Spraying System

The described spraying system addresses nozzle clogging and sagging issues by optimizing polymer cement mortar composition and spraying conditions, enabling efficient adhesion to steel materials for large-scale applications.

JP7596037B2Active Publication Date: 2024-12-09TAIHEIYO MATERIALS CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021059514
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2024-12-09
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Existing mortar spraying methods, such as using a mortar gun or pump, face challenges with nozzle clogging and sagging when applying polymer cement mortar, especially on steel materials, and require adjustments for different materials and conditions.

Method used

A spraying system with specific particle size and content of fine aggregate in polymer cement mortar, combined with controlled discharge rate and air pressure, ensures effective adhesion to steel materials without clogging or sagging.

Benefits of technology

The system provides a polymer cement mortar spraying that prevents nozzle clogging and sagging, ensuring sufficient adhesion to steel materials, allowing efficient large-scale application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596037000001
    Figure 0007596037000001
  • Figure 0007596037000002
    Figure 0007596037000002
Patent Text Reader

Abstract

To provide a spray system of polymer cement mortar capable of securing a sufficient adhesive strength for a steel material without nozzle clogging or dripping when spraying.SOLUTION: A spray system includes a mortar supply apparatus that supplies polymer cement mortar, and an air supply apparatus that supplies a compressed air. The polymer cement mortar is a polymer cement mortar containing cement, fine aggregate, a polymer for cement, and water. An content of the fine aggregate is 120 to 470 pts.mass with respect to 100 pts.mass of the cement. A particle size of the fine aggregate is such that a mass ratio of particles having a particle size of 0.09 mm or more and less than 0.6 mm is 30 mass% or more with respect to the total amount of the fine aggregate. A discharge rate of the polymer cement mortar supplied from the mortar supply apparatus is 0.5 to 2.8 L / min, and an air pressure of a compressed air supplied from the air supply apparatus is 0.15 to 0.7 MPa.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a spray system. [Background technology]

[0002] In bridges and other structures, composite decks, in which steel plates and concrete are integrated, are sometimes used instead of conventional concrete decks. However, in composite decks, the steel plate and concrete sometimes have poor adhesion, and there is a risk of slippage between them. For this reason, in composite decks, anti-slip devices are installed to integrate the steel plate and concrete.

[0003] However, even if the slippage between the steel plate and the concrete can be suppressed, when fine cracks occur due to deterioration of the concrete, moisture and salt may penetrate into the concrete, causing water retention on the surface of the steel plate, which may result in corrosion of the steel plate. Therefore, polymer cement mortars have been developed that aim to improve the integrity of the steel plate and the concrete while protecting the steel plate from rust and corrosion caused by water (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-158314 A Summary of the Invention [Problem to be solved by the invention]

[0005] At mortar construction sites, mortar guns are used for spraying mortar in thin layers, as this method prioritizes the mobility of workers. However, this method results in a small spray area per hour, making it unsuitable for large-scale construction.

[0006] One way to increase efficiency is to use a mortar pump. However, when using a mortar pump, clogging and dripping are likely to occur at the nozzle if the mortar has a high polymer concentration to improve adhesion. On the other hand, unless the mortar has a polymer concentration above a certain level, it is difficult to ensure adhesion to steel materials. In addition, when spraying mortar using a pump, the spraying conditions differ depending on the material, so it is necessary to adjust both the material to be sprayed and the spraying conditions.

[0007] Therefore, an object of the present invention is to provide a polymer cement mortar spraying system that is free from nozzle clogging or dripping during spraying and can ensure sufficient adhesive strength even to steel materials. [Means for solving the problem]

[0008] As a result of extensive research into the above-mentioned problems, the inventors have discovered that by adjusting the particle size and content of fine aggregate in polymer cement mortar, and by adjusting the amount of mortar discharged and the amount of compressed air used during spraying, it is possible to create a spraying system with excellent spraying properties.

[0009] That is, the present invention is as follows. [1] A spraying system comprising a mortar supplying device for supplying polymer cement mortar and an air supplying device for supplying compressed air, wherein the polymer cement mortar is a polymer cement mortar containing cement, fine aggregate, a polymer for cement, and water, the content of the fine aggregate is 120 to 470 parts by mass per 100 parts by mass of cement, the particle size of the fine aggregate is such that the mass ratio of particles having a particle size of 0.09 mm or more and less than 0.6 mm relative to the total amount of the fine aggregate is 30 mass% or more, the discharge rate of the polymer cement mortar supplied from the mortar supplying device is 0.5 to 2.8 L / min, and the air pressure of the compressed air supplied from the air supplying device is 0.15 to 0.7 MPa. [2] The spraying system according to [1], wherein the content of the cement polymer is 5 to 37 parts by mass per 100 parts by mass of cement. [3] The spraying system according to [1] or [2], wherein the polymer cement mortar further contains a fast-hardening admixture comprising calcium aluminate and gypsum. [4] The spraying system according to any one of [1] to [3], wherein the polymer cement mortar further contains fibers. [5] A spraying system according to any one of [1] to [4], wherein the water content is 25 to 50 parts by mass per 100 parts by mass of cement. [6] A spraying system according to any one of [1] to [5], which is for use against steel materials. Effect of the Invention

[0010] According to the present invention, it is possible to provide a polymer cement mortar spraying system that is free from nozzle clogging and dripping during spraying and ensures sufficient adhesive strength even to steel materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, one embodiment of the present invention will be described in detail.

[0012] The spraying system of this embodiment includes a mortar supplying device that supplies polymer cement mortar, and an air supplying device that supplies compressed air.

[0013] [Spray system] The mortar supplying device may be any device capable of supplying polymer cement mortar, such as a squeeze pump or a piston pump. The polymer cement mortar is sent from the mortar supplying device to a pressure feed hose.

[0014] The discharge rate of the polymer cement mortar supplied from the mortar supplying device is 0.5 to 2.8 L / min. If the discharge rate is outside the above range, the spraying characteristics such as the rebound of the mortar and clogging of the nozzle are deteriorated. From the viewpoint of further improving the spraying characteristics, the discharge rate is preferably 0.8 to 2.5 L / min, more preferably 1.0 to 2.0 L / min, and further preferably 1.2 to 1.8 L / min. The discharge rate can be controlled by adjusting the discharge pressure of the mortar supplying device.

[0015] The pressure hose is not particularly limited as long as it is a pressure-resistant hose. The length of the pressure hose can be adjusted appropriately depending on the distance to the construction site. From the viewpoint of further reducing the rebound of mortar, the length of the pressure hose is preferably 0.5 to 20 m, more preferably 1 to 15 m, and even more preferably 2 to 10 m. The inner diameter of the pressure hose is preferably 10 to 55 mm, more preferably 15 to 40 mm, and even more preferably 18 to 32 mm. A plurality of pressure hoses may be connected together.

[0016] The pressure feed hose is provided with a spray nozzle at the end in the direction of discharging the polymer cement mortar. The length of the spray nozzle is preferably 10 to 50 cm, more preferably 15 to 40 cm, and even more preferably 20 to 30 cm. The inner diameter of the spray nozzle is preferably 5 to 30 mm, more preferably 6 to 20 mm, and even more preferably 6 to 10 mm. If the length and inner diameter of the spray nozzle are within the above ranges, clogging of the nozzle with mortar can be further reduced.

[0017] The air supply device is connected to a connecting member such as a Y-shaped pipe installed between the mortar supply device and the spray nozzle, and supplies compressed air from a route different from that of the polymer cement mortar. The connecting member may be installed between a plurality of connected pressure-transfer hoses, or may be installed at the connection between the pressure-transfer hose and the spray nozzle. The connecting member is preferably installed at the connection between the pressure-transfer hose and the spray nozzle, from the viewpoint of more efficient use of compressed air and further suppression of mortar dripping and nozzle clogging. The air supply device may be any device capable of delivering compressed air, and may be, for example, an air compressor.

[0018] The compressed air supplied from the air supply device has a pressure of 0.15 to 0.7 MPa. If the air pressure is outside this range, there is a risk that mortar may adhere to the inside of the spray nozzle or that the sprayed mortar may rebound. From the viewpoint of providing even better spraying characteristics, the air pressure is preferably 0.18 to 0.6 MPa, and more preferably 0.2 to 0.5 MPa.

[0019] The spraying system of this embodiment can be suitably used as a spraying system for steel materials. In this specification, "for steel materials" refers to a spraying system that has an adhesion strength of 3N / mm based on the adhesion test described later. 2 The term "steel" refers to iron and steel used as industrial materials for civil engineering, construction, etc., and includes ordinary steel, special steel with various elements added, stainless steel, and steel materials with chemically or physically surface-treated surfaces.

[0020] [Polymer cement mortar] The polymer cement mortar according to the present embodiment contains cement, fine aggregate, a polymer for cement, and water.

[0021] Various types of cement can be used, including, for example, various Portland cements such as ordinary, early strength, super early strength, low heat and moderate heat; mixed cements containing blast furnace slag, fly ash or silica fume; ecocement, etc. As the cement, early strength Portland cement is preferable from the viewpoint of further increasing the initial strength development. One type of cement may be used alone, or two or more types may be used in combination.

[0022] The fine aggregate is not particularly limited in type as long as the grain size satisfies the requirements described below, and examples thereof include river sand, silica sand, crushed sand, kansui stone, limestone sand, slag aggregate, etc. These fine aggregates may be used alone or in combination of two or more kinds.

[0023] The content of the fine aggregate is 120 to 470 parts by mass relative to 100 parts by mass of cement. If the content of the fine aggregate is outside the above range, it becomes difficult to achieve both good workability and high adhesion to the steel plate. From the viewpoint of easily obtaining better workability and high adhesion to the steel plate, the content of the fine aggregate is preferably 150 to 400 parts by mass, more preferably 180 to 350 parts by mass, and further preferably 200 to 300 parts by mass relative to 100 parts by mass of cement.

[0024] The grain size of the fine aggregate is such that the mass ratio of particles having a particle size of 0.09 mm or more and less than 0.6 mm is 30% by mass or more relative to the total amount of the fine aggregate. If the mass ratio of particles having a particle size of 0.09 mm or more and less than 0.6 mm is outside the above range, the spraying characteristics such as mortar rebound and nozzle clogging are reduced. From the viewpoint of further improving the spraying characteristics, the mass ratio of particles having a particle size of 0.09 mm or more and less than 0.6 mm is preferably 50% by mass or more relative to the total amount of the fine aggregate, more preferably 80% by mass or more, and even more preferably 90% by mass or more. The upper limit of the mass ratio of particles having a particle size of 0.09 mm or more and less than 0.6 mm may be 100% by mass or less relative to the total amount of the fine aggregate, or may be 97% by mass or less.

[0025] The maximum particle size of the fine aggregate is preferably less than 3 mm, more preferably less than 2.7 mm, and even more preferably less than 2.5 mm. If the maximum particle size of the fine aggregate is within the above range, the spraying characteristics and the adhesive strength are further improved.

[0026] In this specification, the particle size of fine aggregate is determined by sieving the entire amount of fine aggregate, and fine aggregate passing through a 2.5 mm sieve is defined as particles having a particle size of less than 2.5 mm, and fine aggregate passing through a 0.6 mm sieve and remaining on a 0.09 mm sieve is defined as particles having a particle size of 0.09 mm or more and less than 0.6 mm.

[0027] The polymer for cement is preferably a polymer specified in JIS A 6203:2015 "Polymer dispersions and re-emulsified powdered resins for cement admixture". Examples of such polymers for cement include polymer dispersions and re-emulsified powdered resins. Examples of polymer dispersions include synthetic rubbers such as styrene butadiene rubber (SBR); natural rubbers; rubber asphalts; ethylene vinyl acetates; acrylic esters; and resin asphalts. Among them, the polymer dispersions are preferably synthetic rubbers, ethylene vinyl acetates, and acrylic esters, and more preferably synthetic rubber latex, polyacrylic esters, and ethylene vinyl acetates. Examples of re-emulsified powdered resins include synthetic rubbers such as styrene butadiene rubber; acrylic esters; ethylene vinyl acetates; vinyl acetate / vinyl versatate esters; vinyl acetate / vinyl versatate / acrylic esters. As the polymer for cement, a polymer dispersion may be used, a re-emulsified powdered resin may be used, or a polymer dispersion and a re-emulsified powdered resin may be used in combination.

[0028] Among the polymers for cement, a polymer dispersion and / or a re-emulsified powder resin of styrene-butadiene rubber is preferred from the viewpoint of further improving adhesion to concrete and steel materials. Styrene-butadiene rubber is a type of synthetic rubber obtained by copolymerizing styrene and butadiene, and the quality can be appropriately adjusted by adjusting the styrene content and the amount of vulcanization. For cement admixture, those with a bound styrene content of 50 to 70 mass% are often used from the viewpoint of improving stability and adhesion. The polymers for cement may be used alone or in combination of two or more.

[0029] The content of the polymer for cement is preferably 5 to 37 parts by mass, more preferably 10 to 34 parts by mass, and even more preferably 15 to 33 parts by mass, in terms of solid content, relative to 100 parts by mass of cement. If the content of the polymer for cement is within the above range, better workability and higher adhesion to concrete and steel plates are likely to be obtained.

[0030] The water is not particularly limited. The content of water is preferably 25 to 50 parts by mass, more preferably 28 to 45 parts by mass, and most preferably 30 to 42 parts by mass, relative to 100 parts by mass of cement. If the content of water is within the above range, it is easier to ensure fluidity, and it is easier to suppress the occurrence of material separation, the increase in shrinkage of the hardened body, and the decrease in early strength development.

[0031] The polymer cement mortar according to the present embodiment may contain a rapid-hardening admixture made of calcium aluminates and gypsums. From the viewpoint of ensuring initial strength development, the content of the rapid-hardening admixture is preferably 10 to 65 parts by mass, more preferably 15 to 60 parts by mass, and even more preferably 20 to 55 parts by mass, per 100 parts by mass of cement.

[0032] The mass ratio of calcium aluminates to gypsums in the fast-setting admixture ([mass of calcium aluminates]:[mass of gypsums]) is preferably 3:7 to 7:3, and more preferably 4:6 to 6:4. When the mass ratio of calcium aluminates to gypsums in the fast-setting admixture is within the above range, the spraying characteristics are likely to be improved, and the adhesive strength is likely to be secured at an early stage.

[0033] Calcium aluminates are classified as C3A, C2A, C, where CaO is C, Al2O3 is A, Na2O is N, and Fe2O3 is F. 12 Calcium aluminate with a mineral composition indicated as A7, CA, or CA2, calcium aluminoferrite indicated as C4AF, calcium aluminate with halogen as a solid solution or as a substitute, C3A3·CaF2, etc. 11 A general term for calcium haloaluminates including calcium fluoroaluminates designated as A7·CaF2, calcium sodium aluminates designated as C8NA3 or C3N2A5, calcium lithium aluminate, alumina cement, and calcium sulfoaluminates designated as C3A3·CaSO4. These calcium aluminates can be crystalline, amorphous, or a mixture of amorphous and crystalline. The calcium aluminates may be used alone or in combination of two or more. From the viewpoint of further improving early strength development, the fineness of calcium aluminates is set to 3000 cm2 in terms of Blaine specific surface area. 2 / g or more, and 2 / g or more. The fineness of calcium aluminates is preferably 8000 cm2 in terms of Blaine specific surface area. 2 It is preferable that the molecular weight is not more than 1 / g.

[0034] Examples of gypsum include anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum. As the gypsum, anhydrous gypsum is preferable from the viewpoint of further improving strength development. One type of gypsum may be used alone, or two or more types may be used in combination. The fineness of the gypsum is preferably 4500 cm2 in terms of Blaine specific surface area from the viewpoint of further improving long-term strength development. 2 / g or more, and 2 / g or more. The fineness of the gypsum is preferably 15,000 cm in terms of Blaine specific surface area. 2 It is preferable that the molecular weight is not more than 1 / g.

[0035] The polymer cement mortar according to the present embodiment may contain a lightweight aggregate. The lightweight aggregate is not particularly limited, and examples thereof include perlite, which is an inorganic expandable aggregate obtained by firing and expanding obsidian, perlite, etc., fly ash balloons generated in thermal power plants, and expanded glass particles (glass balloons). It is preferable to use a lightweight aggregate having a particle size of less than 5 mm (passing a 5 mm sieve) that is usually used. One type of lightweight aggregate may be used alone, or two or more types may be used in combination. For example, the lightweight aggregate preferably has a bulk density (kg / L) of 0.1 to 0.8, and more preferably 0.15 to 0.6. If the bulk density of the lightweight aggregate is within the above range, the effect of weight reduction is easily obtained, the fluidity of the mortar is not easily reduced, and dripping when sprayed can be suppressed.

[0036] The content of the lightweight aggregate is preferably 1 to 25 parts by mass, more preferably 1.5 to 15 parts by mass, and even more preferably 2 to 10 parts by mass, relative to 100 parts by mass of cement. If the content of the lightweight aggregate is within the above range, better workability is likely to be obtained when the mortar is made.

[0037] The polymer cement mortar according to the present embodiment may contain a water reducing agent. The water reducing agent includes a high-performance water reducing agent, a high-performance AE water reducing agent, an AE water reducing agent, and a superplasticizer. Examples of such water reducing agents include those specified in JIS A 6204:2011 "Chemical admixtures for concrete". Examples of the water reducing agent include polycarboxylic acid-based water reducing agents, naphthalenesulfonic acid-based water reducing agents, ligninsulfonic acid-based water reducing agents, melamine-based water reducing agents, and acrylic-based water reducing agents. Among these, naphthalenesulfonic acid-based water reducing agents are preferred. The water reducing agents may be used alone or in combination of two or more types.

[0038] The content of the water reducing agent is preferably 0.5 to 7.5 parts by mass, more preferably 1 to 5 parts by mass, and most preferably 1.5 to 3 parts by mass, relative to 100 parts by mass of cement. If the content of the water reducing agent is within the above range, better workability is easily obtained when the mortar is made, and the compressive strength is also easily improved.

[0039] The polymer cement mortar according to the present embodiment may contain a setting retarder. By containing a setting retarder, it is easy to ensure the working time even when the mixing temperature of the polymer cement mortar is high in summer or the like. Examples of setting retarders include organic acids or salts thereof such as citric acid, gluconic acid, malic acid, and tartaric acid; boric acid, borates such as sodium borate, phosphates, alkali metal carbonates, and alkali metal bicarbonates; and sugars. Among these, citric acid, citrates, tartaric acid, tartrates, and alkali metal carbonates are preferred. The setting retarder may be in the form of a powder or a liquid (for example, an aqueous solution, an emulsion, or a suspension). The setting retarder may be used alone or in combination of two or more types.

[0040] The content of the retarder is preferably 0.1 to 7.5 parts by mass, more preferably 0.3 to 5 parts by mass, and most preferably 0.5 to 3.5 parts by mass, relative to 100 parts by mass of cement. If the content of the retarder is within the above range, the pot life is further ensured and the early strength development is less likely to decrease.

[0041] The polymer cement mortar according to the present embodiment may contain fibers. Examples of the fibers include organic fibers such as cellulose fibers, vinylon fibers, polypropylene fibers, nylon fibers, and acrylic fibers; steel fibers; and inorganic fibers such as glass fibers. From the viewpoint of better dispersibility, the fibers are preferably organic fibers, and cellulose fibers and vinylon fibers are more preferable. One type of fiber may be used alone, or two or more types may be used in combination.

[0042] The length of the fibers is preferably 0.1 to 10 mm, more preferably 0.1 to 5 mm, and even more preferably 0.1 to 0.8 mm. If the length of the fibers is within the above range, the dispersibility in the polymer cement mortar is further improved.

[0043] The content of the fibers is preferably 0.01 to 5 parts by mass, more preferably 0.03 to 3 parts by mass, and even more preferably 0.05 to 2.5 parts by mass, relative to 100 parts by mass of cement. When the content of the fibers is within the above range on a mass basis, the spraying characteristics are further improved, and good toughness is likely to be obtained when hardened.

[0044] The polymer cement mortar according to the present embodiment may contain various admixtures (materials) within the scope of not impairing the effects of the present invention. Examples of the admixtures (materials) include defoamers, waterproofing agents, rust inhibitors, shrinkage reducing agents, thickeners, water retention agents, pigments, water repellents, efflorescence prevention agents, expansion agents, and accelerators.

[0045] The polymer cement mortar according to the present embodiment can be prepared using a kneading tool similar to that used for ordinary polymer cement mortar, and is not particularly limited. Examples of kneading tools that can be used include a Hobart mixer, a hand mixer, a tilting mixer, and a forced twin-shaft mixer.

[0046] According to the spraying system of the present embodiment, it is possible to spray polymer cement mortar that is sufficiently adhesive to steel materials without causing nozzle clogging, dripping, or mortar rebound during spraying. Therefore, such a spraying system can quickly carry out wide-area and uniform construction when repairing and reinforcing concrete structures, roads, etc., and steel-concrete composite structures using steel plates, etc. EXAMPLES

[0047] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto.

[0048] [material] Cement: High early strength Portland cement Fast-hardening admixture: Calcium aluminate (Blaine specific surface area 5500cm 2 / g) and anhydrous gypsum (Blaine specific surface area 6000 cm 2 / g) mass ratio of 6:4 ·Fine aggregate: Silica sand (maximum particle size 2.5mm or less) Lightweight aggregate: Perlite (bulk density 0.23kg / L) ·Cement polymer: SBR emulsion Water reducing agent: Naphthalene sulfonic acid water reducing agent Fiber: Cellulose fiber (fiber length 0.5 mm) · Retarder: Citric acid Water: Tap water

[0049] [Mixture design of polymer cement mortar composition] The mix was designed so that, per 100 parts by mass of cement, the fine aggregate and cement polymer (converted into solids) were used in the proportions shown in Table 1, with 45 parts by mass of fast-hardening admixture, 5 parts by mass of lightweight aggregate, 2 parts by mass of water-reducing agent, 1 part by mass of setting retarder, and 1 part by mass of fiber.

[0050] [Preparation of polymer cement mortar] In a 20°C environment, a polymer for cement (polymer dispersion) was added to a 10 L cylindrical container, and each material of the polymer cement mortar composition designed according to the mix ratio shown in Table 1 and water were added, and the mixture was kneaded for 60 seconds with a hand mixer to produce about 3 L of polymer cement mortar. The water content was 40 parts by mass per 100 parts by mass of cement.

[0051] [Table 1]

[0052] [Spraying polymer cement mortar] The mixed polymer cement mortar was pressure-fed using a squeeze pump with a hopper (power supply: 100 V, power consumption: 0.4 kW, pumping distance: 5 m, inner diameter of pump hose: 25 mm) after adjusting the mortar discharge rate shown in Table 1. A Y-shaped pipe was installed at the connection between the spray nozzle (nozzle length: 30 cm, nozzle diameter: 8 mm) and the pump hose, and compressed air shown in Table 1 was sent from a compressor to spray the mortar.

[0053] [Evaluation method] Each item was evaluated by the following methods. The evaluation results are shown in Table 2. Spray properties Polymer cement mortar was sprayed onto a vertically placed wooden panel (length 900 x width 1800 x height 12 mm) and the spraying properties were evaluated. Those that could be sprayed without clogging of the nozzle and with little mortar rebound were rated as good (○), and those that could be sprayed without dripping up to a thickness of 5 mm were rated as even better (◎). Anything other than that was rated as poor (×). Adhesion strength A zinc-rich paint-coated steel plate (300 mm length x 300 mm width x 6 mm height) with a plastic formwork with inner dimensions of 40 mm x 40 mm x 5 mm was placed vertically, polymer cement mortar was sprayed to a thickness of 5 mm, and the material was cured in air at 20°C for up to 7 days. The bond strength of the attached polymer cement mortar was then measured using a simple tensile tester. The bond strength was 3.0 N / mm 2 The above was judged to be good.

[0054]

Table 2

Claims

1. A spraying system comprising a mortar supplying device for supplying polymer cement mortar and an air supplying device for supplying compressed air, The polymer cement mortar contains cement, fine aggregate, a polymer for cement, and water, The content of the fine aggregate is 120 to 470 parts by mass relative to 100 parts by mass of the cement, The particle size of the fine aggregate is such that the mass ratio of particles having a particle size of 0.09 mm or more and less than 0.6 mm is 30 mass% or more relative to the total amount of the fine aggregate, the polymer cement mortar is supplied from the mortar supply device at a discharge rate of 0.5 to 1.8 L / min; A spraying system, wherein the air pressure of the compressed air supplied from the air supply device is 0.15 to 0.5 MPa.

2. 2. The spraying system according to claim 1, wherein the content of the polymer for cement is 5 to 37 parts by mass per 100 parts by mass of the cement.

3. 3. The spraying system according to claim 1 or 2, wherein the polymer cement mortar further comprises a fast-setting admixture comprising calcium aluminate and gypsum.

4. The spraying system of any one of claims 1 to 3, wherein the polymer cement mortar further comprises fibers.

5. The spraying system according to any one of claims 1 to 4, wherein the content of the water is 25 to 50 parts by mass per 100 parts by mass of the cement.

6. The spraying system according to any one of claims 1 to 5, which is for use against steel materials.

Citation Information

Patent Citations

  • Spraying method and cement-mortar hardened body

    JP2007205015A

  • Polymer cement mortar composition, polymer cement mortar, and steel concrete composite structure

    JP2020158314A