Method for processing single crystal silicon carbide substrate
The method of pulsed laser beam irradiation and subsequent grinding addresses the inefficiencies of existing techniques by allowing precise and cost-effective separation of single-crystal silicon carbide substrates into thin pieces, reducing wear and processing costs.
Patent Information
- Application Number
- JP2021053588
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-26
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-03-26
AI Technical Summary
Existing methods for processing single-crystal silicon carbide substrates are inefficient in modifying shallow positions less than 100 μm from the surface, leading to difficulties in separating the substrate into thin pieces and high processing costs due to wear on grinding wheels.
A method involving pulsed laser beam irradiation followed by grinding, where a pulsed laser beam is used to heat and partially overlap areas on the substrate surface, allowing for controlled separation and removal of heated regions, reducing the need for additional force-based peeling.
Enables precise adjustment of the amount removed, minimizes grinding wheel wear, and lowers processing costs by naturally peeling off heated portions, facilitating thinning of the substrate without additional peeling forces.
Smart Images

Figure 0007596035000001 
Figure 0007596035000002 
Figure 0007596035000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for processing a single crystal silicon carbide substrate. [Background technology]
[0002] In order to realize small and lightweight device chips, there are increasing opportunities to thin semiconductor substrates (semiconductor wafers) on which devices such as integrated circuits are provided on the front side. For example, the front side of the semiconductor substrate is held by a chuck table, and the grinding wheel to which a grinding stone containing abrasive grains is fixed and the chuck table are rotated relative to each other, thereby grinding and thinning the semiconductor substrate.
[0003] Incidentally, power electronics devices such as inverters incorporate semiconductor elements called power devices suitable for controlling electric power. These power devices are manufactured using substrates (hereinafter, single-crystal silicon carbide substrates) made of single-crystal silicon carbide (SiC), which is advantageous in terms of higher voltage resistance and lower loss compared to single-crystal silicon (Si) and the like.
[0004] On the other hand, since single crystal silicon carbide is very hard, grinding a single crystal silicon carbide substrate using the above-mentioned method results in a large wear of the grindstone. In recent years, therefore, a technique has been proposed in which a plurality of regions at a predetermined depth from the surface of a single crystal silicon carbide substrate is modified with a laser beam, and the single crystal silicon carbide substrate is separated into two thin single crystal silicon carbide substrates at a plane including these regions (for example, see Patent Document 1).
[0005] The area modified by the laser beam is more fragile than other areas, and cracks occur between two adjacent modified areas, so by using this technology, the single-crystal silicon carbide substrate can be easily separated into two pieces with little force to make them thinner. In other words, the amount (thickness) to be removed by subsequent grinding is reduced, and wear on the grinding wheel can be kept to a minimum. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-28072 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, with the above-mentioned technique, it is difficult to modify a shallow position less than 100 μm from the surface of the single crystal silicon carbide substrate and separate the single crystal silicon carbide substrate into two pieces at this shallow position. Therefore, for example, when the amount to be removed from the single crystal silicon carbide substrate is small (i.e., when the boundary for separation should be located at a position close to the surface), the above-mentioned technique cannot be adopted.
[0008] In addition, while the above-mentioned technology can reduce wear on the grindstone, it requires two new processes: modifying the single-crystal silicon carbide substrate with a laser beam and separating the single-crystal silicon carbide substrate into two pieces by applying force. Therefore, from the viewpoint of processing costs, etc., a more advantageous technology is needed.
[0009] The present invention has been made in consideration of such problems, and an object of the present invention is to provide a new method for processing a single crystal silicon carbide substrate that can be adopted when the amount to be removed is small (when the thickness to be removed is small) and that keeps the processing costs low. [Means for solving the problem]
[0010] According to one aspect of the present invention, there is provided a method for processing a single-crystal silicon carbide substrate, the single-crystal silicon carbide substrate having a first surface and a second surface located opposite to the first surface, and a c-axis intersecting the first surface and the second surface, the method including a laser beam irradiation step of irradiating the first surface side of the single-crystal silicon carbide substrate with a pulsed laser beam having a wavelength of 9 μm to 11 μm, and a grinding wheel for grinding the single-crystal silicon carbide substrate by rotating a grinding wheel including a grinding wheel and bringing the grinding wheel into contact with the first surface side of the single-crystal silicon carbide substrate irradiated with the pulsed laser beam, the grinding wheel including a grinding wheel being rotated. and a laser beam application step, in which a region to be irradiated with the pulse laser beam is moved on the first surface so that an irradiated region on the first surface of the pulse laser beam irradiated to the single crystal silicon carbide substrate partially overlaps with an irradiated region on the first surface of the pulse laser beam to be subsequently irradiated to the single crystal silicon carbide substrate, and a portion of the single crystal silicon carbide substrate including the irradiated region is heated by irradiation with the pulse laser beam, thereby peeling off and removing the heated portion from a remaining portion of the single crystal silicon carbide substrate.
[0011] Preferably, in the laser beam applying step, the pulsed laser beam is applied to the single crystal silicon carbide substrate under conditions such that the depth of the portion is less than 30 μm from the first surface.
[0012] Preferably, the second surface of the single crystal silicon carbide substrate has a device region including a plurality of devices and a peripheral excess region surrounding the device region, and in the laser beam irradiation step, the pulsed laser beam is irradiated to a region of the first surface side located on the opposite side of the single crystal silicon carbide substrate to the device region, and in the grinding step, the region of the first surface side of the single crystal silicon carbide substrate is ground to form a disk-shaped thin plate portion and an annular thick plate portion surrounding the thin plate portion. Effect of the Invention
[0013] In a method for processing a single crystal silicon carbide substrate according to one aspect of the present invention, when a pulsed laser beam is irradiated onto the single crystal silicon carbide substrate, an area to be irradiated with the pulsed laser beam is moved so that the irradiated areas of the pulsed laser beam partially overlap, and a portion of the single crystal silicon carbide substrate including the irradiated area is heated by irradiating the pulsed laser beam, thereby peeling and removing the heated portion from the remaining area of the single crystal silicon carbide substrate.
[0014] Therefore, the size of the portion to be removed from the single crystal silicon carbide substrate can be easily adjusted by simply changing the conditions for irradiating the pulse laser beam. In other words, even when the amount to be removed is small (when the thickness to be removed is small), the method for processing a single crystal silicon carbide substrate according to one aspect of the present invention can be employed.
[0015] In addition, since the heated portion of the single crystal silicon carbide substrate is naturally peeled off due to the effect of heating caused by the irradiation of the pulsed laser beam, it is not necessary to apply a force for peeling to the single crystal silicon carbide substrate to peel off the heated portion after the irradiation of the pulsed laser beam, which makes it possible to reduce the cost required for processing compared to the conventional method in which a force must be applied after the irradiation of the laser beam. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a perspective view showing an example of a single crystal silicon carbide substrate. [Diagram 2] FIG. 2 is a side view showing an example of a single crystal silicon carbide substrate. [Diagram 3] FIG. 3 is a perspective view showing an example of a laser processing device. [Figure 4] FIG. 4 is a perspective view showing a state in which the single crystal silicon carbide substrate is held by a chuck table. [Diagram 5] FIG. 5 is a perspective view showing how a single crystal silicon carbide substrate is irradiated with a pulsed laser beam. [Figure 6] FIG. 6 is a plan view showing an example of an area irradiated with a pulsed laser beam. [Figure 7]FIG. 7 is a cross-sectional view showing an example of a portion heated by a pulsed laser beam. [Figure 8] FIG. 8 is a cross-sectional view showing an example of a single crystal silicon carbide substrate from which the heated portion has been removed. [Figure 9] FIG. 9 is a perspective view showing an example of a grinding device. [Figure 10] FIG. 10 is a perspective view showing a state in which the single crystal silicon carbide substrate is ground. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] An embodiment of the present invention will be described with reference to the accompanying drawings. Fig. 1 is a perspective view showing an example of a single crystal silicon carbide substrate 11 processed by a method for processing a single crystal silicon carbide substrate according to the present embodiment, and Fig. 2 is a side view showing the example of the single crystal silicon carbide substrate 11. As shown in Figs. 1 and 2, the single crystal silicon carbide substrate 11 is a disk-shaped wafer made of hexagonal single crystal silicon carbide (SiC).
[0018] This single crystal silicon carbide substrate 11 has a circular first surface 11a and a circular second surface 11b located on the opposite side to the first surface 11a and generally parallel to the first surface 11a. On the outer periphery of the single crystal silicon carbide substrate 11, a first orientation flat 13a and a second orientation flat 13b are formed which are generally linear when viewed from a direction perpendicular to the first surface 11a (or the second surface 11b).
[0019] The extension direction of the first orientation flat 13a and the extension direction of the second orientation flat 13b are approximately perpendicular to each other, and the length of the first orientation flat 13a in the direction parallel to the first surface 11a is longer than the length of the second orientation flat 13b in the direction parallel to the first surface 11a.
[0020] The c-axis 15 of the single crystal silicon carbide constituting the single crystal silicon carbide substrate 11 is inclined at an angle α (called an off angle) toward the second orientation flat 13b with respect to a perpendicular line 17 to the first surface 11a (perpendicular line to the second surface 11b). That is, a c-plane 19 perpendicular to the c-axis 15 also forms an angle α with the first surface 11a and the second surface 11b. α is typically 4°. However, α can be freely set within a range of 1° to 6°.
[0021] The second surface 11b of the single crystal silicon carbide substrate 11 is divided into, for example, a generally circular device region and a peripheral excess region surrounding the device region. The device region is further divided into a plurality of small regions by a plurality of streets (planned division lines) intersecting each other, and a device such as a power MOSFET (Metal-Oxide-Semiconductor Field Effect Transistor) is formed in each small region. That is, the device region includes a plurality of devices.
[0022] There are no limitations on the type, number, shape, structure, size, arrangement, etc. of the devices formed on single crystal silicon carbide substrate 11. In this embodiment, the workpiece is single crystal silicon carbide substrate 11 having devices formed on second surface 11b, but the method for processing a single crystal silicon carbide substrate according to the present invention can also be applied to single crystal silicon carbide substrate 11 not provided with devices.
[0023] In the method for processing a single crystal silicon carbide substrate according to the present embodiment, single crystal silicon carbide substrate 11 is processed from first surface 11a to be thinned. Specifically, first, a pulsed laser beam having a wavelength of 9 μm to 11 μm is irradiated onto first surface 11a of single crystal silicon carbide substrate 11 (laser beam irradiation step).
[0024] Fig. 3 is a perspective view showing an example of the laser processing device 2 used in this embodiment. Note that in Fig. 3, some components of the laser processing device 2 are shown in functional blocks. Also, the X1 axis direction (processing feed direction), Y1 axis direction (indexing feed direction), and Z1 axis direction (vertical direction) used in the following description are perpendicular to each other.
[0025] As shown in Fig. 3, the laser processing device 2 has a base 4 on which each component is mounted. A horizontal movement mechanism (processing feed mechanism, indexing feed mechanism) 6 is disposed on the upper surface of the base 4. The horizontal movement mechanism 6 has a pair of Y1-axis guide rails 8 fixed to the upper surface of the base 4 and generally parallel to the Y1-axis direction. A Y1-axis movement plate 10 is attached to the Y1-axis guide rails 8 in a manner that allows it to slide along the Y1-axis direction.
[0026] A nut portion (not shown) constituting a ball screw is provided on the underside of the Y1-axis moving plate 10. A screw shaft 12 that is generally parallel to the Y1-axis guide rail 8 is rotatably connected to this nut portion. A Y1-axis pulse motor 14 is connected to one end of the screw shaft 12. When the screw shaft 12 is rotated by the Y1-axis pulse motor 14, the Y1-axis moving plate 10 moves in the Y1-axis direction along the Y1-axis guide rail 8.
[0027] A pair of X1-axis guide rails 16 that are generally parallel to the X1-axis direction are provided on the upper surface of the Y1-axis moving plate 10. An X1-axis moving plate 18 is attached to the X1-axis guide rails 16 in a manner that allows it to slide along the X1-axis direction. A nut portion (not shown) that constitutes a ball screw is provided on the lower surface side of the X1-axis moving plate 18.
[0028] A screw shaft 20 that is generally parallel to the X1-axis guide rail 16 is rotatably connected to this nut portion. An X1-axis pulse motor 22 is connected to one end of the screw shaft 20. When the screw shaft 20 is rotated by the X1-axis pulse motor 22, the X1-axis moving plate 18 moves in the X1-axis direction along the X1-axis guide rail 16.
[0029] A cylindrical table base 24 is disposed on the upper surface side of the X1-axis moving plate 18. A chuck table (holding table) 26 used to hold the single crystal silicon carbide substrate 11, which is the workpiece, is disposed on the upper part of the table base 24. A rotation drive source (not shown), such as a motor, is connected to the lower part of the table base 24.
[0030] The force generated by this rotary drive source rotates the chuck table 26 around a rotation axis that is roughly parallel to the Z1-axis direction. The table base 24 and the chuck table 26 are also moved in the X1-axis direction and the Y1-axis direction by the horizontal movement mechanism 6 described above (processing feed, indexing feed).
[0031] It is assumed that this laser processing apparatus 2 processes single crystal silicon carbide substrate 11 supported by annular frame 23 via tape 21. That is, before laser processing apparatus 2 irradiates first surface 11a of single crystal silicon carbide substrate 11 with a pulsed laser beam, tape 21 having a diameter larger than that of single crystal silicon carbide substrate 11 is attached to second surface 11b side of single crystal silicon carbide substrate 11.
[0032] Furthermore, an annular frame 23 configured to be able to surround single crystal silicon carbide substrate 11 is fixed to the outer periphery of tape 21. Of course, in the method for processing a single crystal silicon carbide substrate according to the present invention, a pulse laser beam may be irradiated onto single crystal silicon carbide substrate 11 in a state in which tape 21 is not attached or in a state in which it is not supported by frame 23.
[0033] A part of the upper surface of the chuck table 26 is formed of, for example, a porous material, and functions as a holding surface 26a that comes into contact with the tape 21 (or the single-crystal silicon carbide substrate 11 when the tape 21 is not attached) and holds the single-crystal silicon carbide substrate 11. The holding surface 26a is approximately parallel to the X1-axis direction and the Y1-axis direction.
[0034] In addition, holding surface 26a is connected to a suction source (not shown) such as a vacuum pump via a flow path (not shown) or the like provided inside chuck table 26. Four clamps 28 capable of fixing annular frame 23 supporting single crystal silicon carbide substrate 11 are provided around chuck table 26.
[0035] A support structure 30 having a side surface generally perpendicular to the X1-axis direction is provided in an area on one side of the horizontal movement mechanism 6 in the Y1-axis direction. A vertical movement mechanism (height adjustment mechanism) 32 is disposed on the side surface of this support structure 30. The vertical movement mechanism 32 includes a pair of Z1-axis guide rails 34 fixed to the side surface of the support structure 30 and generally parallel to the Z1-axis direction. A Z1-axis movement plate 36 is attached to the Z1-axis guide rails 34 in such a manner that it can slide along the Z1-axis direction.
[0036] A nut portion (not shown) constituting a ball screw is provided on the back side (Z1-axis guide rail 34 side) of the Z1-axis moving plate 36. A screw shaft (not shown) that is generally parallel to the Z1-axis guide rail 34 is rotatably connected to this nut portion. A Z1-axis pulse motor 38 is connected to one end of the screw shaft. When the screw shaft is rotated by the Z1-axis pulse motor 38, the Z1-axis moving plate 36 moves in the Z1-axis direction along the Z1-axis guide rail 34.
[0037] A support 40 is fixed to the front surface side of the Z1-axis moving plate 36, and a part of a laser beam irradiation unit 42 is supported by this support 40. The laser beam irradiation unit 42 includes, for example, a laser oscillator (not shown) fixed to the base 4, a cylindrical housing 44 that is supported by the support 40 and is long in the Y1-axis direction, and an irradiation head 46 provided at an end of the housing 44 (the other end in the Y1-axis direction).
[0038] The laser oscillator uses, for example, carbon dioxide gas as a laser medium, generates a high-output pulsed laser beam suitable for processing the single crystal silicon carbide substrate 11, and radiates it toward the housing 44. In this embodiment, the laser oscillator generates a pulsed laser beam having a wavelength (10.6 μm) that is absorbed by the single crystal silicon carbide substrate 11. Note that single crystal silicon carbide has an absorption band of 9 μm to 11 μm.
[0039] The housing 44 contains a part of the optical system that constitutes the laser beam irradiation unit 42, and guides the pulsed laser beam emitted from the laser oscillator to an irradiation head 46 at the end. The irradiation head 46 contains another part of the optical system that constitutes the laser beam irradiation unit 42. For example, the irradiation head 46 changes the path of the pulsed laser beam guided from the housing 44 downward with an optical element such as a mirror, and focuses the beam at a position of a predetermined height on the chuck table 26 side with a focusing lens.
[0040] A camera (imaging unit) 48 fixed to the housing 44 is disposed in an area on one side in the X1-axis direction of the irradiation head 46. The camera 48 includes a two-dimensional optical sensor such as a CMOS (Complementary Metal-Oxide-Semiconductor) image sensor or a CCD (Charge Coupled Device) image sensor that is sensitive to visible light, and is used when imaging the single crystal silicon carbide substrate 11 held by the chuck table 26, etc.
[0041] The housing 44 and the irradiation head 46 of the laser beam irradiation unit 42, together with the above-mentioned camera 48, are moved in the Z1-axis direction by the vertical movement mechanism 32. In other words, the vertical movement mechanism 32 moves components such as optical elements and lenses provided in the irradiation head 46 in a direction approximately perpendicular to the holding surface 26a of the chuck table 26.
[0042] In this embodiment, the laser oscillator is fixed to the base 4, but the laser oscillator may be supported by the vertical movement mechanism 32 together with the housing 44 and the like, and may be configured to be movable in the Z1-axis direction. Also, an actuator or the like may be provided in the irradiation head 46 so that only the lens inside the irradiation head 46 can be moved independently in the Z1-axis direction.
[0043] The upper part of the base 4 is covered with a cover (not shown) capable of housing each of the components. A touch screen (input / output device) 50 serving as a user interface is disposed on the side of this cover. For example, various conditions applied when processing the single crystal silicon carbide substrate 11 are input to this touch screen 50. Note that instead of the touch screen 50 in which a display device (output device) and an input device are integrated, a display device (output device) such as a liquid crystal display and an input device such as a keyboard and a mouse may be provided separately.
[0044] The components such as the horizontal movement mechanism 6, the vertical movement mechanism 32, the laser beam irradiation unit 42, the camera 48, the touch screen 50, etc. are each connected to a control unit 52. The control unit 52 controls each of the components described above in accordance with a series of steps required for processing the single crystal silicon carbide substrate 11.
[0045] The control unit 52 is configured by a computer including, for example, a processing device such as a central processing unit (CPU), a main storage device such as a dynamic random access memory (DRAM), and an auxiliary storage device such as a hard disk drive or a flash memory. The functions of the control unit 52 are realized by operating the processing device and the like in accordance with software stored in the auxiliary storage device. However, the control unit 52 may be realized only by hardware.
[0046] When irradiating the first surface 11a of the single crystal silicon carbide substrate 11 with a pulsed laser beam, first, the second surface 11b side of the single crystal silicon carbide substrate 11 is held by the chuck table 26 of the above-mentioned laser processing apparatus 2. Specifically, for example, the single crystal silicon carbide substrate 11 is placed on the chuck table 26 so that the tape 21 attached to the second surface 11b of the single crystal silicon carbide substrate 11 is brought into contact with the holding surface 26a of the chuck table 26.
[0047] Then, negative pressure from a suction source is applied to holding surface 26a of chuck table 26. As a result, second surface 11b side of single crystal silicon carbide substrate 11 is held on chuck table 26 via tape 21, and first surface 11a is exposed upward. Frame 23 attached to tape 21 is fixed by four clamps 28. Fig. 4 is a perspective view showing a state in which single crystal silicon carbide substrate 11 is placed on chuck table 26. For convenience of explanation, tape 21, frame 23, clamps 28, etc. are omitted in Fig. 4.
[0048] After the second surface 11b side of the single crystal silicon carbide substrate 11 is held by the chuck table 26, a pulsed laser beam (a pulsed laser beam having a wavelength of 9 μm to 11 μm) generated using carbon dioxide gas as a medium is irradiated onto the exposed first surface 11a of the single crystal silicon carbide substrate 11. Fig. 5 is a perspective view showing how the single crystal silicon carbide substrate 11 is irradiated with a pulsed laser beam 31. Note that the tape 21, the frame 23, the clamps 28, etc. are also omitted in Fig. 5.
[0049] Specifically, for example, the positional relationship between the chuck table 26 and the irradiation head 46 is adjusted by the horizontal movement mechanism 6 or the like so that the intended irradiation area 46a of the pulsed laser beam 31 located directly under the irradiation head 46 is positioned on the first surface 11a of the single crystal silicon carbide substrate 11. Then, the pulsed laser beam 31 generated by the laser oscillator is emitted toward this intended irradiation area 46a. As a result, the pulsed laser beam 31 is irradiated onto a portion (irradiated area) of the first surface 11a that overlaps with the intended irradiation area 46a.
[0050] As described above, in this embodiment, the pulsed laser beam 31 is used, which has a wavelength that is absorbed by the single crystal silicon carbide substrate 11. Therefore, most of the pulsed laser beam 31 irradiated onto the irradiated region of the first face 11a is absorbed by the single crystal silicon carbide substrate 11 and converted into heat. As a result, the portion of the single crystal silicon carbide substrate 11 including the irradiated region is rapidly heated and then rapidly cooled.
[0051] The laser oscillator of the laser beam irradiation unit 42 is configured to generate the pulsed laser beam 31 at a predetermined repetition frequency. Therefore, by operating the horizontal movement mechanism 6 while generating the pulsed laser beam 31 with the laser oscillator and moving the region 46a to be irradiated with the pulsed laser beam 31 relative to the first surface 11a, the pulsed laser beam 31 can be irradiated onto a plurality of different portions (irradiated regions) on the first surface 11a.
[0052] Fig. 6 is a plan view showing an example of an irradiated region 11c of the pulsed laser beam 31, and Fig. 7 is a cross-sectional view showing an example of a portion 11d heated by the pulsed laser beam 31. As shown in Fig. 6 and Fig. 7, in this embodiment, the irradiated region 11c on the first surface 11a of the pulsed laser beam 31 irradiated to the single crystal silicon carbide substrate 11 at a certain timing and the irradiated region 11c on the first surface 11a of the pulsed laser beam 31 irradiated to the single crystal silicon carbide substrate 11 at the next timing are partially overlapped with each other.
[0053] That is, the region 46a to be irradiated with the pulsed laser beam 31 is moved on the first surface 11a in accordance with the repetition frequency of the pulsed laser beam 31, the size of the irradiated region 11c, and the like, so that the irradiated region 11c on the first surface 11a of the pulsed laser beam 31 and the region 11c to be irradiated next on the first surface 11a of the pulsed laser beam 31 partially overlap. This makes it possible to peel off and remove the heated portion 11d including the irradiated region 11c from the remaining portion 11e of the single-crystal silicon carbide substrate 11.
[0054] 8 is a cross-sectional view showing an example of the single crystal silicon carbide substrate 11 from which the heated portion 11d has been removed. It is presumed that the reason why the heated portion 11d is successfully peeled off by the above-mentioned method is that the thermal expansion and thermal contraction of each portion 11d and the thermal gradient caused by the partial overlap of adjacent irradiated regions 11c promote the occurrence of cracks along the boundary between the portion 11d and the portion 11e. In this way, by removing the heated portion 11d to substantially thin the single crystal silicon carbide substrate 11, the amount to be removed by subsequent grinding can be reduced.
[0055] Note that single crystal silicon carbide substrate 11 has the property of being easily cleaved along c-plane 19 perpendicular to c-axis 15. Therefore, it is considered that the above-mentioned crack mainly extends in a direction along c-plane 19 of single crystal silicon carbide substrate 11. In other words, heated portion 11d is separated mainly along c-plane 19 at the boundary with portion 11e.
[0056] The conditions for the irradiation of the pulsed laser beam 31 can be arbitrarily set and changed according to the amount (thickness) to be removed from the single crystal silicon carbide substrate 11. However, if the portion 11d heated by the irradiation of the pulsed laser beam 31 becomes too large, cracks are unlikely to occur at the boundary between this portion 11d and the remaining portion 11e. Therefore, it is desirable to irradiate the single crystal silicon carbide substrate 11 with the pulsed laser beam 31 under conditions such that the depth of this portion 11d is less than 30 μm from the first surface 11a.
[0057] On the other hand, if portion 11d becomes too small, the amount to be removed by subsequent grinding cannot be sufficiently reduced, which reduces the significance of irradiating single crystal silicon carbide substrate 11 with a pulsed laser beam. Therefore, it is desirable to irradiate single crystal silicon carbide substrate 11 with pulsed laser beam 31 under conditions such that the depth of portion 11d is 2 μm or more from first surface 11a.
[0058] More specifically, the output of the pulsed laser beam 31 is set to, for example, 120 W to 130 W, and the repetition frequency is set to, for example, 1 kHz to 200 kHz. The speed at which the region to be irradiated 46a is moved relative to the first surface 11a is set to, for example, 200 mm / s, and the size (diameter) of the irradiated region 11c is set to, for example, 100 μm to 200 μm. When these conditions are applied, the portion 11d at a depth of about 20 μm from the first surface 11a can be removed from the single crystal silicon carbide substrate 11.
[0059] For example, the pulsed laser beam 31 is irradiated onto substantially the entire first surface 11a of the single crystal silicon carbide substrate 11, and when the entire single crystal silicon carbide substrate 11 is substantially thinned, the irradiation of the pulsed laser beam 31 is terminated. Note that, although the intended irradiation region 46a is moved linearly relative to the first surface 11a in this embodiment, the intended irradiation region 46a may be moved curvedly relative to the first surface 11a. For example, the intended irradiation region 46a may be moved so as to draw a spiral trajectory.
[0060] After irradiating the first surface 11a side of the single crystal silicon carbide substrate 11 with the pulsed laser beam 31 and removing the heated portion 11d, the first surface 11a side of the single crystal silicon carbide substrate 11 is ground (grinding step). Fig. 9 is a perspective view showing a grinding apparatus 102 used in this embodiment. Note that the X2 axis direction (front-back direction), Y2 axis direction (left-right direction), and Z2 axis direction (vertical direction) used in the following description are perpendicular to each other.
[0061] As shown in Fig. 9, the grinding device 102 includes a base 104 on which each component is mounted. A columnar support structure 106 is provided at the rear end of the base 104. An opening 104a that is long in the X2 axis direction is formed in the upper surface of the base 104. A ball screw type X2 axis movement mechanism 108 is disposed within the opening 104a.
[0062] The X2-axis moving mechanism 108 includes an X2-axis moving table (not shown) and moves the X2-axis moving table in the X-axis direction. A first cover 110a is disposed above the X2-axis moving table. A bellows-shaped second cover 110b is connected to the front and rear of the first cover 110a. As a result, the upper part of the X2-axis moving mechanism 108 is covered by the first cover 110a and the second cover 110b. An operation panel 112 used for inputting grinding conditions and the like is provided in front of the opening 104a.
[0063] A chuck table (holding table) 114 used to hold the single crystal silicon carbide substrate 11 is provided above the X2-axis moving table so as to be exposed above the first cover 110a. A part of the upper surface of the chuck table 114 is formed of, for example, a porous material, and functions as a holding surface 114a for holding the single crystal silicon carbide substrate 11. The holding surface 114a has, for example, a shape corresponding to the side surface of a cone, and is connected to a suction source (not shown) such as a vacuum pump via a flow path (not shown) or the like provided inside the chuck table 114.
[0064] The chuck table 114 is connected to a rotation drive source (not shown) such as a motor, and rotates about a rotation axis parallel to the Z2-axis direction or a rotation axis slightly tilted with respect to the Z2-axis direction so that the apex of the holding surface 114a, which corresponds to the apex of the cone, becomes the center of rotation. In addition, the chuck table 114 is moved in the X2-axis direction together with the X2-axis moving table by the above-mentioned X2-axis moving mechanism 108.
[0065] A Z2-axis moving mechanism 116 is provided on the front surface of the support structure 106. The Z2-axis moving mechanism 116 has a pair of Z2-axis guide rails 118 that are generally parallel to the Z2-axis direction, and a Z2-axis moving plate 120 is attached in a slidable manner to the Z2-axis guide rails 118. A nut portion (not shown) constituting a ball screw is provided on the rear surface side (back surface side) of the Z2-axis moving plate 120, and a screw shaft 122 that is generally parallel to the Z2-axis guide rails 118 is rotatably connected to the nut portion.
[0066] A Z2-axis pulse motor 124 is connected to one end of the screw shaft 122. By rotating the screw shaft 122 by the Z2-axis pulse motor 124, the Z2-axis moving plate 120 moves in the Z2-axis direction along the Z2-axis guide rail 118. A support 126 that protrudes forward is provided on the front surface (surface) of the Z2-axis moving plate 120.
[0067] A grinding unit 128 for grinding single crystal silicon carbide substrate 11 is supported on support 126. Grinding unit 128 includes a spindle housing 130 fixed to support 126. A spindle 132 serving as a rotation shaft is housed in spindle housing 130 in a rotatable state.
[0068] The lower end of the spindle 132 is exposed to the outside of the spindle housing 130. A disk-shaped mount 134 is provided at the lower end of the spindle 132. A plurality of holes (not shown) penetrating the mount 134 in the thickness direction are provided on the outer periphery of the mount 134, and a bolt 136 or the like is inserted into each hole. A disk-shaped grinding wheel 138 having approximately the same diameter as the mount 134 is fixed to the lower surface of the mount 134 by the bolt 136 or the like.
[0069] The grinding wheel 138 is provided with a disk-shaped (annular) wheel base 140 (FIG. 10) made of stainless steel, aluminum, or the like. The wheel base 140 has upper and lower surfaces that are generally parallel to each other, and a circular opening is formed in the center, penetrating the wheel base 140 from the upper surface to the lower surface. In addition, a flow path is provided inside the wheel base 140 for supplying liquid (machining liquid) such as pure water downward.
[0070] A plurality of grinding wheels 142, each made of abrasive grains such as diamond or cBN (cubic boron nitride) dispersed in a binder such as resin or metal, are arranged in an annular shape on the underside of the wheel base 140. The type (material) of the binder constituting the grinding wheels 142, the material and size of the abrasive grains, etc. are adjusted according to the required flatness, etc. so that the single crystal silicon carbide substrate 11 can be appropriately ground.
[0071] When grinding the first surface 11a side of the single crystal silicon carbide substrate 11, first, the second surface 11b side of the single crystal silicon carbide substrate 11 is held by the chuck table 114 of the above-mentioned grinding apparatus 102. Specifically, for example, the single crystal silicon carbide substrate 11 is placed on the chuck table 114 so that the tape 21 attached to the second surface 11b of the single crystal silicon carbide substrate 11 is brought into contact with a holding surface 114a of the chuck table 114.
[0072] Then, negative pressure from a suction source is applied to holding surface 114a of chuck table 114. As a result, second surface 11b side of single crystal silicon carbide substrate 11 is held on chuck table 114 via tape 21, and first surface 11a is exposed upward. Before placing single crystal silicon carbide substrate 11 on chuck table 114, tape 21 may be cut along the outer edge of single crystal silicon carbide substrate 11 to separate single crystal silicon carbide substrate 11 from frame 23.
[0073] After second surface 11b side of single crystal silicon carbide substrate 11 is held by chuck table 114, grindstone 142 is brought into contact with exposed first surface 11a side of single crystal silicon carbide substrate 11 to grind single crystal silicon carbide substrate 11. Fig. 10 is a perspective view showing a state in which single crystal silicon carbide substrate 11 is ground.
[0074] Specifically, first, the X2-axis moving mechanism 108 is operated to move the chuck table 114 to directly below the grinding wheel 138. Next, the chuck table 114 and the grinding wheel 138 are rotated in a predetermined direction at a predetermined rotation speed. The rotation speed of the chuck table 114 is, for example, 10 rpm to 300 rpm, and the rotation speed of the grinding wheel 138 is, for example, 1000 rpm to 7000 rpm. However, the rotation speeds of the chuck table 114 and the grinding wheel 138 are not limited to these.
[0075] Then, while supplying liquid (working liquid) to single crystal silicon carbide substrate 11 on chuck table 114 through a flow path or the like of wheel base 140, grinding wheel 138 is lowered at a predetermined speed so as to press grindstone 142 against first surface 11a side of single crystal silicon carbide substrate 11. Thereby, as shown in Fig. 10, first surface 11a side of single crystal silicon carbide substrate 11 is machined by grindstone 142 to make single crystal silicon carbide substrate 11 thinner.
[0076] The speed at which the grinding wheel 138 is lowered is, for example, 0.1 μm / s to 5.0 μm / s, and the amount of liquid supplied is, for example, 1.0 L / min to 10.0 L / min. However, the speed at which the grinding wheel 138 is lowered and the amount of liquid supplied are not limited to these. When the single crystal silicon carbide substrate 11 has been processed to a predetermined finishing thickness, the lowering of the grinding wheel 138 is stopped, and grinding of the single crystal silicon carbide substrate 11 is completed.
[0077] In the method for processing a single crystal silicon carbide substrate according to this embodiment, when the single crystal silicon carbide substrate 11 is irradiated with a pulsed laser beam 31, the intended irradiation area 46a of the pulsed laser beam 31 is moved so that the irradiated area 11c of the pulsed laser beam 31 partially overlaps, and a portion 11d including the irradiated area 11c of the single crystal silicon carbide substrate 11 is heated by irradiation with the pulsed laser beam 31, whereby the heated portion 11d is peeled off and removed from the remaining portion 11e of the single crystal silicon carbide substrate 11.
[0078] Therefore, the amount (thickness) to be removed by subsequent grinding can be reduced, and wear of the grindstone 142 can be suppressed. Moreover, the size of the portion 11d to be removed of the single crystal silicon carbide substrate 11 can be easily adjusted by simply changing the conditions for irradiating the pulse laser beam 31. That is, even when the amount to be removed is small (when the thickness to be removed is small), the method for processing a single crystal silicon carbide substrate according to the present embodiment can be employed.
[0079] Furthermore, because the heated portion 11d of the single crystal silicon carbide substrate 11 is naturally peeled off due to the effect of heating caused by the irradiation of the pulsed laser beam 31, it is not necessary to apply a force for peeling to the single crystal silicon carbide substrate 11 to peel off the heated portion 11d after the irradiation of the pulsed laser beam 31. Therefore, the cost required for processing can be kept low compared to the conventional method that requires the application of force after the irradiation of the laser beam.
[0080] The present invention is not limited to the above-described embodiment, and can be modified in various ways. For example, in the above-described embodiment, the single-crystal silicon carbide substrate 11 is processed using both the laser processing device 2 and the grinding device 102, but the single-crystal silicon carbide substrate 11 may be processed using a composite device having both the functions of the laser processing device 2 and the grinding device 102.
[0081] In the above embodiment, an example in which the entire first surface 11a side of the single crystal silicon carbide substrate 11 is processed has been described, but the present invention is also effective in the case of processing only a part of the single crystal silicon carbide substrate 11. For example, it is also possible to irradiate the pulsed laser beam 31 only to the area on the first surface 11a side located opposite the device area, and then grind only the area on the first surface 11a side irradiated with the pulsed laser beam 31. In this case, a disk-shaped thin plate portion and an annular thick plate portion surrounding the thin plate portion are formed.
[0082] In addition, the structures, methods, and the like according to the above-described embodiments and modifications can be implemented without departing from the scope of the present invention. [Explanation of symbols]
[0083] 11: Single crystal silicon carbide substrate 11a: First side 11b: Second side 11c: Irradiated area 11d: Part 11e: Part 13a: First Orientation Flat 13b: Second Orientation Flat 15:c-axis 17: Perpendicular 19 :c side 21: Tape 23: Frame 31: Pulsed laser beam 2: Laser processing equipment 4: Base 6: Horizontal movement mechanism 8: Y1 axis guide rail 10: Y1 axis moving plate 12: Screw shaft 14: Y1 axis stepper motor 16: X1 axis guide rail 18: X1 axis moving plate 20: Screw shaft 22: X1 axis stepper motor 24: Table base 26: Chuck table 26a: Holding surface 28: Clamp 30:Support structure 32: Vertical movement mechanism 34: Z1 axis guide rail 36: Z1 axis moving plate 38: Z1 axis stepper motor 40: Support 42: Laser beam irradiation unit 44: Housing 46: Irradiation head 46a: Area to be irradiated 48: Camera 50: Touch screen 52: Control unit 102: Grinding equipment 104: Foundation 104a: Opening 106 :Support structure 108:X2 axis movement mechanism 110a: First cover 110b: 2nd cover 112: Operation panel 114: Chuck table 114a: Holding surface 116:Z2 axis movement mechanism 118: Z2 axis guide rail 120: Z2 axis moving plate 122: Screw shaft 124: Z2 axis stepper motor 126 :Support 128: Grinding unit 130: Spindle housing 132: Spindle 134: Mount 136: Bolt 138: Grinding wheel 140: Wheel base 142: Grindstone
Claims
1. A method for processing a single-crystal silicon carbide substrate, the method being used when processing a single-crystal silicon carbide substrate having a first surface and a second surface located opposite to the first surface, the single-crystal silicon carbide substrate having a c-axis intersecting the first surface and the second surface, the method comprising: a laser beam irradiation step of irradiating the first surface side of the single crystal silicon carbide substrate with a pulsed laser beam having a wavelength of 9 μm to 11 μm; a grinding step of grinding the single crystal silicon carbide substrate by rotating a grinding wheel including a grinding wheel and bringing the grinding wheel into contact with the first surface side of the single crystal silicon carbide substrate irradiated with the pulsed laser beam, a first surface of the single crystal silicon carbide substrate that is irradiated with the pulsed laser beam and a second surface of the single crystal silicon carbide substrate that is irradiated with the pulsed laser beam are moved on the first surface so that an irradiated area on the first surface of the single crystal silicon carbide substrate that is irradiated with the pulsed laser beam next overlaps with an irradiated area on the first surface of the single crystal silicon carbide substrate that is irradiated with the pulsed laser beam; and a portion of the single crystal silicon carbide substrate that includes the irradiated area is heated by irradiating the single crystal silicon carbide substrate with the pulsed laser beam, thereby peeling and removing the heated portion from the remaining portion of the single crystal silicon carbide substrate.
2. 2. The method for processing a single crystal silicon carbide substrate according to claim 1, wherein in the laser beam applying step, the single crystal silicon carbide substrate is irradiated with the pulsed laser beam under conditions such that the depth of the portion is less than 30 μm from the first surface.
3. the second surface of the single crystal silicon carbide substrate has a device region including a plurality of devices and a peripheral excess region surrounding the device region; In the laser beam irradiation step, the pulse laser beam is irradiated onto a region of the first surface side located on an opposite side to the device region of the single crystal silicon carbide substrate; 3. The method for processing a single crystal silicon carbide substrate according to claim 1, wherein in the grinding step, a region on the first surface side of the single crystal silicon carbide substrate is ground to form a disk-shaped thin plate portion and an annular thick plate portion surrounding the thin plate portion.
Citation Information
Patent Citations
Manufacture of semiconductor wafer
JP1999067700A
Manufacture of semiconductor wafer
JP1999067777A
Method for grinding back side of semiconductor substrate
JP2009123983A
POLYCRYSTALLINE SiC WAFER GENERATING METHOD
JP2017022283A
Wafer thinning method
JP2017028072A