Conductive paste, electronic components, and multilayer ceramic capacitors
A conductive paste with a combined cellulose and polyvinyl acetal resin binder system improves adhesion and uniformity, addressing adhesion issues in multilayer ceramic capacitors, enhancing reliability and capacitance.
Patent Information
- Application Number
- JP2025569341
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-01-09
- Filing Date
- 2024-12-20
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-12-20
AI Technical Summary
Existing conductive pastes for multilayer ceramic capacitors face issues with adhesion between internal electrodes and green sheets, leading to problems such as peeling, misalignment, and poor bonding, which affect the reliability and capacitance of the capacitors, especially when miniaturization and high capacitance are required.
A conductive paste comprising conductive powder, ceramic powder, a dispersant, a binder resin, and an organic solvent, where the binder resin is a combination of cellulose resin and polyvinyl acetal resin, with a polymer compound formed by bonding a cellulose-based compound and a polyvinyl acetal-based compound through a sulfur atom, improving adhesion and uniformity.
The solution results in a smooth dried film with excellent adhesion, enhancing the reliability and capacitance of multilayer ceramic capacitors by preventing electrode detachment and improving electrode alignment, thus addressing the challenges of miniaturization and high capacitance.
Smart Images

Figure 0007948463000004 
Figure 0007948463000005 
Figure 0007948463000001
Abstract
Description
Technical Field
[0001] The present invention relates to a conductive paste, an electronic component, and a multilayer ceramic capacitor.
Background Art
[0002] With the miniaturization and higher performance of electronic devices such as mobile phones and digital equipment, miniaturization and higher capacitance are also desired for electronic components including multilayer ceramic capacitors and the like. A multilayer ceramic capacitor has a structure in which a plurality of dielectric layers and a plurality of internal electrode layers are alternately stacked, and miniaturization and higher capacitance can be achieved by thinning these dielectric layers and internal electrode layers.
[0003] The multilayer ceramic capacitor is manufactured, for example, as follows. First, a conductive paste for internal electrodes is printed (applied) in a predetermined electrode pattern on the surface of a green sheet containing a dielectric powder such as barium titanate (BaTiO₃, which may be hereinafter referred to as "BT") and a binder resin such as polyvinyl acetal resin (PVA), followed by drying to form a dried film. Next, a stacked body is formed, which is an integrated state obtained by stacking and thermocompression bonding such that the dried films and the green sheets are alternately overlapped. This stacked body is cut, subjected to a debinding treatment in an oxidizing atmosphere or an inert atmosphere, and then fired to obtain a fired chip. Subsequently, external electrode paste is applied to both end portions of the fired chip, and after firing, the surfaces of the external electrodes are subjected to nickel plating or the like, whereby a multilayer ceramic capacitor (MLCC) is obtained.
[0004] In recent years, MLCCs have been required to be further miniaturized and have larger capacitance. For example, thinning of dense and highly continuous electrode films for internal electrodes using nickel or the like, and increasing the dielectric constant and thinning of ceramic dielectric materials and dielectric layers using the same have been studied, and those with a dielectric layer thickness of 1.0 μm or less have already been put into practical use. It is also desired that the thickness of the electrode film be 1.0 μm or less.
[0005] The required characteristics for miniaturizing and increasing the capacitance of MLCCs include suppressing the decrease in insulation resistance under high temperature and high voltage, i.e., high reliability. The decrease in insulation resistance is said to be caused by the formation of irregularities on the surface of the Ni electrode layer sandwiching the dielectric layer during the firing process, and the concentration of the electric field on the protrusions. During the firing process, the Ni electrode layer is formed as the Ni powder sintersects and densifies. However, fine Ni powder sintersects quickly, making it easy for the electrodes to break and for spheroidization to occur. As a result, the effective electrode area of the Ni electrode layer decreases, leading to a decrease in the capacitance of the MLCC, and the irregularities on the surface of the Ni electrode layer lead to a decrease in the insulation resistance of the MLCC.
[0006] When MLCCs are thinned, the adhesion between the green sheet and the internal electrode layer decreases, leading to problems such as peeling and misalignment during lamination due to insufficient adhesion. For example, internal electrode paste with added plasticizers is used. However, adding plasticizers can significantly reduce the elastic modulus of the printed film (a decrease in elastic modulus makes the printed film softer and more easily deformed), and even if adhesion improves, it may lead to increased problems such as poor cutting. In addition, the addition of plasticizers increases the amount of gas generated during the deorganic binder process, which can cause cracks.
[0007] When ceramic green sheets are laminated and pressed together in the thickness direction, poor adhesion between the green sheets can lead to poor bonding between them. This poor bonding can cause short-circuit failures, for example, in multilayer ceramic capacitors. In particular, due to the demand for multilayer MLCCs, it is necessary to use dielectric powder with fine particles to reduce the thickness of each dielectric layer and increase the number of layers, so improvement in bonding is desirable. If the adhesion between sheets is weak, structural defects such as delamination, voids, and cracks will occur during firing, and these structural defects will reduce the yield of MLCCs.
[0008] To improve this type of adhesion defect, the following two approaches can be considered: 1) and 2) 1) Increasing the amount of binder or tackifier may be considered, but simply increasing the amount does not significantly improve adhesion. On the contrary, in this case, the amount of organic substances added, such as organic binders and tackifiers, increases, which makes it difficult to remove the organic binder, and even if the organic binder removal treatment is performed, residual organic substances (charcoal residue) may cause structural defects in the MLCC during the firing process. 2) When laminating multiple ceramic green sheets on which a conductive paste film is formed, smoothing the surface of the coating made of conductive paste increases the contact area between the paste film and the ceramic green sheet, thereby improving adhesion.
[0009] The purpose of improving the adhesion between the internal electrodes and the green sheet is to prevent cracking, and using butyral resin as the resin can prevent electrode detachment when the laminate is cut. Cellulose-based resins such as ethyl cellulose have been mainly used as organic binders, but while cellulose-based resins have high compatibility with various solvents and are effective in imparting the desired rheological properties to the conductive paste, they themselves do not have much thermoplasticity, so the dried film portion of the conductive paste has the disadvantage of hardly adhering to the upper surface during thermocompression bonding. As a result, we have not yet obtained a conductive paste for internal electrodes of multilayer ceramic capacitors that can further improve the thermocompression bonding between the internal electrodes of the screen-printed green sheet and the green sheet on top of it, prevent misalignment of the electrode stacking inside the chip, improve electrode alignment, and prevent chip cracking and peeling, while also being able to handle high-layer stacking.
[0010] Therefore, the paste for the internal electrodes may contain an organic resin, and it is preferable that the organic binder resin is a mixture of ethyl cellulose (EC) and polyvinyl butyral (PVB) resin, which is a type of polyvinyl acetal (PVA) resin.
[0011] Ethyl cellulose (EC) is suitable for use as a binder in internal electrode pastes due to its good solubility in solvents, printability, and combustion decomposition properties. Furthermore, by using polyvinyl butyral (PVB) resin, a type of polyvinyl acetal (PVA) resin used in green sheets, as an organic binder resin, the adhesion strength between the green sheet and the dried film of the internal electrode paste can be increased.
[0012] Patent documents 1 and 2 disclose a conductive paste containing a cellulose-based resin and a polyvinyl butyral resin as a binder resin, which improves adhesion to ceramic green sheets. [Prior art documents] [Patent Documents]
[0013] [Patent Document 1] Publication No. 5299904 [Patent Document 2] Publication No. 5224722 [Overview of the project] [Problems that the invention aims to solve]
[0014] However, when two different organic binder resins are mixed, the combination is almost always incompatible. In the case of incompatible systems, the two organic binder resins do not fundamentally mix and exist independently, so not only do they fail to perform as expected, but their functionality is often significantly reduced.
[0015] When the resin becomes less soluble in the solvent, the smoothness of the paste-dried film deteriorates. For example, when EC and PVB are mixed, a typical "sea-island structure" is observed, confirming phase separation. As a result, the distribution of inorganic particles (Ni, BT) in the dried film becomes non-uniform. Thus, the combination of organic materials in the paste composition affects the dispersibility of inorganic particles (Ni, BT) in the dried film.
[0016] By making polymers that would normally not mix compatible with each other, it is possible to combine the characteristics of both polymers, stabilize the interface between different polymers, and achieve a uniform and stable dispersion state.
[0017] Furthermore, the conductive pastes disclosed in Patent Documents 1 and 2 contain polyvinyl butyral resin, which can improve the adhesion between the dried film and the green sheet. However, these technologies use cellulose-based resin and polyvinyl butyral resin in combination, and due to the poor compatibility of the two resins, the dispersion of conductive powder and ceramic powder in the paste was insufficient, and the density and smoothness of the dried film of the conductive paste were insufficient. Such characteristics of the dried film are not sufficient to meet the demands of the increasing capacitance of multilayer ceramic capacitors in recent years.
[0018] In view of these circumstances, the present invention aims to provide a conductive paste, an electronic component, and a multilayer ceramic capacitor that can form an internal electrode layer having a smooth dried film and excellent adhesion, using a conductive paste or ceramic powder that has been miniaturized for the purpose of miniaturizing and thinning multilayer ceramic electronic components. [Means for solving the problem]
[0019] To solve the above problems, the conductive paste of the present invention comprises conductive powder, ceramic powder, a dispersant, a binder resin, and an organic solvent, wherein the binder resin comprises one or more resins selected from cellulose resin and polyvinyl acetal resin, and a polymer compound in which a cellulose-based compound and a polyvinyl acetal-based compound are bonded by a sulfur atom, wherein the molar ratio of the sulfur atom to the cellulose-based compound in the polymer compound is 0.3 to 1.7, and the polymer compound is present in an amount of 20% by mass or more relative to the total mass of the cellulose resin, the polyvinyl acetal resin, and the polymer compound.
[0020] The cellulose-based compound is a cellulose derivative having a thiol group or a vinyl group, the polyvinyl acetal-based compound is a polyvinyl acetal resin having a thiol group or a vinyl group, when the cellulose derivative has a thiol group, the polyvinyl acetal resin has a vinyl group that reacts with the thiol group, and when the cellulose derivative has a vinyl group, the polyvinyl acetal resin may have a thiol group that reacts with the vinyl group.
[0021] The cellulose derivative may be ethyl cellulose having a thiol group or a vinyl group, and the polyvinyl acetal resin may be polyvinyl butyral having a thiol group or a vinyl group.
[0022] The cellulose-based compound is a first esterification reaction product obtained by dehydration condensation between a carboxy group of a carboxylic acid having a thiol group or a vinyl group and a hydroxyl group of cellulose, the polyvinyl acetal-based compound is a second esterification reaction product obtained by dehydration condensation between a carboxy group of a carboxylic acid having a thiol group or a vinyl group and a hydroxyl group of polyvinyl acetal, when the first esterification reaction product has a thiol group, the second esterification reaction product has a vinyl group, when the first esterification reaction product has a vinyl group, the second esterification reaction product has a thiol group, and the polymer compound may be a thiol-ene reaction product of the first esterification reaction product and the second esterification reaction product.
[0023] The first esterification reaction product may be an esterification reaction product obtained by dehydration condensation between a carboxy group of 3-allyloxypropionic acid and a hydroxyl group of ethyl cellulose, and the second esterification reaction product may be an esterification reaction product obtained by dehydration condensation between a carboxy group of 3-mercaptopropionic acid and a hydroxyl group of polyvinyl butyral.
[0024] The cellulose resin may be an ethyl cellulose resin, and the polyvinyl acetal resin may be a polyvinyl butyral resin.
[0025] The conductive powder may be nickel powder.
[0026] The number average particle diameter of the conductive powder may be 0.05 μm or more and 1.0 μm or less.
[0027] The ceramic powder may contain barium titanate.
[0028] The number average particle diameter of the ceramic powder may be 0.01 μm or more and 0.5 μm or less.
[0029] The content of the ceramic powder may be 1 mass% or more and 20 mass% or less.
[0030] The conductive paste of the present invention may be used for internal electrodes of multilayer ceramic components.
[0031] Moreover, to solve the above problems, an electronic component of the present invention is an electronic component formed using the conductive paste of the present invention.
[0032] Moreover, to solve the above problems, a multilayer ceramic capacitor of the present invention at least has a laminate in which dielectric layers and internal electrode layers are laminated, and the internal electrode layers are formed using the conductive paste of the present invention. Effects of the Invention
[0033] According to the present invention, it is possible to provide a conductive paste, an electronic component, and a multilayer ceramic capacitor that can form an internal electrode layer having a smooth dried film and excellent adhesion, in a conductive paste using finely refined conductive powder and ceramic powder for the purpose of miniaturization and thinning of multilayer ceramic electronic components. Brief Description of the Drawings
[0034] [Figure 1A] FIG. 1A is a perspective view showing the multilayer ceramic capacitor according to the present embodiment. [Figure 1B]Figure 1B is a cross-sectional view showing a multilayer ceramic capacitor according to this embodiment. [Modes for carrying out the invention]
[0035] The following describes an embodiment of the conductive paste, electronic component, and multilayer ceramic capacitor of the present invention.
[0036] [Conductive paste] The conductive paste of this embodiment comprises conductive powder, ceramic powder, a dispersant, a binder resin, and an organic solvent. Each component will be described in detail below.
[0037] <Conductive powder> The conductive powder is not particularly limited, and metal powders can be used. For example, one or more powders selected from Ni, Pd, Pt, Au, Ag, Cu, and their alloys can be used. Among these, Ni or its alloy powders are preferred from the viewpoint of conductivity, corrosion resistance, and cost. As a Ni alloy, for example, an alloy of Ni with at least one element selected from the group consisting of Mn, Cr, Co, Al, Fe, Cu, Zn, Ag, Au, Pt, and Pd can be used. The Ni content in the Ni alloy is, for example, 50% by mass or more, preferably 80% by mass or more. In addition, the Ni powder may contain several hundred ppm of sulfur to suppress rapid gas generation due to partial thermal decomposition of the binder resin during the debindering process.
[0038] The method for producing conductive powder is not particularly limited, and for example, methods such as directly precipitating chloride vapor from the gas phase in hydrogen gas, atomization from molten metal, spray pyrolysis using an aqueous solution, and a wet method in which raw material metal salts are reduced in an aqueous solution can be applied.
[0039] The number-average particle size of conductive powder is not particularly limited and can be selected according to the size of the electronic component to be used, for example, it should be between 0.05 μm and 1.0 μm. For example, for multilayer ceramic capacitors where thin films are becoming more common, the number-average particle size of conductive powder is preferably 0.5 μm or less, and more preferably 0.3 μm or less. If the number-average particle size exceeds 0.5 μm, the surface irregularities of the internal electrodes become severe, which can degrade the electrical characteristics of the capacitor and is therefore undesirable. Furthermore, the lower limit of the number-average particle size of conductive powder is not particularly limited, but for example, it is 0.03 μm or more. If the number-average particle size is smaller than 0.03 μm, handling may become extremely difficult.
[0040] The number-average particle size of the conductive powder is determined from observations using a scanning electron microscope (SEM). It is the average value obtained by measuring the particle size of multiple individual particles from images observed with an SEM at a magnification of 10,000x.
[0041] The conductive powder content is preferably 30% by mass or more and less than 70% by mass, and more preferably 40% by mass or more and 60% by mass or less, relative to the total amount of conductive paste. When the conductive powder content is preferably 30% by mass or more and less than 70% by mass, relative to the total amount of conductive paste, the conductivity and dispersibility are excellent.
[0042] <Ceramic powder> The ceramic powder is not particularly limited, and for example, in the case of a conductive paste for the internal electrodes of a multilayer ceramic capacitor, a known ceramic powder can be appropriately selected depending on the type of multilayer ceramic capacitor to be applied. Examples of ceramic powders include perovskite-type oxides containing Ba and Ti, and barium titanate (BaTiO3BT) is preferred.
[0043] As the ceramic powder, a ceramic powder mainly composed of barium titanate and containing oxides as minor components may be used. Examples of oxides include oxides of Mn, Cr, Si, Ca, Ba, Mg, V, W, Ta, Nb, and one or more rare earth elements. Alternatively, as the ceramic powder, a perovskite-type oxide ferroelectric ceramic powder may be used, in which the Ba or Ti atoms of barium titanate (BaTiO3) are substituted with other atoms, such as Sn, Pb, or Zr.
[0044] In the conductive paste for the internal electrodes, a ceramic powder with the same composition as the dielectric ceramic powder constituting the green sheet of the multilayer ceramic capacitor may be used as the ceramic powder. This suppresses the occurrence of cracks due to a mismatch in shrinkage at the interface between the dielectric layer and the internal electrode layer during the sintering process. Examples of such ceramic powders include oxides such as ZnO, ferrite, PZT, BaO, Al2O3, Bi2O3, R(rare earth element)2O3, TiO2, and Nd2O3. One type of ceramic powder may be used, or two or more types may be used.
[0045] The number-average particle size of the ceramic powder is, for example, 0.01 μm to 0.5 μm, preferably in the range of 0.01 μm to 0.3 μm. A number-average particle size of 0.01 μm to 0.5 μm in the ceramic powder allows for the formation of sufficiently fine, thin, and uniform internal electrodes when used as an internal electrode paste. The number-average particle size is determined from observation using a scanning electron microscope (SEM), specifically by measuring the particle size of individual particles from an image observed at a magnification of 50,000x using an SEM, and is the average value obtained from this measurement.
[0046] The ceramic powder content is preferably 1 to 30 parts by mass, and more preferably 3 to 30 parts by mass, per 100 parts by mass of conductive powder. When the ceramic powder content is 1 to 30 parts by mass per 100 parts by mass of conductive powder, excellent conductivity and dispersibility are achieved.
[0047] The ceramic powder content is preferably 1% to 20% by mass, and more preferably 5% to 20% by mass, relative to the total amount of conductive paste. When the ceramic powder content is 1% to 20% by mass relative to the total amount of conductive paste, the conductivity and dispersibility are excellent.
[0048] <Binder resin> The binder resin used in the conductive paste of this embodiment comprises one or more resins selected from cellulose resin and polyvinyl acetal resin, and a polymer compound in which a cellulose-based compound and a polyvinyl acetal-based compound are bonded by a sulfur atom, wherein the molar ratio of the sulfur atom to the cellulose-based compound in the polymer compound is 0.3 to 1.7, and the polymer compound is present in an amount of 20% by mass or more relative to the total mass of the cellulose resin, the polyvinyl acetal resin, and the polymer compound.
[0049] In other words, the binder resin used in the conductive paste of this embodiment contains a polymer compound formed by the bonding of a cellulose-based compound and a polyvinyl acetal-based compound. The mass-average molecular weight (Mw) of this polymer compound is preferably 20,000 to 200,000, calculated using standard polystyrene equivalent values obtained by gel permeation chromatography (GPC). If the number-average molecular weight of the polymer compound is less than 20,000, the viscosity of the conductive paste made using it will be extremely low, making it difficult to adjust to an appropriate viscosity for a conductive paste. Conversely, if the mass-average molecular weight of the polymer compound exceeds 200,000, the viscosity of the conductive paste made using it will be extremely high, making it difficult to adjust to an appropriate viscosity for a conductive paste, or it may be necessary to reduce the amount of conductive powder or ceramic powder to an appropriate level in order to adjust to an appropriate viscosity.
[0050] The binder resin content is preferably 0.5% to 10% by mass, and more preferably 1% to 6% by mass, relative to the total amount of conductive paste. When the binder resin content is in the range of 0.5% to 10% by mass, the conductivity as an internal electrode layer and the dispersibility of conductive powder and ceramic powder in the conductive paste are excellent.
[0051] Furthermore, the content of the polymer compound, which is a combination of a cellulose compound and a polyvinyl acetal compound, is preferably 1 to 10 parts by mass, and more preferably 1 to 8 parts by mass, per 100 parts by mass of conductive powder.
[0052] The polymer compound of this embodiment comprises a portion made up of a cellulose-based compound and a portion made up of a polyvinyl acetal-based compound. Therefore, the dried film obtained from the conductive paste of this embodiment can possess surface smoothness due to the cellulose-based compound and adhesion to the green sheet due to the polyvinyl acetal-based compound. Furthermore, since the polymer compound has structures of cellulose-based and polyvinyl acetal-based compounds that are not individually compatible within the same molecule, poor dispersion of the conductive paste can also be eliminated.
[0053] Here, even if the molar ratio of the sulfur atom to the cellulosic compound in the polymer compound is 0.5 to 2, the surface roughness of the dried film is superior to that of conventional conductive pastes using cellulose and polyvinyl acetal resin as a binder resin. However, if the molar ratio is 0.3 to 1.7, the surface roughness and dried film density of the conductive paste are even better. In the polymer compound, the molar ratio of the sulfur atom to the cellulosic compound is 0.3 to 1.7 (i.e., in the polymer compound, cellulosic compound:sulfur atom = 1.0:0.3 to 1.7), and more preferably, the molar ratio is 0.5 to 1.5 (i.e., in the polymer compound, cellulosic compound:sulfur atom = 1.0:0.5 to 1.5).
[0054] (polymer compound) A polymer compound formed by the combination of a cellulose-based compound and a polyvinyl acetal-based compound, which can be used in this embodiment, will be described in more detail below.
[0055] Both cellulose and polyvinyl acetal possess hydroxyl groups within their molecules. Cellulose compounds are prepared by introducing functional groups that can react with other compounds and form bonds to the hydroxyl groups of cellulose, thereby chemically modifying them with reactive functional groups. Similarly, polyvinyl acetal polymer compounds are prepared by introducing functional groups that can react with other compounds and form bonds to the hydroxyl groups of polyvinyl acetal compounds, but are different from the functional groups introduced in the cellulose compounds, thereby chemically modifying them with reactive functional groups. In other words, the reactive functional groups introduced in cellulose compounds and the reactive functional groups introduced in polyvinyl acetal compounds are different. While the functional groups introduced in cellulose compounds and the functional groups introduced in polyvinyl acetal compounds react, they do not react with each other. This resistance to reaction between identical functional groups is intended to prevent bonding between cellulose compounds and between polyvinyl acetal compounds.
[0056] Furthermore, if the functional groups introduced into the cellulosic compound and the functional groups introduced into the polyvinyl acetal compound combine, a polymer compound in which the cellulosic compound and the polyvinyl acetal compound are bonded can be obtained. Specifically, if thiol groups are introduced into cellulose to form a cellulosic compound, and vinyl groups are introduced into polyvinyl acetal resin to form a polyvinyl acetal compound, then in the presence of a nucleophile or under conditions that generate radicals, the double bond of the vinyl group and the sulfur atom of the thiol group will bond. As a polymer compound for the binder resin used in the conductive paste of this embodiment, a polymer compound in which the cellulosic compound and the polyvinyl acetal compound are bonded can be obtained by utilizing the bonding reaction between thiol groups and vinyl groups. Of course, it is also possible to introduce vinyl groups into the hydroxyl groups of cellulose to form a cellulosic compound, and to introduce thiol groups into the hydroxyl groups of polyvinyl acetal resin to form a polyvinyl acetal compound.
[0057] In other words, the cellulosic compound may be a cellulose derivative having a thiol group or a vinyl group, and the polyvinyl acetal compound may be a polyvinyl acetal resin having a thiol group or a vinyl group. When the cellulose derivative has a thiol group, the polyvinyl acetal resin has a vinyl group that reacts with the thiol group, and when the cellulose derivative has a vinyl group, the polyvinyl acetal resin has a thiol group that reacts with the vinyl group.
[0058] The cellulosic polymer used as the binder resin for the conductive paste in this embodiment is preferably a chemically modified polymer in which the compound is bonded to the hydroxyl groups of cellulose, a natural polymer. Note that the chemical modification described here differs from the chemical modification that introduces the reactive functional groups mentioned above; it refers to chemical modifications such as alkyl etherification and esterification.
[0059] Compound bonding with the hydroxyl groups of cellulose can be achieved through alkyl etherification, esterification, and other methods. Examples of celluloses containing hydroxyl groups include methylcellulose, ethylcellulose, propylcellulose, butylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, hydroxypropylmethylcellulose, hydroxybutylmethylcellulose, cellulose acetate (acetylcellulose, diacetylcellulose, triacetylcellulose, etc.), cellulose acetate propionate, cellulose acetate butyrate, and nitrocellulose. One type of cellulose may be used, or two or more types may be used in combination.
[0060] Since the conductive paste of the embodiment contains an organic solvent, it is preferable that the cellulose is also soluble in the organic solvent. From the viewpoint of solubility in organic solvents and the smoothness of the dried film of the conductive paste, it is even more preferable to use ethyl cellulose as the cellulose.
[0061] The molecular weight of cellulose affects the viscosity of the conductive paste in this embodiment. The number-average molecular weight (Mn) of cellulose, based on standard polystyrene equivalent values calculated by GPC, is preferably between 10,000 and 100,000, and more preferably between 10,000 and 80,000.
[0062] If the number-average molecular weight of cellulose is less than 10,000, the viscosity of the conductive paste may be low, and if the number-average molecular weight of cellulose exceeds 100,000, the viscosity of the conductive paste may be too high.
[0063] Not all hydroxyl groups in cellulose are chemically modified. Each glucose ring that makes up cellulose has three hydroxyl groups attached to it, but in chemically modified cellulose, on average, 0.1 to 1 hydroxyl group per glucose ring remains as a hydroxyl group and is not chemically modified. Reactive functional groups are introduced to these unmodified hydroxyl groups.
[0064] On the other hand, polyvinyl acetal is a polymer typically composed of monomer units of vinyl acetal / vinyl alcohol / vinyl acetate. It can be obtained by saponifying polyvinyl acetate to obtain polyvinyl alcohol, and then acetalizing the polyvinyl alcohol. Specifically, examples include polyvinyl butyral (polyvinyl butyral) and polyvinyl formal (polyvinyl formal).
[0065] Polyvinyl acetal can be a commercially available product, and various types of polyvinyl acetal with different degrees of butyralization, formalization, acetyl group content, hydroxyl group content, and molecular weight are sold by companies such as Sekisui Chemical Co., Ltd. and Kuraray Co., Ltd. One type of polyvinyl acetal may be used, or two or more types may be used in combination.
[0066] It is preferable that the polyvinyl acetal is soluble in organic solvents. Due to its high solubility in organic solvents, it is more preferable that the polyvinyl acetal be polyvinyl butyral.
[0067] The molecular weight of polyvinyl acetal affects its film strength and solution viscosity. Therefore, the number-average molecular weight of polyvinyl acetal is preferably in the range of 0.5 million to 150,000, and more preferably in the range of 10,000 to 100,000, based on standard polystyrene equivalent values obtained by GPC.
[0068] If the number-average molecular weight of polyvinyl acetal is less than 0.5 million, the solution viscosity will be extremely low, making it difficult to adjust the viscosity of the inorganic particle-containing composition (paste or slurry). Furthermore, the strength and adhesion of the film formed by applying and drying the inorganic particle-containing composition may decrease.
[0069] Polyvinyl acetals have at least one hydroxyl group in each molecule. Generally, polyvinyl acetals have 20 to 40 mole% of hydroxyl groups as vinyl alcohol units that make up the polymer. These hydroxyl groups are chemically modified by introducing reactive functional groups.
[0070] Compounds that chemically modify cellulose or polyvinyl acetal by reacting with the hydroxyl groups can be compounds that have a thiol group or vinyl group at one end and a carboxyl group at the other end. The carboxyl group of the compound undergoes dehydration condensation with the hydroxyl groups of the cellulose polymer or polyvinyl acetal compound to form an ester bond.
[0071] Below, an example of a synthesis method for the polymer compounds used in this embodiment will be described. To obtain cellulosic compounds or polyvinyl acetal compounds, esterification or etherification can be performed between a compound having a functional group that reacts with a hydroxyl group and a functional group that has reactivity with other compounds, and the hydroxyl groups of cellulose or polyvinyl acetal. Examples of functional groups that react with a hydroxyl group include carboxyl groups and hydroxyl groups.
[0072] Esterification reactions can be carried out, for example, using a condensing agent. Examples of condensing agents include carbodiimide, diphenyl phosphate azide, and 1-hydroxybenzotriazole. One condensing agent may be used alone, or two or more may be used in combination. Among these, carbodiimide is preferred because of its versatility and reactivity, and because the reaction can proceed under low temperature conditions and without being affected by moisture in the reaction environment.
[0073] Examples of carbodiimides include dicyclohexylcarbodiimide, diisopropylcarbodiimide, N-[3-(dimethylamino)propyl]-N'-ethylcarbodiimide, and N-[3-(dimethylamino)propyl]-N'-ethylcarbodiimidemethiodad. Among these, dicyclohexylcarbodiimide and diisopropylcarbodiimide are preferred from the viewpoint of availability. Furthermore, when using carbodiimide, it is also preferable to use a reaction accelerator such as dimethylaminopyridine or triethylamine as a base in the range of 0.01 mol% to 10 mol% relative to the carbodiimide.
[0074] On the other hand, etherification reactions can be efficiently carried out by using alkali metal hydroxides such as KOH and NaOH, or alkali metal hydrides such as NaH and KH, as reaction catalysts.
[0075] To obtain cellulosic compounds, it is preferable to dissolve cellulose in an aproton solvent such as ethyl acetate, mix it with a compound having a carboxyl group that forms an ester bond with a hydroxyl group and a vinyl group or thiol group, which are functional groups that react with other compounds, and use a condensing agent and a nucleophile such as a base, such as dimethylaminopyridine, in a range of 0.01 mol% to 10 mol% to promote the esterification reaction.
[0076] The polymer compound used in this embodiment has a molar ratio of sulfur atoms to the cellulosic compound of 0.3 to 1.7 (cellulosic compound:sulfur atoms = 1.0:0.3 to 1.7). Therefore, for every 1 mole of cellulose, it is necessary to add 0.3 to 1.7 moles of the compound containing a functional group that reacts with other compounds.
[0077] The reaction temperature for synthesizing cellulosic compounds is preferably in the range of room temperature to 50°C. After the synthesis reaction of cellulosic compounds is complete, the system contains a mixture of unreacted cellulose (where no functional groups reactive with other compounds have been introduced to the hydroxyl groups), cellulosic compounds with one reactive functional group introduced, and cellulosic compounds with multiple reactive functional groups introduced. While chemical modification is a matter of probability, cellulosic compounds with one hydroxyl group chemically modified are the most common. In this invention, the mixture of these unreacted cellulose, cellulose with multiple functional groups introduced, and cellulose with one reactive functional group introduced is considered the cellulosic compound. Once the synthesis of the cellulosic compound is complete, the solvent can be removed by distillation.
[0078] To synthesize polyvinyl acetal compounds, it is preferable to dissolve polyvinyl acetal in an aprotic solvent such as ethyl acetate, mix it with a compound having a carboxyl group that forms an ester bond with a hydroxyl group and a vinyl group or thiol group which are functional groups that react with other compounds, and use a condensing agent and a nucleophile such as a base, such as dimethylaminopyridine, in a range of 0.01 mol% to 10 mol% to promote the esterification reaction.
[0079] The reaction temperature for the chemical modification of the hydroxyl groups of polyvinyl acetal is preferably in the range of room temperature to 50°C. While thiol or vinyl functional groups are introduced to the polyvinyl acetal, not all of the polyvinyl acetal is modified; unreacted polyvinyl acetal remains. In this invention, a mixture of this unreacted polyvinyl acetal and the polyvinyl acetal to which the functional groups have been introduced is used as the polyvinyl acetal compound. After the synthesis of the polyvinyl acetal compound is complete, the solvent can be removed by distillation.
[0080] The polymer compound used in this embodiment can be synthesized by dissolving a cellulose compound and a polyvinyl acetal compound in a solvent, adding a radical generator, and heating the mixture. This causes a reaction between the vinyl group on one of the cellulose compound and the thiol group on the other, resulting in the bonding of the cellulose compound and the polyvinyl acetal compound.
[0081] Alternatively, polymer compounds may be synthesized by dissolving a cellulose-based compound and a polyvinyl acetal-based compound in a solvent, adding a nucleophile such as a base like an amine, and heating the mixture.
[0082] The reaction temperature for bonding cellulose compounds and polyvinyl acetal compounds can be selected as appropriate, but a temperature of 60°C or higher is preferable.
[0083] The solvent can be an acetate-based solvent such as isobornyl acetate, isobornyl propinate, isobornyl butyrate and isobornyl isobutyrate, ethylene glycol monobutyl ether acetate, dipropylene glycol methyl ether acetate, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate, which are solvents that can be used in conductive pastes, or a terpene-based solvent such as terpineol, dihydroterpineol, dihydroterpinyl acetate, and terpinyl acetate. If a solvent used in conductive pastes is used as the solvent, the resulting polymer compound can be made into a vehicle dissolved in the solvent.
[0084] For example, the cellulose derivative may be ethylcellulose having a thiol group or a vinyl group, and the polyvinyl acetal resin may be polyvinyl butyral having a thiol group or a vinyl group.
[0085] Specifically, the cellulosic compound may be a first esterification reaction product obtained by dehydration condensation of a carboxyl group of a carboxylic acid having a thiol group or a vinyl group with a hydroxyl group of cellulose, and the polyvinyl acetal compound may be a second esterification reaction product obtained by dehydration condensation of a carboxyl group of a carboxylic acid having a thiol group or a vinyl group with a hydroxyl group of polyvinyl acetal. Furthermore, if the first esterification reaction product has a thiol group, the second esterification reaction product has a vinyl group, and if the first esterification reaction product has a vinyl group, the second esterification reaction product has a thiol group, and the polymer compound may be a thiol-ene reaction product of the first esterification reaction product and the second esterification reaction product.
[0086] More specifically, the first esterification product may be an esterification product obtained by dehydration condensation of the carboxyl group of 3-allyloxypropionic acid and the hydroxyl group of ethylcellulose, and the second esterification product may be an esterification product obtained by dehydration condensation of the carboxyl group of 3-mercaptopropionic acid and the hydroxyl group of polyvinyl butyral.
[0087] (Cellulose resin, polyvinyl acetal resin) Ideally, the entire binder resin of the conductive paste should be composed of the aforementioned polymer compound. However, as mentioned above, the synthesis of the polymer compound involves multiple chemical reactions, resulting in a compound that is more expensive than general cellulose resin or polyvinyl acetal resin. Therefore, the inventors investigated the combined use of the polymer compound with cellulose resin or polyvinyl acetal resin, to the extent that it does not impair the beneficial function that the polymer compound provides to the conductive paste.
[0088] In the conductive paste of this embodiment, the ratio of the polymer compound to the total mass of the binder resin, one or more resins selected from cellulose resin and polyvinyl acetal resin, and the polymer compound is 20% by mass or more, and preferably 30% by mass or more.
[0089] Furthermore, by using a binder resin composition consisting of cellulose resin, polyvinyl acetal resin, and the aforementioned polymer compound, it becomes possible to more freely adjust the viscosity of the conductive paste, which is not possible with the polymer compound alone. In other words, by using the binder resin composition of this embodiment, the viscosity of the conductive paste can be increased compared to when only the polymer compound is used as the binder resin.
[0090] Generally, cellulose resin and polyvinyl acetal resin are incompatible as described above. However, the polymer compound helps to make the cellulose resin and polyvinyl acetal resin compatible, and can suppress phase separation between the cellulose resin and the polyvinyl acetal resin. This effect is due to the polymer compound having a cellulosic backbone and a polyacetal backbone in its molecule. If the ratio of the polymer compound to the total mass of the cellulose resin, polyvinyl acetal resin, and the polymer compound is less than 20% by mass, the suppression of phase separation will be limited to a portion of the conductive paste, and satisfactory results may not be achieved. The ratio of the polymer compound to the total mass of the cellulose resin, polyvinyl acetal resin, and the polymer compound in the binder resin can be 99% by mass or less, or 95% by mass or less.
[0091] In other words, the content of the polymer compound in the binder resin is 20% by mass or more, more preferably 30% by mass or more, and can be 99% by mass or less, or 95% by mass or less. To put it another way, the mass ratio of the total of the cellulose resin and the polyvinyl acetal resin to the polymer compound can be set to 1-80:20-99, more preferably 5-70:30-95.
[0092] When such phase separation occurs, the dried film obtained by printing (coating) a conductive paste contains uneven distribution of binder resin, conductive powder, and ceramic powder. As a result, voids without conductive material may form in the internal electrodes obtained by firing the dried film, due to the uneven distribution of binder resin and ceramic powder. When voids form in the internal electrodes, the surface area of the internal electrodes becomes smaller, which may lead to a decrease in the capacitance of the MLCC. The effect of polymer compounds in suppressing phase separation of cellulose resin and polyvinyl acetal resin is that they contribute to the homogenization of the distribution of conductive powder and ceramic powder particles in the dried film. As a result, the film breakage phenomenon in the internal electrode layer obtained by firing the dried film is resolved, and the capacitance of the MLCC is increased.
[0093] In this embodiment, the conductive paste can contain one or more resins selected from cellulose resin and polyacetal resin, thus improving the flexibility in adjusting the viscosity of the conductive paste. In other words, since cellulose resin and polyacetal resin can be added as appropriate within the scope of this embodiment, the viscosity of the conductive paste can be easily adjusted.
[0094] The cellulose resin can be selected from methylcellulose resin, ethylcellulose resin, ethylhydroxyethylcellulose resin, nitrocellulose resin, etc., with ethylcellulose resin being preferred among these resins. Two or more of these resins may also be used in combination. Polyvinyl butyral can be selected as the polyvinyl acetal resin. Either the cellulose resin or the polyvinyl acetal resin may be used, or both may be used. Furthermore, the blending ratio of the cellulose resin, polyvinyl acetal resin and the polymer compound can be appropriately selected as long as it does not deviate from the scope of this embodiment. By selecting these resins and their blending ratios, the viscosity of the conductive paste and the adhesion of the resulting dried film to the green sheet can be appropriately adjusted.
[0095] In this embodiment, in addition to cellulose resin and polyvinyl acetal resin, known binder resins such as acrylic resin and maleic acid ester resin can also be added. The number-average molecular weight of the resins that can be added in this way, in addition to cellulose resin and polyvinyl acetal resin, is approximately 20,000 to 300,000, as determined by GCP (gel permeation chromatography) analysis.
[0096] (Organic solvents) The organic solvent is not particularly limited, and any known organic solvent capable of dissolving the binder resin can be used. Examples of organic solvents include acetate-based solvents such as isobornyl acetate, isobornyl propinate, isobornyl butyrate and isobornyl isobutyrate, ethylene glycol monobutyl ether acetate, dipropylene glycol methyl ether acetate, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate; terpene-based solvents such as terpineol, dihydro terpineol, dihydro terpinyl acetate, and terpinyl acetate; hydrocarbon-based solvents such as tridecane, nonane, and cyclohexane; and petroleum-based hydrocarbon solvents such as mineral spirits. One type of organic solvent may be used, or two or more types may be used. Compatibility with the ceramic green sheet may also be considered when selecting the solvent.
[0097] The content of the organic solvent is preferably 40 parts by mass or more and 100 parts by mass or less, and more preferably 65 parts by mass or more and 95 parts by mass or less, per 100 parts by mass of conductive powder. When the content of the organic solvent is 40 parts by mass or more and 100 parts by mass or less per 100 parts by mass of conductive powder, the conductivity and dispersibility are excellent.
[0098] The content of the organic solvent is preferably 20% to 60% by mass, and more preferably 35% to 55% by mass, relative to the total amount of the conductive paste. When the content of the organic solvent is 20% to 60% by mass relative to the total amount of the conductive paste, the conductivity and dispersibility are excellent.
[0099] (Dispersant) The conductive paste of this embodiment may contain a dispersant. The role of the dispersant is to adsorb onto the surface of the inorganic powder (conductive powder and ceramic powder) to suppress aggregation of the inorganic powders, or to improve wettability with the organic vehicle and disperse it within the conductive paste. The dispersant (surfactant) may include acidic dispersants containing higher fatty acids, polymeric surfactants, etc., cationic dispersants other than acidic dispersants, nonionic dispersants, amphoteric surfactants, polymeric dispersants, etc.
[0100] Furthermore, one or more dispersants may be selected, and the amount of conductive paste can be appropriately selected considering the viscosity, viscosity, and long-term storage properties of the conductive paste, and may be included within a range that does not hinder the effects of the present invention.
[0101] Furthermore, the mass-average molecular weight of the dispersant is preferably 200 to 100,000, more preferably 300 to 30,000. If the mass-average molecular weight is less than 200, the particles may not obtain sufficient electrostatic repulsion, which may reduce the dispersibility and storage stability of the particles. Normally, the dispersant is adsorbed onto the particle surface to form an adsorption layer of the dispersant, and by imparting electrostatic and steric repulsion to the particles, a paste with excellent dispersibility can be obtained. However, it is thought that over time, collisions between particles will overcome the repulsive force of the adsorption layer and cause the particles to aggregate, so a mass-average molecular weight of 200 or higher is preferable. Also, if the mass-average molecular weight is greater than 100,000, the compatibility with organic vehicles and organic solvents may decrease, leading to aggregation of particles and a decrease in dispersibility and storage stability. In addition, the viscosity of the conductive paste may become high.
[0102] The amount of dispersant added is preferably 0.01 to 5.00 parts by mass, and more preferably 0.20 to 2.00 parts by mass, per 100 parts by mass of conductive metal powder. If the amount of dispersant is less than 0.01 parts by mass, it tends to be difficult to obtain sufficient dispersibility. On the other hand, if it exceeds 5.00 parts by mass, drying performance deteriorates, and problems such as a decrease in the dry film density may occur.
[0103] The polymeric dispersant is preferably anionic and contains carboxyl groups or carboxylic acid anhydride groups. By using anionic polymeric dispersants, the dispersibility of inorganic powders such as conductive powders and ceramic powders into organic vehicles can be further improved. Here, a carboxylic acid anhydride group refers to a state in which H2O has been dehydrated from two carboxyl groups, resulting in an anhydride. Examples include acid anhydrides such as phthalic anhydride and maleic anhydride, which are molecular units composed of two carboxyl groups that have been dehydrated.
[0104] Anionic polymer dispersants are preferably equipped with graft chains. These graft chains are also expected to improve solubility in various organic solvents.
[0105] The mass-average molecular weight of the anionic polymer dispersant is preferably between 1,000 and 100,000, more preferably between 5,000 and 70,000, and even more preferably between 10,000 and 60,000. By setting the mass-average molecular weight of the polymer dispersant to 1,000 or more, the dispersibility of inorganic powders into organic vehicles can be improved. If the mass-average molecular weight is greater than 100,000, the compatibility with organic vehicles and organic solvents may decrease, or it may cause aggregation of particles such as conductive powders and ceramic powders, leading to a decrease in dispersibility and storage stability.
[0106] Such polymeric dispersants have carboxyl groups or carboxylic acid anhydride groups in the functional groups of their main chain. For anionic polymeric dispersants, it is desirable to further include oxyethylene groups in the graft chains for better adsorption with inorganic powders.
[0107] The anionic polymer dispersant may contain one or more types. That is, multiple types of polymer dispersants may be included depending on the length of the main chain, the length of the graft chain, and the presence or absence of graft chains. The content of the anionic polymer dispersant in the conductive paste can be appropriately selected considering the viscosity, viscosity, and long-term storage properties of the conductive paste, and may be included within a range that does not hinder the effects of the present invention.
[0108] Furthermore, the conductive paste of this embodiment may contain a dispersant in addition to the anionic polymer dispersant. For example, the dispersant (surfactant) may include acidic dispersants containing higher fatty acids, phosphoric acid, polymeric surfactants, etc., cationic dispersants other than acidic dispersants, nonionic dispersants, amphoteric surfactants, and polymeric dispersants.
[0109] Furthermore, the amount of dispersant in the conductive paste can be appropriately selected considering the viscosity, viscosity, and long-term storage properties of the conductive paste, and may be included within a range that does not hinder the effects of the present invention.
[0110] Furthermore, for both anionic polymer dispersants and other dispersants, the mass-average molecular weight of the dispersant is preferably 200 to 100,000. More preferably, it is 300 to 30,000. If the mass-average molecular weight is less than 200, the dispersibility and storage stability of the particles may decrease. Normally, a paste with excellent dispersibility is obtained by adsorbing the dispersant onto the particle surface to form an adsorption layer of the dispersant, and by imparting electrostatic and steric repulsion to the particles. However, it is thought that over time, collisions between particles cause the cohesive force of the particles to overcome the repulsive force of the adsorption layer, leading to particle aggregation, so a mass-average molecular weight of 200 or higher is preferable. Also, if the mass-average molecular weight is greater than 100,000, the compatibility with organic vehicles and organic solvents may decrease, leading to particle aggregation, and causing a decrease in dispersibility and storage stability. In addition, problems such as high paste viscosity may occur.
[0111] The total amount of anionic polymer dispersants and other dispersants added is preferably 0.01 to 5.00 parts by mass, and more preferably 0.20 to 2.00 parts by mass, per 100 parts by mass of conductive metal powder. If the amount of dispersant is less than 0.01 parts by mass, it tends to be difficult to obtain sufficient dispersibility. On the other hand, if it exceeds 5.00 parts by mass, drying performance will deteriorate, and problems such as a decrease in the dry film density may occur.
[0112] (Other additives) Furthermore, known additives such as plasticizers can be added to the conductive paste to impart flexibility to the dried film obtained from the conductive paste.
[0113] (Method for manufacturing conductive paste) The method for manufacturing the conductive paste of this embodiment is not particularly limited, and conventionally known methods can be used. The conductive paste can be manufactured, for example, by preparing each of the above components and stirring and kneading them in a three-roll mill, ball mill, mixer, etc. In this case, if a dispersant is applied to the surface of the conductive powder in advance, the conductive powder will not aggregate and will be sufficiently loosened, and the dispersant will spread evenly over the surface, making it easier to obtain a uniform conductive paste. Alternatively, the binder resin may be dissolved in an organic solvent for the vehicle to prepare an organic vehicle, and the conductive powder, ceramic powder, organic vehicle and dispersant may be added to the organic solvent for the paste, and the mixture may be stirred and kneaded in a mixer to produce the conductive paste.
[0114] Furthermore, it is preferable to use the same organic solvent for the conductive paste as the organic solvent used to adjust the viscosity of the conductive paste, in order to improve the compatibility of the organic vehicle with the conductive paste. The content of the organic solvent for the vehicle is, for example, 5 parts by mass or more and 80 parts by mass or less per 100 parts by mass of conductive powder. Also, the content of the organic solvent for the vehicle is preferably 10% by mass or more and 40% by mass or less relative to the total amount of conductive paste.
[0115] The surface smoothness of the dried film formed by printing the conductive paste can be evaluated by its surface roughness. The surface roughness of the conductive paste can be measured, for example, by the method described in the examples (a method of measuring the arithmetic mean height Sa based on the ISO 25178 standard using a VK-X120 manufactured by Keyence Corporation). When the surface smoothness of the dried film is evaluated by the arithmetic mean height Sa, it is preferable that the value is 0.10 μm or less.
[0116] If the surface roughness is 0.10 μm or less using the method described in the examples, low surface roughness can be achieved even after printing and drying on the green sheet. Considering the manufacturing process of multilayer ceramic capacitors, if the surface roughness of the dried conductive paste film is low, the dried conductive paste film adheres to the green sheet as a surface, resulting in excellent adhesion between the dried conductive paste film and the green sheet. Therefore, it is desirable for the surface roughness of the dried conductive paste film to be as low as possible.
[0117] [Electronic components, multilayer ceramic capacitors] The conductive paste of the present invention can be suitably used in electronic components such as multilayer ceramic capacitors. A multilayer ceramic capacitor has a dielectric layer formed using a green sheet and an internal electrode layer formed using the conductive paste.
[0118] In multilayer ceramic capacitors, it is preferable that the dielectric ceramic powder contained in the green sheet and the ceramic powder contained in the conductive paste have the same composition; for example, barium titanate can be used. In multilayer ceramic capacitors manufactured using the conductive paste of this embodiment, sheet attack and peeling defects of the green sheet are suppressed even when the thickness of the green sheet is, for example, 3 μm or less.
[0119] Embodiments of the electronic components of the present invention will be described below with reference to the drawings. In the drawings, schematic representations and changes in scale may be made as appropriate. The position and orientation of the components will be described with reference to the XYZ Cartesian coordinate system shown in Figures 1A and 1B as appropriate. In this XYZ Cartesian coordinate system, the X and Y directions are horizontal directions, and the Z direction is vertical (up and down direction).
[0120] Figures 1A and 1B are perspective and side cross-sectional views, respectively, of a multilayer ceramic capacitor 1, which is an example of an electronic component according to the embodiment. The multilayer ceramic capacitor 1 comprises a ceramic laminate 10 in which dielectric layers 12 and internal electrode layers 11 are alternately stacked, and an external electrode 20.
[0121] The manufacturing method of the multilayer ceramic capacitor 1 using the conductive paste described above will be explained below. First, a conductive paste is printed onto a dielectric layer made of a green sheet and dried to form a dried film. Multiple dielectric layers having this dried film on their upper surface are stacked and pressed together to obtain a laminate. After that, the laminate is fired to integrate it, thereby creating a ceramic laminate 10 in which internal electrode layers 11 and dielectric layers 12 are stacked alternately. Subsequently, a pair of external electrodes 20 are formed at both ends of the ceramic laminate 10 to manufacture the multilayer ceramic capacitor 1. A more detailed explanation will be provided below.
[0122] First, a green sheet, which is an unfired ceramic sheet using a dielectric material, is prepared. Examples of this green sheet include a dielectric layer paste obtained by adding an organic binder such as polyvinyl butyral and a solvent such as terpineol to a predetermined ceramic raw material powder such as barium titanate, which is then applied in a sheet shape to a support film such as a PET film, dried, and the solvent removed. The thickness of the dielectric layer made of the green sheet is not particularly limited, but from the viewpoint of miniaturizing multilayer ceramic capacitors, a thickness of 0.05 μm to 3 μm is preferred.
[0123] Next, several sheets are prepared by printing (coating) the above-mentioned conductive paste onto one side of the green sheet using a known method such as screen printing, and then drying them to form a dried film. It is preferable that the thickness of the conductive paste (dried film) after printing is such that the thickness of the dried film after drying is 1 μm or less, from the viewpoint of the requirement for thinning the internal electrode layer 11.
[0124] Next, the green sheets are peeled off the support film, and the dielectric layers made of the green sheets and the dried films formed on one side of them are laminated alternately. Then, a laminate is obtained by heating and pressurizing. Alternatively, protective green sheets without conductive paste can be further arranged on both sides of the laminate.
[0125] Next, the laminate is cut to a predetermined size to form green chips, and then the green chips are subjected to a debinder treatment and fired in a reducing atmosphere to produce the ceramic laminate 10. The atmosphere used for the debinder treatment is preferably air or an N2 gas atmosphere. The temperature used for the debinder treatment is, for example, 200°C to 400°C. Furthermore, the holding time at the above temperature during the debinder treatment is preferably 0.5 hours to 24 hours. The firing is performed in a reducing atmosphere to suppress oxidation of the metal used in the internal electrode layer, and the firing temperature of the laminate is, for example, 1000°C to 1350°C, with a holding time at the temperature of 0.5 hours to 8 hours.
[0126] By firing the green chips, the organic binder in the green sheet is completely removed, and the ceramic raw material powder is fired to form a ceramic dielectric layer 12. In addition, the organic vehicle in the dried film is removed, and nickel powder or nickel-based alloy powder is sintered or melted and integrated to form an internal electrode layer 11, thereby forming a multilayer ceramic fired body in which multiple dielectric layers 12 and internal electrode layers 11 are alternately stacked. Furthermore, from the viewpoint of incorporating oxygen into the dielectric layer to improve reliability and suppressing re-oxidation of the internal electrodes, the multilayer ceramic fired body may be subjected to annealing treatment after firing.
[0127] Then, a multilayer ceramic capacitor 1 is manufactured by providing a pair of external electrodes 20 to the fabricated multilayer ceramic firing body. For example, the external electrodes 20 comprise an external electrode layer 21 and a plating layer 22. The external electrode layer 21 is electrically connected to the internal electrode layer 11. Suitable materials for the external electrodes 20 include, for example, copper, nickel, or alloys thereof. The electronic component is not limited to a multilayer ceramic capacitor, but may be an electronic component other than a multilayer ceramic capacitor, such as a varistor. [Examples]
[0128] The present invention will be described in detail below based on examples and comparative examples, but the present invention is not limited in any way by the examples.
[0129] <Synthesis of polymer compounds> [Materials used] <Conductive powder> Ni powder (number-average particle size of 0.2 μm as measured by SEM) was used as the conductive powder.
[0130] <Ceramic powder> Barium titanate (number-average particle size of 0.05 μm as measured by BaTiO3 SEM) was used as the ceramic powder.
[0131] <Binder resin> The binder resin was synthesized as follows:
[0132] (Synthesis of cellulosic compounds (1a) containing vinyl groups) Ethyl cellulose (Dow Chemical's "EthoCell STD-100," number-average molecular weight Mn (standard polystyrene equivalent value by GPC): 63420, average number of unetherified hydroxyl groups on one cyclic structure of the glucose ring: 0.48) was prepared and dried. The purpose of drying the ethyl cellulose here is to remove the water adsorbed by the ethyl cellulose. Drying was performed at room temperature under reduced pressure.
[0133] A solution was obtained by dissolving 100 parts by mass of the dried ethylcellulose in 900 parts by mass of ethyl acetate. To the obtained solution, 0.17 parts by mass of 3-allyloxypropionic acid (corresponding to an average of 1 group per molecule of ethylcellulose), 0.20 parts by mass of diisopropylcarbodiimide as a condensing agent, and 0.004 parts by mass of dimethylaminopyridine as a reaction accelerator were added, and the reaction was carried out by stirring at a temperature of 40°C for 5 hours. After that, by removing the ethyl acetate, a cellulosic compound (1a) in which a vinyl group was introduced into ethylcellulose was obtained as a solid.
[0134] Analysis of a portion of the obtained solid cellulosic compound (1a) by FT-IR and 1H-NMR confirmed the formation of ester bonds and the introduction of the same molar amount of vinyl groups as the charged 3-allyloxypropionic acid into the ethylcellulose.
[0135] Note that cellulosic compound (1a) contains a mixture of ethylcellulose into which a vinyl group has been introduced, as well as unreacted ethylcellulose. In this example, this mixture is referred to as cellulosic compound (1a). The same applies to cellulosic compound (2a), which will be described later.
[0136] (Synthesis of polyvinyl butyral compounds (1b) having thiol groups) Polyvinyl butyral (BM-SZ, manufactured by Sekisui Chemical Co., Ltd., number average molecular weight Mn (standard polystyrene equivalent value by GPC): 55,000, hydroxyl group amount: approximately 22 mol%) was prepared and dried. The purpose of drying the polyvinyl butyral is to remove the water adsorbed by it. Drying was performed at room temperature under reduced pressure. 100 parts by mass of the dried polyvinyl butyral was dissolved in 900 parts by mass of ethyl acetate. To the resulting solution, 0.20 parts by mass of 3-mercaptopropionic acid (corresponding to an average of 1 thiol group per molecule of polyvinyl butyral), 0.24 parts by mass of diisopropylcarbodiimide as a condensing agent, and 0.005 parts by mass of dimethylaminopyridine as a reaction accelerator were added, and the reaction was carried out by stirring at a temperature of 40°C for 5 hours. After that, by removing the ethyl acetate, a polyvinyl butyral compound (1b) in which thiol groups were introduced into polyvinyl butyral was obtained as a solid.
[0137] Analysis of a portion of the obtained solid polyvinyl butyral compound (1b) by FT-IR and 1H-NMR confirmed the formation of ester bonds and the introduction of the same molar amount of thiol groups as the charged 3-mercaptopropionic acid into the polyvinyl butyral.
[0138] Note that polyvinyl butyral compound (1b) contains a mixture of polyvinyl butyral with thiol groups introduced and unreacted polyvinyl butyral. In this example, this mixture is referred to as polyvinyl butyral compound (1b). The same applies to polyvinyl butyral compound (2b), which will be described later.
[0139] (Synthesis of cellulosic compounds (2a) containing vinyl groups) Cellulose-based compound (2a) was synthesized in the same manner as cellulose-based compound (1a), except that 3-allyloxypropionic acid, equivalent to an average of two molecules per molecule of ethylcellulose, was added.
[0140] (Synthesis of polyvinyl butyral compounds (2b) having thiol groups) Polyvinyl butyral compound (2b) was synthesized in the same manner as polyvinyl butyral compound (1b), except that 3-mercaptopropionic acid equivalent to an average of two molecules per molecule of polyvinyl butyral was added.
[0141] (Synthesis of polymer compound 1) Five parts by mass of cellulosic compound (1a) and four and a half parts by mass of polyvinyl butyral compound (1b) were dissolved in sixty parts by mass of dihydroterpineol as a solvent. This solution was transferred to a glass flask reaction vessel, purged with nitrogen, and then 0.1 parts by mass of azobisisobutyronitrile was added to the solution as a radical generator. The reaction was carried out at 80°C for three hours with stirring to obtain organic vehicle 1 containing polymer compound 1. Here, the cellulosic compound (1a) and polyvinyl butyral compound (1b) were in the same number of moles. Organic vehicle 1 contained 13.5% by mass of polymer compound 1.
[0142] In this example, polymer compound 1 is a polymer compound formed by the bonding of a cellulosic compound (1a) and a polyvinyl butyral compound (1b), and contains a mixture of unreacted ethylcellulose and unreacted polyvinyl butyral. In this example, this mixture is referred to as polymer compound 1. The same applies to polymer compound 2, which will be described below.
[0143] Furthermore, analysis of the generated polymer compound 1 by FT-IR and 1H-NMR confirmed the presence of -S- bonds, indicating that the desired structure was obtained. In addition, the mass-average molecular weight (Mw: standard polystyrene equivalent value calculated by GPC) of polymer compound 1 was measured.
[0144] (Synthesis of polymer compound 2) Polymer compound 2, synthesized from a cellulosic compound (2a) and a polyvinyl butyral compound (2b), was synthesized in the same manner as polymer compound 1 to obtain organic vehicle 2. The content of polymer compound 2 in organic vehicle 2 was set to 13.5% by mass.
[0145] Furthermore, analysis of the generated polymer compound 2 by FT-IR and 1H-NMR confirmed the presence of -S- bonds, indicating that the desired structure was obtained. In addition, the mass-average molecular weight (Mn: GPC equivalent value for standard polystyrene) of polymer compound 2 was measured.
[0146] Table 1 shows the characteristics of the cellulose-based compounds (1a) and (2a) and the polyvinyl acetal-based compounds (1b) and (2b) used in polymer compounds 1 and 2, as well as the mass-average molecular weight of the polymer compounds.
[0147] [Table 1]
[0148] [Reference example 1] Reference Example 1 is an example in which only polymer compound 1 is used as the binder resin, without using ethylcellulose and polyvinyl butyral resin. A conductive paste was prepared as follows, and the physical properties of the dried film obtained using the conductive paste were evaluated.
[0149] <Creating conductive paste> <Preparation of conductive paste 1a> A conductive paste 1a according to Reference Example 1 was prepared by blending 47% by mass of Ni powder, 4.7% by mass of ceramic (BT) powder, 26.67% by mass of organic vehicle 1, 0.4% by mass of an anionic polymer dispersant of high molecular weight polycarboxylic acid (mass average molecular weight 40000), and 21.23% by mass of the remaining organic solvent (dihydroterpineol), for a total of 100% by mass. These materials were then mixed to prepare conductive paste 1a according to Reference Example 1. The prepared conductive paste 1a was printed and dried as follows, and the surface roughness and dry film density of the dried film were evaluated, and the surface of the dried film was observed.
[0150] <Preparation of conductive paste 1b> For cross-sectional observation of the dried film, conductive paste 1b was prepared by mixing conductive paste 1a (25.5% by mass), organic vehicle 1 (46.5% by mass), and dihydroterpineol (28% by mass) so that the total weight of Ni powder was 12% by mass. These materials were then mixed to prepare conductive paste 1b according to Reference Example 1. The conductive paste 1b was printed and dried as follows, and the resulting dried film was cut to obtain a sample for cross-sectional observation of the dried film according to Reference Example 1. Conductive paste 1b contains 12% by mass of Ni powder and 53.34% by mass of organic vehicle (twice the amount of conductive paste 1a).
[0151] For cross-sectional observation of the dried film, conductive paste 1b was prepared by adding organic vehicle 1 and dihydroterpineol to conductive paste 1a to reduce the Ni powder content in the paste. This is because, when observing a dried film formed using conductive paste 1a, which has a Ni powder content of 47% by mass, it can be difficult to observe the uneven distribution of the binder resin due to the excessive amount of Ni powder. The same applies to Example 1 and Comparative Examples 1 and 2. With a Ni powder content of 12% by mass, as in conductive paste 1b, it becomes easier to observe the uneven distribution and phase separation of the binder resin in the cross-section of the dried film. However, binder resins that are prone to uneven distribution and phase separation will continue to exhibit problems such as uneven distribution even if the Ni powder content is increased.
[0152] [Evaluation Method] (Dispersibility: Surface roughness of the dried film and SEM observation of the dried film) <Surface roughness, SEM observation of the dry film surface> A 20 mm square, 1-3 μm thick dried film was fabricated by screen printing the prepared conductive paste 1a onto a 2.54 cm (1 inch) square heat-resistant tempered glass surface and drying it in air at 120°C for 1 hour. When the conductive paste has good dispersibility, the surface of the dried film is smooth. When the dispersibility is poor, aggregation occurs within the conductive paste, the surface of the dried film becomes rough, and the surface smoothness decreases. Therefore, the surface roughness Sa (arithmetic mean height) of the fabricated dried film was measured using a laser microscope (Keyence VK-X120) according to the ISO 25178 standard. A smaller value of surface roughness Sa (arithmetic mean height) indicates a smoother surface of the dried film. The surface of the obtained dried film was also observed using a scanning electron microscope (SEM).
[0153] <SEM observation of a cross-section of a dried film> Using conductive paste 1b, a dried film was prepared in the same manner as conductive paste 1a. The dried film was then split to form a cross-section, which was observed using SEM. This observation allows us to confirm the effect of phase separation, caused by the poor mismatch between ethyl cellulose and polyvinyl butyral resin, on the distribution (dispersion) of inorganic particles (Ni particles, BT particles) in the dried film. In reference example 1, ethyl cellulose and polyvinyl butyral resin were not used as binders, and only polymer compound 1 was used. Therefore, the cross-section of the dried film is in the best condition and should be used for comparison with the cross-sections of dried films in other examples.
[0154] <Dry film density> The prepared conductive paste 1a was placed on a PET film and spread to a length of approximately 100 mm using an applicator with a width of 50 mm and a gap of 125 μm. The resulting PET film was dried at 120°C for 40 minutes to form a dry body. After that, the dry body was cut into four 2.54 cm (1 inch) squares, the PET film was peeled off, and the thickness and weight of each of the four dry films were measured to calculate the average dry film density.
[0155] The evaluation results are shown in Tables 2 and 3. Table 2 shows the binder resin information, the surface roughness of the dried film, and the dried film density. Table 3 shows the type of polymer compound used, the proportion of the polymer compound in the binder resin, the total proportion of ethylcellulose and polyvinyl butyral resin in the binder resin, the SEM image of the surface of the dried film, and the SEM image of the cross-section of the dried film. Note that the binder resin contained in conductive paste 1a related to Reference Example 1 is 3.6% by mass.
[0156] [Comparative Example 1] Comparative Example 1 is an example in which ethyl cellulose and polyvinyl butyral resin are used as binder resins, and neither polymer compound 1 nor 2 is used. A conductive paste was prepared as follows, and the physical properties of the dried film obtained using the conductive paste were evaluated.
[0157] <Creating conductive paste> <Preparation of conductive paste 2a> Organic vehicle 3a was prepared by dissolving 5 parts by mass of ethylcellulose (EC Dow Chemical's "Etocell STD-100", number average molecular weight Mn (standard polystyrene equivalent value by GPC): 63420, average number of unetherified hydroxyl groups in one molecule of the cyclic structure of the glucose ring: 0.48) in 30 parts by mass of terpineol. Organic vehicle 3b was prepared by dissolving 4.35 parts by mass of polyvinyl butyral resin (PVB Sekisui Chemical's "BM-SZ", number average molecular weight Mn (standard polystyrene equivalent value by GPC): 55000, hydroxyl group amount: approximately 22 mol%) in 30 parts by mass of terpineol. Organic vehicle 3 was then prepared by mixing organic vehicle 3a and organic vehicle 3b in equal amounts.
[0158] Conductive paste 2a was prepared by mixing 47% by mass of Ni powder, 4.7% by mass of ceramic (BT) powder, 26.67% by mass of organic vehicle 3, 0.4% by mass of anionic polymer dispersant of molecular polycarboxylic acid (weight-average molecular weight 40000), and 21.23% by mass of the remaining organic solvent (dihydroterpineol), for a total of 100% by mass.
[0159] <Preparation of conductive paste 2b> For observing the cross-section of the dried film, conductive paste 2b was prepared by mixing conductive paste 2a (25.5% by mass), organic vehicle 3 (46.5% by mass), and dihydroterpineol (28% by mass) so that the Ni powder content was 12% by mass. These materials were then mixed to produce conductive paste 2b according to Comparative Example 1.
[0160] Using the obtained conductive pastes 2a and 2b, the surface roughness of the dried film of Comparative Example 1, SEM observation of the dried film surface and cross-section, and measurement of the dried film density were performed in the same manner as in Reference Example 1.
[0161] [Example 1] Example 1 is an example in which ethyl cellulose, polyvinyl butyral resin, and polymer compound 1 are used as binder resins. A conductive paste was prepared as follows, and the physical properties of the dried film obtained using the conductive paste were evaluated.
[0162] <Creating conductive paste> <Preparation of conductive paste 3a> A conductive paste 3a according to Example 1 was prepared by blending 47% by mass of Ni powder, 4.7% by mass of ceramic (BT) powder, 8% by mass of organic vehicle 1, 18.67% by mass of organic vehicle 3, 0.4% by mass of an anionic polymeric dispersant of high molecular weight polycarboxylic acid (weight-average molecular weight 40000), and 21.23% by mass of the remaining organic solvent (dihydroterpineol), for a total of 100% by mass. These materials were then mixed to produce conductive paste 3a according to Example 1.
[0163] The total amount of binder resin contained in conductive paste 3a is 3.6% by mass, with polymer compound 1 accounting for 1.08% by mass, ethyl cellulose for 1.35% by mass, and polyvinyl butyral resin for 1.17% by mass. The proportion of polymer compound 1 in the binder resin is 30% by mass, and the total proportion of ethyl cellulose and polyvinyl butyral resin in the binder resin is 70% by mass. In Example 1, polymer compound 1 had an average of 1 functional group introduced into the cellulosic compound and the polyvinyl butyral compound; that is, one vinyl group was introduced per molecule of ethyl cellulose and one thiol group was introduced per molecule of polyvinyl butyral.
[0164] <Preparation of conductive paste 3b> For observing the cross-section of the dried film, conductive paste 3b was prepared by mixing conductive paste 3a (25.5% by mass), organic vehicle 1 (14.0% by mass), organic vehicle 3 (32.5% by mass), and dihydroterpineol (28% by mass) so that the Ni powder content was 12% by mass. These materials were then mixed to produce conductive paste 3b according to Example 1.
[0165] Using the obtained conductive pastes 3a and 3b, the surface roughness of the dried film in Example 1, SEM observation of the dried film surface and cross-section, and measurement of the dried film density were performed in the same manner as in Reference Example 1.
[0166] [Comparative Example 2] Comparative Example 2 is an example in which ethyl cellulose, polyvinyl butyral resin, and polymer compound 2 are used as binder resins. A conductive paste was prepared as follows, and the physical properties of the dried film obtained using the conductive paste were evaluated.
[0167] <Creating conductive paste> <Preparation of conductive paste 4a> A conductive paste 4a according to Comparative Example 2 was prepared by blending 47% by mass of Ni powder, 4.7% by mass of ceramic (BT) powder, 8% by mass of organic vehicle 2, 18.67% by mass of organic vehicle 3, 0.4% by mass of an anionic polymeric dispersant of high molecular weight polycarboxylic acid (weight-average molecular weight 40000), and 21.23% by mass of the remainder of the organic solvent (dihydroterpineol), totaling 100% by mass. These materials were then mixed to prepare conductive paste 4a according to Comparative Example 2.
[0168] The total amount of binder resin contained in conductive paste 4a is 3.6% by mass, with polymer compound 2 accounting for 1.08% by mass, ethyl cellulose for 1.35% by mass, and polyvinyl butyral resin for 1.17% by mass. The proportion of polymer compound 2 in the binder resin is 30% by mass, and the total proportion of ethyl cellulose and polyvinyl butyral resin in the binder resin is 70% by mass. In comparative example 2, polymer compound 2 had an average of 2 functional groups introduced into the cellulosic compound and the polyvinyl butyral compound; that is, 2 vinyl groups were introduced per molecule of ethyl cellulose and 2 thiol groups were introduced per molecule of polyvinyl butyral.
[0169] Using the obtained conductive paste 4a, the surface roughness and dry film density of the dried film of Comparative Example 2 were measured in the same manner as in Reference Example 1.
[0170] [Table 2]
[0171] [Table 3]
[0172] [Evaluation Results] As shown in Table 2, the dried films formed with the conductive pastes of Reference Example 1 and Example 1 had a lower surface roughness Sa (arithmetic mean height) of 0.1 μm or less and a dried film density of 5 g / cm³ compared to Comparative Example 1. 3The results were as described above. In contrast, Comparative Example 2, in which an average of two functional groups were introduced into the polymer compound, showed a high dry film density but inferior surface roughness. Here, a higher dry film density is preferable because it results in less shrinkage during firing.
[0173] Table 3 shows SEM images of the surface and cross-section of the dried films in Reference Example 1, Example 1, and Comparative Example 1. Although Comparative Example 2 used a polymer compound, its surface roughness was inferior to that of Example 1 and Reference Example 1, so SEM observation of the surface and cross-section of the dried film was not performed, and the results are not shown in Table 3. As can be seen from the SEM image of the cross-section of the dried film in Example 1 in Table 3, it is a film with fewer irregularities compared to the dried film of Comparative Example 1.
[0174] Furthermore, the cross-sectional SEM images in Table 3 show that while both Reference Example 1 and Example 1 have fine voids scattered throughout the dried film, Comparative Example 1 has voids approximately 20 μm in thickness.
[0175] From the above results, it is considered that in the internal electrode films obtained by firing the dried films of Reference Example 1 and Example 1, voids without conductive material are unlikely to occur. However, in the internal electrode film obtained by firing the dried film of Comparative Example 1, it is highly likely that voids without conductive material will occur, caused by voids of about 20 μm in the thickness direction of the dried film. The voids of about 20 μm seen in the cross-sectional SEM image of Comparative Example 1 shown in Table 3 are considered to be voids formed due to phase separation caused by the poor compatibility of ethyl cellulose and polyvinyl butyral resin, which are binder resins of the conductive paste related to Comparative Example 1. [Industrial applicability]
[0176] Based on the above, the conductive paste of the present invention can be suitably used as a raw material for internal electrodes of multilayer ceramic capacitors, which are chip components (electronic components) of electronic devices such as mobile phones and digital devices, and is therefore industrially useful. [Explanation of Symbols]
[0177] 1. Multilayer ceramic capacitor 10 Ceramic Laminate 11 Internal electrode layer 12 Dielectric layer 20 External electrode 21 External electrode layer 22 Plating layer
Claims
1. It contains conductive powder, ceramic powder, a dispersant, a binder resin, and an organic solvent. The binder resin comprises one or more resins selected from cellulose resin and polyvinyl acetal resin, and a polymer compound in which a cellulose-based compound and a polyvinyl acetal-based compound are bonded by a sulfur atom. In the polymer compound, the molar ratio of the sulfur atom to the cellulosic compound is 0.3 to 1.
7. A conductive paste comprising 20% by mass or more of the polymer compound, relative to the total mass of the cellulose resin, the polyvinyl acetal resin, and the polymer compound.
2. The aforementioned cellulosic compound is a cellulose derivative having a thiol group or a vinyl group, The polyvinyl acetal compound is a polyvinyl acetal resin having a thiol group or a vinyl group. If the cellulose derivative comprises a thiol group, the polyvinyl acetal resin comprises a vinyl group that reacts with the thiol group. The conductive paste according to claim 1, wherein, if the cellulose derivative comprises a vinyl group, the polyvinyl acetal resin comprises a thiol group that reacts with the vinyl group.
3. The cellulose derivative is ethylcellulose having a thiol group or a vinyl group, The conductive paste according to claim 2, wherein the polyvinyl acetal resin is polyvinyl butyral having thiol groups or vinyl groups.
4. The aforementioned cellulosic compound is a first esterification reaction product obtained by dehydration condensation of a carboxyl group of a carboxylic acid having a thiol group or a vinyl group and a hydroxyl group of cellulose. The aforementioned polyvinyl acetal compound is a second esterification reaction product obtained by dehydration condensation of a carboxyl group of a carboxylic acid having a thiol group or a vinyl group and a hydroxyl group of polyvinyl acetal. If the first esterification reaction product comprises a thiol group, the second esterification reaction product comprises a vinyl group, If the first esterification reaction product comprises a vinyl group, the second esterification reaction product comprises a thiol group, The conductive paste according to claim 1, wherein the polymer compound is a thiol-ene reaction product of the first esterification reaction product and the second esterification reaction product.
5. The first esterification reaction product is an esterification reaction product obtained by dehydration condensation of the carboxyl group of 3-allyloxypropionic acid and the hydroxyl group of ethylcellulose. The conductive paste according to claim 4, wherein the second esterification reaction product is an esterification reaction product obtained by dehydration condensation of the carboxyl group of 3-mercaptopropionic acid and the hydroxyl group of polyvinyl butyral.
6. The conductive paste according to claim 1, wherein the cellulose resin is an ethyl cellulose resin and the polyvinyl acetal resin is a polyvinyl butyral resin.
7. The conductive paste according to claim 1, wherein the conductive powder is nickel powder.
8. The conductive paste according to claim 1, wherein the number-average particle size of the conductive powder is 0.05 μm or more and 1.0 μm or less.
9. The conductive paste according to claim 1, wherein the ceramic powder contains barium titanate.
10. The conductive paste according to claim 1, wherein the number-average particle size of the ceramic powder is 0.01 μm or more and 0.5 μm or less.
11. The conductive paste according to claim 1, wherein the content of the ceramic powder is 1% by mass or more and 20% by mass or less.
12. The conductive paste according to claim 1, for use as an internal electrode in a multilayer ceramic component.
13. An electronic component formed using the conductive paste described in claim 1.
14. The laminate comprises at least a dielectric layer and an internal electrode layer, The internal electrode layer is formed using the conductive paste described in claim 1, in a multilayer ceramic capacitor.
Citation Information
Patent Citations
Printer
JP1977024722A
Method of electrolytically oxidizing metallic ions
JP1977099904A
Conductive paste for internal electrode of multilayer electronic component and multilayer electronic component using the same
JP2004186339A
Polymer compound and polymer composition containing the same, and inorganic particle-containing composition
JP2020029479A
Resin composition for paste and inorganic particle-dispersed paste
JP2020090661A