Manufacturing method for ceramic circuit board

By using a Ag-free brazing material with Cu and Sn/In in the ceramic circuit board manufacturing process, and employing a pH-controlled etching and polishing method, the durability and precision of the etching process are improved, addressing the issue of varying bonding layer sizes and enhancing TCT characteristics.

JP7596515B2Active Publication Date: 2024-12-09NITERRA MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023511240
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-30
Filing Date
2022-03-28
Publication Date
2024-12-09
Estimated Expiration
2042-03-28

AI Technical Summary

Technical Problem

The deterioration of chemical solutions used in the etching process for ceramic circuit boards leads to variations in the size of the protruding portion of the bonding layer, affecting the thermal cycle test (TCT) characteristics, especially when using a nitride-based ceramic substrate with a brazing material containing Ti, which reacts to form a titanium nitride layer.

Method used

A method for manufacturing ceramic circuit boards using a brazing material layer that does not contain Ag and includes Cu and one or more of Sn and In, employing a copper etching step with a pH-controlled etching solution of hydrogen peroxide and ammonium peroxodisulfate, followed by chemical polishing to control the size of the brazing material layer.

Benefits of technology

This method improves the durability of the etching solution, reduces the number of etching steps, and maintains precise control over the size of the protruding portion of the bonding layer, enhancing the TCT characteristics and yield of ceramic circuit boards, even for larger sizes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596515000012
    Figure 0007596515000012
  • Figure 0007596515000013
    Figure 0007596515000013
  • Figure 0007596515000014
    Figure 0007596515000014
Patent Text Reader

Abstract

The present invention provides a method for producing a ceramic circuit board in which a copper plate is joined to at least one surface of a ceramic substrate via a brazing material layer, said method being characterized in that the brazing material layer contains no Ag and contains one or two from among Sn or In, and Cu and Ti, and in that said method comprises: a chemical polishing step for preparing a ceramic circuit board in which a portion of the brazing material layer is exposed between pattern shapes of the copper plate, and chemically polishing the portion of the brazing material layer; and a brazing material etching step for etching the portion of the chemically polished brazing material layer with an etchant of pH 6 or less which contains one or two substances selected from hydrogen peroxide and ammonium peroxodisulfate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiment relates to a method for manufacturing a ceramic circuit board. [Background technology]

[0002] Power modules are becoming increasingly powerful. This has led to the guaranteed operating temperature of semiconductor elements rising to 175°C or higher. This has created a demand for improved thermal cycle test (TCT) characteristics in ceramic circuit boards that mount semiconductor elements. For example, International Publication No. 2017 / 056360 (Patent Document 1) describes providing a gradient structure on the side surface of a copper plate and optimizing the size of the protruding portion of the bonding layer. In Patent Document 1, excellent TCT characteristics are obtained. In particular, Patent Document 1 states that it is preferable to optimize the size of the protruding portion of the bonding layer. In order to control the size of the protruding portion of the bonding layer, the brazing material layer is etched. For example, International Publication No. 2019 / 054294 (Patent Document 2) discloses an etching process for the brazing material layer. In Patent Document 2, a chemical polishing process and an etching process are combined. By such a method, the size of the protruding portion of the bonding layer can be controlled. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2017 / 056360 [Patent Document 2] International Publication No. 2019 / 054294 Summary of the Invention [Problem to be solved by the invention]

[0004] As shown in Patent Document 1, an active metal bonding method is used to bond a ceramic substrate and a copper plate. In the active metal bonding method, a brazing material containing Ti, which is an active metal, is used. When the ceramic substrate is a nitride-based ceramic substrate, the Ti in the brazing material reacts with the ceramic substrate to form a titanium nitride (TiN) layer. The etching process for the ceramic circuit substrate requires the removal of both the bonding layer and the titanium nitride layer. For this reason, various chemicals are used in the etching process of ceramic circuit boards. In Patent Document 2, different chemicals are used to remove the brazing material layer and the titanium nitride layer. When the etching process is repeated, the chemicals deteriorate. The deterioration of the chemicals leads to a decrease in etching accuracy. For this reason, when the etching process is repeated, a problem occurs in that the size of the protruding part of the bonding layer varies. The present invention has been made to address such problems, and aims to provide a method for manufacturing a ceramic circuit board with improved durability of the chemical solution used in the etching step. [Means for solving the problem]

[0005] The manufacturing method of the ceramic circuit board according to the embodiment includes a step of preparing a bonded body in which a copper member is bonded to at least one surface of a ceramic substrate via a brazing material layer that does not contain Ag and contains Cu, an active metal, and one or more first elements selected from Sn and In; a first copper etching step of etching a part of the copper member and a layer contained in the brazing material layer and containing Cu and the first element as main components; a first brazing material etching step of etching an active metal reaction layer contained in the brazing material layer using an etching solution having a pH of 4 to 12 and containing one or two elements selected from hydrogen peroxide and ammonium peroxodisulfate; and a first chemical polishing step of chemically polishing an end portion of the brazing material layer exposed by the first brazing material etching step. [Brief description of the drawings]

[0006] [Figure 1]1A to 1C are process diagrams illustrating the first embodiment. [Diagram 2] FIG. 6 is a process diagram illustrating a second embodiment. [Diagram 3] FIG. 11 is a process diagram illustrating a third embodiment. [Figure 4] 13A to 13C are process diagrams illustrating a fourth embodiment. [Diagram 5] 13A to 13C are process diagrams illustrating a fifth embodiment. [Figure 6] 1A to 1C are cross-sectional views illustrating manufacturing processes of the embodiment. [Figure 7] FIG. 2 is a plan view illustrating a portion of a ceramic circuit board. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The manufacturing method of the ceramic circuit board according to the embodiment includes a step of preparing a bonded body in which a copper member is bonded to at least one surface of a ceramic substrate via a brazing material layer that does not contain Ag and contains Cu, an active metal, and one or more first elements selected from Sn and In; a first copper etching step of etching a part of the copper member and a layer contained in the brazing material layer and containing Cu and the first element as main components; a first brazing material etching step of etching an active metal reaction layer contained in the brazing material layer using an etching solution having a pH of 4 to 12 and containing one or two elements selected from hydrogen peroxide and ammonium peroxodisulfate; and a first chemical polishing step of chemically polishing an end portion of the brazing material layer exposed by the first brazing material etching step.

[0008] A ceramic circuit board is a member in which a ceramic substrate and a copper plate are joined together via a brazing material layer. Examples of ceramic substrates include silicon nitride substrates, aluminum nitride substrates, aluminum oxide substrates, and alumina substrates. For example, the thickness of the ceramic substrate is 0.2 to 0.8 mm. For example, the thermal conductivity of the silicon nitride substrate is 80 W / m·K or more, and the three-point bending strength is 600 MPa or more. For example, the thermal conductivity of the aluminum nitride substrate is 150 W / m·K or more, and the three-point bending strength is 300 to 550 MPa. For example, the thermal conductivity of the aluminum oxide substrate is 20 to 40 W / m·K, and the three-point bending strength is 400 to 500 MPa. The arugil substrate is a substrate containing zirconium oxide and aluminum oxide. The thermal conductivity of the arugil substrate is 20 to 40 W / m·K, and the three-point bending strength is 450 to 600 MPa. The strength of the silicon nitride substrate is high, so the substrate can be thinned to 0.33 mm or less. The aluminum nitride substrate has high thermal conductivity. Although the thermal conductivity of the aluminum oxide substrate and the arugil substrate is low, these substrates are inexpensive. The type of ceramic substrate can be appropriately selected according to the purpose. Furthermore, the silicon nitride substrate and the aluminum nitride substrate are called nitride-based ceramics. The aluminum oxide substrate, the arugil substrate, and the zirconium oxide substrate are called oxide-based ceramics. Furthermore, the silicon nitride substrate is a Si-containing ceramic. The aluminum oxide substrate, the arugil substrate, and the aluminum nitride substrate are Al-containing ceramics.

[0009] The copper member is preferably made of oxygen-free copper. This oxygen-free copper is copper with a purity of 99.96 wt% or more. If there is a large amount of oxygen in the copper member, there is a possibility that the bonding strength will decrease during active metal bonding. The copper member may be a copper plate or a copper film formed on a brazing material layer. The copper member may also be made of a composite material of copper and carbon and have a structure in which a layer of graphite exists in the copper. In the following, the case where the copper member is a copper plate will be described. The thickness of the copper plate is preferably 0.2 mm or more. By increasing the thickness to 0.7 mm or more, the heat dissipation of the copper plate can be improved. The upper limit of the plate thickness is not particularly limited, but is preferably 5 mm or less. If the plate thickness exceeds 5 mm, the warping of the bonded body when the copper plate and the ceramic substrate are bonded may be large. In addition, it becomes difficult to process the copper plate into a pattern shape by etching. The copper plate may be bonded to both sides of the ceramic substrate, or may be bonded to only one side of the ceramic substrate. More preferably, the copper plate is bonded to both sides of the ceramic substrate. When the copper plates are bonded to both sides, the thicknesses of these copper plates may be the same or different from each other. In consideration of mass production, it is preferable that the thicknesses of these copper plates are the same. When a pattern shape (circuit shape) is provided to the copper plate, the number of pattern shapes provided is not particularly limited. The pattern shape may be provided at one place on the copper plate, or the pattern shape may be provided at multiple places on the copper plate.

[0010] The brazing material layer is characterized by not containing silver (Ag) but containing Cu, Ti, and a first element. The first element is one or more selected from Sn and In. Here, the brazing material that does not contain Ag is also called Ag-less brazing material. "Not containing silver" means that the silver content is 0.01 wt% or less. 0.01 wt% or less means that it may contain unavoidable impurities. In addition, active metal bonding is used to bond the ceramic substrate and the copper plate. In the active metal bonding method, a brazing material containing Ti (titanium) as an active metal is used. A general active metal brazing material contains Ag (silver), Cu (copper), and Ti (titanium). Ag and Cu are components that form a eutectic with each other. By forming an AgCu eutectic, the bondability is improved. In the brazing material layer containing Ag, silver chloride (AgCl) was formed when chlorides such as iron chloride and copper chloride were used in etching the copper plate. This silver chloride has a very low solubility and poor etching properties. Therefore, the chemical solution for etching the brazing material layer containing Ag is easily deteriorated. When the chemical solution deteriorates, it is necessary to replace the chemical solution. If the frequency of replacing the chemical solution increases, it will lead to increased costs. By using a brazing material layer that does not contain Ag, the durability of the chemical solution can be improved. In addition, when comparing a brazing material layer that does not contain Ag with a brazing material layer that contains Ag, if the same amount is etched, the brazing material layer that does not contain Ag can shorten the etching time. In addition, the number of etchings can be reduced. From this point of view, the durability of the chemical solution can be improved. In addition, in Patent Document 2, a chemical polishing process was required before the etching process of the brazing material layer in order to remove silver chloride.

[0011] The brazing material layer is composed of Cu (copper) and Ti (titanium). Cu is the base material of the brazing material layer. Ti is an active metal, and reacts with the ceramic substrate to form a Ti reaction layer. The Ti reaction layer can improve the bonding strength between the ceramic substrate and the copper plate. In an oxide ceramic substrate, the Ti reaction layer is mainly titanium oxide (TiO2). In a nitride ceramic substrate, the Ti reaction layer is mainly titanium nitride (TiN). Examples of oxide ceramic substrates include alumina substrates, zirconia substrates, and alumina substrates. Examples of nitride ceramic substrates include aluminum nitride substrates and silicon nitride substrates. These TiN layers may contain copper, which is a brazing material component. Here, the titanium nitride (TiN) layer is called the active metal reaction layer. The active metal reaction layer is also sometimes called the active metal brazing material layer. Other active metals such as Zr, Hf, and Nb may be added as the active metal, but the amount of the active metal used in this case is preferably 25 mass % or less in total with Ti. There are also portions in this active metal brazing material layer that contain copper, tin, or indium. The brazing material layer contains one or both of Sn (tin) and In (indium). Sn or In has the effect of lowering the melting point of the brazing material. The brazing material may contain C (carbon). Carbon can improve the fluidity of the brazing material. In order to apply the brazing material to a large ceramic substrate, it is desirable for the brazing material to have good fluidity. In the brazing material, when the entire powder raw material is taken as 100 mass%, the Cu content is preferably 20 mass% or more and 90 mass% or less. The Ti element or compound content is preferably 0.5 mass% or more and 25 mass% or less. The Ti element or compound is added as Ti or titanium hydride (TiH2). The Sn or In content is preferably 5 mass% or more and 50 mass% or less in total. The C content is preferably 0 mass% or more and 5 mass% or less. For example, when the brazing material is made of Cu, Ti, and Sn, Cu+Ti+Sn=100 mass%. When the brazing material is made of Cu, TiH2, Sn, and C, Cu+TiH2+Sn+C=100 mass%.

[0012] The brazing material is used to manufacture a bonded body of a ceramic substrate and a copper plate. Examples of bonding methods using the brazing material include a method of mixing brazing material components with a solvent and applying the paste, and a method of processing an alloy foil or the like into a predetermined shape and bonding the same. A bonding method using a paste is preferable because it reduces the effort required for processing the material into a predetermined shape. Here, the brazing material dissolved in a solvent (containing an organic compound) is called a brazing material paste. The brazing material paste is applied onto a ceramic substrate, and a copper plate is placed on top of the brazing material paste. Thereafter, a heat bonding process is performed. The thickness of the brazing material paste applied is preferably within a range of 10 μm to 100 μm. It is more preferable that the thickness of the brazing material paste applied is within a range of 10 μm to 60 μm. The temperature of the heat bonding process is preferably within a range of 650° C. to 900° C. The atmosphere of the bonding process is a vacuum (10 -3 Pa or less) or an inert atmosphere is preferred. An inert atmosphere refers to an atmosphere with a low oxygen concentration. An inert atmosphere with an oxygen partial pressure of 5% or less is preferred. Examples of the inert atmosphere include a nitrogen atmosphere and a rare gas atmosphere such as argon, neon, helium, and xenon. The vacuum or inert atmosphere may be created before heating. After the heating and bonding process, the brazing paste becomes a brazing layer.

[0013] The length of the long side of the ceramic substrate may be 100 mm or more. The length of the long side of the ceramic substrate may be 200 mm or more. By increasing the long side of the ceramic substrate, it becomes possible to produce multiple pieces. The method of producing multiple pieces is a method of dividing a large ceramic circuit substrate to produce multiple ceramic circuit substrates. In the case of producing multiple pieces in this way, it is preferable to form a scribe groove in the ceramic substrate. The timing of forming the scribe groove is not particularly limited. The timing of the formation may be before the copper member is bonded, or any timing after the bonding. In addition, when the scribe groove is formed before the bonding with the copper member, it is more preferable to form the scribe groove on the sintered ceramic substrate. The shape of the scribe groove may be a dot shape, a line shape, a combination of these, or other shapes. In addition, the scribe groove may or may not have a through portion. The shape of the scribe groove is not particularly limited. In addition, a breaking (splitting) process may be provided separately from the formation of the scribe groove. Furthermore, the bonded body may be formed with a notch or a through hole as necessary. Thus, the specific shape of the bonded body is arbitrary and is not particularly limited. As described later, a bonded body is prepared by bonding a copper plate to a large ceramic substrate. By using a large ceramic substrate, a large bonded body can be prepared. After etching the copper plate to give a desired pattern shape, the ceramic circuit substrate is divided by scribing. By dividing the large bonded body, mass productivity can be improved. The upper limit of the length of the long side of the ceramic substrate is not particularly limited, but is preferably 500 mm or less. If the length of the long side of the ceramic substrate exceeds 500 mm, the ceramic substrate may become too heavy, which may increase the load of the transportation work. The length of the short side of the ceramic substrate is not particularly limited, but is preferably 50 mm or more. In addition, the length of each side of the ceramic substrate may be the same. According to the manufacturing method of the ceramic circuit substrate according to the embodiment, the etching property is good even if the ceramic substrate becomes large.The method for manufacturing a ceramic circuit board according to the embodiment can also be applied to a ceramic board having a long side of less than 100 mm or a short side of less than 50 mm. The difference in size between the ceramic substrate and the copper plate in the longitudinal and lateral directions of the bonded body is preferably within ±2 mm. The longitudinal and lateral sizes of the ceramic substrate and the copper plate are preferably substantially the same. In addition, in the bonded body, the copper plates are preferably bonded to both sides of the ceramic substrate. By bonding the copper plates to both sides, a pattern shape can be imparted to both the front and back copper plates. In addition, in the bonded body, the same surface of the ceramic substrate may have copper plate patterns at locations where the distance between the copper plate patterns is 2 mm or less. The distance between the copper plate patterns refers to the shortest distance between adjacent copper plates after a circuit pattern is provided by etching. When the copper plate side surface has an inclined shape, the shortest distance between the inclined shapes is the distance between the copper plate patterns. According to the method for manufacturing a ceramic circuit board of the embodiment, even fine patterns with a distance between copper plate patterns of 2 mm or less can be manufactured with a good yield. In other words, even if it is a large-sized substrate with a long side length of 100 mm or more and a ceramic circuit board with a distance between copper plate patterns of 2 mm or less, the yield is good. In addition, the distance between copper plate patterns of 2 mm or less means that the narrowest distance between patterns is 2 mm or less. In other words, as long as there is a place where the narrowest distance between patterns is 2 mm or less, there may be a place where the distance between patterns exceeds 2 mm.

[0014] FIG. 1 shows an example of a manufacturing process for a ceramic circuit board according to an embodiment. The manufacturing method according to the embodiment includes a step of preparing a ceramic copper bonded body having a copper plate bonded thereto, a first copper etching step, a first brazing material etching step, a first chemical polishing step, and a final cleaning step. In the first copper etching step, the copper plate and a layer mainly composed of at least one of copper tin and copper indium are etched. In the first brazing material etching step, an active metal reaction layer, which is a part of the brazing material layer, is etched with an etching solution having a pH of 4 to 12 and containing one or two selected from hydrogen peroxide and ammonium peroxodisulfate. In the first chemical polishing step, the end of the brazing material layer exposed by the first brazing material etching step is chemically polished. In the final cleaning step, the treated bonded body (ceramic circuit board) is cleaned.

[0015] In the first copper etching step, the copper plate in the ceramic copper joint and the layer mainly composed of copper tin or copper indium of the brazing material layer are etched. The copper plate is etched to form a pattern. In other words, after etching, the copper plate corresponding to the pattern remains, and the copper between the patterns is removed. In addition, the layer mainly composed of copper tin or copper indium is etched to expose the active metal reaction layer between the patterns of the copper plate. The layer mainly composed of copper tin or copper indium refers to an area containing 40% or more of one or both of copper tin and copper indium. Hereinafter, the layer mainly composed of copper tin or copper indium is called the "copper alloy layer". The active metal reaction layer is a part of the brazing material layer. The first copper etching step prepares a joint with the active metal reaction layer exposed. In the copper etching process, an etching resist is applied to the areas that are to be left as a pattern. In the copper etching process, an aqueous solution of iron chloride or copper chloride is mainly used. Iron chloride or copper chloride is effective for etching copper plates, copper layers, copper tin layers, copper indium layers, etc. On the other hand, iron chloride or copper chloride cannot etch active metal reaction layers that contain active metals. Therefore, the first copper etching process can leave areas where the active metal reaction layer is exposed. Because the brazing layer does not contain Ag, it is possible to etch both the copper plate and the copper alloy layer in a single etching process. If necessary, a cleaning step may be performed after the copper etching step. In addition, for etching the copper plate and the copper alloy layer, ferric chloride (FeCl3) may be used as the iron chloride, and copper chloride (I) (CuCl) may be used as the copper chloride. The concentration of the aqueous solution of iron chloride or copper chloride is not particularly limited, but is preferably 0.2 wt% or more. In this way, etching can be performed efficiently. The concentration of the aqueous solution is preferably 50 wt% or less. If the concentration exceeds 50 wt%, the etching speed cannot be adjusted, and overetching may occur. Even when copper chloride and iron chloride are mixed, it is preferable that the total concentration of the aqueous solutions is within the above-mentioned range. A more preferable range of the concentration of the aqueous solution containing iron chloride or copper chloride is 5 wt% or more and 40 wt% or less. The etching process of the copper plate and the copper alloy layer may be performed only once, or may be performed in two or more steps. Furthermore, after the first copper etching process, a small amount of the copper alloy layer may remain between the copper plate patterns.

[0016] In the next brazing material etching step, an active metal reaction layer, which is a part of the brazing material layer, is etched with an etching solution containing one or two selected from hydrogen peroxide and ammonium peroxodisulfate. The pH of the brazing material etching solution used in the brazing material etching process is preferably 4 or more. If the pH is less than 4, the brazing material layer may be etched too quickly. In order to improve the TCT characteristics of the ceramic circuit board, it is effective to leave the brazing material protruding portion (protruding portion of the bonding layer). The brazing material protruding portion refers to the portion that protrudes in the in-plane direction from the copper plate between the copper plate patterns when viewed in a plan view. The plan view refers to the view from a direction perpendicular to the ceramic substrate surface. The in-plane direction is the direction parallel to the ceramic substrate surface. If the etching rate of the brazing material layer is too fast, it becomes difficult to control the size of the brazing material protruding portion. In addition, the pH of the brazing material etching solution is preferably 12 or less. If the pH is greater than 12, the etching rate may be difficult to adjust because the solution is too alkaline. The relationship between the solution property and pH will be described. An aqueous solution with a pH of less than 7 is an acidic aqueous solution. An aqueous solution with a pH of 7 is a neutral aqueous solution. An aqueous solution with a pH of greater than 7 is a basic (alkaline) aqueous solution. Here, the properties of hydrogen peroxide and ammonium peroxodisulfate (whether they are acidic, neutral, or basic) will be considered. An aqueous solution of hydrogen peroxide is an acidic aqueous solution. An aqueous solution of ammonium peroxodisulfate is also an acidic aqueous solution. Therefore, in order to neutralize or basic the property of an aqueous solution containing one or two selected from hydrogen peroxide and ammonium peroxodisulfate, it is necessary to mix it with a basic aqueous solution, which may increase the amount of solute required and increase costs. As a method of making the etching solution basic by mixing it with a basic solution, for example, a method of mixing it with sodium hydroxide or the like to adjust the pH can be mentioned. In order to adjust the pH to a basic aqueous solution of 12 or less, it becomes necessary to add other components. Considering the cost, it is preferable that the liquid is acidic (pH less than 7). When the brazing material etchant is acidic (pH less than 7), the etching rate of the brazing material layer slows down if the pH is greater than 6. Therefore, the pH of the brazing material etchant is more preferably 4.0 or more and 6.0 or less. The pH of the brazing material etchant is more preferably from 4.0 to 5.8, in which case both the protruding brazing material portion and the etching rate can be controlled. It is more preferable to mix a fluorine-containing compound into an etching solution having a pH of 4 or more and containing one or two selected from hydrogen peroxide and ammonium peroxodisulfate. Examples of the fluorine-containing compound include fluoroboric acid, ammonium fluoride, hydrogen fluoride, hexafluorophosphoric acid, and trifluoroacetic acid (TFA). The fluorine-containing compound is preferably a fluoride. Among the fluorides, it is more preferable to contain one or more selected from fluoroboric acid, ammonium fluoride, and hydrogen fluoride. In addition, none of the above-mentioned fluorides is a strong base. Therefore, it is difficult to adversely affect the control of the pH. "One or more" means that only one type may be used, or two or three types may be mixed. Furthermore, an etching solution containing one or two members selected from hydrogen peroxide and ammonium peroxodisulfate and having a pH of 4 or more preferably contains a pH stabilizer. The etching solution having a pH of 4 or more and containing one or two selected from hydrogen peroxide and ammonium peroxodisulfate preferably contains hydrogen peroxide and ammonium fluoride as a fluorine-containing compound, and more preferably contains a pH stabilizer in the aqueous solution containing hydrogen peroxide and ammonium fluoride.

[0017] Hydrogen peroxide (H2O2) or ammonium peroxodisulfate ((NH4)2S2O8) has the effect of removing Cu. These components can ionize and remove Cu. The effect of ionization is enhanced by making the liquid acidic (especially pH 6 or less). Hydrogen peroxide or ammonium peroxodisulfate also has the effect of acting as an oxidizing agent to oxidize active metals, Sn, In, and carbon. For example, when Ti is used as the brazing material, TiN (titanium nitride) is formed on the nitride ceramic substrate. The above-mentioned etching components have the effect of changing Ti or TiN to TiO2. Similarly, they have the effect of changing Sn or Sn nitride in the brazing material to SnO2. The same applies to In, etc. Therefore, the etching solution containing hydrogen peroxide or ammonium peroxodisulfate is effective for removing the active metal reaction layer. Also, even if a small amount of copper alloy layer remains after etching the copper member and the copper alloy layer, the etching solution containing hydrogen peroxide or ammonium peroxodisulfate can remove the remaining copper alloy layer. The hydrogen peroxide preferably has the quality specified in JIS-K-1463 (2007), which is based on ISO 6352-2, and the ammonium peroxodisulfate preferably has the quality specified in JIS-K-8252 (2010). Ammonium fluoride (NH4F) acts as an oxide etchant. It can convert active metal oxides from oxides to compounds or ions that contain fluorine atoms. For example, TiO2 can be converted to TiOF2 or TiF6. 2- It can be removed by changing it into ammonium hydrogen fluoride ((NH4)HF2). Ammonium fluoride also includes ammonium hydrogen fluoride ((NH4)HF2). As mentioned above, oxides such as TiO2 are formed by oxidizing agents such as hydrogen peroxide (H2O2) or ammonium peroxodisulfate ((NH4)2S2O8), and can also be formed when bonding with oxide ceramics.

[0018] The pH stabilizer can stabilize the pH of a mixed solution of ammonium fluoride and one or two selected from hydrogen peroxide and ammonium peroxodisulfate. The pH stabilizer is preferably one or more selected from HBF4, EDTA, NTA, CyDTA, DTPA, TTHA, GEDTA, glycine, dicarboxylic acid, tricarboxylic acid, oxycarboxylic acid, and salts thereof. These pH stabilizers can adjust the pH to within the range of 4 to 6. The pH stabilizer is preferably HBF4. By using HBF4, the pH can be adjusted to 4.0 or more and 5.8 or less. HBF4 is tetrafluoroboric acid. HBF4 is also called hydroboric acid.

[0019] HBF4 may be combined with one or more selected from EDTA, NTA, CyDTA, DTPA, TTHA, GEDTA, glycine, dicarboxylic acids, tricarboxylic acids, oxycarboxylic acids, and salts thereof. EDTA, NTA, CyDTA, DTPA, TTHA, GEDTA, glycine, dicarboxylic acid, tricarboxylic acid, oxycarboxylic acid, and their salts are called chelating agents. Chelating agents have the effect of suppressing the precipitation of Cu. The brazing material layer contains Cu. As etching of the brazing material layer proceeds, Cu ions increase in the etching solution. When the Cu ions exceed a certain amount, Cu precipitates. When Cu that has been etched once precipitates again, the etching rate decreases. In addition, the pH of the etching solution can be lowered by adding a chelating agent. As the chelating agent, one selected from CyDTA, glycine, dicarboxylic acid, tricarboxylic acid, oxycarboxylic acid, and their salts is preferable. These chelating agents are materials that easily form complex ions with Cu ions. In addition, when one selected from CyDTA, glycine, dicarboxylic acid, tricarboxylic acid, oxycarboxylic acid, and their salts is used as the chelating agent, the content in the etching solution is preferably 0.01 wt% or more and 5 wt% or less. This content makes it possible to adjust the pH of the etching solution to within the range of 4.0 to 5.8.

[0020] When the total mass of hydrogen peroxide, ammonium fluoride, and pH stabilizer is 100 wt%, the hydrogen peroxide content is preferably 5 wt% or more and 90 wt% or less. The ammonium fluoride content is preferably 2 wt% or more and 45 wt% or less. The pH stabilizer content is preferably 2 wt% or more and 50 wt% or less. Within this range, the role of each component can be fully utilized. In addition, the oxidation-reduction potential (ORP) can be increased when etching the brazing material. This can increase the rate of brazing material etching.

[0021] The hydrogen peroxide, ammonium fluoride and pH stabilizer are preferably mixed as aqueous solutions. In the hydrogen peroxide-containing aqueous solution, the hydrogen peroxide content is preferably 5 wt% or more and 70 wt% or less. In the ammonium fluoride-containing aqueous solution, the ammonium fluoride content is preferably 5 wt% or more and 60 wt% or less. In the pH stabilizer-containing aqueous solution, the pH stabilizer content is preferably 5 wt% or more and 60 wt% or less. A brazing material etchant is prepared by mixing an aqueous solution containing hydrogen peroxide, an aqueous solution containing ammonium fluoride, and an aqueous solution containing a pH stabilizer. The brazing material etchant may be diluted by mixing with water. When the total amount of the aqueous solution containing hydrogen peroxide, the aqueous solution containing ammonium fluoride, and the aqueous solution containing a pH stabilizer is 1 L (liter), 0.5 to 2 L of water may be mixed. It is also preferable to thoroughly stir and mix uniformly. Examples of methods for stirring and mixing include a method of mixing by rotating a stirrer such as a magnetic stirrer, a method of stirring using a stirrer, and a method using a pump. The quality of the water preferably satisfies JIS-K-0557 (1998). JIS-K-0557 specifies qualities of A1 to A4. For JIS-K-0557, ISO3696 is referred to. Furthermore, the smaller the amount of impurities contained in the total components of the etching solution used, the better. By reducing the impurities contained in the etching solution, the number of times the solution needs to be replaced can be further reduced. In addition to the water added to the etching solution, it is preferable that the solution also has a high purity.

[0022] When the total mass of ammonium peroxodisulfate, ammonium fluoride, and pH stabilizer is taken as 100 wt%, the content of ammonium peroxodisulfate is preferably 20 wt% to 95 wt%, the content of ammonium fluoride is 3 wt% to 55 wt%, and the content of pH stabilizer is 2 wt% to 60 wt%. Within these ranges, the role of each component can be fully utilized. In addition, the oxidation-reduction potential (ORP) can be increased when etching the brazing material. By increasing the oxidation-reduction potential (ORP), the etching speed increases. Therefore, by increasing the oxidation-reduction potential (ORP), the speed of brazing material etching can be increased while being controlled to a level that allows the protruding brazing material to be left.

[0023] The brazing material etching solution is prepared by mixing an aqueous solution containing ammonium peroxodisulfate, an aqueous solution containing ammonium fluoride, and an aqueous solution containing a pH stabilizer. The brazing material etching solution may be diluted by mixing with water. When the total amount of the aqueous solution containing ammonium peroxodisulfate, the aqueous solution containing ammonium fluoride, and the aqueous solution containing a pH stabilizer is 1L (liter), 0.5L to 2L of water may be mixed. In addition, it is preferable to thoroughly stir and mix uniformly. The water is preferably pure water that satisfies the quality of JIS-K-0557 (1998). JIS-K-0557 specifies qualities of A1 to A4. The etching time can be shortened by etching the brazing material layer using the brazing material etchant containing hydrogen peroxide or ammonium peroxodisulfate described above. If the brazing material layer is 60 μm thick or less, it can be etched in 30 minutes or less.

[0024] The brazing material etching step is preferably performed while applying ultrasonic waves to the bonded body through a brazing material etching solution. Here, ultrasonic waves are defined as sound waves with a frequency of 10 kHz or more. The frequency of the ultrasonic waves is preferably 10 kHz or more and 100 kHz or less. If the frequency is less than 10 kHz, the effect of applying the ultrasonic waves may not be sufficient. On the other hand, if the frequency is greater than 100 kHz, the effect of applying the ultrasonic waves may be too large, making it difficult to control the etching rate. By performing the brazing material etching step while applying ultrasonic waves, the brazing material etching time can be further shortened. By performing the brazing material etching step while applying ultrasonic waves, the time for one brazing material etching step can be reduced to 15 minutes or less. The lower limit of the brazing material etching step time is not particularly limited, but is preferably 1 minute or more. If it is less than 1 minute, the effect of removing the brazing material layer and the effect of oxidizing the brazing material layer are likely to be insufficient. If these effects are small, the third or subsequent brazing material etching steps may be required. If the number of brazing material etching steps increases, the manufacturing equipment for ceramic circuit boards will become larger. When the brazing material etching step is performed two or more times, the brazing material etching solution and etching conditions (temperature, time, ultrasonic waves, etc.) may be changed. In the brazing material etching process, it is also effective to heat the brazing material etching solution to 30°C or more and 70°C or less. By heating, the kinetic energy of the molecules contained in the etching solution can be increased, and the etching reaction of the brazing material can be activated. On the other hand, if the heating temperature is higher than 70°C, the etching speed may become too fast and uncontrollable. Therefore, when heating the etching solution, it is preferable to keep it at 70°C or less. In addition, during heating, a constant temperature may be maintained at all times, or heating may be performed only when necessary so that the temperature is between 30°C and 70°C. The amount of brazing material etching solution is set to an amount that completely immerses the bonded body. In addition, it is preferable that the aqueous solutions are not mixed as much as possible during each etching step and between the etching step and the chemical polishing step. If the aqueous solutions are mixed, when a large amount of the aqueous solution used in the previous step is attached to the substrate surface, the components of the solution may adversely affect the next step. Therefore, a cleaning step may be inserted between each etching step and between the etching step and the chemical polishing step. If a cleaning step is not performed, the substrate may be tilted so that the aqueous solution components fall, or a draining basket or a net may be used to allow the aqueous solution components to fall. Alternatively, the substrate may be naturally dried, or the aqueous solution may be blown off by blowing air, nitrogen, or an inert gas.

[0025] After the brazing material etching step, a chemical polishing step is performed. The chemical polishing step includes a step of chemically polishing the end of the brazing material layer. If the brazing material layer is not completely removed after the chemical polishing step, it is effective to perform the brazing material etching step again. It is also more preferable to perform a cleaning step after the brazing material etching step and after the chemical polishing step. By performing the cleaning step, it is possible to prevent the brazing material etching solution or the chemical polishing solution from remaining and adversely affecting the next step. In the brazing material layer, copper ions may receive electrons during etching of the active metal reaction layer, and copper may precipitate. This copper precipitation is due to the fact that copper ions have a higher redox potential than titanium and hydrogen ions and are more likely to receive electrons. In other words, the ionization tendency of copper is smaller than that of titanium and hydrogen. Here, the ionization tendency refers to the ease with which an atom becomes a monovalent cation. In other words, atoms with a smaller ionization tendency are less likely to become ions and more likely to receive electrons. Copper ions are generated from copper in the copper plate or brazing material. If precipitated copper is present, the shape and length of the protruding portion cannot be controlled. Therefore, in the chemical polishing process, it is necessary to remove the copper precipitated at the end of the brazing material layer. In the chemical polishing process, it is preferable to use a chemical polishing solution containing sulfuric acid or hydrochloric acid. The chemical polishing solution may contain both sulfuric acid and hydrochloric acid, but it is preferable to contain only one of sulfuric acid and hydrochloric acid. The chemical polishing solution is preferably an aqueous solution of sulfuric acid, an aqueous solution of hydrochloric acid, or an aqueous solution of sulfuric acid and hydrogen peroxide. The sulfuric acid aqueous solution also includes an aqueous solution containing a sulfate such as sodium thiosulfate (Na2S2O3). The quality of sulfuric acid preferably satisfies JIS-K-8951 (2006). The quality of hydrochloric acid preferably satisfies JIS-K-8180 (2015). JIS-K-8951 and JIS-K-8180 correspond to ISO6352-2. The quality of sodium thiosulfate preferably satisfies JIS-K-8638 (2011). For JIS-K-8638, ISO6352-2 is referred to.

[0026] For the sulfuric acid aqueous solution, the sulfuric acid concentration is preferably in the range of 0.5 wt% to 25 wt%. For the hydrochloric acid aqueous solution, the hydrochloric acid concentration is preferably in the range of 0.5 wt% to 20 wt%. For the aqueous solution of a mixture of sulfuric acid and hydrogen peroxide, the total of sulfuric acid and hydrogen peroxide is preferably in the range of 0.5 wt% to 30 wt%. If the concentration is less than 0.5 wt%, the effect of chemical polishing may be insufficient. If the concentration is more than 30 wt%, the effect of chemical polishing may be too high. If the effect of chemical polishing is too high, it becomes difficult to adjust the size of the protruding portion of the brazing material. For this reason, the concentrations of sulfuric acid, hydrochloric acid, and hydrogen peroxide are preferably in the range of 0.5 wt% to 20 wt%. More preferably, each concentration is in the range of 1 wt% to 10 wt%. In addition, when a sodium thiosulfate aqueous solution is used as the sulfuric acid aqueous solution, it is preferable to add a chelating agent of 0.01 wt% to 1 wt%. The pH can be lowered by adding a chelating agent.

[0027] It is preferable that one chemical polishing process is 5 minutes or less. If it is longer than 5 minutes, there is a possibility that the copper plate surface will become rough. If it is 5 minutes or less, the surface roughness Ra of the copper plate will be 2 μm or less. In addition, if the chemical polishing process time is 20 seconds or more and 2 minutes or less, the copper plate can maintain a flat surface with a surface roughness Ra of 1 μm or less. Therefore, even if the etching resist applied to the copper plate surface is peeled off during the copper etching process before the brazing material etching process, the copper plate can have a flat surface with a surface roughness Ra of 0.1 μm or more and 1 μm or less. This makes it possible to avoid problems caused by the reaction between the etching resist and the brazing material etching solution or the etching resist and the chemical polishing solution. Two or more kinds of chemical polishing liquids may be used in one chemical polishing step. That is, in one chemical polishing step, chemical polishing may be performed using a chemical polishing liquid containing a certain component, and then chemical polishing may be performed using a chemical polishing liquid containing another component. When two or more chemical polishing steps are performed, the chemical polishing liquid and conditions (such as time) may be changed for each step. In addition, by performing a second brazing material etching step, the shape of the protruding portion can be adjusted. Therefore, it is preferable to perform a second brazing material etching step as necessary. In addition, it is more preferable to have a second chemical polishing step after the second brazing material etching step, as after the first brazing material etching step. By having such a second chemical polishing step, the copper precipitated in the second brazing material etching step can be removed. Here, the difference between chemical polishing and etching will be explained. "Chemical polishing" refers to a process in which the amount of removed is smaller than that of the process expressed as "etching". When etching or chemical polishing is performed using the above-mentioned solution in this way, a plurality of bonded bodies may be etched or chemically polished at the same time, or the bonded bodies may be etched or chemically polished one by one. The number of bonded bodies to be simultaneously subjected to each step is not particularly limited. In the process using each etching solution or chemical polishing solution, the method of using the solution is not particularly limited. In the etching or solution chemical polishing process, the bonded body may be placed in any orientation relative to a container containing each solution, or each solution may be sprayed onto the bonded body like a spray. The final cleaning process is the last cleaning process. Hereinafter, the final cleaning process may be simply called the cleaning process. In the cleaning process, one or more types of cleaning selected from water cleaning, alkali cleaning, and alcohol cleaning are performed. Water cleaning can be classified into immersion type and water flow type. The immersion type is a method in which the bonded body is immersed in a cleaning tank filled with water. The water flow type is a method in which a flow is imparted to the cleaning water. The water flow type includes a shower type and a method in which a water flow is imparted to the cleaning water in the cleaning tank. In the method of providing a nozzle to adjust the flow rate, a nozzle may be provided on both the front and back sides of the substrate to clean both the front and back sides at the same time. By cleaning both the front and back sides at the same time in this way, the bonded body can be cleaned more efficiently. A cleaning step may be provided after the etching step and after the chemical polishing step. In such a cleaning step, normal water cleaning may be performed, or water cleaning with a controlled flow rate may be performed. The normal cleaning step is a method of immersing the bonded body in a water cleaning tank. As described above, when the bonded body is immersed in pure water, the immersion time may be 10 seconds to 10 minutes. Each cleaning step may be either a batch type or a continuous type. The batch type is a method of storing a plurality of bonded bodies in a cleaning basket and performing the cleaning step. The continuous type is a method of carrying out the cleaning step while transporting a plurality of bonded bodies on a belt conveyer. When performing cleaning, ultrasonic waves may be applied via water. The application of ultrasonic waves is expected to have the effect of increasing the cleaning efficiency. In addition, each etching step or chemical polishing step may be performed by using a cleaning method. About If an etching step or a chemical polishing step is carried out as the next step, a small amount of the solution component of the next step may be added to the cleaning water in order to prevent the solution of the next step from being diluted by cleaning. When only water washing is performed, it is preferable that a water flow type water washing step is performed at least once. In particular, it is preferable that the final washing step is a water flow type water washing step. In the washing step when only water washing is performed, the number of water flow type washing steps may be large. In addition, a plurality of washing methods may be combined in one washing step. It is preferable that these washings are performed not only on the conductor portion but also on the entire bonded body. In addition, by performing washing between each etching step and between the etching step and the chemical polishing step, it is possible to prevent aqueous solutions of different compositions from mixing with each other, and it is possible to reduce the number of times that the etching solution is replaced or the number of times that chemical solutions are added for adjusting the components. Therefore, it is more preferable to provide a washing step between each etching step and between the etching step and the chemical polishing step. In the water washing, the flow rate is preferably 1.3 L (liters) / min or more. If the flow rate is 1.3 L / min or more, the effect of washing away the components of the aqueous solution attached to the copper plate surface can be sufficiently obtained. If the flow rate is less than 1.3 L / min, the washing effect may be insufficient. For example, in a method in which the bonded body is immersed in a washing tank filled with water and left there, the flow rate is insufficient and the effect of washing away the components of the aqueous solution cannot be sufficiently obtained. The upper limit of the flow rate is not particularly limited, but it is preferably 10 L / min or less. If the flow rate is greater than 10 L / min, the water pressure may be too high and the copper plate surface may be deformed. For this reason, the flow rate of the water washing is preferably 1.3 L / min or more and 10 L / min or less. More preferably, the flow rate of the water washing is 1.5 L / min or more and 6 L / min or less. Methods for adjusting the flow rate include a method of controlling the flow rate by circulating the water stored in the cleaning tank, and a method of controlling the flow rate using a nozzle. The method of controlling the flow rate using a nozzle is preferable. It is easier to control the flow rate when a nozzle is used. When circulating the water stored in the cleaning tank, it may be difficult to control the flow rate when the amount of water is large. When a nozzle is used, the flow rate of the water sprayed from the nozzle is set to 1.3 L / min or more. Ultrasonic waves may be applied to the water, and carbon dioxide or oxygen may be dissolved in the water. The distance between the nozzle and the bonded body is preferably in the range of 5 cm to 40 cm. It is more preferable that the distance is in the range of 5 cm to 20 cm. If the distance is in this range, it is easy to adjust the amount of water hitting the bonded body. The shape of the water sprayed from the nozzle can be various shapes such as a dot shape, a circle shape, an ellipse shape, a flat shape, a square shape, etc. The nozzle shape can be various shapes such as a cone shape, a fan shape, etc. When using a nozzle, multiple nozzles may be used per bonded body, and the front conductor part and the back conductor part may be washed simultaneously. In addition, it is preferable that the washing is performed on the entire surface of the bonded body. In the method of providing a nozzle to adjust the flow rate and washing the entire surface of the bonded body in this way, a method of providing nozzles on both the front and back sides of the substrate and washing the front and back sides at the same time may be used. By washing the front and back sides at the same time in this way, it is possible to wash more efficiently. The amount of water that hits the joint is 0.01 L / (min cm) per nozzle. 2 ) or more 0.1L / (min cm 2 The amount of water that hits the bonded body is called the impact water amount. The impact water amount is the amount of water that hits the bonded body when viewed from above. 2 The amount of water that lands on the bonded body can be adjusted by adjusting the amount of water from the nozzle, the nozzle type, the distance from the nozzle, and the like. Air can also be sprayed when spraying water from the nozzle. Ultrasonic waves may be applied in the cleaning process. It is also effective to perform the cleaning process while transporting the bonded body. In this case, the bonded body may be tilted to improve cleaning efficiency (liquid recovery efficiency) and installation area efficiency. "Tilt" means that at least one side of the bonded body is not parallel to a horizontal plane perpendicular to the direction of gravity. It is more preferable that the angle between the horizontal plane and the at least one side is 10 degrees or more and less than 90 degrees. The flow rate from the nozzle is 1.3 L / min or more, and the amount of water that lands on the bonded body is 0.01 L / min / cm per nozzle while transporting the bonded body. 2 More than 0.1L / min / cm 2 It is efficient to keep the value within the following range.

[0028] The quality of the water preferably satisfies JIS-K-0557 (1998). JIS-K-0557 specifies qualities of A1 to A4. For JIS-K-0557, ISO3696 is referenced. Alkaline washing refers to the process of washing the conjugate with an alkaline aqueous solution of pH 10 or more. Examples of alkaline aqueous solutions of pH 10 or more include aqueous solutions of organic alkali, metal hydroxides, and salts of metal hydroxides and weak acids. In particular, when metal hydroxides and their salts are used, examples of the metals used include lithium, potassium, sodium, barium, calcium, etc. b If the base dissociation constant is too small, the amount of solute required increases, so the metal type of the metal hydroxide and its salt to be used is preferably selected from potassium, sodium and lithium. In particular, taking cost into consideration, sodium hydroxide, sodium metasilicate, sodium carbonate, sodium phosphate, and sodium pyrophosphate are preferred, and an aqueous solution containing one or more selected from these sodium compounds is preferred. An aqueous solution containing 0.5% by mass to 5% by mass of these components is more preferred. Alkaline washing has the effect of removing organic matter such as resist on the copper plate surface and suppressing contamination of the etching solution. It is preferable that the purity of these alkaline aqueous solutions is high. It is more preferable that the purity is 96% by mass or more. If the purity is less than 96% by mass, the frequency of changing the cleaning solution may increase. It is even more preferable that the purity is 98% by mass or more. This purity (mass %) is the value obtained by dividing the sum of the mass of the solvent and the alkaline compound (or the sum of the compounds if they are mixed) by the total mass of the aqueous solution and multiplying the result by 100 to obtain a percentage. Organic compounds are often used in resists. The polarity of organic compounds is lower than that of water, so organic compounds have the property of dissolving in organic solvents. Therefore, when organic compounds are used in resists, cleaning with alcohols or ketones may be performed. Examples of alcohols include isopropanol, methanol, butanol, hexanol, and ethanol. Examples of ketones include acetone. Considering the solubility and volatility of organic compounds, ethanol or isopropanol is preferable. Isopropanol has a CAS registration number of 67-63-0 and its IUPAC name is 2-propanol. Isopropanol is also called IPA or isopropyl alcohol. The purity of these alcohols excluding water and solvent components is preferably 99% by mass or more. If the purity of the alcohols or ketones used for cleaning excluding water and solvent components is less than 99% by mass, the cleaning solution may need to be replaced more frequently. In addition, in the alcohol cleaning, two or more kinds of alcohols may be mixed. Furthermore, alcohol may be mixed with water. When alcohol is mixed with water, the quality of the water used preferably satisfies JIS-K-0557 (1998). A ketone such as acetone may be added to the alcohol as a solvent. In other words, the solution used in the alcohol cleaning preferably has an impurity content of 1 mass % or less excluding water or solvent. Cleaning using alcohols is called alcohol cleaning. Considering the cost, the cleaning method is preferably alkaline cleaning or water cleaning rather than alcohol cleaning. In addition, a combination of multiple cleaning methods may be used, such as alkaline cleaning followed by water cleaning. In addition, it is preferable to provide a drying step after these cleaning steps. By carrying out the above-mentioned cleaning step, the number of times the etching solution needs to be replaced can be reduced. In addition, the cleaning step is preferably carried out after the step of removing the resist. When the step of removing the resist is carried out multiple times, it is preferable to carry out the cleaning step each time. The above cleaning method is preferably carried out as a finishing cleaning step. The finishing cleaning step is the cleaning step carried out last in the manufacturing process of a ceramic circuit board. For example, when a resist removal step is carried out last, the cleaning after the last resist removal step is carried out by the above cleaning method, and the cleaning after the other resist removal steps may be normal water cleaning. In this case, it is preferable to set the time of the cleaning step after the last resist removal step longer than the time of the other cleaning steps. As a cleaning method, there is also a method using a chlorine-based cleaning agent. The amount of chlorine on the copper plate surface may increase with a chlorine-based cleaning agent. The increase in the amount of chlorine may have a negative effect on the reliability of the bond when a circuit board is bonded to the bonding layer or plating film of a semiconductor element. Therefore, the use of a chlorine-based cleaning agent is less preferable than the above-mentioned cleaning methods. In addition, a cleaning process using water vapor or ozone water is not preferable because it may oxidize the copper plate. For this reason, a cleaning process using water cleaning, alkali cleaning, or alcohol cleaning is preferable. The above steps allow the manufacture of a ceramic circuit board according to the embodiment. Specifically, a pattern shape is imparted to the copper member by at least one copper etching step, and the brazing material layer is divided by at least one brazing material etching step, so that the bonded body is processed into a ceramic circuit board. The brazing material layer may be divided by a chemical polishing step after the brazing material etching step, and the bonded body may be processed into a ceramic circuit board.

[0029] The drying step may be natural drying. For efficient drying, it is preferable to perform at least one or more treatments with a solution that easily volatilizes, centrifugal force treatment, air blowing treatment, etc. in the drying step. In addition, when one or more cleaning steps are performed, it is preferable to have at least one or more drying steps after the cleaning step. The timing of this drying step is preferably particularly after the finishing cleaning step. When water is used in the cleaning step, for example, if a large amount of this water adheres to the bonded body, there is a possibility that the components of the etching solution or chemical polishing solution will be diluted when the next step is performed. This may increase the number of times the solution in the next step is replaced compared to when there is no drying step. When there is a drying step after the finishing cleaning step, the bonded body is dried more efficiently than natural drying, thereby improving the yield. In addition, efficient drying results in a shorter time of contact with oxygen than when natural drying is used, and therefore there is less oxidation. Examples of the drying process include a treatment with a volatile solution, a centrifugal force treatment, and an air blowing treatment. A plurality of drying processes may be combined. The bonded body after cleaning may be washed with a volatile solvent such as alcohols such as methanol, ethanol, and isopropanol, or ketones such as acetone to wash away remaining water. The alcohols and ketones may be mixed. In this case, isopropanol is preferably used in consideration of safety aspects such as flammability. The bonded body after cleaning may be rotated and centrifugal force may be used to remove remaining water droplets. The bonded body may be tilted. This tilt refers to a state in which, when any direction on a plane perpendicular to the direction of gravity is taken as the horizontal direction, the direction of one or more sides of the bonded body is not parallel to this horizontal direction. In this case, when the angle between the horizontal direction and the direction of gravity is taken as 90 degrees, it is more preferable that the angle between the horizontal direction and the direction of one or more sides of the bonded body is 10 degrees or more and 90 degrees or less. It is more preferable that the orientation of the bonded body is tilted. By tilting the orientation of the bonded body in this way, water droplets attached to the bonded body are more likely to fall due to gravity. For example, a method of tilting the bonded body may be to make the diagonal line of the bonded body tilted. The bonded body may also be dried by standing it up so that its diagonal line is approximately parallel to the direction of gravity. It is preferable to blow dry air or nitrogen gas onto the bonded body that has been dried to a certain extent in this way to blow off any remaining water droplets. The method of blowing air, dry air, or nitrogen gas is sometimes called an air knife. This air knife is a type of air blower. In order to dry the bonded body obtained in this manner more reliably, wind having a temperature of 10° C. or more and a humidity of 70% or less may be blown onto the bonded body at a wind speed of 20 m / s to 150 m / s. The drying process of blowing wind onto the bonded body in this manner is called air blowing. The preferable temperature of the wind in this air blowing process is 10° C. or more and 150° C. or less, and more preferably 15° C. or more and less than 100° C. If the temperature exceeds this temperature, the surface of the copper member may be oxidized by heat. The preferable humidity in the air blowing process is 5% to 70%. If the humidity is more than 70%, the time required for the drying process may be long. To reduce the humidity to less than 5%, the cost may increase. The wind speed is preferably 20 m / s to 150 m / s. The wind speed is more preferably 20 m / s to 100 m / s. If the wind speed is too low, it takes a long time to dry. If the wind speed is too high, it may have a negative effect on the transportation of the copper plate. When carrying out this drying process, by combining it with other drying processes, the drying time for applying hot air when using a hot air drying process can be shortened, and oxidation of the copper plate surface, which is the conductor, due to the heat of the hot air can be suppressed. For this reason, multiple drying processes may be combined.

[0030] FIG. 1 is a process diagram illustrating a method for manufacturing a ceramic circuit board according to a first embodiment. The manufacturing method according to the first embodiment includes a step of preparing a bonded body, a first copper etching step 1-1, a first cleaning step 4-1, a first brazing material etching step 2-1, a first chemical polishing step 3-1, and a finish cleaning step 5. In the bonded body, a ceramic substrate and a copper member are bonded to each other. In the first copper etching step, the copper member and the copper alloy layer are etched. In the first cleaning step 4-1, the joined body treated in the first copper etching step is cleaned. In the first brazing material etching step, the active metal reaction layer exposed by the first copper etching step is etched. In the first chemical polishing step, the copper precipitated on the end of the brazing material layer exposed by the first brazing material etching step is removed. In the final cleaning step, the joined body (ceramic circuit board) is cleaned. If necessary, one or more of a cleaning step and a drying step may be performed between the first brazing material etching step and the first chemical polishing step. The term "one or more" means that both a drying step and a cleaning step may be performed. FIG. 2 is a process diagram illustrating a method for manufacturing a ceramic circuit board according to the second embodiment. The manufacturing method according to the second embodiment differs from the first embodiment in that two cleaning steps are performed before the final cleaning step. The manufacturing method according to the second embodiment includes a first copper etching step 1, a first cleaning step 4-1, a first brazing material etching step 2-1, a second cleaning step 4-2, a first chemical polishing step 3-1, and a final cleaning step 5-1. A cleaning step is provided after each of the first brazing material etching step 2-1 and the first chemical polishing step 3-1. By performing each cleaning step, it is possible to prevent the etching solution or chemical polishing solution from remaining in the bonded body. In addition, after the cleaning step, a drying step is performed as necessary. FIG. 3 is a process diagram illustrating a method for manufacturing a ceramic circuit board according to a third embodiment. The manufacturing method according to the third embodiment includes a first copper etching step 1, a first brazing material etching step 2-1, a first chemical polishing step 3-1, a second brazing material etching step 2-2, and a second chemical polishing step 3-2. As shown in FIG. 3, the brazing material etching step and the chemical polishing step may be repeated. The brazing material etching step and the chemical polishing step are performed alternately. A cleaning step may be performed between the brazing material etching step and the chemical polishing step. The manufacturing method according to the third embodiment is effective when the brazing material layer cannot be sufficiently removed by the first brazing material etching step 2-1 and the first chemical polishing step 3-1. The components of the brazing material etching solution used in the second brazing material etching step 2-2 may be the same as or different from the components of the brazing material etching solution used in the first brazing material etching step 2-1. The components of the chemical polishing solution used in the second chemical polishing step 3-2 may be the same as or different from the components of the chemical polishing solution used in the first chemical polishing step 3-1. After the second chemical polishing step 3-2, a brazing material etching step and a chemical polishing step may be further performed. Between the brazing material etching step and the chemical polishing step, one or more of a cleaning step and a drying step may be performed. 4 is a process diagram illustrating a method for manufacturing a ceramic circuit board according to the fourth embodiment. Compared with the third embodiment, the manufacturing method according to the fourth embodiment further includes a finish cleaning step 5-1 and a finish drying step 5-2. The finish cleaning step 5-1 is performed after the last chemical polishing step. The finish drying step 5-2 is performed after the finish cleaning step 5-1. FIG. 5 is a process diagram illustrating a method for manufacturing a ceramic circuit board according to the fifth embodiment. Compared with the third embodiment, the manufacturing method according to the fifth embodiment further includes a second copper etching step 1-2. The second copper etching step is performed after the first chemical polishing step. As shown in FIG. 5, after the second copper etching step 1-2, a second brazing material etching step 2-2 and a second chemical polishing step 3-2 may be performed. Thereafter, a final cleaning step 5-1 and a final drying step 5-2 may be performed, similarly to the example shown in FIG. 4. Other steps for the ceramic circuit board obtained by the manufacturing method according to the embodiment are not particularly limited. For example, a step of applying a rust inhibitor may be provided before the finishing cleaning step, or a step of plating the obtained circuit board may be provided. In addition, a semiconductor element may be directly mounted on a copper member to which a pattern shape has been imparted to form a semiconductor device, or a semiconductor element may be mounted via a solder layer or a silver layer. The rust inhibitor used may be a benzotriazole-based compound or a non-benzotriazole-based compound. The timing of the step of applying the rust inhibitor is not particularly limited, but it is more preferable to provide a finishing cleaning step after applying the rust inhibitor.

[0031] 6(a) to 6(d) are cross-sectional views illustrating the manufacturing process of the ceramic circuit board according to the embodiment. In Fig. 6(a) to 6(d), 10 is a bonded body, 11 is a ceramic substrate, 12 is a brazing material layer, and 13 is a copper plate. The brazing material layer 12 includes a copper alloy layer 12a and an active metal brazing material layer 12b. The active metal brazing material layer 12b is located between the ceramic substrate 11 and the copper alloy layer 12a. FIG. 6(a) illustrates a prepared joint. A copper plate is joined to one surface of a ceramic substrate via a brazing material layer. A part of the copper plate is removed by a first copper etching process. As shown in FIG. 6(b), the active metal brazing material layer is exposed between the patterns provided on the copper plate. For convenience of explanation, the copper member divided into several parts by etching and provided with a circuit shape is also referred to as a "copper plate". FIG. 6(c) illustrates a state in which a part of the exposed active metal brazing material layer is removed by a first brazing material etching process. At the end of the brazing material layer 12, there is a precipitate 12c in which Cu in the etching solution is precipitated. FIG. 6(d) illustrates a state after a first chemical polishing process. The precipitate 12c at the end of the brazing material layer is removed by a first chemical polishing process. After the precipitate is removed, the part of the brazing material layer 12 that protrudes laterally from the copper plate is the brazing material protruding part 12d. For example, in the bonded body shown in FIG. 6(c) and FIG. 6(d), the patterns are electrically insulated from each other, forming a ceramic circuit board. Although not shown, if there is a possibility that the brazing material layer remains after the first brazing material etching step, a second brazing material etching step and a second chemical polishing step may be performed as exemplified in FIG. 3 and FIG. 4. If necessary, a third brazing material etching step and a third chemical polishing step may be performed after the second brazing material etching step. Also, FIG. 6 shows an etching step for the copper plate and brazing material layer provided on the front surface of the ceramic substrate. If a copper plate is also bonded to the rear surface of the ceramic substrate via a brazing material layer, an etching step can be performed on the copper plate and brazing material layer on the rear surface as necessary. Also, when the concentration of the brazing material etching solution changes due to the continuous production of a plurality of ceramic circuit substrates, a necessary amount of etching solution is added. The same applies to the chemical polishing solution.

[0032] As a guide for the change in concentration of the brazing material etching solution, when the hydrogen peroxide concentration drops by 10 to 20 wt% from the initial concentration, it is effective to add hydrogen peroxide to make up for the drop. The same applies when ammonium peroxodisulfate is used. Hydrogen peroxide or ammonium peroxodisulfate functions as an ionizer or oxidizer for the active metal brazing material layer components. The etching process of the active metal brazing material layer begins when these functions are fulfilled. Since hydrogen peroxide or ammonium peroxodisulfate are consumed first, the change in their concentrations is the most significant in the etching solution composition. Therefore, it is preferable to check these concentration changes and use them as a guide for refilling. In addition, as hydrogen peroxide or ammonium peroxodisulfate decreases, the pH of the brazing material etching solution changes. It is also effective to measure the pH of the brazing material etching solution and refill it accordingly. The amount of brazing material etchant consumed varies depending on the area of ​​the active brazing material layer to be etched. When etching multiple ceramic circuit boards at once, the total area of ​​the active brazing material layer to be etched should be used. It is preferable to replenish the brazing material etchant while checking the component amounts and pH of the brazing material etchant. It is also possible to proceed with the brazing material etching process while replacing all of the brazing material etchant. In addition, since the brazing material layer does not contain Ag, the life of the etching solution can be extended compared to a brazing material layer containing Ag. As described above, it is possible to reduce the number of brazing material etching steps and shorten the processing time. This allows the life of the etching solution to be extended. As an example, if the etching step for the brazing material layer containing Ag is performed three times, the etching step for the brazing material layer not containing Ag only needs to be performed once or twice. Since the number of processing steps is reduced, the life of the etching solution can be extended. In addition, when the number of brazing material etching steps and the processing time are the same, the concentration of the etching solution can be reduced. For an etching solution for a brazing material layer containing Ag, the etching solution concentration can be set to a range of 40wt% to 70wt%. As an example, assume that a brazing material layer containing Ag is etched using a brazing material etching solution containing 30wt% hydrogen peroxide. When etching a brazing material layer that does not contain Ag, the hydrogen peroxide concentration can be set to a range of 12wt% to 21wt%.

[0033] The first copper etching step for the copper plate and the copper alloy layer of the brazing material layer is a process for forming a joint before etching the active metal brazing material layer. In the first copper etching step, it is preferable to apply an etching resist to the copper plate and then etch the copper plate and the copper alloy layer to process these members into a pattern shape. By applying the etching resist, the pattern shape and the distance between the patterns can be changed arbitrarily. After the first copper etching step, it is preferable to perform brazing material etching on the bonded body from which the etching resist has been removed. By removing the etching resist, it is possible to prevent the etching resist from reacting with the brazing material etchant or chemical polishing solution, which may cause defects. If the etching resist reacts, the pH of the brazing material etchant may exceed 6. When a combination of HBF4 and a chelating agent is used as a pH stabilizer, the pH of the brazing material etchant can be prevented from exceeding 6 even if the brazing material layer is etched while leaving the etching resist.

[0034] In the manufacturing method of the ceramic circuit board according to the embodiment, the number of times of the brazing material etching process can be, for example, two or less. In addition, the time for one brazing material etching process can be 15 minutes or less, so that the damage to the copper plate is small. Therefore, even if the etching resist is removed and the brazing material etching process is performed, the surface roughness Ra of the copper plate can be 0.2 μm or more and 1 μm or less. If the surface roughness Ra of the copper plate is set to 0.2 μm or more and 1 μm or less, the adhesion of the copper plate to the molded resin is improved. A semiconductor device having a semiconductor element mounted on a ceramic circuit board is molded with resin. In order to improve the adhesion strength between the copper plate and the resin, a process of roughening the copper plate surface is performed. In the manufacturing method of the ceramic circuit board according to the embodiment, the surface roughness of the copper plate surface can be controlled by performing the brazing material etching process. Therefore, it is not necessary to perform a special process of roughening the copper plate surface, such as blasting. This also improves the manufacturing efficiency. In particular, the method is suitable for manufacturing a ceramic circuit board that is molded with resin. The above-mentioned method for manufacturing a ceramic circuit board can shorten the time for one brazing material etching step to 15 minutes or less, or even 7 minutes or less. In addition, even if the distance between patterns is narrowed to 2 mm or less, or even 1.5 mm or less, a ceramic circuit board can be manufactured. In addition, even if the distance between patterns is shortened as described above, the occurrence of ion migration can be suppressed compared to the case of using a brazing material containing silver. This is because ion migration occurs more easily with silver than with copper. In addition, the size of the brazing material protruding portion can be left at 10 μm to 200 μm, or even 10 μm to 100 μm. In other words, the time for the brazing material etching step can be shortened while controlling the distance between patterns and the size of the brazing material protruding portion. In addition, when the total area of ​​exposed brazing material per ceramic circuit board is 2000 mm 2 Even if the space is wider than this, ceramic circuit boards can be manufactured with a good yield. In addition, since the brazing material layer does not contain Ag, even large ceramic circuit boards can be manufactured with a good yield. The obtained ceramic circuit board may be divided into multiple pieces as necessary. In addition, a ceramic circuit board may be manufactured using a ceramic board that has been scribed in advance.

[0035] (Examples 1 to 5, Comparative Example 1) The ceramic substrates used were a silicon nitride substrate (substrate thickness 0.32 mm, thermal conductivity 90 W / m K, three-point bending strength 650 MPa) and an aluminum nitride substrate (substrate thickness 0.635 mm, thermal conductivity 180 W / m K, three-point bending strength 350 MPa). The silicon nitride substrate is referred to as "Si3N4" and the aluminum nitride as "AlN". We also prepared three types of copper plates with thicknesses of 0.3 mm, 0.5 mm, and 0.8 mm. The 0.3 mm copper plate was designated "Copper Plate 1," the 0.5 mm copper plate "Copper Plate 2," and the 0.8 mm copper plate "Copper Plate 3." The length and width of the ceramic substrate are as shown in Table 1. The length and width of the copper plate are the same as those of the ceramic substrate.

[0036] [Table 1]

[0037] Next, a heat bonding step was carried out to manufacture a bonded body using the active metal brazing material shown in Table 2. In the examples, a brazing material not containing Ag was used, and in the comparative examples, a brazing material containing Ag was used.

[0038] [Table 2]

[0039] For the joints of the examples and the comparative examples, an etching resist was applied to the copper plate on the front side, and then the copper plate was etched into a pattern shape. An aqueous solution of ferric chloride was used to etch the copper plate and the copper alloy layer. The copper plate pattern was provided with a pattern distance of 1.5 mm and 2.0 mm. copper plate The brazing filler metal layer was exposed by etching the copper alloy layer. The area of ​​the exposed brazing filler metal layer was calculated as the total area (mm 2 ) are shown in Table 3.

[0040] [Table 3]

[0041] Next, the brazing material etching solution shown in Table 4 and the chemical polishing solution shown in Table 5 were prepared. For the brazing material etching solution, the mass ratios of hydrogen peroxide (H2O2), ammonium fluoride (NH4F), and pH stabilizer are shown when the total mass of the solution is 100 wt%. They were mixed in an aqueous solution to obtain the mass ratios shown in Table 3. Hydroboric acid (HBF4) was used as the pH stabilizer. In addition, the amount of pure water (L: liters) mixed for a total of 1 L of the aqueous solution containing hydrogen peroxide (H2O2), the aqueous solution containing ammonium fluoride (NH4F), and the aqueous solution containing the pH stabilizer is shown. The pH of the brazing material etching solution is also shown. The chemical polishing solutions used and their contents (wt%) are shown in Table 5. Citric acid in Table 5 is a type of chelating agent and a tricarboxylic acid.

[0042] [Table 4]

[0043] [Table 5]

[0044] The joined bodies according to the examples and comparative examples, brazing material etching solutions 1 to 4, and chemical polishing solutions 1 to 3 were combined to perform the manufacturing method of the ceramic circuit board shown in Table 6. In each example, the exposed areas of the brazing material layer between the patterns of the copper plate were removed. After the brazing material etching process and the chemical polishing process, a cleaning process using pure water was performed for 5 minutes. The brazing material etching process was performed while applying "ultrasonic waves" and was marked with "x ultrasonic waves." The ultrasonic waves had a frequency range of 10 to 100 kHz. The brazing material etching solution was heated to 30 to 60°C while the etching process was performed.

[0045] [Table 6]

[0046] The brazing material etching process was carried out on 30 joined pieces at a time. The amount of remaining brazing material protruding from the resulting joined pieces was examined. The percentage of areas where the length of the brazing material protruding from the edge of the copper plate between the copper plate pattern shapes was within the range of 20 μm to 60 μm was calculated. FIG. 7 is a plan view illustrating a part of a ceramic circuit board, and is a schematic diagram for explaining a method for calculating the ratio of the region. FIG. 7 shows copper plates 13-1 and 13-2 divided by a copper etching process. A groove T is formed between the copper plates 13-1 and 13-2. When viewed in plan, the soldering material protruding portions 12d-1 and 12d-2 are visible between the copper plates 13-1 and 13-2. In a first direction D1 connecting the pattern shapes, the length from the side of the copper plate 13-1 to the tip of the soldering material protruding portion 12d-1 was measured as the length L1 of the soldering material protruding portion. In addition, in the first direction D1, the length from the side of the copper plate 13-2 to the tip of the soldering material protruding portion 12d-2 was measured as the length L2 of the soldering material protruding portion. A length L3 between the pattern shapes in a second direction D2 along the groove T was measured. The second direction D2 is perpendicular to the first direction D1. The first direction D1 and the second direction D2 are parallel to the in-plane direction. In each of the solder metal protruding portions 12d-1 and 12d-2, a region in which both the lengths L1 and L2 were within the range W1 of 20 μm or more and 60 μm or less was identified. The length L4 in the second direction D2 of the identified region was measured. The length L3 between the patterns of the copper plate was set to 100, and the ratio (L4 / L3) of both the lengths L1 and L2 falling within the range W1 was calculated. The surface roughness Ra (μm) of the copper plate was also measured. The results are shown in Table 7.

[0047] [Table 7]

[0048] As can be seen from the table, the manufacturing method of the ceramic circuit board according to the embodiment was able to control the size of the protruding portion of the brazing material. Therefore, even large ceramic circuit boards can be manufactured with a good yield. In addition, in Comparative Example 1, since the brazing material layer contains Ag, the yield decreased when the ceramic circuit board was made larger. According to the embodiment, the number of etching steps can be reduced, and the life of the etching solution was also extended.

[0049] (Examples 6 to 7) Brazing filler metal etchants 5 and 6 shown in Table 8 were prepared. The concentration of brazing filler metal etchant 5 is about half that of brazing filler metal etchant 1. The concentration of brazing filler metal etchant 6 is about half that of brazing filler metal etchant 2.

[0050] [Table 8]

[0051] The brazing material etching step was carried out under the same conditions as in Comparative Example 1. Example 6 was an example in which the brazing material etchant 1 in Comparative Example 1 was replaced with brazing material etchant 5. Example 7 was an example in which the brazing material etchant 1 in Comparative Example 1 was replaced with brazing material etchant 6. As in Comparative Example 1, the remaining amount of the protruding brazing material and the surface roughness of the copper plate surface were examined. The results are shown in Table 9.

[0052] [Table 9]

[0053] As can be seen from Table 9, the embodiment obtained better results than the comparative example even when the concentration of the brazing material etching solution was lowered. It was found that the brazing material does not contain Ag, so that good results can be obtained even when the concentration of the brazing material etching solution is lowered. From this point of view, it was found that the life of the brazing material etching solution can be extended. In addition, the amount of various residues was measured to examine the effect of the final cleaning process. The measurement method was an XPS method described below.

[0054] The cleaning method, flow rate, and drying step for each Example are shown in Table 10. "None" in the table indicates that the step was not performed. In addition, "IPA" in the cleaning step indicates that cleaning was performed using isopropanol. "Alkaline" indicates that cleaning was performed using an alkaline solution with a pH of 10 or higher. In addition, the flow rate (L / min / cm2) and the drying step are also shown for each cleaning method. 2The numbers in the table indicate that a nozzle was used. The word "immersed" indicates that the assembly was immersed in a cleaning tank. "None" indicates that a cleaning step was not performed. Next, the drying process will be explained. Natural drying in the drying process is a method in which the bonded body is left to stand without removing any water droplets adhering to the surface. Diagonally is a method in which the bonded body is placed at an angle to reduce the amount of adhering water droplets. "Acetone" indicates that acetone was used. "Air blow" indicates that air blow was used.

[0055] [Table 10]

[0056] The correlation between the cleaning method and the residue shown in Table 10, and the correlation between the cleaning method and the durability of each solution were investigated. The results are shown in Table 11. The etching solution was replaced when the concentration of hydrogen peroxide decreased by 10 to 20 wt% from the initial concentration. In Table 11, when the amount of nitrogen, oxygen, carbon, and copper on the copper member surface was 100 atomic %, the case where nitrogen, oxygen, and carbon were 30 atomic % or less was recorded as "○". The case where nitrogen, oxygen, and carbon exceeded 30 atomic % was recorded as "×". XPS analysis was used to measure the atomic weight on the surface. An XPS analyzer manufactured by SSI was used. In the XPS analysis, AlKα radiation (hν=1486.6 eV) was used, and the X-ray spot diameter was set to a diameter of 1 mm. The durability is the durability of the etching solution. The number of uses until the etching rate decreased by 20% was shown as the durability.

[0057] [Table 11]

[0058] As can be seen from Tables 10 and 11, there is a correlation between the finishing cleaning method and the amount of residue, and cleaning methods other than immersion were able to reduce the amount of residue. Therefore, by carrying out a finishing cleaning process, it is possible to provide a board with less residue. This shows that it is possible to provide a board that is easy to use and has less adverse effects due to various residues when mounting, for example, semiconductor elements. Also, from Table 10, it was found that by providing a cleaning process or drying process between each etching process or chemical polishing process, the frequency of changing the etching solution in the next process can be further reduced.

[0059] Although some embodiments of the present invention have been illustrated above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. In addition, the above-mentioned embodiments can be implemented in combination with each other. [Explanation of symbols]

[0060] 1-1, 1-2…Copper etching process 2-1, 2-2…Brazing material etching process 3-1,3-2…Chemical polishing process 4-1, 4-2…Cleaning process 5-1…Finishing cleaning process 5-2…Finishing drying process 10...Ceramic circuit board 11...Ceramics substrate 12...Brazing layer 12a...Copper alloy layer 12b...Active brazing metal layer 12c…Copper precipitate 12d…Protruding brazing material 13,13-1,13-2…Copper plate

Claims

1. A step of preparing a joined body in which a copper member is joined to at least one surface of a ceramic substrate via a brazing material layer that does not contain Ag, and that contains Cu, an active metal, and one or more first elements selected from Sn and In; a first copper etching step in which a portion of the copper member and a layer containing Cu and the first element as main components in the brazing material layer are etched with an aqueous solution containing at least one of iron chloride and copper chloride, thereby forming an exposed portion of an active metal reaction layer in the brazing material layer; a first brazing material etching step of etching the exposed active metal reaction layer using an etching solution having a pH of 4 to 12, the etching solution containing one or two selected from hydrogen peroxide and ammonium peroxodisulfate; a first chemical polishing step of chemically polishing an end portion of the brazing material layer exposed by the first brazing material etching step; A method for manufacturing a ceramic circuit board comprising the steps of:

2. 2. The method for manufacturing a ceramic circuit board according to claim 1, wherein the length of a long side of the ceramic substrate is 100 mm or more.

3. 3. The method for manufacturing a ceramic circuit board according to claim 1, wherein the length of a long side of the ceramic board is 200 mm or more.

4. 4. The method for manufacturing a ceramic circuit board according to claim 1, wherein the distance between the etched copper members is 2 mm or less in some places.

5. 5. The method for producing a ceramic circuit board according to claim 1, wherein the etching solution further contains ammonium fluoride and a pH stabilizer.

6. The pH stabilizer is HBF 4 6. The method for producing a ceramic circuit board according to claim 5, wherein the anionic surfactant is at least one selected from the group consisting of EDTA, NTA, CyDTA, DTPA, TTHA, GEDTA, glycine, dicarboxylic acids, tricarboxylic acids, oxycarboxylic acids and salts thereof.

7. 7. The method for producing a ceramic circuit board according to claim 1, wherein the pH of the etching solution is from 4.0 to 6.

0.

8. 8. The method for producing a ceramic circuit board according to claim 1, further comprising a cleaning step of cleaning the bonded body after the first brazing material etching step and the first chemical polishing step.

9. 9. The method for manufacturing a ceramic circuit board according to claim 1, wherein the ceramic board is a nitride-based ceramic board.

10. 10. The method for manufacturing a ceramic circuit board according to claim 1, wherein in the first copper etching step, an etching resist is applied to the copper member, and then the part of the copper member is etched to process the copper member into a pattern shape.

11. 11. The method for producing a ceramic circuit board according to claim 10, wherein after the copper member is etched, the first brazing material etching step is carried out on the bonded body from which the etching resist has been removed.

12. 12. The method for producing a ceramic circuit board according to claim 1, wherein the first brazing material etching step is performed while applying ultrasonic waves to the bonded body.

13. 13. The method for producing a ceramic circuit board according to claim 1, further comprising the step of: performing a second copper etching step of etching the copper member after the first chemical polishing step.

14. 14. The method for producing a ceramic circuit board according to claim 1, wherein a finishing cleaning step is performed with a cleaning water flow rate of 1.3 L (liters) / min or more.

15. As a finishing cleaning step, a cleaning step is performed in which water is sprayed from a nozzle to clean the bonded body, 14. The method for producing a ceramic circuit board according to claim 1, wherein in the cleaning step, a distance between a nozzle and the bonded body is set within a range of 5 cm to 40 cm.

16. As a finishing cleaning step, a cleaning step is performed in which water is sprayed from a nozzle to clean the bonded body, 14. The method for manufacturing a ceramic circuit board according to claim 1, wherein in the cleaning step, the amount of water landing per nozzle is set within a range of 0.01 L (liter) / (min·cm2) to 0.1 L / (min·cm2).

17. The method for manufacturing a ceramic circuit board according to any one of claims 14 to 16, characterized in that the drying step after the finish cleaning step is performed by blowing air having a humidity of 70% or less at a speed in the range of 20 m / s to 150 m / s.

Citation Information

Patent Citations

  • Copper-ceramic interface structure of high-reliability silicon nitride copper-coated ceramic substrate and preparation method of copper-ceramic interface structure

    CN111403347A

  • Conductive paste for aluminum nitride substrate

    JP1989206508A

  • Circuit substrate and semiconductor device

    WO2017056360A1

  • Method for manufacturing ceramic circuit board

    WO2019054294A1