Release agent composition, as well as rigid release paper and release film.
The release agent composition, combining alkyd resin, amino resin, and organopolysiloxane, addresses the issues of reusability and surface condition deterioration in synthetic leather production, providing enhanced peelability and surface quality.
Patent Information
- Application Number
- JP2024540343
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-08-08
- Filing Date
- 2023-07-21
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-07-21
AI Technical Summary
Existing release agent compositions for synthetic leather production exhibit poor reusability, significant changes in release properties upon repeated use, and deterioration of surface condition, failing to meet the requirements for high gloss and minimal repelling.
A release agent composition comprising an alkyd resin with a hardness of 8 to 30 MPa, an amino resin, and an organopolysiloxane with functional groups that chemically bond with these resins in specific ratios, forming a coating film with improved peelability, reusability, and surface condition.
The composition achieves excellent release properties, reusability, and maintains a superior surface condition even after multiple uses, ensuring consistent quality in synthetic leather production.
Smart Images

Figure 0007948322000001 
Figure 0007948322000002 
Figure 0007948322000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a release agent composition, as well as rigid release paper and release film. [Background technology]
[0002] Conventionally, a release agent is applied to the surface of a sheet-like substrate such as paper or plastic, and a hardened film is formed to impart adhesive or release properties to tacky substances.
[0003] Release paper and release film have a wide range of applications, including use with adhesive materials such as labels, stickers, and tapes, as well as in the molding process of non-adhesive materials such as ceramic layers and urethane resins. Different performance characteristics are required depending on the application.
[0004] An example of a non-adhesive material used in the molding process is process paper used in the manufacture of synthetic leather. In the manufacturing process of synthetic leather, a release agent is cured on a base material to form process paper, and then a resin such as urethane resin, polyvinyl chloride resin, polyamide resin, or polyamino acid resin is applied to this process paper and dried. An adhesive layer is formed on the dried resin, a base fabric is bonded to it, and the resin is peeled off the process paper to produce synthetic leather.
[0005] Synthetic leather comes in matte (non-glossy) and enamel (high-gloss) types. In the manufacturing of enamel-type synthetic leather, the surface condition of the release agent coating is reflected in the finished product. Therefore, a release agent coating with high gloss and minimal repelling is required. Furthermore, to increase the productivity of synthetic leather production, process paper is generally used multiple times. For this reason, it is desirable that the release properties (mold release properties) do not change significantly after repeated use.
[0006] For example, Patent Document 1 discloses a release agent composition for process release paper comprising an alkyd resin, an amino resin, and a silicone resin containing a functional group reactive with the alkyd resin and the amino resin, wherein the amino resin mainly contains a methylated melamine resin having one or more methylol groups per triazine core, and it is stated that it is "useful for producing process release paper with excellent release properties at high temperatures, gloss, surface condition, and reusability, and can be cured and dried at low temperatures." However, the release agent composition described in Patent Document 1 has insufficient reusability, resulting in a problem of poor reusability of process release paper.
[0007] Patent Document 2 discloses a release agent composition comprising an alkyd resin, an amino resin, a silicone resin having a functional group reactive with the alkyd resin and / or the amino resin, and a cationic surfactant, and states that it "excels in gloss, release properties, and surface condition, has antistatic properties, and is excellent for repeated use." However, the release agent composition of Patent Document 2 shows a significant change in release properties when repeatedly used due to the addition of the surfactant, and improvement in reusability was necessary.
[0008] Patent Document 3 discloses a process paper for manufacturing synthetic leather, comprising a melamine resin and a cured product of a release agent composition containing a silicone-modified alkyd resin, wherein the content of the silicone-modified alkyd resin is a specific amount relative to the melamine resin. It is described as having "high gloss, excellent scratch resistance, and high repeatability." However, the release agent composition in Patent Document 3 has the drawback that the surface condition of the coating film of the release agent tends to deteriorate, and the release agent composition requires improvement in release properties.
[0009] Patent Document 4 discloses a release agent composition containing a resin selected from acrylic resins and alkyd resins, a resin selected from full-ether type methylated melamine resin, methylol type methylated melamine resin, and polymers thereof, a silicone resin, and a monohydric alcohol having 1 to 8 carbon atoms. It is stated that the composition has "good release properties and reusability, excellent low-temperature curing properties, and excellent storage stability." However, the release agent composition of Patent Document 4 also has the drawback that it requires improvement in release properties and the surface condition of the coating film of the release agent tends to deteriorate. [Prior art documents] [Patent Documents]
[0010] [Patent Document 1] Japanese Patent Publication No. 2000-095929 [Patent Document 2] Patent No. 4827282 [Patent Document 3] Patent No. 6707795 [Patent Document 4] International Publication No. 2020 / 153281 [Overview of the Initiative] [Problems that the invention aims to solve]
[0011] The present invention has been made in view of the above circumstances, and aims to provide a release agent composition that has good peelability and reusability, and a superior surface condition of the coating film of the release agent. [Means for solving the problem]
[0012] The inventors have conducted diligent studies to achieve the above objectives and have found that by providing a release agent composition containing (A) an alkyd resin with a hardness of 8 to 30 MPa, (B) an amino resin, and (C) an organopolysiloxane having a functional group that can chemically bond with one or more resins of component (A) and component (B) in a specific mass ratio, it is possible to obtain a release agent composition that has good release properties and reusability, and when the release agent is applied to form a coating film, the coating film is less prone to repelling, the gloss of the coated surface is excellent, and the surface condition is excellent.
[0013] Accordingly, the present invention provides the following invention. 1. (A) Alkyd resin with a hardness of 8-30 MPa, (B) Amino resin, and (C) An organopolysiloxane having two or more functional groups in one molecule that can chemically bond with one or more resins selected from components (A) and (B), A stripping agent composition containing the following: 2. The stripping agent composition according to (A), wherein the hydroxyl value of component (A) is 120 to 150 mg KOH / g. 3. The stripping agent composition according to claim 1 or 2, wherein the mass ratio of component (A) to component (B) (A) / (B) is 66 / 34 to 38 / 62. 4. A stripping agent composition according to any one of 1 to 3, wherein the mass ratio of component (C) to component (B) (C) / (B) is 1 / 99 to 20 / 80. 5. A rigid release paper or release film having a base material and a release layer formed on its surface, wherein the release layer is made of a cured product of the release agent composition described in any of 1 to 4. [Effects of the Invention]
[0014] The present invention provides a release agent composition that exhibits good release properties and reusability, and when a release layer is formed, the surface condition of the release layer is excellent. [Modes for carrying out the invention]
[0015] The present invention will be described in more detail below. [Component (A)] The component (A) of the present invention is an alkyd resin having a hardness of 8 to 30 MPa, and may be used singly or in combination of two or more kinds. The alkyd resin is a synthetic resin obtained by polycondensation and transesterification reaction of a polyhydric alcohol and a polybasic acid with a fatty acid or a fatty oil. The alkyd resin can be synthesized according to a conventionally known method such as that described in JP-A-2007-308658, and a commercially available product may be used.
[0016] Among the monomers forming the alkyd resin, specific examples of the polyhydric alcohol include dihydric alcohols such as ethylene glycol, polyethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, polypropylene glycol, 1,3-butanediol, 2,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 2,2-dimethyl-1,3-propanediol (neopentyl glycol), 2,2-dialkyl-1,3-propanediol, 2,4,4-trimethyl-1,3-pentanediol, butylene glycol, hydrogenated bisphenol A, ethylene oxide adduct of bisphenol A, and propylene oxide adduct of bisphenol A, as well as trihydric or higher polyhydric alcohols such as glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and tris-(2-hydroxyethyl) isocyanurate. These polyhydric alcohols may be used singly or in appropriate combination of two or more kinds. Among them, it is preferable to use a dihydric alcohol as an essential polyhydric alcohol component, and optionally use a trihydric or higher polyhydric alcohol in combination.
[0017] Among the monomers forming the alkyd resin, specific examples of polybasic acids include, for example, saturated polybasic acids such as phthalic anhydride, terephthalic acid, succinic acid, adipic acid, and sebacic acid; unsaturated polybasic acids such as maleic acid, maleic anhydride, fumaric acid, itaconic acid, citraconic anhydride, isophthalic acid, and trimellitic anhydride; and polybasic acids obtained via Diels-Alder reaction such as cyclopentadiene-maleic anhydride adducts, terpene-maleic anhydride adducts, and rosin-maleic anhydride adducts. In addition to the above polybasic acids, benzoic acid which is a monobasic acid may also be used in combination in some cases.
[0018] Specific examples of fatty acids or fatty oils include octylic acid, lauric acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, eleostearic acid, ricinoleic acid, as well as animal and vegetable oils such as dehydrated ricinoleic acid, linseed oil, soybean oil, safflower oil, tung oil, perilla oil, hempseed oil, tall oil, rice bran oil, castor oil, dehydrated castor oil, rapeseed oil, cottonseed oil, coconut oil, fish oil, and squid liver oil, and fatty acids thereof. It is preferable to use coconut oil, soybean oil, castor oil, and dehydrated castor oil.
[0019] Known alkyd resins can be used. For example, those produced using animal and vegetable oils or animal and vegetable oil fatty acids, various saturated fatty acids, and the like are used. The oil length of these alkyd resins is preferably 0 to 65, more preferably 25 to 55, even more preferably 27 to 45, and particularly preferably 29 to 40. Among them, it is preferable to use coconut oil-modified alkyd resins, soybean oil-modified alkyd resins, and castor oil-modified alkyd resins, and coconut oil-modified alkyd resins are particularly preferred. It is also possible to modify or mix these alkyd resins with acrylic resins, polyester resins, epoxy resins, phenolic resins and the like for use within a range that does not impair the effects of the present invention.
[0020] The hardness of the alkyd resin is 8 to 30 MPa, preferably 9 to 25 MPa, and more preferably 10 to 20 MPa. If the hardness is less than 8 MPa, cissing tends to occur on the coated surface, and the surface condition deteriorates. On the other hand, if the hardness is greater than 30 MPa, synthesis of the alkyd resin becomes difficult.
[0021] The hardness referred to in this specification is measured by the nanoindentation method. For example, it is the value obtained by analyzing measurement data obtained when a Berkovich indenter is pressed into alkyd resin to a maximum indentation depth of 100 nm using a nanoindenter (Triboindenter TI-950, manufactured by Hysitron Inc.) at a room temperature of 23°C, and then analyzing the data using the dedicated software (triboscan) attached to the measurement device.
[0022] The weight-average molecular weight of the alkyd resin is preferably 40,000 to 300,000, more preferably 60,000 to 280,000, even more preferably 80,000 to 260,000, and particularly preferably 100,000 to 240,000. When the weight-average molecular weight is within the above range, the surface condition is better.
[0023] The weight-average molecular weight referred to herein is the value obtained using polystyrene as a standard substance by gel permeation chromatography (GPC) under the following conditions. [Measurement conditions] GPC: HLC-8320 (manufactured by Tosoh Corporation) Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.6mL / min Detector: Differential refractive index detector (RI) Column: TSK Guardcolomn SuperH-L TSKgel SuperHM-N(6.0mmI.D.×15cm×1) TSKgel SuperH2500(6.0mmI.D.×15cm×1) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 50 μL (0.5 wt% THF solution)
[0024] The hydroxyl value of the alkyd resin is preferably 100 to 165 mg KOH / g, and more preferably 120 to 150 mg KOH / g. When the hydroxyl value is within the above range, the peelability and reusability are better. The above hydroxyl value is measured by the potentiometric titration method specified in JIS K0070:1922.
[0025] [(B) Component] The amino resin used in the present invention is a resin obtained by a condensation reaction between a compound having an amino group and formaldehyde, and acts as a crosslinking agent that reacts with component (A) and / or component (C), and one or more types can be used. The amino resin can be synthesized by known methods, such as those described in Japanese Patent Publication No. 53-061684, or commercially available products may be used.
[0026] Examples of amino resins include urea S resin, melamine resin, aniline resin, and guanamine resin, but melamine resin is preferred from the viewpoint of curability.
[0027] Melamine resin is a synthetic resin obtained by condensing melamine and formaldehyde, and is a condensate consisting of monomers or polymers of two or more units. It contains a structure in which a functional group is bonded to a triazine ring via three nitrogen atoms, and has an imino group, a methylol group, or an alkoxymethyl group as a functional group in one molecule, and depending on the functional group, it can be classified as a full ether type, methylol type, imino type, or methylol / imino type.
[0028] Furthermore, melamine resins are classified according to the type of alkoxymethyl group, including methylated melamine resins in which all alkoxymethyl groups are methoxymethyl groups, n-butylated melamine resins in which all alkoxymethyl groups are n-butoxymethyl groups, and methylated / n-butylated melamine resins in which alkoxymethyl groups are mixed with methoxymethyl and n-butoxymethyl groups.
[0029] From the viewpoint of release properties, the melamine resin is preferably a full ether type methylated melamine resin, a full ether type methylated / n-butylated melamine resin, a methylol type methylated melamine resin, or a methylol type methylated / n-butylated melamine resin, more preferably a full ether type methylated melamine resin or a methylol type methylated melamine resin, and even more preferably a full ether type methylated melamine resin.
[0030] Examples of commercially available melamine resins include Cymel 300, Cymel 301, Cymel 303LF (all manufactured by Ornex Japan Co., Ltd., full ether-type methylated melamine resins), Cymel 350, Cymel 370N (all manufactured by Ornex Japan Co., Ltd., methylol-type methylated melamine resins), Cymel 325, Cymel 327 (all manufactured by Ornex Japan Co., Ltd., imino-type methylated melamine resins), Cymel 232, Cymel 235 (all manufactured by Ornex Japan Co., Ltd., full ether-type methylated / n-butylated melamine resins), and Cymel 251 (all manufactured by Ornex Japan Co., Ltd., methylol-type methylated / n-butylated melamine resins).
[0031] The mass ratio of component (A) to component (B), (A) / (B), is preferably 66 / 34 to 38 / 62, more preferably 62 / 38 to 40 / 60, even more preferably 58 / 42 to 43 / 57, and particularly preferably 55 / 45 to 46 / 54. When the mass ratio of component (A) to component (B) is within the above range, the repeatability and surface condition are better. The proportion of component (B) in the total of components (A) to (C) is not particularly limited, but may be 10 to 90% by mass, preferably 20 to 80% by mass, and more preferably 35 to 60% by mass.
[0032] [(C) component] Component (C) of the present invention is an organopolysiloxane having two or more functional groups in one molecule that can chemically bond with one or more resins selected from components (A) and (B), and can be used alone or in appropriate combinations of two or more. The organopolysiloxane must have two or more functional groups in one molecule that can chemically bond with one or more resins selected from components (A) and (B). This allows components (A) and (B), which form the release layer, and the silicone resin, which is the release component, to adopt a structure in which they are chemically bonded in the release layer, thereby suppressing the migration of the silicone resin to the adhesive layer. Examples of such functional groups include hydroxyl groups, amino groups, carboxyl groups, epoxy groups, isocyanate groups, silanol groups, and aminosilyl groups, with amino groups, hydroxyl groups, and epoxy groups being preferred, and hydroxyl groups being more preferred.
[0033] The organopolysiloxane may have either a linear or branched structure, as long as it can exert the effects of the present invention, but one represented by the following average composition formula (1) is preferred. [ka] (In the formula, R 1 (These may be the same or different, and are unsubstituted or substituted organic groups having 1 to 20 carbon atoms, possessing a hydroxyl group, amino group, carboxyl group, epoxy group, or isocyanate group, and may be substituted with heteroatoms. Each molecule contains two or more of these organic groups. a is an integer greater than or equal to 2, b is an integer greater than or equal to 1, c is an integer greater than or equal to 0, and d is an integer greater than or equal to 0, such that 5 ≤ a + b + c + d ≤ 500.)
[0034] Preferred organic groups having 1 to 20 carbon atoms include, specifically, alkyl groups having 1 to 6 carbon atoms such as methyl, ethyl, propyl, and butyl groups; cycloalkyl groups having 5 to 8 carbon atoms such as cyclohexyl groups; aryl groups having 6 to 10 carbon atoms such as phenyl and tolyl groups; and aralkyl groups having 7 to 10 carbon atoms such as benzyl groups. Alternatively, alkyl groups having 1 to 10 carbon atoms selected from hydroxypropyl groups, 1-chloropropyl groups, 3,3,3-trifluoropropyl groups, etc., in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with polyether groups, alkoxyalkyl groups, halogen atoms, etc. Among these, methyl and phenyl groups are more preferred from the viewpoint of exfoliation.
[0035] As organic groups having 1 to 20 carbon atoms, which may be substituted with heteroatoms, having the above-mentioned hydroxyl group, amino group, carboxyl group, epoxy group, or isocyanate group, hydroxyalkyl groups such as hydroxymethyl group, hydroxyethyl group, hydroxypropyl group, hydroxybutyl group, hydroxypentyl group, hydroxyhexyl group, hydroxyheptyl group, hydroxyoctyl group, -(CH2)3-(OCH2CH2) n Polyethylene glycol group represented by -OH, -(CH2)3-(OCH2CH2CH2) n Examples include polypropylene glycol groups represented by -OH, 3-aminopropyl groups, N-2-(aminoethyl)-3-aminopropyl groups, carboxyoctyl groups, 3-glycidoxypropyl groups, 2-(3,4-epoxycyclohexyl)ethyl groups, and 3-isocyanatetopropyl groups. Among these, hydroxyalkyl groups, polyethylene glycol groups, and polypropylene glycol groups are more preferred from the viewpoint of curability.
[0036] The above functional group R 1 Preferably, the compound contains 5 to 50 mol% of aryl groups and aralkyl groups, more preferably 8 to 45 mol%, even more preferably 11 to 40 mol%, and particularly preferably 14 to 35 mol%. Within these ranges, peelability is better.
[0037] In the above formula (1), a, b, c, and d are such that a is an integer of 2 or more, preferably between 2 and 30; b is an integer of 1 or more, preferably between 1 and 500; c is an integer of 0 or more, preferably between 0 and 10; and d is an integer of 0 or more, preferably between 0 and 10, such that 5 ≤ a + b + c + d ≤ 500, preferably 10 ≤ a + b + c + d ≤ 400, and more preferably 20 ≤ a + b + c + d ≤ 300.
[0038] (C) Specific examples of component (C) are listed below, but are not limited to these. In the following formulas, Me and Ph represent a methyl group and a phenyl group, respectively, and the bonding order of each siloxane unit is not limited to those shown below. [ka]
[0039] The mass ratio of component (C) to component (B), (C) / (B), is preferably 1 / 99 to 20 / 80, more preferably 1.5 / 98.5 to 16 / 84, even more preferably 2 / 98 to 12 / 88, and particularly preferably 2.5 / 97.5 to 10 / 90. When the mass ratio of component (C) to component (B), (C) / (B), is within the above range, the peelability is better.
[0040] [(D) component] The composition of the present invention may contain any amount of solvent as component (D), either alone or in combination of two or more solvents. Dilution with a solvent improves handling and coating properties.
[0041] Suitable solvents include aromatic hydrocarbon compounds such as toluene and xylene, aliphatic hydrocarbon compounds such as hexane, heptane, and isoparaffin, ketone compounds such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, ester compounds such as ethyl acetate and butyl acetate, ether compounds such as diisopropyl ether and 1,4-dioxane, and alcohol compounds such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, and 2-butanol. Aromatic hydrocarbon compounds, ketone compounds, ester compounds, and alcohol compounds are preferred, with toluene, xylene, acetone, methyl ethyl ketone, ethyl acetate, butyl acetate, methanol, and 1-butanol being particularly preferred, but any compound that can dissolve the compound is acceptable.
[0042] When component (D) is included, the amount to be included is preferably 20 to 10,000 parts by mass, and more preferably 50 to 5,000 parts by mass, per 100 parts by mass of the total of components (A) to (C).
[0043] [(E) component] An acidic catalyst can be used in the composition of the present invention in order to promote the crosslinking reaction between component (A), component (B), and component (C). The acidic catalyst can be used alone or in combination of two or more types. Examples of acidic catalysts include inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, and boric acid; carboxylic acids such as acetic acid, monochloroacetic acid, dichloroacetic acid, and butyric acid; and organic sulfonic acids such as benzenesulfonic acid, p-toluenesulfonic acid, xylenesulfonic acid, p-phenolsulfonic acid, methanesulfonic acid, ethanesulfonic acid, and dodecylbenzenesulfonic acid. The use of organic acids is preferred, and p-toluenesulfonic acid and dodecylbenzenesulfonic acid are more preferred.
[0044] When an acidic catalyst is included, the amount should be sufficient to promote the reaction. For example, 0.1 to 20 parts by mass is preferred, and 1 to 10 parts by mass is more preferred, per 100 parts by mass of the total of components (A) to (C). Within this range, the curing properties are excellent, and the peelability and reusability are good. When components (D) to (E) are included, the total amount of components (A) to (E) in the release agent composition of the present invention is appropriately selected within the range of 80 to 100% by mass.
[0045] [Other optional components] The stripping agent composition of the present invention may further contain optional components other than those listed above, as long as they do not impair the effects of the present invention. Examples of optional components include antioxidants such as phenolic, quinone, amine, phosphorus, phosphite, sulfur, and thioether-based antioxidants; light stabilizers such as triazole and benzophenone-based light stabilizers; flame retardants such as phosphate esters, halogens, phosphorus, and antimony-based light retardants; dyes; pigments; defoamers; fillers; leveling agents; thickeners; and surfactants. These can be used individually or in appropriate combinations of two or more. In addition, from the viewpoint of repeated durability, the amount of cationic surfactant in the stripping agent composition of the present invention should be small, and may even be omitted. The amount of optional components is not particularly limited as long as it does not impair the effects of the present invention, but it is preferably 20% by mass or less in the stripping agent composition.
[0046] [Manufacturing method] The composition of the present invention can be prepared by mixing components (A) to (C), and optionally components (D), (E), and other optional components. However, in terms of storage stability, it is preferable to first uniformly mix components (A), (B), (C), (D), and other optional components, and then add component (E) immediately before use. The mixing method is not particularly limited, and known methods can be used.
[0047] [Release paper or release film (for coated materials)] The present invention provides a rigid release paper or release film having a substrate and a release layer formed on its surface, wherein the release layer is made of a cured product of the release agent composition. The release paper or release film can be obtained by coating the substrate with the release agent composition and then heating it to form a cured film.
[0048] Specifically, for example, the above-mentioned release agent composition can be applied as is, or further diluted within the range described above with the diluting solvent, and then applied to one or both sides of a sheet-like substrate such as paper or film using a coating method such as a comma coater, lip coater, roll coater, die coater, knife coater, blade coater, rod coater, kiss coater, gravure coater, wire bar coater, screen coater, dipping coater, or cast coater, at a rate of 0.01 to 100 g / m². 2 After coating, heating at 50-200°C for 1-120 seconds forms a hardened film on the substrate and creates a release layer.
[0049] The coating amount is 0.01 to 100 g / m². 2 Preferably, 0.03 to 20 g / m 2 It is more preferable that the drying temperature is 50 to 200°C, and more preferably 70 to 180°C. The drying time is 1 to 120 seconds, and more preferably 5 to 90 seconds. When forming a release layer on both sides of the substrate, it is preferable to perform the cured film (release layer) formation operation on one side of the substrate at a time.
[0050] Examples of sheet substrates include polyethylene laminated paper, glassine paper, fine paper, kraft paper, clay coated paper, mirror coated paper and other coated papers, synthetic paper such as Yupo, polyethylene film, polypropylene film such as CPP and OPP, polyester film such as polyethylene terephthalate film, polyamide film, polyimide film, polylactic acid film, polyphenol film, and polycarbonate film. To improve the adhesion between these substrates and the release layer, substrates that have been corona-treated, etched, or plasma-treated may be used. [Examples]
[0051] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0052] <Raw materials used> (Component A) (A-1) Coconut oil-modified alkyd resin (50% by mass xylene solution, hydroxyl value 133 mg KOH / g) 10.9 (A-2) Coconut oil-modified alkyd resin (50% by mass xylene solution, hydroxyl value 139 mg KOH / g) 12.5 (A-3) Coconut oil-modified alkyd resin (50% by mass xylene solution, hydroxyl value 125 mg KOH / g) 16.4 (A-4) Coconut oil-modified alkyd resin (50% by mass xylene solution, hydroxyl value 142 mg KOH / g) 8.6 (A-5) Comparative product, Haliftal 732-60 (manufactured by Harima Chemicals, 60% xylene solution of coconut oil-modified alkyd resin, hydroxyl value 130 mg KOH / g) 4.1 (A-6) Comparative product, Alkydia J-524-A (manufactured by DIC, 60% xylene solution of coconut oil-modified alkyd resin, hydroxyl value 126 mg KOH / g) 6.8
[0053] (B component) (B-1) Cymel 303LF (manufactured by Ornex Japan: Full ether-type methylated melamine resin)
[0054] (C component) (C-1) Polyorganosiloxanes represented by general formula (3): In the following formula, Me and Ph represent a methyl group and a phenyl group, respectively, and the bonding order of each siloxane unit is not limited to the following. [ka] (C-2) Polyorganosiloxane represented by general formula (4): In the following formula, Me and Ph represent a methyl group and a phenyl group, respectively, and the bonding order of each siloxane unit is not limited to the following. [ka]
[0055] (D component) A mixed solution of toluene and xylene (mass ratio 50:50)
[0056] (E component) p-toluenesulfonic acid
[0057] [hardness] The hardness of component (A) was measured using the nanoindentation method with a nanoindenter (Triboindenter TI-950, Hysitron Inc.). Component (A) was weighed into a round aluminum petri dish with a diameter of 6 cm and a depth of 1 cm so that the solid content of component (A) was 10 g, and the solvent was evaporated by heating in a hot air dryer at 150°C for 5 hours. The sample was then allowed to cool for 24 hours at room temperature of 23°C to obtain the measurement sample. The obtained samples were fixed to a dedicated sample holder with the (A) component surface in contact with the indenter. Hardness was determined by analyzing the data obtained when a Berkovich-type indenter was pressed into the surface of component (A) at a pressing speed of approximately 17 nm / sec and a pressing depth of approximately 100 nm under room temperature conditions of 23°C, using dedicated software (triboscan). The same procedure was performed on five different points for each sample to determine hardness, and the average values are shown in Tables 1 and 2.
[0058] [Examples 1-6, Comparative Examples 1-4] Using components (A) to (C) as raw materials, a coating composition was prepared according to the following procedure. Components (A), (B), and (C) were placed in a flask according to the mixing ratios shown in Tables 1 and 2, and component (D) was added to achieve a solid content concentration of 40% by mass, and the mixture was uniformly mixed. To the resulting solution, component (E) was added in an amount of 5 parts by mass per 100 parts by mass of the total of components (A) to (C), and the mixture was stirred to obtain a release agent composition. Using this composition, release paper having a release layer was prepared by the method described below, and the following evaluation was performed. The results are shown in the table. Note that component (A) contains a solvent, but the amounts listed in the table represent the pure amount excluding the solvent.
[0059] [Peel strength] The resulting release agent composition was applied to 165 μm thick mirror-coated paper using a bar coater at a rate of 5.0 g / m². 2 The material was applied in this manner, heated in a 170°C hot air dryer for 60 seconds to form a release agent layer, and then a one-component polyurethane solution [Crisbon 5516S (manufactured by Dainippon Ink and Chemicals, Inc.)] was applied to the surface of the cured film to a thickness of 30 μm, and heat-treated at 130°C for 2 minutes to form a polyurethane layer. Next, Nitto 31B tape was bonded to this treated surface and pressed back and forth once with a 2 kg roller, and after aging at 25°C for 20 hours, the sample was cut into 3 cm wide strips, and the bonded tape was pulled at a 180° angle at a peeling speed of 0.3 m / min using a tensile testing machine, and the force required to peel it off (gf / 30 mm) was measured. This value was defined as the first peel strength and evaluated based on the following indicators. ○: First peel strength is 20gf / 30mm or less △: First peel strength is greater than 20gf / 30mm but less than or equal to 30gf / 30mm. ×: First peel strength exceeds 30gf / 30mm
[0060] [Reusability] Similar to the peel strength test described above, a polyurethane solution was applied after forming a release agent layer to form a polyurethane layer. The polyurethane was peeled off three times, and the measurement taken on the third attempt was defined as the third peel strength. From the formula of (3rd peel strength - 1st peel strength) / 1st peel strength × 100 (%), the increase rate of peel force after repeated use was determined. A lower increase rate indicates better reusability, and evaluation was performed based on the following criteria. ○: Increase rate of 20% or less △: Increase rate of more than 20% and 50% or less ×: Increase rate of more than 50%
[0061] [Surface State (Cissing)] The surface of the coating film formed in the above peel strength test (400 cm 2 ) was visually observed, and the number of cissing defects was counted. A smaller number of cissing defects indicates a better surface state, and evaluation was performed based on the following criteria. ○: Number of cissing defects is 0 to 2 △: Number of cissing defects is 3 to 5 ×: Number of cissing defects is 6 or more
[0062] [Surface State (Glossiness)] The 60-degree specular gloss of the surface of the coating film formed in the above peel strength test was measured using a gloss meter VG7000 manufactured by Nippon Denshoku Industries Co., Ltd. A higher specular gloss indicates a better surface state, and evaluation was performed based on the following criteria. ○: Specular gloss is 96% or more △: Specular gloss is 92% or more and less than 96% ×: Specular gloss is less than 92%
[0063] [Table 1]
[0064] [Table 2]
Claims
1. (A) Alkyd resin having a hardness of 8 to 30 MPa, (B) Full ether-type methylated melamine resin, and (C) An organopolysiloxane having two or more functional groups in one molecule that can chemically bond with one or more resins selected from components (A) and (B), A stripping agent composition comprising (A) and having a mass ratio of (A) to (B) of (B) of 55 / 45 to 46 / 54.
2. The stripping agent composition according to claim 1, wherein the hydroxyl value of component (A) is 120 to 150 mg KOH / g.
3. The release agent composition according to claim 1, wherein the hardness of component (A) is 10 to 20 MPa.
4. The stripping agent composition according to claim 1, wherein the mass ratio of component (C) to component (B), (C) / (B), is 1 / 99 to 20 / 80.
5. The stripping agent composition according to claim 1, wherein the mass ratio (C) / (B) of component (C) to component (B) is 2.5 / 97.5 to 10 / 90.
6. Component (C) is the following average composition formula (1) 【Chemistry 1】 (In the formula, R1 may be the same or different, and is an unsubstituted or substituted organic group having 1 to 20 carbon atoms, and each molecule has two or more organic groups having 1 to 20 carbon atoms that may be substituted with heteroatoms, having a hydroxyl group, an amino group, a carboxyl group, an epoxy group, or an isocyanate group.) a is an integer greater than or equal to 2, b is an integer greater than or equal to 1, c is an integer greater than or equal to 0, 5 ≤ a + b + c + d ≤ 500, and R1 contains 14 to 35 mol% of an aryl group or an aralkyl group. The stripping agent composition according to claim 1, wherein the organopolysiloxane is represented.
7. The stripping agent composition according to claim 1, which does not contain a cationic surfactant.
8. A rigid release paper or release film having a base material and a release layer formed on its surface, wherein the release layer is made of a cured product of the release agent composition described in any one of claims 1 to 7.
Citation Information
Patent Citations
JP1973027282A
Carrier film for green sheet forming
JP1995137218A
Release agent composition for process release paper
JP2000095929A
Release film
JP2000117899A
Releasant composition and releasant
JP2002047476A