toner

A core-shell toner with an oxazoline group and polyvalent metal shell structure addresses charge deterioration in harsh environments, maintaining chargeability and image quality in high-speed printing.

JP7596123B2Active Publication Date: 2024-12-09CANON KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020185498
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-06
Publication Date
2024-12-09
Estimated Expiration
2040-11-06

AI Technical Summary

Technical Problem

Toner charge build-up properties deteriorate in harsh environments due to moisture adsorption by highly hydrophilic charge control agents and resins, leading to reduced charging resistance and image quality issues in high-speed printing.

Method used

A toner with a core-shell structure containing a binder resin and a shell with an oxazoline group and polyvalent metal, where the shell thickness is 1.0 nm to 15.0 nm and the polyvalent metal concentration is 0.0010 atomic% to 0.5000 atomic%, forming a crosslinked structure to maintain chargeability.

Benefits of technology

The toner maintains excellent chargeability even after exposure to harsh conditions, ensuring high-quality images from the initial stage of printing in high-speed image forming apparatus.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596123000001
    Figure 0007596123000001
  • Figure 0007596123000002
    Figure 0007596123000002
  • Figure 0007596123000003
    Figure 0007596123000003
Patent Text Reader

Abstract

To provide a toner that maintains the electrification rising property of the toner even after being left standing in a severe environment and can output an excellent image from an initial stage of printing in a high-speed printing image forming apparatus.SOLUTION: A toner contains a toner particle that has a core particle containing a binder resin, and a shell on the surface of the core particle. The shell contains an oxazoline group and polyvalent metal. In an electron image of the cross section of the toner particles photographed by using a transmission electron microscope, the atomic concentration C (M) of the polyvalent metal obtained through energy dispersion type X-ray analysis in the shell is 0.0010 atomic% or more and 0.5000 atomic% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to toners used to form toner images by developing electrostatic latent images formed by methods such as electrophotography, electrostatic recording, and toner jet recording. [Background technology]

[0002] Electrophotography, used in copiers, printers, facsimile receiving devices, etc., is becoming more and more demanding from users as the equipment develops. In electrophotography, toner is given an electric charge by frictional charging with various members such as carriers and blades, and then transferred to media such as paper. In recent years, with the trend toward faster printing speeds, there is a strong demand for improved charge build-up properties of toner so that the desired charge can be given to the toner in a short time. To improve the charge rising property of a toner, a charge control agent or a charge control resin that easily generates a charge is often used. For example, Patent Document 1 discloses a core-shell toner using a resin containing an oxazoline group. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-054891 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, many charge control agents and charge control resins are highly hydrophilic and are easily affected by high temperature and high humidity environments, such as by absorbing moisture. In recent years, printers are increasingly being used in a variety of environments, including outdoors, in addition to offices. When toner is used and left in harsh environments for long periods of time, the surface properties of the toner particles change, causing the toner's charge rise property to decrease. For this reason, it was found that there are issues with regard to the charge rise property of the toner after being left in harsh environments. The present disclosure provides a toner that maintains charge build-up properties even after being left in a harsh environment, and that can output excellent images from the initial printing stage in a high-speed image forming apparatus. [Means for solving the problem]

[0005] The present disclosure provides a toner comprising core particles containing a binder resin and toner particles having a shell on the surface of the core particles, the shell contains an oxazoline group and a polyvalent metal; the average thickness of the shell is 1.0 nm or more and 15.0 nm or less; In an electron image of a cross section of the toner particle taken using a transmission electron microscope, The toner has an atomic concentration C(M) of the polyvalent metal in the shell, as determined by energy dispersive X-ray analysis, of 0.0010 atomic % or more and 0.5000 atomic % or less. Effect of the Invention

[0006] According to the present disclosure, it is possible to provide a toner that maintains the charge rise property of the toner even after being left in a harsh environment, and that can output excellent images from the initial printing stage in a high-speed image forming apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] In the present disclosure, the expressions "XX or more and YY or less" and "XX to YY" representing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified. When numerical ranges are stated in stages, the upper and lower limits of each numerical range may be combined in any combination. It is possible to do so.

[0008] The present disclosure provides a toner comprising core particles containing a binder resin and toner particles having a shell on the surface of the core particles, the shell contains an oxazoline group and a polyvalent metal; In an electron image of a cross section of the toner particle taken using a transmission electron microscope, The toner has an atomic concentration C(M) of the polyvalent metal in the shell, as determined by energy dispersive X-ray analysis, of 0.0010 atomic % or more and 0.5000 atomic % or less.

[0009] The present inventors have found that by incorporating an oxazoline group and a polyvalent metal in the shell, the charge rise property of the toner is maintained even after it is left under harsh conditions. Specifically, it is essential that the shell contains an oxazoline group and a polyvalent metal, and that in an electron image of a cross section of the toner taken with a transmission electron microscope, the atomic concentration C(M) of the polyvalent metal in the shell obtained by energy dispersive X-ray analysis is 0.0010 atomic % or more and 0.50 atomic % or less.

[0010] The present inventors consider the detailed mechanism by which the charge rising property of the toner is maintained even after it is left under harsh conditions to be as follows. Since the oxazoline group is highly hydrophilic, it is likely to orient itself toward the surface of the toner particles when the toner particles are left in a harsh environment such as high temperature and high humidity. When the oxazoline group orients itself toward the surface of the toner particles, the charge flows more easily on the surface of the toner particles, and the charge is lost to the outside of the toner particles, resulting in a decrease in the charge rise property. However, when a polyvalent metal is present in the shell, it is believed that the oxazoline group and the polyvalent metal form a crosslinked structure. The polyvalent metal acts as a crosslinking point, making it difficult for the oxazoline group to move, and changes to the toner particle surface are suppressed even in harsh environments. By suppressing changes to the toner particle surface, the charge rise property is maintained even after being left in harsh conditions. The oxazoline group refers to one having an unopened oxazoline ring.

[0011] In an electron image of a cross section of a toner particle taken with a transmission electron microscope, it is essential that the atomic concentration C(M) of the polyvalent metal in the shell obtained by energy dispersive X-ray analysis is 0.0010 atomic % or more and 0.5000 atomic % or less. By setting C(M) to 0.0010 atomic % or more and 0.5000 atomic % or less, good charge rise property can be obtained at the beginning of printing and after being left in a harsh environment. C(M) is preferably set to 0.0030 atomic % or more and 0.4000 atomic % or less, and more preferably set to 0.0100 atomic % or more and 0.3000 atomic % or less. C(M) can be controlled by the amount of metal added.

[0012] A preferred embodiment of the toner will now be described. The oxazoline concentration of the toner particles obtained by time-of-flight secondary ion mass spectrometry TOF-SIMS is preferably 0.10 mmol / g or more and 10.00 mmol / g or less. When the oxazoline concentration is 0.10 mmol / g or more, the charge rising property is improved. On the other hand, when the oxazoline concentration is 10.00 mmol / g or less, the charge becomes moderate, so that electrostatic aggregation is suppressed and the fluidity of the toner particles is improved. A more preferable range is 1.0 mmol / g or more and 5.00 mmol / g or less. The oxazoline concentration can be controlled by the amount and ratio of the oxazoline group-containing monomer added.

[0013] There is no particular limitation on the means for incorporating an oxazoline group into the shell. For example, it is preferable that the shell contains a resin containing an oxazoline group. The resin containing an oxazoline group is It preferably contains a structure represented by formula (1). The content of the structure represented by formula (1) in the resin containing an oxazoline group is preferably about 30% by mass to 98% by mass, and more preferably about 40% by mass to 95% by mass.

[0014] [ka]

[0015] R in formula (1) 1 R is a hydrogen atom or an alkyl group (preferably having 1 to 4 carbon atoms). 1The alkyl group represented by R is preferably a methyl group, an ethyl group, or an isopropyl group. 1 is more preferably a hydrogen atom, a methyl group, or an ethyl group, and even more preferably a hydrogen atom or a methyl group. The structure shown in formula (1) can be introduced by using a polymerizable monomer having an oxazoline group, specifically, 2-vinyl-2-oxazoline or 2-isopropenyl-2-oxazoline.

[0016] The polyvalent metal contained in the shell preferably contains at least one selected from the group consisting of Mg, Al, and Ca, because Mg, Al, and Ca do not affect the color of the toner even if they are contained in the toner. More preferably, it is at least one selected from the group consisting of Mg and Al, which have a small ionic radius. Since the ionic radius is small, it is easy to form a crosslinked structure with the oxazoline group, and therefore it is easy to suppress changes in the toner particle surface after being left in a harsh environment.

[0017] The average shell thickness is preferably 1.0 nm to 15.0 nm. By having the shell layer thickness in this range, the charge rise property can be improved and problems such as contamination of components due to peeling of the shell and toner melting can be suppressed. A more preferable range is from 1.0 nm to 5.0 nm. The thickness of the shell layer can be controlled by the amount of the raw material that becomes the shell added. The shell does not necessarily need to cover the entire surface of the core particle, and the core particle may have a portion that is partially exposed.

[0018] The binder resin is preferably a styrene-acrylic resin, which has low polarity and is less likely to adhere to components such as a developing blade and a developing roller, and can suppress the occurrence of development streaks caused by the adhesion of deteriorated toner to various components. The binder resin is preferably a polyester resin, which is more positively charged than styrene resin or acrylic resin in the electrostatic charge series, and improves the charge rise property in the case of a positively charged toner.

[0019] In addition, the oxazoline group reacts with a carboxy group to form an amide bond. If the core particle contains a carboxy group, an amide bond is formed between the carboxy group of the core particle and the oxazoline group of the shell, improving the adhesion of the film and suppressing the adverse effects of peeling of the shell.

[0020] From the viewpoint of the reaction between the oxazoline group and the carboxy group, the acid value of the binder resin is preferably 1.0 mgKOH / g or more and 30.0 mgKOH / g or less. When the acid value of the binder resin is 1.0 gKOH / g or more, the adhesion between the shell layer and the binder resin is improved. On the other hand, when the acid value is 30.0 mgKOH / g or less, the distortion between the core and shell due to excessive crosslinking is reduced, and the adverse effects such as toner fusion caused by toner cracking can be suppressed. More preferably, it is 3.0 mgKOH / g or more and 30.0 mgKOH / g or less, and even more preferably, it is 8.0 mgKOH / g or more and 15.0 mgKOH / g or less. The acid value of the binder resin can be controlled by the type and amount of the raw materials used.

[0021] The method for producing the toner particles is not particularly limited. From the viewpoint of efficiently introducing a polyvalent metal into the shell, a method for producing the toner particles in an aqueous medium, such as a suspension polymerization method, an emulsion aggregation method, or a dissolution suspension method, is preferred. As the dispersion stabilizer for the toner particles in the suspension polymerization method, inorganic and organic dispersion stabilizers are known, but it is preferable to use an inorganic dispersion stabilizer as the poorly water-soluble inorganic fine particles. Note that an organic dispersion stabilizer (e.g., a surfactant) may be used in combination with the poorly water-soluble inorganic fine particles. The poorly water-soluble inorganic fine particles act as a dispersion stabilizer for the polymerizable monomer composition present in the dispersion liquid during the granulation process of toner particles. Here, the poorly water-soluble fine particles refer to those having a solubility in water (measurement temperature: 60°C) of 10 or less in a specific pH range (for example, 4.0 to 10.0) and an average volume particle size of 1.0 μm or less.

[0022] Examples of poorly water-soluble inorganic fine particles include inorganic dispersion stabilizers (poorly water-soluble inorganic dispersion stabilizers) such as calcium phosphate, magnesium phosphate, aluminum phosphate, zinc phosphate, magnesium carbonate, calcium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, bentonite, silica, and alumina. Among these, magnesium hydroxide is preferably used because it has a sharp particle size distribution and can easily introduce metal elements into the shell. When magnesium hydroxide particles are produced, magnesium remains in the water. With magnesium remaining in the water, an oxazoline group-containing compound is added to form a shell, and magnesium is introduced into the inside of the shell containing the oxazoline group. A detailed production example will be described later.

[0023] In the emulsion polymerization method, when emulsified particles are aggregated and coalesced, a pH adjuster, an aggregating agent, a stabilizer, etc. are added to and mixed in an aqueous medium, and temperature, mechanical power, etc. are appropriately applied to form toner particles in the aqueous medium. Examples of the pH adjuster include alkalis such as ammonia, sodium hydroxide, and sodium hydrogen carbonate, and acids such as nitric acid and citric acid. Examples of the flocculant include monovalent metal salts such as sodium and potassium, divalent metal salts such as calcium and magnesium, trivalent metal salts such as iron and aluminum, and alcohols such as methanol, ethanol, and propanol. Specifically, for example, aluminum sulfate can be used. The stabilizer mainly includes a polar surfactant itself or an aqueous medium containing the same, etc. For example, when the polar surfactant contained in each particle dispersion is anionic, a cationic stabilizer can be selected.

[0024] These pH adjusters, flocculants and stabilizers may be used alone or in combination of two or more. Among these, aluminum sulfate and magnesium chloride are preferred because they allow the polyvalent metal to be easily introduced into the shell. By adding an organic compound to form a shell, a polyvalent metal is introduced into the inside of the shell containing the oxazoline group. The polyvalent metal is preferably Mg derived from magnesium hydroxide, Mg derived from magnesium chloride, or Al derived from aluminum sulfate.

[0025] [Binding resin] The resin that can be used as the binder resin is not particularly limited, and resins that are conventionally used in toners can be used, such as polyester resins, vinyl resins, polyamide resins, furan resins, epoxy resins, xylene resins, and silicone resins. Preferably, the binder resin includes at least one selected from the group consisting of vinyl resins and polyester resins. Among the vinyl resins, styrene-acrylic resins are preferred. Examples of the styrene-acrylic resin include the following copolymers of styrene-based monomers and unsaturated carboxylic acid esters.

[0026] Examples of polymerizable monomers capable of forming the vinyl resin include styrene monomers such as styrene, α-methylstyrene, and divinylbenzene; unsaturated carboxylic acid esters such as methyl acrylate, butyl acrylate, methyl methacrylate, 2-hydroxyethyl methacrylate, t-butyl methacrylate, and 2-ethylhexyl methacrylate; unsaturated carboxylic acids such as acrylic acid and methacrylic acid; unsaturated dicarboxylic acids such as maleic acid; unsaturated dicarboxylic anhydrides such as maleic anhydride; nitrile vinyl monomers such as acrylonitrile; halogen-containing vinyl monomers such as vinyl chloride; and nitro vinyl monomers such as nitrostyrene. These may be used alone or in combination.

[0027] When using polyester resin, known polyester resins can be used.Specific examples include dibasic acids and their derivatives (carboxylic acid halides, esters, acid anhydrides) and polycondensates of dihydric alcohols.If necessary, trivalent or higher polybasic acids and their derivatives (carboxylic acid halides, esters, acid anhydrides), monobasic acids, trivalent or higher alcohols, monohydric alcohols, etc. may be used.

[0028] Examples of dibasic acids include aliphatic dibasic acids such as maleic acid, fumaric acid, itaconic acid, oxalic acid, malonic acid, succinic acid, dodecylsuccinic acid, dodecenylsuccinic acid, adipic acid, azelaic acid, sebacic acid, and decane-1,10-dicarboxylic acid; and aromatic dibasic acids such as phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, tetrabromophthalic acid, tetrachlorophthalic acid, HET acid, himic acid, isophthalic acid, terephthalic acid, and 2,6-naphthalenedicarboxylic acid. Furthermore, examples of derivatives of dibasic acids include carboxylic acid halides, esters and acid anhydrides of the above aliphatic dibasic acids and aromatic dibasic acids.

[0029] On the other hand, examples of dihydric alcohols include acyclic aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, and neopentyl glycol; bisphenols such as bisphenol A and bisphenol F; alkylene oxide adducts of bisphenol A such as an ethylene oxide adduct of bisphenol A and a propylene oxide adduct of bisphenol A; and aralkylene glycols such as xylylenediglycol. Examples of trivalent or higher polybasic acids and anhydrides thereof include trimellitic acid, trimellitic anhydride, pyromellitic acid, and pyromellitic anhydride.

[0030] As described above, it is preferable that the shell contains a resin containing an oxazoline group, and that the resin containing an oxazoline group contains a structure represented by formula (1). The resin containing an oxazoline group is preferably a vinyl resin. In addition to the polymerizable monomer that forms the structure represented by formula (1) having an oxazoline group, the above-mentioned polymerizable monomers that can form a vinyl resin can be used. Copolymers of oxazoline-containing monomers such as 2-vinyl-2-oxazoline and 2-isopropenyl-2-oxazoline and unsaturated carboxylic acid esters are preferred. The content of the shell in the toner particles is preferably about 0.5 to 8.0 parts by mass, and more preferably about 1.0 to 4.0 parts by mass, relative to 100 parts by mass of the core particles.

[0031] [Coloring agent] The toner may contain a colorant. The colorants include the following: Examples of black colorants include carbon black, and a mixture of a yellow colorant, a magenta colorant, and a cyan colorant toned to black. As the colorant, a pigment may be used alone, but it is more preferable to use a dye and a pigment in combination to improve the clarity of the colorant from the viewpoint of the image quality of a full-color image. Magenta colored pigments include: CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 57:1, 58, 60, 63, 64, 68, 81:1, 83, 87, 88, 89, 90, 112, 114, 122, 123, 146, 147, 150, 163, 184, 202, 206, 207, 209, 238, 269, 282; CI Pigment Violet 19; CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35. Magenta coloring dyes include: CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, 27; CI Disperse Violet 1, and other solvent dyes; CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; and CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28, and other basic dyes.

[0032] Cyan coloring pigments include the following: CI Pigment Blue 2, 3, 15:2, 15:3, 15:4, 16, 17; CI Vat Blue 6; CI Acid Blue 45, copper phthalocyanine pigments having 1 to 5 phthalimidomethyl groups substituted on the phthalocyanine skeleton. Cyan coloring dyes include CI Solvent Blue 70. Yellow coloring pigments include: CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65, 73, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 185; CI Vat Yellow 1, 3, 20. Yellow coloring dyes include CI Solvent Yellow 162. The amount of the colorant used is preferably 0.1 parts by mass or more and 30.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin.

[0033] [wax] The toner preferably contains a wax. Examples of the wax include the following. Hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of hydrocarbon waxes such as oxidized polyethylene wax or block copolymers thereof; waxes whose main component is fatty acid esters such as carnauba wax; and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax. Further examples include the following: saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and parinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; esters of fatty acids such as palmitic acid, stearic acid, behenic acid, and montanic acid with alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, hexamethylene Saturated fatty acid bisamides such as bisstearamide; unsaturated fatty acid amides such as ethylene bisoleamide, hexamethylene bisoleamide, N,N' dioleyl adipamide, and N,N' dioleyl sebacamide; aromatic bisamides such as m-xylene bisstearamide and N,N' distearyl isophthalamide; fatty acid metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; waxes grafted onto aliphatic hydrocarbon waxes using vinyl monomers such as styrene and acrylic acid; partial esters of fatty acids and polyhydric alcohols, such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats.

[0034] Among these waxes, from the viewpoint of improving low-temperature fixing property and anti-wrapping property after fixing, hydrocarbon waxes such as paraffin wax and Fischer-Tropsch wax are preferred. The content of the wax is preferably 0.5 parts by mass or more and 25.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin. From the viewpoint of achieving both storage stability and high-temperature offset resistance of the toner, it is preferable that the peak temperature of the maximum endothermic peak present in the temperature range of 30°C or more and 200°C or less in the endothermic curve upon temperature rise measured by a differential scanning calorimeter (DSC) is 50°C or more and 110°C or less.

[0035] [Charge control agent] If necessary, the toner may contain a charge control agent. As the charge control agent, known substances can be used. The charge control agent may be added internally or externally to the toner particles. The amount of the charge control agent added is preferably 0.2 parts by mass or more and 10.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin.

[0036] [Career] The toner may be mixed with a magnetic carrier and used as a two-component developer, since this allows stable images to be obtained over a long period of time. As the magnetic carrier, the following known materials can be used: iron powder with an oxidized surface, or unoxidized iron powder, iron, lithium, calcium, magnesium, nickel, copper, zinc, etc. Metal particles such as lead, cobalt, manganese, chromium, and rare earth elements, alloy particles, oxide particles, and magnetic materials such as ferrite, as well as magnetic material-dispersed resin carriers (so-called resin carriers) that contain magnetic materials and a binder resin that holds the magnetic materials in a dispersed state.

[0037] The toner particles may be produced by any method. For example, a method of producing a toner directly in a hydrophilic medium, such as an emulsion aggregation method, a dissolution suspension method, or a suspension polymerization method, may be used. A pulverization method may also be used, and the toner obtained by the pulverization method may be thermally spheronized. The production method using the pulverization method will be described below. In the pulverization method, the resin, which is an essential component, is mixed with optional components such as a colorant, a wax, and a charge control agent, and the resulting mixture is melt-kneaded. The resulting melt-kneaded product is then pulverized and classified to obtain core particles having a desired particle size.

[0038] The formation of the shell that covers the core particles is preferably carried out by a method in which the core particles are dispersed in an aqueous medium and a material for forming the shell is added to the aqueous medium. After adding the core particles to the aqueous medium, the method of dispersing the core particles well in the aqueous medium includes a method of mechanically dispersing the core particles in the aqueous medium using a device capable of strongly stirring the dispersion liquid, and a method of dispersing the core particles in an aqueous medium containing a dispersant. The method using a dispersant is advantageous in that the core particles are uniformly dispersed in the aqueous medium, and therefore the shell can be easily formed without exposing the surface of the core particles. As an apparatus capable of vigorously stirring the dispersion, an apparatus such as Hivismix (manufactured by Primix Co., Ltd.) is preferable.

[0039] The temperature at which the shell is formed is preferably 65° C. or higher, and more preferably 70° C. or higher. By forming the shell within such a temperature range, the formation of the shell can be smoothly promoted while coalescence of the formed toner particles can be suppressed. After the shell is formed as described above, the dispersion liquid containing the core particles covered with the shell is cooled to room temperature to obtain a dispersion liquid of toner particles. Thereafter, if necessary, a washing step for washing the toner particles, a drying step for drying the toner particles, and an external addition step for attaching an external additive to the surface of the toner particles are performed to obtain a toner.

[0040] If necessary, an external additive may be attached to the surface of the toner particles. A suitable method for attaching an external additive to the surface of the toner particles obtained by the above method includes a method of mixing the toner particles and the external additive using a mixer such as an FM mixer (manufactured by Nippon Coke & Engineering Co., Ltd.) while adjusting conditions so that the external additive is not embedded in the surface of the toner particles.

[0041] The methods for measuring various physical properties will be described below. <Identification of resins contained in core particles and shell> The composition and ratio of the constituent compounds of the resin contained in the core particle and the shell are identified using a pyrolysis gas chromatography mass spectrometer (hereinafter also referred to as "pyrolysis GC / MS") and NMR. Note that if the resin contained in the core and the shell can be obtained separately, it can also be measured separately.

[0042] Pyrolysis GC / MS is used to analyze the types of constituent compounds of resins. The types of constituent compounds are identified by analyzing the mass spectrum of the components of the resin decomposition products that are generated when the resin is pyrolyzed at 550℃ to 700℃. The specific measurement conditions are as follows: [Measurement conditions for pyrolysis GC / MS] Pyrolysis device: JPS-700 (Japan Analysis Industry) Decomposition temperature: 590℃ GC / MS equipment: Focus GC / ISQ (Thermo Fisher) Column: HP-5MS, length 60 m, inner diameter 0.25 mm, film thickness 0.25 μm Inlet temperature: 200℃ Flow pressure: 100kPa Split: 50mL / min MS ionization: EI Ion source temperature: 200℃ Mass Range 45-650

[0043] The ratio of the constituent compounds of the identified resin was then determined by 1 The structure was determined by nuclear magnetic resonance spectroscopy ( 1 H-NMR [400 MHz, CDCl3, room temperature (25 °C)]. Measuring device: FT NMR device JNM-EX400 (manufactured by JEOL Ltd.) Measurement frequency: 400MHz Pulse condition: 5.0μs Frequency range: 10500Hz Number of times accumulated: 1024 The molar ratio of each monomer component is determined from the integral value of the obtained spectrum, and the composition ratio (mass %) is calculated based on this.

[0044] <Isolation of toner particles from toner> When toner particles are used as a sample, toner particles obtained by removing external additives from the toner by the following method can also be used. (1) Place 5 g of toner containing external additives in a sample bottle and add 200 mL of methanol. If necessary, add a few drops of a surfactant. As a surfactant, "Contaminon N" (a 10% aqueous solution of a nonionic surfactant, anionic surfactant, and organic builder, a pH 7 neutral detergent for cleaning precision measuring instruments, manufactured by Wako Pure Chemical Industries, Ltd.) can be used. (2) Disperse the sample in an ultrasonic cleaner for 5 minutes to separate the external additives. (3) The toner particles and the external additives are separated by suction filtration (10 μm membrane filter). (4) The above steps (2) and (3) are repeated three times. By the above-mentioned operation, toner particles from which the external additives have been removed can be obtained.

[0045] <Measuring the amount of metal in the shell of toner particles> The content of polyvalent metals is measured from an electron image of a cross section of a toner particle using a transmission electron microscope (TEM) by the following method. The measurement sample is prepared by mixing a visible light curable embedding resin (D-800, manufactured by Nissin EM Co., Ltd.) with toner, and pressurizing and molding the mixture into a disk shape with a diameter of 7.9 mm and a thickness of 1.0±0.3 mm using a tablet molding machine in an environment of 25°C, and embedding the toner into the sample. The pressure molding conditions are 35 MPa and 60 seconds. From this sample, a thin sample with a film thickness of 100 nm is cut out using an ultra-microtome (EM UC7: manufactured by Leica Co., Ltd.) equipped with a diamond blade at a cutting speed of 0.6 mm / s. This sample is magnified 500,000 times using a transmission electron microscope (TEM) (JEM2800 type: manufactured by JEOL Ltd.) under conditions of an acceleration voltage of 200 V and an electron beam probe size of 1 mm, and the cross section of the toner particle is observed. The cross section to be observed is to have a major axis of ±10% of the weight average particle diameter (D4) of the toner particle to be observed. The shell and core particles can be distinguished from each other based on the type and concentration of the constituent elements of the shell and the core. For example, if the shell contains an oxazoline group and the core particle is made of a polyester resin, the oxazoline group contains nitrogen, and therefore the region containing the nitrogen element can be distinguished as the shell. Next, the spectrum of the constituent elements of the cross section of the obtained toner particle is collected using an energy dispersive X-ray dispersion method (EDS: NSS Thermo electron). Quantitative analysis is performed inside the shell using the Cliff-Lorimer method, and the polyvalent metal content C(M)atomic% is calculated by averaging measurements taken at 10 points inside the shell of the same toner particle. C(M)atomic% is the atomic weight fraction when all elements detected during analysis are taken as 100%. The analysis conditions for the Cliff-Lorimer method are qualitative sensitivity 5, overvoltage 1.5 keV, and number of oxygen atoms 0, and matrix correction is performed to correct for the effects of coexisting elements before calculation. The above measurement is carried out for 20 toner particles, and the arithmetic average value is adopted. (Methods to eliminate the effects of external additives containing polyvalent metals) When an external additive containing a polyvalent metal is attached to the toner particles, the influence of the polyvalent metal derived from the external additive can be removed by the following method. The shape of the external additive can be identified from the constituent elements of the external additive. A region of only the shell is selected from the cross section of the toner particle to be observed, avoiding the external additive, and a spectrum is collected by the energy dispersive X-ray dispersion method.

[0046] <Measuring the average shell thickness> The measurement sample is prepared by mixing a visible light curable embedding resin (D-800, manufactured by Nissin EM Co., Ltd.) with toner, and pressurizing the mixture into a disk shape with a diameter of 7.9 mm and a thickness of 1.0±0.3 mm using a tablet press at 25°C. The pressurization conditions are 35 MPa and 60 seconds. The sample was then cut using a diamond blade ultramicrotome (EM UC7:L Using a cutting tool (manufactured by Eica), a thin sample with a film thickness of 100 nm is cut out at a cutting speed of 0.6 mm / s. The obtained sample is stained with osmium tetroxide. This operation selectively stains only the shell in the toner particle. Next, the cross section of the obtained thin sample is photographed at 500,000 times magnification using a transmission electron microscope (TEM) (JEM2800 type: manufactured by JEOL Ltd.) under conditions of an acceleration voltage of 200 V and an electron beam probe size of 1 mm. The TEM image is then analyzed using image analysis software to measure the shell thickness. Specifically, two perpendicular lines are drawn at approximately the center of the cross section of a toner particle, and the shell thickness is measured at each of the four points where the two lines intersect with the shell. The arithmetic average of the thicknesses measured at the four points is regarded as the shell thickness of the toner particle. The shell thickness is then measured for each of 20 toner particles, and the number-average value of the measured thicknesses is regarded as the evaluation value of the toner being measured (average shell thickness).

[0047] <Method of measuring weight average particle size (D4) of toner particles> The weight-average particle diameter (D4) of the toner particles is measured with an effective measurement channel count of 25,000 channels using a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube, and the accompanying dedicated software, "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.), for setting measurement conditions and analyzing measurement data. The weight-average particle diameter (D4) of the toner particles is measured with an effective measurement channel count of 25,000 channels, and the measurement data is analyzed and calculated. The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1 mass %, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.). Before carrying out the measurements and analyses, the dedicated software is set up as follows. In the "Change Standard Measurement Method (SOM) Screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter, Inc.). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1,600 μA, the gain to 2, the electrolyte to ISOTON II, and check the aperture tube flush after measurement. In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.

[0048] The specific measurement method is as follows. (1) Pour about 200 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) Approximately 30 mL of the aqueous electrolyte solution is placed in a 100 mL flat-bottom glass beaker, and approximately 0.3 mL of the diluent described below is added as a dispersant. Dilution solution: "Contaminon N" (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water. (3) A specified amount of ion-exchanged water is placed in the water tank of the ultrasonic disperser described below, which has two oscillators with an oscillation frequency of 50 kHz built in with a phase shift of 180 degrees and an electrical output of 120 W, and approximately 2 mL of the Conaminon N is added to this water tank. Ultrasonic disperser: "Ultrasonic Dispersion System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 15°C or higher and 40°C or lower. (6) Using a pipette, add the electrolytic solution (5) in which the toner has been dispersed to the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the Analysis / Volume Statistics (Arithmetic Mean) screen is the weight-average particle size (D4).

[0049] <Oxazoline concentration measurement of toner particles> The oxazoline concentration on the toner particle surface is measured using a TOF-SIMS (TRIFT-IV, manufactured by ULVAC-PHI, Inc.) under the following analytical conditions. Sample preparation: Toner particles are deposited on an indium sheet. Sample preparation: None Primary ion: Au + Acceleration voltage: 30 kV Charge neutralization mode: On Measurement mode: Positive Raster size: 100μm Accumulation time: 180 seconds The oxazoline group concentration is calculated from the intensity derived from the oxazoline group in the secondary ion mass spectrum (vertical axis: normalized intensity, horizontal axis: mass number = m / z) obtained under the above conditions, using a calibration curve created based on samples of known concentration. The normalized intensity is calculated from (mass spectrum intensity derived from oxazoline group) / (total of all ion intensities of mass numbers m / z = 1 to 1850). Specifically, three or more samples of known concentration are prepared, and a calibration curve (vertical axis: concentration = mmol / g, horizontal axis: normalized intensity) is created. The oxazoline concentration is calculated based on the calibration curve from the normalized intensity derived from the oxazoline group obtained from the toner particles.

[0050] <Acid value> The acid value of a resin, such as a binder resin, is the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of a sample. The acid value of a polar resin is measured in accordance with JIS K 0070-1992, and specifically, it is measured according to the following procedure. Titration is performed using a 0.1 mol / L potassium hydroxide ethyl alcohol solution (Kishida Chemical Co., Ltd.). The factor of the potassium hydroxide ethyl alcohol solution can be determined using a potentiometric titrator (Kyoto Electronics Manufacturing Co., Ltd., potentiometric titration measuring device AT-510 (product name)). 100 mL of 0.100 mol / L hydrochloric acid is placed in a 250 mL tall beaker and titrated with the potassium hydroxide ethyl alcohol solution to determine the amount of potassium hydroxide ethyl alcohol solution required for neutralization. The 0.100 mol / L hydrochloric acid used is prepared in accordance with JIS K 8001-1998.

[0051] The conditions for measuring the acid value are shown below. Titrator: Potentiometric titrator AT-510 (product name, manufactured by Kyoto Electronics Manufacturing Co., Ltd.) Electrode: Composite glass electrode double junction type (Kyoto Electronics Manufacturing Co., Ltd.) Control software for titrator: AT-WIN Titration analysis software: Tview The titration parameters and control parameters during titration are as follows: Titration parameters Titration mode: Blank titration Titration method: Total volume titration Maximum titer: 20mL Waiting time before titration: 30 seconds Titration direction: automatic Control parameters End point potential: 30dE End point potential: 50 dE / dmL End point detection judgment: Not set Control speed mode: Standard Gain: 1 Data collection potential: 4mV Data collection titration volume: 0.1mL

[0052] This test; Weigh out 0.100 g of the sample to be measured into a 250 mL tall beaker, add 150 mL of a mixed solution of toluene / ethanol (3:1), and dissolve for 1 hour. Using the above potentiometric titration apparatus, titrate with the above potassium hydroxide ethyl alcohol solution. Blank test; The titration is carried out in the same manner as above, except that no sample is used (i.e., only the toluene / ethanol (3:1) mixed solution is used). The obtained result is substituted into the following formula to calculate the acid value (Av). Av = [(CB) × f × 5.61] / S (In the formula, Av is the acid value (mgKOH / g), B is the amount of potassium hydroxide ethyl alcohol solution added for the blank test (mL), C is the amount of potassium hydroxide ethyl alcohol solution added for the main test (mL), f is the factor of the potassium hydroxide ethyl alcohol solution, and S is the mass of the sample (g).) EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples. In the examples and comparative examples, the parts and percentages are all based on mass unless otherwise specified.

[0054] <Production of Polyester Resin 1 for Core Particles> In a reaction vessel equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, the amounts of monomers shown in Table 1 were placed, and then 1.5 parts of dibutyltin oxide were added as a catalyst per 100 parts of the total amount of monomers. Next, the temperature was quickly raised to 180°C under normal pressure in a nitrogen atmosphere, and then water was distilled off while heating from 180°C to 210°C at a rate of 10°C / hour to carry out polycondensation. After the temperature reached 210° C., the pressure inside the reaction tank was reduced to 5 kPa or less, and polycondensation was carried out under conditions of 210° C. and 5 kPa or less, to obtain polyester resin 1.

[0055] <Production of polyester resins 2 and 3 for core particles> Polyesters 2 and 3 were produced in the same manner as for Polyester Resin 1, except that the raw materials were changed as shown in Table 1.

[0056] [Table 1] In the table, the abbreviations are as follows: BPA-PO: Bisphenol A propylene oxide 2 mol adduct BPA-EO: Bisphenol A with 2 mol of ethylene oxide

[0057] <Production of Toner 1> (Preparation of Dispersion) In a granulation tank, 250.0 parts of ion-exchanged water and 10.2 parts of magnesium chloride were dissolved to prepare an aqueous magnesium chloride solution. An aqueous solution of 6.2 parts of sodium hydroxide in 50.0 parts of ion-exchanged water was gradually added to the granulation tank while stirring at a peripheral speed of 25 m / s using a TK homomixer (trade name, manufactured by Tokushu Kika Kogyo Co., Ltd.), to obtain a dispersion containing magnesium hydroxide (fine particles).

[0058] (Preparation of Pigment Dispersion Composition) Polymerizable monomer (styrene) 39.0 parts Colorant (CI Pigment Blue 15:3) 7.0 parts The above materials were introduced into an attritor (manufactured by Nippon Coke Corporation) and stirred at 200 rpm at 25° C. for 180 minutes using zirconia beads with a radius of 1.25 mm to prepare a pigment dispersion composition.

[0059] (Preparation of Colorant-Containing Composition) The following materials were placed in a container and mixed and dispersed at a peripheral speed of 20 m / s using a TK homomixer (product name, manufactured by Tokushu Kika Kogyo). 46.0 parts of the above pigment dispersion composition Polymerizable monomer: styrene 31.0 parts Polymerizable monomer: n-butyl acrylate 30.0 parts Charge control agent: FCA-5 (product name, manufactured by Fujikura Chemical) 1.2 parts Crosslinking agent: 0.5 parts divinylbenzene Further, after heating to 60° C., 10.0 parts of a release agent (behenyl behenate) was added, and the mixture was dispersed and mixed for 30 minutes to prepare a colorant-containing composition.

[0060] (Preparation of Polymerizable Monomer Composition Particles) The colorant-containing composition was added to a dispersion liquid containing magnesium hydroxide particles, and stirred at a peripheral speed of 30 m / s with a TK homomixer (trade name, manufactured by Tokushu Kika Kogyo) under a nitrogen atmosphere at a temperature of 60° C. To this was added 9.0 parts of a polymerization initiator t-butyl peroxypivalate (manufactured by Nippon Oil & Fats Corporation, trade name "Perbutyl PV", molecular weight: 174.2, 10-hour half-life temperature: 58° C.) to prepare a dispersion liquid containing polymerizable monomer composition particles. Next, the dispersion liquid of the polymerizable monomer composition particles was transferred to another tank, and the temperature was raised to 70° C. while stirring with a paddle stirring blade to carry out a polymerization reaction. When the conversion rate of the polymerizable monomer reached 95%, the temperature was raised to 90°C, and 0.2 parts of methyl methacrylate as a polymerizable monomer for the shell, 1.8 parts of 2-vinyl-2-oxazoline, and 10 parts of ion-exchanged water as a water-soluble initiator were added to the mixture to form a mixture. A polymerization reaction was carried out at 90° C. for 3 hours to obtain a polymerization reaction liquid (polymerization slurry) containing toner particles 1. After cooling, sulfuric acid was added to adjust the pH to 6.5 or less, and the mixture was stirred for 2 hours to dissolve the poorly water-soluble inorganic fine particles on the surface of the toner particles. The dispersion of the toner particles was filtered, washed with water, and then dried at a temperature of 40°C for 48 hours to obtain toner particles 1 having a core-shell structure and a weight average particle size (D4) of 6.8 μm.

[0061] (External addition process) 100.0 parts of toner particles 1 and 1.5 parts of dry silica particles ("AEROSIL (registered trademark) REA90" manufactured by Nippon Aerosil Co., Ltd.: positively charged hydrophobically treated silica particles) were mixed for 3 minutes using an FM mixer (manufactured by Nippon Coke and Engineering Co., Ltd.) to adhere the silica particles to the toner particles 1. The mixture was then sieved through a 300 mesh (opening 48 μm) to obtain toner 1.

[0062] <Production of Toner 2> In preparing the polymerizable monomer composition particles of toner 1, 0.4 parts of methyl methacrylate and 3.6 parts of 2-vinyl-2-oxazoline were used as the polymerizable monomer for the shell, and 10 parts of ion-exchanged water was used as the water-soluble initiator. Toner 2 was obtained in the same manner as toner 1, except that an aqueous solution in which 0.4 parts of methyl ether was dissolved was added, and an aqueous solution in which 0.5 parts of magnesium chloride was dissolved was further added to 5.0 parts of ion-exchanged water.

[0063] <Production of Toner 3> In preparing the polymerizable monomer composition particles of toner 1, 0.8 parts of methyl methacrylate and 7.2 parts of 2-vinyl-2-oxazoline were used as the polymerizable monomer for the shell, and 2,2'-azobis(N-butyl-2-methylpropionate) was used as the water-soluble initiator in 20 parts of ion-exchanged water. Toner 3 was obtained in the same manner as Toner 1, except that an aqueous solution in which 0.8 parts of methyl ether was dissolved was added, and an aqueous solution in which 1.0 parts of magnesium chloride was dissolved in 5.0 parts of ion-exchanged water was further added.

[0064] <Production of Toner 4> Toner 4 was obtained in the same manner as Toner 1, except that in the preparation of the polymerizable monomer composition particles of Toner 1, 30 parts of an aqueous solution of an oxazoline group-containing resin for the shell ("Epocross WS-300" manufactured by Nippon Shokubai Co., Ltd., solids concentration: 10% by mass) was added instead of the polymerizable monomer for the shell.

[0065] <Production of Toner 5> (Production of Polyester Resin A) The following materials were added to an autoclave equipped with a pressure reducing device, a water separating device, a nitrogen gas introducing device, a temperature measuring device and a stirring device. Terephthalic acid 32.3 parts (50.0 mol%) Bisphenol A-propylene oxide 2 mole adduct 67.7 parts (50.0 mol%) Potassium titanium oxalate (catalyst) 0.02 parts Subsequently, the reaction was carried out under a nitrogen atmosphere and normal pressure at 220° C. until the desired molecular weight was reached. After lowering the temperature, the mixture was pulverized to obtain a polyester resin A. The acid value of the polyester resin A was 8.0 mgKOH / g.

[0066] (Preparation of Dispersion) In a granulation tank, 100.0 parts of ion-exchanged water, 2.0 parts of sodium phosphate, and 0.9 parts of 10% by mass hydrochloric acid were added to prepare an aqueous sodium phosphate solution, which was then heated to 50°C. An aqueous calcium chloride solution prepared by dissolving 1.2 parts of calcium chloride hexahydrate in 8.2 parts of ion-exchanged water was added to the granulation tank, and the solution was stirred for 30 minutes at a peripheral speed of 25 m / s using a TK homomixer (trade name, manufactured by Tokushu Kika Kogyo Co., Ltd.). As a result, a dispersion (aqueous dispersion) containing calcium phosphate (fine particles) as poorly water-soluble inorganic fine particles was obtained.

[0067] (Preparation of Pigment Dispersion Composition) Polymerizable monomer (styrene) 39.0 parts Colorant (CI Pigment Blue 15:3) 7.0 parts The above materials were introduced into an attritor (manufactured by Nippon Coke Corporation) and stirred at 200 rpm at 25° C. for 180 minutes using zirconia beads with a radius of 1.25 mm to prepare a pigment dispersion composition.

[0068] (Preparation of Colorant-Containing Composition) The following materials were placed in a container and mixed and dispersed at a peripheral speed of 20 m / s using a TK homomixer (product name, manufactured by Tokushu Kika Kogyo). 46.0 parts of the above pigment dispersion composition Polymerizable monomer: styrene 31.0 parts Polymerizable monomer: n-butyl acrylate 30.0 parts Polyester resin A 2.0 parts Crosslinking agent: 0.5 parts divinylbenzene Further, after heating to 60° C., 10.0 parts of a release agent (behenyl behenate) was added, and the mixture was dispersed and mixed for 30 minutes to prepare a colorant-containing composition.

[0069] (Preparation of Polymerizable Monomer Composition Particles) The colorant-containing composition was added to a dispersion liquid containing calcium phosphate microparticles, and stirred at a peripheral speed of 30 m / s with a TK homomixer (trade name, manufactured by Tokushu Kika Kogyo) under a nitrogen atmosphere at a temperature of 60° C. To this was added 9.0 parts of a polymerization initiator t-butyl peroxypivalate (manufactured by Nippon Oil & Fats Corporation, trade name "Perbutyl PV", molecular weight: 174.2, 10-hour half-life temperature: 58° C.) to prepare a dispersion liquid containing polymerizable monomer composition particles. Next, the dispersion liquid of the above polymerizable monomer composition particles was transferred to another tank, and the temperature was raised to 70°C while stirring with a paddle stirring blade. After reacting at 70°C for 5 hours, the liquid temperature was increased to 85°C and the reaction was continued for another 2 hours. After the polymerization reaction was completed, the obtained slurry was cooled and allowed to stand to allow the particles to settle, and a portion of the supernatant liquid was removed to obtain a core slurry having a solid content of 25% by mass.

[0070] (Shell formation) A 1 L three-neck flask equipped with a thermometer and a stirring blade was placed in a water bath, and 400 g of the obtained core slurry was placed in the flask. The temperature inside the flask was then adjusted to 30° C. using the water bath. Next, an aqueous solution of an oxazoline group-containing resin ("Epocross WS-300" manufactured by Nippon Shokubai Co., Ltd., solid content concentration: 10% by mass) in an amount shown in Table 2 was added to the flask. The amount added in Table 2 indicates the number of parts of the oxazoline group-containing resin (solid content) relative to 100 parts of core particles in the core slurry. The contents of the flask were then stirred at a rotation speed of 200 rpm for 1 hour, after which 300 g of ion-exchanged water was added to the flask. Subsequently, 6 mL of an aqueous ammonia solution having a concentration of 1% by mass was added to the flask. Next, the temperature inside the flask was raised to 55° C. at a rate of 0.5° C. / min while stirring the contents of the flask at a rotation speed of 150 rpm. Next, the temperature (55° C.) was maintained for 2 hours while stirring the contents of the flask at a rotation speed of 100 rpm. Subsequently, an aqueous ammonia solution having a concentration of 1% by mass was added to the flask to adjust the pH of the content in the flask to 7. Subsequently, the obtained slurry was cooled to room temperature (about 25° C.). Thereafter, while maintaining stirring, dilute hydrochloric acid was added until the pH reached 1.5 to dissolve the dispersion stabilizer. The solid content was filtered off, thoroughly washed with ion-exchanged water, and then vacuum-dried at 40° C. for 24 hours to obtain toner particles 5.

[0071] (External addition process) Toner 5 was obtained in the same manner as in the external addition step of toner particles 1, except that toner particles 5 were used.

[0072] <Production of Toner Particles 6> (Production of core particles) Polyester resin 1: 90.0 parts CI Pigment Blue 15:3 (copper phthalocyanine): 5.0 parts Ester wax (behenyl behenate: melting point 72°C): 15.0 parts Fischer-Tropsch wax (Sasol C105, melting point: 105°C): 2.0 copies The above materials were premixed in a Mitsui Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and then melt-kneaded using a twin-screw extruder (product name: PCM-30, manufactured by Ikegai Iron Works Co., Ltd.) with the temperature set so that the molten temperature at the discharge outlet was 140°C. The kneaded product obtained was cooled, coarsely pulverized with a hammer mill, and then finely pulverized with a pulverizer (product name: Turbo Mill T250, manufactured by Turbo Kogyo Co., Ltd.). The finely pulverized powder obtained was classified with a multi-division classifier utilizing the Coanda effect to obtain core particles having a weight average particle size (D4) of 6.8 μm.

[0073] (Shell formation) A 1 L three-neck flask equipped with a thermometer and a stirring blade was placed in a water bath, and 300 g of ion-exchanged water was placed in the flask. The temperature inside the flask was then adjusted to 30° C. using the water bath. Next, an aqueous solution of an oxazoline group-containing resin ("Epocross WS-300" manufactured by Nippon Shokubai Co., Ltd., solids concentration: 10% by mass) in the amount shown in Table 2 was poured into the flask. Further, an aqueous solution of magnesium chloride prepared by dissolving 0.5 parts (1.5 g) of magnesium chloride as solid content in 10 g of ion-exchanged water was added. Next, 300 g of the toner cores prepared in the above-mentioned procedure was added to the flask, and the contents of the flask were stirred at a rotation speed of 200 rpm for 1 hour, after which 300 g of ion-exchanged water was added to the flask. Subsequently, 6 mL of an aqueous ammonia solution having a concentration of 1% by mass was added to the flask. Next, the temperature inside the flask was raised to 55° C. at a rate of 0.5° C. / min while stirring the contents of the flask at a rotation speed of 150 rpm. Next, the temperature (55° C.) was maintained for 2 hours while stirring the contents of the flask at a rotation speed of 100 rpm. Subsequently, an aqueous ammonia solution having a concentration of 1% by mass was added to the flask to adjust the pH of the flask content to 7. Subsequently, the obtained slurry was cooled to room temperature (about 25° C.), washed, filtered, and separated into solid and liquid, and then dried using a vacuum dryer to obtain toner particles 6.

[0074] (External addition process) Toner 6 was obtained in the same manner as in the external addition step of toner particles 1, except that toner particles 6 were used.

[0075] <Production of Toner Particles 7 to 12> Toner particles 7 to 12 were obtained by the same production method as for toner particles 6, except that the resin was changed as shown in Table 2.

[0076] [Table 2] The amount added in Table 2 indicates the number of parts of the oxazoline group-containing resin (solid content) relative to 100 parts of the core particles.

[0077] <Toner particles 13> (Preparation of Polyester Resin Particle Dispersion) 1,200 parts polyester resin -500 parts deionized water The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted. While thoroughly stirring at 7,800 rpm using a homogenizer (IKA Ultra Turrax T50), 0.1 mol / L sodium bicarbonate was added to adjust the pH to greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining a polyester resin particle dispersion. The particle size distribution of this polyester resin particle dispersion was measured using a particle size measuring device (LA-920, manufactured by Horiba, Ltd.), and the number-average particle size of the polyester resin particle dispersion contained therein was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0078] (Preparation of Wax Particle Dispersion) -500 parts deionized water Wax (hydrocarbon wax; maximum endothermic peak temperature 77°C) 250 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted. While thoroughly stirring at 7,800 rpm using a homogenizer (IKA Ultra Turrax T50), 0.1 mol / L sodium bicarbonate was added to adjust the pH to greater than 7.0. Thereafter, a mixed solution of 5 parts of sodium dodecylbenzenesulfonate and 245 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the wax particles. The particle size distribution of the wax particles contained in this wax particle dispersion was measured using a particle size measuring device (LA-920, manufactured by Horiba, Ltd.), and the number-average particle size of the wax particles contained was 0.35 μm, and no coarse particles exceeding 1 μm were observed.

[0079] (Preparation of Colorant Particle Dispersion) CI Pigment Blue 15:3 100 parts Sodium dodecylbenzenesulfonate 5 parts -Ion-exchanged water 400 parts The above was mixed and dispersed using a sand grinder mill. The particle size distribution of the colorant particles contained in this colorant particle dispersion was measured using a particle size measuring device (LA-920, manufactured by Horiba, Ltd.), and the number-average particle size of the colorant particles contained was 0.2 μm, and no coarse particles exceeding 1 μm were observed.

[0080] (Production of core particles) Polyester resin particle dispersion 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts A polyester resin particle dispersion, a wax particle dispersion, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, anchor blade with baffles) and mixed uniformly. Meanwhile, a colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. One part of an aluminum sulfate aqueous solution was added dropwise as a solid while stirring the obtained mixed dispersion to form aggregated particles. After the dropwise addition was completed, the system was purged with nitrogen and the temperature was maintained at 50° C. for 1 hour and then at 55° C. for 1 hour. The temperature was then raised to 90°C and maintained for 30 minutes. The temperature was then lowered to 63°C and maintained for 3 hours to form fused particles. After the specified time had elapsed, the temperature was lowered to 30°C at a rate of 0.5°C per minute, and ion-exchanged water was added to adjust the temperature, to obtain a core particle dispersion with a solid content of 25% by mass.

[0081] (Production of toner particles 13) To the above core particle dispersion, an aqueous solution of an oxazoline group-containing resin ("Epocross WS-300" manufactured by Nippon Shokubai Co., Ltd., solid content concentration: 10% by mass) shown in Table 2 was added in the flask. Subsequently, 6 mL of an aqueous ammonia solution having a concentration of 1% by mass was added to the flask. Next, the temperature inside the flask was raised to 55° C. at a rate of 0.5° C. / min while stirring the contents of the flask at a rotation speed of 150 rpm. Next, the temperature (55° C.) was maintained for 2 hours while stirring the contents of the flask at a rotation speed of 100 rpm. Subsequently, an aqueous ammonia solution having a concentration of 1% by mass was added to the flask to adjust the pH of the flask content to 7. Subsequently, the obtained slurry was cooled to room temperature (about 25° C.), washed, filtered, and separated into solid and liquid, and then dried using a vacuum dryer to obtain toner particles 13.

[0082] (External addition process) Toner 13 was obtained in the same manner as in the external addition step of toner particles 1, except that toner particles 13 were used.

[0083] <Production of Toner 14> Toner 14 was obtained in the same manner as Toner 6, except that the resin was changed as shown in Table 2, and the aqueous magnesium chloride solution was not added to the flask in the formation of the shell of Toner 6.

[0084] <Production of Toner 15> The resin was changed as shown in Table 2, and no aqueous magnesium chloride solution was added to the flask in forming the shell of Toner 6. In addition, 6 mL of acetic acid with a concentration of 99% by mass was added while the temperature in the flask was raised to 55° C. at a rate of 0.5° C. / min, and other than this, Toner 15 was obtained in the same manner as Toner 6.

[0085] <Production of Toner 16> (Preparation of Polyester Resin Particle Dispersion) Using polyester resin 1, a polyester resin particle dispersion was obtained in the same manner as in toner 13. (Preparation of Wax Particle Dispersion) A wax resin particle dispersion was obtained in the same manner as in Toner 13. (Preparation of Colorant Particle Dispersion) A colorant particle dispersion was obtained in the same manner as in Toner 13.

[0086] (Preparation of core particles) Polyester resin particle dispersion 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts A polyester resin particle dispersion, a wax particle dispersion, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, anchor blade with baffles) and mixed uniformly. Meanwhile, a colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 3.0 parts of an ammonium sulfate aqueous solution (solid content) was added dropwise to the obtained mixed dispersion while stirring to form aggregated particles. After the dropwise addition was completed, the system was purged with nitrogen and the temperature was maintained at 50° C. for 1 hour and then at 55° C. for 1 hour. The temperature was then raised to 90°C and held there for 30 minutes. The temperature was then lowered to 63°C and held there for 3 hours to form fused particles. After the specified time had elapsed, the temperature was lowered to 30°C at a rate of 0.5°C per minute. The mixture was cooled until the solid concentration reached 25% by mass, and ion-exchanged water was added to obtain a core particle dispersion having a solid concentration of 25% by mass.

[0087] (Production of toner particles 16) Toner particles 16 were obtained in the same manner as Toner 13, except that the oxazoline group-containing resin aqueous solution was changed as shown in Table 2. (External addition process) Toner 16 was obtained in the same manner as in the external addition step of toner particles 1, except that toner particles 16 were used.

[0088] <Production of Toner 17> Toner 17 was obtained in the same manner as in the preparation of the polymerizable monomer composition particles of toner 1, except that an aqueous solution in which 2.0 parts of methyl methacrylate was used as the shell polymerizable monomer and 0.2 parts of 2,2'-azobis(N-butyl-2-methylpropionamide) was dissolved in 10 parts of ion-exchanged water as a water-soluble initiator was added.

[0089] <Production of Toner 18> Toner 18 was obtained in the same manner as Toner 1, except that in the preparation of the polymerizable monomer composition particles of Toner 1, an aqueous solution containing 0.8 parts of methyl methacrylate and 7.2 parts of 2-vinyl-2-oxazoline as shell polymerizable monomers, and 0.8 parts of 2,2'-azobis(N-butyl-2-methylpropionamide) as a water-soluble initiator in 20 parts of ion-exchanged water was added, and an aqueous solution containing 2.0 parts of magnesium chloride in 5.0 parts of ion-exchanged water was further added.

[0090] <Production of Toner 19> Toner 19 was obtained in the same manner as Toner 6, except that the resin was changed as shown in Table 2, and in forming the shell of Toner 6, an aqueous magnesium chloride solution prepared by dissolving 0.2 parts (0.6 g) of magnesium chloride as a solid content in 10 g of ion-exchanged water was added to the flask.

[0091] <Physical properties of toners 1 to 19> The above-mentioned various physical properties of Toners 1 to 19 were measured, and the obtained physical properties are shown in Table 3.

[0092] [Table 3] The concentration of the polyvalent metal in the shell is expressed in atomic percent.

[0093] <Image evaluation> The image forming apparatus used was a Hewlett-Packard color laser beam printer (HP LaserJet Enterprise Color M652n), which was modified to have a process speed of 300 mm / sec. The cartridge used was an HP 656X genuine LaserJet toner cartridge (cyan). The product toner was removed from the inside of the cartridge, and after cleaning with an air blower, 300 g of the toner to be evaluated was filled in. The following evaluations were carried out using the image forming apparatus and cartridge described above. The above cartridge was mounted in the cyan station, and dummy cartridges were mounted in the other stations to carry out the evaluation. Furthermore, various potential settings were changed so that development with positively charged toner was possible.

[0094] [Fogging evaluation at initial stage and after exposure to harsh environment] Toner after exposure to harsh conditions was left in a thermostatic chamber at 40°C and 95% RH for 30 days. Fog evaluation was performed using the initial toner before exposure and the toner after exposure. Evaluation conditions were a high temperature and high humidity environment (temperature 32°C / humidity 85% RH), and the reflectance (%) of the non-image area was measured using a REFLECTOMETER MODEL TC-6DS (Tokyo Denshoku Co., Ltd.). The reflectance obtained was subtracted from the reflectance (%) of unused printout paper (standard paper) measured in the same manner, and the result was used for evaluation. The smaller the value, the more suppressed the image fog. The evaluation was done in glossy paper mode on plain paper (HP Brochure Paper 200g, Glossy, HP, 200g / m 2 ) was used. (Evaluation Criteria) A: Less than 0.5% B: 0.5% or more but less than 1.5% C: 1.5% or more and less than 3.0% D: 3.0% or more

[0095] [Development streaks] In a high temperature and humidity environment (temperature 32°C / humidity 85% RH), a horizontal line image with a printing rate of 1% was printed out 30,000 times. After the test, a LETTER size XEROX 4200 paper (XEROX, 75g / m 2 ) and halftone (toner load: 0.3mg / cm 2 The halftone image was printed out and observed for the presence or absence of vertical streaks in the paper ejection direction, and durability was evaluated as follows. (Evaluation Criteria) A: Not occurred B: Vertical stripes in the paper ejection direction appear in 1 to 3 places on the halftone image. C: Four to six vertical streaks in the ejection direction appear on the halftone image. D: Seven or more vertical stripes appear in the halftone image in the paper ejection direction, or the width is 0.5 mm or more.

[0096] [Poor regulation] After completing a test in a low temperature and low humidity environment (15°C, 10% RH) in which 20,000 sheets of horizontal line images with a printing rate of 1% were printed, the toner loading amount was 0.3 mg / cm 2 The amount of spot-like streaks and toner clumps appearing on the halftone images was evaluated. A: Not occurred B: No spot-like streaks, but a few small toner clumps C: There are some spot-like streaks on the edges or 4 or 5 small toner clumps D: Spot-like streaks are present over the entire surface, or there are five or more small or obvious toner clumps.

[0097] [Examples 1 to 13] In Examples 1 to 13, the above evaluations were carried out using toners 1 to 13, respectively. The evaluation results are shown in Table 4.

[0098] [Comparative Examples 1 to 6] In Comparative Examples 1 to 6, the above evaluations were carried out using toners 14 to 19, respectively. The evaluation results are shown in Table 4.

[0099] [Table 4]

Claims

1. A toner comprising core particles containing a binder resin and toner particles having a shell on the surface of the core particles, the shell contains an oxazoline group and a polyvalent metal; the average thickness of the shell is 1.0 nm or more and 15.0 nm or less; In an electron image of a cross section of the toner particle taken using a transmission electron microscope, The toner is characterized in that the atomic concentration C(M) of the polyvalent metal in the shell, as determined by energy dispersive X-ray analysis, is 0.0010 atomic % or more and 0.5000 atomic % or less.

2. 2. The toner according to claim 1, wherein the oxazoline concentration of the toner particles obtained by time-of-flight secondary ion mass spectrometry TOF-SIMS is 0.10 mmol / g or more and 10.00 mmol / g or less.

3. the shell comprises a resin containing an oxazoline group; 3. The toner according to claim 1, wherein the resin containing an oxazoline group comprises a structure represented by the following formula (1): [In formula (1), R 1 is a hydrogen atom or an alkyl group.

4. The polyvalent metal comprises at least one selected from the group consisting of Mg, Al and Ca. The toner according to any one of claims 1 to 3.

5. 5. The toner according to claim 1, wherein the binder resin comprises at least one selected from the group consisting of vinyl resins and polyester resins.

6. 6. The toner according to claim 1, wherein the binder resin contains a styrene-acrylic resin.

7. 6. The toner according to claim 1, wherein the binder resin contains a polyester resin.

8. 8. The toner according to claim 7, wherein the acid value of the polyester resin is from 3.0 mgKOH / g to 30.0 mgKOH / g.

9. The toner according to any one of claims 1 to 8, wherein the polyvalent metal is Mg derived from magnesium hydroxide.

10. The toner according to any one of claims 1 to 8, wherein the polyvalent metal is Al derived from aluminum sulfate.

11. The toner according to any one of claims 1 to 8, wherein the polyvalent metal is Mg derived from magnesium chloride.

Citation Information

Patent Citations

  • Electrophotographic toner

    JP2005250096A

  • Decolorable toner and process for production thereof

    JP2013019971A

  • Toner and method for manufacturing the same

    JP2013109326A

  • Toner for electrostatic latent image development

    JP2018054891A

  • Toner for electrostatic latent image development

    JP2018185466A