Element mounting board and method for manufacturing element mounting board

The heat sink design with optimized flatness and curvature on both sides of a metal-silicon carbide composite, integrated with a ceramic plate, addresses thermal expansion issues, enhancing bonding and heat dissipation in power modules.

JP7596363B2Active Publication Date: 2024-12-09DENKA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022511755
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-31
Filing Date
2021-03-11
Publication Date
2024-12-09
Estimated Expiration
2041-03-11

AI Technical Summary

Technical Problem

Existing heat sinks with optimized curvature for integration with other components fail to achieve optimal heat dissipation performance due to variations in thermal expansion and bending caused by mounted electronic elements, particularly in power modules.

Method used

A heat sink design with metal layers containing aluminum or magnesium on both sides of a flat metal-silicon carbide composite, featuring a flatness of 600 μm or less on one surface and a convex curvature on the opposite surface, integrated with a ceramic plate electronic element, to enhance bonding and heat dissipation.

Benefits of technology

The design improves heat dissipation performance by ensuring optimal flatness and curvature, reducing thermal stress and enhancing bonding strength, resulting in efficient heat transfer and improved reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596363000003
    Figure 0007596363000003
  • Figure 0007596363000004
    Figure 0007596363000004
  • Figure 0007596363000005
    Figure 0007596363000005
Patent Text Reader

Abstract

This element-mounted substrate is provided with a heat-dissipating plate (1) having a metal layer containing aluminum or magnesium formed on the front and rear surfaces of a flat plate-shaped metal-silicon carbide complex containing aluminum or magnesium; and an electronic element (11) that is mounted on one surface (main surface 3A) of the heat-dissipating plate 1 and that includes a ceramic plate (12), wherein the flatness of the other surface (main surface 3B) of the heat-dissipating plate 1 is 600 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a device mounting board and a method for manufacturing the device mounting board, and more particularly to a device mounting board in which electronic devices including a ceramic plate are mounted on at least one surface of a specific heat sink. [Background technology]

[0002] In recent years, heat sinks made of metal-silicon carbide composites have come to be used as heat dissipation components for power modules in electric vehicles and electric railways, replacing the conventional copper. The metal in metal-silicon carbide composites is often aluminum or its alloys.

[0003] A heat sink is usually used such that electronic elements, including power semiconductor elements, are mounted on one side of the heat sink, and the other side of the heat sink is often joined to other heat dissipation components, such as heat dissipation fins or a heat dissipation unit, in order to improve the dissipation of heat generated by the electronic elements.

[0004] In order to obtain sufficient heat dissipation performance, it is important that the heat sink is joined to other heat dissipation components with as few gaps as possible. For this reason, the properties of the other side of the heat sink (the side opposite to the side on which the electronic elements are mounted) are important. For example, when joining a heat sink to another heat dissipation component, the heat sink is generally fixed to the other heat dissipation component with screws using holes provided on the periphery of the heat sink. However, if the "other surface" of the heat sink is concave or has many small irregularities, a gap will be created between the heat sink and the other heat dissipation component, reducing thermal conductivity.

[0005] In order to avoid the above problems, a heat sink has been proposed in which the surface that joins with other heat sink components is slightly convexly curved so as to minimize the gap between the heat sink and other heat sink components. This is because, as mentioned above, heat sinks are typically used by fixing them to other heat dissipation components with fixing members such as screws, and because the mating surface with other heat dissipation components is convexly curved, when fixed with a fixing member the mating surface becomes "suitably flat," improving the adhesion (bonding) with other heat dissipation components.

[0006] As an example, Patent Document 1 describes a silicon carbide composite plate formed by impregnating a porous silicon carbide molded body with a metal whose main component is aluminum, the plate composite having four or more holes within its surface for screwing the convex surface of the plate composite to another heat dissipation component, the silicon carbide composite being characterized in that the relationship between the amount of warping (Cx; μm) per 10 cm in the direction between the holes (X direction) and the amount of warping (Cy; μm) per 10 cm in the direction perpendicular thereto (Y direction) is 50≦Cx≦250 and −50≦Cy≦200 (excluding Cy=0).

[0007] As another example, Patent Document 2 describes a plate-shaped composite body made by impregnating a porous silicon carbide molded body with a metal whose main component is aluminum, and which has a warpage of 250 μm or less per 10 cm length of the main surface of the composite. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 3468358 [Patent Document 2] International Publication No. 2015 / 115649 Summary of the Invention [Problem to be solved by the invention]

[0009] As described above, it is known that (1) first, a slightly curved heat sink is manufactured, and then (2) when it is joined to other heat dissipation components, the curve is "flattened" by the force of fixing members such as screws, thereby improving the adhesion between the heat sink and other heat dissipation components and thereby improving heat dissipation.

[0010] However, the curved heat sinks described in Patent Documents 1, 2 and the like have a specific amount of curvature for the heat sink alone. As described above, a heat sink usually has electronic elements mounted on one side and other heat dissipation components attached to the other side. When a heat sink is used in this manner, even if the degree of curvature of the heat sink alone is optimized, the degree of curvature may not be optimal when the heat sink is actually mounted on an electronic device (due to the influence of the electronic elements mounted thereon).

[0011] In addition, the electronic element (typically a power element) mounted on one side of the heat sink usually contains a ceramic material such as a ceramic plate, and due to the difference in the thermal expansion coefficient between the ceramic material and the heat sink, unintended curvature or undesirable stress may occur.

[0012] In recent years, there has been a demand for further improvements in heat dissipation in power modules. Therefore, in order to achieve optimal heat dissipation performance, it is considered to consider ways to improve heat dissipation by integrating electronic elements, heat sinks, and other heat dissipation components. However, as described above, past studies have been limited to optimizing the amount of curvature of the heat sink alone. As far as the inventors know, there has been insufficient research into improving heat dissipation performance by integrating the electronic element, the heat sink, and other heat dissipation members.

[0013] In light of the above circumstances, the present inventors have conducted research aimed at obtaining an electronic device with good heat dissipation properties, not from the perspective of the heat sink alone, but from the perspective of the entire assembly including the electronic elements etc. mounted on the heat sink. [Means for solving the problem]

[0014] As a result of extensive investigations, the present inventors have completed the invention provided below and have solved the above-mentioned problems.

[0015] According to the present invention, A heat sink having aluminum or magnesium-containing metal layers formed on both sides of a flat metal-silicon carbide composite containing aluminum or magnesium; and an electronic element including a ceramic plate mounted on one surface side of the heat sink. The element mounting board is provided such that the flatness of the other surface of the heat sink is 600 μm or less. According to the present invention, there is also provided a method for manufacturing the above-mentioned device mounting board, comprising the steps of: A preparation step of preparing a heat sink having aluminum or magnesium-containing metal layers formed on both sides of a flat plate-shaped metal-silicon carbide composite containing aluminum or magnesium; a flatness adjusting step of adjusting the flatness of at least one surface of the heat sink; a mounting step of mounting an electronic element including a ceramic plate on a surface of the heat sink opposite to the one surface; The present invention provides a method for manufacturing a device mounting board, comprising the steps of: Effect of the Invention

[0016] According to the present invention, a device mounting board (electronic device) having good heat dissipation properties can be obtained. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a schematic diagram (cross-sectional view) showing an example of a device mounting board. [Diagram 2] 10 is a diagram for explaining the shape of a main surface 3B. FIG. [Diagram 3] FIG. 13 is a diagram for explaining "hot pressing" in the manufacturing process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In all drawings, similar components are given similar symbols and descriptions thereof are omitted where appropriate. In order to avoid complexity, (i) when there are multiple identical components in the same drawing, only one of them is given a reference symbol and not all of them, or (ii) especially in Figure 2 and subsequent figures, components similar to those in Figure 1 are not given a reference symbol again. All drawings are for illustrative purposes only. The shapes and dimensional ratios of each component in the drawings do not necessarily correspond to the actual objects. In particular, the shapes and dimensional ratios may be exaggerated for ease of explanation. In particular, the magnitude of "curvature" in each drawing is exaggerated compared to the actual objects.

[0019] Unless otherwise specified, the term "approximately" used in this specification means that a range taking into consideration manufacturing tolerances, assembly variations, and the like, is included unless otherwise specified. Unless otherwise specified, for various numerical values ​​(especially measured values) in this specification that may change depending on temperature, values ​​at room temperature (25° C.) can be used.

[0020] <Device mounting board> FIG. 1 is a schematic diagram (cross-sectional view) showing an example of a device mounting board according to this embodiment. The device mounting board in FIG. 1 comprises a heat sink 1 and an electronic device 11 mounted on one surface of the heat sink 1.

[0021] The heat sink 1 is a flat plate-shaped metal-silicon carbide composite 2 (hereinafter also referred to as composite 2) containing aluminum or magnesium, with an aluminum or magnesium-containing metal layer 3 (hereinafter also referred to as metal layer 3) formed on both the front and back sides. Of the two main surfaces of the heat sink 1, the surface on which the electronic element 11 is mounted is referred to as main surface 3A, and the other surface is referred to as main surface 3B.

[0022] For example, the heat sink 1 has a plurality of through holes 5 on its periphery. More specifically, when the heat sink 1 is substantially rectangular as described below, it is preferable that the through holes 5 are provided in at least the four corners of the heat sink 1. The through holes 5 are used when joining the heat sink 1 to another heat dissipating part (such as a heat dissipating fin) with a screw or the like.

[0023] The electronic element 11 includes at least a ceramic plate 12. In Fig. 1, the electronic element 11 has a structure in which the ceramic plate 12 is sandwiched between two metal layers 13. The electronic element 11 is mounted on the main surface 3A of the heat sink 1, for example, by soldering with solder 14. When the electronic element 11 is viewed from above with the main surface 3A of the heat sink 1 facing upward, 10 to 80% of the area of ​​the heat sink 1 is covered by the electronic element 11.

[0024] In the device mounting board of FIG. 1, the flatness of the main surface 3B (that is, the surface opposite to the surface on which the electronic device 11 is mounted) is 50 to 600 μm, preferably 100 to 500 μm, and more preferably 150 to 450 μm. When electronic elements 11 are mounted on the heat sink 1 alone, it is believed that the flatness of the main surface 3B within the above range results in good heat dissipation performance for the element mounting board and other heat dissipation components as a whole. In other words, when electronic elements 11 are mounted on heat sink 1 to form an element mounting board, if the flatness of main surface 3B is an appropriate value, then when the element mounting board is joined to another heat dissipation component, the bonding between main surface 3B and the other heat dissipation component will be good, and excellent heat dissipation performance will be obtained.

[0025] The flatness is defined as the distance between two parallel planes when a planar object is sandwiched between the two parallel planes and the distance between the two parallel planes is at a minimum (see JIS B 0621). An example of a flatness measuring device is the VR-3000 device manufactured by Keyence Corporation.

[0026] The preferred embodiment of the device mounting board of this embodiment will now be described.

[0027] [Characteristics of heat sink 1] It is preferable that the main surface 3B (the surface of the heat sink 1 opposite to the surface on which the electronic element 11 is mounted) be curved convexly in the direction opposite to the main surface 3A. This makes it easier to make the bonding surface "flat" when the heat sink 1 is fixed to another heat sink member (such as a heat sink fin) with a fixing member such as a screw, and further improves the bonding (adhesion) between the heat sink 1 and the heat sink fin, etc.

[0028] The heat sink 1 is preferably substantially rectangular in shape. That is, when the heat sink 1 is viewed from above with one of its main surfaces as the upper surface, the shape of the heat sink 1 is substantially rectangular. Here, "substantially rectangular" means that at least one of the four corners of the heat sink 1 may be processed to have a rounded shape rather than a right angle (of course, the four corners may also be right angled). If at least one of the four corners of the heat sink 1 is processed into a rounded shape, the point where the straight lines of the short side and long side intersect when extended when the heat sink 1 is viewed from above can be defined as the "vertex" of the rectangle. In this case, the "length of the short side" and the "length of the long side" of the heat sink 1 can be defined with the above-mentioned "vertex" as the start point or end point.

[0029] When the heat sink 1 is substantially rectangular, the length and width of the heat sink 1 are, for example, approximately 40 mm×90 mm to 250 mm×140 mm. The thickness of the heat sink 1 is, for example, 2 mm to 6 mm, preferably 3 mm to 5 mm. If the thickness of the heat sink 1 is not uniform, it is preferable that at least the thickness at the center of gravity of the heat sink 1 is within the above range. The thickness of the metal layer 3 is, for example, about 50 to 300 μm including the top and bottom.

[0030] In addition to the flatness of the main surface 3B as a whole being within the above-mentioned numerical range, by designing the curvature of the main surface 3B more precisely, the heat dissipation performance can be further improved. Regarding this, consider the case where heat sink 1 is substantially rectangular, the long side of the rectangle has a length a, the short side has a length b, and main surface 3B is curved convexly in the direction opposite to main surface 3A.

[0031] 2(a) is a diagram for explaining the form of the main surface 3B, in other words, a diagram clearly showing only the main surface 3B of the heat sink 1 in the device mounting board of the present embodiment. 2(b) is a cross-sectional view of the main surface 3B taken along the cross section β in FIG. 2(a), and FIG. 2(c) is a cross-sectional view of the main surface 3B taken along the cross section γ in FIG. 2(a). In these drawings, auxiliary lines and the like are included for the purpose of explanation.

[0032] Here, the straight line connecting the midpoints of the two short sides of main surface 3B (indicated by M1 and M3 in the figure) is defined as l1, and the straight line connecting the midpoints of the two long sides of main surface 3B (indicated by M2 and M4 in the figure) is defined as l2.

[0033] When the main surface 3B is cut at a cross section β that includes l1 and is substantially perpendicular to the main surface 3B, the maximum distance between l1 and any point on the curve formed by the main surface 3B in the cross section is defined as h1. When the main surface 3B is cut at a cross section γ that includes l2 and is substantially perpendicular to the main surface 3B, the maximum distance between l2 and any point on the curve formed by the main surface 3B in the cross section is defined as h2.

[0034] In this case, it is preferable to design the device mounting board so that h1 / a>h2 / b. More specifically, the value of (h1 / a) / (h2 / b) is preferably 1.0 or more and 1.9 or less, and more preferably 1.07 or more and 1.6 or less.

[0035] The above inequality can be interpreted as follows. It can be said that h1 / a means the "curvature per unit length in the long side direction" of the heat sink 1. Similarly, h2 / b can be said to mean the "curvature per unit length in the short side direction" of the heat sink 1. In this case, "h1 / a>h2 / b" can be interpreted as meaning that, even if we take into account the fact that the long side is longer than the short side, the "degree of curvature" in the long side direction is greater than that in the short side direction.

[0036] When the heat sink 1 on which the electronic element 11 is mounted is pressed against and joined to another component using a screw or the like, the rectangular (oblong) heat sink 1 is more likely to deform (bend) in the long side direction than in the short side direction. Therefore, by making the "degree of curvature" in the long side direction greater than that in the short side direction, the heat sink 1 can be joined more snugly to another heat dissipating component, which is believed to result in further improvements in heat dissipation and reliability.

[0037] The arithmetic mean roughness Ra (hereinafter also referred to as "surface roughness Ra") of the portion of the main surface 3A of the heat sink 1 on which the electronic elements 11 are not mounted (the portion where the main surface 3A is exposed) is preferably 0.2 to 2.0 μm, and more preferably 0.5 to 1.6 μm. As described above, the electronic element 11 is mounted on the heat sink 1 by, for example, soldering with the solder 14. It is believed that an appropriate value for the surface roughness Ra enhances the wettability of the solder, thereby increasing the bonding strength between the heat sink 1 and the electronic element 11. In addition, although the details are unclear, it is believed that an appropriate roughness (surface roughness Ra) of the main surface 3A creates a kind of "play" between the heat sink 1 and the electronic element 11. This is thought to prevent deterioration of the bond even if there is external force, heat cycles, or distortion when connecting the element mounting board to other heat dissipation components.

[0038] Although not shown in Fig. 1, a plating layer may be present on the outermost surface of the heat sink 1. This can, for example, further improve the bond with the electronic element 11 (specifically, make it easier to solder to the electronic element 11). The plating layer can be, for example, Ni plating. The thickness of the plating layer can be about 10 µm per layer, and about 20 µm in total for the top and bottom.

[0039] [Characteristics of Electronic Element 11] The electronic element 11 can be, for example, a power semiconductor element. A large amount of heat can be released from the electronic element 11, which is a power semiconductor element, but the heat can be efficiently released by appropriately joining the element mounting board of this embodiment to another heat dissipation member (such as a heat dissipation fin).

[0040] As described above, the electronic element 11 includes at least the ceramic plate 12. The electronic element 11 also typically includes a metal layer 13.

[0041] The material of the ceramic plate 12 is not particularly limited as long as it is a ceramic material. For example, it may be a nitride ceramic such as silicon nitride or aluminum nitride, an oxide ceramic such as aluminum oxide or zirconium oxide, a carbide ceramic such as silicon carbide, a boride ceramic such as lanthanum boride, etc. Among them, aluminum nitride, silicon nitride, and aluminum oxide are preferable from the viewpoints of insulation, strength of bonding with the metal layer 13, mechanical strength, etc.

[0042] The metal layer 13 is preferably made of copper, a copper alloy, aluminum, or an aluminum alloy from the viewpoints of electrical conductivity and thermal conductivity, etc. For example, it can be made of pure copper (C1020 material or C1011 material), an oxygen-free copper plate, etc. A portion of the metal layer 13 may be removed by etching or the like to form a circuit pattern.

[0043] The three-layer structure of the electronic element 11, metal layer 13-ceramic plate 12-metal layer 13, can be obtained, for example, by joining a ceramic plate and a metal plate with an appropriate brazing material.

[0044] The brazing material is preferably an Ag-Cu brazing material. That is, the brazing material is preferably a mixture of Ag powder, Cu powder, etc. From the viewpoint of making the melting temperature appropriate, it is preferable that the Ag powder is 75 parts by mass or more and 98 parts by mass or less, and the Cu powder is 2 parts by mass or more and 25 parts by mass or less, when the total amount of the Ag powder and the Cu powder is 100 parts by mass.

[0045] The brazing material may contain Sn or In for the purpose of improving wettability with the ceramic plate, etc. The blending amount of these elements is preferably 0.4 parts by mass or more and 3.5 parts by mass or less.

[0046] The brazing material preferably contains an active metal from the viewpoint of increasing the reactivity with the ceramic plate, etc. Examples of the active metal include titanium, zirconium, hafnium, niobium, etc. From the viewpoint of high reactivity with aluminum nitride substrates and silicon nitride substrates and extremely high bonding strength, it is preferable that the brazing material contains titanium. The amount of the active metal added is preferably 1.5 parts by mass or more and 5.0 parts by mass or less per 100 parts by mass of the total of the Ag powder, the Cu powder, and the Sn powder or the In powder. By appropriately adjusting the amount of the active metal added, the occurrence of poor bonding can be further suppressed.

[0047] The brazing material can be obtained by mixing the above-mentioned metal powder with an organic solvent or binder as necessary. For mixing, a grinding machine, a planetary mixer, a three-roll mill, etc. can be used. This makes it possible to obtain, for example, a paste-like brazing material. The organic solvent that can be used here is not particularly limited, and examples thereof include methyl cellosolve, ethyl cellosolve, isophorone, toluene, ethyl acetate, terpineol, diethylene glycol monobutyl ether, and texanol. The binder that can be used here is not particularly limited, and examples thereof include polymer compounds such as polyisobutyl methacrylate, ethyl cellulose, methyl cellulose, acrylic resin, and methacrylic resin.

[0048] The electronic device 11 can be obtained, for example, as follows. (1) Brazing paste is applied to both sides of a ceramic plate, and a copper plate is placed in contact with the applied surface. (2) The ceramic plate and the copper plate are joined by heat treatment in a vacuum or inert atmosphere.

[0049] The method for applying the brazing paste to the ceramic plate in the above (1) is not particularly limited. For example, a roll coater method, a screen printing method, a transfer method, etc. are included. The screen printing method is preferred because it is easy to apply uniformly. The bonding of the ceramic plate and the copper plate in (2) above is preferably performed in a vacuum or in an inert atmosphere of nitrogen, argon, or the like at a temperature of, for example, 770° C. to 830° C. for 10 to 60 minutes.

[0050] [Relationship between heat sink 1 and electronic element 11, and design of entire element mounting board] As described above, the design concept of the device mounting board of this embodiment is to improve heat dissipation not by the heat sink 1 alone but by treating the heat sink 1 and the electronic device 11 as a single body.

[0051] In this regard, for example, when the thermal expansion coefficient of the heat sink 1 at a temperature of 25 to 400° C. is α1 and the thermal expansion coefficient of the ceramic plate 12 at a temperature of 25 to 400° C. is α2, the difference between α1 and α2 is 5.0 ppm K. -1 The result is as follows.

[0052] From another perspective, when the device mounting board is viewed from above with the main surface 3A of the heat sink 1 as the upper surface, preferably 10 to 80%, and more preferably 15 to 70%, of the area of ​​the heat sink 1 is covered with the electronic device 11. When electronic elements 11 having the above-mentioned area ratio are mounted on main surface 3A, by setting the flatness of main surface 3B to 50 to 600 μm and appropriately designing the values ​​of h1 / a, h2 / b, etc., it is possible to sufficiently minimize the occurrence of unintended distortion and thermal stress while improving heat dissipation.

[0053] [Solder] The type of solder 14 is not particularly limited, but for example, lead-tin eutectic solder or lead-free solder can be used. The thickness of the solder coating can be, for example, 0.1 to 0.2 mm. The reflow conditions are not particularly limited and may be set appropriately depending on the melting temperature of the solder 14, but typically can be about 250 to 350°C for 5 to 30 minutes. By ensuring that the temperature is not too high / time is not too long, unintended changes in flatness can be suppressed.

[0054] [Method of manufacturing element mounting board] The device mounting board of this embodiment can be manufactured, for example, as follows. (1) Preparation of heat sink: A heat sink is prepared by forming an aluminum or magnesium-containing metal layer on both sides of a flat metal-silicon carbide composite containing aluminum or magnesium. (2) Flatness adjustment: The flatness of at least one surface of the heat sink prepared in (1) is adjusted. Preferably, at least one surface of the heat sink prepared is provided with a convex curve in the direction opposite to the one surface. (3) Bonding: The heat sink whose flatness has been adjusted in the above (2) is bonded to a separately prepared electronic element by soldering or the like.

[0055] The above procedure will now be described in more detail.

[0056] (1) Preparation of heat sink: For example, by carrying out the steps of (i) forming silicon carbide powder into a flat plate and sintering it to obtain a flat plate-shaped molded body (preform), and (ii) impregnating the molded body (preform) with a metal, a heat sink having a metal layer on both the front and back sides of a flat metal-silicon carbide composite can be obtained.

[0057] In the above step (i), first, silicon carbide powder as a raw material (preferably one or more types of silicon carbide particles having an average particle size of 1 to 300 μm) is formed into a tabular shape by an appropriate method. The method for forming the sheet can be appropriately selected from known methods, such as dry pressing, wet pressing, extrusion molding, injection molding, casting, and sheet molding followed by punching.

[0058] When forming the silicon carbide powder into a plate shape, an inorganic or organic binder may be added as appropriate to provide strength that will prevent abnormalities such as cracks during metal impregnation. Silica sol is preferred as the binder because it is easy to obtain a high-strength molded body. The binder is preferably added in a volume ratio of 20 or less per 100 silicon carbide solids for the reason of improving the relative density.

[0059] The flat plate obtained above is usually dried and heated for degreasing, and then sintered, although this varies depending on the manufacturing conditions. This makes it possible to obtain a molded body (also called a preform) with sufficient strength. The firing conditions are preferably in an inert atmosphere or in air at a temperature of 700° C. or higher. However, if firing is performed in air at a temperature of 1100° C. or higher, silicon carbide may be oxidized and the thermal conductivity of the resulting composite may decrease. Therefore, firing at a temperature below this temperature is preferable.

[0060] The relative density of the preform obtained by firing is preferably 55 to 75%. By setting the relative density of the preform to 55 to 75%, it is easy to design the thermal expansion coefficient of the heat sink 1 to about 6 to 10 ppm / K. The relative density is defined as the volume ratio of silicon carbide to the volume of a silicon carbide molded body (preform) having voids before being impregnated with metal. In order to make the relative density of the preform 55 to 75%, it is preferable to mix silicon carbide powders with different particle sizes in the stage of obtaining a flat plate before firing. In the case of silicon carbide, examples include the use of a powder mixed with a powder having an average particle size of 100 μm and a powder having an average particle size of 10 μm or finer, or a powder mixed with a powder having an average particle size of 60 μm and a powder having an average particle size of 10 μm or finer. Here, the average particle size can be determined by calculating the average diameter of 1,000 particles using a scanning electron microscope (e.g., JSM-T200 type manufactured by JEOL Ltd.) and an image analyzer (e.g., manufactured by Nippon Avionics Co., Ltd.).

[0061] In order to obtain a preferred flatness for the main surface of the heat sink, a part of the obtained preform may be machined before the preform is impregnated with a metal. For example, at least one surface of the preform may be machined to have a convex curved shape toward the outside by a cutting / grinding machine such as a lathe. When machining (cutting) is performed at the preform stage, there is an advantage that it is not necessary to use a special tool for metal cutting, and the degree of curvature and flatness can be easily controlled.

[0062] In the above step (ii) (impregnation with metal), the so-called melt forging method or die casting method can be adopted to impregnate the metal into the preform obtained by firing.

[0063] In the case of the molten metal casting method, a preform is impregnated with a metal containing aluminum or magnesium to produce a metal-silicon carbide composite having a composite portion containing silicon carbide and a metal, and a surface metal layer on the outer surface of the composite portion. As a method for impregnating a preform with a metal (alloy) containing aluminum or magnesium to obtain a metal-silicon carbide composite, for example, the following method is available. One or more of fibers, spherical particles, and crushed particles made of alumina or silica are placed on both surfaces of the preform so that they are in direct contact with each other, and the preform is sandwiched between release plates to form a block. This block is preheated to 500°C to 650°C, and one or more blocks are placed in a high-pressure vessel. Then, as quickly as possible to prevent the block from losing temperature, a molten metal containing aluminum or magnesium is pressurized at a pressure of 30 MPa or more, and the metal is impregnated into the voids of the preform. As a result of the above, a metal-silicon carbide composite is obtained, which comprises a composite portion containing silicon carbide and a metal, and a surface metal layer on the outer surface of the composite portion.

[0064] In the die casting method, a preform is set in a mold having a cavity of the product shape, the mold is clamped, and then metal is injected at high speed to obtain a metal-silicon carbide composite.

[0065] Here, for example, in the above-mentioned molten metal casting method, by devising the shape of the concave and / or convex mold, more specifically, by providing a "gap" equivalent to the metal layer between the mold and the preform, a metal layer can be provided on the surface of the metal-silicon carbide composite (i.e., it is possible to obtain a heat sink 1 in which a metal layer 3 is formed on both the front and back sides of a composite 2, as shown in Figure 1). Incidentally, when the metal layer is formed in this manner, the composition of the metal impregnated in the composite body is basically the same as the composition of the metal constituting the metal layer.

[0066] The metal to be impregnated is not particularly limited as long as it contains aluminum or magnesium. The metal is preferably a metal containing aluminum or magnesium as a main component, and more preferably a metal containing aluminum as a main component.

[0067] The impregnating metal may include other elements besides aluminum or magnesium. For example, the metal to be impregnated may contain aluminum as the main component, 0.1% by mass to 1.5% by mass of magnesium, and 0.1% by mass to 18% by mass of silicon. Alloying aluminum with silicon and magnesium has the advantage of lowering the melting point of the alloy and lowering the viscosity of the molten metal at high temperatures, making it easier to obtain a dense composite by high-temperature casting or the like.

[0068] Annealing may be performed to remove distortion caused during impregnation, etc. The annealing for removing distortion is preferably performed at a temperature of 400° C. to 550° C. for 10 minutes or more. If the annealing temperature is 400° C. or higher, the distortion inside the heat sink 1 is sufficiently released, and it is possible to prevent the curvature from changing significantly during the annealing process after machining. If the annealing temperature is 550° C. or less, the metal used for the impregnation (for example, an aluminum alloy) can be prevented from melting. If the annealing time is 10 minutes or more, the distortion inside the heat sink 1 is sufficiently released, and the curvature can be prevented from changing significantly during the annealing process for removing the machining distortion after the machining process.

[0069] (2) Flatness adjustment: As an example, the flatness can be adjusted by hot pressing the heat sink 1 obtained above. Specifically, as shown in Figures 3(a), 3(b), and 3(c), the heat sink 1 is sandwiched between a press convex die 100 and a press concave die 110 and hot-pressed (pressed while being heated). This allows the flatness of the main surface of the heat sink 1 to be adjusted. The press convex mold 100 and the press concave mold 110 are shaped so as to impart a predetermined curvature to the heat sink 1. Typically, the shape of the convex portion of the press convex mold 100 and the shape of the concave portion of the press concave mold 110 are substantially the same. That is, typically, when the press convex mold 100 and the press concave mold 110 are stacked without sandwiching the heat sink 1 therebetween, there is almost no gap between the press convex mold 100 and the press concave mold 110.

[0070] There are no particular limitations on the material of the press convex die 100 and the press concave die 110, provided that they do not substantially deform under the temperature and pressure conditions described below. Specifically, ceramics such as carbon and boron nitride, and metal materials such as cemented carbide and stainless steel are preferably used.

[0071] The heating temperature during hot pressing is not particularly limited as long as a heat sink 1 with an appropriate curvature can be obtained. However, from the viewpoint of productivity and reducing pressure, the heating temperature is preferably as high as possible within a range in which the metal in the heat sink 1 does not melt. In this embodiment, considering that the metal contained in the heat sink 1 is aluminum, magnesium, or the like (including alloys), the heating temperature is preferably 450°C or higher and 550°C or lower.

[0072] The pressure during the hot pressing is not particularly limited as long as a heat sink 1 having an appropriate curvature can be obtained. The pressure may be appropriately adjusted depending on the thickness and heating temperature of the heat sink 1. However, from the viewpoints of productivity and reliably imparting a curve, the pressure is preferably 10 kPa or more, and more preferably 30 kPa or more and 250 kPa or less.

[0073] The time for the hot pressing is not particularly limited as long as a heat sink 1 having an appropriate curvature can be obtained. However, from the viewpoint of reliably curving the heat sink 1, the time for the temperature of the heat sink 1 itself to reach 450° C. or higher is preferably 30 seconds or more, and more preferably 30 seconds or more and 300 seconds or less.

[0074] On the other hand, as another example, the flatness adjustment may be performed by machining (grinding, cutting, etc.) at least one surface (the surface that will become the main surface 3B when made into a device mounting board) of the heat sink 1 obtained above. Specifically, the flatness of at least one main surface (main surface 3B) of the heat sink 1 can be adjusted by a tool capable of precise cutting (grinding, cutting, etc.) such as a lathe.

[0075] Since the amount of warping changes before and after mounting electronic elements 11 on heat sink 1, it is preferable to adjust the flatness in advance, taking this change into consideration. For example, six electronic elements 11 (ceramic substrates) each measuring 50 mm x 58 mm are mounted on a heat sink 1 measuring 187.5 mm x 137.5 mm (coverage area 174 cm 2 / 257cm 2Under the condition of a surface area coverage rate of 67.5%), the amount of warping before and after mounting is reduced by approximately 150 μm in the longitudinal direction and approximately 6 μm in the transverse direction.

[0076] In addition, when adjusting the flatness, both the hot pressing and the machining may be performed.

[0077] The manufacturing process of the heat sink may include other steps not described above. As an example, the manufacturing process of the heat sink may include a process of forming holes for screws. Specifically, the holes for screws for joining to another heat sink component may be formed by machining or the like. The step of drilling the screw holes may be performed at any stage, but it is preferable to perform the step before machining, particularly when machining is performed to adjust the flatness of the heat sink, so that the drilled holes can also be used for fixing to a lathe, etc.

[0078] As another example, the manufacturing process of the heat sink may include a step of polishing one or both sides of the heat sink as appropriate, which makes it possible to adjust, for example, the arithmetic mean roughness Ra of the heat sink surface. As yet another example, the manufacturing process of the heat sink may include a step of providing a plating layer on the outermost surface of the heat sink. The significance of providing the plating layer is as described above.

[0079] (3) Bonding: For example, (i) first, a solder paste made by adding flux to the surface of the heat sink whose flatness, etc. have been adjusted as described above is applied, (ii) an electronic element (e.g., a ceramic circuit board) is placed on the applied solder paste, and (iii) the solder is melted by reflow to obtain an element mounting board. This joining typically results in some change in flatness of one surface of the heat sink (main surface 3B in FIG. 1), with the flatness being 50 to 600 μm. As mentioned above, by adjusting, for example, the flatness of the main surface of the heat sink before bonding, the type and thickness of the solder used, the area occupied by the electronic element when the heat sink is viewed from above, etc., it becomes easier to obtain a desired flatness in the final element mounting board.

[0080] The components, materials, manufacturing method, etc. of the electronic element (ceramic circuit board) are as described above, so a detailed explanation will be omitted. The solder that can be preferably used is as described above, and therefore a detailed description will be omitted.

[0081] The reflow conditions are not particularly limited and may be set appropriately depending on the melting temperature of the solder, but typically may be about 5 to 30 minutes at 250 to 350° C. If the temperature is not too high / the time is not too long, unintended changes in flatness can be suppressed.

[0082] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0083] The embodiments of the present invention will be described in detail based on examples and comparative examples. However, the present invention is not limited to the examples.

[0084] 1. Manufacturing of heat sinks (Formation of silicon carbide porous body) First, silicon carbide powder A, silicon carbide powder B, and silica sol were mixed in a stirrer mixer for 30 minutes to obtain a mixture. Silicon carbide powder A (manufactured by Pacific Random Co., Ltd.: NG-150, average particle size: 100 μm) 300 g Silicon carbide powder B (Yakushima Denko Co., Ltd.: GC-1000F, average particle size: 10 μm) 150 g Silica sol (Nissan Chemical Industries, Ltd.: Snowtex) 30g

[0085] The mixture obtained was placed in a mold and pressed at a pressure of 10 MPa to obtain a plate-shaped molded body with dimensions of 185 mm x 135 mm x 5.5 mm. The molded body obtained was fired in air at a temperature of 900°C for 2 hours to obtain a silicon carbide-based porous body with a relative density (bulk density) of 65% by volume.

[0086] The surface of this silicon carbide-based porous body, which would become the main surface 2B of the completed heat dissipation member, was machined using a surface grinder. Then, the surface that would become the main surface 2A was machined into a convex curved shape using a lathe with an R=11 m. At this time, the thickness of the silicon carbide-based porous body at the center was adjusted to 4.8 mm. For the following steps, 30 similar silicon carbide porous bodies were prepared.

[0087] (Metal Impregnation) Alumina fiber (manufactured by Tanaka Seishi Kogyo Co., Ltd., 97% purity, sheet form) was placed on the main surface 2A side of the machined silicon carbide porous body, and 30 sheets were stacked by sandwiching it between stainless steel plates with dimensions of 210 mm x 160 mm x 0.8 mm and carbon coated on both sides. Next, 6 mm thick steel plates were placed on both sides, connected with six M10 bolts, and tightened with a torque wrench so that the tightening torque in the surface direction was 3 Nm to form a single block. The integrated block was then preheated to 620°C in an electric furnace, and then placed in a preheated press mold with an inner diameter of 400 mm. Molten aluminum alloy containing 12% by mass of silicon and 1.0% by mass of magnesium was poured into the press mold, and pressure was applied at 100 MPa for 20 minutes. This allowed the silicon carbide porous body to be impregnated with the aluminum alloy.

[0088] After the impregnation was completed, the sample was cooled to 25°C, then cut into the shape of the release plate using a wet band saw, and the sandwiched stainless steel plate was peeled off.Furthermore, to remove distortion caused by the impregnation, the sample was annealed at a temperature of 500°C for 3 hours. In this manner, an aluminum-silicon carbide composite was obtained.

[0089] (Post-impregnation treatment) The outer periphery of the obtained aluminum-silicon carbide composite was machined with an NC lathe to a length and width of 190 mm × 140 mm, after which eight through holes with a diameter of 7 mm and four countersinks with a diameter of 10-4 mm were machined on the periphery.

[0090] In addition, the side of the aluminum-silicon carbide composite corresponding to the main surface 2A was machined with a turning center to have a radius of curvature of R=11 m. After machining, the aluminum-silicon carbide composite was annealed in a muffle furnace at a temperature of 500° C. for 4 hours. This removed machining distortion.

[0091] Furthermore, the aluminum-silicon carbide composite was cleaned by blasting with alumina abrasive grains under conditions of a pressure of 0.4 MPa and a conveying speed of 1.0 m / min, and then electroless Ni-P and Ni-B plating was performed, forming a plating layer 8 μm thick (Ni-P: 6 μm, Ni-B: 2 μm) on the surface of the composite.

[0092] In this manner, a heat dissipation plate (heat dissipation member) was obtained.

[0093] 2. Preparation of Electronic Devices The material of the ceramic plate, its linear expansion coefficient, the material of the copper layer, and the overall size and thickness are as follows: The ceramic material may be a nitride ceramic such as silicon nitride or aluminum nitride, an oxide ceramic such as aluminum oxide or zirconium oxide, a carbide ceramic such as silicon carbide, a boride ceramic such as lanthanum boride, etc. Among these, aluminum nitride, silicon nitride, and aluminum oxide are preferred from the viewpoints of insulation, strength of bonding with the metal layer 13, mechanical strength, etc. Thermal expansion coefficient: Silicon nitride 3ppm / K, Aluminum nitride 4.6ppm / K (room temperature 25℃~400℃) · Materials of copper: copper, copper alloy, aluminum and aluminum alloy Metal plate thickness: 0.15~0.8mm Ceramic substrate size: □50mm×58mm Ceramic substrate thickness: 0.32mm~1.00mm

[0094] 3. Soldering of heat sink and electronic components The composition of the solder used for soldering the heat sink and the electronic element, the soldering conditions, thickness, and coverage area by the substrate are as follows. Solder composition: Lead / tin eutectic solder (63% tin) Soldering temperature: 250℃ Flux: Yes Coating thickness: 0.2mm - Coverage area by substrate: Six ceramic substrates of 50mm x 58mm were mounted on a heat sink of 187.5mm x 137.5mm. (Coverage area 174cm 2 / 257cm 2 , coverage rate 67.5%)

[0095] 4. Flatness measurement (Measurement of f) For the heat sink 1 on which the electronic element 11 is mounted, the flatness of the main surface 3B on the side on which the electronic element 11 is not mounted was measured using a VR-3000 device manufactured by Keyence Corporation to obtain the flatness f. At this time, since the main surface 3B did not fall within the observation field of the device, the center (geometric center of gravity) of the main surface 3B as viewed from above was aligned with the center of the observation field of the measuring device, and an area of ​​190 mm x 100 mm was measured. The results of measuring nine heat sinks 1 of the examples (Examples 1 to 9) are shown in Table 1. The flatness f was 363.7 μm on average, 480 μm at maximum, 246 μm at minimum, and 77.3 at standard deviation.

[0096] (Measurement of h1 and h2) Data on the shape of the main surface 3B was obtained using a laser three-dimensional shape measuring device, and the data was analyzed to determine h1 and h2. In addition, h1 and h2 were obtained before and after mounting the electronic element 11, and the extent of change before and after mounting was confirmed. Equipment: Laser 3D shape measuring machine (a combination of the following four devices) XYθ stage unit: K2-300 (manufactured by Kozu Seiki Co., Ltd.) High-precision laser displacement meter: LK-G500 (Keyence Corporation) Motor controller: SC-200K (manufactured by Kozu Seiki Co., Ltd.) AD converter: DL-100 (manufactured by Kozu Seiki Co., Ltd.) Table 1 shows (h1 / a) / (h2 / b) for nine heat sinks 1 as examples (Examples 1 to 9). In Examples 1 to 9, (h1 / a) / (h2 / b) was a minimum of 1.27 and a maximum of 1.78, falling within the range of 1 or more and 1.9 or less shown in the embodiment. Table 2 also shows the change in the amount of warping before and after mounting the electronic element 11 on three heat sinks 1 as examples (Examples 10 to 12). In these examples, the amount of warping is reduced by approximately 150 μm in the longitudinal direction and approximately 6 μm in the lateral direction. By adjusting the flatness in advance in anticipation of this change, it is possible to achieve the desired adhesion and heat dissipation properties.

[0097] 5. Measurement of arithmetic mean roughness Ra (surface roughness Ra) For the heat sinks 1 of the embodiment (129 sheets), the surface roughness Ra of the portions of the main surface 3A where the electronic elements 11 were not mounted (portions where the main surface 3A was exposed) was measured in accordance with ISO4287-1997 using a Mitutoyo measuring device, Surftest SJ-310. As a result of measuring the heat sink 1 of the example, the surface roughness Ra was 1.02 μm on average, 1.52 on maximum, 0.84 on minimum, and 0.11 on standard deviation.

[0098] 6.Performance Evaluation When the heat sink 1 of Examples 1 to 9 shown in Table 1 was joined to a heat sink fin with screws and the adhesion between the heat sink 1 and the heat sink fin, heat dissipation, etc. were evaluated, the adhesion and heat dissipation were good. That is, it was shown that by using the heat sink 1 of Examples 1 to 9, it is possible to manufacture a power module having good heat dissipation properties, and also possible to improve the yield when manufacturing such a power module. In addition, when the flatness was 700 μm and the rest was the same as in Example 1 (Comparative Example), an M-shape was formed when the plate was fixed to the Cu plate or Al plate with screws, and a gap was generated between the plate and the Cu plate or Al plate. Furthermore, after mounting on the substrate, the case covering the upper part did not fit when manufacturing the power module. [Table 1] [Table 2]

[0099] This application claims priority based on Japanese Patent Application No. 2020-063126, filed on March 31, 2020, the disclosure of which is incorporated herein in its entirety. [Explanation of symbols]

[0100] 1 Heat sink 2 Composites (metal-silicon carbide composites containing aluminum or magnesium) 3 Metal layer (aluminum or magnesium-containing metal layer) 3A: Principal surface (surface on which electronic element 11 is mounted) 3B Principal surface (the other surface of principal surface 3A) 5 Through hole 11 Electronic elements 12 Ceramic plate 13 Metal layer 100 Press convex type 110 Press concave type

Claims

1. A heat sink having aluminum or magnesium-containing metal layers formed on both sides of a flat metal-silicon carbide composite containing aluminum or magnesium; and an electronic element including a ceramic plate mounted on one surface side of the heat sink, The flatness of the other surface of the heat sink is 600 μm or less, the heat sink is substantially rectangular; The length of the long side of the rectangle is a and the length of the short side is b, A straight line connecting the midpoints of the two short sides of the other surface is denoted by l 1 , and a straight line connecting the midpoints of the two long sides of the other surface is denoted by l 2 ; When the heat sink is viewed in cross section along a cross section that includes l 1 and is substantially perpendicular to the other surface, the maximum distance between l 1 and a point on the curve formed by the other surface is defined as h 1 ; When the heat sink is viewed in cross section along a cross section that includes l 2 and is substantially perpendicular to the other surface, the maximum distance between l 2 and a point on the curve formed by the other surface is defined as h 2 . A device mounting board in which (h 1 / a) / (h 2 / b) is 1.07 or more and 1.9 or less.

2. 2. The device mounting board according to claim 1, The thermal expansion coefficient of the heat sink between room temperature and 400°C is α 1 The thermal expansion coefficient of the ceramic plate between room temperature and 400°C is α 2 Then, α 1 and α 2 The difference is 5.0 ppmK. -1 The following is an element mounting board.

3. 3. The device mounting board according to claim 1, The element mounting board has an arithmetic mean roughness Ra of 0.2 to 2.0 μm in a portion of the one surface of the heat sink where the electronic element is not mounted.

4. The device mounting board according to any one of claims 1 to 3, When the device mounting board is viewed from above with the one surface side of the heat sink as the upper surface, 10 to 80% of the area of ​​the heat sink is covered with the electronic device.

5. A method for manufacturing a device mounting board according to any one of claims 1 to 4, comprising the steps of: A preparation step of preparing a heat sink having aluminum or magnesium-containing metal layers formed on both sides of a flat metal-silicon carbide composite containing aluminum or magnesium; a flatness adjusting step of adjusting the flatness of at least one surface of the heat sink; a mounting step of mounting an electronic element including a ceramic plate on a surface of the heat sink opposite to the one surface; A method for manufacturing a device mounting board comprising the steps of:

Citation Information

Patent Citations

  • Aluminum alloy-ceramic composite and its production method

    JP2006117491A

  • SILICON CARBIDE COMPOSITE, MANUFACTURING METHOD THEREOF, AND HEAT DISPERSION USING THE SAME

    JP3468358B2

  • Silicon carbide complex, method for manufacturing same, and heat dissipation component using same

    WO2015115649A1

  • Aluminum-silicon carbide composite and production method therefor

    WO2016017689A1

  • Heat dissipation component and method for manufacturing same

    WO2016021645A1