Lithium secondary battery and method of manufacturing same

By using a specific positive electrode additive and adjusting the CC/DC ratio and weight change rate, the battery reduces oxygen gas generation and improves safety and performance, addressing the limitations of conventional lithium secondary batteries.

JP7595986B2Active Publication Date: 2024-12-09LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023521395
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-03
Filing Date
2022-06-02
Publication Date
2024-12-09
Estimated Expiration
2042-06-02

AI Technical Summary

Technical Problem

Conventional lithium secondary batteries face issues with oxygen gas generation during charging and discharging due to irreversible positive electrode additives, leading to electrode expansion, reduced performance, and safety concerns, especially during high-temperature storage.

Method used

Incorporating a positive electrode additive represented by the chemical formula Li p Co (1-q) M 1 q O 4, where M 1 is selected from specific elements, with a CC/DC ratio of initial discharge capacity to initial charge capacity adjusted to 50 to 100, and controlling the weight change rate of the positive electrode composite layer to 0.01 to 2.00%, along with specific manufacturing processes.

Benefits of technology

Reduces oxygen gas generation, improves open circuit voltage, suppresses self-discharge, and enhances battery safety and performance, particularly during high-temperature storage, making it suitable for use in medium and large-sized devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595986000005
    Figure 0007595986000005
  • Figure 0007595986000006
    Figure 0007595986000006
  • Figure 0007595986000007
    Figure 0007595986000007
Patent Text Reader

Abstract

The present invention relates to a lithium secondary battery and a method for manufacturing the same. The lithium secondary battery includes a positive electrode additive represented by Chemical Formula 1 as an irreversible additive in a positive electrode composite layer, and the ratio CC / DC of the initial discharge capacity DC to the initial charge capacity CC during initial charge and discharge is adjusted within a specific range. This reduces the amount of oxygen gas generated during charge and discharge of the lithium secondary battery. At the same time, the open circuit voltage of the battery is increased during initial activation and / or subsequent high-temperature storage, thereby suppressing self-discharge and improving the operating voltage. Therefore, a lithium secondary battery including the same can be useful as a power source for medium- to large-sized devices such as electric vehicles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lithium secondary battery containing a positive electrode additive capable of replenishing lithium ions lost in irreversible reactions, and a method for producing the same.

[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0071872, filed on June 3, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference. [Background technology]

[0003] With the development of technology and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and working potential, long cycle life, and low self-discharge rate, have been commercialized and are widely used.

[0004] Recently, as lithium secondary batteries are used as power sources for medium- to large-sized devices such as electric vehicles, there is an increasing demand for high capacity, high energy density, and low cost lithium secondary batteries. As a result, active research has been conducted on irreversible positive electrode additives that can replenish lithium ions lost due to irreversible reactions that occur at the negative electrode during initial charging, thereby improving capacity during subsequent charging and discharging, and irreversible additives such as Li2NiO2 and Li6CoO4 have been developed.

[0005] However, such conventional irreversible additives are generally prepared by reacting a precursor such as cobalt oxide or nickel oxide with an excess amount of lithium oxide. The irreversible additives prepared in this manner are structurally unstable and generate gases such as oxygen gas (O2) during charging. The generated oxygen gas can induce volume expansion of the electrode assembly, which can act as one of the main factors leading to a deterioration in battery performance.

[0006] [ka]

[0007] In addition, the irreversible additive may be transformed into a thermally unstable structure when stored at high temperatures of 60°C or higher after the initial charge / discharge, which may lead to further release of oxygen gas and limit the progress of self-discharge of the battery.

[0008] Therefore, there is a need to develop a lithium secondary battery that can realize a high operating voltage by using a non-reversible additive in the positive electrode, and that has improved safety and improved self-discharge by reducing oxygen gas generation during activation and subsequent high-temperature storage. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Korean Patent Publication No. 10-2019-0078392 Summary of the Invention [Problem to be solved by the invention]

[0010] Therefore, an object of the present invention is to provide a lithium secondary battery that can realize high electrical performance by using a non-reversible additive in a positive electrode, and that can improve the safety of the battery by reducing the amount of oxygen gas generated during the activation step and the subsequent charge / discharge step, and can improve the self-discharge of a charged battery during high-temperature storage. [Means for solving the problem]

[0011] To solve the above problems, In one embodiment, the present invention comprises: a positive electrode including a positive electrode current collector and a positive electrode mixture layer located on the positive electrode current collector and containing a positive electrode active material and a positive electrode additive represented by the following chemical formula 1; a negative electrode including a negative electrode current collector and a negative electrode mixture layer located on the negative electrode current collector; The positive electrode additive provides a lithium secondary battery in which the ratio CC / DC of an initial discharge capacity DC to an initial charge capacity CC during initial charge / discharge is 50 to 100:

[0012] [Chemical formula 1] Li p Co (1-q) M 1 q O4

[0013] In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4, respectively.

[0014] Specifically, the ratio CC / DC of an initial discharge capacity DC to an initial charge capacity CC during initial charge and discharge of the positive electrode additive may be 60-80.

[0015] The positive electrode mixture layer may have a weight change rate of 0.01 to 2.00% before and after initial charge and discharge.

[0016] The positive electrode additive contained in the positive electrode mixture layer may have a tetragonal structure whose space group is P42 / nmc, and the content of the positive electrode additive may be 0.01 to 5 parts by weight with respect to 100 parts by weight of the entire positive electrode mixture layer.

[0017] In addition, the positive electrode active material contained in the positive electrode mixture layer may be a lithium metal composite oxide represented by the following Chemical Formula 2:

[0018] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u

[0019] In the above Chemical Formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the range of 1.0≦x≦1.30, 0.1≦y<0.95, and 0.01, respectively. <z≦0.5、0≦w≦0.5、0≦v≦0.2、1.5≦u≦4.5である。

[0020] Additionally, the positive electrode mixture layer may contain 0.1 to 5 parts by weight of a conductive material relative to the total weight, and usable conductive materials may include one or more selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber.

[0021] The negative electrode mixture layer may contain a carbon material and a silicon material, and the content of the silicon material may be 1 to 20 parts by weight per 100 parts by weight of the negative electrode mixture layer.

[0022] In this case, the carbon material may include at least one selected from the group consisting of natural graphite, artificial graphite, graphene, carbon nanotubes, carbon black, acetylene black, ketjen black, and carbon fiber.

[0023] The silicon material may include at least one of silicon (Si) particles and silicon oxide (SiOx, 1≦x≦2) particles.

[0024] Moreover, in one embodiment, the present invention provides a positive electrode including a positive electrode current collector and a positive electrode mixture layer located on the positive electrode current collector and containing a positive electrode active material and a positive electrode additive represented by the following chemical formula 1; a negative electrode current collector; and a negative electrode composite layer located on the negative electrode current collector. A method for initially charging the lithium secondary battery comprising: applying a current of 1 C or less to the lithium secondary battery; The present invention provides a method for producing a lithium secondary battery, wherein the ratio CC / DC of an initial discharge capacity DC to an initial charge capacity CC of the positive electrode additive during initial charge and discharge is 50 to 100:

[0025] [Chemical formula 1] Li p Co (1-q) M 1 q O4

[0026] In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4, respectively.

[0027] Here, the initial charging step may be performed in an activation 1 step in which a current of 0.05C to 0.2C is applied to the lithium secondary battery to charge it to an SOC of 30% or less; an activation 2 step in which a current of 0.3C to 0.5C is applied to the lithium secondary battery that has undergone the activation 1 step to charge it to an SOC of more than 30% but less than 70%; and an activation 3 step in which a current of 0.6C to 0.9C is applied to the lithium secondary battery that has undergone the activation 2 step to charge it to an SOC of 70% or more.

[0028] The initial charging step may be performed under a temperature condition of 20 to 70° C., and the lithium secondary battery may be charged with a current of 5 to 900 kgf / cm. 2 The reaction may be carried out under pressure conditions of 0.1 to 1000 MPa. Effect of the Invention

[0029] The lithium secondary battery according to the present invention includes a cathode additive represented by Chemical Formula 1 as a non-reversible additive in a cathode composite layer, and adjusts the ratio CC / DC of the initial discharge capacity DC to the initial charge capacity CC of the cathode additive during initial charge / discharge within a specific range, thereby reducing the amount of oxygen gas generated during charge / discharge of the lithium secondary battery. At the same time, the reduction in the open circuit voltage OCV of the battery during initial charge / discharge and / or subsequent high temperature storage can be suppressed, thereby preventing self-discharge and improving the operating voltage. Thus, a lithium secondary battery including the same can be usefully used as a power source for medium to large devices such as electric vehicles. [Brief description of the drawings]

[0030] [Figure 1] 1 is a graph showing the charge capacity according to the ratio of the charge capacity CC to the discharge capacity DC of a positive electrode additive during initial charge and discharge. [Diagram 2] 1 is a graph showing the cumulative amount of gas generated by the positive electrode additive according to the ratio of the charge capacity CC to the discharge capacity DC during charge and discharge at 45° C. [Diagram 3] 1 is a graph showing the cumulative amount of gas generated by the positive electrode additive according to the ratio of the charge capacity CC to the discharge capacity DC during storage at 60° C. for 4 weeks. [Figure 4] 1 is a graph showing the open circuit voltage OCV of the positive electrode additive at the ratio of the charge capacity CC to the discharge capacity DC according to the charge / discharge cycle when stored at 60° C. for 4 weeks. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] While the present invention may be modified in many ways and may have a variety of embodiments, a specific embodiment will be described in detail in the detailed description.

[0032] However, it should be understood that this is not intended to limit the invention to the particular embodiment, but includes all modifications, equivalents, and alternatives falling within the spirit and technical scope of the invention.

[0033] In the present invention, the terms "comprise" or "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0034] In addition, in the present invention, when a layer, film, region, plate, or other portion is described as being "on" another portion, this includes not only the case where it is "directly on" the other portion, but also the case where there is another portion in between. Conversely, when a layer, film, region, plate, or other portion is described as being "under" the other portion, this includes not only the case where it is "directly under" the other portion, but also the case where there is another portion in between. In addition, in the present application, being "located on" may include not only the case where it is located at the top, but also the case where it is located at the bottom.

[0035] In addition, in the present invention, a "major component" means 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, 95% by weight or more, or 97.5% by weight or more of the total weight of the composition or specific component, and in some cases, it can also mean 100% by weight when it constitutes the entire composition or specific component.

[0036] In the present invention, "Ah" is a unit of capacity of a lithium secondary battery, and is called "ampere-hour" and means the amount of current per hour. For example, if a battery capacity is "3000mAh", it means that it can be discharged at a current of 3000mA for one hour.

[0037] The present invention will now be described in more detail.

[0038] Lithium secondary battery In one embodiment, the present invention comprises: a positive electrode including a positive electrode current collector and a positive electrode mixture layer located on the positive electrode current collector and containing a positive electrode active material and a positive electrode additive represented by the following chemical formula 1; a negative electrode including a negative electrode current collector and a negative electrode mixture layer located on the negative electrode current collector; The positive electrode additive provides a lithium secondary battery in which the ratio CC / DC of an initial discharge capacity DC to an initial charge capacity CC during initial charge / discharge is 50 to 100:

[0039] [Chemical formula 1] Li p Co (1-q) M 1 q O4

[0040] In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4, respectively.

[0041] The lithium secondary battery according to the present invention includes a positive electrode and a negative electrode, and a separator may be interposed between the positive electrode and the negative electrode, or the separator may be omitted. In addition, the positive electrode and the negative electrode are connected to each other by a lithium ion (Li + ) for the transport of oxygen.

[0042] In this case, the positive electrode includes a positive electrode mixture layer prepared by applying a positive electrode slurry containing a positive electrode active material and a positive electrode additive onto a positive electrode current collector, drying and pressing the positive electrode mixture layer, and the positive electrode mixture layer may selectively further include a conductive material, a binder, other additives, and the like, as necessary.

[0043] The positive electrode active material may include a lithium metal composite oxide containing three or more elements selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn) and aluminum (Al), and the lithium metal composite oxide may optionally contain other transition metals (M 1For example, the positive electrode active material may be a lithium metal composite oxide capable of reversible intercalation and deintercalation, as shown in Chemical Formula 2 below:

[0044] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u

[0045] In the above Chemical Formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the range of 1.0≦x≦1.30, 0.1≦y<0.95, and 0.01, respectively. <z≦0.5、0≦w≦0.5、0≦v≦0.2、1.5≦u≦4.5である。

[0046] The lithium metal composite oxide represented by the above formula 2 is a composite metal oxide containing lithium and nickel, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.6 Co 0.2 Mn 0.1 Al 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.15 Al 0.05 O2 and LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1The gas may contain one or more compounds selected from the group consisting of O2.

[0047] The content of the positive electrode active material may be 85 to 95 parts by weight, specifically 88 to 95 parts by weight, 90 to 95 parts by weight, 86 to 90 parts by weight, or 92 to 95 parts by weight, relative to 100 parts by weight of the positive electrode mixture layer.

[0048] The positive electrode mixture layer may include a positive electrode additive that provides irreversible capacity together with a positive electrode active material that exhibits electrical activity, and the positive electrode additive may include a lithium metal oxide represented by the following Chemical Formula 1:

[0049] [Chemical formula 1] Li p Co (1-q) M 1 q O4

[0050] In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4, respectively.

[0051] The positive electrode additive contains an excess of lithium and can provide lithium to replace lithium consumption that occurs due to irreversible chemical and physical reactions at the negative electrode during initial charging, thereby increasing the charging capacity of the battery and reducing the irreversible capacity, thereby improving the life characteristics.

[0052] Among them, the positive electrode additive represented by Chemical Formula 1 has a higher lithium ion content than nickel-containing oxides commonly used in the industry, and therefore can replenish lithium ions lost due to irreversible reactions during initial charging and discharging of the battery, thereby significantly improving the charge and discharge capacity of the battery. Also, compared to iron and / or manganese-containing oxides commonly used in the industry, there is no side reaction caused by the elution of transition metals during charging and discharging of the battery, and therefore the battery has excellent stability. Examples of lithium metal oxides represented by Chemical Formula 1 include Li6CoO4, Li6Co 0.5 Zinc 0.5 O4, Li6Co 0.7 Zinc 0.3 It may also include O4.

[0053] In addition, the positive electrode additive represented by Chemical Formula 1 may have a tetragonal crystal structure, and may be included in the space group P42 / nmc having a distorted tetrahedral structure formed by cobalt and oxygen atoms. The positive electrode additive has a distorted tetrahedral structure formed by cobalt and oxygen atoms, and is structurally unstable. Therefore, a large amount of oxygen gas may be generated during initial charge and discharge (i.e., "activation") and / or subsequent charge and discharge, which may induce volume expansion of the electrode assembly, reducing battery performance and safety; when stored at high temperatures of 60°C or higher after initial charge and discharge, the structure is transformed into a thermally unstable structure, further releasing oxygen gas, and causing self-discharge of the battery.

[0054] However, the lithium secondary battery according to the present invention includes a positive electrode additive represented by Chemical Formula 1, and by adjusting the charge / discharge capacity ratio CC / DC of the positive electrode additive during initial charge / discharge within a specific range, the amount of oxygen gas generated during charge / discharge of the lithium secondary battery can be reduced, and at the same time, the open circuit voltage of the battery can be improved during initial activation and subsequent high temperature storage, thereby suppressing self-discharge and improving the operating voltage.

[0055] Specifically, the lithium secondary battery may have a ratio CC / DC of the discharge capacity DC to the charge capacity CC of the positive electrode additive at the time of initial charge and discharge of 50 to 100. For example, the lithium secondary battery may have a ratio CC / DC of the initial discharge capacity DC to the initial charge capacity CC of the positive electrode additive at the time of initial charge and discharge of 50 to 90, 50 to 75, 50 to 70, 60 to 90, 60 to 80, 60 to 70, 75 to 100, 65 to 75, or 70 to 78. The ratio CC / DC of the initial discharge capacity DC to the initial charge capacity CC of the positive electrode additive can be adjusted depending on the type and content of the positive electrode additive contained in the positive electrode mixture layer, and in some cases, can be controlled by the initial charge and discharge conditions. The present invention can reduce the amount of oxygen gas generated during charging and discharging of the lithium secondary battery by adjusting the ratio CC / DC of the initial charge and discharge capacity of the positive electrode additive to satisfy the above range, and at the same time, can improve the open circuit voltage of the battery during initial charge and discharge and subsequent high temperature storage, suppress self-discharge, and improve the operating voltage. Specifically, when the ratio CC / DC exceeds 100, a significant decrease in the open circuit voltage of the battery during high temperature storage can be prevented, and when the ratio CC / DC is significantly low at less than 50, a large amount of gas is generated during charging and discharging after activation of the battery.

[0056] In addition, in the lithium secondary battery, the weight change rate of the positive electrode mixture layer before and after the initial charge and discharge may be 0.01 to 2.00%, specifically, 0.01 to 1.80%, 0.01 to 1.60%, 0.01 to 1.50%, 0.01 to 1.40%, 0.1 to 1.20%, 0.01 to 1.00%, 0.01 to 0.08%, 0.01 to 0.06%, It may be 0.01-0.05%, 0.01-0.04%, 0.04-0.4%, 0.04-0.5%, 0.04-1.0%, 0.04-1.5%, 0.05-1.0%, 0.08-0.5%, 1.0-2.0%, 1.5-2.0%, 0.05-0.9%, 0.2-1.7%, 1.0-1.7%, or 0.1-0.8%.

[0057] By adjusting the weight change rate of the positive electrode composite layer before and after the initial charge and discharge of the lithium secondary battery within the above-mentioned range, the present invention can reduce the amount of oxygen gas generated during charge and discharge of the lithium secondary battery, and at the same time, can improve the open circuit voltage of the battery during the initial charge and discharge and subsequent high temperature storage, suppress self-discharge, and improve the operating voltage.

[0058] In addition, the positive electrode additive may be included in an amount of 0.01 to 5 parts by weight relative to 100 parts by weight of the positive electrode composite layer, specifically, 0.01 to 4 parts by weight, 0.01 to 3 parts by weight, 0.01 to 2 parts by weight, 0.01 to 1 part by weight, 0.5 to 2 parts by weight, 0.1 to 0.9 parts by weight, 0.2 to 1.5 parts by weight, or 1 to 2 parts by weight relative to 100 parts by weight of the positive electrode composite layer. By adjusting the content of the positive electrode additive within the above range, the present invention can prevent a decrease in charge / discharge capacity due to insufficient replenishment of lithium ions lost due to an irreversible reaction due to a low content of the positive electrode additive, and can prevent a large amount of oxygen gas from being generated during charging and discharging of the battery due to an excessive amount of the positive electrode additive.

[0059] Moreover, the positive electrode mixture layer may further contain a conductive material, a binder, an additive, and the like, in addition to the positive electrode active material and the positive electrode additive.

[0060] In this case, the conductive material can be used to improve the performance of the positive electrode, such as electrical conductivity, and can be one or more carbon-based materials selected from the group consisting of natural graphite, artificial graphite, graphene, carbon nanotubes, carbon black, acetylene black, ketjen black, and carbon fibers. For example, the conductive material may include acetylene black.

[0061] The conductive material may be contained in an amount of 0.1 to 5 parts by weight, specifically 0.5 to 4 parts by weight, and the conductive material may be contained in an amount of 1 to 3.5 parts by weight, or 0.5 to 1.5 parts by weight, relative to 100 parts by weight of the positive electrode mixture layer.

[0062] The binder may include one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-co-HFP), polyvinylidene fluoride (PVdF), polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As an example, the binder may include polyvinylidene fluoride.

[0063] The binder may be contained in an amount of 1 to 10 parts by weight, specifically 2 to 8 parts by weight, or 1 to 5 parts by weight, relative to 100 parts by weight of the entire positive electrode mixture layer.

[0064] Additionally, the average thickness of the positive electrode composite layer is not particularly limited, but may be specifically 50 μm to 300 μm, and more specifically 100 μm to 200 μm, 80 μm to 150 μm, 120 μm to 170 μm, 150 μm to 300 μm, 200 μm to 300 μm, or 150 μm to 190 μm.

[0065] In addition, the positive electrode may be a positive electrode current collector having high conductivity without inducing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. may be used, and in the case of aluminum or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may be formed with fine irregularities on the surface to increase the adhesive strength of the positive electrode active material, and may be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the current collector may be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the positive electrode to be manufactured.

[0066] Meanwhile, the negative electrode includes a negative electrode mixture layer prepared by applying a negative electrode active material onto a negative electrode current collector, drying and pressing the negative electrode mixture layer, and the negative electrode mixture layer may further include the same conductive material, binder, and other additives as those of the positive electrode, as necessary.

[0067] The negative electrode active material may include, for example, a carbon material and a silicon material. The carbon material means a carbon material mainly composed of carbon atoms, and examples of such carbon materials include graphite having a perfect layered crystal structure like natural graphite, soft carbon having a low crystalline layered crystal structure (graphene structure; a structure in which hexagonal honeycomb-shaped carbon planes are arranged in layers), and hard carbon in which such a structure is mixed with a non-crystalline portion, artificial graphite, expanded graphite, carbon fiber, non-graphitizable carbon, carbon black, acetylene black, ketjen black, carbon nanotubes, fullerene, activated carbon, graphene, carbon nanotubes, etc., and preferably, may include at least one selected from the group consisting of natural graphite, artificial graphite, graphene, and carbon nanotubes. More preferably, the carbon material may include natural graphite and / or artificial graphite, and may include at least one of graphene and carbon nanotubes together with the natural graphite and / or artificial graphite. In this case, the carbon material may contain 50 to 95 parts by weight of graphene and / or carbon nanotubes relative to 100 parts by weight of the total carbon material, and more specifically, may contain 60 to 90 parts by weight, or 70 to 80 parts by weight of graphene and / or carbon nanotubes relative to 100 parts by weight of the total carbon material.

[0068] The silicon material is a particle containing silicon (Si) as a metal component as a main component, and is a silicon (Si) particle and a silicon oxide (SiO X , 1≦X≦2) particles. As an example, the silicon material may include silicon (Si) particles, silicon monoxide (SiO) particles, silicon dioxide (SiO2) particles, or a mixture of these particles.

[0069] In addition, the silicon material may have a mixed form of crystalline particles and amorphous particles, and the ratio of the amorphous particles may be 50 to 100 parts by weight, specifically 50 to 90 parts by weight, 60 to 80 parts by weight, or 85 to 100 parts by weight, based on 100 parts by weight of the total silicon material. By controlling the ratio of the amorphous particles contained in the silicon material within the above range, the present invention can improve thermal stability and flexibility without deteriorating the electrical properties of the electrode.

[0070] In addition, the silicon material may include a carbon material and a silicon material, and may be included in an amount of 1 to 20 parts by weight relative to 100 parts by weight of the negative electrode composite layer. Specifically, the silicon material may be included in an amount of 5 to 20 parts by weight, 3 to 10 parts by weight, 8 to 15 parts by weight, 13 to 18 parts by weight, or 2 to 7 parts by weight relative to 100 parts by weight of the negative electrode composite layer.

[0071] By adjusting the contents of the carbon material and silicon material contained in the negative electrode active material to the above ranges, the present invention can reduce the lithium consumption and irreversible capacity loss during the initial charge and discharge of the battery, and improve the charge capacity per unit mass.

[0072] For example, the negative electrode active material may include 95±2 parts by weight of graphite and 5±2 parts by weight of a mixture of silicon monoxide (SiO) particles and silicon dioxide (SiO2) particles uniformly mixed, relative to 100 parts by weight of the negative electrode composite layer. By adjusting the contents of the carbon material and silicon material contained in the negative electrode active material within the above ranges, the present invention can reduce lithium consumption and irreversible capacity loss during initial charging and discharging of the battery, and improve the charging capacity per unit mass.

[0073] The negative electrode mixture layer may have an average thickness of 100 μm to 200 μm, specifically, 100 μm to 180 μm, 100 μm to 150 μm, 120 μm to 200 μm, 140 μm to 200 μm, or 140 μm to 160 μm.

[0074] In addition, the negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and for example, copper, stainless steel, nickel, titanium, calcined carbon, etc. can be used. In the case of copper or stainless steel, it is also possible to use a material that has been surface-treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode current collector can be formed with fine irregularities on the surface to strengthen the binding force with the negative electrode active material, as with the positive electrode current collector, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the negative electrode current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the negative electrode to be manufactured.

[0075] Moreover, the lithium secondary battery according to the present invention may have a separator between the positive electrode and the negative electrode, and in this case, the separator is a thin insulating film having high ion permeability and mechanical strength. The separator is not particularly limited as long as it is one commonly used in the art, and specifically, a sheet or nonwoven fabric made of chemically resistant and hydrophobic polypropylene, glass fiber, or polyethylene may be used, and in some cases, a composite separator in which inorganic particles / organic particles are coated with an organic binder polymer on a porous polymer substrate such as the sheet or nonwoven fabric may be used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte may also serve as the separator. In addition, the pore diameter of the separator may be an average of 0.01 to 10 μm, and the thickness may be an average of 5 to 300 μm.

[0076] Meanwhile, the positive electrode and the negative electrode may be wound in a jelly roll form and housed in a cylindrical battery, a prismatic battery, or a pouch-type battery, or may be housed in a pouch-type battery in a folded or stack-and-folded form, but is not limited thereto.

[0077] The lithium salt-containing electrolyte according to the present invention may be composed of an electrolyte and a lithium salt. The electrolyte may be a non-aqueous organic solvent, an organic solid electrolyte, or an inorganic solid electrolyte.

[0078] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0079] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymeric materials containing ionic dissociation groups.

[0080] Examples of the inorganic solid electrolyte that can be used include nitrides, halides, and sulfates of Li, such as Li3N, LiI, Li5Ni2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2.

[0081] The lithium salt is a substance that is easily dissolved in a non-aqueous electrolyte, and examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium 4-phenylboronate, imides, etc. can be used.

[0082] In addition, for the purpose of improving charge / discharge characteristics, flame retardancy, etc., the electrolyte may contain, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. In some cases, in order to impart non-flammability, a halogen-containing solvent such as carbon tetrachloride or ethylene trifluoride may be further contained, and in order to improve high-temperature storage characteristics, carbon dioxide gas may be further contained, and FEC (Fluoro-Ethylene Carbonate), PRS (Propene Sultone), etc. may be further contained.

[0083] Manufacturing method of lithium secondary battery Moreover, in one embodiment, the present invention provides a positive electrode including a positive electrode current collector and a positive electrode mixture layer located on the positive electrode current collector and containing a positive electrode active material and a positive electrode additive represented by the following chemical formula 1; a negative electrode current collector; and a negative electrode composite layer located on the negative electrode current collector. A method for initially charging the lithium secondary battery comprising: applying a current of 1 C or less to the lithium secondary battery; Provided is a method for producing a lithium secondary battery in which the ratio CC / DC of an initial discharge capacity DC to an initial charge capacity CC of a positive electrode additive during initial charge and discharge is 50 to 100:

[0084] [Chemical formula 1] Li p Co (1-q) M 1 q O4

[0085] In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4, respectively.

[0086] A method for manufacturing a lithium secondary battery according to the present invention includes a step of initially charging the above-mentioned lithium secondary battery of the present invention, the lithium secondary battery including: a positive electrode current collector; a positive electrode composite layer located on the positive electrode current collector and containing a positive electrode active material and a positive electrode additive represented by Chemical Formula 1 below; and a negative electrode including a negative electrode current collector and a negative electrode composite layer located on the negative electrode current collector. In this case, the current applied to the lithium secondary battery is low, such as 1C or less, and the ratio CC / DC of the initial discharge capacity DC of the positive electrode additive contained in the positive electrode composite layer to the initial charge capacity CC during initial charge / discharge may be adjusted to satisfy 50 to 100.

[0087] Specifically, the initial charging step includes a three-stage charging process, that is, activation stages 1 to 3, which are successively performed on the lithium secondary battery.

[0088] More specifically, the initial charging step may be performed by an activation 1 step in which a current of 0.05C to 0.2C is applied to the lithium secondary battery to charge it to an SOC of 30% or less; an activation 2 step in which a current of 0.3C to 0.5C is applied to the lithium secondary battery that has undergone the activation 1 step to charge it to an SOC of more than 30% but less than 70%; and an activation 3 step in which a current of 0.6C to 0.9C is applied to the lithium secondary battery that has undergone the activation 2 step to charge it to an SOC of 70% or more.

[0089] As an example, the initial charging step may be performed by applying a current of 0.08C to 0.15C to the lithium secondary battery to charge it to an SOC of 30% or less; an activation step 2, in which a current of 0.35C to 0.45C is applied to the lithium secondary battery that has undergone the activation step 1 to charge it to an SOC of more than 30% but less than 70%; and an activation step 3, in which a current of 0.65C to 0.8C is applied to the lithium secondary battery that has undergone the activation step 2 to charge it to an SOC of 70% or more.

[0090] The present invention controls the current applied to a lithium secondary battery during initial charging to be 1C or less, and the current value gradually increases as the SOC increases, thereby making it possible to uniformly form an SEI coating on the negative electrode composite layer, and to prevent electrical degradation caused by the positive electrode active material dissociating lithium ions earlier than the positive electrode additive at a significantly low current, or by overlithiation of the positive electrode additive being induced due to a current exceeding 1C.

[0091] In addition, the initial charging step may be performed at a temperature higher than room temperature to reduce the resistance of the electrode. Specifically, each activation step may be performed at a temperature of 20°C to 70°C, more specifically, at a temperature of 20°C to 60°C, 20°C to 40°C, 20°C to 25°C, 40°C to 60°C, 45°C to 60°C, 50°C to 65°C, 50°C to 60°C, 52°C to 58°C, 40°C to 50°C, or 42°C to 48°C. By performing the activation step under a temperature condition that satisfies the above range, the secondary battery can be charged under a lower resistance condition of the positive electrode, so that the charging efficiency can be increased and the uniformity of the SEI coating film formed on the negative electrode mixture layer can be improved.

[0092] Meanwhile, in the initial charging step, the outer surface of the lithium secondary battery may be pressurized using a pressure device such as a jig while charging the lithium secondary battery or continuously after charging, and the pressure may be 5 to 900 kgf / cm. 2 This can be done for 4 to 6 seconds.

[0093] Also, after the initial charging step, the method may further include a step of discharging the charged lithium secondary battery. In this case, the discharging may be performed under a current condition of 0.1 to 1C, specifically, 0.1 to 0.9C, 0.1 to 0.8C, 0.1 to 0.6C, 0.1 to 0.5C, 0.5 to 1C, 0.2 to 0.8C, or 0.4 to 0.6C.

[0094] Moreover, the method for manufacturing a lithium secondary battery according to the present invention may further include an aging step of aging the charged lithium secondary battery after the initial charging step. The aging step may further stabilize the SEI coating by thermal energy and electrochemical energy and re-form it to a uniform thickness. To this end, the aging step may be performed at 20 to 80°C, specifically, 30 to 70°C or 45 to 65°C, for 0.5 to 30 hours.

[0095] The method for manufacturing a lithium secondary battery according to the present invention has the above-mentioned configuration, and thus the ratio CC / DC of the initial charge / discharge capacity of the positive electrode additive containing the positive electrode additive represented by Chemical Formula 1 in the positive electrode mixture layer and / or the weight ratio of the positive electrode mixture layer before and after the initial charge / discharge can be easily controlled within the range of the present invention, thereby reducing the amount of oxygen gas generated during the charge / discharge of the manufactured lithium secondary battery, and improving the open circuit voltage of the battery during the initial activation and / or during subsequent high temperature storage, thereby suppressing self-discharge and improving the operating voltage, and thus the battery can be usefully used as a power source for medium and large devices such as electric vehicles.

[0096] The present invention will now be described in more detail with reference to examples and experimental examples.

[0097] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.

[0098] Examples 1 to 4 and Comparative Examples 1 to 4. Production of Lithium Secondary Batteries N-methylpyrrolidone was poured into a homo mixer, and LiNi as a positive electrode active material was mixed with 100 parts by weight of the positive electrode slurry solids. 0.6 Co 0.2 Mn 0.2 O2 and Li6CoO4 or Li6Co as cathode additive 0.7 Zinc 0.3 97.8 parts by weight of O4, 0.7 parts by weight of a mixture (75:25 wt. / wt.) of carbon nanotubes (average size: 60±10 nm) and denka black (average size: 2±0.5 μm) as a conductive material, and 1.5 parts by weight of PVdF as a binder were weighed and added, and mixed at 2,000 rpm for 60 minutes to prepare a positive electrode slurry for a lithium secondary battery. Here, the content of the positive electrode additive per 100 parts by weight of the positive electrode slurry solids (≒ weight of the positive electrode mixture layer) is as shown in Table 1 below. The prepared positive electrode slurry was applied to one side of an aluminum current collector, dried at 100 ° C., and rolled to prepare a positive electrode. At this time, the total thickness of the positive electrode mixture layer was 130 μm, and the total thickness of the prepared positive electrode was about 200 μm.

[0099] A negative electrode slurry was prepared by preparing 84 parts by weight of natural graphite and 14 parts by weight of silicon (SiOx, where 1≦x≦2) particles as a negative electrode active material and 2 parts by weight of styrene butadiene rubber (SBR) as a binder for 100 parts by weight of the negative electrode slurry solid content, and carrying out the same method as the method for producing the positive electrode slurry. At this time, the graphite used in the production of the negative electrode mixture layer was natural graphite (average particle size: 0.01 to 0.5 μm), and the silicon (SiOx) particles had an average particle size of 0.9 to 1.1 μm. The prepared negative electrode slurry was applied to one side of a copper current collector, dried at 100 ° C., and rolled to produce a negative electrode. At this time, the total thickness of the negative electrode mixture layer was 150 μm, and the total thickness of the produced negative electrode was about 250 μm.

[0100] The prepared positive and negative electrodes were laminated with a separator (thickness: about 16 μm) made of a porous polyethylene (PE) film interposed between them, and E2DVC was injected as an electrolyte to prepare a full cell type lithium secondary battery.

[0101] Here, "E2DVC" refers to a type of carbonate-based electrolyte, a solution in which lithium hexafluorophosphate (LiPF6, 1.0M) and vinyl carbonate (VC, 2% by weight) are mixed with a mixture of ethylene carbonate (EC): dimethyl carbonate (DMC): diethyl carbonate (DEC) = 1:1:1 (volume ratio).

[0102] The manufactured cell was initially charged and discharged at 22±2° C. under the current conditions shown in Table 1 below, to measure the initial charge capacity CC and initial discharge capacity DC of the positive electrode additive, and the ratio CC / DC was calculated. At this time, the potential range of the battery was 2.5 to 4.25 V. In addition, the positive electrode was disassembled from the full cell, the positive electrode mixture layer was peeled off from the positive electrode current collector, and the weight of the positive electrode mixture layer after the initial charge and discharge was measured. The weight change rate before and after the initial charge and discharge was derived from the measured weights before and after the initial charge and discharge.

[0103] [Table 1]

[0104] Experimental example 1. In order to confirm the difference in effect due to the ratio CC / DC of the initial charge capacity CC and the initial discharge capacity DC of the positive electrode additive, the following experiment was carried out.

[0105] a) Manufacturing of lithium secondary batteries In order to confirm the effect of the ratio of the positive electrode additive contained in the lithium secondary battery on the initial charge and discharge capacity, the positive electrode slurry was divided into 100 parts by weight of the positive electrode slurry solids, and the positive electrode additive Li6CoO4 or Li6Co 0.7 Zinc 0.3 Except for using 97.8 parts by weight of O4, the same procedures as in Examples 2 and 4 and Comparative Examples 1 to 4 were carried out to prepare lithium secondary batteries represented by corresponding Examples 2a and 4a and Comparative Examples 1a to 4a.

[0106] The prepared cell was initially charged and discharged at 22±2° C. under the current conditions shown in Table 2 below, to measure the initial charge capacity CC and initial discharge capacity DC of the positive electrode additive, and calculate the ratio CC / DC. At this time, the potential range of the battery was 2.5 to 4.25 V.

[0107] [Table 2]

[0108] B) Evaluation of gas generation rate After initial charging and discharging of the lithium secondary batteries manufactured in Examples 2a and 4a and Comparative Examples 1a to 4a, each secondary battery was repeatedly charged and discharged 50 times at 45° C. and 0.3 C / 0.3 C to measure (1) the amount of gas generated during charging and discharging, and (2) the amount of gas generated during storage for 4 weeks at 60° C. The results are shown in Table 3 below and in FIGS. 2 and 3.

[0109] C) Evaluation of high-temperature storage characteristics The lithium secondary batteries prepared in Examples 2a and 4a and Comparative Examples 1a to 4a were stored at 60° C. for 4 weeks, and the open circuit voltage (OCV) was measured. The change in the open circuit voltage was calculated based on the open circuit voltage before storage. The results are shown in Table 3 and FIG. 4.

[0110] [Table 3]

[0111] As shown in Table 3 and FIGS. 2 to 4, the lithium secondary battery according to the present invention has an advantage in that it has a low amount of gas generation during charging and discharging, as well as improved storage stability at high temperatures and suppressed reduction in open circuit voltage OCV, and thus has excellent electrical performance.

[0112] Specifically, the lithium secondary batteries manufactured in Examples 2a and 4a contain a positive electrode additive represented by Chemical Formula 1, and the ratio CC / DC of the charge capacity CC and discharge capacity DC of the positive electrode additive during initial charge and discharge is adjusted within a specific range, the weight change rate of the positive electrode composite layer meets a certain range, and the cumulative gas generation during charge and discharge after the initial charge and discharge and during high temperature storage for 4 weeks increases as the content of the positive electrode additive increases, but is reduced when compared to the same amount. Also, it was shown that the open circuit voltage change ΔOCV after high temperature storage of the lithium secondary batteries of the examples is reduced.

[0113] From these results, it can be seen that the lithium secondary battery according to the present invention includes a cathode additive represented by Chemical Formula 1 as a non-reversible additive in a cathode composite layer, and by adjusting the ratio CC / DC of the initial discharge capacity DC to the initial charge capacity CC of the cathode additive during initial charge and discharge within a specific range, the amount of oxygen gas generated during charge and discharge of the lithium secondary battery can be reduced, and at the same time, the open circuit voltage of the battery can be improved during initial activation and / or subsequent high temperature storage, thereby suppressing self-discharge and improving the operating voltage.

[0114] Although the present invention has been described above with reference to preferred embodiments thereof, it will be understood that a person skilled in the art or having ordinary knowledge in the art can make various modifications and variations to the present invention without departing from the spirit and technical scope of the present invention as described in the claims below.

[0115] Therefore, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.

Claims

1. a positive electrode including a positive electrode current collector and a positive electrode mixture layer located on the positive electrode current collector and containing a positive electrode active material and a positive electrode additive represented by the following Chemical Formula 1; a negative electrode including a negative electrode current collector and a negative electrode mixture layer located on the negative electrode current collector; The positive electrode additive has a ratio CC / DC of an initial discharge capacity DC to an initial charge capacity CC during initial charge / discharge of 50 to 100; The initial charging stage is An activation step in which a current of 0.05C to 0.2C is applied to the lithium secondary battery to charge it to an SOC of 30% or less; A second activation step in which a current of 0.3 C to 0.5 C is applied to the lithium secondary battery that has undergone the first activation step to charge the battery to an SOC of more than 30% and less than 70%; and The activation step is a third activation step in which a current of 0.6C to 0.9C is applied to the lithium secondary battery that has undergone the second activation step to charge it to an SOC of 70% or more. The initial discharge stage is performed under a current condition of 0.1C to 1C. Lithium secondary battery: [Chemical formula 1] Li p Co (1-q) M 1 q O 4 In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4, respectively.

2. 2. The lithium secondary battery according to claim 1, wherein the positive electrode additive has a ratio CC / DC of an initial discharge capacity DC to an initial charge capacity CC during initial charge and discharge of 60 to 80.

3. The lithium secondary battery according to claim 1, wherein the positive electrode mixture layer has a weight change rate of 0.01% to 2.00% before and after initial charge and discharge.

4. The positive electrode additive has a space group of P4 2 2. The lithium secondary battery according to claim 1, having a tetragonal structure in which the lattice constant is 0.1-0.1 / nmc.

5. 2. The lithium secondary battery according to claim 1, wherein the content of the positive electrode additive is 0.01 to 5 parts by weight per 100 parts by weight of the entire positive electrode mixture layer.

6. The lithium secondary battery according to claim 1, wherein the positive electrode active material is a lithium metal composite oxide represented by the following chemical formula 2: [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u In the above Chemical Formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v and u are within the ranges of 1.0≦x≦1.30, 0.1≦y<0.95, 0.01<z≦0.5, 0≦w≦0.5, 0≦v≦0.2, and 1.5≦u≦4.5, respectively.

7. 2. The lithium secondary battery according to claim 1, wherein the positive electrode mixture layer contains 0.1 to 5 parts by weight of a conductive material based on the total weight.

8. 2. The lithium secondary battery according to claim 1, wherein the positive electrode mixture layer contains one or more conductive materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber.

9. The negative electrode mixture layer includes a carbon material and a silicon material, and 2. The lithium secondary battery according to claim 1, wherein the content of the silicon material is 1 to 20 parts by weight based on 100 parts by weight of the negative electrode mixture layer.

10. 10. The lithium secondary battery according to claim 9, wherein the carbon material comprises at least one selected from the group consisting of natural graphite, artificial graphite, graphene, carbon nanotubes, carbon black, acetylene black, ketjen black, and carbon fibers.

11. 10. The lithium secondary battery of claim 9, wherein the silicon material comprises at least one of silicon (Si) particles and silicon oxide (SiOx, 1≦x≦2) particles.

12. a positive electrode including a positive electrode current collector and a positive electrode mixture layer located on the positive electrode current collector and containing a positive electrode active material and a positive electrode additive represented by the following Chemical Formula 1; a negative electrode current collector; and a negative electrode composite layer located on the negative electrode current collector. A method for initially charging the lithium secondary battery comprising: applying a current of 1 C or less to the lithium secondary battery; The ratio CC / DC of the initial discharge capacity DC to the initial charge capacity CC during the initial charge / discharge is 50 to 100; The initial charging stage is An activation step in which a current of 0.05C to 0.2C is applied to the lithium secondary battery to charge it to an SOC of 30% or less; A second activation step in which a current of 0.3 C to 0.5 C is applied to the lithium secondary battery that has undergone the first activation step to charge the battery to an SOC of more than 30% and less than 70%; and The activation step is a third activation step in which a current of 0.6C to 0.9C is applied to the lithium secondary battery that has undergone the second activation step to charge it to an SOC of 70% or more. The initial discharge step is performed under a current condition of 0.1C to 1C. [Chemical formula 1] Li p Co (1-q) M 1 q O 4 In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4, respectively.

13. The initial charging stage is An activation step in which a current of 0.08C to 0.15C is applied to the lithium secondary battery to charge it to an SOC of 30% or less; A second activation step in which a current of 0.35C to 0.45C is applied to the lithium secondary battery that has undergone the first activation step to charge the battery to an SOC of more than 30% and less than 70%; and The method for manufacturing a lithium secondary battery according to claim 12, wherein the lithium secondary battery is subjected to a third activation step of charging the lithium secondary battery after the second activation step to an SOC of 70% or more by applying a current of 0.65C to 0.8C.

14. The method for manufacturing a lithium secondary battery according to claim 12, wherein the initial charging step is performed under a temperature condition of 20 to 70°C.

15. The initial charging stage is 5 kgf / cm2 for the lithium secondary battery. 2 ~900kgf / cm 2 The method for producing a lithium secondary battery according to claim 12, wherein the reaction is carried out under a pressure condition of

Citation Information

Patent Citations

  • Method of manufacturing secondary battery

    JP2003109662A

  • Additives for positive electrode, method for manufacturing the same, positive electrode including the same, and lithium recharegable battery including the same

    KR1020190078392A

  • Positive active material for rechargeable lithium battery and rechargeable lithium battery including same

    US20130171524A1

  • Pre-doping agent, positive electrode, lithium ion secondary battery, and method for producing same

    WO2015011883A1

  • Nonaqueous-electrolyte secondary battery and method for manufacturing nonaqueous-electrolyte secondary battery