersion of fused particles (core-shell particles) in which the aggregated particles were fused together.
[0137] The resulting core-shell particle dispersion was cooled to 30°C, and the dispersion was suction filtered to separate the solids. The solids were then washed with deionized water at 25°C and suction filtered at 25°C for 2 hours. The resulting particles were then vacuum dried at 33°C for 24 hours using a vacuum constant temperature dryer "DRV622DA" (manufactured by ADVANTEC) to obtain toner particles. The resulting toner particles had a particle size of 7.0 μm and a circularity of 0.970. The composition ratio (mass ratio) of the binder resins in the resulting toner particles was Resin AH1 / Resin AL1 = 70 / 30.
[0138] 100 parts by mass of the obtained toner particles and 0.5 parts by mass of hydrophobic silica "TG820F" (manufactured by Cabot Corporation, hydrophobic treatment agent: HMDS and cyclic silazane, average particle diameter 8 nm) and 1.0 part by mass of hydrophobic silica "NA50Y" (manufactured by Nippon Aerosil Co., Ltd., hydrophobic treatment agent: silicone oil and aminosilane, average particle diameter 40 nm) as external additives were mixed in a Henschel mixer (manufactured by Nippon Coke and Engineering Co., Ltd.) at a rotation speed of 3000 r / min (circumferential speed 32 m / sec) for 3 minutes to obtain a toner.
[0139] Test Example [Charging Stability of Toner] Under conditions of a temperature of 25°C and a relative humidity of 50%, 0.6 g of toner and 19.4 g of silicone ferrite carrier (manufactured by Kanto Denka Kogyo Co., Ltd., average particle size 90 μm) were placed in a 50 mL polyethylene container and mixed using a ball mill at 250 r / min. The charge amount of the toner was measured using a Q / M meter (manufactured by EPPING) using the following method.
[0140] After 60 or 600 seconds of mixing, a specified amount of toner and carrier mixture was placed in a cell attached to the Q / M meter, and the toner alone was suctioned through a 32 μm mesh sieve (stainless steel, twill weave, wire diameter: 0.0035 mm) for 90 seconds. The voltage change on the carrier was monitored, and the value [total charge (μC) after 90 seconds / amount of suctioned toner (g)] was taken as the charge amount (μC / g). The ratio of the charge amount after 60 seconds of mixing to the charge amount after 600 seconds of mixing (charge amount after 60 seconds of mixing / charge amount after 600 seconds of mixing) was calculated to evaluate charge stability. The results are shown in Table 7. A higher value indicates better charge stability.
[0141] [Table 7]
[0142] The above results show that the toners of Examples 1 to 19 have good charge stability compared to Comparative Example 1, which has a low content of quaternary ammonium salt compound, and Comparative Example 2, which contains an amorphous polyester resin without PET. In particular, a comparison between Example 1 and Example 13 shows that the charge stability of the toner is further improved by including a polymeric quaternary ammonium salt compound. [Industrial Applicability]
[0143] The toner for developing electrostatic images of the present invention is suitably used for developing latent images formed in electrophotography, electrostatic recording, electrostatic printing and the like.
Claims
1. A toner for developing electrostatic images, comprising an amorphous polyester resin A and a quaternary ammonium salt compound X, wherein the amorphous polyester resin A is a polycondensate of an alcohol component, a carboxylic acid component, and polyethylene terephthalate, and the content of the quaternary ammonium salt compound X is 3 parts by mass or more and 30 parts by mass or less relative to 100 parts by mass of the amorphous polyester resin A.
2. 2. The toner for developing electrostatic images according to claim 1, wherein the content of polyethylene terephthalate is 5 mol % or more and 75 mol % or less of the total amount of the alcohol component, the carboxylic acid component and the polyethylene terephthalate, assuming that a terephthalic acid-ethylene glycol unit is 1 mol.
3. 2. The toner for developing electrostatic images according to claim 1, wherein the content of polyethylene terephthalate is 20 mol % or more and 50 mol % or less of the total amount of the alcohol component, the carboxylic acid component and the polyethylene terephthalate, assuming that a terephthalic acid-ethylene glycol unit is 1 mol.
4. 4. The toner for developing electrostatic images according to claim 1, wherein the quaternary ammonium salt compound X is a quaternary ammonium salt-containing resin.
5. 4. The toner for developing electrostatic images according to claim 1, wherein the content of the quaternary ammonium salt compound X is 8 parts by mass or more and 20 parts by mass or less based on 100 parts by mass of the amorphous polyester resin A.
6. 4. The toner for developing electrostatic images according to claim 1, wherein the IV value of the polyethylene terephthalate is from 0.40 to 0.
85.
7. 4. The toner for developing electrostatic images according to claim 1, wherein the amorphous polyester resin A contains amorphous resins having different softening points, the difference between which is 10° C. or more.
8. 8. The toner for developing electrostatic images according to claim 7, wherein the amorphous resin having a higher softening point has a softening point of 100° C. or more and 170° C. or less.
9. 8. The toner for developing electrostatic images according to claim 7, wherein the softening point of the amorphous resin having a lower softening point is 70° C. or more and 130° C. or less.
10. 8. The toner for developing electrostatic images according to claim 7, wherein the mass ratio of the amorphous resin having a higher softening point to the amorphous resin having a lower softening point is 10 / 90 or more and 90 / 10 or less.
11. 4. The toner for developing electrostatic images according to claim 1, wherein the amorphous polyester resin A is contained as a binder resin, and the content of the amorphous polyester resin A in the binder resin is 70% by mass or more.
12. 4. The toner for developing electrostatic images according to claim 1, wherein the quaternary ammonium salt compound X is a styrene-based resin containing a quaternary ammonium salt.
Citation Information
Patent Citations
Electrostatic charge image developing toner
JP2004280085A
Binder resin composition for toner
JP2019066536A
Polycondensation resin for toner
JP2019099624A
Toner for electrostatic charge image development
JP2022016369A
Toner for electrostatic charge image development
JP2022102326A