Polyurethane urea resin solution and paints, printing inks, coating agents and adhesives using the same
The polyurethane urea resin solution with a tailored molecular structure addresses adhesive weaknesses and environmental concerns, offering strong, stable adhesion to polyolefin, polyester, and nylon substrates without harmful substances, suitable for paints, inks, and adhesives.
Patent Information
- Application Number
- JP2020095398
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-25
- Filing Date
- 2020-06-01
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2040-06-01
AI Technical Summary
Conventional polyurethane resins lack sufficient adhesive strength to polyolefin base materials and generate harmful substances during disposal, while chlorinated polyolefins limit application base materials and decrease adhesiveness over time due to surface treatments like corona or plasma treatment, and toluene-based solvents face environmental regulation challenges.
A polyurethane urea resin solution with a specific molecular structure and solvent composition, featuring hydroxyl-modified polyolefin, polyisocyanate, and chain extender, providing excellent adhesion to polyolefin, polyester, and nylon substrates without harmful substances, and maintaining solution stability.
The solution exhibits excellent adhesion to various plastics, stability, and mechanical strength, avoiding harmful substances and environmental impact, suitable for paints, inks, and adhesives.
Smart Images

Figure 0007596082000001 
Figure 0007596082000002 
Figure 0007596082000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyurethane urea resin solution and a paint, a printing ink, a coating agent and an adhesive using the same. [Background technology]
[0002] Conventionally, polyurethane resins have been used in the fields of paints, printing inks, adhesives (binders), and coating agents due to their excellent durability, chemical resistance, and abrasion resistance. In particular, polyurethane resins have excellent adhesion to substrates such as polyester and nylon, and solvent solutions of polyurethane resins are widely used from the viewpoint of handling and drying. However, polyurethane resins do not have sufficient adhesion to polyolefin substrates such as polyethylene and polypropylene, and chlorinated polyolefin resins are widely used instead for polyolefin substrates. However, chlorinated polyolefin resins do not have sufficient adhesion to substrates such as polyester and nylon, so there is a problem that the substrates to which they can be applied are limited. For the purpose of improving the adhesive strength of polyester, nylon and polyolefin substrates and making them versatile for use with various plastics, it has been proposed to use a mixture of polyurethane and chlorinated polyolefin (see, for example, Patent Document 1) or a urethane-modified product of oxidized chlorinated polyolefin as a binder (see, for example, Patent Document 2). Also, a method has been proposed in which the surface of the substrate is subjected to a corona treatment or plasma treatment to improve the adhesive strength (see, for example, Patent Document 3).
[0003] However, in recent years, environmental issues have come to be emphasized, and there is a strong demand for suppressing the generation of harmful substances in the disposal of used products. The chlorinated polyolefins used in Patent Documents 1 and 2 contain chlorine, and therefore may generate harmful substances during incineration, causing environmental pollution. Furthermore, in the method of subjecting the surface of the substrate to a corona treatment or plasma treatment, there is a problem in that the adhesiveness decreases with the lapse of time after the treatment. Furthermore, toluene is widely used as a solvent for paints, printing inks, adhesives, and coating agents. However, the revision of the Industrial Safety and Health Act has strengthened the regulation of the environmental concentration of toluene, and the demand for solvent systems that do not contain toluene has increased, and more recently, there has been an increasing demand for alcohol-based solvent systems that are more environmentally friendly. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-251594 [Patent Document 2] Japanese Patent Application Publication No. 11-323236 [Patent Document 2] JP 2000-319426 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in consideration of the above problems, and has an object to provide a polyurethane urea resin solution which does not contain harmful substances such as chlorine and toluene, does not impair mechanical strength, exhibits particularly excellent adhesion to plastic (polyolefin, polyester, nylon, etc.) substrates that have not been subjected to corona treatment or plasma treatment, and has excellent solution stability, as well as a paint, printing ink, coating agent, and adhesive using the same. [Means for solving the problem]
[0006] The present inventors have conducted extensive research to achieve the above object, and have arrived at the present invention. That is, the present invention relates to a polyurethane urea resin solution containing a polyurethane urea resin (U) having as essential constituent monomers a hydroxyl-modified polyolefin (A), a polyisocyanate (B), and a chain extender (C) having a number average molecular weight or chemical formula weight of less than 500, and a solvent (S), in which the weight ratio (ethylene:α-olefin) of ethylene, which is the constituent monomer of the hydroxyl-modified polyolefin (A), to an α-olefin having 3 to 8 carbon atoms, is 5:95 to 95:5, the isotacticity of the α-olefin unit chain of the hydroxyl-modified polyolefin (A) is 1 to 50%, and the number average molecular weight of the hydroxyl-modified polyolefin (A) is 1,000 to 6,000; and a paint, printing ink, coating agent, and adhesive containing the polyurethane urea resin solution. Effect of the Invention
[0007] The polyurethane urea resin solution of the present invention, and the paint, printing ink, coating agent, and adhesive using the same do not contain harmful substances such as chlorine and toluene, do not impair mechanical strength, and exhibit particularly excellent adhesion to plastic (polyolefin, polyester, nylon, etc.) substrates that have not been subjected to corona treatment or plasma treatment, and have the effect of excellent solution stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The polyurethane urea resin solution of the present invention contains a polyurethane urea resin (U) having, as essential constituent monomers, a hydroxyl group-modified polyolefin (A), a polyisocyanate (B), and a chain extender (C) having a number average molecular weight or chemical formula weight of less than 500, and a solvent (S).
[0009] <Polyurethane urea resin (U)> In the present invention, the polyurethane urea resin (U) contains a hydroxyl group-modified polyolefin (A), a polyisocyanate (B), and a chain extender (C) having a number average molecular weight or chemical formula weight of less than 500 as essential constituent monomers. In the present invention, the weight ratio (ethylene:α-olefin) of the constituent monomers of the hydroxyl-modified polyolefin (A) between ethylene and an α-olefin having 3 to 8 carbon atoms is 5:95 to 95:5, the isotacticity of the α-olefin unit chain of the hydroxyl-modified polyolefin (A) is 1 to 50%, and the number average molecular weight of the hydroxyl-modified polyolefin (A) is 1,000 to 6,000. In the present invention, by using as (A) a material having a moderate amount of α-olefin structure, a number average molecular weight within the above range, and an isotacticity within the above range, it is possible to provide the molecular structure of the polyurethane urea resin (U) with a portion having high affinity for plastics in moderate units while making the molecular structure of (U) low in crystallinity, and it is presumed that this makes it possible to achieve both adhesion to plastics and solubility in solvents.
[0010] The hydroxyl-modified polyolefin (A) can be obtained by reacting an acid-modified polyolefin (X) in which a polyolefin (A1) having a carbon-carbon double bond is modified with an unsaturated (poly)carboxylic acid (anhydride) (E) with an amino alcohol (G), or by reacting the acid-modified polyolefin (X) with an alkylene oxide.
[0011] The polyolefin (A1) having a carbon-carbon double bond in the present invention contains ethylene and an α-olefin having 3 to 8 carbon atoms as constituent monomers. Examples of the α-olefin include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene. Although two or more types of α-olefins may be used in combination, one type is preferred. Among the above α-olefins, propylene is preferred from the viewpoints of mechanical strength and productivity.
[0012] The weight ratio of ethylene, which is a constituent monomer of the polyolefin (A1) having a carbon-carbon double bond, to an α-olefin having 3 to 8 carbon atoms (ethylene:α-olefin) is 5:95 to 95:5, preferably 10:90 to 60:40, and more preferably 15:85 to 40:60. If the weight ratio (ethylene:α-olefin) is less than 5:95, the adhesiveness is poor, and if it exceeds 95:5, the mechanical strength is poor. The weight ratio (ethylene:α-olefin) is, for example, 1 It can be calculated using H-MNR.
[0013] The (A1) may contain, as a constituent monomer, another monomer other than ethylene and an α-olefin having a carbon number of 3 to 8. In that case, the weight of the other monomer is preferably 10% by weight or less, more preferably 5% by weight or less, and particularly preferably 1% by weight or less, based on the weight of all the monomers constituting (A1). Examples of the other monomers include α-olefins having a carbon number (sometimes abbreviated as C) of 9 to 30 (1-decene, 1-dodecene, etc.), and unsaturated monomers having a carbon number of 4 to 30 other than α-olefins (for example, olefins such as 2-butene and isobutene, and vinyl monomers such as styrene, acrylonitrile, acrylamide, and vinyl acetate).
[0014] The number average molecular weight (hereinafter abbreviated as Mn) of the polyolefin (A1) having a carbon-carbon double bond is preferably 800 to 5,800, and more preferably 800 to 3,800, from the viewpoints of adhesiveness, mechanical strength and solvent solubility.
[0015] In the present invention, Mn is measured by GPC (gel permeation chromatography) under the following conditions. Apparatus: High temperature gel permeation chromatograph ["Alliance GPC V2000", Waters, Inc.] Detector: Refractive index detector Solvent: orthodichlorobenzene Reference material: Polystyrene Sample concentration: 3mg / ml Column stationary phase: PLgel 10μm, MIXED-B 2 columns in series [Manufactured by Polymer Laboratories, Inc.] Column temperature: 135℃
[0016] The number of double bonds in the polyolefin (A1) having a carbon-carbon double bond [the number of carbon-carbon double bonds at the molecular terminals and in the molecular chain of (A1)] per 1,000 carbon atoms is preferably 3 to 30, and more preferably 4 to 20, from the viewpoints of reactivity with the unsaturated (poly)carboxylic acid (anhydride) (E) described below and productivity. The number of double bonds in (A1) is 1 It can be obtained from a spectrum of H-NMR (nuclear magnetic resonance) spectroscopy. That is, the peaks in the spectrum are assigned, and the relative value between the number of double bonds in (A1) and the number of carbon atoms in (A1) is obtained from the integral value derived from the double bonds at 4.5 to 6 ppm of (A1) and the integral value derived from (A1), and the number of double bonds per 1,000 carbons in (A1) is calculated. The number of double bonds in the examples described below was determined according to the above method.
[0017] The isotacticity of the α-olefin unit sequence of the polyolefin (A1) having a carbon-carbon double bond is preferably 1 to 50%, more preferably 5 to 45%, from the viewpoint of adhesion and solvent solubility. The isotacticity of the α-olefin unit sequence of the polyolefin (A1) tends to be directly reflected in the isotacticity of the α-olefin unit sequence of the acid-modified polyolefin (X) and the hydroxyl-modified polyolefin (A) described below. The isotacticity of the α-olefin unit sequence of the polyolefin (A1) having a carbon-carbon double bond tends to be reflected in the isotacticity of the α-olefin unit sequence of the raw material polyolefin (A0) described below, and can be adjusted by the raw material polyolefin (A0) used.
[0018] The isotacticity of the α-olefin unit sequence in the present invention is, for example, 13It can be calculated using C-NMR (nuclear magnetic resonance spectroscopy). In general, it is known that a side chain methyl group is affected by the configuration (meso or racemo) of the methyl groups on both sides (triad), on both sides of the triad (pentad), and on both sides of the pentad (heptad), and peaks are observed at different chemical shifts. The stereoregularity is generally evaluated for the pentad, and the isotacticity in the present invention can also be calculated based on the evaluation of the pentad. That is, when the α-olefin is propylene, 13 Regarding the carbon peaks derived from the side chain methyl groups in propylene obtained by C-NMR, when each pentad peak (H) and a peak derived from the methyl groups in isotactic propylene in which the pentad is formed only of mesostructure (Ha) are taken as the peaks, isotacticity is calculated by the following formula. Isotacticity (%) = [(Ha) / Σ(H)] × 100 (1) In the formula, Ha is the peak height of an isotactic signal (pentads are formed only in the mesostructure), and H is the height of each peak of the pentad.
[0019] An example of a method for producing the polyolefin (A1) having a carbon-carbon double bond in the present invention is a method in which a high molecular weight (preferably Mn of 60,000 to 400,000, more preferably Mn of 80,000 to 250,000) polyolefin (A0) is thermally degraded.
[0020] The thermal degradation method includes a method in which the high molecular weight polyolefin (A0) is thermally degraded (1) in the absence of an organic peroxide, for example, at 300 to 450°C for 0.5 to 10 hours, and (2) in the presence of an organic peroxide [for example, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane], for example, at 180 to 300°C for 0.5 to 10 hours. Of these, the method (1) is preferred from the industrial viewpoint and from the viewpoint of modification properties, since it is easy to obtain a polymer having a larger number of double bonds at the molecular terminals and / or in the molecular chain.
[0021] The weight ratio [ethylene:α-olefin] of ethylene and α-olefin (having 3 to 8 carbon atoms), which are the monomers constituting the above (A1), tends to be maintained the same as the weight ratio [ethylene:α-olefin] of the high molecular weight polyolefin (A0). The higher the thermal degradation temperature and the longer the thermal degradation time, the greater the number of double bonds per 1,000 carbon atoms tends to be. Furthermore, the smaller the Mn of (A0), the higher the thermal degradation temperature, and the longer the thermal degradation time, the smaller the Mn of (A1) tends to be.
[0022] Examples of the unsaturated (poly)carboxylic acid (anhydride) (E) in the present invention include C3-30 (poly)carboxylic acid (anhydride) having one polymerizable unsaturated group. In the present invention, the unsaturated (poly)carboxylic acid (anhydride) means an unsaturated monocarboxylic acid, an unsaturated polycarboxylic acid and / or an unsaturated polycarboxylic acid anhydride. Examples of the unsaturated monocarboxylic acid include aliphatic unsaturated monocarboxylic acids (C3-24, such as acrylic acid, methacrylic acid, α-ethylacrylic acid, crotonic acid, and isocrotonic acid) and alicyclic-containing unsaturated monocarboxylic acids (C6-24, such as cyclohexene carboxylic acid). Examples of the unsaturated poly(2-3 or more) carboxylic acid (anhydride) include unsaturated dicarboxylic acid (anhydride) [aliphatic dicarboxylic acid (anhydride) (C4-24, for example, maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, and anhydrides thereof) and alicyclic ring-containing dicarboxylic acid (anhydride) (C8-24, for example, cyclohexene dicarboxylic acid, cycloheptene dicarboxylic acid, bicycloheptene dicarboxylic acid, methyltetrahydrophthalic acid, and anhydrides thereof)]. (E) may use one type alone, or two or more types in combination. Among (E), from the viewpoint of reactivity with the polyolefin (A1), unsaturated dicarboxylic acid anhydrides are preferred, and maleic anhydride is more preferred.
[0023] The acid-modified polyolefin (X) contains the polyolefin (A1) having a carbon-carbon double bond and an unsaturated (poly)carboxylic acid (anhydride) (E) as constituent monomers. The weight ratio of the constituent monomers (A1) and (E) in the acid-modified polyolefin (X) [(A1):(E)] is preferably 80:20 to 99.5:0.5, and more preferably 90:10 to 99:1, from the viewpoint of the balance between mechanical strength and adhesiveness.
[0024] The acid-modified polyolefin (X) can be produced by reacting a polyolefin (A1) and an unsaturated (poly)carboxylic acid (anhydride) (E) in the presence of a radical initiator (F), if necessary, in a suitable organic solvent [C3 to C18, for example, a hydrocarbon (hexane, heptane, octane, dodecane, benzene, toluene, xylene, etc.), a halogenated hydrocarbon (di-, tri-, or tetrachloroethane, dichlorobutane, etc.), a ketone (acetone, methyl ethyl ketone, di-t-butyl ketone, etc.), and an ether (ethyl-n-propyl ether, di-n-butyl ether, di-t-butyl ether, dioxane, etc.)]. The radical initiator (F) may be a known one, for example, an azo initiator (azobisisobutyronitrile, etc.) or a peroxide initiator (dicumyl peroxide, etc.), with the peroxide initiator being preferred.
[0025] The reaction temperature is preferably 100 to 270°C, more preferably 120 to 250°C, and particularly preferably 130 to 240°C, from the viewpoints of the reactivity between (A1) and (E) and productivity.
[0026] From the viewpoint of the solvent solubility and adhesiveness of the polyurethane urea resin (U), the acid value of the acid-modified polyolefin (X) is preferably 1 to 100 mgKOH / g, more preferably 3 to 75 mgKOH / g, and particularly preferably 5 to 50 mgKOH / g. The acid value here is a value measured according to JIS K0070:1992 by the following procedures (i) to (iii). (i) Dissolve 1 g of (X) in 100 g of xylene adjusted to 100°C. (ii) At the same temperature, titration is performed with 0.1 mol / L potassium hydroxide ethanol solution [product name "0.1 mol / L ethanolic potassium hydroxide solution", manufactured by Wako Pure Chemical Industries, Ltd.] using phenolphthalein as an indicator. (iii) Convert the amount of potassium hydroxide required for the titration into mg to calculate the acid value (unit: mgKOH / g). In addition, the above measurement gives the result that one acid anhydride group is equivalent to one carboxyl group. The acid value can be appropriately adjusted by the number of double bonds in (A1), the weight of (A1), the type of (E), and the weight of (E).
[0027] The Mn of the acid-modified polyolefin (X) is preferably from 900 to 5,900, more preferably from 900 to 5,000, and particularly preferably from 900 to 4,000, from the viewpoints of the solvent solubility and adhesiveness of the polyurethane urea resin (U).
[0028] The isotacticity of the α-olefin unit chain of the acid-modified polyolefin (X) is preferably 1 to 50%, more preferably 5 to 45%, and particularly preferably 10 to 40%, from the viewpoints of the solvent solubility, adhesiveness, and mechanical strength of the polyurethane urea resin (U).
[0029] Examples of the hydroxyl-modified polyolefin (A) in the present invention include a reaction product of the acid-modified polyolefin (X) with an aminoalcohol (G) and a reaction product of the acid-modified polyolefin (X) with an alkylene oxide (hereinafter abbreviated as AO).
[0030] Examples of the amino alcohol (G) include linear alkanolamines, cycloalkanolamines and alkylalkanolamines having 2 to 12 carbon atoms (e.g., 2-aminoethanol, 3-aminopropanol, 1-amino-2-propanol, 2-amino-2-methyl-1-propanol, 4-aminobutanol, 5-aminopentanol, 6-aminohexanol, diethanolamine, di-n- or isopropanolamine, 3-aminomethyl-3,5,5-trimethylcyclohexanol, methylethanolamine and ethylethanolamine), and the like, with 2-aminoethanol being preferred.
[0031] Examples of AO include AOs having a carbon number of 2 to 12 (ethylene oxide, 1,2- or 1,3-propylene oxide, 1,2-, 2,3- or 1,3-butylene oxide, tetrahydrofuran, 3-methyltetrahydrofuran, styrene oxide, α-olefin oxide, etc.), preferably those having a carbon number of 2 to 4, and more preferably ethylene oxide and propylene oxide. The AOs may be used alone or in combination of two or more. The number of moles of AO added is preferably 1 to 10 moles or more, more preferably 1 to 5 moles, and particularly preferably 1 mole, per carboxyl group of the acid-modified polyolefin (X).
[0032] The modification of the acid-modified polyolefin (X) with the aminoalcohol (G) can be carried out by a known method, for example, by adding an excess (for example, 1.1 to 2 times the molar amount or more) of the aminoalcohol to the carboxyl group (carbonyl group in the case of anhydride) of the acid-modified polyolefin (X) to react, and then removing the unreacted aminoalcohol by a method such as distillation. The reaction can be carried out in the presence or absence of an organic solvent. The reaction temperature is preferably 100 to 220°C, more preferably 120 to 200°C. The modification of the acid-modified polyolefin (X) with AO is carried out by a known method. For example, the reaction temperature when ring-opening addition polymerization of AO is preferably 40 to 200° C., more preferably 70 to 160° C. The reaction pressure is preferably −0.1 to 0.5 MPa. The reaction is carried out in the presence of a catalyst as necessary.
[0033] The weight ratio of ethylene and an α-olefin having 3 to 8 carbon atoms (ethylene:α-olefin), which are constituent monomers of the hydroxyl group-modified polyolefin (A), is 5:95 to 95:5, preferably 10:90 to 60:40, and more preferably 15:85 to 40:60. If the weight ratio (ethylene:α-olefin) is less than 5:95, the adhesiveness is poor, and if it exceeds 95:5, the mechanical strength is poor. The weight ratio of ethylene and the α-olefin having 3 to 8 carbon atoms, which are the constituent monomers of the hydroxyl-modified polyolefin (A), can be appropriately adjusted by the ratio of ethylene and the α-olefin having 3 to 8 carbon atoms used in (A0).
[0034] The isotacticity of the α-olefin unit chain of the hydroxyl group-modified polyolefin (A) is 1 to 50%, preferably 5 to 45%. If the isotacticity is less than 1%, the adhesiveness is poor, and if it exceeds 50%, the solvent solubility is poor. The isotacticity of the α-olefin unit sequence of (A) can be appropriately adjusted by the isotacticity of (A0).
[0035] The Mn of the hydroxyl-modified polyolefin (A) is from 1,000 to 6,000, and preferably from 1,000 to 4,000, from the viewpoints of adhesiveness and solvent solubility. Mn of (A) can be appropriately adjusted by controlling Mn of (A1), the type and amount of (E) used, and the reaction between (A1) and (E).
[0036] The hydroxyl value (mgKOH / g) of the hydroxyl-modified polyolefin (A) is preferably 14 to 110, preferably 20 to 100, and more preferably 25 to 80. When the hydroxyl value is 14 or more, the solvent solubility of the polyurethane urea resin (U) tends to be improved, and when it is 110 or less, the adhesion of (U) to a polyolefin film tends to be improved. The hydroxyl value of (A) can be appropriately adjusted by the number of double bonds in (A1), the amount of (A1) used, and the type and amount of (E) used. The acid value (mgKOH / g) of (A) is preferably 0-10, and more preferably 0-5. The hydroxyl value and acid value of (A) are values measured in accordance with JIS K0070-1992.
[0037] In the present invention, the number of hydroxyl groups per molecule of the hydroxyl-modified polyolefin (A) is preferably 1.5 to 2.0, more preferably 1.6 to 2.0, from the viewpoints of the solvent solubility, adhesiveness and mechanical strength of the polyurethane urea resin (U). The number of hydroxyl groups per molecule of the hydroxyl-modified polyolefin (A) can be calculated by the following mathematical formula (1). Number of hydroxyl groups per molecule = Mn A ×OHV / 56100 (1) Mn A : (A) Mn OHV: Hydroxyl value of (A) (mgKOH / g)
[0038] When the polyurethane urea resin (U) uses multiple types of hydroxyl group-modified polyolefins (A), the weight average number of hydroxyl groups in all of the hydroxyl group-modified polyolefins (A) constituting the polyurethane urea resin (U) is preferably 1.5 to 2.0, and more preferably 1.6 to 2.0, from the viewpoints of the solvent solubility, adhesiveness and mechanical strength of the polyurethane urea resin (U).
[0039] The polyurethane urea resin (U) in the present invention contains a hydroxyl group-modified polyolefin (A) as an essential constituent monomer. (A) may be used alone or in combination of two or more kinds.
[0040] The polyurethane urea resin (U) can further contain, in combination with a polyol component, at least one polyol (H) selected from the group consisting of condensation type polyester polyols (H1), polylactone polyols (H2), polycarbonate polyols (H3), polyether polyols (H4) and poly(meth)acrylic polyols (H5). The hydroxyl value (mgKOH / g) of the polyol (H) is preferably from 22 to 225, and more preferably from 28 to 113, from the viewpoint of solvent solubility. The hydroxyl value of (H) is a value measured in accordance with JIS K0070-1992.
[0041] The Mn of the polyol (H) is preferably from 500 to 5,000, and more preferably from 1,000 to 4,000, from the viewpoint of solvent solubility. The number average molecular weight (Mn) of the polyol (H) in the present invention can be measured by gel permeation chromatography (GPC) under the following conditions, for example. Apparatus: "Waters Alliance 2695" [Waters] Column: "Guardcolumn Super HL" (1 piece), "TSKgel A combination of one each of SuperH2000, TSKgel SuperH3000, and TSKgel SuperH4000 (all manufactured by Tosoh Corporation) Sample solution: 0.25% by weight tetrahydrofuran solution Solution injection volume: 10μl Flow rate: 0.6ml / min Measurement temperature: 40℃ Detector: Refractive index detector Reference material: Standard polyethylene glycol
[0042] The condensation type polyester polyol (H1) may be, for example, one obtained by condensing a diol having an Mn of less than 500 with a dicarboxylic acid or an ester-forming derivative thereof [such as an acid anhydride, a lower (C1-4) alkyl ester, or an acid halide].
[0043] Examples of diols having an Mn of less than 500 include aliphatic dihydric alcohols having 2 to 8 carbon atoms [linear diols (ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, etc.) and diols having branched alkyl chains (1,2-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2,2-diethyl-1,3-propanediol, 1,2-, 1,3- or 2,3-butanediol, etc.)]; Examples of the dihydric alcohols include alicyclic group-containing dihydric alcohols [1,4-bis(hydroxymethyl)cyclohexane and 2,2-bis(4-hydroxycyclohexyl)propane, etc.]; aromatic ring-containing dihydric alcohols having 8 to 20 carbon atoms [m- or p-xylylene glycol, bis(hydroxyethyl)benzene, bis(hydroxyethoxy)benzene]; AO adducts of bisphenols (bisphenol A, bisphenol S, bisphenol F, etc.), AO adducts of dihydroxynaphthalene, and bis(2-hydroxyethyl)terephthalate, etc.]. Diols having an Mn of less than 500 may be used alone or in combination of two or more.
[0044] Examples of dicarboxylic acids or their ester-forming derivatives include aliphatic dicarboxylic acids having 2 to 15 carbon atoms [oxalic acid, succinic acid, adipic acid, sebacic acid, glutaric acid, azelaic acid, maleic acid, fumaric acid, etc.], aromatic dicarboxylic acids having 8 to 12 carbon atoms [terephthalic acid, isophthalic acid, etc.], and their ester-forming derivatives [acid anhydrides, lower alkyl esters (dimethyl esters, diethyl esters, etc.), acid halides (acid chlorides, etc.)], etc. One type of dicarboxylic acid may be used alone, or two or more types may be used in combination.
[0045] Specific examples of the condensation type polyester polyol (H1) include polyethylene adipate diol, polybutylene adipate diol, polyhexamethylene adipate diol, polyhexamethylene isophthalate diol, polyneopentyl adipate diol, polyethylene propylene adipate diol, polyethylene butylene adipate diol, polybutylene hexamethylene adipate diol, poly(polyoxytetramethylene) adipate diol, poly(3-methylpentylene adipate) diol, polyethylene azelate diol, polyethylene sebacate diol, polybutylene azelate diol, polybutylene sebacate diol, and polyneopentyl terephthalate diol.
[0046] Among the condensation type polyester polyols (H1), from the viewpoint of adhesiveness and solvent solubility, polyester diols having branched alkyl chains are preferred, polyneopentyl adipate diol and poly(3-methylpentylene adipate) diol are particularly preferred, and poly(3-methylpentylene adipate) diol is most preferred. (H1) may be used alone or in combination of two or more kinds.
[0047] The polylactone polyol (H2) may be one obtained by ring-opening polymerization of lactone monomers (γ-butyrolactone, γ-valerolactone, ε-caprolactone, and mixtures of two or more of these, etc.) using the above-mentioned diol having an Mn of less than 500 as an initiator. Specific examples of the polylactone polyol (H2) include polybutyrolactone diol, polyvalerolactone diol, and polycaprolactone diol. (H2) may be used alone or in combination of two or more.
[0048] The polycarbonate polyol (H3) may be a polycarbonate diol produced by condensing the diol having an Mn of less than 500 with a low molecular weight carbonate compound (for example, a dialkyl carbonate having an alkyl group with 1 to 6 carbon atoms, an alkylene carbonate having an alkylene group with 2 to 6 carbon atoms, and a diaryl carbonate having an aryl group with 6 to 9 carbon atoms) while causing a dealcoholization reaction. One type of (H3) may be used alone, or two or more types may be used in combination.
[0049] Specific examples of the polycarbonate polyol (H3) include polyhexamethylene carbonate diol, polypentamethylene carbonate diol, polytetramethylene carbonate diol, and poly(tetramethylene / hexamethylene) carbonate diol (for example, a diol obtained by condensing 1,4-butanediol and 1,6-hexanediol with a dialkyl carbonate while causing a dealcoholization reaction).
[0050] Examples of the polyether polyol (H4) include the above-mentioned AO adducts having 2 to 12 carbon atoms to the diols having an Mn of less than 500. The AO may be used alone or in combination of two or more types as block copolymers or random copolymers.
[0051] Among the polyether polyols (H4), those having a branched alkyl chain are preferred from the viewpoint of solvent solubility, i.e., those using as a raw material a diol having a branched alkyl chain among diols having an Mn of less than 500, and those using 1,2-propylene oxide, 1,2-, 2,3- or 1,3-butylene oxide, 3-methyltetrahydrofuran, etc. as AO in the AO adduct, and more preferred are aliphatic polyether diols of dihydric alcohols having a branched alkyl, and particularly preferred is polyoxypropylene glycol. (H4) may be used alone or in combination of two or more kinds.
[0052] The poly(meth)acrylic polyol (H5) may be, for example, a homopolymer or copolymer of a (meth)acrylic acid ester having a hydroxyl group. The (meth)acrylic polyol may also be obtained by copolymerizing a compound having a polymerizable unsaturated bond in addition to a (meth)acrylic acid ester having a hydroxyl group. In the present invention, "(meth)acrylic" means "methacrylic and / or acrylic".
[0053] The (meth)acrylic acid ester having a hydroxy group includes those having one (meth)acryloyl group, and examples thereof include those having a hydroxyalkyl group having 2 to 20 carbon atoms {for example, hydroxyalkyl (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate} and (meth)acrylic acid monoesters of trihydric alcohols {for example, a (meth)acrylic acid monoester of glycerin, a (meth)acrylic acid monoester of trimethylolpropane, and the like}.
[0054] The compound having a polymerizable unsaturated bond includes a compound having one polymerizable unsaturated bond, and examples thereof include (meth)acrylic acid alkyl esters having 4 to 50 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, lauryl (meth)acrylate, glycidyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; unsaturated carboxylic acids having 3 to 50 carbon atoms, such as (meth)acrylic acid, maleic acid, and itaconic acid; unsaturated amides having 3 to 50 carbon atoms, such as (meth)acrylamide, N-methylol (meth)acrylamide, and diacetone (meth)acrylamide; and other polymerizable monomers, such as styrene, vinyl toluene, vinyl acetate, acrylonitrile, and dibutyl fumarate.
[0055] Examples of the polymerization method of the (meth)acrylic acid ester having a hydroxy group or the compound having a polymerizable unsaturated bond include emulsion polymerization, suspension polymerization, dispersion polymerization, solution polymerization, etc. The emulsion polymerization can also be carried out in stages.
[0056] Specific examples of the commercially available poly(meth)acrylic polyol (H5) include "ARUFON UH-2000, UH-2041, UH-2190, UHE-2012" manufactured by Toagosei Co., Ltd., and "Actflow UT-1001, UMM-1001" manufactured by Soken Chemical & Engineering Co., Ltd.
[0057] Among the poly(meth)acrylic polyols (H5), from the viewpoint of solvent solubility, a polyacrylic polyol using at least one compound having a polymerizable unsaturated bond selected from the group consisting of n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, lauryl (meth)acrylate, and 2-ethylhexyl (meth)acrylate is preferred, and a polyacrylic diol using n-butyl (meth)acrylate and / or 2-ethylhexyl (meth)acrylate is more preferred. (H5) may be used alone or in combination of two or more.
[0058] When the hydroxyl-modified polyolefin (A) is used in combination with at least one member selected from the group consisting of condensation type polyester polyol (H1), polylactone polyol (H2), polycarbonate polyol (H3), polyether polyol (H4) and poly(meth)acrylic polyol (H5), the ratio of the total weight of the condensation type polyester polyol (H1), polylactone polyol (H2), polycarbonate polyol (H3), polyether polyol (H4) and poly(meth)acrylic polyol (H5) to the weight of the hydroxyl-modified polyolefin (A) is preferably 100% by weight or less, more preferably 10 to 90% by weight, from the viewpoints of the solvent solubility and mechanical strength of the polyurethane urea resin (U).
[0059] Examples of the polyisocyanate (B) in the present invention include aliphatic diisocyanates (B1) having 4 to 22 carbon atoms, alicyclic diisocyanates (B2) having 8 to 18 carbon atoms, aromatic diisocyanates (B3) having 8 to 26 carbon atoms, and araliphatic diisocyanates (B4) having 10 to 18 carbon atoms.
[0060] Examples of the aliphatic diisocyanate (B1) having 4 to 22 carbon atoms include ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, dodecamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl) fumarate, and bis(2-isocyanatoethyl) carbonate.
[0061] Examples of the alicyclic diisocyanate (B2) having 8 to 18 carbon atoms include isophorone diisocyanate (hereinafter abbreviated as IPDI), 4,4-dicyclohexylmethane diisocyanate, cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, bis(2-isocyanatoethyl)-4-cyclohexene-1,2-dicarboxylate, and 2,5- or 2,6-norbornane diisocyanate.
[0062] Examples of the aromatic diisocyanate (B3) having 8 to 26 carbon atoms include 1,3- or 1,4-phenylene diisocyanate, 2,4- or 2,6-tolylene diisocyanate, 4,4'- or 2,4'-diphenylmethane diisocyanate, polyaryl diisocyanate, 4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatodiphenylmethane, 1,5-naphthylene diisocyanate, and m- or p-isocyanatophenylsulfonyl isocyanate.
[0063] Examples of the aralkyl diisocyanate (B4) having 10 to 18 carbon atoms include m- or p-xylylene diisocyanate and α,α,α',α'-tetramethylxylylene diisocyanate.
[0064] Among these, from the viewpoint of adhesiveness, preferred is the alicyclic diisocyanate having 8 to 18 carbon atoms (B2), and further preferred from the viewpoints of the solvent solubility and adhesiveness of the polyurethane urea resin (U) is IPDI. The polyisocyanate (B) may be used alone or in combination of two or more kinds.
[0065] In the present invention, examples of the chain extender (C) having an Mn or chemical formula weight of less than 500 include polyamines (C1) and polyols (C2). (C) may be used alone or in combination of two or more.
[0066] Examples of the polyamine (C1) include diamines having 2 to 12 carbon atoms (ethylene diamine, propylene diamine, hexamethylene diamine, isophorone diamine, toluene diamine, piperazine, etc.), poly(n=2 to 6) alkylene (having 2 to 6 carbon atoms) poly(n=3 to 7) amines (diethylene triamine, dipropylene triamine, dihexylene triamine, triethylene tetramine, tetraethylene pentamine, pentaethylene hexamine, hexaethylene heptamine, etc.), and hydrazine or a derivative thereof (dibasic acid dihydrazide, for example, adipic acid dihydrazide, etc.). Among these, from the viewpoints of adhesion and solvent solubility, alicyclic diamines are preferred, and isophorone diamine is more preferred.
[0067] Examples of the polyol (C2) include the same diols as those exemplified above as diols having an Mn of less than 500, and from the viewpoints of adhesion and solvent solubility, 1,4-butanediol is preferred.
[0068] In obtaining the polyurethane urea resin (U), in addition to the essential components (A), (B) and (C), a reaction terminator (D) can be used for the purpose of adjusting the molecular weight of the polyurethane urea resin.
[0069] Examples of the reaction terminator (D) include monoalcohols having 1 to 10 carbon atoms (methanol, propanol, butanol, 2-ethylhexanol, etc.) and monoamines having 2 to 8 carbon atoms [mono- or di-alkylamines having 2 to 8 carbon atoms (n-butylamine, di-n-butylamine, etc.), mono- or dialkanolamines having 2 to 6 carbon atoms (monoethanolamine, diethanolamine, propanolamine, etc.)]. Among these, mono- or dialkanolamines having 2 to 6 carbon atoms are preferred. The reaction terminator (D) may be used alone or in combination of two or more kinds.
[0070] The amine value of the polyurethane urea resin (U) is preferably 0.1 to 20 mgKOH / g, more preferably 0.1 to 5 mgKOH / g, and particularly preferably 0.2 to 2 mgKOH / g. When the amine value is 0.1 mgKOH / g or more, the adhesiveness is good, and when it is 20 mgKOH / g or less, the viscosity and molecular weight have good stability over time.
[0071] The weight ratio [{(A)+(H1)-(H5)}:(B):(C)] of the total amount of the hydroxyl-modified polyolefin (A) and the polyols (H1)-(H5) used as needed to the polyisocyanate (B) and the chain extender (C) in the polyurethane urea resin (U) is preferably 100:(10-40):(1-20), more preferably 100:(12-35):(2-18), from the viewpoints of the solvent solubility, adhesiveness and mechanical strength of the polyurethane urea resin (U).
[0072] The method for producing the polyurethane urea resin (U) is not particularly limited, and may be any of a one-shot method in which a hydroxyl-modified polyolefin (A), a polyisocyanate (B), a chain extender (C), and optionally a polyol (H) and a reaction terminator (D) are reacted at once, or a multi-stage method in which they are reacted stepwise [for example, a method in which (A), (B), and optionally (H) and (C) are reacted to form an isocyanate-terminated prepolymer, and then (C) and optionally (D) are added and further reacted to produce the resin]. From the viewpoint of adhesion, however, a method in which an isocyanate-terminated prepolymer is formed, and then an amino group is introduced to the end of the polyurethane urea molecular chain by using a diamine having 2 to 12 carbon atoms as the chain extender (C) such that the total value of the amino groups in the diamine is in excess relative to the equivalent weight of the isocyanate groups in the prepolymer is preferred.
[0073] In producing the polyurethane urea resin (U), the molar ratio of the isocyanate groups of the polyisocyanate (B) to the active hydrogen-containing groups of the hydroxyl group-modified polyolefin (A), the chain extender (C), and the polyol (H) and reaction terminator (D) used as needed (isocyanate groups:active hydrogen-containing groups) is preferably 0.7:1 to 0.99:1, and more preferably 0.8:1 to 0.98:1, from the viewpoints of the solvent solubility and mechanical strength of the polyurethane urea resin (U).
[0074] The urethane group concentration of the polyurethane urea resin (U) in the present invention is preferably 0.4 to 1.5 mmol / g, and more preferably 0.6 to 1.0 mmol / g, based on the weight of (U), from the viewpoints of adhesiveness, mechanical strength, and solvent solubility. The urea group concentration of the polyurethane urea resin (U) in the present invention is preferably 0.3 to 1.3 mmol / g, and more preferably 0.3 to 1.2 mmol / g, based on the weight of (U), from the viewpoints of adhesiveness, mechanical strength, and solvent solubility. The total concentration of the urethane group and the urea group in the polyurethane urea resin (U) in the present invention is preferably 0.7 to 2.2 mmol / g, and more preferably 1.0 to 2.0 mmol / g, based on the weight of (U), from the viewpoints of adhesiveness, mechanical strength, and solvent solubility. In order to adjust the urea group content in the polyurethane urea resin (U) to fall within a desired range, the amino group content, water content and isocyanate group content in the raw materials for (U) may be appropriately adjusted. The urethane group concentration and urea group concentration in polyurethane urea resin (U) are determined by the N atom content quantified by a nitrogen analyzer. 1 It can be calculated from the ratio of urethane groups and urea groups as well as the contents of allophanate groups and biuret groups quantified by H-NMR.
[0075] In the present invention, the urethane group concentration and the urea group concentration of the polyurethane urea resin (U) can be measured as follows. (Urethane group concentration and urea group concentration of polyurethane urea resin (U)) The urethane group concentration and urea group concentration of the polyurethane urea resin (U) were determined by the N atom content quantified by a nitrogen analyzer [ANTEK7000 (manufactured by Antec)]. 1 It is calculated from the ratio of urethane groups and urea groups quantified by H-NMR and the contents of allophanate groups and biuret groups described below. 1 The H-NMR measurement is carried out according to the method described in "Structural Study of Polyurethane Resins by NMR: Takeda Research Institute Report 34(2), 224-323 (1975)". 1 H-NMR is measured, and when an aliphatic isocyanate is used, the weight ratio of the urea group to the urethane group is determined from the ratio of the integral amount of hydrogen derived from the urea group at a chemical shift of about 6 ppm to the integral amount of hydrogen derived from the urethane group at a chemical shift of about 7 ppm, and the contents of the urethane group and urea group are calculated from the weight ratio, the above-mentioned N atom content, and the allophanate group and biuret group contents. When an aromatic isocyanate is used, the weight ratio of the urea group to the urethane group is calculated from the ratio of the integral amount of hydrogen derived from the urea group at a chemical shift of about 8 ppm to the integral amount of hydrogen derived from the urethane group at a chemical shift of about 9 ppm, and the contents of the urethane group and urea group are calculated from this weight ratio, the above-mentioned N atom content, and the allophanate group and biuret group contents.
[0076] (Allophanate group and biuret group content) The total content of allophanate groups and biuret groups in the polyurethane urea resin (U) is calculated by a gas chromatograph [Shimadzu GC-9A {manufactured by Shimadzu Corporation}]. 50 g of DMF solution containing 0.01 wt% di-n-butylamine and 0.01 wt% naphthalene (internal standard) is prepared. A sample is weighed into a test tube with a stopper, 2 g of the above DMF solution is added, and the test tube is heated in a constant temperature water bath at 90 ° C for 2 hours. After cooling to room temperature, 10 μl of acetic anhydride is added and shaken and stirred for 10 minutes. Further, 50 μl of di-n-propylamine is added, and after shaking for 10 minutes, gas chromatographic measurement is performed. A blank measurement is performed in parallel, and the amount of amine consumed is calculated from the difference with the test value, and the total content of allophanate groups and biuret groups is measured. (Gas chromatograph conditions) Equipment: Shimadzu GC-9A Column: 10% PEG-20M on Chromosorb WAW DMLS 60 / 80mesh glass column, 3mmφ×2m Column temperature: 160°C, sample inlet temperature: 200°C, carrier gas: nitrogen 40ml / min Detector: FID, Sample injection volume: 2 μl (Calculation formula for the total content of allophanate groups and biuret groups) Total content of allophanate group and biuret group = {(BA) / B} x 0.00155 / S A: Peak area of di-n-butylacetamide / peak area of naphthalene of the sample B: Blank (peak area of di-n-butylacetamide / peak area of naphthalene) S: Amount of polyurethane urea resin (U) collected (g)
[0077] The reaction between the hydroxyl-modified polyolefin (A) and the polyisocyanate (B) is carried out at a temperature of preferably 20 to 140°C, more preferably 40 to 120°C. The reaction temperature of the polyisocyanate (B) or the isocyanate-terminated prepolymer obtained by reacting the hydroxyl-modified polyolefin (A) with the polyisocyanate (B) with the chain extender (C) is preferably 100°C or lower, more preferably 0 to 80°C.
[0078] In the reaction, in order to accelerate the reaction, a catalyst generally used in urethane reactions [amine catalysts (triethylamine, N-ethylmorpholine, triethylenediamine, etc.), tin catalysts (dibutyltin dilaurate, dioctyltin dilaurate, tin octylate, etc.), titanium catalysts (tetrabutyl titanate, etc.)], etc. may be used as necessary. The amount of catalyst used is preferably 0.1% by weight or less based on the polyurethane urea resin.
[0079] The reaction may be carried out in a solvent (S), and the solvent (S) may be added during or after the reaction. Examples of the solvent (S) include ester-based solvents (ethyl acetate, butyl acetate, ethyl cellosolve acetate, etc.), ketone-based solvents (acetone, methyl isobutyl ketone, methyl isobutyl ketone, etc.), ether-based solvents (dioxane, tetrahydrofuran, propylene glycol monomethyl ether, etc.), aliphatic hydrocarbon-based solvents (n-hexane, n-heptane, cyclohexane, methylcyclohexane, etc.), and alcohol-based solvents (ethanol, methanol, n-propyl alcohol, isopropyl alcohol, n-butanol, etc.).
[0080] Among these, from the viewpoint of the solubility of the polyurethane urea resin (U), at least one selected from the group consisting of ethyl acetate, butyl acetate, propylene glycol monomethyl ether, methyl ethyl ketone, methyl isobutyl ketone, n-propyl alcohol, methylcyclohexane and isopropyl alcohol is preferred, and at least one selected from the group consisting of ethyl acetate, methyl ethyl ketone, methylcyclohexane and isopropyl alcohol is more preferred. The solvent (S) may be used alone or in combination of two or more.
[0081] The number average molecular weight (Mn) of the polyurethane urea resin (U) in the present invention is preferably 10,000 to 40,000. When Mn is 10,000 or more, the adhesiveness in one-component use is good, and when Mn is 40,000 or less, the solubility and workability are good.
[0082] <Polyurethane urea resin solution> The polyurethane urea resin solution of the present invention contains the polyurethane urea resin (U) and a solvent (S). Examples of the solvent (S) include those mentioned above. From the viewpoint of the solubility of the polyurethane urea resin (U), preferred are ethyl acetate, propylene glycol monomethyl ether, methyl ethyl ketone, methylcyclohexane, n-propyl alcohol, and isopropyl alcohol, and more preferred are ethyl acetate, methyl ethyl ketone, methylcyclohexane, and isopropyl alcohol.
[0083] The content of the polyurethane urea resin (U) in the polyurethane urea resin solution of the present invention is preferably 10 to 50% by weight, and more preferably 20 to 40% by weight, based on the weight of the polyurethane urea resin solution, from the viewpoint of handleability. The polyurethane urea resin (U) in the polyurethane urea resin solution of the present invention has good mechanical strength and excellent adhesion to plastic substrates (polyolefin, polyester, nylon, etc.), and the polyurethane urea resin solution of the present invention has excellent solution stability. Therefore, by using the polyurethane urea resin solution of the present invention, it is possible to obtain paints, printing inks, coating agents, and adhesives which have good mechanical strength, excellent adhesion to plastic substrates, and excellent solution stability.
[0084] <Paint> The coating material of the present invention contains the polyurethane urea resin solution of the present invention. In the coating material of the present invention, the polyurethane urea resin (U) exhibits functions such as a binder and a pigment dispersing resin. The content of the polyurethane urea resin (U) of the present invention in the coating material of the present invention is preferably 1 to 40% by weight, more preferably 2 to 30% by weight, based on the weight of the coating material, from the viewpoints of adhesion, mechanical strength and handleability.
[0085] The coating material of the present invention may contain any of the additives commonly used in coating materials. Examples of additives include pigments, curing agents, diluents, leveling agents such as acrylic resins and silicone resins, silicone-based and acrylic-based anti-repellents, anti-skinning agents, thixotropic agents, defoamers, color separation inhibitors, smoothing agents, wetting agents, dispersants, thickeners, anti-settling agents, polymerization inhibitors, structural viscosity imparting agents, electrostatic coating property improvers, anti-sagging agents, curing accelerators, antioxidants, light stabilizers, antifouling agents, flame retardants, coating aids, etc. Preferred examples of light stabilizers and antioxidants include the compounds described in JP-A-2004-117997.
[0086] The coating film formed by the coating material can be applied to any thickness depending on the application, but the final coating film thickness is preferably 0.1 to 10,000 μm, more preferably 0.1 to 2,000 μm, even more preferably 1 to 1,000 μm, even more preferably 5 to 1,000 μm, and even more preferably 5 to 200 μm. The coating method may be any method, including spraying, dipping, roller coating, flow coating, flow painting, electrocoating, powder flow painting, brush painting, and the like. Drying after application varies depending on the paint components, but can be done by natural drying or heat drying (generally at room temperature to 180°C for about 10 to 90 minutes).
[0087] From the viewpoint of handleability, the viscosity (20° C.) of the coating material of the present invention is preferably from 100 to 5,000 mPa·s, and more preferably from 500 to 3,000 mPa·s. The viscosity of the paint can be measured using a B-type viscometer in accordance with JIS-K7117-1.
[0088] The coating material of the present invention can be applied to any substrate, such as metals (steel plates, iron and steel, non-ferrous metals, light metals, etc.), plastics (polyolefins, polyesters, nylons, etc.), wood, glass, concrete, resins, rubber, leather, paper, skin, etc., depending on the application, to form a coating film and produce a desired member, but from the viewpoint of adhesion, plastic substrates are preferred as substrates. The coating material of the present invention can be used, for example, as an automotive coating material for automotive parts, automotive bumpers, and vehicle bodies, an electrical appliance coating material, an architectural coating material, an anti-rust coating material, and the like, and is particularly useful as an automotive coating material.
[0089] <Printing ink> The printing ink of the present invention contains the polyurethane urea resin solution of the present invention. In the printing ink of the present invention, the polyurethane urea resin (U) exhibits functions such as a binder and a pigment dispersing resin. The content of the polyurethane urea resin (U) in the printing ink of the present invention is preferably 5 to 40% by weight, more preferably 10 to 30% by weight, based on the weight of the printing ink, from the viewpoints of adhesion, mechanical strength and handleability.
[0090] The printing ink of the present invention may contain additives such as pigments, other resins, and pigment dispersants that are generally preferably used in printing inks, if necessary. The other resins and additives may be used alone or in combination of two or more.
[0091] The pigment is not particularly limited, and preferably, inorganic pigments and organic pigments used in printing inks can be used. Examples of the other resins include polyamide resins, nitrocellulose, acrylic resins, vinyl acetate resins, styrene-maleic acid copolymer resins, chlorinated polypropylene resins, epoxy resins, and rosin resins, etc. The amount of these other resins used is preferably 30% by weight or less, more preferably 20% by weight or less, based on the weight of the printing ink.
[0092] The method for producing the printing ink is not particularly limited, and the printing ink can be produced by any known method using, for example, a general-purpose ink production apparatus such as a three-roll mill, a ball mill, or a sand grinder mill.
[0093] An example of the formulation of the printing ink of the present invention is as follows. Polyurethane urea resin (U): 5 to 40% by weight (preferably 10 to 30% by weight) Pigment: 5 to 40% by weight (preferably 10 to 30% by weight) Other resins: 0 to 30% by weight (preferably 0 to 20% by weight) Solvent: 30 to 80% by weight (preferably 40 to 70% by weight)
[0094] The printing ink made using the polyurethane urea resin solution of the present invention may be used as a one-component printing ink, but may also be used as a two-component printing ink in combination with, for example, a polyisocyanate-based curing agent. In this case, the polyisocyanate-based curing agent is preferably, for example, an adduct from 1 mole of trimethylolpropane and 3 moles of 1,6-hexamethylene diisocyanate, tolylene diisocyanate or IPDI; an isocyanurate group-containing trimer synthesized by cyclic trimerization of the isocyanate group of 1,6-hexamethylene diisocyanate or IPDI; a partial biuret reaction product derived from 1 mole of water and 3 moles of 1,6-hexamethylene diisocyanate, and a mixture of two or more of these. When used as a two-component printing ink, the amount of the polyisocyanate-based curing agent used is preferably 0.5 to 10% by weight based on the weight of the polyurethane urea resin (U).
[0095] Printing methods using the printing ink of the present invention include printing methods such as special gravure printing, inkjet printing, offset printing and thermal transfer printing that are conventionally used for printing on plastic films.
[0096] The printing ink of the present invention has particularly excellent adhesion to plastics and can be suitably used for printing on various plastic films such as polyester film, nylon film, polyolefin film (surface-treated or untreated polypropylene film, polyethylene film, etc.), polyvinyl acetal film, acetate film, polyvinyl chloride film, and these films subjected to aluminum deposition.
[0097] <Coating agent> The coating agent of the present invention contains the polyurethane urea resin solution of the present invention. In the coating agent of the present invention, the polyurethane urea resin (U) exhibits a function as a binder or the like. The content of the polyurethane urea resin (U) in the coating agent of the present invention is preferably 5 to 50% by weight, more preferably 10 to 40% by weight, based on the weight of the coating agent, from the viewpoints of adhesion, mechanical strength and handleability.
[0098] The coating agent of the present invention may contain other resins than the polyurethane urea resin (U), such as polyurethane resins other than (U), polyester resins, polyacrylic resins, epoxy resins, etc. From the viewpoint of adhesion, the content of other resins is preferably 50% by weight or less, more preferably 30% by weight or less, based on the weight of the polyurethane urea resin (U).
[0099] Any additives generally used in coating agents may be contained. Examples of additives include stabilizers (antioxidants, ultraviolet absorbers, etc.), fillers, colorants (dyes and pigments), flame retardants (antimony oxide, etc.), dispersants, defoamers, and leveling agents. The content of the additives is preferably 10% by weight or less, more preferably 0.5 to 5% by weight, based on the weight of (U) in the coating agent. Examples of the antioxidant include hindered phenols [Irganox 1010 (Ciba-Geigy) and the like] and hindered amines [Sanol LS770 (Ciba-Geigy) and the like]. Examples of the ultraviolet absorbers include triazoles [Tinuvin 320 (Ciba-Geigy) and the like] and benzophenones [Cyasorb UV9 (Cyanamido) and the like]. Examples of the fillers include clay, calcium carbonate, barium sulfate, alumina, silica, carbon black, zinc oxide, calcium oxide, lead dioxide, titanium oxide, diatomaceous earth, glass fibers and their crushed products (cut glass, milled glass, glass flakes, etc.), talc, and mica.
[0100] The viscosity (20° C.) of the coating agent of the present invention is preferably from 100 to 5,000 mPa·s, and more preferably from 500 to 3,000 mPa·s, from the viewpoint of handleability. The viscosity of the coating agent can be measured using a B-type viscometer in accordance with JIS-K7117-1.
[0101] Substrates to which the coating agent of the present invention can be applied include plastic molded bodies [polyolefins (polyethylene and polypropylene, etc.), polystyrene, ABS, polyvinyl chloride, polycarbonate, polyacetal, polyester, nylon, polyamide, polyurethane, modified PPO, polymethyl methacrylate, epoxy resin, phenolic resin, melamine resin, etc.], rubbers [natural rubber, synthetic rubber (chloroprene rubber, isoprene rubber, SBR, NBR, butyl rubber, EP rubber, etc.)], porous materials [wood, paper, cloth (woven or nonwoven fabrics of natural fibers and synthetic fibers, etc.), plastic foams (polyolefin foams, polyurethane foams, etc.), etc.], and inorganic materials [metals (iron, tinplate, galvanized iron, aluminum, galvanized steel sheets, etc.), glass, tile slate, ceramics, etc.]. Among these, plastics are preferred, and polyolefins, polyesters, and nylons are more preferred.
[0102] The coating agent of the present invention exhibits excellent performance, particularly as an undercoat agent for painting polyolefin resin molded bodies (such as automobile bumpers) and electrodeposition-coated steel sheets of automobile bodies. When used as an undercoat agent for painting, the coating amount (after drying) can be selected according to the purpose, but is preferably 1 to 50 μm, more preferably 2 to 40 μm. As a coating method, known methods such as spray coating, brush coating, roll coating, flow coating, and immersion method can be used. The drying (baking) temperature is preferably 40 to 130° C., more preferably 60 to 80° C., and the drying time is preferably 0.5 to 60 minutes, more preferably 3 to 30 minutes.
[0103] As the topcoat, known thermosetting or thermoplastic resin paints, such as acrylic enamel, one-component and two-component polyurethane paints, acrylic urethane paints, acrylic melamine paints, and alkyd melamine paints, are used. The coating amount of the topcoat (after drying) is preferably 20 to 80 μm. Methods for coating and drying the topcoat include known methods, such as the two-coat one-bake (wet-on-wet coating) method and the two-coat two-bake (dry-on-wet coating) method. The topcoat layer may be one layer or two or more layers.
[0104] <Adhesive> The adhesive of the present invention contains the polyurethane urea resin solution of the present invention. The content of the polyurethane urea resin (U) in the adhesive of the present invention is preferably 1 to 50% by weight, more preferably 2 to 40% by weight, based on the weight of the adhesive, from the viewpoints of adhesion, mechanical strength and handleability.
[0105] The adhesive of the present invention may further contain various additives, if necessary, in addition to the polyurethane urea resin solution of the present invention. The additives include one or more selected from the group consisting of tackifiers, plasticizers, adsorbents, colorants, flame retardants, fillers, lubricants, nucleating agents, antioxidants, release agents, light stabilizers, fragrances, and ultraviolet absorbers.
[0106] Examples of tackifiers include terpene resins, terpene phenol resins, phenol resins, aromatic hydrocarbon modified terpene resins, rosin resins, modified rosin resins, synthetic petroleum resins (aliphatic, aromatic or alicyclic synthetic petroleum resins, etc.), coumarone-indene resins, xylene resins, styrene-based resins, dicyclopentadiene resins, and hydrogenated products of those having unsaturated double bonds that can be hydrogenated among these.
[0107] As the plasticizer, various plasticizers [for example, those described in Adhesion Technology Vol. 20, (2), 21 (2000)] can be used, and examples thereof include process oils (paraffin, naphthene or aromatic compound type); liquid resins (Mn 300 to 6,000, for example, liquid polybutene, liquid polybutadiene, liquid polyisoprene); hydrogenated products of the liquid resins; low molecular weight (Mn 300 to 10,000) polyisobutylene; and mixtures of two or more of these.
[0108] Examples of the adsorbent include alumina, silica gel, and molecular sieves.
[0109] Examples of colorants include inorganic pigments [white pigments, cobalt compounds, iron compounds, sulfides, etc.], organic pigments [azo pigments, polycyclic pigments, etc.], dyes [azo-based, indigoid-based, sulfide-based, alizarin-based, acridine-based, thiazole-based, nitro-based, aniline-based, etc.], and the like.
[0110] Examples of the flame retardant include a halogen-containing flame retardant, a sulfur-containing flame retardant, a phosphorus-containing flame retardant, and a metal hydroxide-containing flame retardant.
[0111] Examples of the filler include inorganic fillers (calcium carbonate, talc, clay, etc.).
[0112] Examples of the lubricant include calcium stearate, butyl stearate, and oleic acid amide.
[0113] Nucleating agents include sorbitol, metal phosphates, metal benzoates, metal phosphates, and the like.
[0114] Examples of the antioxidant include phenol compounds [monocyclic phenols (e.g., 2,6-di-t-butyl-p-cresol), bisphenols (e.g., 2,2'-methylenebis(4-methyl-6-t-butylphenol)], polycyclic phenols (e.g., 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene)], sulfur compounds (e.g., dilauryl 3,3'-thiodipropionate), and phosphorus compounds (e.g., triphenyl phosphite).
[0115] Examples of the release agent include carboxy-modified silicone oil and hydroxyl-modified silicone oil.
[0116] Examples of the light stabilizer include hindered amine compounds [(bis-2,2,6,6-tetramethyl-4-piperidyl)sebacate, etc.].
[0117] Fragrances include diterpenes, limonene, and the like.
[0118] Examples of the ultraviolet absorber include benzotriazoles [2-(2'-hydroxy-5'-methylphenyl)benzotriazole, etc.], benzophenones [2-hydroxy-4-methoxybenzophenone, etc.], and salicylates [phenyl salicylate, etc.].
[0119] The total content of the additives is preferably 50% by weight or less, more preferably 0.002 to 40% by weight, and particularly preferably 1 to 30% by weight, based on the total weight of the adhesive, from the viewpoints of the additive effect and adhesiveness.
[0120] When the additives mentioned above overlap, each additive should not be used in the amount necessary to exert its corresponding additive effect, but should be adjusted in amount according to the purpose of use, taking into consideration that the effects of other additives can be obtained at the same time.
[0121] <Adhesive body> The adhesive of the present invention can be used to bond adherends to obtain an adherend. Examples of the adherend include various plastics [polyolefins (polyethylene and polypropylene, etc.), polyesters, nylons, polystyrenes, syndiotactic polystyrenes, ABS, polyvinyl chloride, polycarbonates, polyacetals, polyamides, polyimides, polyurethanes, modified PPOs, polymethyl methacrylates, liquid crystal polymers, epoxy resins, phenolic resins, and melamine resins, etc.], rubbers [natural rubbers, synthetic rubbers (chloroprene rubbers, isoprene rubbers, SBRs, NBRs, butyl rubbers, and EP rubbers, etc.)], porous materials [wood, paper, cloths (woven or nonwoven fabrics of natural and synthetic fibers, etc.), plastic foams (polyolefin foams, polyurethane foams, etc.), etc.], and inorganic materials [metals (copper, iron, tinplate, galvanized iron, aluminum, and galvanized steel sheets, etc.), glass, tile slates, and ceramics, etc.]. Among these, from the viewpoint of adhesion, plastic substrates are preferred, and polyolefins, polyesters, and nylons are more preferred. It is preferred that at least one of the adherends is a polyolefin substrate.
[0122] The method for applying the adhesive of the present invention to the adherend is not particularly limited, and the adhesive can be applied with a spatula, comb, roller, trowel, rake, etc., or by extrusion or spraying with a sealing gun, or by hand or machine application to form a coating film of any thickness, film sheet, thick object, or any other shape. A coating film can also be formed by incorporating a compound having anti-sagging properties and applying the coating to vertical surfaces, wall surfaces, curved surfaces, depressions, etc. with a roller, lysine gun, airless gun, etc.
[0123] The adhesive of the present invention can be used as an adhesive for automobile parts using polyolefin parts such as bumpers, for building parts, and for polyolefin-based laminate films, and is particularly useful as an adhesive for automobile parts and laminate films. EXAMPLES
[0124] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. In the following, "parts" refers to parts by weight.
[0125] Manufacturing Example 1 In a reaction vessel, 1000 parts of polyolefin (A0-1) [Mn: 113,000, isotacticity: 50%, trade name "Vistamaxx3980", manufactured by Exxonmobil] consisting of 91% by weight of propylene and 9% by weight of ethylene as constituent monomers was charged, and while nitrogen was passed through the liquid phase, it was heated and melted with a mantle heater, and thermal degradation was performed at 370 ° C for 60 minutes while stirring to obtain polyolefin (A1-1). 65 parts of maleic anhydride (E-1) was charged here, and after nitrogen replacement, it was heated to 180 ° C under nitrogen aeration to dissolve uniformly, and a solution in which 5 parts of radical initiator [dicumyl peroxide, trade name "Percumyl D", manufactured by NOF Corp.] (F-1) was dissolved in 50 parts of xylene was dropped over 5 minutes, and stirring was continued for 1 hour under xylene reflux. Thereafter, unreacted maleic anhydride was distilled off under reduced pressure (1.5 kPa) to obtain an acid-modified polyolefin (X-1). 500 parts of (X-1) and 32 parts of 2-aminoethanol (G-1) were charged into a similar reaction vessel and reacted at 180°C for 1 hour under a nitrogen gas atmosphere. Then, unreacted 2-aminoethanol was distilled off under reduced pressure of 180°C and 2.7 kPa to obtain a hydroxyl-containing modified polyolefin (A-1). (A-1) had a hydroxyl value of 29, an acid value of 0.2, an Mn of 3,500, and an isotacticity of 43%. The number of double bonds per 1,000 carbons of the polyolefin (A1-1) used for modification was 7.5.
[0126] Manufacturing Example 2 Except for using polyolefin (A0-2) [Mn: 76,000, isotacticity: 20%, product name "Vistamaxx6202", manufactured by Exxonmobil] having 85% by weight of propylene and 15% by weight of ethylene as constituent monomers in the reaction vessel, the reaction was carried out in the same manner as in Production Example 1 under the conditions described in Table 1 to obtain an acid-modified polyolefin (X-2), which was then reacted with 2-aminoethanol (G-1) in the same manner as in Production Example 1 to obtain a hydroxyl-containing modified polyolefin (A-2). The results are shown in Table 1.
[0127] Production Example 3 Using polyolefin (A0-1) whose constituent monomers were 91% by weight propylene and 9% by weight ethylene, a reaction was carried out in the same manner as in Production Example 1 under the conditions shown in Table 1 to obtain an acid-modified polyolefin (X-3), which was then reacted with 2-aminoethanol (G-1) in the same manner as in Production Example 1 to obtain a hydroxyl-containing modified polyolefin (A-3). The results are shown in Table 1.
[0128] Production Example 4 Using polyolefin (A0-2) whose constituent monomers were 85% by weight propylene and 15% by weight ethylene, a reaction was carried out in the same manner as in Production Example 1 under the conditions shown in Table 1 to obtain an acid-modified polyolefin (X-4), which was then reacted with 2-aminoethanol (G-1) in the same manner as in Production Example 1 to obtain a hydroxyl-containing modified polyolefin (A-4). The results are shown in Table 1.
[0129] Production Example 5 1000 parts of polyolefin (A0-3) [Mn: 200,000, isotacticity: 33%, trade name "Tafmer S4030", manufactured by Mitsui Chemicals] was charged, and while nitrogen was passed through the liquid phase, it was heated and melted with a mantle heater, and thermal degradation was performed at 380 ° C for 80 minutes while stirring to obtain polyolefin (A1-3). 47 parts of maleic anhydride (E-1) was charged thereto, and after nitrogen replacement, it was heated to 200 ° C under nitrogen ventilation and continued stirring for 10 hours. Thereafter, unreacted maleic anhydride was distilled off under reduced pressure (1.5 kPa) to obtain acid-modified polyolefin (X-5). 500 parts of (X-5) and 23 parts of 2-aminoethanol (G-1) were charged in a similar reaction vessel, and reacted at 180 ° C for 1 hour under a nitrogen gas atmosphere. The unreacted 2-aminoethanol was then distilled off at 180° C. under a reduced pressure of 2.7 kPa to obtain a hydroxyl group-containing modified polyolefin (A-5). The results are shown in Table 1.
[0130] Production Example 6 A polyolefin (A0-4) having 27% by weight of propylene and 73% by weight of ethylene as constituent monomers [Mn: 40,000, isoactivity: 3%, trade name "TAFMER P0280", manufactured by Mitsui Chemicals, Inc.] was used, and a reaction was carried out in the same manner as in Production Example 1 under the conditions described in Table 1 to obtain an acid-modified polyolefin (X-6). This was then further reacted with 2-aminoethanol (G-1) in the same manner as in Production Example 1 to obtain a hydroxyl group-containing modified polyolefin (A- 6 The results are shown in Table 1.
[0131] Comparative Manufacturing Example 1 Except for using polyolefin (A0-5) [Mn: 100,000, isotacticity: 90%, product name "SunAllomer PZA20A", manufactured by SunAllomer Co., Ltd.] whose constituent monomers are 98% by weight of propylene and 2% by weight of ethylene, a reaction was carried out in the same manner as in Production Example 1 under the conditions shown in Table 1 to obtain an acid-modified polyolefin (X-7), which was then reacted with 2-aminoethanol (G-1) in the same manner as in Production Example 1 to obtain a hydroxyl-containing modified polyolefin (A'-1). The results are shown in Table 1.
[0132] Comparative Manufacturing Example 2 Except for using polyolefin (A0-2) whose constituent monomers were 85% by weight of propylene and 15% by weight of ethylene, the reaction was carried out in the same manner as in Production Example 1 under the conditions shown in Table 1 to obtain acid-modified polyolefin (X-8), which was then reacted with 2-aminoethanol (G-1) in the same manner as in Production Example 1 to obtain hydroxyl-containing modified polyolefin (A'-2). The results are shown in Table 1.
[0133] [Table 1]
[0134] Example 1 In a reaction vessel equipped with a stirrer, 223 parts of the hydroxyl-containing modified polyolefin (A-1) obtained in Production Example 1, 3.20 parts of 1,4-butanediol, and 52.11 parts of IPDI were charged and reacted for 6 hours at 110°C under a nitrogen atmosphere to obtain a urethane prepolymer with an NCO content of 3.50% by weight. After cooling to 40°C, 350 parts of methylcyclohexane were added to obtain a homogeneous solution. Next, 350 parts of isopropanol were added and stirred until homogeneous, after which 16.43 parts of isophoronediamine and 5.06 parts of diethanolamine were added and reacted for 1 hour at 40°C to obtain a solution of polyurethane urea resin (U-1) of the present invention. The viscosity of the solution of (U-1) at 20°C was 1,000 mPa·s, and the Mn of (U-1) was 13,000.
[0135] Examples 2 to 14, Comparative Examples 1 to 3 The reaction was carried out in the same manner as in Example 1, except that the raw materials used in Example 1 were changed to the types and amounts shown in Table 2, to obtain solutions of polyurethane urea resins (U-2) to (U-14) and (U'-1) to (U'-3). The results are shown in Table 2.
[0136] The raw materials used in the examples and comparative examples are as follows. Polyol (H-1): Kuraray Polyol P-2010: Poly(3-methyl-1,5-pentanediol, adipic acid polycondensate) with Mn=2,000, manufactured by Kuraray Co., Ltd. Polyol (H-2): PTMG2000: Poly(oxytetramethylene) glycol with Mn=2,000 [Mitsubishi Chemical Co., Ltd.] Polyol (H-3): Sannix PP-2000: Polypropylene glycol with Mn=2,000 [manufactured by Sanyo Chemical Industries, Ltd.] Polyol (H-4): Actflow UT-1001: Polyacryldiol with Mn=2,000 [manufactured by Soken Chemical Industries, Ltd.]
[0137] [Table 2]
[0138] Examples 15 to 28 and Comparative Examples 4 to 6 The storage stability of the polyurethane urea resin (U) solutions obtained in Examples 1 to 14 and Comparative Examples 1 to 3 at 25° C. was evaluated according to the following criteria by comparing the appearance immediately after production and one day after production. The results are shown in Table 3. <Evaluation criteria> ○: No change in appearance. ×: The solution separated.
[0139] A white pigment dispersion was prepared according to the following recipe using the solutions of the polyurethane urea resins (U) obtained in Examples 1 to 14 and Comparative Examples 1 to 3, and an adhesion test was carried out. The results are shown in Table 3.
[0140] [Preparation of white pigment dispersion] A mixture of 35 parts of polyurethane urea resin (U) solution, 35 parts of titanium oxide ("Titanix JR809" manufactured by Teika Corporation), 10 parts of isopropyl alcohol, 20 parts of ethyl acetate, and 100 parts of glass beads was kneaded in a paint conditioner (manufactured by Red Devil Co., Ltd.) for 1 hour, and the glass beads were removed by filtration to obtain a white pigment dispersion.
[0141] [Adhesion test method] A white pigment dispersion was applied to the treated surfaces of a surface-treated polypropylene film (OPP) [Toyobo Co., Ltd.'s "Pylen P-2161" (thickness 30 μm)], a surface-treated polyester film (PET) [Toyobo Co., Ltd.'s "Espet E-5102" (thickness 12 μm)], and a surface-treated nylon film [Toyobo Co., Ltd.'s "Harden N-1130" (thickness 15 μm)] using a bar coater so that the thickness after drying was 2 to 3 μm, and the test pieces were prepared by drying at 60 ° C for 1 minute, and then cellophane tape (Nichiban, 12 mm wide) was applied to the coated surface, and one end of the cellophane tape was rapidly peeled off in a direction perpendicular to the coated surface to observe the state of the coated surface and determine the area % where the ink was not peeled off. The untreated side of each film that was not surface-treated was also tested in the same manner.
[0142] Dry films were prepared according to the following recipes using the solutions of the polyurethane urea resins (U) obtained in Examples 1 to 14 and Comparative Examples 1 to 3, and the physical properties of the films were measured. The results are shown in Table 3. [Production of dry film] A release film was attached to a polypropylene mold, and the polyurethane urea resin solution (U) obtained in the Examples and Comparative Examples, which had been prepared in advance to a solid content concentration of 20% by weight, was gently poured into the mold so that the film would have a thickness of approximately 200 μm after drying. The polyurethane urea resin solution was then spread evenly over the entire mold, and the mold was left to stand at 25°C for 12 hours. The mold was then dried at 70°C for 1 hour using a circulating air dryer, and then further dried under reduced pressure at 105°C and a pressure of 1.3 kPa for 1 hour to obtain a dry film.
[0143] <Coating film properties> [100% modulus, breaking strength and breaking elongation] The dried film obtained above was cut into a dumbbell-shaped test piece No. 3 in accordance with JIS K6251, and the 100% modulus, breaking strength, and breaking elongation were measured at a tensile speed of 500 mm / min using an autograph [Shimadzu Corporation's "AGS-500D"]. The 100% modulus and breaking strength are indicators of the strength of the coating film when applied to the surface of a substrate as a paint, printing ink, or coating agent, and a 100% modulus of 1.0 MPa or more and a breaking strength of 3.0 MPa or more can be said to be at a usable level. In addition, the breaking elongation is an indicator of the conformability to the substrate when used as a paint, printing ink, coating agent, or adhesive, and a breaking elongation of 300% or more can be said to conform to the substrate and not to deteriorate in adhesion even if the substrate is deformed.
[0144] [Table 3]
[0145] From the results in Table 3, it can be seen that the polyurethane urea resin solution of the present invention has excellent solution stability, does not contain harmful substances such as chlorine and toluene, exhibits excellent adhesion to not only surface-treated plastic substrates but also to untreated plastic substrates, and has good mechanical strength. On the other hand, from the evaluation results of Comparative Example 6, it can be seen that the conventional polyurethane urea resin solution has good solution stability but extremely poor adhesion to polyolefin films, polyester films and nylon films that are not surface-treated. Also, from the evaluation results of Comparative Examples 4 and 5, it can be seen that the polyurethane urea resin solution using the hydroxyl group-modified polyolefin (A'-1) or (A'-2) whose Mn is too small or too large, whose polyolefin structure contains too many α-olefin structures, or whose isotacticity is too large, has poor solution stability and extremely poor adhesion to plastic substrates. [Industrial Applicability]
[0146] The polyurethane urea resin solution of the present invention and the paint, printing ink, coating agent and adhesive using the same do not contain harmful substances such as chlorine and toluene, do not impair mechanical strength, and exhibit particularly excellent adhesion to plastics (polyolefin, polyester, nylon, etc.) that have not been subjected to corona treatment or plasma treatment, and have excellent solution stability, so that the paint containing the polyurethane urea resin solution of the present invention can be used as automobile paints such as automobile parts and automobile bodies, paints for electrical appliances, architectural paints, and rust-preventive paints, and is particularly useful as automobile paints. In addition, the printing ink containing the polyurethane urea resin solution of the present invention is particularly suitable as a printing ink for special gravure printing, flexographic printing, inkjet printing, offset printing, and thermal transfer printing. In addition, the polyurethane urea resin solution of the present invention is useful not only for the above-mentioned applications, but also as a coating agent for adhesives and paper, etc.
Claims
1. A polyurethane urea resin solution containing a polyurethane urea resin (U) having as essential constituent monomers a hydroxyl-modified polyolefin (A), a polyisocyanate (B), and a chain extender (C) having a number average molecular weight or chemical formula weight of less than 500, and a solvent (S), wherein the chain extender (C) contains a polyamine (C1), the number of hydroxyl groups per molecule of the hydroxyl-modified polyolefin (A) is 1.5 to 2.0, the weight ratio (ethylene:α-olefin) of the constituent monomers of the hydroxyl-modified polyolefin (A) to an α-olefin having 3 to 8 carbon atoms is 9:91 to 95:5, the isotacticity of the α-olefin unit chain portion of the hydroxyl-modified polyolefin (A) is 1 to 50%, and the number average molecular weight of the hydroxyl-modified polyolefin (A) is 1,000 to 6,000.
2. The polyurethane urea resin solution according to claim 1, wherein the hydroxyl value of the hydroxyl-modified polyolefin (A) is 14 to 110 mg KOH / g.
3. The polyurethane urea resin solution according to claim 1 or 2, wherein the hydroxyl-modified polyolefin (A) is a reaction product of an acid-modified polyolefin (X) in which a polyolefin (A1) having a carbon-carbon double bond is modified with an unsaturated (poly)carboxylic acid (anhydride) (E) and an amino alcohol (G), or a reaction product of the acid-modified polyolefin (X) and an alkylene oxide, and the polyolefin (A1) having a carbon-carbon double bond is a thermal degradation product of a polyolefin (A0) having a number average molecular weight of 60,000 to 400,000.
4. A paint comprising the polyurethane urea resin solution according to any one of claims 1 to 3.
5. A printing ink comprising the polyurethane urea resin solution according to any one of claims 1 to 3.
6. A coating agent comprising the polyurethane urea resin solution according to any one of claims 1 to 3.
7. An adhesive comprising the polyurethane urea resin solution according to any one of claims 1 to 3.
Citation Information
Patent Citations
Master batch composition
JP1995082424A
Coating agent
JP1995331159A
Coating material
JP1996003505A
Coating material
JP1996003506A
Coating material
JP1996003507A