Image formation method

The image forming method optimizes toner particle distribution to maintain color reproducibility and scratch resistance by using developers with specific refractive index particles, addressing issues with fillers in electrophotographic methods.

JP7596175B2Active Publication Date: 2024-12-09CANON KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021028014
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-24
Publication Date
2024-12-09
Estimated Expiration
2041-02-24

AI Technical Summary

Technical Problem

Electrophotographic methods face challenges in maintaining color reproducibility and scratch resistance when using fillers to reduce toner raw material costs, leading to issues like light scattering and toner peeling on coated papers.

Method used

An image forming method using developers with toner particles of specific refractive indices, where the content of these particles in stacked toner layers follows a defined relationship, ensuring they are predominantly in lower layers to suppress light scattering and enhance scratch resistance.

Benefits of technology

The method maintains color reproducibility and improves scratch resistance by optimizing the distribution of toner particles with refractive indices 1.5 to 1.7, particularly using calcium carbonate, without impairing color gamut or adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596175000001
    Figure 0007596175000001
  • Figure 0007596175000002
    Figure 0007596175000002
  • Figure 0007596175000003
    Figure 0007596175000003
Patent Text Reader

Abstract

To obtain an image with no loss of color reproducibility and with high scratch resistance even when a filler is used.SOLUTION: An image forming method includes forming toner image by using a first developer, a second developer, and a third developer. Each developer has toner particles containing particles having a refractive index of 1.5 or more and 1.7 or less. At least an area where the first toner image, the second toner image, and the third toner image are laminated is present in a transfer toner image formed on a transfer material. In the area, when A (mass%) is the content of the particles having a refractive index of 1.5 or more and 1.7 or less contained in a toner layer A closest to a surface of the transfer material, B is the content of the particles having a refractive index of 1.5 or more and 1.7 or less contained in a toner layer B formed on the toner layer A, and C is the content of the particles having a refractive index of 1.5 or more and 1.7 or less contained in a toner layer C formed on the toner layer B, A, B, and C satisfy the relationships of A>B and A>C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an image forming method used in an electrophotographic system, an electrostatic recording system, an electrostatic printing system, or a toner jet system. [Background technology]

[0002] In recent years, full-color electrophotographic copying machines have come into widespread use, and there is a demand for high speed, high image quality, high productivity, and low cost. To achieve such cost reduction, a technique is known in which an inexpensive filler is used to reduce the amount of toner raw materials used (Patent Document 1). However, the use of such a filler can result in a decrease in the color reproducibility of an image due to light scattering at the interface between the filler and the toner raw materials, particularly when forming a secondary color by overlapping toners.

[0003] On the other hand, in bookbinding or package printing, when a medium to which toner does not easily adhere, such as coated paper, is used, the printed toner may peel off due to strong external stress such as contact with a human fingernail or a sharp object, resulting in a phenomenon known as scratch wear. Reducing the amount of filler reduces the cost advantage and can also reduce the scratch resistance of the image as described above. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-145886 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to solve the above problems and to provide an image forming method which does not reduce the color gamut even when a filler is used and has high scratch resistance. [Means for solving the problem]

[0006] According to one aspect of the present invention, a charging step of charging an electrostatic latent image carrier by a charging means; an exposure step of exposing the charged electrostatic latent image carrier to light to form an electrostatic latent image; a developing step of developing the electrostatic latent image with a developer containing toner and a magnetic carrier to form a toner image; a transfer step of transferring the toner image onto a transfer material with or without an intermediate transfer member; and 1. An image forming method having a fixing step of fixing a transferred toner image onto a transfer material, The developing step comprises: developing the first electrostatic latent image with a first developer to form a first toner image; developing the second electrostatic latent image with a second developer to form a second toner image; developing the third electrostatic latent image with a third developer to form a third toner image; It has the first developer, the second developer and the third developer all have toner particles containing particles having a refractive index of 1.5 or more and 1.7 or less; the transferred toner image formed on the transfer material has at least an area where the first toner image, the second toner image and the third toner image are laminated; In this region, The content of particles having a refractive index of 1.5 or more and 1.7 or less contained in the toner layer A closest to the surface of the transfer material is defined as A (mass%), The content of particles having a refractive index of 1.5 or more and 1.7 or less contained in toner layer B formed on toner layer A is defined as B (mass%), When the content of particles having a refractive index of 1.5 or more and 1.7 or less contained in a toner layer C formed on a toner layer B is C (mass %), A, B and C are A>B A>C Fulfilling the relationship death, The particles having a refractive index of 1.5 or more and 1.7 or less are calcium carbonate particles. A method of forming an image is provided. According to the present invention, by suppressing light scattering caused by the filler, a method for forming an image having high scratch resistance and without impairing color reproducibility can be obtained even when a filler is used. Effect of the Invention

[0007] According to one aspect of the present invention, it is possible to provide an image forming method that does not impair color reproducibility and has high scratch resistance even when a filler is used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following describes in detail exemplary embodiments of the present invention, but the scope of the present invention is not limited to the following embodiments. In this specification, the descriptions "xx or more and xx or less" and "xx to xx" expressing a numerical range are as follows: Unless otherwise specified, numerical ranges are intended to include the endpoints, lower and upper limits.

[0009] First, the image forming method according to the present invention has the following steps. a charging step of charging the electrostatic latent image carrier by a charging means; an exposure step of exposing the charged electrostatic latent image carrier to light to form an electrostatic latent image; a developing step of developing the electrostatic latent image with a developer containing toner and a magnetic carrier to form a toner image; A transfer step in which the toner image is transferred to a transfer material with or without an intermediate transfer member, where the transfer material refers to a recording medium. Furthermore, the steps from the charging step to the transfer step are carried out for each color, and a fixing step is provided in which the transferred toner image is fixed onto a transfer material.

[0010] The developing step comprises: developing the first electrostatic latent image with a first developer to form a first toner image; developing the second electrostatic latent image with a second developer to form a second toner image; Developing the third electrostatic latent image with a third developer to form a third toner image. The image forming units are arranged in series within the main body of the image forming apparatus, and processing is carried out in parallel, with each toner image being transferred directly to the transfer material, with the first toner image being transferred to the transfer material, then the second toner image being transferred to the transfer material, and then the third toner image being transferred to the transfer material. When transferring to a transfer material, which is a recording medium, via an intermediate transfer body, the arrangement order of the image forming units is reversed compared to when no intermediate transfer body is used.

[0011] The present invention is characterized by: the first developer, the second developer and the third developer all have toner particles containing particles having a refractive index of 1.5 or more and 1.7 or less; the transferred toner image formed on the transfer material has at least an area where the first toner image, the second toner image and the third toner image are laminated; In the region, the content of particles having a refractive index of 1.5 or more and 1.7 or less contained in the toner layer A closest to the surface of the transfer material is defined as A (mass %), The content of particles having a refractive index of 1.5 or more and 1.7 or less contained in toner layer B formed on toner layer A is defined as B (mass%), When the content of particles having a refractive index of 1.5 or more and 1.7 or less contained in a toner layer C formed on a toner layer B is C (mass %), A, B and C are A>B A>C The aim is to satisfy the relationship. The content of the particles having a refractive index of 1.5 or more and 1.7 or less contained in each toner layer is the same as the content of the particles contained in the toner constituting the toner layer.

[0012] By using such a form, even when a filler is used, it is possible to obtain an image with high scratch resistance without compromising the color gamut. The reason why it is possible to obtain an image with high scratch resistance without impairing the color gamut is believed to be as follows. By not including a large amount of particles with a refractive index of 1.5 or more and 1.7 or less in the upper layer of the fixed toner layer, scattering of incident light onto the toner layer is suppressed, and the color gamut is not impaired. On the other hand, by including a large amount of particles having a refractive index of 1.5 or more and 1.7 or less in the lower layer of the fixed toner layer, the particles have an effect of reinforcing the image.

[0013] In the image forming method of the present invention, the order of image formation on the transfer material of the cyan toner, yellow toner, and magenta toner is preferably cyan toner, yellow toner, and magenta toner, from the viewpoint of obtaining excellent color development. In other words, it is preferable that the cyan toner is directly laminated on the recording medium, then the yellow toner is laminated, and then the magenta toner is laminated.

[0014] The particles used in the present invention have a refractive index of 1.5 or more and 1.7 or less. These particles are achromatic and have a refractive index of 1.5 or more and 1.7 or less. Examples of such particles include calcium carbonate (CaCO3) particles, kaolin (a mineral whose main component is Al2Si2O5(OH)4) particles, talc (Mg3Si4O 10 Examples of suitable particles include (OH)2-based mineral particles and barium sulfate (BaSO4) particles. From the viewpoint of not impairing the color gamut, calcium carbonate particles are preferred. By using calcium carbonate particles, higher color reproducibility can be achieved.

[0015] The pigment used in the present invention is The cyan toner contains at least one cyan pigment selected from the group consisting of CI Pigment Blue 15:3 and CI Pigment Blue 15:4, the yellow toner contains at least one yellow pigment selected from the group consisting of CI Pigment Yellow 74, CI Pigment Yellow 180, and CI Pigment Yellow 185; It is preferable that the magenta toner contains at least one magenta pigment selected from the group consisting of CI Pigment Red 122, CI Pigment Red 150, and CI Pigment Red 238 in order to achieve a wide color gamut.

[0016] The content of particles with a refractive index of 1.5 to 1.7 is 5.0 mass%≦A≦15.0 mass% 0.5 mass%≦B≦5.0 mass%, 0.5 mass%≦C≦5.0 mass%, By setting the content within this range, it is possible to achieve both high levels of color gamut and scratch resistance.

[0017] moreover, AB≧3% by mass, AC≧3% by mass By setting the content within this range, it is possible to achieve a high level of both color gamut and scratch resistance.

[0018] Furthermore, the number-average particle size of the calcium carbonate particles is preferably 200 nm or more and 800 nm or less, because higher color reproducibility can be achieved by controlling the particle size within this range. Furthermore, when the calcium carbonate particles are subjected to X-ray diffraction measurement using CuKα radiation, the toner has peaks in the Bragg angle (2θ) ranges of 26.5±0.5 and 29.5±0.5, The crystallite size of the crystals at a Bragg angle (2θ) of 29.5±0.5 is 100 Å or more and 450 Å or less, It is preferable that the ratio (peak intensity ratio) of the crystalline peak intensity (first peak intensity) assigned to a Bragg angle (2θ) of 26.5±0.5 to the crystalline peak intensity (second peak intensity) assigned to a Bragg angle (2θ) of 29.5±0.5 is 0.15 or more and 0.24 or less. The peak intensity ratio is calculated by the following formula. Peak intensity ratio=(first peak intensity) / (second peak intensity) By using such calcium carbonate, higher color reproducibility can be achieved. Preferred configurations of the present invention will now be described in detail. First, the raw materials of the toner used in the present invention will be described.

[0019] <Pigments> Examples of the pigment include known organic pigments. Examples of cyan pigments include copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds.

[0020] Examples of magenta pigments include condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds.

[0021] Examples of yellow pigments include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. The pigments may be used alone or in combination of two or more.

[0022] The pigment of the present invention is The cyan toner contains at least one cyan pigment selected from the group consisting of CI Pigment Blue 15:3 and CI Pigment Blue 15:4, the yellow toner contains at least one yellow pigment selected from the group consisting of CI Pigment Yellow 74, CI Pigment Yellow 180, and CI Pigment Yellow 185; The magenta toner contains at least one magenta pigment selected from the group consisting of CI Pigment Red 122, CI Pigment Red 150, and CI Pigment Red 238. is preferable in order to achieve a wide color gamut.

[0023] <Binding resin> A general resin can be used as the binder resin used in the toner used in electrophotography. Specifically, polyester resin, styrene-acrylic acid copolymer, polyolefin resin, vinyl resin, fluororesin, phenol resin, silicone resin, epoxy resin, etc. can be exemplified. These resins have a refractive index of 1.5 to 1.7. Among them, from the viewpoint of improving low-temperature fixability, amorphous polyester resin is used, and from the viewpoint of achieving both excellent low-temperature fixability and hot offset resistance, it is known to use low-molecular-weight polyester and high-molecular-weight polyester in combination. In addition, from the viewpoint of achieving both further improvement in low-temperature fixability and blocking resistance during storage, crystalline polyester may be used as a plasticizer.

[0024] <Release agent> If necessary, a release agent for suppressing the occurrence of hot offset during the heat fixing of the toner may be used. Typical examples of the release agent include low molecular weight polyolefins, silicone wax, fatty acid amides, ester waxes, carnauba wax, and hydrocarbon waxes.

[0025] <External additives> The external additive is preferably an inorganic fine powder such as silica, titanium oxide, or aluminum oxide. The inorganic fine powder is preferably hydrophobized with a hydrophobizing agent such as a silane compound, silicone oil, or a mixture thereof. As an external additive to improve fluidity, 2 / g or more 400m 2 / g or less is preferable, and for durability stabilization, a specific surface area of ​​10 m 2 / g or more 50m 2 In order to achieve both improved fluidity and stabilized durability, inorganic fine powders having a specific surface area within the above range may be used in combination. The external additive is preferably used in an amount of 0.1 parts by mass to 10.0 parts by mass based on 100 parts by mass of toner particles. A known mixer such as a Henschel mixer can be used to mix the toner particles and the external additive.

[0026] <Toner manufacturing method> The toner may be produced by any one of the following methods alone or in combination: kneading and pulverizing, dissolution suspension, suspension polymerization, and emulsion aggregation. Specific examples of the toner production method using the kneading and pulverizing method will be described below, but the method is not limited to these.

[0027] <Kneading and grinding method> In the kneading and pulverizing method, first, the pigment dispersion and amorphous resin, which are the constituent materials of the toner, as well as the release agent, colorant, and other additives added as necessary, are thoroughly mixed and melt-kneaded using a known heat kneader such as a heated roll or kneader (kneading step).Then, the mixture is mechanically pulverized to a desired toner particle size (pulverizing step), and classified to a desired particle size distribution (classification step) to produce a toner.

[0028] (Kneading process) The melt-kneading of the toner constituent materials can be carried out using a known heat kneading machine such as a heating roll, a kneader, etc. In the kneading step, it is preferable that the toner constituent materials are sufficiently mixed in advance using a mixer. Examples of mixers include the following: Henschel Mixer (manufactured by Mitsui Mining Co., Ltd.), Super Mixer (manufactured by Kawata Co., Ltd.), Ribocone (manufactured by Okawara Manufacturing Co., Ltd.), Nauta Mixer, Turbulizer, Cyclomix (manufactured by Hosokawa Micron Corporation), Spiral Pin Mixer (manufactured by Pacific Machinery Co., Ltd.), and Loedige Mixer (manufactured by Matsubo Co., Ltd.).

[0029] Examples of thermal kneaders include the following: KRC kneader (Kurimoto Iron Works); Buss-Co kneader (Buss); TEM type extruder (Toshiba Machine); TEX twin-screw kneader (Japan Steel Works); PCM kneader (Ikegai Iron Works); three-roll mill, mixing roll mill, kneader (Inoue Seisakusho); Kneadex (Mitsui Mining); MS-type pressure kneader, Niderruder (Moriyama Seisakusho); Banbury mixer (Kobe Steel, Ltd.).

[0030] (Crushing process) The pulverization step is a step in which the kneaded product obtained in the kneading step is cooled until it reaches a pulverizable hardness, and then mechanically pulverized to a toner particle size by a known pulverizer such as a collision plate jet mill, a fluidized bed jet mill, or a rotary mechanical mill. From the viewpoint of pulverization efficiency, it is desirable to use a fluidized bed jet mill as the pulverizer.

[0031] Examples of pulverizers include the following: Counter Jet Mill, Micron Jet, Innomizer (manufactured by Hosokawa Micron Corporation), IDS type mill, PJM jet pulverizer (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), Cross Jet Mill (manufactured by Kurimoto Iron Works Co., Ltd.), Urmax (manufactured by Nisso Engineering Co., Ltd.), SK Jet-O-Mill (manufactured by Seishin Enterprise Co., Ltd.), Cryptron (manufactured by Kawasaki Heavy Industries, Ltd.), Turbo Mill (manufactured by Turbo Kogyo Co., Ltd.), Super Rotor (manufactured by Nisshin Engineering Co., Ltd.), etc.

[0032] (Classification process) The classification step is a step in which the finely pulverized product obtained in the pulverization step is classified to obtain a toner having a desired particle size distribution. As a classifier used for classification, known devices such as a wind classifier, an inertial classifier, and a sieve classifier can be used. Specific examples include the following: Classeal, Micron Classifier, and Spedic Classifier (manufactured by Seishin Enterprise Co., Ltd.); Turbo Classifier (manufactured by Nisshin Engineering Co., Ltd.); Micron Separator, Turbo Flex (ATP), and TSP Separator (manufactured by Hosokawa Micron Corporation); Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), Dispersion Separator (manufactured by Nippon Pneumatic Mfg. Co., Ltd.); and YM Microcut (manufactured by Yaskawa Shoji Co., Ltd.).

[0033] To the toner produced through the above steps, inorganic fine particles such as silica, alumina, titania, calcium carbonate, etc., and resin fine particles such as vinyl resin, polyester resin, silicone resin, etc., may be added by applying a shear force in a dry state, as necessary. These inorganic fine particles and resin fine particles function as external additives such as a flowability aid and a cleaning aid. The toner and methods for measuring various physical properties will be described below.

[0034] [Content of particles with refractive index of 1.5 to 1.7 in toner particles] Add 1.70 g of sucrose (Kishida Chemical) to 100 mL of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. Add 31 g of the concentrated sucrose solution and 6 mL of Contaminon N (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments, pH 7, consisting of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) to a centrifuge tube to prepare a dispersion. Add 1.0 g of toner to this dispersion, and break up the toner clumps with a spatula or the like. Next, shake the centrifuge tube with a shaker. After shaking, transfer the solution to a glass tube (50 mL) for a swing rotor and separate it in a centrifuge at 3500 rpm for 30 minutes. This operation separates the toner particles from the removed external additives. It is visually confirmed that the toner particles and the external additives are sufficiently separated, and the toner particles are collected and filtered using a vacuum filter, and then dried in a dryer for at least 1 hour to obtain toner particles from which the external additives have been separated.

[0035] Next, materials such as binder resin are separated from the toner particles by utilizing the difference in solubility in a solvent, and then the mass of each is measured to measure the content of particles with a refractive index of 1.5 to 1.7. Specific methods for separation include, for example, the following methods. The toner particles are dissolved in tetrahydrofuran (THF) at a temperature of 23°C, and the soluble portion (binder resin) and the insoluble portion (particles with a refractive index of 1.5 to 1.7, release agent, pigment, etc.) are separated, and the soluble portion is dried. The insoluble portion separated above is dissolved in hexane at a temperature of 23°C, and the soluble portion (release agent, etc.) and the insoluble portion (particles with a refractive index of 1.5 to 1.7 and pigment) are separated, and the soluble portion is dried. Finally, the insoluble portion in the hexane is dispersed in tetrahydrofuran, placed in a centrifuge tube with an inner diameter of 10 mm, and centrifuged at 3000 rpm for 1 minute using a centrifuge, and the supernatant is collected and dried to obtain the pigment. The sediment is then separated to obtain particles with a refractive index of 1.5 to 1.7. The mass of each of the above components is measured to obtain the content of binder resin particles having a refractive index of 1.5 to 1.7 in the toner particles.

[0036] [Refractive index of particles with refractive index of 1.5 to 1.7 in toner particles] Using the particles with a refractive index of 1.5 to 1.7 isolated by the above-mentioned method, measure the refractive index using an Abbe refractometer (e.g., DR-M2 (manufactured by Ohara Corporation)) or a spectroscopic ellipsometer (e.g., VASE, manufactured by J.A. Woollam Japan, etc.).

[0037] [Pigment structure in toner particles] The pigment isolated by the above method is subjected to 1H-NMR and 13C-NMR spectrum measurement using ECA-400 (400 MHz) manufactured by JEOL Ltd., to identify its structure.

[0038] [Number average particle size of particles with refractive index of 1.5 to 1.7] The number-average particle size of particles having a refractive index of 1.5 to 1.7 is calculated by observing the cross section of a toner particle with a scanning electron microscope (S-4800, Hitachi High-Technologies Corporation), measuring the major axis of 100 particles, and calculating the average value (arithmetic mean value).

[0039] [X-ray diffraction measurement of calcium carbonate in toner particles] The X-ray diffraction measurement of calcium carbonate in the toner particles is performed using a measuring device "RINT-TTRII" (manufactured by Rigaku Corporation) with CuKα characteristic X-rays at a Bragg angle (2θ±0.20 deg) in the range of 3 deg to 35 deg. From the total integrated intensity of the obtained spectrum, The crystallite size of the crystals assigned to the Bragg angle (2θ) of 29.5±0.5, The ratio of the peak intensity of the crystals attributable to a Bragg angle (2θ) of 26.5±0.5 to the peak intensity of the crystals attributable to a Bragg angle (2θ) of 29.5±0.5 is calculated. The measurement conditions are as follows.

[0040] X-ray:Cu / 50kV / 300mA Goniometer: Rotor horizontal goniometer (TTR-2) Attachment: Standard sample holder Divergence slit: open Divergence vertical limit slit: 10.00mm Scattering slit: open Receiving slit: open Counter: Scintillation counter Scanning mode: Continuous Scan speed: 4.0000° / min. Sampling width: 0.0200° Scan axis: 2θ / θ Scanning range: 10.0000~40.0000° EXAMPLES

[0041] The present invention will be described in more detail below with reference to examples and comparative examples, but these are not intended to limit the present invention in any way. In the following formulations, parts are by weight unless otherwise specified.

[0042] <Production of cyan pigment masterbatch C1> Cyan pigment (PB15:3) 30 parts by weight Light calcium carbonate (number average particle size 400 nm) 50 parts by mass Amorphous polyester A 20 parts by weight (Amorphous polyester A: composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening temperature (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 ) 0.5 )

[0043] The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for a rotation time of 5 minutes, the mixture was kneaded in a twin-screw kneader (PCM-30 type, manufactured by Ikegai Corporation) at a temperature of 120° C. The kneaded product obtained was cooled and coarsely pulverized in a pin mill to a particle size of 100 μm or less to obtain a coarsely pulverized product of cyan pigment master batch C1.

[0044] <Manufacture of cyan pigment masterbatches C2 to C6> Except for changing the materials shown in Table 1, the same production method as for the cyan pigment master batch C1 was used to obtain cyan pigment master batches C2 to C6.

[0045] [Table 1] In Table 1, PB15:3 indicates CI Pigment Blue 15:3, and PB15:4 indicates CI Pigment Blue 15:4.

[0046] <Manufacture of cyan toner CT1> Amorphous polyester A 75.25 parts by weight (Composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening temperature (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 )0.5) Cyan pigment masterbatch C1 16.75 parts by weight Synthetic wax 1 8.00 parts by weight (Hydrocarbon wax, maximum endothermic peak temperature 90℃)

[0047] The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for 5 minutes at 100°C, the mixture was kneaded at 130°C in a twin-screw kneader (PCM-30, Ikegai Corporation). The kneaded mixture was cooled and coarsely pulverized to a particle size of 100 μm or less in a pin mill to obtain a coarsely pulverized product. The coarsely pulverized product was finely pulverized in a mechanical pulverizer (T-250, Turbo Kogyo Co., Ltd.) by adjusting the rotation speed and number of passes to obtain the target particle size. The mixture was further classified using a rotary classifier (200TSP, Hosokawa Micron Corporation) to obtain toner particles.

[0048] The operating conditions of the rotary classifier (200TSP, manufactured by Hosokawa Micron Corporation) were such that the rotation speed was adjusted so as to obtain the target particle size and particle size distribution, and classification was performed. 1.8 parts by mass of the following silica fine particles were added to 100 parts by mass of the obtained toner particles, and the mixture was mixed in a Henschel mixer (FM-75 type, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 10 minutes rotation time to obtain a cyan toner CT1. Silica fine particles: Specific surface area measured by the BET method is 200 m 2 / g, and silica particles that have been hydrophobized with silicone oil

[0049] <Manufacturing example of cyan toner CT2 to CT14> Except for changing the materials shown in Table 2, the same production method as for cyan toner CT1 was used to obtain cyan toners CT2 to CT14.

[0050] [Table 2]

[0051] <Manufacture of magenta pigment masterbatch M1> Magenta pigment (PR122) 30 parts by weight Magenta pigment (PR150) 10 parts by weight Light calcium carbonate (number average particle size 400 nm) 15 parts by mass Amorphous polyester A 45 parts by weight (Amorphous polyester A: composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening temperature (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 )0.5)

[0052] The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for a rotation time of 5 minutes, the mixture was kneaded in a twin-screw kneader (PCM-30 type, manufactured by Ikegai Corporation) at a temperature of 120° C. The kneaded product was cooled and coarsely pulverized in a pin mill to a particle size of 100 μm or less to obtain a coarsely pulverized product of magenta pigment master batch M1.

[0053] <Manufacture of magenta pigment masterbatches M2 to M6> Except for changing the materials shown in Table 3, the magenta pigment master batches M2 to M6 were produced in the same manner as the magenta pigment master batch M1.

[0054] [Table 3] In Table 3, PR122 indicates CI Pigment Red 122, and PR238 indicates CI Pigment Red 238.

[0055] <Manufacture of Magenta Toner MT1> Amorphous polyester A 92.5 parts by weight (Composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening temperature (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 )0.5) Magenta pigment master batch M1 12.5 parts by weight Synthetic wax 1 8.0 parts by weight (Hydrocarbon wax, maximum endothermic peak temperature 90℃)

[0056] The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for 5 minutes at 100°C, the mixture was kneaded at 130°C in a twin-screw kneader (PCM-30, Ikegai Corporation). The kneaded mixture was cooled and coarsely pulverized in a pin mill to a volume average particle size of 100 μm or less to obtain a coarsely pulverized product. The coarsely pulverized product was finely pulverized in a mechanical pulverizer (T-250, Turbo Kogyo Co., Ltd.) by adjusting the rotation speed and number of passes to obtain the target particle size. The mixture was further classified using a rotary classifier (200TSP, Hosokawa Micron Corporation) to obtain toner particles.

[0057] The operating conditions of the rotary classifier (200TSP, manufactured by Hosokawa Micron Corporation) were such that the rotation speed was adjusted so as to obtain the target particle size and particle size distribution, and classification was performed. 1.8 parts by mass of the following silica fine particles were added to 100 parts by mass of the obtained toner particles, and the mixture was mixed in a Henschel mixer (FM-75 type, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 10 minutes rotation time to obtain a magenta toner MT1. Silica microparticles: Silica microparticles with a specific surface area of ​​200 m2 / g measured by the BET method and hydrophobized with silicone oil

[0058] <Production example of magenta toner MT2 to MT14> Except for changing the materials shown in Table 4, the magenta toners MT2 to MT14 were produced in the same manner as the magenta toner MT1.

[0059] [Table 4]

[0060] <Production of Yellow Pigment Masterbatch Y1> Yellow pigment (PY180) 30 parts by weight Light calcium carbonate (number average particle size 400 nm) 55 parts by mass Amorphous polyester A 15 parts by weight (Amorphous polyester A: composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening temperature (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 ) 0.5 )

[0061] The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for a rotation time of 5 minutes, the mixture was kneaded in a twin-screw kneader (PCM-30 type, manufactured by Ikegai Corporation) at a temperature of 120° C. The kneaded product obtained was cooled and coarsely pulverized in a pin mill to a volume average particle size of 100 μm or less to obtain a coarsely pulverized product of yellow pigment masterbatch Y1.

[0062] <Production of Yellow Pigment Masterbatches Y2 to Y8> Except for changing the materials shown in Table 5, the same production method as for the yellow pigment master batch Y1 was used to obtain yellow pigment master batches Y2 to Y8.

[0063] [Table 5] In Table 5, PY74 indicates CI Pigment Yellow 74, PY180 indicates CI Pigment Yellow 180, and PY185 indicates CI Pigment Yellow 185.

[0064] <Production of Yellow Toner YT1> Amorphous polyester A 72.0 parts by weight (Composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening temperature (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 )0.5) Yellow pigment masterbatch Y1 20.0 parts by mass Synthetic wax 1 8.0 parts by weight (Hydrocarbon wax, maximum endothermic peak temperature 90℃)

[0065] The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for 5 minutes at 100°C, the mixture was kneaded at 130°C in a twin-screw kneader (PCM-30, Ikegai Corporation). The kneaded mixture was cooled and coarsely pulverized in a pin mill to a volume average particle size of 100 μm or less to obtain a coarsely pulverized product. The coarsely pulverized product was finely pulverized in a mechanical pulverizer (T-250, Turbo Kogyo Co., Ltd.) by adjusting the rotation speed and number of passes to obtain the target particle size. The mixture was further classified using a rotary classifier (200TSP, Hosokawa Micron Corporation) to obtain toner particles.

[0066] The operating conditions of the rotary classifier (200TSP, manufactured by Hosokawa Micron Corporation) were such that the rotation speed was adjusted so as to obtain the target particle size and particle size distribution, and classification was performed. 1.8 parts by mass of the following silica fine particles were added to 100 parts by mass of the obtained toner particles, and the mixture was mixed in a Henschel mixer (FM-75 type, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 10 minutes rotation time to obtain a yellow toner YT1. Silica fine particles: Specific surface area measured by the BET method is 200 m 2 / g, and silica particles that have been hydrophobized with silicone oil

[0067] <Production examples of yellow toner YT2 to YT16> Except for changing the materials shown in Table 6, the same production method as for yellow toner YT1 was used to obtain yellow toners YT2 to YT16.

[0068] [Table 6]

[0069] <Magnetic Carrier 1 Manufacturing Example> Number average particle size: 0.30μm, magnetization strength under a magnetic field of (1000 / 4π(kA / m): 65Am 2 / kg) of magnetite 1 Number average particle size: 0.50μm, magnetization strength under a magnetic field of (1000 / 4π(kA / m): 65Am 2 / kg) of magnetite 2 To 100 parts of each of the above materials, 4.0 parts of a silane compound (3-(2-aminoethylaminopropyl)trimethoxysilane) was added, and the mixture was mixed and stirred at high speed in a container at 100° C. or higher to treat each of the fine particles. Phenol: 10% by weight Formaldehyde solution: 6% by mass (40% by mass of formaldehyde, 10% by mass of methanol, 50% by mass of water) Magnetite treated with the above silane compound 1:58 mass% Magnetite treated with the above silane compound 2: 26% by mass

[0070] 100 parts of the above material, 5 parts of a 28% by mass aqueous ammonia solution, and 20 parts of water were placed in a flask, and the mixture was heated to 85°C over 30 minutes and held at that temperature while stirring and mixing. A polymerization reaction was carried out for 3 hours, and the resulting phenolic resin was cured. Thereafter, the hardened phenolic resin was cooled to 30° C., and water was further added thereto. The supernatant liquid was then removed, and the precipitate was washed with water and then air-dried. This was then dried under reduced pressure (5 mmHg or less) at a temperature of 60° C. to obtain magnetic material-dispersed spherical magnetic carrier 1. The volume-based 50% particle diameter (D50) of magnetic carrier 1 was 34.2 μm.

[0071] <Production example of cyan two-component developer CD1> 8.0 parts of cyan toner CT1 was added to 92.0 parts of magnetic carrier 1, and mixed in a V-type mixer (V-20, manufactured by Seishin Enterprise Co., Ltd.) to obtain a cyan two-component developer CD1.

[0072] <Manufacturing examples of cyan two-component developers CD2 to CD14> Cyan two-component developers CD2 to CD14 were obtained by carrying out production in the same manner as in the production example of the cyan two-component developer CD1, except that the toner was changed as shown in Table 7.

[0073] <Production example of magenta two-component developer MD1> 8.0 parts of magenta toner MT1 was added to 92.0 parts of magnetic carrier 1, and mixed in a V-type mixer (V-20, manufactured by Seishin Enterprises) to obtain magenta two-component developer MD1.

[0074] <Production examples of magenta two-component developers MD2 to MD14> In the production example of magenta two-component developer MD1, production was carried out in the same manner except that the toner was changed as shown in Table 7, to obtain magenta two-component developers MD2 to MD14.

[0075] <Production example of yellow two-component developer YD1> To 92.0 parts of the magnetic carrier 1, 8.0 parts of the yellow toner YT1 were added, and mixed in a V-type mixer (V-20, manufactured by Seishin Enterprise Co., Ltd.) to obtain a yellow two-component developer YD1.

[0076] <Production examples of yellow two-component developers YD2 to YD16> Yellow two-component developers YD2 to YD16 were obtained by carrying out production in the same manner as in the production example of yellow two-component developer YD1, except that the toner was changed as shown in Table 7.

[0077] [Table 7] The method for evaluating images obtained using the above toner is described below.

[0078] <Color gamut evaluation> The evaluation was performed using a Canon full-color copier imageRUNNER ADVANCE C5255 as the image forming apparatus. In this apparatus, a cyan toner layer made of cyan toner, a yellow toner layer made of yellow toner, and a magenta toner layer made of magenta toner are layered on the transfer material, which is a non-recording medium, in this order from the side closest to the surface of the transfer material.

[0079] The evaluation environment was normal temperature and humidity (temperature 23°C, relative humidity 50%), and the evaluation paper was GFC-081 plain copy paper (A4, basis weight 81.4 g / m 2 A 1cm x 1cm patch image was printed using a printer (sold by Canon Marketing Japan Inc.), and the toner amount of each patch was set to 0.35 g / m by the controller. 2 Then, the fixed image of the patch image was output.

[0080] The image evaluation was performed using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite) to measure the L of the primary and secondary colors of each image sample. * a * b * Chromaticity in the color system (L * , a * , b * ) was measured. The measurement results were used to simulate the color gamut volume, and the percentage change in the color gamut volume relative to the reference was evaluated. In addition, Examples 1, 4 to 12 and Comparative Examples 1 and 2 were based on Comparative Example 3, Example 2 was based on Comparative Example 4, and Example 3 was based on Comparative Example 5. The evaluation results are shown in Table 8.

[0081] (Color Gamut Evaluation Criteria) A: 105% or more B: 100% or more but less than 105% C: 95% or more but less than 100% D: Less than 95%

[0082] <Scratch resistance> ·Paper: Océ Top Coated Pro Silk 270(270.0g / m 2 ) (Sold by Oce Corporation) Evaluation image: A 2cm x 15cm secondary color image is placed in the center of the A4 paper. - Toner loading on paper for each toner: 0.35mg / cm 2 (Adjusted by DC voltage VDC of developer carrier, charging voltage VD of electrostatic latent image carrier, and laser power) Test environment: Normal temperature and humidity (temperature 23°C, relative humidity 50% (hereinafter N / N)) Fixing temperature: 160℃ Process speed: 400mm / s

[0083] The recording paper on which the above evaluation image was printed was evaluated using a surface property tester HEIDON TYPE14FW manufactured by Shinto Scientific Co., Ltd., by placing a 200g weight on it and scratching the image with a needle having a diameter of 0.75mm at a speed of 60mm / min and a length of 30mm. The ratio of the area where the toner peeled off was determined by binarizing the area where the toner peeled off occurred relative to the scratched area through image processing. The measurement results are shown in Table 8.

[0084] (Evaluation Criteria) A: The area ratio of toner peeled off due to image scratches is 0% or more but less than 1.0% B: The area ratio of toner peeled off due to image scratches is 1.0% or more and less than 4.0% C: The area ratio of toner peeled off due to image scratches is 4.0% or more and less than 7.0% D: The area ratio of toner peeled off due to image scratches is 7.0% or more.

[0085] [Table 8] Incidentally, Example 12 was evaluated as a reference example.

Claims

1. a charging step of charging the electrostatic latent image carrier by a charging means; an exposure step of exposing the charged electrostatic latent image carrier to light to form an electrostatic latent image; a developing step of developing the electrostatic latent image with a developer containing toner and a magnetic carrier to form a toner image; a transfer step of transferring the toner image onto a transfer material with or without an intermediate transfer member; and 1. An image forming method having a fixing step of fixing a transferred toner image onto a transfer material, The developing step comprises: developing the first electrostatic latent image with a first developer to form a first toner image; developing the second electrostatic latent image with a second developer to form a second toner image; developing the third electrostatic latent image with a third developer to form a third toner image; It has the first developer, the second developer and the third developer all have toner particles containing particles having a refractive index of 1.5 or more and 1.7 or less; the transferred toner image formed on the transfer material has at least an area where the first toner image, the second toner image and the third toner image are laminated; In this region, The content of particles having a refractive index of 1.5 or more and 1.7 or less contained in the toner layer A closest to the surface of the transfer material is defined as A (mass %), The content of particles having a refractive index of 1.5 or more and 1.7 or less contained in the toner layer B formed on the toner layer A is defined as B (mass %), When the content of particles contained in the toner layer C formed on the toner layer B is 1.5 to 1.7% by mass, C (mass %) is the content of particles A, B, and C. A>B A>C Fulfilling the relationship, The image forming method is characterized in that the particles having a refractive index of 1.5 or more and 1.7 or less are calcium carbonate particles.

2. the toner constituting the toner layer A is a cyan toner, the toner constituting the toner layer B is a yellow toner, 2. The image forming method according to claim 1, wherein the toner constituting the toner layer C is a magenta toner.

3. The cyan toner contains at least one cyan pigment selected from the group consisting of C.I. Pigment Blue 15:3 and C.I. Pigment Blue 15:4, The yellow toner contains at least one yellow pigment selected from the group consisting of C.I. Pigment Yellow 74, C.I. Pigment Yellow 180, and C.I. Pigment Yellow 185; 3. The image forming method according to claim 2, wherein the magenta toner contains at least one magenta pigment selected from the group consisting of C. I. Pigment Red 122, C. I. Pigment Red 150, and C. I. Pigment Red 238.

4. The A (mass%), the B (mass%), and the C (mass%) are 5.0≦A≦15.0 0.5≦B≦5.0, 0.5≦C≦5.0, The image forming method according to any one of claims 1 to 3, wherein

5. The A (mass%), the B (mass%), and the C (mass%) are A-B≧3 (mass%) A-C≧3 (mass%) The image forming method according to any one of claims 1 to 4, wherein

6. 6. The image forming method according to claim 1, wherein the calcium carbonate particles have a number average particle size of 200 nm or more and 800 nm or less.

7. The calcium carbonate particles are When the toner was subjected to X-ray diffraction measurement using CuKα radiation, it had peaks in the Bragg angle (2θ) range of 26.5±0.5 and 29.5±0.5, The crystallite size of the crystals assigned to a Bragg angle (2θ) of 29.5±0.5 is 100 Å or more and 450 Å or less; The image forming method according to any one of claims 1 to 6, wherein the ratio of the peak intensity of the crystals attributable to a Bragg angle (2θ) of 26.5±0.5 to the peak intensity of the crystals attributable to a Bragg angle (2θ) of 29.5±0.5 is 0.15 or more and 0.24 or less.

Citation Information

Patent Citations

  • Image forming apparatus

    JP2004205890A

  • Resin particle for toner and its manufacturing method

    JP2005049858A

  • Full-color image forming method

    JP2009151276A

  • Toner for electrostatic charge image development, developer for electrostatic charge image development, and image forming apparatus

    JP2014145886A

  • Image forming method and toner set for electrostatic latent image development