Method and apparatus for producing spinning dope composition
The intensive mixing and controlled dissolution of cellulosic pulp in alkaline solution at low temperatures address the challenges of enzyme consumption and gelation, enabling stable and efficient production of a spinning dope composition with high cellulose concentration and low filter clogging.
Patent Information
- Application Number
- JP2022155666
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-04-14
- Filing Date
- 2022-09-29
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2037-04-12
AI Technical Summary
Existing methods for producing cellulose stock solutions for rayon fibers and cellophane films face issues such as high enzyme consumption, lengthy and energy-intensive processes, poor mechanical properties, and instability against gelation, with insufficient guidance on equipment design and filter clogging.
A method involving intensive mixing of cellulosic pulp in alkaline solution at low temperatures, followed by controlled dissolution, ensuring rapid dispersion and stable production of a spinning dope composition with high cellulose concentration and low filter clogging, using high-shear mixing and controlled temperature conditions.
The method achieves a spinning dope composition with high cellulose concentration, low filter clogging, and resistance to gelation, facilitating efficient industrial-scale production with improved mechanical properties and stability.
Smart Images

Figure 0007596338000001 
Figure 0007596338000002 
Figure 0007596338000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a spinning dope composition and an apparatus directed to the production of said spinning dope composition. [Background technology]
[0002] Most dissolving pulps produced and used industrially today to produce viscose rayon fiber and cellophane film are not sufficiently alkaline soluble as is. This problem of alkaline solubility is real even though the xanthation process (viscose process) using carbon disulfide and sodium hydroxide promotes dissolution in alkali. In the viscose process, the cellulose is adapted by a steeping process that involves alkali cellulose swelling and thermo-oxidative hydrolysis, resulting in a reduction in DP and improved accessibility of the chemicals prior to contact of the pulp with carbon disulfide. Similarly, dissolving pulps need to be adapted before they can be fully dissolved directly in alkali. Several methods have been proposed in the literature for such adaptation. These include enzymatic treatment of cellulose (EP 2116557A1), acid hydrolysis and / or steam explosion (STEX) alone (US 5401447, US 4634470) or in combination with wet grinding in alkali (US 7108907B1), hydrothermal hydrolysis in an autoclave (US 6106763), hydrothermal treatment with or without the addition of hydrogen bond breakers in a twin-screw extruder (US 4634470). It has also been suggested that simultaneous accommodation and dissolution under "Q conditions" can be achieved by inducing cavitation in the pulp alkaline slurry by ultrasonic treatment (US 5605567).
[0003] EP 2116557 A1 indicates that cellulose stock solution compositions can be produced from fibrous cellulose raw materials such as paper pulp or dissolving grade pulp with a DP in the range of 500-1200 by first carrying out a mechanical treatment in the wet state, which at least partially destroys the outer surface of the fibers, followed by an enzymatic treatment (endoglucanase-type cellulase) that reduces the DP by 30-60% compared to the initial DP. After the enzymatic pretreatment, the cellulose raw material is mixed in an aqueous solution containing an alkali metal hydroxide (e.g., sodium hydroxide) and a zinc salt (e.g., zinc oxide) to create conditions in which the cellulose raw material can begin to dissolve. The final concentrations of NaOH and ZnO are given as 4.5-6.5% and 0.5-1.5%, respectively. Furthermore, it is indicated that for the production of cellulose fibers, the target cellulose concentration must be at least 5.0%. After mixing the cellulose raw material with the alkaline aqueous solution, the resulting intermediate product (slurry) is frozen to make the product solid. Before the final product (e.g., fiber) is produced from the frozen product, the product is thawed. The cellulose dissolves so the solution is clear and, when examined under a microscope, free of insoluble parts and is ready for further processing.
[0004] There are several problems associated with the method described in EP 2116557A1 for producing a cellulose stock solution composition, the most important being that a large amount of enzymes is consumed, which are expensive and make the OPEX very high. The steps of freezing the slurry of pulp fibres in alkali (to -35°C as shown in the examples) followed by melting are time consuming and energy demanding. The fact that no insoluble parts are visible in the stock solution composition under a microscope does not mean that the stock solution composition is suitable for e.g. water. It can contain gel particles that are still not visible under a microscope and therefore suitable for fibre production. EP 2116557A1 does not disclose data on filter clogging values that can be used to determine the content of gel particles and therefore the suitability of the produced stock solution composition. There is no industrial scale fibre production, nor data on the stability of the stock solution composition against gelling over time. There is no guidance on the design of any preferred or optimised equipment to be used for the melting of the frozen slurry to form the final cellulose stock solution composition.
[0005] U.S. Patent No. 4,634,470 discloses a cellulose stock solution composition comprising an aqueous alkali solution containing at least 3% cellulose having a DP of at least 100, and the amount of dissolved cellulose is 13In the C-NMR spectrum, the C4 carbon peak is found at a magnetic field at least 7 ppm higher than that of the C4 carbon peak of solid cellulose. US Patent 4,634,470 shows that a cellulose stock solution composition can be produced from wood pulp by subjecting a mixture of pulp and a hydrogen bond cleavage solution (e.g. water) to a temperature of 100-350°C for some time at a pressure of 10-250 bar, followed by rapid release of the mixture to the open air, thereby reducing the DP of the treated cellulose. To form the stock solution composition, the resulting cellulose is mixed with an aqueous alkali solution maintained at a temperature of 50°C or less. The mixture is stirred at a temperature of 10°C or less to dissolve the cellulose. The treatment of the pulp before dissolution can be carried out, for example, in a twin-screw extruder or an autoclave (STEX). The best results regarding the solubility of the pulp in cold alkali and the stability of the resulting stock solution composition were obtained when the pulp was subjected to some degree of acid hydrolysis before the high temperature and high pressure treatment.
[0006] The problem with the teaching of U.S. Pat. No. 4,634,470 to obtain a concentrate composition that is free of undissolved debris and that is stable against gelling for several days at room temperature is that an acid hydrolysis process of the pulp is required prior to high temperature / pressure treatment, a total process that is slow and expensive.
[0007] US Patent 5,401,447 describes steam explosion (STEX) and dissolution of wood pulp in aqueous alkali with alkali concentrations of 5-15%. US Patent 5,401,447 focuses on acid coagulation chemistry and temperature as well as steaming as a method to slightly improve wet strength of the coagulated fibers and films. The publication lacks detailed information on the quality of the stock solution composition.
[0008] US Patent 6,106,763 shows that the cellulose stock solution composition can be produced by first hydrothermally treating the pulp at a temperature in the range of 100°C to 200°C under a pressure in the range of 0.1MPa to 1.5Ma for about 2 to 6 hours to dissolve the pulp. The pressure reduction is performed slowly and non-explosively. In the examples, the DP is reduced from 577 to about 290 to 390, i.e., by 30 to 50%. The treated cellulose is then dissolved in an aqueous solution of alkali metal hydroxide at at least 0°C to a homogeneous cellulose solution containing 5 to 10% cellulose and up to 10% alkali metal hydroxide. In a further embodiment, the dissolution is performed in an alkali hydroxide solution containing a zinc compound (e.g., ZnO) and / or urea. The addition of a zinc compound and / or urea to the alkali hydroxide solution is said to increase the stability of the stock solution against gelation. In the given examples, dried and hydrothermally treated cellulose was first dispersed in water at a temperature ranging from 3 to 7 °C, then cold (-10 °C to -5 °C) alkaline solution (18% NaOH and about 1.0% ZnO) was added under continuous stirring (mixer rotation speed 150-200 rpm). Stirring was continued for 30-60 minutes and the temperature of the final stock composition was about 6-8 °C. The concentrations of cellulose and sodium hydroxide ranged from 5.1-6.9% and 8.0-8.9%, respectively.
[0009] There are several problems with the method of producing the cellulose stock solution composition described in US Patent 6,106,763. The mixing time required after the addition of the cold sodium hydroxide solution is very long, which requires the production of the stock solution composition in a batchwise manner using large mixing tanks under industrially relevant production conditions. The mixing time required after the addition of the cold sodium hydroxide solution is very long, which requires the production of the stock solution composition in a batchwise manner using large mixing tanks under industrially relevant production conditions. Furthermore, the dissolution temperature of at least 0°C may be too high to achieve rapid dissolution of the cellulose. No guidance is given for the preferred or optimized design of the mixer used to dissolve the cellulose, and no details are given on the best way to combine the hydrothermally treated cellulose with the cold alkali. In some examples included in US Patent 6,106,763, fibers are spun from the stock solution composition produced according to the principles presented. Fiber strength is generally low (10 cN / tex) compared to commodity rayon fiber (20 cN / tex), indicating that the stock solution composition is not well suited for commercial fiber production. It is further known that concentrate compositions prepared according to US Pat. No. 6,106,763 have very limited stability against gelling at room temperature and must be stored under refrigerated conditions.
[0010] US Patent 7108907B1 discloses cellulose stock compositions that can be produced from pretreated (acid hydrolysis and / or STEX) or non-pretreated dissolving pulp, have high cellulose concentrations (5-10%), are stable to gelling at room temperature, and exhibit low amounts (less than 1.0%) of undissolved cellulose, allowing the pulp to be wet-milled to a particle size of less than 30 μm prior to dissolution without the use of anything other than aqueous sodium hydroxide (6.5-11.0%) as a solvent. It is further taught that the wet milling must be carried out in an aqueous slurry containing 0.5-6.5% sodium hydroxide with a cellulose consistency of at least 5.0%. Dissolution is accomplished by adjusting the sodium hydroxide concentration of the slurry to 6.5-11.0% and stirring the slurry at a temperature less than 10°C, limiting the shear rate to a maximum of 9000 s-1, and further requiring external stirring elements to be less than 500 m / min. The crystallinity of the cellulose in the wet milled slurry, as measured by NMR analysis at 50% or less, is a few other structural features of the cellulose in the final stock composition, which are also characterized by NMR analysis.
[0011] The main problem associated with the method for producing a cellulose stock composition described in US Pat. No. 7,108,907 B1 is the high energy consumption in wet-milling to particle sizes below 30 μm, which makes the production of the stock composition uneconomical.
[0012] US Patent 5,605,567 discloses the production of a cellulose stock solution composition by subjecting an alkaline pulp slurry to cavitation, for example by ultrasonic treatment. According to the disclosure, the temperature should be in the range of -7 to 4°C and the concentration of sodium hydroxide should be in the range of 6 to 10%. The energy from the cavitation induced under alkaline conditions for a long time results in a reduction in DP of about 50 to 80%, which promotes dissolution in cold alkali.
[0013] A problem associated with the process for producing a cellulose dope composition described in US Patent No. 5,605,567 is that only a portion of the cellulose is dissolved, making the dope composition unsuitable for fiber spinning, unless the DP is very low, e.g., 195. Such a low DP results in a product with poor mechanical properties.
[0014] One object of the present invention is to provide a method for obtaining a spinning dope in cold alkali which has a high cellulose concentration, a low filter clogging value and is resistant to gelling at room temperature. Summary of the Invention
[0015] The object of the present invention is to provide a method for producing a homogenization process which comprises vigorous mixing of a cellulosic pulp material in an alkaline solution, said vigorous mixing being achieved by providing an agitator used in said homogenization process with a power of at least 150 kW / m 3 (kW supplied to the agitator per mixing unit of liquid volume), a dissolving step in which a cellulosic pulp material is mixed in the alkaline solution to obtain a spinning dope composition, and the power density supplied to the agitator used in the dissolving step is up to 75 kW / m 3 (kW delivered to agitator per mixing unit of liquid volume), and the cellulosic pulp material in the alkaline solution is maintained at a temperature below 0° C. during the homogenization and at least a portion of the dissolution.
[0016] With reference to the above disclosed methods, the following definitions and expressions are set forth below.
[0017] First of all, homogenization and dissolution can be considered as two separate process steps, although these two steps can be carried out in a single tank or tube reactor or in several tank and / or tube reactors that can be arranged in series or parallel.
[0018] Second, the term "vigorous mixing" in homogenization refers to high shear dispersive mixing. The vigorous mixing of the pulp and liquid in the mixer ensures that the pulp fibers are dispersed almost instantly, and the fibers experience a homogenous chemical and thermal environment more or less immediately within at least 120 seconds, preferably within 60 seconds, more preferably within 30 seconds, and even more preferably within 15 seconds after the alkali is combined with the pulp. This is further described below with respect to the figures and examples.
[0019] Additionally, the time can also be calculated as the average residence time in a high shear dispersive mixing device by dividing the internal volume of the device by the volumetric flow rate.
[0020] Moreover, in the dissolution step or zone, vigorous mixing is also applied. However, as noted below, the mixing speed is not as high as in the homogenization step or zone in order to prevent a rapid temperature rise due to viscous dissipation of mechanical energy. Thus, the "vigorous mixing" of homogenization is significantly more intense than the "mixing" of dissolution. Preferably, the power density for the agitator used in the homogenization step is between 150 and 4000 kW / m 3 The power density supplied to the agitator used in the dissolution process is up to 50 kW / m 3 According to yet another embodiment, the power density supplied to the agitator used in the homogenization step is 150 to 2500 kW / m 3 (kW power supplied to the agitator per mixing unit of liquid volume), preferably in the range of 150 to 2000 kW / m 3 More preferably, it is within the range of 200 to 2000 kW / m 3 and the corresponding power density during the melting stage is in the range of 2-50 kW / m 3 Within the range of 5 to 30 kW / m 3 The range is.
[0021] Power density is calculated by dividing the total power supplied to the agitator by the total volume of liquid it is agitating. 3When mixing a liquid volume of 10 ... 3 =400kW / m 3 It becomes.
[0022] Furthermore, in the dissolving step of this method, strong mixing is also applied. However, as described below, the mixing energy is not as high as in the homogenizing step in order to prevent a rapid temperature rise due to viscous dissipation of mechanical energy. Therefore, the "intense mixing" of homogenization is much more powerful than the "mixing" of dissolving. In general, the power density supplied to the agitator for homogenization is at least 5 times, preferably at least 10 times, more preferably 10 to 100 times, more preferably 20 to 100 times, and preferably the time for performing dissolving is at least 5 times, preferably at least 10 times, than the time for performing homogenization.
[0023] As can be seen from above, in addition to the mixing profile, the temperature is also an important parameter of the process. As mentioned above, the temperature is kept below 0° C. during homogenization and at least part of the dissolution. The spinning dope composition produced in the dissolution can be kept at a temperature slightly above 0° C. at the end of the dissolution process if the dissolution process is carried out batchwise, in a tubular reactor, or in several CSTRs (Continuously Stirred Tank Reactors) in succession, but preferably more than 50% of the duration of the dissolution step occurs at a temperature below 0° C. If a continuous dissolution process is carried out in only one CSTR or in a CSTR only, the temperature should always be kept below 0° C., preferably below −3° C., as further disclosed below.
[0024] The cellulose pulp material and the alkaline solution are preferably cooled separately prior to homogenization. To give some examples, the cellulose pulp material can be cooled to a temperature close to its freezing point, such as in the range of 0-5°C. Additionally, the alkaline solution is cooled to a temperature below 0°C, such as in the range of -5°C to about -9°C, the latter being close to its freezing point. The exact combination of temperatures depends on the moisture content in the cellulosic pulp material. Suitable temperatures are discussed further below.
[0025] The combination of the two steps, namely homogenization and dissolution, involving the above mixing and temperature conditions is not disclosed or suggested in the above prior art. [Brief description of the drawings]
[0026] [Figure 1] FIG. 1 is a graph showing the relationship between viscosity and shear rate for a 7.0 wt % NaOH spin dope composition under different conditions. [Diagram 2] FIG. 2 is a graph showing the relationship between viscosity and shear rate for a 7.5 wt % NaOH spin dope composition under different conditions. [Diagram 3] FIG. 3 is a graph showing the relationship between viscosity and shear rate for an 8.0 wt % NaOH spin dope composition under different conditions. [Figure 4] FIG. 4 is a schematic diagram showing the configuration of a system according to an embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic diagram showing the configuration of a system according to another embodiment of the present invention. [Figure 6] FIG. 6 is a characteristic diagram showing the preferred range or window of power density versus residence time in a homogenizer. [Figure 7] FIG. 7 is a characteristic diagram showing the relationship between a preferred range or window of power density and residence time in a resolver. [Figure 8] FIG. 8 is a characteristic diagram showing the relationship between a preferred range or window of power density and residence time in a refiner. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] With respect to the cellulosic pulp material, the cellulosic feedstock used in the present invention is a cellulosic pulp that can be produced by commercial processes for delignification of lignocellulosic biomass, including, but not limited to, Kraft, sulfite, organosolv, or processes in which the lignin and cellulose are separated by acid hydrolysis. The cellulosic starting cellulosic material is preferably a dissolving cellulose pulp having a high alpha cellulose content, preferably greater than about 88% alpha cellulose content.
[0028] The present invention aims to solve the problem of continuously producing a dissolving pulp spinning dope composition that has a high cellulose concentration, low filter clogging, and is resistant to gelation at room temperature and is suitable for use in cold alkali.
[0029] To be industrially viable, a cellulose spinning dope composition and a process for its production must meet several requirements. Important aspects are listed below:
[0030] - To ensure acceptable operating costs (OPEX), the cellulose concentration in the concentrate composition must be sufficiently high (preferably 5% or more).
[0031] - In order to obtain acceptable mechanical properties of the final product, the degree of polymerization (DP) of the cellulose in the concentrate composition must be sufficiently high (preferably higher than 200), where the intrinsic viscosity is measured in a coupled ethylenediamine (CED) solution according to ISO 351:2010(E) = 0.7277 * (IV) 1.105 The intrinsic viscosity (IV) of the polymer was calculated.
[0032] - The filterability of the dope composition needs to be sufficiently high (preferably a filter clogging value of 200 or less) to avoid a large amount of rejects (backwash filters) and frequent filter changes (press filters) that negatively impact OPEX. Especially in fiber production, it is important to remove non-dissolved cellulose fragments, gel particles and certain other contaminants to a sufficient extent to avoid clogging of the spinneret capillaries, which can have a negative impact on the forming process and the final fiber properties. With reference to the clogging values above and the examples below, the clogging values were evaluated by carrying out filtration. A filter (SIKA-FIL20, average pore size 20 μm, 600 g / m, GKN Sinter Metals Filter GmbH, Germany) was used. 2 Metal fiber fleece, air permeability at 200 Pa: 415 l / min / dm 2 The amount of solution passing through the filter was recorded every second after application of an external pressure of 0.5 bar. The inverse mean flow rate (s / g, grams per second) versus time (seconds) was plotted and a linear regression was calculated. The first data point from each measurement was excluded from the calculation. The slope of the approximately linear curve (after the initial transient) multiplied by 10000 was reported as the clogging value.
[0033] - The viscosity of the concentrate composition is sufficiently low (preferably less than 1s) to facilitate degassing (removal of air bubbles), filtration, and shaping, for example in fibers, sponges or films (low pressure drop). -1 The shear rate must be less than 10 Pa when measured at 100 rpm.
[0034] During the processes of degassing, filtering, storing and extruding, the dope composition must be stable against gelling. Since the viscosity decreases with increasing temperature (which is favorable for degassing, filtering and forming), it is advantageous if the dope composition is stable against gelling for a sufficiently long time (preferably more than 24 hours) even at higher temperatures, including room temperature.
[0035] - The process for producing the stock solution composition (combining the alkali and the adapted dissolving pulp to form the stock solution composition) is preferred in its detailed embodiment in that the above requirements 1 to 5 are met and can be applied in a feasible and practical manner on an industrial scale.
[0036] It should be pointed out that some of the above requirements are in conflict with each other: for example, high cellulose DP and high cellulose concentration are both known to adversely affect filterability and degassing, increase viscosity, and shorten gelation time.
[0037] The present invention aims to provide an optimal method for producing a spinning dope composition, a spinning dope composition, and a system for producing a spinning dope composition based on the above-mentioned background and all of the above-mentioned aspects. One example of the main focus of the present invention is to provide a composition range of acid hydrolyzed dissolving pulp, sodium hydroxide, zinc oxide, and water in combination with a specific direct dissolution process that can produce a spinning dope composition with a high cellulose concentration, good filterability (clog resistance), and excellent gelation stability at room temperature. Good gelation stability facilitates degassing, filtration, transportation of the dope composition, and processing at room temperature where the viscosity of the dope composition is low. Conventional dope compositions have the problem of rapid gelation at high temperatures, and require storage and handling (filtration, degassing, transportation, processing) under refrigerated conditions (0°C to 10°C), which increases the viscosity and makes handling difficult. The process for producing the spinning dope composition of the present invention is characterized by the very rapid establishment, in a homogenization step, of a homogenous environment in terms of chemical composition and temperature surrounding the cellulose fibers and their fragments, which is followed by a dissolution step with less intense mixing, during which the actual dissolution of the cellulose pulp in the alkaline solution occurs. The process for producing the spinning dope composition is preferably operated in a continuous manner and is characterized by being very fast compared to the processes of the prior art (for example, viscose, lyocell, direct dissolution in cold alkali).
[0038] Yet another focus is to provide a system suitable for forming the spinning dope composition. As mentioned above, the method according to the invention includes both homogenization and dissolution, and a suitable system is adapted for such steps.
[0039] There are several process parameters that are preferably considered for the method of the present invention, one of which is time. According to one embodiment, the homogenization or residence time in the homogenization unit is carried out for a time period of less than 120 seconds, preferably less than 60 seconds, more preferably less than 30 seconds, and most preferably less than 15 seconds. The homogenization step involves vigorous mixing, and part of this step should be carried out within a time range short enough to immediately disperse the pulp fibers in the alkali and pulp material mixture.
[0040] However, the dissolution step involves relatively mild mixing conditions, even if this step is also carried out with vigorous mixing. According to one embodiment, the dissolution is carried out for a time sufficient for complete dissolution of the cellulose polymer in the alkaline solution. With regard to the term "complete dissolution", this should not be interpreted in an absolute sense, so that substantially complete dissolution covered by this term should also be considered.
[0041] In yet another embodiment of the present invention, the dissolution is carried out for a time of at least 4 minutes, preferably 5 to 60 minutes, more preferably 5 to 45 minutes, and most preferably 5 to 30 minutes. The dissolution should be carried out for a time sufficient to produce an optimal spinning dope composition solution, which is advantageous in that it has a low clogging value, e.g., as described below, down to 200 or less, or even 50 or less.
[0042] According to one embodiment, the temperature in the slurry (cellulosic pulp material in the alkaline solution) is kept within the range of -8°C to -3°C during homogenization and at least part of dissolution. The temperature profile and residence time of the inventive method are interesting aspects. With respect to the temperature range of -8°C to -3°C, the alkaline solution may have a temperature lower than this range, such as a temperature of -8°C to -25°C, before mixing the alkaline solution with the pulp material. Furthermore, the expression "at least part of dissolution" refers again to the fact that the final spinning dope composition produced at the end of dissolution may have a temperature above a certain temperature range, such as a temperature of 2°C. The strong mixing carried out during the dissolution stage results in an increase in the temperature of the solution. Preferably, the solution is kept within the temperature range of -8°C to -3°C during the majority of the dissolution process, i.e. for more than 50% of the time. Furthermore, according to a preferred embodiment, the temperature is kept within the range of -6°C to -3°C during homogenization and at least part of dissolution.
[0043] According to one embodiment of the invention, the vigorous mixing in homogenization includes high shear mixing at a rotation speed of at least 1000 rpm, for example in the range of 1000-3000 rpm. As mentioned above, the mixing in the dissolving step is less vigorous. In one embodiment of the invention, the mixing in dissolving is performed at a rotation speed of less than 300 rpm, preferably in the range of 10-200 rpm, for example in the range of 10-100 rpm. The mixing in the dissolving step can have different temperatures depending on the particular type of arrangement used to carry out the process. As mentioned above, the temperature should be kept below 0°C during at least a portion of the dissolving, although in the case of a batch-type process, the temperature at the end of the batch may be slightly above 0°C. Preferably, the step is carried out such that the spinning dope composition produced in this step does not have a temperature above -3°C. In the case of a continuous process, such as a single CSTR or multiple CSTRs arranged in parallel, the temperature is preferably kept at a constant level, such as preferably below -3°C, more preferably below -4°C.
[0044] Of course, the type of starting material may also be relevant to the method of the present invention. In one embodiment of the present invention, the cellulosic pulp material to be treated is a non-derivatized or low-derivatized cellulose pulp, such as a carbamate-derivatized cellulose pulp. To provide relevant references, WO 03 / 064476 discloses one method for the preparation of carbamate cellulose. Another example of the preparation of carbamate-derivatized cellulose pulp is described in WO 01 / 07485.
[0045] In yet another embodiment, the treated cellulosic pulp material is pretreated prior to homogenization by shortening the chains of the cellulose polymers by scission of the cellulose chains, preferably by random cleavage of the cellulose chains. The chain shortening process can also be called "adaptation". Furthermore, the chain shortening of the cellulose polymers can be performed at least in part by wet milling in water or alkali. According to yet another embodiment, the chain shortening of the cellulose polymers is performed at least in part by a method selected from hydrolysis with sulfuric acid, steam explosion treatment or hydrothermal treatment. Other treatments such as mild acid hydrolysis or enzymatic treatment or treatment with ionizing radiation (e.g. electron beam) are also possible.
[0046] During the process of shortening the chains of the cellulose polymer, other parameters than the actual chain length may also be affected. One example is the viscosity value. The pretreatment including chain shortening may be carried out to provide an intrinsic viscosity value as measured in cupri-ethylenediamine (CEO) solution according to ISO 5351:2010(E) of less than 500, preferably less than 300, most preferably less than 275. Furthermore, the addition of alkali may be carried out in different ways. An alkali solution, for example a solution containing sodium hydroxide, may be added in only one step before or during homogenization or may be added in two or several steps during the process. Furthermore, the type and concentration of the alkali may also be varied according to the invention. In one embodiment of the invention, the alkali solution contains sodium hydroxide in a concentration range of 7-8% by weight calculated on the total weight of the spinning dope composition. In yet another embodiment, the concentration of sodium hydroxide is in the range of 7.2-7.8% by weight, preferably 7.4-7.6% by weight, for example about 7.5% by weight, calculated on the total weight of the spinning dope composition.
[0047] Furthermore, the cellulose concentration may also be varied according to the invention. In one embodiment of the invention, the cellulose concentration is in the range of 5-12% by weight, calculated on the total weight of the spinning dope composition. The preferred range of cellulose concentration for underivatized pulp is usually in the range of 6-12% by weight, whereas for underivatized cellulose pulp the comparable range is 5-8% by weight.
[0048] Further, other substances may be added according to the method of the present invention. In one embodiment, an anti-gelling additive, preferably urea or a zinc-containing additive, is added so that the additive is present during homogenization. Such additive is preferably added before or at the beginning of the homogenization step, but may also be added during other stages of the process. Furthermore, in one embodiment, the anti-gelling additive to be added so that it is present during the homogenization process is ZnO, added in a concentration range of 0.5-2.0 wt.%, for example 0.5-1.4 wt.%, 0.8-1.2 wt.%, calculated on the total weight of the spinning dope composition. An effective and preferred example is a 7.5 wt.% NaOH concentration with about 1.0 wt.%, for example 1.1 wt.% ZnO.
[0049] The process of the present invention can be carried out in many different modes of operation such as batch, semi-batch, and continuous. In one preferred embodiment of the present invention, the process including homogenization and dissolution is carried out continuously.
[0050] In addition to the homogenization and dissolution steps, and possible pre-treatment steps including adaptation, the invention can also include other steps. According to one embodiment, dissolution is completed by passing the pulp material through an alkaline solution, following a mechanical processing step in which high shear forces are applied to raise the temperature of the dope to within the range of 0-30°C, for example 5-10°C. This is a post-treatment step in which the temperature of the dope composition is increased at the same time as it is mechanically processed.
[0051] In the context of the present invention, it can be stated that the spinning dope composition can be advantageously used to prepare regenerated cellulosic fibers. The spinning dope of the present invention can be produced by extruding it through several fine nozzles into a coagulation bath containing one or more acids and / or one or more salts and additives or organic solvents.
[0052] The spinning dope composition contains cellulose in a concentration range of 5-12% by weight and sodium hydroxide in a concentration range of 7-8% by weight, calculated based on the total weight of the spinning dope, and can be obtained by the method disclosed above. The filter clogging value of the unfiltered spinning dope composition has a value in the range of 0-250, such as a value in the range of 0-200, for example a value in the range of 0-100, such as a value in the range of 10-200, preferably a value less than 150, for example a value in the range of 10-70, or even a value less than 50.
[0053] The present invention provides an optimum spinning dope composition having high stability against gelation and indeed good clogging values.
[0054] In one preferred embodiment of the present invention, the concentration range of sodium hydroxide is 7.2-7.8% by weight, calculated on the total weight of the spinning dope composition. In yet another preferred embodiment, the concentration range of sodium hydroxide is 7.4-7.6% by weight, preferably about 7.5% by weight, calculated on the total weight of the spinning dope composition.
[0055] In yet another embodiment of the present invention, the spinning dope composition also contains ZnO in a concentration range of 0.5-2.0% by weight, preferably 0.8-1.2% by weight, calculated on the total weight of the spinning dope composition. As mentioned above, instead of or in combination with ZnO, urea can also be used.
[0056] To provide a further example of interest, a spin dope composition of the invention comprising acid hydrolyzed dissolving pulp and about 7.5% NaOH / 1.1% ZnO (wt %) exhibits excellent stability against gelation when stored at temperatures ranging from 5° C. to 21° C.
[0057] The present invention also provides a method for producing a semiconductor device comprising the steps of: - adapted to receive a cellulose pulp material and an alkaline solution, having high shear mixing means for homogenizing the cellulose pulp material in the alkaline solution, said high shear mixing means being provided with a power of at least 150 kW / m 3a homogenization unit configured to provide a power density of - adapted to receive the cellulosic pulp material homogenized in the alkaline solution from the homogenization unit, having mixing means for mixing the cellulosic pulp material in the alkaline solution, said mixing means being supplied with a maximum of 75 kW / m 3 a melting unit configured to provide a power density of The present invention is directed to an apparatus for producing a spinning dope composition comprising the steps of:
[0058] According to one embodiment of the present invention, the homogenization unit has a heat capacity of 150 to 4000 kW / m 3 in the range of 150 to 2500 kW / m 3 More preferably, in the range of 200 to 2000 kW / m 3 while the dissolving unit is configured to supply a power density to the high shear mixing means used in the homogenization stage in the range of up to 50 kW / m 3 , more preferably 2 to 50 kW / m 3 , and more preferably 5 to 30 kW / m 3 The melting unit is adapted to supply a power density to a mixing means in the melting unit.
[0059] Furthermore, according to another embodiment of the present invention, the high shear mixing means of the homogenization unit is configured to provide a rotational speed of at least 1000 rpm.
[0060] Still further, according to another embodiment, the mixing means of the dissolution unit is configured to provide a rotation speed of less than 300 rpm.
[0061] According to one preferred embodiment, the dissolving unit has cooling means. It should be noted that the homogenization unit may also have cooling means. Thus, in one embodiment, both the homogenization unit and the dissolving unit have cooling means. An example of such a system is shown in Fig. 4 and Fig. 5. It should be noted that the invention embodies both parallel systems and systems operating in series. Furthermore, different types of systems are possible. An example is a system with a batch or continuous dissolving unit. The homogenization step should be carried out continuously, but the setup may be carried out with one or more tubular reactors in series or parallel, or one or more CSTR(s) in series or parallel. In this connection, it should be mentioned that CSTRs or other types of tank reactors can also be used as one or more dissolving units in series or parallel. In one embodiment, several parallel batch operated tank reactors are used as dissolving units, and the dissolving step is carried out in semi-batch mode. However, the homogenization step is still carried out continuously.
[0062] According to one preferred embodiment, the system of the present invention is a continuous system, and preferably the average residence time of the alkaline solution and the cellulosic pulp material in the dissolution unit is at least 5 times, preferably 10 times, more preferably at least 20 times, and most preferably at least 50 times greater than the average residence time of the alkaline solution and the cellulosic pulp material in the homogenization unit.
[0063] According to yet another embodiment, the system operates continuously according to the plug flow principle at least for the homogenization unit, the latter having the advantage that debris or residues of "old pulp" that could otherwise increase the gelling tendency of the freshly fed pulp.
[0064] Also combined system options are entirely possible. One such continuous alternative is that the homogenization unit operates according to the plug reaction principle (e.g., in a tubular reactor) and the dissolution unit operates according to the principle of a continuous tank reactor. The continuous tank reactors can be arranged in series or in parallel according to the present invention.
[0065] Based on the above, it can be further stated that according to one embodiment of the present invention, homogenization is performed according to the plug flow principle and dissolution is performed according to the continuous stirred tank reactor principle.
[0066] When using plug flow, there is no recycle / holdover of partially dissolved cellulose at this stage. Furthermore, the dissolution stage requires more time for dissolution, which also requires some buffering to be provided. For this reason, a CSTR is a suitable alternative to a dissolution unit.
[0067] When comparing the homogenization process and the unit for carrying it out with the dissolution process and the unit for carrying it out, the two mixing operations and the differences between them are important features according to the present invention. According to one embodiment, the homogenization unit comprises a high shear rotor-stator mixer that can be operated at high mixing speeds of 1000 rpm or more, such as in the range of 1000-3000 rpm. Furthermore, according to another embodiment, the homogenization unit operates at mixing speeds in the range of 1000-3000 rpm. It also comprises a twin-shaft counter-rotating agitator suitably arranged in series with the high shear rotor-stator mixer.
[0068] Moreover, according to yet another embodiment of the invention, the dissolving means is operated at a mixing speed of, for example, less than 300 rpm. It is provided with a mixing means in the form of a rotating scraper. The scraper facilitates the heat transfer between the concentrate composition and the tank wall and also prevents freeze-gelling against the tank wall. In this connection, reference can be made to the difference in power density between the homogenization step and the dissolving step as described above.
[0069] Furthermore, the system preferably includes one or more beating units connected to the dissolving unit. The beating units are adapted to receive the cellulosic pulp material dissolved in the alkaline solution from the dissolving unit. The beating units preferably have shearing means. These shearing means can operate according to the rotor-stator principle. In one preferred embodiment, the beating units are high shear mixers, such as high shear rotor / stator devices that can intensely shear the raw liquid composition, for example the "homogenizer" available from Ing A. Maurer SA Ittigen, Switzerland. In such devices, the raw liquid composition is pumped between a stationary disc and a rotating disc, the two discs having similar axes and arranged at a distance from each other, to generate a strong shear effect according to the refiner principle.
[0070] The beating unit results in a temperature increase of the dope composition due to viscous dissipation, for example above 0° C., between 0° C. and 10° C., in the range of 0° C. to 15° C., or for example in the range of 5° C. to 15° C., possibly in the range of 10° C. to 20° C. According to one embodiment, the temperature increase caused by the action of the beating unit of the dope composition is such that the final temperature of the dope composition is in the range of 5° C. to 10° C. Furthermore, the residence time in the refiner is usually a few seconds (1 to 5 seconds) and the power density is 1000 to 6000 kW / m 3 One or more beaters can be used in parallel or in series.
[0071] As mentioned above, the method of the present invention includes at least one beating step following the dissolving step, which brings about viscous dissipation and temperature increase due to shearing to the spinning dope composition. According to one embodiment of the present invention, the temperature increase in the beating step is 0.2-10°C, preferably 2-8°C, more preferably 4-6°C. Furthermore, according to another preferred embodiment, the beating step is carried out during a time period of less than 120 seconds, preferably less than 60 seconds, more preferably less than 30 seconds, and most preferably less than 15 seconds.
[0072] Further, according to one embodiment of the present invention, the beating unit has a pulverizing capacity of 1000 to 8000 kW / m 3 , more preferably 1000 to 6000 kW / m 3 Preferably, the beating unit is configured (or the beating process is carried out) to deliver a power density (kW delivered to the refiner per mixed unit of liquid volume) in the range of 1000 to 15000 rpm. Preferably, the beating unit has two discs, at least one of which rotates relative to the other disc. The latter may, for example, be such that both discs rotate in a different direction from each other, or one is fixed and the other rotates. Preferably, the two discs are arranged on a similar axis and spaced apart at a distance from each other.
[0073] Further, according to another embodiment, the beating unit has a pulverizing capacity of 2000 to 6000 kW / m 3 in the range of 3000 to 5000 kW / m 3 (kW delivered to the beater per mixed unit of liquid density) in the range of
[0074] The beating step can be carried out as a final step, but also between several dissolution steps, as shown in Figure 5. Thus, at least one further dissolution step may be carried out after the beating step.
[0075] By way of further explanation, the term "beating" can be interpreted as a process that involves supplying sufficient energy to provide deagglomeration or deflocculation, i.e. mechanical dispersion.
[0076] The present invention aims to provide an industrial process and an industrial system, which implies a supply of cellulose pulp to the homogenization zone of about 1000 kg / h or even 5000 kg / h, higher than 100 kg / h, and often higher than 500 kg / h. Of course, it is noted that the system of the present invention can also include other units and operating means. Some examples are suitable for suitable transport and supply systems for pulp material and alkali, pumps connected to tubes and / or tank units, including for example rotor-stator pumps, and jacket cooling devices for tank and / or tube units. Furthermore, the tank and / or tubes can be provided with scrapers to scrape the walls and facilitate cooling of the jacket. This also facilitates homogenizing the mixture during the process. [Detailed description of the drawings] 1 to 3 show graphs of shear rate versus viscosity for 7.0 wt% NaOH, 7.5 wt% NaOH, and 8.0 wt% NaOH in the spinning dope compositions under different conditions, respectively. The spinning dope compositions with 7.0% NaOH and 8.0% NaOH already showed strong gelation (1s) after 24 hours of storage at both 5°C and 21°C. -1 <γ<10s -1 In the case of d 2 (log(η)) / d(log(γ)) 2 The spinning dope composition containing 7.5% NaOH showed clear viscosity behavior with only slight changes in the viscosity curve even after 48 hours of storage at both 5°C and 21°C, and the viscosity increased at 1s -1 <γ<10s -1 In the case of d 2 (log(η)) / d(log(γ)) 2 It should be noted that is less than zero. From these figures, it is clear that the preferred concentration range of sodium hydroxide according to the present invention is 7.2 to 7.8% by weight, more preferably 7.4 to 7.6% by weight, and further preferably about 7.5% by weight, calculated based on the total weight of the spinning dope composition.
[0077] Possible systems according to the invention are shown in Figures 4 and 5, which are further explained below.
[0078] The following examples demonstrate the importance of dispersing the pulp fibers very quickly in the cold alkali, so that each fiber is more or less instantly exposed to the same chemical and thermal environment in order to produce a high quality stock composition with less clogging. EXAMPLES
[0079] In the experiment, the alkaline solution was cooled to -8.5°C in a 0.5L jacketed mixing vessel. Wet pulp (40% OD (oven dried), sulfuric acid treated Buckeye V67 cellulose pulp, IV = 229 ml / g) stored at 0°C was quickly added to the cold alkaline solution in the mixing vessel and then immediately dissolved using a counter-rotating (1000 rpm) two-shaft rotary mixer (Electrolux Easy Compact, Model: EHM4 (100), available from Electrolux AB, SE). During mixing, the mixing time was 14 minutes and the temperature of the stock composition was about -5°C. In this way, 0.4 kg of stock composition containing 5.5% cellulose, 8.0% NaOH, and 1.2% ZnO was produced. The clogging value of the resulting stock composition was 32 and no undissolved fiber fragments were detected between the crossed Polaroids in the microscope field. In an otherwise identical experiment, half the pulp was added first, followed by mixing at 1000 rpm for 15 seconds. The second half of the pulp was then quickly added and mixing continued for 14 minutes. The resulting stock composition had a clogging value of 167, and some undissolved fiber fragments were observed under a microscope.
[0080] A tentative explanation is that when the second half of the pulp is in the vessel, a significant portion of the first added pulp has already gone into solution, making the mixture more viscous and preventing the transport (diffusion) of ions to the later added fibers. In a large-scale batch process, it is difficult to uniformly and quickly disperse a large amount of pulp in a large amount of solvent, resulting in poor solubility.
[0081] In another trial, the alkaline solution was cooled to -8.5°C in a 0.5L jacketed mixing vessel. Wet pulp (44.0% oven-dried, sulfuric acid hydrolyzed Buckeye V67, IV=220ml / g) stored at 0°C was quickly added (submerged) to the cold alkaline solution in the mixing vessel after the agitators of a counter-rotating twin-shaft mixer were set and left in place. The pulp was then dissolved using three different procedures.
[0082] A) After the pulp was introduced into the cold alkali in the mixing vessel, mixing (1000 rpm) was started immediately. During mixing, the mixing time was 14 minutes and the temperature of the stock composition was about -5°C. In this way, 0.4 kg of stock composition containing 6.3% cellulose, 7.5% NaOH, and 1.1% ZnO was produced. The clogging value of the resulting stock composition was 31, and no undissolved fiber fragments were detected between the crossed polaroids in the microscope field.
[0083] B) Mixing (1000 rpm) and dissolution were started 30 seconds after the introduction of the pulp into the cold alkali in the mixing vessel. During mixing, the mixing time was 14 minutes and the temperature of the stock composition was about -5°C. In this way, 0.4 kg of stock composition with 6.3% cellulose, 7.5% NaOH, and 1.1% ZnO was produced. The clogging value of the resulting stock composition was 58, and some undissolved fiber fragments were detected between the crossed polaroids in the microscope field.
[0084] C) After introducing the pulp into the cold alkali in the mixing vessel, mixing (1000 rpm) and dissolution were started after 60 seconds. During mixing, the mixing time was 14 minutes and the temperature of the stock composition was about -5°C. In this way, 0.4 kg of stock composition was produced with 6.3% cellulose, 7.5% NaOH, and 1.1% ZnO. The clogging value of the resulting stock composition was 534, and undissolved fiber fragments could be detected between the crossed polaroids in the microscope field.
[0085] A tentative explanation for the high clogging values in the concentrate composition is that the surface of the pulp fiber mass (aggregates) in contact with the cold alkali solution under static conditions rapidly forms a highly viscous and cohesive layer, making it difficult to disperse and homogenize and diffuse the alkali into the pulp fibers when the mixing vessel starts to stir. Cellulose molecules can move directly from a solid state to a gel state under static conditions where the local chemical environment is not optimal (high concentration of cellulose) and the dissolved molecules are not removed by convection. In large-scale batch processes, it is difficult to disperse a large amount of pulp fibers uniformly and quickly in a large amount of solvent. It can be expected that a large proportion of the cohesive pulp aggregates will be generated under more or less static conditions before being subjected to the shearing action of the flocculant / mixing elements.
[0086] To avoid the above problems associated with the slow and uneven dispersion of the pulp in the cold alkali, a continuous process with attention to the rapid homogenization of the pulp in the alkali has been shown to be useful. An example of such a process is shown in Figure 4. In this variant, moist shredded pulp (with or without a small amount of alkali) that is not frozen at a temperature close to 0 ° C and has a consistency of about 12 to 90%, preferably 30 to 50%, can be charged into the hopper by any feeding device (e.g. conveying band or screw feeder) that is gravimetrically fed. The temperature of the pulp can be lowered below 0 ° C in case the pulp contains a few percent of alkali (less than 5% NaOH). Frozen pulp is disadvantageous for a good dispersion of the pulp in the alkali. The cold liquid alkali (water and sodium hydroxide) containing a small amount of dissolved ZnO is pumped into the hopper in a spiral flow pattern, flushing the hopper walls and allowing the powder to be mixed with the homogenization unit 1, which is a counter-rotating intermeshing type twin-shaft agitator 2 or a similar highly efficient mixer operating according to the plug flow principle. The mass flow rates and composition (concentrations of NaOH and ZnO in water) of the cold alkali and pulp mass flows indicate that the composition of the mixed stream entering homogenization unit 1 contains 5-8% cellulose, 7.8% NaOH, and 0.8-1.2% ZnO.
[0087] The temperature of the cold alkali is further adjusted so that the temperature obtained after combining and thoroughly mixing the alkali and pulp in the homogenization unit 1 is in the range of -8 to -3°C, preferably -6°C to -4°C. The speed of the pump 4 is adjusted so that the slurry / liquid level in the hopper is maintained constant during operation. The high shear (HS) mixer 3, which is part of the homogenization unit 1, is of the rotor-stator type. The vigorous mixing of the pulp and the liquid in the mixer of the homogenization unit 1 ensures that the pulp fibers are dispersed almost instantly and that the fibers experience a more or less homogenous chemical and thermal environment after combining the alkali and the pulp, preferably for about 120 seconds or less, more preferably for about 60 seconds or less, even more preferably for about 30 seconds or less, and most preferably for 15 seconds or less. The alkali pulp slurry is further pumped to a stirring tank (dissolving unit 5) equipped with a rotating scraper 7, which also serves as an agitator. If necessary, the stirring tank of the dissolving unit 5 can be equipped with an internal high shear mixer in addition to the scraper 7. The scraper 7 is important to avoid gelling of the dope composition rotating against the cold tank wall. The volume (size) of the stirred tank is adjusted so that the average residence time is about 5-15 minutes, which can work according to the principle of a continuous stirred tank reactor (CSTR). The jacketed stirred tank is thermostated to about -5°C. The dope composition is then pumped through a set of beating units 6 (one or more in series), which increase the temperature of the dope composition by viscous dissipation (shear) to a final temperature of about 0°C-20°C, 5°C-15°C, for example 5°C-10°C, but can also be 10°C-20°C.
[0088] In another variant shown in FIG. 5, an aqueous pulp slurry with a consistency of about 8-15%, preferably 9-12%, with or without alkali at a temperature close to 0° C. but not frozen, is pumped to the inlet of a homogenization unit 1 equipped with a rotor-stator type high shear mixer 3. If the aqueous pulp slurry contains a few percent of alkali (less than 5% NaOH), the temperature can be reduced to below 0° C. A low-temperature liquid alkali (water and sodium hydroxide) containing a small amount of dissolved ZnO is also pumped to the inlet of the same high shear mixer 3. The vigorous mixing ensures that the pulp fibers are dispersed almost instantly and that after combining the alkali with the pulp, the fibers experience a homogenous chemical and thermal environment for more or less at least 120 seconds, preferably 60 seconds, even more preferably within 30 seconds, most preferably within 15 seconds. The mass flow rate and composition of the cold alkali (concentration of NaOH and ZnO in water) and the mass flow rate of the pulp are adjusted so that the composition of the mixed flow entering the high shear mixer 3 is 5-8% cellulose, 7.2-7.8% NaOH and 0.8-1.2% ZnO. The temperature of the cold alkali is further adjusted so that the temperature obtained after combining and thoroughly mixing the alkali and the pulp in the high shear mixer 3 of the homogenization unit 1 is in the range of -8 to -3 °C, preferably -6 °C to -4 °C. The alkaline pulp slurry is further led to a stirred tank (dissolving unit 5) equipped with a rotating scraper 7. If necessary, the stirred tank of the dissolving unit 5 can be equipped with an internal high shear mixer in addition to the scraper 7. The scraper 7 is important to avoid gelling of the stock composition rotating against the cold tank wall. The volume (size) of the dissolving section 5 is adjusted so that the average residence time is about 5 to 15 minutes. The stock composition is then pumped through a set of beating units 6 (one or more in series) where viscous dissipation (shear) raises the temperature of the stock composition to about 0°C-20°C, 5°C-15°C, for example 5-10°C, but may be 10°C-20°C.
[0089] It is preferred to use a continuous dissolution method. Batch dissolution is problematic as shown in the following examples. Dissolving pulp in cold alkali in a batchwise manner leads to a deterioration in the quality of the concentrate composition in terms of clogging value (a measure of how fast the concentrate composition flows through the filtration medium under a certain pressure drop) in subsequent batches after the first batch is dissolved in a clean dissolution tank. A high clogging value (CV) indicates that the concentrate composition contains a high concentration of gel particles and / or undissolved fiber pieces that will clog the subsequent filters. In the following examples, a 35 kg batch of concentrate composition was prepared in a 60 liter jacketed batch mixer (dissolution unit 5) equipped with a scraper 7 and an internal high shear mixer. The formulation was 5.3% cellulose (sulfuric acid hydrolyzed buckeye V67, IV=229 ml / g), 8% NaOH and 1.2% ZnO. The alkali solution (9.4% NaOH, 1.4% ZnO and balance H2O) was cooled to -9.8°C. The set temperature of the cooling jacket of the dissolving section 5 was -5°C. 30.3 kg of cold alkali was pumped into the dissolving unit 5 where 4.7 kg of wet pulp at 0°C was added. The dissolving unit 5 was closed and the scraper 7 and the high shear mixer were started. The high shear mixer was run for 3 minutes. The temperature of the stock composition was about -4.5°C. After 12 minutes, the high shear mixer was started again and run until the temperature of the stock composition reached 5°C. After the first dissolving batch, the stock composition was poured out of the dissolving tank, leaving about 0.5 kg of stock composition on the tank walls and on the mixing elements (scraper and high shear mixer). This process was then repeated to produce a total of three batches under the same conditions. No undissolved fiber fragments could be detected under the microscope between the crossed polaroids in any of the stock compositions. However, the measured clogging values of the batches were 16, 146 and 160, respectively. The result can be explained by the fact that the concentrate composition remaining on the dissolving unit walls is gelling against the cold dissolving unit surface during the empty phase, contaminating the next batch. The remaining concentrate composition can even freeze-gel upon contact with the cold alkali having a temperature lower than the freezing point of the concentrate composition.Thus, it is difficult to produce expensive concentrate compositions in a batchwise manner without thoroughly cleaning the dissolution unit 5 between batches, which is a time-consuming, expensive and impractical process.
[0090] Another configuration of the dissolution unit 5 is shown in FIG. 5. The lower part of FIG. 5 shows an apparatus with a dissolution unit 5 including three relatively small continuous stirred tank reactors (CSTRs) 105', 105'', 105'''' arranged in series, indicated by dashed lines from the high shear mixer 3 of the homogenization unit 1, then passes through each of the three consecutive CSTRs of the dissolution unit 5 and further through the beating unit 6. In this arrangement, the risk of part of the stock composition passing through the dissolution unit 5 without undergoing the desired residence time for proper dissolution of the cellulose polymer in the alkaline solution is reduced. Turning to FIG. 5, the dissolution unit 5 may be arranged as a single stand-alone unit or as several units in series or parallel. As shown, when multiple dissolution units 5 are arranged in series, one or more beating units 106 can be arranged between one or more of the dissolution units 105', 105'', 105'''.
[0091] FIG. 6 shows a preferred range or window of residence time versus power density in the homogenizer of the present invention. Furthermore, FIG. 7 shows a preferred range or window of power density versus residence time in the dissolver of the present invention. Based on the above, according to one embodiment of the present invention, a power density of 200 to 2000 kW / m 3 The power density x residence time product in the homogenization process with a residence time of 1 to 30 seconds is 4000 to 20000 (kW * s) / m 3 in the range of 6000 to 14000 (kW * s) / m 3 The range is 4 to 50 kW / m 3 The product of power density * residence time in the melting process with a residence time of 240 to 1800 seconds is 4000 to 25000 (kW * s) / m 3 in the range of 7000 to 15000 (kW * s) / m 3The range may be:
[0092] Further, FIG. 8 shows a preferred range or time window of power density and residence time in the refiner of the present invention. Based on the above, according to one embodiment of the present invention, the power density is 1000 to 6000 kW / m 3 And the product of power density * residence time in the beating process with a residence time of 0.5 to 5 seconds is 2000 to 15000 (kW * s) / m 3 range, preferably 3000 to 12000 (kW * s) / m 3 The range may be: The invention as originally claimed in the present application is set forth below. [1] In homogenization involving vigorous mixing of cellulosic pulp material in an alkaline solution, the agitator used in the homogenization process must have a torque of at least 150 kW / m 3 power density (kW delivered to the agitator per unit of mixed liquid volume) of 1000 rpm, followed by In the dissolution step, which involves mixing a cellulosic pulp material in an alkaline solution to obtain a spinning dope composition, the power density (kW supplied to the agitator per mixing unit of liquid volume) supplied to the agitator used in the dissolution step is set to a maximum of 75 kW / m 3 year, A method for producing a spinning dope composition, characterized in that the cellulosic pulp material in the alkaline solution is maintained at a temperature of less than 0°C during the homogenization period and at least a portion of the dissolution period. [2] The power density supplied to the agitator used in the homogenization step is 150 to 4000 kW / m 3 and the power density supplied to the agitator used in the dissolution process is set to a maximum of 50 kW / m 3 The method according to [1], characterized in that [3] The method of any one of [1] or [2], wherein the dissolution is carried out for a time sufficient to substantially completely dissolve the cellulose polymers of the cellulosic pulp material in the alkaline solution. [4] The method according to any one of [1] to [3], characterized in that the homogenization is carried out for a time period of less than 120 seconds, preferably less than 60 seconds, more preferably less than 30 seconds, and most preferably less than 15 seconds, preferably the power density supplied to the agitator used for the homogenization (power density supplied to the agitator per mixing unit of liquid volume) is at least 5 times, more preferably at least 10 times, and even more preferably 10 to 100 times higher than the power density supplied to the agitator used for the dissolution, preferably the time period for which the dissolution is carried out is at least 5 times, more preferably at least 10 times, higher than the time period for which the homogenization is carried out. [5] The method according to any one of [1] to [4], wherein the dissolution is carried out for at least 4 minutes, preferably 5 to 60 minutes, more preferably 5 to 45 minutes, and most preferably 5 to 30 minutes. [6] The power density supplied to the agitator used in the homogenization step (kW supplied to the agitator per mixing unit of liquid volume) is 150 to 2500 kW / m 3 in the range of 150 to 2000 kW / m 3 More preferably, in the range of 200 to 2000 kW / m 3 The method according to any one of [1] to [5], characterized in that [7] The power density supplied to the agitator used in the dissolution process is 2 to 50 kW / m 3 More preferably, in the range of 5 to 30 kW / m 3 The method according to any one of [1] to [6], wherein the range is [8] The product of power density and residence time in the homogenization step is 200 to 2000 kW / m 3 4000~20000(kW*s) / m at a power density range of 1~30 seconds and a residence time range of 1~30 seconds. 3 in the range of 6000 to 14000 (kW * s) / m 3 is in the range of The product of the power density and the residence time in the melting step is 4 to 50 kW / m 3 and residence time in the range of 240 to 1800 seconds, 4000 to 25000 (kW * s) / m 3 in the range of 7000 to 15000 (kW * s) / m 3 The method according to any one of [1] to [7], characterized in that the range of [9] The method according to any one of [1] to [8], characterized in that the temperature of the cellulosic pulp material in the alkaline solution is maintained within the range of -8°C to -3°C during the homogenization period and at least a portion of the dissolution period.
[10] The method according to any one of [1] to [9], characterized in that the vigorous mixing in the homogenization includes high shear mixing at a rotation speed of at least 1000 rpm.
[11] The method according to any one of [1] to
[10] , characterized in that the mixing in the dissolution is carried out at a rotation speed of 300 rpm or less.
[12] The method according to any one of [1] to
[11] , wherein the cellulosic pulp material being treated is underivatized or underivatized cellulose pulp.
[13] The method according to any one of [1] to
[12] , further comprising at least one beating step subsequent to the dissolving step, the beating step providing viscous dissipation and temperature increase to the spinning dope composition by shear.
[14] The method according to
[13] , characterized in that the temperature increase in the beating step is 0.2 to 10°C.
[15] The beating process is carried out at a pressure of 1000 to 8000 kW / m 3 , more preferably 1000 to 6000 kW / m 3 The method according to any one of
[13] or
[14] , characterized in that it is carried out at a power density (kW supplied to the beater per mixed unit of liquid volume) in the range of:
[16] The beating process is carried out at a pressure of 2000 to 6000 kW / m 3 in the range of 3000 to 5000 kW / m 3 The method according to any one of
[13] to
[15] , characterized in that it is carried out at a power density (kW supplied to the beater per mixed unit of liquid volume) in the range of
[17] The product of power density and residence time in the beating step is 1000 to 6000 kW / m 3 2000-15000 (kW * s) / m for power densities in the range of 0.5-5 seconds and residence times in the range of 0.5-5 seconds. 3 range, preferably 3000 to 12000 (kW * s) / m 3 The method according to any one of
[13] to
[16] , characterized in that
[18] The method according to any one of
[13] to
[17] , characterized in that at least one further dissolution step is carried out after at least one of the at least one beating steps.
[19] The cellulosic pulp material is pretreated prior to homogenization by shortening the chains of the cellulose polymers by scission of the cellulose chains, preferably by random cleavage of the cellulose chains. A method according to any one of [1] to
[18] .
[20] The method according to
[19] , characterized in that the chain shortening of the cellulose polymer is carried out at least in part by wet grinding in alkali.
[21] The method according to any one of
[19] or
[20] , characterized in that the chain shortening of the cellulose polymer is carried out, at least in part, by a method selected from the group consisting of hydrolysis with sulfuric acid, steam explosion treatment, and hydrothermal treatment.
[22] The method according to any one of [1] to
[21] , wherein the alkaline solution contains sodium hydroxide in a concentration range of 7 to 8% by weight, calculated based on the total weight of the spinning dope composition.
[23] The method according to
[22] , wherein the concentration of the sodium hydroxide is within the range of 7.2 to 7.8% by weight, calculated based on the total weight of the spinning dope composition.
[24] The method according to any one of [1] to
[23] , wherein the concentration of the cellulose is in the range of 5 to 12% by weight calculated based on the total weight of the spinning dope composition.
[25] The method according to any one of [1] to
[24] , characterized in that an additive for preventing gelling, preferably an additive containing urea or zinc, is added so that the additive is present during the homogenization.
[26] The method according to
[25] , wherein the additive for preventing gelation is ZnO added in a concentration range of 0.5 to 1.4 wt % calculated based on the total weight of the spinning dope composition.
[27] The method according to any one of [1] to
[26] , characterized in that the processes including the homogenization and the dissolution are carried out continuously.
[28] The method according to any one of [1] to
[27] , characterized in that the dissolution is completed by passing the pulp material through the alkaline solution after a mechanical working step of increasing the temperature of the spinning dope composition to within the range of 0 to 30°C by applying high shear force.
[29] The method according to any one of [1] to
[28] , characterized in that the method comprises a subsequent treatment of the dope composition in a coagulation bath, preferably comprising the sodium carbonate or sodium sulfate.
[30] The method according to any one of [1] to
[29] , characterized in that the homogenization is carried out according to the plug flow principle and the dissolution is carried out according to the continuous stirred tank reactor principle.
[31] A method for homogenizing a cellulose pulp material in an alkaline solution, comprising: 3 a homogenization unit (1) configured to provide a power density (kW provided to the agitator per mixed unit of liquid volume) of a homogenizing unit (1) adapted to receive the cellulosic pulp material homogenized with the alkaline solution from the homogenization unit (1), comprising a mixing means (7) for mixing the cellulose solution in the alkaline solution, and a power source (10) for supplying a maximum of 75 kW / m 3 a dissolving unit (5) configured to provide a power density (kW delivered to the agitator per mixed unit of liquid volume) of An apparatus for producing a concentrate composition comprising:
[32] The homogenization unit (1) supplies 150 to 4000 kW / m to the high shear mixing means (3). 3 in the range of 150 to 2500 kW / m 3 More preferably, in the range of 150 to 2000 kW / m 3 More preferably, in the range of 200 to 2500 kW / m3
[0023] configured to provide a power density in the range of The melting unit (5) supplies a maximum of 50 kW / m 3 , more preferably 2 to 50 kW / m 3 , and more preferably 5 to 30 kW / m 3 The apparatus according to
[31] , characterized in that it is configured to provide a power density in the range of
[33] The apparatus according to any one of
[31] or
[32] , characterized in that the dissolution unit (5) comprises a cooling means.
[34] A continuously operating system, preferably wherein the average residence time of the alkaline solution and the cellulosic pulp material in the dissolution unit (5) is at least 5 times, preferably at least 10 times, greater than the average residence time of the alkaline solution and the cellulosic pulp material in the homogenization unit, preferably wherein the homogenization unit (1) is operated according to the plug flow principle. The apparatus according to any one of
[31] to
[33] , characterized in that the dissolution unit (5) is adapted to be operated according to the continuous stirred tank reactor principle.
[35] The apparatus according to any one of
[31] to
[34] , characterized in that the homogenization unit (1) comprises a high shear rotor-stator mixer (3).
[36] The apparatus according to any one of
[31] to
[35] , characterized in that the homogenization unit (1) comprises a twin-shaft counter-rotating agitator (2).
[37] The apparatus according to any one of
[31] to
[36] , characterized in that the high shear mixing means (3) of the homogenization unit (1) is configured to provide a rotation speed of at least 1000 rpm.
[38] Apparatus according to any one of
[31] to
[37] , characterized in that the mixing means (7) of the dissolution unit (5) is configured to provide a rotation speed of less than 300 rpm.
[39] The apparatus according to any one of
[31] to
[38] , further comprising a beating unit (6) connected to the dissolving unit (5), the beating unit (6) including a shearing means.
[40] The beating unit (6) has a power consumption of 1000 to 8000 kW / m 3 , more preferably 1000 to 6000 kW / m 3 , more preferably 2000 to 6000 kW / m 3 in the range of 3000 to 5000 kW / m 3
[39] , characterized in that the refining unit (6) is configured to supply a power density (kW supplied to the refining unit per mixed unit of liquid) in the range of 0.1 to 1.0 kW, preferably wherein the refining unit (6) comprises at least two discs, at least one of which is arranged to rotate relative to the other disc, and even more preferably wherein the two discs are refining discs spaced apart from each other and arranged on a common axis.
Claims
1. a shear mixing means (3) adapted to receive the cellulose pulp material and the alkaline solution and having a single agitator or a plurality of agitators for homogenizing the cellulose pulp material in the alkaline solution, said shear mixing means (3) being provided with a power of at least 150 kW / m 3 a homogenization unit (1) configured to provide a power density (kW provided to said single agitator or agitators per mixed unit of liquid volume); a mixing means (7) adapted to receive the homogenized cellulose pulp material in the alkaline solution from the homogenization unit (1) and carry out dissolution, the mixing means (7) having a single agitator or a plurality of agitators for mixing the cellulose pulp material in the alkaline solution, the mixing means (7) having a maximum power of 75 kW / m 3 a dissolution unit (5) configured to provide a power density (kW provided to said single agitator or agitators per mixed unit of liquid volume) of having 13. An apparatus for producing a spinning dope composition, characterized in that the dissolution unit (5) is adapted to maintain the cellulose pulp material in the alkaline solution at a temperature below 0° C. during at least a portion of the dissolution.
2. 2. Apparatus according to claim 1, characterized in that the homogenization unit (1) is adapted to keep the cellulose pulp material in the alkaline solution at a temperature below 0° C. during the homogenization period.
3. 3. The apparatus according to claim 1 or 2, characterized in that the homogenization unit (1) and the dissolution unit (5) are adapted to keep the cellulose pulp material in the alkaline solution at a temperature below 0°C during the homogenization and at least a part of the dissolution.
4. The homogenization unit (1) applies a power of 150 to 4000 kW / m to the shear mixing means (3). 3 [0023] configured to provide a power density in the range of The dissolving unit (5) supplies a maximum of 50 kW / m 3 4. An apparatus as claimed in claim 1, 2 or 3, configured to provide a power density of
5. The homogenization unit (1) applies a power of 150 to 2500 kW / m to the shear mixing means (3). 3 5. Apparatus according to any one of claims 1 to 4, characterized in that it is arranged to provide a power density in the range of
6. The homogenization unit (1) applies a power of 150 to 2000 kW / m to the shear mixing means (3). 3 6. Apparatus according to any one of claims 1 to 5, configured to provide a power density in the range of
7. The homogenization unit (1) applies a power of 200 to 2000 kW / m to the shear mixing means (3). 3 7. Apparatus according to any one of claims 1 to 6, configured to provide a power density in the range of
8. The dissolving unit (5) supplies 2 to 50 kW / m to the mixing means (7). 3 8. Apparatus according to any one of claims 1 to 7, characterized in that it is arranged to provide a power density in the range of
9. The dissolving unit (5) supplies 5 to 30 kW / m to the mixing means (7). 3 9. Apparatus according to any one of claims 1 to 8, configured to provide a power density in the range of
10. 10. Apparatus according to any one of the preceding claims, characterized in that the dissolution unit (5) comprises cooling means.
11. 11. Apparatus according to any one of the preceding claims, characterized in that the homogenization unit (1) is a cooling means.
12. 12. Apparatus according to any one of the preceding claims, characterized in that the dissolution unit (5) and / or the homogenization unit (1) comprise cooling means arranged to maintain the temperature of the cellulose pulp material in the alkaline solution within the range of -8°C to -3°C during the homogenization and at least a part of the dissolution.
13. 13. Apparatus according to any one of the preceding claims, characterized in that it is a continuously operating system.
14. 14. The apparatus according to claim 1, wherein the average residence time of the alkaline solution and the cellulose pulp material in the dissolution unit (5) is at least 5 times longer than the average residence time of the alkaline solution and the cellulose pulp material in the homogenization unit (1).
15. 15. The apparatus according to claim 1, wherein the average residence time of the alkaline solution and the cellulose pulp material in the dissolution unit (5) is configured to be at least 10 times longer than the average residence time of the alkaline solution and the cellulose pulp material in the homogenization unit (1).
16. 16. Apparatus according to any one of the preceding claims, characterized in that the homogenization unit (1) is adapted to operate according to the plug flow principle.
17. 17. Apparatus according to any one of the preceding claims, characterized in that the dissolution unit (5) is adapted to operate according to the principle of a continuous stirred tank reactor.
18. Apparatus according to any one of the preceding claims, characterized in that the homogenization unit (1) comprises a shear rotor-stator mixer (3).
19. 19. Apparatus according to any one of the preceding claims, characterized in that the homogenization unit (1) comprises a twin-shaft counter-rotating agitator (2).
20. 20. Apparatus according to any one of the preceding claims, characterized in that the mixing means (7) of the dissolution unit (5) are adapted to provide a rotation speed of less than 300 rpm.
21. 21. Apparatus according to any one of the preceding claims, further comprising a beating unit (6) connected to the dissolving unit (5), said beating unit (6) including shearing means.
22. The beating unit (6) has a power of 1000 to 8000 kW / m 3 22. The apparatus of claim 21, configured to provide a power density (kW delivered to the beating unit per mixed unit of liquid volume) in the range of:
23. The beating unit (6) has a power of 1000 to 6000 kW / m 3 23. The apparatus according to claim 21 or 22, characterized in that it is configured to deliver a power density (kW delivered to the beating unit per mixed unit of liquid volume) in the range of:
24. The beating unit (6) has a power of 2000 to 6000 kW / m 3 24. The apparatus according to any one of claims 21 to 23, characterized in that it is configured to deliver a power density (kW delivered to the beating unit per mixed unit of liquid volume) in the range of
25. The beating unit (6) has a power of 3000 to 5000 kW / m 3 25. Apparatus according to any one of claims 21 to 24, characterized in that it is configured to deliver a power density (kW delivered to the beating unit per mixed unit of liquid volume) in the range of
26. The beating unit (6) has at least two discs, 26. Apparatus according to any one of claims 21 to 25, wherein one of the at least two disks is arranged to rotate relative to the other disk.
27. The beating unit (6) has at least two discs, 27. Apparatus according to any one of claims 21 to 26, characterized in that the at least two discs are beating discs arranged on a common axis with a distance between them.
28. 28. Apparatus according to any one of the preceding claims, comprising a mechanical processing unit for completing said dissolution by subjecting the pulp material in the alkaline solution to shear forces.
29. 29. Apparatus according to any one of the preceding claims, characterized in that it comprises a plurality of said homogenization units (1) and / or a plurality of said dissolving units (5).
30. 30. Apparatus according to any one of the preceding claims, comprising means for adding at least one additive to the cellulose pulp material and / or to the cellulose pulp material in the alkaline solution.
31. 31. Apparatus according to claim 30, characterized in that the means for adding at least one additive adds at least one additive before or in the homogenization unit (1).
32. 32. The device of claim 31, wherein the at least one additive is an anti-gelling additive.
33. 32. The apparatus of claim 31, wherein the at least one additive is urea or a zinc-containing additive.
34. 34. An apparatus according to any one of the preceding claims, characterized in that it is connected to at least one pre-treatment unit arranged before the homogenization unit (1), the pre-treatment unit being arranged to pre-treat the cellulose pulp material before homogenizing it in an alkaline solution.
35. 35. The apparatus according to claim 1, further comprising a unit for after-treating the produced dope composition in a coagulation bath.
36. 36. Apparatus according to any one of the preceding claims, characterized in that it is complemented with a subsequent filter unit for filtering the produced spinning dope composition.
37. 37. An apparatus according to any one of claims 1 to 36, wherein the cellulose pulp material being treated is underivatised cellulose pulp.
Citation Information
Patent Citations
Preparation of cellulose solution
JP1997316101A
Method for producing cellulose molding
JP2001139697A
JPP4028003B
Cellulose dope and process for producing the same
WO2001034655A1