Electrophotographic photoreceptor, process cartridge and electrophotographic device
A photoreceptor surface layer made of polyarylate and polycarbonate with specific structural units enhances scratch resistance, addressing image defects in low-temperature, low-humidity environments by increasing resin entanglement and impact absorption.
Patent Information
- Application Number
- JP2022188615
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-25
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2042-11-25
AI Technical Summary
Electrophotographic photoreceptors experience streak-like image defects due to scratches caused by external additives and hard foreign substances in low-temperature, low-humidity environments, as the contact member becomes hard and scratches occur at the point of contact.
The photoreceptor's surface layer is composed of a mixture of polyarylate and polycarbonate with specific structural units, enhancing scratch resistance by increasing resin entanglement and absorbing external impacts.
The surface layer with polyarylate and polycarbonate improves scratch resistance, preventing image defects during long-term use in low-temperature, low-humidity conditions.
Smart Images

Figure 0007596350000029 
Figure 0007596350000030 
Figure 0007596350000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an electrophotographic photoreceptor, a process cartridge, and an electrophotographic apparatus. [Background technology]
[0002] 2. Description of the Related Art In electrophotographic photosensitive members, process cartridges and electrophotographic apparatuses, extensive studies have been made to date in order to improve image quality during long-term use. As an example, Patent Document 1 describes that an electrophotographic photoreceptor (hereinafter also referred to as "photoreceptor") containing a polyarylate and a polycarbonate having a specific skeleton in a photosensitive layer can improve the wear resistance and scratch resistance of the photoreceptor against load. However, it is believed that because it is difficult to uniformly disperse the two types of resins in the layer, fine irregularities are formed on the surface. It is believed that this structure functions to reduce the contact area with external substances. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 04862663 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when the inventors used the photoconductor described in Patent Document 1 for a long period of time in a low-temperature, low-humidity environment, they found that streaky image defects due to scratches occurred. The cause of this was that external additives contained in the toner, paper powder, or other hard foreign matter became caught in the contact member at the rubbing portion between the surface layer of the photoconductor and the contact member, and scratches started from there. It is believed that one of the reasons why this phenomenon was observed in a low-temperature, low-humidity environment is that the contact member itself became hard due to the effect of low temperature. Therefore, the inventors focused on the resin that constitutes the surface layer of the electrophotographic photoreceptor and found that the use of a surface layer that is a mixture of polyarylate and polycarbonate having a specific structure improves scratch resistance against external impact, leading to the present invention.
[0005] SUMMARY OF THE PRESENTLY PREFERRED EMBODIMENTS Accordingly, an object of the present invention is to provide an electrophotographic photoreceptor, a process cartridge and an electrophotographic apparatus which are capable of suppressing image defects by selecting a resin having high resistance to external impact. [Means for solving the problem]
[0006] The above object can be achieved by the present invention as described below. That is, a first aspect of the present invention is an electrophotographic photoreceptor having a surface layer containing polyarylate and polycarbonate, The polyarylate has at least one structural unit selected from the group consisting of a structural unit represented by the following formula (1-1), a structural unit represented by the following formula (1-2), and a structural unit represented by the following formula (1-3), The polycarbonate has a structural unit represented by the following formula (2-1). [ka] [ka] [ka] [ka]
[0007] A second embodiment is an electrophotographic photoreceptor having a surface layer containing polyarylate and polycarbonate, In the component analysis of the polymer component recovered from the surface layer, The polyarylate In pyrolysis gas chromatography mass spectrometry in the presence of TMAH, the TIC has a peak having an MS spectrum in which components of m / z = 242 and m / z = 227 are detected, Deuterated chloroform was used 1 In the H-NMR spectrum, it has peaks at 2.40±0.02 ppm and 2.35±0.02 ppm. The polycarbonate is In pyrolysis gas chromatography mass spectrometry in the presence of TMAH, the TIC has a peak having an MS spectrum in which components of m / z = 242 and m / z = 227 are detected, Deuterated chloroform was used 1 The electrophotographic photoreceptor is characterized by having a peak at 2.40±0.02 ppm in the H-NMR spectrum.
[0008] Furthermore, the process cartridge according to the present invention is a process cartridge which integrally supports the electrophotographic photosensitive member and at least one means selected from the group consisting of a charging means and a developing means, and is detachably attachable to the main body of the electrophotographic apparatus.
[0009] The electrophotographic apparatus of the present invention is an electrophotographic apparatus having the electrophotographic photosensitive member, a charging means, an exposing means, a developing means and a transferring means. Effect of the Invention
[0010] According to the present invention, it is possible to provide an electrophotographic photoreceptor in which the surface layer of the electrophotographic photoreceptor has high scratch resistance and therefore the occurrence of streak-like image defects can be suppressed through long-term use in a low-temperature, low-humidity environment. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a diagram showing an example of a layer structure of an electrophotographic photoreceptor according to the present invention. [Diagram 2] 1 shows an example of a schematic configuration of an electrophotographic apparatus and a process cartridge according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present disclosure will be described in detail below with reference to preferred embodiments. In the first aspect of the present invention, the polyarylate has at least one structural unit selected from the group consisting of the structural unit represented by the above formula (1-1), the structural unit represented by the above formula (1-2), and the structural unit represented by the above formula (1-3), and the polycarbonate has the structural unit represented by the above formula (2-1), thereby improving the scratch resistance of the surface layer.
[0013] The inventors speculate that the reason is as follows. It is generally believed that during printing, a hard foreign object is sandwiched between the surface layer of the photoconductor and a contacting member such as paper or abutting member, and the surface layer is subjected to an external impact, resulting in scratches. There are two ways in which the external impact is received at this time. The first is that the surface of the surface layer is gradually rubbed in a parallel direction against the surface layer due to the external impact, resulting in scratches. The second is that the external impact instantly creates a hole in the vertical direction, which grows and becomes a scratch. The polyarylate according to the present invention is stronger than the polycarbonate according to the present invention in terms of scratch resistance caused by rubbing in the parallel direction, but weaker than the polycarbonate according to the present invention in terms of impact in the perpendicular direction. On the other hand, the polycarbonate according to the present invention is weaker than the polyarylate according to the present invention in terms of scratch resistance caused by rubbing in the parallel direction, but stronger than the polyarylate according to the present invention in terms of impact in the perpendicular direction. Furthermore, it is speculated that the electrophotographic photoreceptor according to the present invention contains the polyarylate and polycarbonate according to the present invention in the surface layer, and the action of the methyl group attached to the aromatic ring enhances the entanglement between the resins, and external impact can be absorbed, further enhancing scratch resistance. Therefore, it is speculated that the surface layer is strong against external impact overall, and shows high scratch resistance.
[0014] Next, the electrophotographic photoreceptor according to one embodiment of the present disclosure will be specifically described. [Electrophotographic photoreceptor] The electrophotographic photoreceptor of the present invention has a surface layer. Fig. 1 is a diagram showing an example of the layer structure of an electrophotographic photoreceptor. In Fig. 1, an undercoat layer 102, a charge generating layer 103, and a charge transport layer (surface layer) 104 are laminated in this order on a support 101. The method for producing the electrophotographic photoreceptor includes a method of preparing the coating liquid for each layer described later, coating the layers in the desired order, and drying the liquid. In this case, the coating liquid can be applied by dip coating, spray coating, inkjet coating, roll coating, die coating, blade coating, curtain coating, wire bar coating, ring coating, etc. Among these, dip coating is preferred from the viewpoint of efficiency and productivity. Each layer will be described below.
[0015] <Support> The support is preferably a conductive support. The shape of the support may be cylindrical, belt-like, sheet-like, or the like. Of these, a cylindrical support is preferable. The outer surface of the support may be subjected to electrochemical treatment such as anodization to form an oxide film, or may be subjected to blasting or cutting. The material of the support is preferably metal, resin, glass, or the like. Examples of metals include aluminum, iron, nickel, copper, gold, stainless steel, and alloys thereof. Among them, an aluminum support using aluminum is preferable, and an aluminum alloy having an oxide film on the outer surface is more preferable. By having an oxide film, injection of electric charge from the support can be suppressed, and thus the charging stability is high. Furthermore, the resin or glass may be made conductive by a process such as mixing or coating with a conductive material.
[0016] <Conductive layer> A conductive layer may be provided on the support. By providing the conductive layer, scratches and irregularities on the surface of the support can be concealed and light reflection on the surface of the support can be controlled. The conductive layer preferably contains conductive particles and a resin. The conductive particles may be made of a material such as metal oxide, metal, or carbon black. Examples of metal oxides include zinc oxide, aluminum oxide, indium oxide, silicon oxide, zirconium oxide, tin oxide, titanium oxide, magnesium oxide, antimony oxide, bismuth oxide, etc. Examples of metals include aluminum, nickel, iron, nichrome, copper, zinc, silver, etc. Among these, it is preferable to use metal oxides as the conductive particles, and it is particularly preferable to use titanium oxide, tin oxide, or zinc oxide. When a metal oxide is used as the conductive particles, the surface of the metal oxide may be treated with a silane coupling agent or the like, or the metal oxide may be doped with an element such as phosphorus or aluminum or an oxide thereof. The conductive particles may have a laminated structure having a core particle and a coating layer that covers the core particle. Examples of the core particle include titanium oxide, barium sulfate, zinc oxide, etc. Examples of the coating layer include metal oxides such as tin oxide. Furthermore, when a metal oxide is used as the conductive particles, the volume average particle size thereof is preferably 1 nm or more and 500 nm or less, and more preferably 3 nm or more and 400 nm or less.
[0017] Examples of the resin include polyvinyl acetal resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, and alkyd resin. The conductive layer may further contain silicone oil, resin particles, a masking agent such as titanium oxide, and the like. The average thickness of the conductive layer is preferably from 1 μm to 50 μm, and particularly preferably from 3 μm to 40 μm. The conductive layer can be formed by preparing a coating solution for the conductive layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of the dispersion method for dispersing the conductive particles in the coating solution for the conductive layer include a method using a paint shaker, a sand mill, a ball mill, and a liquid collision type high-speed disperser.
[0018] <Undercoat layer> An undercoat layer may be provided on the support or the conductive layer. By providing an undercoat layer, the adhesion between layers can be improved and a charge injection blocking function can be imparted. The undercoat layer preferably contains a resin. Alternatively, the undercoat layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group. Examples of the resin include polyvinyl acetal resin, acrylic resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl phenol resin, alkyd resin, polyvinyl alcohol resin, polyethylene oxide resin, polypropylene oxide resin, polyamide resin, polyamic acid resin, polyimide resin, polyamideimide resin, and cellulose resin. Examples of the polymerizable functional group contained in the monomer having a polymerizable functional group include an isocyanate group, a blocked isocyanate group, a methylol group, an alkylated methylol group, an epoxy group, a metal alkoxide group, a hydroxyl group, an amino group, a carboxyl group, a thiol group, a carboxylic anhydride group, and a carbon-carbon double bond group.
[0019] For the purpose of improving electrical properties, the undercoat layer may further contain an electron transporting material, a metal oxide, a metal, a conductive polymer, etc. Among these, it is preferable to use an electron transporting material or a metal oxide. Examples of the electron transport substance include a quinone compound, an imide compound, a benzimidazole compound, a cyclopentadienylidene compound, a fluorenone compound, a xanthone compound, a benzophenone compound, a cyanovinyl compound, an aryl halide compound, a silole compound, a boron-containing compound, etc. An electron transport substance having a polymerizable functional group may be used as the electron transport substance, and the undercoat layer may be formed as a cured film by copolymerizing the electron transport substance with the monomer having the polymerizable functional group. Examples of metal oxides include indium tin oxide, tin oxide, indium oxide, titanium oxide, zinc oxide, aluminum oxide, silicon dioxide, etc. Examples of metals include gold, silver, aluminum, etc. The undercoat layer may further contain an additive.
[0020] The average thickness of the undercoat layer is preferably from 0.1 μm to 50 μm, more preferably from 0.2 μm to 40 μm, and particularly preferably from 0.3 μm to 30 μm. The undercoat layer can be formed by preparing a coating solution for the undercoat layer containing the above-mentioned materials and solvent, forming a coating film from the coating solution, and drying and / or curing the coating solution. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.
[0021] <Photosensitive layer> The photosensitive layer of an electrophotographic photoreceptor is provided on a support, a conductive layer, or an undercoat layer, and is mainly classified into (1) a multi-layer type photosensitive layer and (2) a single-layer type photosensitive layer. (1) The multi-layer type photosensitive layer has a charge generation layer containing a charge generation material and a charge transport layer containing a charge transport material. (2) The single-layer type photosensitive layer has a photosensitive layer containing both a charge generation material and a charge transport material.
[0022] (1) Laminated photosensitive layer The laminated photosensitive layer includes a charge generating layer and a charge transport layer.
[0023] (1-1) Charge generation layer The charge generating layer preferably contains a charge generating material and a resin. Examples of the charge generating material include azo pigments, perylene pigments, polycyclic quinone pigments, indigo pigments, and phthalocyanine pigments. Among these, azo pigments and phthalocyanine pigments are preferred. Among phthalocyanine pigments, oxytitanium phthalocyanine pigments, chlorogallium phthalocyanine pigments, and hydroxygallium phthalocyanine pigments are preferred. The content of the charge generating material in the charge generating layer is preferably from 40% by mass to 85% by mass, and more preferably from 60% by mass to 80% by mass, based on the total mass of the charge generating layer. Examples of the resin include polyarylate, polycarbonate, polyvinyl acetal resin, polyvinyl butyral resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl alcohol resin, cellulose resin, polystyrene resin, polyvinyl acetate resin, polyvinyl chloride resin, etc. Among these, polyvinyl butyral resin is more preferable. The charge generating layer may further contain additives such as an antioxidant and an ultraviolet absorbing agent, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, and benzophenone compounds.
[0024] The average thickness of the charge generating layer is preferably from 0.1 μm to 0.8 μm, and more preferably from 0.15 μm to 0.4 μm. The charge generating layer can be formed by preparing a coating solution for the charge generating layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.
[0025] (1-2) Charge transport layer The charge transport layer preferably contains a charge transport material and a resin. Examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these materials. Among these, triarylamine compounds and benzidine compounds are preferred because they have a high effect of suppressing the generation of black spots.
[0026] Preferred charge transport materials are listed below. [Table 1]
[0027] The content of the charge transport material in the charge transport layer is preferably from 25% by weight to 70% by weight, and more preferably from 30% by weight to 55% by weight, based on the total weight of the charge transport layer. Examples of the resin include polyarylate, polycarbonate, acrylic resin, polystyrene resin, etc. When the charge transport layer is to be the surface layer, it is necessary to contain, among these, polyarylate and polycarbonate having the structure according to the present invention from the viewpoint of scratch resistance.
[0028] The resins used in the first embodiment of the present invention are shown below. The polyarylate has at least one structural unit selected from the group consisting of a structural unit represented by the following formula (1-1), a structural unit represented by the following formula (1-2), and a structural unit represented by the following formula (1-3), The polycarbonate has a structural unit represented by the following formula (2-1). [ka] [ka] [ka] [ka]
[0029] In the surface layer according to the present invention, it is preferable from the viewpoint of scratch resistance that the structural unit represented by the formula (2-1) is contained in an amount of 5 mol % to 40 mol %, which increases entanglement between resins and improves scratch resistance. Furthermore, when the polycarbonate according to the present invention contains 20 mol % or more and 60 mol % or less of the structural unit represented by the formula (2-1), entanglement between the resins is further increased, and scratch resistance is improved.
[0030] A second aspect of the present invention is an electrophotographic photoreceptor having a surface layer containing polyarylate and polycarbonate, In the component analysis of the polymer component recovered from the surface layer, The polyarylate In pyrolysis gas chromatography mass spectrometry in the presence of tetramethylammonium hydroxide (TMAH), the total ion chromatogram (TIC) had peaks with an MS spectrum in which components of m / z = 242 and m / z = 227 were detected; Deuterated chloroform was used 1 In the H-NMR spectrum, it has peaks at 2.40±0.02 ppm and 2.35±0.02 ppm. The polycarbonate is In pyrolysis gas chromatography mass spectrometry in the presence of TMAH, the TIC has a peak having an MS spectrum in which components of m / z = 242 and m / z = 227 are detected, Deuterated chloroform was used 1 The H-NMR spectrum has a peak at 2.40±0.02 ppm.
[0031] The total ion chromatogram (TIC) had peaks with MS spectra in which components of m / z = 242 and m / z = 227 were detected, and deuterated chloroform was used. 1 The presence of a peak at 2.40±0.02 ppm in the H-NMR spectrum indicates the presence of the structural unit of the above formula (2-1).
[0032] In addition, the total ion chromatogram (TIC) had peaks with MS spectra in which components of m / z = 242 and m / z = 227 were detected, and deuterated chloroform was used. 1 The presence of a peak at 2.35±0.02 ppm in the H-NMR spectrum indicates the presence of a structural unit of the following formula (2-2). [ka]
[0033] Therefore, when the polyarylate has the above spectrum, it is shown that it contains at least the structures of the above formula (2-1) and formula (2-2), and it is shown that the polycarbonate contains at least the structure of formula (2-1).
[0034] When the surface layer of the photoreceptor of the present invention contains the polyarylate represented by formula (1-3), the above spectrum is also shown, so that the spectrum is a mixture of both polycarbonate and polyarylate.
[0035] The electrophotographic photoreceptor has a surface layer containing polyarylate and polycarbonate, and the polyarylate and polycarbonate have the above-mentioned specific spectra, which improves the scratch resistance of the surface layer. It is presumed that the polyarylate has a skeleton of the structural part of the above formula (2-1) and a structural part similar thereto, and the polycarbonate has the common structural part of the above formula (2-1), which increases the entanglement between the resins, making it possible to absorb external impacts and further improve scratch resistance. A specific method for analyzing the surface layer will be described below.
[0036] ■Reprecipitation of resin in the surface layer of the photoreceptor Cutting the photoconductor Cut the photoconductor using a jigsaw at a position 10 cm from the end of the photoconductor in the generatrix direction. Wash the inside of the cut 10cm drum Wipe the inside of the cylinder with Silbon paper soaked in chloroform. Dissolve the surface layer Immerse 3 cm of the cut end of the drum in chloroform. (Put about 60cc of chloroform into a 100mL beaker and soak for 5 minutes at room temperature.) Concentrate (concentrate liquefy) Concentrate using a rotary evaporator until the volume is 2 mL and then stop. Re-sink Prepare 50 mL of a methanol / acetone mixture (volume ratio 1:1) and dropwise add the entire amount of the above concentrated solution while stirring. Filter Perform suction filtration using a Kiriyama funnel. (Funnel: SU-40, filter paper: No. 5C-40, both made by Kiriyama Seisakusho Ltd.) Dry Collect the residue on the filter paper with a spatula and vacuum dry (70°C for 1 hour).
[0037] ■Pyrolysis GCMS Equipment configuration: Pyrolysis equipment + gas chromatography (GC) equipment + mass spectrometry (MS) equipment Pyrolysis equipment: Japan Analytical Industry Co., Ltd. JPS-700 GC equipment: Thermo Fisher Scientific FOCUS-GC MS device: ISQ manufactured by Thermo Fisher Scientific Co., Ltd. Sample amount: 0.1 mg (contains TMAH (manufactured by Tama Chemicals Co., Ltd.)) Thermal decomposition temperature: 590°C (using Pyrofoil F590 manufactured by Japan Analytical Industry Co., Ltd.) Column: "HP5-MS" (Agilent Technologies, Inc., 19091S-433, length 30 m, inner diameter 0.25 mm, film thickness 0.25 μm) GC inlet conditions: Inlet Temp: 250℃ Split Flow: 50mL / min GC heating conditions: 40℃ (5min) → 10℃ / min (300℃) → 300℃ (20min) MS conditions: Ion Source Temp: 200℃ MS Transfer Line Temp: 250℃
[0038] ■ NMR measurements Measurement sample preparation 20 mg of a sample is dissolved in 1 g of deuterated chloroform containing tetramethylsilane as a reference substance, and the entire amount is transferred to an NMR tube. (Deuterated chloroform: Sigma-Aldrich Japan Co., Ltd., chloroform-d, model number 612200) (NMR tube: Norell, ST500-7, model number S3010) ·NMR measurement Equipment: Bruker, AVANCE500 Conditions: Proton NMR, automated measurement by ICON-NMR Number of times: 32 Reference peak: The methyl group peak of tetramethylsilane is set as 0 ppm. ■ Separation of polyarylate and polycarbonate The resin is separated from the reprecipitated resin in the surface layer of the photoreceptor using a separation device capable of separating and recovering components, such as size exclusion chromatography or high performance liquid chromatography.
[0039] The content ratio of the charge transport material to the resin is preferably from 4:10 to 20:10, and more preferably from 5:10 to 10:10, by mass ratio.
[0040] The charge transport layer may also contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, and abrasion resistance improvers. Specific examples include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, boron nitride particles, etc. Among these, silica particles are preferred from the viewpoint of scratch resistance, and a volume average particle size of 0.1 μm or more and 0.5 μm or less in the charge transport layer of the present invention can easily absorb external impacts and suppress scratches.
[0041] The average thickness of the charge transport layer is preferably from 5 μm to 50 μm, more preferably from 8 μm to 40 μm, and particularly preferably from 10 μm to 30 μm. The charge transport layer can be formed by preparing a coating solution for the charge transport layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Among these solvents, ether-based solvents or aromatic hydrocarbon-based solvents are preferred.
[0042] ■Volume average particle size The volume average particle size of the particles is measured by the following method. Particles were separated from the layer, and 100 primary particles of these silica particles were observed at 100,000 times magnification using a SEM (scanning electron microscope), the longest and shortest diameters of each primary particle were measured, and the equivalent sphere diameter was calculated from the intermediate value. The 50% diameter (D50v) of the cumulative frequency of the obtained equivalent sphere diameters was calculated, and this was taken as the volume average particle diameter of the particles.
[0043] (2) Single-layer photosensitive layer The single-layer type photosensitive layer can be formed by preparing a coating solution for the photosensitive layer containing a charge generating material, a charge transporting material, a resin and a solvent, forming a coating film of this, and drying it. The charge generating material, the charge transporting material and the resin are the same as the examples of materials in "(1) Multi-layer type photosensitive layer" above.
[0044] <Protective layer> When the protective layer is a surface layer, it contains the resin according to the present invention. The protective layer may contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, scratch resistance / abrasion resistance improvers, and polymerization initiators. Specific examples include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane modified resins, silicone oils, fluororesin microparticles, polystyrene resin microparticles, polyethylene resin microparticles, silica microparticles, alumina microparticles, boron nitride microparticles, titanium oxide, zinc oxide, tin oxide, indium oxide, etc. Among these, silica microparticles are preferred from the viewpoint of scratch resistance, and a volume average particle size of 0.1 μm or more and 0.5 μm or less in the protective layer of the present invention can easily absorb external impacts and suppress scratches.
[0045] Furthermore, a siloxane resin or a charge transporting material can be added. Examples of the charge transporting material include triarylamine compounds, hydrazone compounds, stilbene compounds, pyrazoline compounds, oxazole compounds, thiazole compounds, and triarylmethane compounds. The average thickness of the protective layer is preferably 0.5 μm or more and 10 μm or less, and more preferably 1 μm or more and 7 μm or less. When applying the coating solution for each of the above layers, a coating method such as a dip coating method (dipping method), a spray coating method, a spinner coating method, a bead coating method, a blade coating method, or a beam coating method can be used.
[0046] [Process cartridge and electrophotographic device] The process cartridge according to one embodiment of the present disclosure is characterized in that it integrally supports the electrophotographic photosensitive member described above and at least one means selected from the group consisting of a charging means, a developing means, and a cleaning means, and is detachably attachable to the main body of the electrophotographic apparatus. An electrophotographic apparatus according to one aspect of the present disclosure is characterized by having a process cartridge having at least an electrophotographic photosensitive member and a charging member, and at least one selected from the group consisting of an exposure unit, a developing unit, and a transfer unit.
[0047] FIG. 2 shows an example of a schematic configuration of the process cartridge 21 and an electrophotographic apparatus having the process cartridge 21. In FIG. A cylindrical electrophotographic photoreceptor 11 is driven to rotate around an axis 12 in the direction of an arrow at a predetermined peripheral speed. The surface of the electrophotographic photoreceptor 11 is charged to a predetermined positive or negative potential by a charging means 13. In this embodiment, the charging means 13 may adopt a roller charging method using a roller-type charging member. The charged surface of the electrophotographic photoreceptor 11 is irradiated with exposure light 14 from an exposure means (not shown), and an electrostatic latent image corresponding to the target image information is formed. The electrostatic latent image formed on the surface of the electrophotographic photoreceptor 11 is developed by supplying toner contained in a developing means 15, and a toner image is formed on the surface of the electrophotographic photoreceptor 11. The toner image formed on the surface of the electrophotographic photoreceptor 11 is transferred to a transfer material 17 by a transfer means 16. The transfer material 17 to which the toner image has been transferred is transported to a fixing means 18, where the toner image is fixed, and the transfer material 17 is printed out outside the electrophotographic apparatus. The electrophotographic apparatus may have a cleaning means 19 for removing deposits such as toner remaining on the surface of the electrophotographic photoreceptor 11 after transfer. The cleaning means is preferably a cleaning blade having a urethane resin. A so-called cleanerless system may be used in which the deposits are removed by a developing means or the like without providing a separate cleaning means. The electrophotographic apparatus may have a charge removing mechanism for removing charge from the surface of the electrophotographic photoreceptor 11 by pre-exposure light 20 from a pre-exposure means (not shown). A guide means 22 such as a rail may be provided to make the process cartridge 21 according to one embodiment of the present disclosure detachable from the main body of the electrophotographic apparatus.
[0048] The electrophotographic photoreceptor according to one embodiment of the present disclosure can be used in laser beam printers, LED printers, copiers, facsimiles, and multifunction machines thereof. EXAMPLES
[0049] The process cartridge and electrophotographic apparatus according to the present disclosure will be described in more detail below using examples and comparative examples. Note that the present disclosure is not limited to the configuration embodied in the following examples. Note that in the following description of the examples, "parts" are based on mass unless otherwise specified.
[0050] <Production Example of Polyarylate A1> In a reaction vessel equipped with a stirrer, 100.00 parts by mass of the following structural formula (B-1) as a dihydric phenol component, 1.77 parts by mass of p-tert-butylphenol (PTBP) as an end-capping agent, 34.67 parts by mass of sodium hydroxide (NaOH) as an alkali, 1.04 parts by mass of a 50% aqueous solution of tri-n-butylbenzylammonium chloride (TBBAC) as a polymerization catalyst, and 0.50 parts by mass of sodium hydrosulfite as an antioxidant were charged and dissolved in 3300 parts by mass of water (aqueous phase). Separately, 121.79 parts by mass of the following structural formula (B-2) was dissolved in 2600 parts by mass of methylene chloride (organic phase). The molar ratios are as follows: Structural formula (B-1): PTBP: Structural formula (B-2): TBBAC:NaOH =100.00:2.86:100.00:0.68:210.00 (molar ratio). The aqueous phase was stirred in advance, and the organic phase was added to the aqueous phase under strong stirring, and polymerization was performed by interfacial polymerization at 15°C for 2 hours. After this, stirring was stopped, and the aqueous phase and the organic phase were separated by decantation. After removing the aqueous phase, 500 parts by mass of methylene chloride, 3000 parts by mass of pure water, and 10 parts by mass of acetic acid were added to stop the reaction, and the mixture was stirred at 15°C for 30 minutes. Then, the organic phase was washed 10 times with pure water, and the organic phase was added to methanol to precipitate the polymer. The precipitated polymer was filtered and then dried under vacuum at 150°C for 24 hours to obtain polyarylate A1. The viscosity average molecular weight of the obtained polyarylate A1 was 47,000. [ka] [ka]
[0051] <Production Example of Polyarylate A2> In a reaction vessel equipped with a stirrer, 50.00 parts by mass of the structural formula (B-1) as a dihydric phenol component, 50.00 parts by mass of the following structural formula (B-3), 1.77 parts by mass of p-tert-butylphenol (PTBP) as an end-capping agent, 34.67 parts by mass of sodium hydroxide (NaOH) as an alkali, 1.04 parts by mass of a 50% aqueous solution of tri-n-butylbenzylammonium chloride (TBBAC) as a polymerization catalyst, and 0.50 parts by mass of sodium hydrosulfite as an antioxidant were charged and dissolved in 3300 parts by mass of water (aqueous phase). In addition, 121.79 parts by mass of the above structural formula (B-2) was dissolved (organic phase). The molar ratios are as follows: Structural formula (B-1): Structural formula (B-3): PTBP: Structural formula (B-2): TBBAC:NaOH =50.00:50.00: 2.86:100.00:0.68:210.00 (molar ratio). The aqueous phase was stirred in advance, and the organic phase was added to the aqueous phase under strong stirring, and polymerization was performed by interfacial polymerization at 15°C for 2 hours. After this, stirring was stopped, and the aqueous phase and the organic phase were separated by decantation. After removing the aqueous phase, 500 parts by mass of methylene chloride, 3000 parts by mass of pure water, and 10 parts by mass of acetic acid were added to stop the reaction, and the mixture was stirred at 15°C for 30 minutes. Then, the organic phase was washed 10 times with pure water, and the organic phase was added to methanol to precipitate the polymer. The precipitated polymer was filtered and then dried under vacuum at 150°C for 24 hours to obtain polyarylate A2. The viscosity average molecular weight of the resulting polyarylate A2 was 48,000. [ka]
[0052] <Production Examples of Polyarylates A3 to A14> Polyarylate A2 was produced in the same manner as in Production Example 1, except that the structures (structural units contained in the structural units of the present invention) and ratios were changed to those in Table 2 in Production Example 1 of Polyarylate A2.
[0053] [Table 2]
[0054] <Production example of polycarbonate P1> 677.00g (2.52mol) of the following structural formula (B-4), 360.36g (1.68mol) of the following structural formula (B-5), 0.4g of triethylbenzylammonium chloride, and 5.0g of hydrosulfite were dissolved in 5.4L of 9.0w / w% aqueous sodium hydroxide (NaOH). 2.4L of methylene chloride was added thereto, and while stirring, 540g of phosgene was blown in for 30 minutes while maintaining the temperature at 15°C. After the blowing of phosgene was completed, 21g of pt-butylphenol was added, and the reaction liquid was emulsified by vigorously stirring. After the emulsification, 11ml of triethylamine was added, and the mixture was stirred at a temperature of 20 to 25°C for about 1 hour to polymerize. After the polymerization was completed, the reaction solution was separated into an aqueous phase and an organic phase, and the organic phase was neutralized with phosphoric acid. The organic phase was repeatedly washed with water until the conductivity of the washing water was 10 μS / cm or less. The obtained organic phase was dropped into hot water kept at 62°C, and the solvent was evaporated and removed to obtain a white powdery precipitate. The obtained precipitate was filtered and dried at a temperature of 120°C for 24 hours to obtain the target polycarbonate P1. The viscosity average molecular weight of the obtained polycarbonate was 41,000. [ka] [ka]
[0055] Measurement method for viscosity average molecular weight The resin to be measured is dissolved in dichloromethane to prepare a solution with a concentration of 6.00 g / L. The specific viscosity at 25°C is measured using an Ubbelohde viscometer. The limiting viscosity is calculated from this specific viscosity, and the viscosity average molecular weight is calculated by setting K (proportional constant part) and a (exponent part; sometimes written as α) of the Mark-Houwink viscosity formula to 1.23 x 10-4 and 0.83, respectively.
[0056] <Production examples of polycarbonates P2 to P12> Polycarbonate P1 was produced in the same manner as in Production Example 1 of Polycarbonate P1, except that the structural units and ratios were changed to those shown in Table 3 in Production Example 1 of Polycarbonate P1.
[0057] [Table 3]
[0058] Example 1 (Support) The support was a machined aluminum alloy cylinder having an outer diameter of 24 mm, a length of 257 mm and a wall thickness of 0.75 mm.
[0059] (Formation of Undercoat Layer) The dispersion for the undercoat layer was prepared as follows: Rutile-type titanium dioxide having an average primary particle size of 40 nm (Ishihara Sangyo Kaisha, Ltd., "TTO55N") and 3% by mass of methyldimethoxysilane (Toshiba Silicones, Inc., "TSL8117") based on the titanium dioxide were charged into a high-speed fluid mixer kneader (Kawata Corp., "SMG300") and mixed at high speed at a rotational speed of 34.5 m / sec to obtain a surface-treated titanium dioxide. The resulting surface-treated titanium dioxide was dispersed in a methanol / 1-propanol ball mill to obtain a dispersed slurry of hydrophobic treated titanium dioxide. The dispersion slurry, a mixed solvent of methanol / 1-propanol / toluene, and pellets of copolymerized polyamide having a composition molar ratio of ε-caprolactam [compound represented by the following formula (A)] / bis(4-amino-3-methylcyclohexyl)methane [compound represented by the following formula (B)] / hexamethylenediamine [compound represented by the following formula (C)] / decamethylenedicarboxylic acid [compound represented by the following formula (D)] / octadecamethylenedicarboxylic acid [compound represented by the following formula (E)] of 75% / 9.5% / 3% were heated and stirred while mixing to dissolve the polyamide pellets, and then ultrasonic dispersion treatment was performed to obtain a dispersion for undercoat layer having a solid concentration of 18.0%, containing methanol / 1-propanol / toluene in a mass ratio of 7 / 1 / 2 and hydrophobic treated titanium oxide / copolymerized polyamide in a mass ratio of 3 / 1. The support was dip-coated with this undercoat layer coating solution to form a coating film, which was then dried at 100° C. for 10 minutes to form a 2.00 μm undercoat layer. [ka]
[0060] (Formation of Charge Generation Layer) As a charge generating substance, 10 parts of Y-type oxytitanium phthalocyanine crystals having a strong peak at 27.3° of the Bragg angle (2θ±0.2°) in CuKα characteristic X-ray diffraction and 150 parts of 4-methoxy-4-methylpentanone-2 were placed in a sand mill using glass beads with a diameter of 1 mm, and were ground and dispersed using the sand grinding mill for 1.5 hours. Next, 105 parts of a solution in which 5 parts of polyacetal resin (product name: S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.) had been dissolved in 100 parts of 4-methoxy-4-methylpentanone-2 was added, and the mixture was dispersed for 0.5 hours. Then, 250 parts of 1,2-dimethoxyethane was added to prepare a coating solution for the charge generation layer. The coating solution for the charge generation layer was dip-coated onto the obtained undercoat layer to form a coating film, and the coating film was dried at 100° C. for 10 minutes to form a 0.15 μm charge generation layer.
[0061] The X-ray diffraction measurements were carried out under the following conditions. [Powder X-ray diffraction measurement] Measuring equipment used: Rigaku Electric Co., Ltd., X-ray diffraction device RINT-TTRII X-ray tube:Cu Tube voltage: 50KV Tube current: 300mA Scan method: 2θ / θ scan Scan speed: 4.0° / min Sampling interval: 0.02° Start angle (2θ): 5.0° Stop angle (2θ): 40.0° Attachment: Standard sample holder Filter: Not used Incident Monochromator: Used Counter monochromator: Not used Divergence slit: open Divergence vertical limit slit: 10.00mm Scattering slit: open Receiving slit: open Flat plate monochromator: Used Counter: Scintillation counter
[0062] (Formation of charge transport layer) Next, 6 parts of the charge transport material represented by CTM1, 7 parts of the polyarylate represented by A1, and 3 parts of the polycarbonate represented by P1 were dissolved in a mixed solvent of 23 parts of orthoxylene, 23 parts of methyl benzoate, and 23 parts of dimethoxymethane to prepare a coating solution for the charge transport layer. This coating solution for the charge transport layer was dip-coated onto the charge generating layer to form a coating film, which was then dried at 125°C for 30 minutes to form a charge transport layer having a thickness of 24 μm. The results of pyrolysis GCMS of the resin in the surface layer of the obtained photoreceptor showed that the TIC had an MS spectrum in which components of m / z=242 and m / z=227 were detected. 1 Since the H-NMR spectrum had a peak at 2.4 ppm, it was identified as containing the formula (2-1).
[0063] The electrophotographic device used was a modified version of a laser beam printer manufactured by Hewlett-Packard, product name HPColor LaserJet Enterprise M653dn. First, the electrophotographic device and the prepared electrophotographic photosensitive member were left to stand for 24 hours or more in an environment of a temperature of 15° C. and a humidity of 10% RH, and then the electrophotographic device was fitted to a cyan cartridge and inserted into the main body. After that, 100 halftone images were printed, the cartridge was removed, and only deep scratches that could be visually recognized were counted for the scratches present on the photoreceptor. Furthermore, the maximum valley depth Rv of each of the counted scratches was measured, and the maximum values are shown in Table 5. After that, 40,000 sheets were printed with a horizontal line image with a density of 1.5% per sheet, the cartridge was removed, and only deep scratches that could be visually recognized were counted for scratches present on the photoreceptor. Furthermore, Rv was measured for the counted scratches, and the maximum value is shown in Table 5. Note that when Rv exceeds 1.0 μm, there is a tendency for image defects to occur. The results are shown in Table 5. The Rv measurement was carried out under the following conditions. Company name: Kosaka Laboratory Co., Ltd. Roughness meter name: SE3500 Cutoff value: 0.08mm Spare length: cut off x 1 Filter characteristic: 2CR Evaluation length: 2.5mm Vertical magnification: 10000 Horizontal magnification: 50 Feed length: 0.1mm / sec Leveling: Straight line (all areas) JIS B0601-1982 Processing from the entire evaluation length: Interval evaluation length 8000 equal parts λs filter: None Polarity: normal
[0064] [Examples 2 to 73, Comparative Examples 1 to 11] A photoreceptor was prepared in the same manner as in Example 1, except that the polyarylate type, polycarbonate type, CTM type, binder ratio, and CTM / binder ratio were used as shown in Table 4. The results are shown in Table 5.
[0065] Example 74 7 parts of polyarylate represented by A1 and 3 parts of polycarbonate represented by P1 were dissolved in a mixed solvent of 23 parts of orthoxylene / 23 parts of methyl benzoate, and then 1 part of silica fine particles QSG-170 (manufactured by Shin-Etsu Chemical Co., Ltd., volume average particle size 170 nm) was added, followed by dispersion using a microfluidizer (Powrex Corporation, M110-P). Thereafter, 8 parts of a charge transport material represented by CTM3 and 23 parts of dimethoxymethane were added to the above dispersion and dissolved to prepare a coating solution for the charge transport layer. The coating solution for the charge transport layer was dip-coated on the charge generating layer to form a coating film, which was then dried at 125°C for 30 minutes to form a charge transport layer with a thickness of 18 μm. The results are shown in Table 5.
[0066] Example 75 A photoreceptor was prepared in the same manner as in Example 74, except that the polycarbonate and fine particles shown in Table 4 were changed to silica fine particles KE-S10 (volume average particle size 0.1 μm, manufactured by Nippon Shokubai Co., Ltd.). The results are shown in Table 5.
[0067] Example 76 A photoreceptor was prepared in the same manner as in Example 74, except that the polycarbonate and fine particles shown in Table 4 were changed to silica fine particles KE-S30 (volume average particle size 0.3 μm, manufactured by Nippon Shokubai Co., Ltd.). The results are shown in Table 5.
[0068] Example 77 A photoreceptor was prepared in the same manner as in Example 74, except that the polycarbonate and fine particles shown in Table 4 were changed to silica fine particles KE-P50 (volume average particle size 0.5 μm, manufactured by Nippon Shokubai Co., Ltd.). The results are shown in Table 5.
[0069] Example 78 A photoreceptor was prepared in the same manner as in Example 74, except that the polycarbonate and the fine particles shown in Table 4 were changed to silica fine particles 43-00-701 (volume average particle size 0.07 μm, Corefront Co., Ltd.). The results are shown in Table 5.
[0070] Example 79 A photoreceptor was prepared in the same manner as in Example 74, except that the polycarbonate and fine particles shown in Table 4 were changed to silica fine particles SO-C4 (Admatechs Korea Co., Ltd., volume average particle size 0.9 to 1.2 μm) in Example 74. The results are shown in Table 5.
[0071] Example 80 A photoreceptor was prepared in the same manner as in Example 74, except that the polycarbonate and fine particles shown in Table 4 were changed to alumina fine particles AKP-53 (Sumitomo Chemical Co., Ltd., volume average particle size 0.17 μm). The results are shown in Table 5.
[0072] Example 81 A photoreceptor was prepared in the same manner as in Example 74, except that the polycarbonate and fine particles shown in Table 4 were changed to silica fine particles SO-C1 (Admatechs Korea Co., Ltd., volume average particle size 0.2 to 0.4 μm) in Example 74. The results are shown in Table 5.
[0073] Example 82 A photoreceptor was prepared in the same manner as in Example 74, except that the polycarbonate and fine particles shown in Table 4 were changed to silica fine particles QCB-100 (Shin-Etsu Chemical Co., Ltd., volume average particle size 0.2 μm). The results are shown in Table 5.
[0074] [Table 4]
[0075] [Table 5]
[0076] The disclosure of this embodiment includes the following configuration. [Configuration 1] An electrophotographic photoreceptor having a surface layer containing polyarylate and polycarbonate, The polyarylate has at least one structural unit selected from the group consisting of a structural unit represented by the following formula (1-1), a structural unit represented by the following formula (1-2), and a structural unit represented by the following formula (1-3), The polycarbonate has a structural unit represented by the following formula (2-1): 1. An electrophotographic photoreceptor comprising: [ka] [ka] [ka] [ka] [Configuration 2] The electrophotographic photoreceptor according to Constitution 1, wherein the surface layer contains the structural unit represented by formula (2-1) in an amount of 5 mol % to 40 mol %. [Configuration 3] 3. The electrophotographic photoreceptor according to embodiment 1 or 2, wherein the polycarbonate contains 20 mol % or more and 60 mol % or less of the structural unit represented by the formula (2-1). [Configuration 4] An electrophotographic photoreceptor having a surface layer containing polyarylate and polycarbonate, In the component analysis of the polymer component recovered from the surface layer, The polyarylate is In pyrolysis gas chromatography mass spectrometry in the presence of TMAH, the TIC has a peak having an MS spectrum in which components of m / z = 242 and m / z = 227 are detected, Deuterated chloroform was used 1 In the H-NMR spectrum, it has peaks at 2.40±0.02 ppm and 2.35±0.02 ppm. The polycarbonate is In pyrolysis gas chromatography mass spectrometry in the presence of TMAH, the TIC has a peak having an MS spectrum in which components of m / z = 242 and m / z = 227 are detected, Deuterated chloroform was used 1 1. An electrophotographic photoreceptor having a peak at 2.40±0.02 ppm in a H-NMR spectrum. [Configuration 5] 5. The electrophotographic photoreceptor according to any one of Configurations 1 to 4, wherein the surface layer contains silica fine particles. [Configuration 6] 6. The electrophotographic photoreceptor according to Configuration 5, wherein the silica fine particles have a volume average particle size of 0.1 μm or more and 0.5 μm or less. [Configuration 7] A process cartridge integrally supporting the electrophotographic photosensitive member according to any one of configurations 1 to 6 and at least one means selected from the group consisting of a charging means, a developing means and a cleaning means, and being detachably mountable to a main body of an electrophotographic apparatus. [Configuration 8] An electrophotographic apparatus comprising the electrophotographic photoreceptor according to any one of Configurations 1 to 6, a charging unit, an exposing unit, a developing unit and a transferring unit. [Explanation of symbols]
[0077] 101:Support 102: Undercoat layer 103: Charge generating layer 104: Charge transport layer (surface layer) 11: Electrophotographic photoreceptor 12: Axis 13: Charging means 14: Image exposure light 15: Developing method 16: Transcription method 17: Transfer material 18: Fixing method 19: Cleaning means 20: Pre-exposure light 21: Process cartridge 22: Guidance means
Claims
1. An electrophotographic photoreceptor having a surface layer containing polyarylate and polycarbonate, The polyarylate has at least one structural unit selected from the group consisting of a structural unit represented by the following formula (1-1), a structural unit represented by the following formula (1-2), and a structural unit represented by the following formula (1-3), The polycarbonate has a structural unit represented by the following formula (2-1):
1. An electrophotographic photoreceptor comprising: 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】
2. 2. The electrophotographic photoreceptor according to claim 1, wherein the surface layer contains the structural unit represented by the formula (2-1) in an amount of 5 mol % to 40 mol %.
3. 2. The electrophotographic photoreceptor according to claim 1, wherein the polycarbonate contains the structural unit represented by the formula (2-1) in an amount of 20 mol % or more and 60 mol % or less.
4. An electrophotographic photoreceptor having a surface layer containing polyarylate and polycarbonate, In the component analysis of the polymer component recovered from the surface layer, The polyarylate is In pyrolysis gas chromatography mass spectrometry in the presence of TMAH, the TIC has a peak having an MS spectrum in which components of m / z = 242 and m / z = 227 are detected; Deuterated chloroform was used 1 In the H-NMR spectrum, it has peaks at 2.40±0.02 ppm and 2.35±0.02 ppm. The polycarbonate is In pyrolysis gas chromatography mass spectrometry in the presence of TMAH, the TIC has a peak having an MS spectrum in which components of m / z = 242 and m / z = 227 are detected; Deuterated chloroform was used 1 The electrophotographic photoreceptor has a peak at 2.40±0.02 ppm in a H-NMR spectrum.
5. The electrophotographic photoreceptor according to claim 1 , wherein the surface layer contains fine silica particles.
6. 6. The electrophotographic photoreceptor according to claim 5, wherein the silica fine particles have a volume average particle size of 0.1 [mu]m or more and 0.5 [mu]m or less.
7. 7. A process cartridge which integrally supports the electrophotographic photosensitive member according to claim 1 and at least one means selected from the group consisting of a charging means, a developing means and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus.
8. 7. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to claim 1, a charging means, an exposing means, a developing means and a transferring means.
Citation Information
Patent Citations
JP04862663B
Electrophotographic photoreceptor, image-forming device using the same and cartridge
JP2007122036A
Electrophotographic photoreceptor and image forming apparatus
JP2014095867A
Electrophotographic photoreceptor, manufacturing method for the same, process cartridge and electrophotographic device
JP2016164651A
Electrophotographic photoreceptor, manufacturing method for the same, process cartridge and electrophotographic device
JP2016164652A