Carbon nanomaterial coating composition

The carbon nanomaterial coating composition addresses high costs and moisture issues in existing solutions by using a dipolar compound and polyvinyl dispersant, enabling efficient and cost-effective low-temperature drying.

JP7596456B2Active Publication Date: 2024-12-09CARBON T&C CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023112263
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-07-11
Filing Date
2023-07-07
Publication Date
2024-12-09
Estimated Expiration
2043-07-07

AI Technical Summary

Technical Problem

Existing carbon nanomaterial coating solutions using ionic dispersants are costly and require high-temperature drying, which can lead to moisture ingress and increased costs.

Method used

A carbon nanomaterial coating composition using a dipolar compound, polyvinyl dispersant, and solvent, which allows for lower-temperature drying and reduces costs by using a polymeric dispersant.

Benefits of technology

The composition reduces coating time and costs while preventing moisture ingress, achieving efficient and cost-effective carbon nanomaterial coating at lower temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596456000002
    Figure 0007596456000002
  • Figure 0007596456000003
    Figure 0007596456000003
  • Figure 0007596456000004
    Figure 0007596456000004
Patent Text Reader

Abstract

To provide a composition for carbon nanomaterial coating containing a bipolar compound, an amine-based dispersant, and a solvent.SOLUTION: Unlike conventional coating solutions using an ionic dispersant, the composition for coating a carbon nanomaterial of the present invention is used together with a polymer-based dispersant to reduce the cost incurred during the coating, and the coating is completed within minutes, thereby reducing the coating time. In addition, unlike the conventional coating solutions that require drying at a temperature of 150°C or higher, the coating composition of the present invention can be dried at a low temperature, thereby exhibiting time and cost saving effects.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating composition for carbon nanomaterials, comprising a bipolar compound, a polyvinyl dispersant and a solvent. [Background technology]

[0002] Recently, interest in energy storage technology has been on the rise, and carbon materials have been commercialized in leisure products and are now gradually expanding their scope of use to automobiles, aviation, IT, new renewable energy, and more.

[0003] Nano carbon materials are carbon-based nano materials, and refer to carbon quantum dots or fullerenes, which are zero-dimensional structures of carbon, carbon nanoribbons and carbon nanotubes, which are one-dimensional structures, graphene, which is a two-dimensional structure, etc. Nano carbon materials can be broadly divided into carbon quantum dots, fullerenes, carbon nanoribbons, carbon nanotubes, graphene, etc. according to the state of matter, and these can be divided into top-down and bottom-up methods according to their production methods.

[0004] It has the characteristics of a carbon material, being strong and having high thermal conductivity, and in particular, when the size of the material is very small, such as carbon quantum dots, it is possible to observe quantum physical phenomena (various characteristics such as light emission, band gap changes, and down-conversion due to energy transition). Such nanocarbon materials have excellent electrical, physical, chemical, and mechanical properties, and are attracting attention as new materials that overcome the technological limitations of existing industrial fields.

[0005] As existing parts materials are gradually being replaced by carbon materials, private companies are also showing increasing interest in carbon materials to strengthen their competitiveness and are actively researching commercialization methods. Furthermore, nano carbon materials are attracting attention as conductive materials for electromagnetic shielding and coating materials for touch panels, and are rapidly spreading as they replace conventional electrically conductive polymer composite materials.

[0006] The unique physical properties of CNTs have the potential to influence innovation in a variety of application fields, and it is expected that a variety of product innovations using CNTs will emerge in these fields in the future. Due to the lightweight and high strength characteristics of carbon fiber, there is increasing demand in the civil engineering and construction fields, such as building materials, concrete structures, and earthquake reinforcement, as well as in the alternative energy field, such as compressed natural gas (CNG) storage tanks, wind power generation blades, centrifuge rotors, and flywheels.

[0007] In addition, the unique properties of graphene, a nano carbon material, make it a material that is expected to bring innovation to various application fields, just like CNTs. While CNTs have a linear structure, graphene has a plate-like structure, and like CNTs, its demand is increasing in various fields.

[0008] Recently, with the development of 5G and 6G, there is a growing need to improve the heat dissipation properties of alumina or boron powder used as heat dissipation materials, and heat dissipation of LEDs used in automobiles is also becoming an issue.

[0009] When manufacturing typical chip components such as multilayer ceramic capacitors, inductors, and chip resistors, ceramic powder and numerous additives are added, and progress is being made in reducing the size and capacity of these components by improving the performance of these additives. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Republic of Korea Patent No. 10-1321097 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention provides a coating composition for carbon nanomaterials, comprising a dipolar compound, a polyvinyl dispersant and a solvent.

[0012] According to another embodiment of the present invention, 1) mixing a material to be coated with a carbon nano material dispersion liquid containing a carbon nano material, a polyvinyl dispersant, a polyamine dispersant, and a solvent to adsorb the carbon nano material onto the surface of the material to be coated; 2) Adding a carbon nano material coating composition according to any one of claims 1 to 12 to coat the carbon nano material on the surface of the coating target material; 3) drying the material to be coated; The present invention provides a method for coating a carbon nanomaterial, comprising the steps of: [Means for solving the problem]

[0013] The present invention provides a coating composition for carbon nanomaterials, comprising a dipolar compound, a polyvinyl dispersant and a solvent.

[0014] The bipolar compound may be selected from the group consisting of caffeine, adenosine, alanine, arginine, histidine, ethanolamine, urea, aminosulfate, and MBA (N-N'-Methylenebisacrylamide), but is not limited thereto.

[0015] The polyvinyl dispersant may be a polymer containing pyrrolidone, but is not limited thereto.

[0016] The polyvinyl dispersant may be, but is not limited to, Poly(4VP-co-NVP) or PEG (Poly Ethylene Glycol)-PVP (Poly Vinyl Pyrrolidone) copolymer.

[0017] The Poly(4VP-co-NVP) can be polymerized with 4-vinylpyridine and N-vinylpyrrolidone, but is not limited thereto.

[0018] The solvent may be any one selected from the group consisting of H2O, ethanol, N-methylpyrrolidone (NMP), DMF, DMSO, and acetone, but is not limited thereto.

[0019] The carbon nano material coating composition may be used together with a carbon nano material dispersion liquid including a carbon nano material, a polyacrylic dispersant, a polyvinyl dispersant, and a solvent, but is not limited thereto.

[0020] The carbon nano material may be selected from the group consisting of carbon nanotubes (CNTs), carbon fibers, graphene, carbon black, and combinations thereof, but is not limited thereto.

[0021] The polyacrylic dispersant may be selected from the group consisting of polyacrylonitrile, polyacrylic acid, polyvinylpyrrolidone, polymethacrylate, PMMA (polymethyl methacrylate), PEMA (polyethyl methacrylate), Poly-HEMA (poly-2-hydroxyethyl methacrylate), and combinations thereof, but is not limited thereto.

[0022] The carbon nanomaterial dispersion liquid further contains a polyethylene-based dispersant, which may be selected from the group consisting of SDS (sodium dodecyl sulfate), SLS (sodium lauryl sulfate), SDP (sodium dodecyl phosphate), PVC (polyvinyl chloride), PVDC (poly(vinylidene dichloride)), PGA (polyglycolide), PEG (polyethylene glycol), PEO (polyethylene oxide), and combinations thereof, but is not limited thereto.

[0023] The polyvinyl dispersant may be the same as the polyvinyl dispersant of claim 1, but is not limited thereto.

[0024] The solvent may be selected from the group consisting of, but is not limited to, H2O, ethanol, N-methylpyrrolidone (NMP), DMF, DMSO, and acetone.

[0025] According to another embodiment of the present invention, 1) mixing a material to be coated with a carbon nano material dispersion liquid containing a carbon nano material, a polyvinyl dispersant, a polyamine dispersant, and a solvent to adsorb the carbon nano material onto the surface of the material to be coated; 2) adding a carbon nano material coating composition according to any one of claims 1 to 12 to coat the carbon nano material on the surface of the coating target material; and 3) A method for coating a carbon nano material, comprising the step of drying the material to be coated.

[0026] The coating target material may be any one of a lithium battery positive electrode material, SiOx, SiNx, SiOxNy, AlOx, zinc oxide (ZnO), and silicon carbide (SiC), but is not limited thereto.

[0027] The lithium battery cathode material is LTO (Li14 Ti 15 O 12 , LCO (LiCoO2), NCM (Li[Ni,Co,Mn]O2), NCMA (Li[Ni.Co.Mn.Al]O2), NCA (Li[Ni,Co,Al]O2), LMO (LiMn2O4), LFP (LiFePO4) and LCP (LiCoPO4), but is not limited thereto. Effect of the Invention

[0028] The carbon nanomaterial coating composition of the present invention is used together with a polymeric dispersant, unlike existing coating solutions that use ionic dispersants, thereby reducing the costs incurred during coating, and since coating is completed within the water, the time required for coating is shortened. Unlike existing coating solutions that require drying at temperatures of 150°C or higher, drying is possible at low temperatures, so the coating composition of the present invention has the effect of saving time and costs. [Brief description of the drawings]

[0029] [Figure 1] 1 is a SEM image showing carbon nanotubes coated on a polycrystalline (NCM) surface using the carbon nanomaterial coating liquid composition of the present invention. [Diagram 2] 1 is a SEM image for confirming carbon nanotubes coated on the surface of an NCM (Single Crystal) using the carbon nanomaterial coating liquid composition of the present invention. [Diagram 3] 1 is a SEM image showing carbon nanotubes coated on the surface of an LFP using the carbon nanomaterial coating liquid composition of the present invention. [Figure 4] 1 is a SEM image showing carbon nanotubes coated on a SiOx surface using the carbon nanomaterial coating liquid composition of the present invention. [Diagram 5]1 is a SEM image showing carbon nanotubes coated on a SiC surface using the carbon nanomaterial coating liquid composition of the present invention. [Figure 6] 1 is a SEM image showing carbon nanotubes coated on a SiC surface using the carbon nanomaterial coating liquid composition of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Throughout the specification of the present invention, when a part is said to "include" a certain element, this means that it can further include other elements, not excluding other elements, unless specifically stated to the contrary.

[0031] Throughout the specification of the present invention, when a step is said to be located "on" or "before" another step, this includes not only cases where a step is in a direct chronological relationship with another step, but also cases where a step is in an indirect chronological relationship with another step, where the chronological order of the two steps may change, such as a mixing step after each other.

[0032] The terms "about", "substantially", and the like used throughout the present specification are used in the sense of a numerical value or close to a numerical value when the manufacturing and material tolerances inherent in the described meaning are given, and are used to prevent unscrupulous infringers from unfairly exploiting the disclosure in which precise or absolute numerical values ​​are described to aid in the understanding of the present invention. The terms "step of" or "step of" used throughout the present specification do not mean "step for".

[0033] The present invention provides a coating composition for carbon nanomaterials, comprising a bipolar compound, a polyvinyl dispersant and a solvent, the coating composition for carbon nanomaterials comprising 96-99% by weight of the solvent, 0.1-1% by weight of the bipolar compound and 0.1-3% by weight of the polyvinyl dispersant.

[0034] The carbon nano material coating composition may be used together with a carbon nano material dispersion liquid including a carbon nano material, a polyacrylic dispersant, a polyvinyl dispersant, and a solvent, but is not limited thereto.

[0035] The carbon nanomaterial dispersion liquid may contain 93 to 98% by weight of a solvent, 0.1 to 2% by weight of a carbon nanomaterial, 0.1 to 3% by weight of a polyacrylic dispersant, and 0.1 to 2% by weight of a polyvinyl dispersant.

[0036] The carbon nano material dispersion liquid may further include a polyethylene-based dispersant. The polyethylene-based dispersant may be added to improve the dispersion effect. Although a polymer dispersant is effective as a primary dispersant, the dispersion force may be slightly reduced due to the bonding force between polymers. Therefore, when the polyethylene-based dispersant is added as a secondary dispersant, the dispersion effect can be improved.

[0037] According to another embodiment of the present invention, 1) mixing a material to be coated with a carbon nano material dispersion liquid containing a carbon nano material, a polyvinyl dispersant, a polyamine dispersant, and a solvent to adsorb the carbon nano material onto the surface of the material to be coated; 2) Adding a carbon nano material coating composition according to any one of claims 1 to 12 to coat the carbon nano material on the surface of the coating target material; 3) drying the material to be coated; The present invention provides a method for coating a carbon nanomaterial, comprising the steps of:

[0038] In step 1), 100 parts by weight of the carbon nano material dispersion may be mixed with 100 to 300 parts by weight of the coating target material, but is not limited thereto.

[0039] In step 2), 50 to 200 parts by weight of the carbon nano material coating composition may be mixed with 100 parts by weight of the carbon nano material dispersion, but is not limited thereto.

[0040] The temperature of the drying step may be 50 to 100° C., but is not limited thereto.

[0041] <Example 1> 1. Carbon nanotube dispersion production 2 g of polyacrylic acid and 1 g of polyvinyl dispersant Poly(4VP-co-NVP) were added to 96 g of N-methylpyrrolidone solvent and stirred, and then 1 g of carbon nanotubes was added and dispersed to prepare a final carbon nanotube dispersion.

[0042] 2. Carbon nano material coating liquid manufacturing A carbon nanomaterial coating solution was prepared by adding 0.6g of dipolar charged substance EDA (ethanolamine) and 1g of polyvinyl dispersant Poly(4VP-co-NVP) to 98.4g of solvent N-methylpyrrolidone and stirring.

[0043] 3. Carbon nanotube coating using dispersion and coating liquid 200 g of the NCM to be coated was added to 100 g of the prepared carbon nanotube dispersion and mixed to allow the carbon nanotubes to be adsorbed onto the surface of the NCM, and then 100 g of the carbon nanomaterial coating solution was added to allow the adsorbed carbon nanotubes to be coated onto the surface of the NCM.

[0044] The carbon nanotube-coated NCM surface was dried at 80° C. and observed under a SEM microscope, confirming that the NCM surface was coated with carbon nanotubes (FIG. 1).

[0045] <Example 2> 1. Carbon nanotube dispersion production 2 g of polyvinylpyrrolidone and 1 g of a polyvinyl dispersant PEG-PVP were added to 96 g of solvent water and stirred, and then 1 g of carbon nanotubes was added and dispersed to prepare a final carbon nanotube dispersion.

[0046] 2. Carbon nano material coating liquid manufacturing A carbon nanomaterial coating solution was prepared by adding 0.6 g of caffeine (a substance having a bipolar charge) and 1 g of a polyvinyl dispersant PEG-PVP to 98.4 g of solvent water and stirring them.

[0047] 3. Carbon nanotube coating using dispersion and coating liquid 200 g of the NCM to be coated was added to 100 g of the prepared carbon nanotube dispersion and mixed to allow the carbon nanotubes to be adsorbed onto the surface of the NCM, and then 100 g of the carbon nanomaterial coating solution was added to allow the adsorbed carbon nanotubes to be coated onto the surface of the NCM.

[0048] The carbon nanotube-coated NCM surface was dried at 80° C. and observed under a SEM microscope, confirming that the carbon nanotubes were coated on the NCM surface (FIG. 2).

[0049] <Example 3> 1. Carbon nanotube dispersion production 2 g of polyvinyl alcohol and 1 g of polyvinyl dispersant Poly(4VP-co-NVP) were added to 96 g of N-methylpyrrolidone solvent and stirred, and then 1 g of carbon nanotubes was added and dispersed to prepare a final carbon nanotube dispersion.

[0050] 2. Carbon nano material coating liquid manufacturing A carbon nanomaterial coating solution was prepared by adding 0.6g of dipolar charged substance EDA (ethanolamine) and 1g of polyvinyl dispersant Poly(4VP-co-NVP) to 98.4g of solvent N-methylpyrrolidone and stirring.

[0051] 3. Carbon nanotube coating using dispersion and coating liquid 200 g of NCM to be coated was added to 100 g of the prepared carbon nanotube dispersion and mixed to allow the carbon nanotubes to be adsorbed onto the LFP surface, and then 100 g of carbon nano material coating solution was added to allow the adsorbed carbon nanotubes to be coated onto the LFP surface.

[0052] The LFP surface coated with the carbon nanotubes was dried at a temperature of 80°C and then observed under a SEM microscope, confirming that the LFP surface was coated with carbon nanotubes (Figure 3).

[0053] <Example 4> 1. Carbon nanotube dispersion production 2 g of polyacrylonitrile and 1 g of polyvinyl dispersant Poly(4VP-co-NVP) were added to 96 g of N-methylpyrrolidone solvent and stirred, and then 1 g of carbon nanotubes was added and dispersed to prepare a final carbon nanotube dispersion.

[0054] 2. Carbon nano material coating liquid manufacturing A carbon nanomaterial coating solution was prepared by adding 0.6 g of adenosine (a substance having a bipolar charge) and 1 g of polyvinyl dispersant Poly(4VP-co-NVP) to 98.4 g of N-methylpyrrolidone solvent and stirring.

[0055] 3. Carbon nanotube coating using dispersion and coating liquid 200 g of SiOx to be coated was added to 100 g of the prepared carbon nanotube dispersion and mixed to allow the carbon nanotubes to be adsorbed onto the SiOx surface, and then 100 g of carbon nano material coating solution was added to allow the adsorbed carbon nanotubes to be coated onto the SiOx surface.

[0056] The carbon nanotube-coated SiOx surface was dried at 80° C. and observed under a SEM microscope, confirming that the SiOx surface was coated with carbon nanotubes (FIG. 4).

[0057] <Example 5> 1. Carbon nanotube dispersion production 2 g of polyvinylpyrrolidone and 1 g of polyvinyl dispersant Poly(4VP-co-NVP) were added to 96 g of N-methylpyrrolidone solvent and stirred, and then 1 g of carbon nanotubes was added and dispersed to prepare a final carbon nanotube dispersion.

[0058] 2. Carbon nano material coating liquid manufacturing A carbon nanomaterial coating solution was prepared by adding 0.6g of dipolar charged substance EDA (ethanolamine) and 1g of polyvinyl dispersant Poly(4VP-co-NVP) to 98.4g of solvent N-methylpyrrolidone and stirring.

[0059] 3. Carbon nanotube coating using dispersion and coating liquid 200 g of SiC to be coated was added to 100 g of the prepared carbon nanotube dispersion and mixed to allow the carbon nanotubes to be adsorbed onto the SiC surface, and then 100 g of carbon nano material coating liquid was added to allow the adsorbed carbon nanotubes to be coated onto the SiC surface.

[0060] The carbon nanotube-coated SiC surface was dried at a temperature of 80° C. and observed under a SEM microscope, confirming that the SiC surface was coated with carbon nanotubes (FIG. 5).

[0061] <Example 6> 1. Graphene dispersion preparation 2 g of polyvinylpyrrolidone and 1 g of a polyvinyl dispersant Poly(4VP-co-NVP) were added to 96 g of N-methylpyrrolidone solvent and stirred, and then 1 g of graphene was added and dispersed to prepare a final graphene dispersion.

[0062] 2. Carbon nano material coating liquid manufacturing A carbon nanomaterial coating solution was prepared by adding 0.6g of dipolar charged substance EDA (ethanolamine) and 1g of polyvinyl dispersant Poly(4VP-co-NVP) to 98.4g of solvent N-methylpyrrolidone and stirring.

[0063] 3. Graphene coating using dispersion and coating liquid 200 g of SiC to be coated was added to 100 g of the prepared graphene dispersion and mixed to allow the graphene to be adsorbed onto the surface of the SiC, and then 100 g of the prepared carbon nano material coating solution was added to allow the adsorbed graphene to be coated onto the surface of the SiC.

[0064] The graphene-coated SiC surface was dried at a temperature of 80° C. and observed under a SEM microscope. It was confirmed that the SiC surface was coated with graphene (FIG. 6).

[0065] <Experimental Example> 1. Electrochemical Characterization The electrical resistance of NCM523 was measured and compared with that of NCM523 coated with CNT as follows.

[0066] In Experimental Example 1, bare NCM523, Super-P, and PVdF, which were not coated with CNTs, were mixed at a ratio of 98:1:1 and coated on an aluminum current collector.

[0067] In Experimental Example 2, bare NCM523, CNT, and PVdF, which were not coated with CNT, were mixed at a ratio of 98:1:1 and coated on an aluminum current collector.

[0068] In Experimental Example 3, bare NCM523 without CNT coating, CNT, Super-P, and PVdF were mixed in a ratio of 97.5:0.5:1:1 and coated on an aluminum current collector.

[0069] In Experimental Example 4, NCM523 coated with 0.5% CNT: Super-P: PVdF was mixed at a ratio of 97.5 (+0.5% CNT): 1: 1 and coated on an aluminum current collector. At this time, 0.1wt% PVP was used as a dispersant for CNT coating based on the total weight of the carbon nano material dispersion.

[0070] In Experimental Example 5, NCM523 coated with 0.5% CNT: Super-P: PVdF was mixed at a ratio of 97.5 (+0.5% CNT): 1: 1 and coated on an aluminum current collector. At this time, 0.5wt% PVP was used as a dispersant for CNT coating based on the total weight of the carbon nano material dispersion.

[0071] In Experimental Example 6, NCM523 coated with 0.5% CNT: Super-P: PVdF was mixed at a ratio of 97.5 (+0.5% CNT): 1: 1 and coated on an aluminum current collector. At this time, 1.0 wt% PVP was used as a dispersant for CNT coating based on the total weight of the carbon nano material dispersion.

[0072] The aluminum current collectors coated with the coatings in Experimental Examples 1 to 6 were subjected to vacuum drying (100° C. for 6 hours) and then measured using a surface measuring device (ST-4).

[0073] [Table 1]

[0074] Experimental examples 1 and 2 show data comparing the sheet resistance of conductive materials Super-P and CNT, and show that CNT has superior conductivity compared to Super-P.

[0075] Experimental Examples 3 and 4 show the sheet resistance of bare NCM and CNT-coated NCM. When CNT is added separately to the conductive material and when CNT is coated on NCM in advance, the NCM coated with CNT first has an advantage in terms of CNT dispersion, and thus has a lower sheet resistance.

[0076] Experimental Examples 4, 5, and 6 show that the surface resistance increases as the content of binder used in coating the CNTs increases.

[0077] The data above shows that CNT is a better conductive material than Super-P, and when CNT is coated on NCM in advance, the dispersion of CNT is better and the surface resistance is lower.

[0078] Although the specific parts of the present invention have been described in detail above, it is obvious to those skilled in the art that such specific techniques are merely preferred embodiments and do not limit the scope of the present invention. Therefore, the substantial scope of the present invention is to be defined by the appended claims and their equivalents.

Claims

1. The composition includes a dipolar compound, a polyvinyl dispersant, and a solvent. The bipolar compound is any one selected from the group consisting of caffeine, adenosine, alanine, arginine, histidine, ethanolamine, urea, aminosulfate, and MBA (N-N'-Methylenebisacrylamide); The solvent is any one selected from the group consisting of H2O, ethanol, N-methylpyrrolidone (NMP), DMF, DMSO, and acetone; Used with a carbon nano material dispersion liquid containing a carbon nano material, a polyacrylic dispersant, a polyvinyl dispersant and a solvent, A carbon nanomaterial coating composition, 1) mixing the carbon nano material dispersion with a coating target material to adsorb the carbon nano material onto the surface of the coating target material; 2) adding the carbon nano material coating composition to coat the carbon nano material on the surface of the coating target material; 3) drying the material to be coated; A carbon nanomaterial coating composition for use in a carbon nanomaterial coating method, comprising:

2. The carbon nanomaterial coating composition according to claim 1, wherein the bipolar compound is any one selected from the group consisting of caffeine, adenosine, and ethanolamine.

3. A carbon nanomaterial coating composition as described in claim 1, characterized in that the polyvinyl dispersant in the carbon nanomaterial coating composition is a polymer containing pyrrolidone.

4. A carbon nanomaterial coating composition as described in claim 1, characterized in that the polyvinyl dispersant in the carbon nanomaterial coating composition is Poly(4VP-co-NVP) or PEG (PolyEthylene Glycol)-PVP (PolyVinylPyrrolidone) copolymer.

5. The carbon nano material coating composition according to claim 4, characterized in that the Poly(4VP-co-NVP) is polymerized by 4-vinylpyridine and N-vinylpyrrolidone.

6. The solvent in the carbon nanomaterial coating composition is H 2 2. The carbon nanomaterial coating composition according to claim 1, characterized in that the carbon nanomaterial coating composition is any one selected from the group consisting of O-methylpyrrolidone and N-methylpyrrolidone (NMP).

7. The carbon nanomaterial coating composition according to claim 1, wherein the carbon nanomaterial is selected from the group consisting of carbon nanotubes (CNT), carbon fibers, graphene, carbon black, and combinations thereof.

8. The carbon nanomaterial coating composition according to claim 1, characterized in that the polyacrylic dispersant is selected from the group consisting of polyacrylonitrile, polyacrylic acid, polyvinylpyrrolidone, polymethacrylate, PMMA (polymethyl methacrylate), PEMA (polyethylmethacrylate), Poly-HEMA (Poly-2-hydroxyethyl methacrylate), and combinations thereof.

9. The carbon nanomaterial coating composition according to claim 1, characterized in that the carbon nanomaterial dispersion further contains a polyethylene-based dispersant, and the polyethylene-based dispersant is selected from the group consisting of SDS (sodium dodecyl sulfate), SLS (sodium lauryl sulfate), SDP (sodium dodecyl phosphate), PVC (polyvinyl chloride), PVDC (poly(vinylidene dichloride)), PGA (polyglycolide), PEG (polyethylene glycol), PEO (polyethylene oxide) and combinations thereof.

10. A carbon nanomaterial coating composition as described in claim 1, characterized in that the polyvinyl-based dispersant in the carbon nanomaterial dispersion is equal to the polyvinyl-based dispersant in the carbon nanomaterial coating composition of claim 1.

11. The solvent in the carbon nanomaterial dispersion liquid is H 2 The carbon nanomaterial coating composition according to claim 1, characterized in that the solvent is any one selected from the group consisting of O, ethanol, N-methylpyrrolidone (NMP), DMF, DMSO and acetone.

12. 1) mixing a coating target material with a carbon nano material dispersion liquid including a carbon nano material, a polyvinyl dispersant, a polyacrylic dispersant, and a solvent to adsorb the carbon nano material onto the surface of the coating target material; 2) adding a carbon nanomaterial coating composition according to any one of claims 1 to 11 to coat the carbon nanomaterial on the surface of the coating target material; 3) drying the material to be coated; A carbon nanomaterial coating method comprising the steps of:

13. The carbon nanomaterial coating method according to claim 12, characterized in that the material to be coated is any one of a lithium battery positive electrode material, SiOx, SiNx, SiOxNy, AlOx, zinc oxide (ZnO), and silicon carbide (SiC).

14. The lithium battery cathode material is LTO (Li 14 Ti 15 O 12 ), LCO(LiCoO 2 ), NCM(Li[Ni,Co,Mn]O 2 ), NCMA(Li[Ni.Co.Mn.Al]O 2 ), NCA(Li[Ni,Co,Al]O 2 ), LMO(LiMn 2 O 4 ), LFP(LiFePO 4 ) and LCP(LiCoPO 4 14. The carbon nanomaterial coating method according to claim 13, characterized in that it includes one or more selected from the group consisting of:

Citation Information

Patent Citations

  • Electrode composition for battery

    JP2016025077A

  • Carbon nanotube dispersion liquid and use of the same

    JP2019192537A

  • Carbon nanotube dispersion and utilization thereof

    JP2020189770A

  • Dispersant composition for electricity storage device electrodes

    JP2022063854A

  • Carbon NANO tube transparent electrode, method for manufacturing the same, and coating composition for carbon NANO tube transparent electrode

    KR101321097B1