Electrode assembly and secondary battery containing the same
The electrode assembly design in cylindrical batteries adjusts the negative electrode insertion to reduce relative sliding, preventing separator damage and internal short circuits, thereby enhancing stability and lifespan.
Patent Information
- Application Number
- JP2025535407
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-07-05
- Filing Date
- 2024-07-07
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-07-07
AI Technical Summary
Cylindrical batteries with jelly roll-shaped electrode assemblies experience significant deformation due to contraction and expansion, leading to separator membrane damage and internal short circuits, especially with multiple tabs or silicon-based active materials, which increase pressure and risk of heat generation and ignition.
The electrode assembly design includes a negative electrode with a negative electrode current collector and active material layer, and a plain portion, where the active material layer extends 0.5 turns or less from the positive electrode end, allowing for adjusted insertion of the negative electrode to facilitate sliding and reduce relative sliding, thereby preventing damage to the separator membrane and internal short circuits.
This design enhances battery stability and lifespan by preventing separator membrane damage and internal short circuits, improving charge-discharge efficiency and extending the battery's life characteristics.
Smart Images

Figure 0007948514000002 
Figure 0007948514000003 
Figure 0007948514000004
Abstract
Description
[Technical Field]
[0001] The present invention relates to an electrode assembly and a secondary battery including the same, and more specifically to an electrode assembly in which the amount of core negative electrode input is adjusted and a cylindrical secondary battery including the same. This application claims the benefit as of the filing date of Korean Patent Application No. 10-2023-0088068, filed with the Korean Intellectual Property Office on July 7, 2023, the contents of which are contained herein. [Background technology]
[0002] In the case of cylindrical batteries, a jelly roll-shaped electrode assembly is manufactured by winding long electrodes of a fixed width into a roll. Cylindrical batteries manufactured by inserting such electrode assemblies into a battery case undergo repeated contraction and expansion of the electrodes during charging and discharging. In particular, if an in tab is located in the core of the electrode assembly, or if silicon-based active material is added to the negative electrode, increasing the degree of contraction and expansion of the electrode assembly, the pressure acting on the core of the electrode assembly will increase significantly.
[0003] Recently, with the increasing demand for low-resistance / high-capacitance designs, electrode assemblies are increasingly incorporating multiple tabs or silicon-based active materials. This increases the possibility of deformation of the electrode assembly located in the core due to contraction / expansion of the electrode assembly. In particular, if the separator membrane located between the negative and positive electrodes is damaged, the negative and positive electrodes can come into direct contact, causing an internal short circuit that generates heat and ignition.
[0004] To solve the problems of separation membrane damage and internal short circuits caused by deformation of such electrode assemblies, there is a need to develop technologies that can protect the negative electrode and separation membrane in the affected area and suppress the occurrence of internal short circuits. [Overview of the Initiative] [Problems that the invention aims to solve]
[0005] The present invention aims to provide an electrode assembly with a modified design and a secondary battery containing the same.
[0006] However, the problems that the present invention aims to solve are not limited to those described above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0007] One embodiment of the present invention provides an electrode assembly in which a negative electrode, a separator membrane, and a positive electrode are sequentially laminated and wound together in a core portion, wherein the negative electrode includes a negative electrode current collector and a negative electrode active material layer portion provided on at least one surface of the negative electrode current collector; and a negative electrode plain portion including a negative electrode current collector without the negative electrode active material layer, and the longitudinal length of the negative electrode active material layer portion extending from the longitudinal end of the positive electrode is 0.5 turns or less from the longitudinal end of the positive electrode.
[0008] Another embodiment of the present invention provides a secondary battery including the electrode assembly and a battery case for housing the electrode assembly. [Effects of the Invention]
[0009] An electrode assembly according to one embodiment of the present invention can adjust the amount of negative electrode inserted into the core to facilitate the sliding of the negative electrode during battery charging and discharging, and can reduce the relative sliding of the positive electrode end relative to the negative electrode.
[0010] Furthermore, a secondary battery according to one embodiment of the present invention can prevent damage to the negative electrode and separator membrane due to relative sliding of the positive electrode ends, and can prevent internal short circuits between the positive and negative electrodes, thereby improving battery stability and lifespan characteristics.
[0011] The effects of the present invention are not limited to those described above, and any effects not mentioned will be clearly understood by those skilled in the art from this specification and the accompanying drawings. [Brief explanation of the drawing]
[0012] [Figure 1] This is a diagram schematically showing an electrode assembly according to one embodiment of the present invention. [Figure 2] This is a diagram schematically showing an electrode assembly according to one embodiment of the present invention. [Figure 3] This is a diagram schematically showing an electrode assembly according to one embodiment of the present invention. [Figure 4] This is a CT image showing the evaluation results of cycle stability of the secondary batteries according to Example 1, Comparative Example 1 and Comparative Example 2. [Figure 5] This is a diagram showing a method for evaluating the presence or absence of separator damage in the core part of an electrode assembly according to one embodiment of the present invention. [Figure 6] This is a graph showing the evaluation results of the presence or absence of separator damage in the core part of the secondary batteries according to Example 1 and Comparative Example 2. [Figure 7] This is a diagram showing an electrode assembly according to one embodiment of the present invention and a secondary battery including the same. [Figure 8] This is a diagram showing an electrode assembly according to one embodiment of the present invention and a secondary battery including the same. [Mode for Carrying Out the Invention]
[0013] Throughout the present specification, when a part is said to "comprise" a certain constituent element, this means that, unless otherwise specifically stated, it does not exclude other constituent elements, but may further include other constituent elements.
[0014] Throughout the present specification, when a member is described as being located "on" another member, this includes not only the case where a member is in contact with another member, but also the case where another member exists between the two members.
[0015] Throughout this specification, “winding axis of electrode assembly” may mean a hypothetical line located at the center of the hollow core H of the wound electrode assembly 1. The hollow core H may be formed at the location of a winding core C that has been removed after being used to wind the components included in the electrode assembly.
[0016] As a result, the components included in the wound electrode assembly may each have a defined direction in the winding axis direction of the electrode assembly, that is, a direction parallel to the winding axis of the electrode assembly (Z-axis direction).
[0017] Furthermore, with respect to a cross-section (XY plane) perpendicular to the winding shaft of the electrode assembly, the components included in the wound electrode assembly may each be defined in a direction opposite to the winding shaft of the electrode assembly, that is, a direction toward the center of the hollow H of the core portion of the wound electrode assembly 1.
[0018] The present invention will be described in detail below with reference to the drawings. However, the drawings are for illustrative purposes only, and the scope of the present invention is not limited by the drawings.
[0019] One embodiment of the present invention provides an electrode assembly in which a negative electrode, a separator membrane, and a positive electrode are sequentially laminated and wound together in a core portion, wherein the negative electrode includes a negative electrode current collector and a negative electrode active material layer portion provided on at least one surface of the negative electrode current collector; and a negative electrode plain portion including a negative electrode current collector without the negative electrode active material layer, and the longitudinal length of the negative electrode active material layer portion extending from the longitudinal end of the positive electrode is 0.5 turns or less from the longitudinal end of the positive electrode.
[0020] An electrode assembly according to one embodiment of the present invention allows for easy sliding of the negative electrode during battery charging and discharging by adjusting the amount of negative electrode inserted into the core, thereby reducing the relative sliding of the positive electrode end relative to the negative electrode. Furthermore, by reducing the relative sliding of the positive electrode end relative to the negative electrode during battery charging and discharging, damage to the negative electrode and separator membrane due to deformation of the electrode assembly caused by electrode contraction / expansion can be prevented, and internal short circuits between the positive and negative electrodes can be prevented, thereby improving battery stability and life characteristics. Specifically, the effect of reducing the relative sliding of the positive electrode end by adjusting the amount of negative electrode inserted into the core within the range described above can be further enhanced when a negative electrode in tab is included.
[0021] Here, the "core portion" refers to a region that includes a hollow space located on the winding shaft of the electrode assembly and a part of the stacked structure of the wound negative electrode / separator / positive electrode, and may mean a region within two turns of the positive electrode from one longitudinal end of the positive electrode located at the innermost corner of the electrode assembly.
[0022] Figures 1 to 3 schematically show an electrode assembly according to one embodiment of the present invention.
[0023] Referring to Figures 1 to 3, an electrode assembly according to one embodiment of the present invention may be an electrode assembly in which negative electrodes 100, 100', separation membranes 20, 20', and positive electrodes 300 are laminated and wound together, and in the core portion of the electrode assembly, the negative electrode 100 may include a negative electrode current collector 101 and negative electrode active material layers 102, 103 provided on at least one surface of the negative electrode current collector 101. Specifically, the negative electrode 100 may include a negative electrode active material layer portion 10 including a negative electrode current collector 101 and negative electrode active material layers 102, 103 provided on at least one surface of the negative electrode current collector 101, and a negative electrode plain portion 12 including a negative electrode current collector 101 without the negative electrode active material layer.
[0024] According to one embodiment of the present invention, the positive electrode 300 includes a first surface in the winding axis direction of the electrode assembly and a second surface opposite to the first surface, and the negative electrode 100 in contact with the first surface of the positive electrode may include the negative electrode active material layer 10 and the negative electrode plain portion 12 extending from the longitudinal end 310 of the positive electrode.
[0025] According to one embodiment of the present invention, the negative electrode active material layer 10 may represent an area extending from the longitudinal end 310 of the positive electrode to a point in contact with the plain negative electrode portion extending from the negative electrode active material layer, or it may represent an area having a predetermined longitudinal length L1.
[0026] According to one embodiment of the present invention, the negative electrode blank portion 12 may represent an area extending from the negative electrode active material layer portion 10 and in contact with the longitudinal end of the negative electrode active material layer portion to the longitudinal end of the negative electrode, or it may represent an area having a predetermined longitudinal length L2.
[0027] According to one embodiment of the present invention, the longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode may be 0.5 turns or less from the longitudinal end of the positive electrode. Specifically, the longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode may be 0.45 turns or less, or 0.4 turns or less from the longitudinal end of the positive electrode.
[0028] Here, "Turn" refers to the length required to wind 360° from a reference point of the positive or negative electrode included in the electrode assembly, and the length may be determined by the outer diameter of the winding core C used to wind the electrode assembly, the thickness of the electrode, and the number of turns of the electrode located on the inside. For example, one turn of the negative electrode 100 in contact with the first surface of the positive electrode 300 may refer to the length required to wind the negative electrode 100 360° from the longitudinal end 310 of the positive electrode towards the winding start end of the negative electrode 100.
[0029] According to one embodiment of the present invention, the longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode may be less than 70% of the circumference of the inner circumferential surface of the electrode assembly, based on 100% of the circumference of the inner circumferential surface of the electrode assembly. Specifically, the longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode may be 68% or less, 66% or less, 64% or less, or 62% or less, based on 100% of the circumference of the inner circumferential surface of the electrode assembly.
[0030] Here, "around the inner circumferential surface" refers to the circumference of a virtual circle whose radius is the largest value among the distances from the winding shaft of the electrode assembly to the innermost corner layer that contacts the hollow core H of the electrode assembly, and the length of this circle may be determined according to the outer diameter of the winding core C used to wind the electrode assembly. For example, the circumference of the inner circumferential surface may have a value of approximately 10 mm.
[0031] According to one embodiment of the present invention, in the core portion of the electrode assembly, the negative electrode and the separation membrane may extend longer than the longitudinal end of the positive electrode. Specifically, referring to Figure 3, the negative electrode 100 and the separation membranes 20, 20' may extend longer than the longitudinal end 310 of the positive electrode. In other words, the negative electrode and the separation membrane may be wound together with the positive electrode after the negative electrode and separation membrane have been wound together around the core for 0.5 turns or more. That is, in the core portion of the electrode assembly, the longitudinal ends of the negative electrode and the separation membrane may be located inward from the longitudinal end of the positive electrode.
[0032] According to one embodiment of the present invention, the longitudinal length of the negative electrode extending from the longitudinal end of the positive electrode may be 1.5 turns or more and 2.5 turns or less from the longitudinal end of the positive electrode. Specifically, referring to Figures 1 and 3, the longitudinal length L1+L2 of the negative electrode extending from the longitudinal end 310 of the positive electrode may be 1.6 turns or more or 1.7 turns or more, and 2.4 turns or less or 2.3 turns or less from the longitudinal end 310 of the positive electrode.
[0033] If the longitudinal length of the negative electrode extending from the longitudinal end of the positive electrode satisfies the aforementioned range, the length of the negative electrode plain portion may be suitable for further including a negative electrode tab 50, specifically a negative electrode in tab, which is provided on one surface of the negative electrode current collector described later. For example, if a negative electrode in tab is provided, the length L2 of the negative electrode plain portion may be approximately 19 mm. Furthermore, the relative sliding reduction effect of the positive electrode end due to adjusting the longitudinal length of the negative electrode within the aforementioned range can be better when a negative electrode in tab is included.
[0034] According to one embodiment of the present invention, the longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode may be 35% or less, based on 100% of the longitudinal length of the negative electrode blank portion extending from the end of the negative electrode active material layer. Specifically, referring to Figures 1 and 3, the longitudinal length L1 of the negative electrode active material layer extending from the longitudinal end 310 of the positive electrode may be 10% or more, 11% or more, or 12% or more, and may be 34% or less, 33% or less, or 32% or less, based on 100% of the longitudinal length L2 of the negative electrode blank portion extending from the end of the negative electrode active material layer.
[0035] If the longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode satisfies the aforementioned range, even if a negative electrode in tab is included, the amount of negative electrode material inserted into the core can be adjusted to facilitate the sliding of the negative electrode during charging and discharging of the battery, thereby reducing the relative sliding of the positive electrode end relative to the negative electrode. Specifically, the effect of reducing the relative sliding of the positive electrode end by adjusting the longitudinal length of the negative electrode active material layer within the aforementioned range can be even better when a negative electrode in tab is included.
[0036] According to one embodiment of the present invention, the longitudinal length of the negative electrode extending from the longitudinal end of the positive electrode may be 0.5 turns or more and 1 turn or less from the longitudinal end of the positive electrode. Specifically, referring to Figures 2 and 3, the longitudinal length L1+L2 of the negative electrode extending from the longitudinal end 310 of the positive electrode may be 0.6 turns or more or 0.7 turns or more, and may be 0.9 turns or less or 0.8 turns or less from the longitudinal end 310 of the positive electrode.
[0037] If the longitudinal length of the negative electrode extending from the longitudinal end of the positive electrode satisfies the aforementioned range, it may have a length suitable for the negative electrode plain portion when a negative electrode in tab is not provided. For example, when a negative electrode in tab is not provided, the length L2 of the negative electrode plain portion may be approximately 3 mm. Furthermore, the relative sliding reduction effect of the positive electrode end due to length adjustment of the negative electrode in the longitudinal direction within the aforementioned range can be better when the negative electrode in tab is not included.
[0038] According to one embodiment of the present invention, the longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode may be 150% or more and 230% or less, based on 100% of the longitudinal length of the negative electrode plain portion extending from the end of the negative electrode active material layer. Specifically, referring to Figures 2 and 3, the longitudinal length L1 of the negative electrode active material layer extending from the longitudinal end 310 of the positive electrode may be 155% or more, 160% or more, or 165% or more, and may be 225% or less, 220% or less, or 215% or less, based on 100% of the longitudinal length L2 of the negative electrode plain portion extending from the end of the negative electrode active material layer.
[0039] If the longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode satisfies the aforementioned range, even if the negative electrode in tab is not included, the amount of negative electrode material added to the core can be adjusted to facilitate the sliding of the negative electrode during battery charging and discharging, thereby reducing the relative sliding of the positive electrode end relative to the negative electrode. Specifically, the effect of reducing the relative sliding of the positive electrode end by adjusting the longitudinal length of the negative electrode active material layer within the aforementioned range can be better when the negative electrode in tab is not included.
[0040] According to one embodiment of the present invention, the longitudinal length of the negative electrode may be greater than the longitudinal length of the positive electrode. Furthermore, the longitudinal lengths of the separation membranes located on one and the opposite sides of the negative electrode may be greater than the longitudinal length of the positive electrode.
[0041] When the negative electrode and the separator membrane extend longer than the longitudinal end of the positive electrode, the transfer of lithium ions from the positive electrode to the negative electrode can be made easier in the chemical reaction of the lithium-ion battery. When the length and width of the negative electrode are made wider, the area of the negative electrode that receives lithium ions increases, which can prevent a decrease in charge-discharge efficiency and improve battery stability and lifespan characteristics.
[0042] According to one embodiment of the present invention, the weight of the negative electrode active material layer extending from the longitudinal end of the positive electrode and further wound up may be 70% or more and less than 110% of the weight of the negative electrode plain portion extending from the end of the negative electrode active material layer and further wound up. Specifically, referring to Figures 1 and 3, the weight of the negative electrode active material layer 10 extending from the longitudinal end 310 of the positive electrode may be 70% or more and 100% or 80% or more and 100% or less of the weight of the negative electrode plain portion 12 extending from the end of the negative electrode active material layer.
[0043] When the weight range of the negative electrode active material layer is met as described above, the amount of negative electrode material added to the core can be adjusted to facilitate the sliding of the negative electrode during battery charging and discharging, thereby reducing the relative sliding of the positive electrode end relative to the negative electrode. Specifically, the effect of reducing the relative sliding of the positive electrode end by adjusting the weight of the core negative electrode active material layer within the aforementioned range can be further enhanced when a negative electrode in tab is included.
[0044] According to one embodiment of the present invention, the negative electrode active material layer portion 10 may include an end face surface portion 11 that includes one surface of the negative electrode current collector on which the negative electrode active material layer is provided, and another surface on which the negative electrode current collector is directly exposed and on which the negative electrode active material layer is not provided. Specifically, the end face surface portion 11 may have a negative electrode active material layer provided on one surface facing the winding shaft of the negative electrode current collector, and a negative electrode active material layer not provided on the other surface, on which the negative electrode current collector is directly exposed. When the end face surface portion is included, the amount of negative electrode active material applied to the area not facing the positive electrode can be minimized to ensure economy. Furthermore, when the negative electrode active material layer is provided on one surface of the end face surface portion facing the winding shaft of the negative electrode current collector, the formation of a step due to the thickness of the negative electrode active material can be minimized.
[0045] According to one embodiment of the present invention, the longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode may be 5 mm or more and less than 7 mm. Specifically, referring to Figures 1 and 3, the longitudinal length L1 of the negative electrode active material layer extending from the longitudinal end 310 of the positive electrode may be 5.2 mm or more, 5.4 mm or more, or 5.6 mm or more, and may be 6.8 mm or less, 6.6 mm or less, or 6.4 mm or less.
[0046] When the longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode is within the range described above, the amount of negative electrode core inserted can be adjusted to facilitate the sliding of the negative electrode during charging and discharging of the battery, thereby reducing the relative sliding of the positive electrode end relative to the negative electrode. Specifically, the effect of reducing the relative sliding of the positive electrode end by adjusting the longitudinal length of the negative electrode active material layer within the range described above can be further enhanced when a negative electrode in tab is included.
[0047] According to one embodiment of the present invention, the negative electrode includes a negative electrode active material layer portion on which a negative electrode active material layer is formed on the negative electrode current collector, and a negative electrode blank portion on which the negative electrode active material layer is not formed, and a tab may be included on the negative electrode blank portion. Specifically, referring to Figures 1 and 3, the negative electrode 100 includes a negative electrode blank portion 12 and may include a negative electrode tab 50 provided on the negative electrode blank portion. Thus, the manufactured electrode assembly may include one or more negative electrode tabs. That is, the manufactured electrode assembly may include a negative electrode in-tab, and may further include a protective tape 40 to prevent short circuits due to the thickness of the negative electrode in-tab.
[0048] According to one embodiment of the present invention, the longitudinal length of the negative electrode end surface area may be 0 mm or more and 2 mm or less. Specifically, referring to Figure 3, the longitudinal length L1' of the negative electrode end surface area area may be 0.1 mm or more, 0.3 mm or more, 0.5 mm or more, or 0.7 mm or more, and may be 1.9 mm or less, 1.7 mm or less, 1.5 mm or less, or 1.3 mm or less, for example, 1 mm. When the longitudinal length of the negative electrode end surface area area is within the range described above, the amount of negative electrode inserted into the core can be adjusted to facilitate the sliding of the negative electrode during battery charging and discharging, and the relative sliding of the positive electrode end relative to the negative electrode can be reduced. Specifically, the effect of reducing the relative sliding of the positive electrode end by adjusting the longitudinal length of the negative electrode end surface area area within the range described above can be better when a negative electrode in tab is included.
[0049] According to one embodiment of the present invention, the negative electrode active material layer may include a negative electrode active material comprising one or more selected from the group consisting of silicon-based materials and carbon-based materials. The negative electrode active material layer may further include a negative electrode conductive material and a negative electrode binder, and the negative electrode active material, negative electrode conductive material, and negative electrode binder can be any material used in the industry without limitation.
[0050] According to one embodiment of the present invention, the negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and is conductive. For example, the negative electrode current collector may be made of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treatment of carbon, nickel, titanium, silver, etc. Specifically, transition metals that effectively adsorb carbon, such as copper and nickel, can be used as the negative electrode current collector. The thickness of the negative electrode current collector may be 6 μm or more and 80 μm or less, but the thickness of the negative electrode current collector is not limited thereto.
[0051] According to one embodiment of the present invention, the negative electrode binder may contain at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which the hydrogen atoms of these are substituted with Li, Na, or Ca, and may also contain various copolymers thereof.
[0052] According to one embodiment of the present invention, the negative electrode conductive material is not particularly limited as long as it does not cause a chemical change in the battery and is conductive. For example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives may be used.
[0053] According to one embodiment of the present invention, the electrode assembly may include a plurality of separation membranes. For example, the electrode assembly may have a structure in which separation membrane / negative electrode / separation membrane / positive electrode are stacked in that order. The separation membrane separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. It can be used without particular limitations as long as it is the type of separation membrane that is normally used in secondary batteries, and is particularly preferred if it has low resistance to ion movement of the electrolyte while having excellent electrolyte moisture retention capacity. Specifically, porous polymer films, such as porous polymer films made from polyolefin polymers such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or stacked structures of two or more layers thereof can be used. Alternatively, ordinary porous nonwoven fabrics, such as nonwoven fabrics made of high-melting-point glass fibers or polyethylene terephthalate fibers, may be used. Furthermore, the separation membrane may typically have a thickness of 10 μm to 20 μm. The separation membrane may be made by coating the aforementioned separation membrane material with a slurry containing ceramic components or polymer substances on the substrate layer to ensure heat resistance or mechanical strength. It may also be used selectively in a single-layer or multi-layer structure.
[0054] According to one embodiment of the present invention, the positive electrode may include a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector. Specifically, referring to Figure 3, the positive electrode 300 may include a positive electrode current collector 301 and positive electrode active material layers 302 and 303 formed on one or both sides of the positive electrode current collector 301 and containing positive electrode active material. That is, the positive electrode active material layer is formed on the positive electrode surface portion of the positive electrode current collector, and the surface on which the positive electrode active material layer is not provided can be represented as a positive electrode blank portion.
[0055] According to one embodiment of the present invention, the positive electrode current collector may include a positive electrode surfaced portion on which a positive electrode active material is applied and a positive electrode blank portion on which the positive electrode active material is not applied, and may include a tab on the positive electrode blank portion. Specifically, the positive electrode current collector may include a positive electrode blank portion and may include a positive electrode tab formed on the positive electrode blank portion.
[0056] According to one embodiment of the present invention, in the core portion of the electrode assembly, the positive electrode may include a positive electrode current collector and a positive electrode active material layer provided on at least one surface of the positive electrode current collector and having its longitudinal end at the same position as the positive electrode current collector. Specifically, referring to Figure 3, in the core portion of the electrode assembly, the positive electrode 300, the separation membranes 20, 20' and the negative electrode 100 are laminated and wound together, and the positive electrode 300 may include a positive electrode current collector 301 and positive electrode active material layers 302, 303 provided on at least one surface of the positive electrode current collector 301 and having their longitudinal end 310 at the same position as the positive electrode current collector 301. That is, the longitudinal end 310 of the positive electrode may be in a free-edge form.
[0057] This reduces the area of unnecessary blank portions on the positive electrode current collector, thereby ensuring cost-effectiveness. It also allows the slitting process to be performed after the active material layer is formed on the electrode, and enables the roll-to-roll process, including the slitting and winding processes, to be carried out more efficiently. Here, "same position" means that the longitudinal ends are the same, and may include cases where the ends are formed at substantially the same position due to process errors that may occur in the slitting process or other processes.
[0058] According to one embodiment of the present invention, the positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and is conductive. Specifically, the positive electrode current collector may be stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treatment of carbon, nickel, titanium, silver, etc. In other words, the positive electrode current collector may be provided in the form of surface-treated stainless steel, aluminum foil, etc.
[0059] Furthermore, the positive electrode current collector may typically have a thickness of 3 to 50 μm, and fine irregularities can be formed on the surface of the current collector to enhance the adhesion of the positive electrode active material. For example, it may be used in various forms such as film, sheet, foil, net, porous material, foam, or nonwoven fabric.
[0060] According to one embodiment of the present invention, the positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound with the chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (0 ≤ x ≤ 0.33), LiMnO3, LiMn2O3, LiMnO2; vanadium oxides such as lithium copper oxide (Li2CuO2), LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-y M y Ni-site type lithium nickel oxide represented as O2 (where M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and satisfies 0.01 ≤ y ≤ 0.3); chemical formula LiMn 2-z M z Lithium manganese composite oxides represented as O2 (where M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, satisfying 0.01 ≤ z ≤ 0.1) or Li2Mn3MO8 (where M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); LiMn2O4 in which part of the Li in the chemical formula is substituted with alkaline earth metal ions, etc., are examples but are not limited to these. The positive electrode may be Li-metal.
[0061] According to one embodiment of the present invention, the positive electrode active material layer may further include a positive electrode conductive material and a positive electrode binder. The positive electrode conductive material is used to impart conductivity to the electrode and can be used without particular limitations as long as it does not cause chemical changes and has electronic conductivity in the battery that is constructed. Specifically, the positive electrode conductive material can be graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, or carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, or silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used.
[0062] Furthermore, the positive electrode binder plays a role in improving the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used.
[0063] According to one embodiment of the present invention, the angle between the initial position of the longitudinal end of the negative electrode and the position of the longitudinal end of the negative electrode after 200 or more further charging and discharging cycles at 40°C or higher, with respect to the winding shaft of the electrode assembly, may be 5° or more. Specifically, the angle between the initial position of the longitudinal end of the negative electrode and the position of the longitudinal end of the negative electrode after 200 or more further charging and discharging cycles at 40°C or higher, with respect to the winding shaft of the electrode assembly, may be 5° or more, 10° or more, 15° or more, or 20° or more, and may be 45° or less, 40° or less, 35° or less, 30° or less, or 25° or less, for example, 5° or more and 30° or less. More specifically, the initial position of the longitudinal end of the negative electrode may be measured after activation. Here, "after activation" may mean after a predetermined cycle for the manufacture of the secondary battery and product completion has been carried out. Specifically, the term "after activation" includes the period before the start of active use, which involves multiple cycles for power supply purposes, i.e., the pre-sale and subsequent storage conditions, and may include the state in which self-discharge occurred during storage.
[0064] When the aforementioned angular range is met, the amount of negative electrode inserted into the core can be adjusted to facilitate the sliding of the negative electrode during battery charging and discharging, thereby reducing the relative sliding of the positive electrode end relative to the negative electrode.
[0065] According to one embodiment of the present invention, if charging and discharging are performed 200 or more times at 40°C or higher after activation, the angle between the positive electrode and the negative electrode may be 25° or less. Specifically, the positive electrode includes a first surface in the winding axis direction of the electrode assembly and a second surface opposite to the first surface, and the first extension line drawn by extending a straight line connecting two points on the first surface of the positive electrode where the curvature direction changes within a distance of 5 mm from the longitudinal end of the positive electrode, and the second extension line drawn by extending a straight line connecting two points on the surface of the negative electrode facing the first surface of the positive electrode where the distance from the longitudinal end of the positive electrode is 5 mm, may form an angle of 25° or less. When the above angle range is satisfied, damage to the negative electrode and the separator membrane due to relative sliding of the positive electrode end can be prevented, and internal short circuits between the positive and negative electrodes can be prevented, thereby improving battery stability and life characteristics.
[0066] Figures 7 and 8 show an electrode assembly and a secondary battery containing the same according to one embodiment of the present invention.
[0067] One embodiment of the present invention provides a secondary battery including the electrode assembly and a battery case for housing the electrode assembly. Specifically, referring to Figures 7 and 8, the secondary battery 2 may include the electrode assembly 1 according to the above-described embodiment and the battery case 60 for housing the electrode assembly 1. More specifically, the electrode assembly 1 may or may not include a negative electrode tab 50.
[0068] A secondary battery according to one embodiment of the present invention can prevent damage to the negative electrode and separator membrane due to relative sliding of the positive electrode ends, and can prevent internal short circuits between the positive and negative electrodes, thereby improving battery stability and lifespan characteristics.
[0069] According to one embodiment of the present invention, the battery case may be of a cylindrical type. Specifically, the battery case may be of a cylindrical type, a prismatic type, or a pouch type depending on the application. When the battery case is of a cylindrical type, it is more suitable for accommodating an electrode assembly, and when the battery case is of a cylindrical type, the shape of a secondary battery including the electrode assembly and the battery case for accommodating the electrode assembly may be cylindrical.
[0070] According to one embodiment of the present invention, the inside of the battery case may contain an electrolyte. Specifically, examples of the electrolyte include, but are not limited to, an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, or a molten inorganic electrolyte that can be used in the production of a lithium secondary battery. Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.
[0071] According to one embodiment of the present invention, examples of the non-aqueous organic solvent may include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, and ethyl propionate.
[0072] According to one embodiment of the present invention, the metal salt may be a lithium salt, and the lithium salt is a substance that is easily soluble in the non-aqueous electrolyte. For example, as the anion of the lithium salt, F - , Cl - , I - , NO3 - , N(CN)2- BF4 - ClO4 - PF6 - (CF3)2PF4 - (CF3)3PF3 - (CF3)4PF2 - (CF3)5PF - (CF3)6P - CF3SO3 - CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - CF3CF2(CF3)2CO - (CF3SO2) 2CH - (SF5)3C - (CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - CH3CO2 - SCN - and (CF3CF2SO2)2N - You may use one or more selected from the group consisting of the following:
[0073] According to one embodiment of the present invention, in addition to the electrolyte components, the electrolyte may further contain one or more additives for the purpose of improving battery life characteristics, suppressing battery capacity degradation, and improving battery discharge capacity, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphate triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride.
[0074] The present invention will be described in detail below with reference to examples. However, the examples of the present invention can be modified into various other forms, and the scope of the present invention should not be construed as being limited to the examples described below. The examples herein are provided to give a more complete explanation of the present invention to a person of average skill in the art.
[0075] Examples Example 1 Manufacturing of electrode assemblies An Al foil with a thickness of 15 μm and a width of 63.9 mm was prepared as the positive electrode current collector. A positive electrode active material layer was formed on the positive electrode current collector by coating and drying an NMCA (Ni-Mn-Co-Al) composite with a Ni content of 92% or more as the positive electrode active material and a CNT slurry containing carbon nanotubes as the conductive material, thereby producing a positive electrode with a thickness of 154 μm.
[0076] Next, a Cu foil with a thickness of 8 μm and a width of 65.1 mm was prepared as a negative electrode current collector. A negative electrode active material layer was formed on the negative electrode current collector by coating and drying a negative electrode active material slurry containing 50 parts by weight each of artificial graphite and natural graphite as negative electrode active materials, thereby producing a negative electrode with a thickness of 187 μm.
[0077] On the other hand, two sheet-like polyethylene separation membranes were prepared.
[0078] Subsequently, the negative electrode and positive electrode were sequentially added to manufacture the electrode assembly. In this process, the core portion of the electrode assembly was provided with a negative electrode active material layer portion having a longitudinal length of 6 mm (with a longitudinal length of 1 mm for the surfaced portion of the negative electrode end face) and a negative electrode plain portion having a longitudinal length of 19 mm, and was configured to have the conditions shown in Table 1 and the structure shown in Figure 1.
[0079] Manufacturing of rechargeable batteries After inserting the electrode assembly into a cylindrical battery case, an electrolyte solution was injected, which consisted of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) mixed in a volume ratio (vol%) of 20:5:75 to contain 0.7M of LiPF6. The cylindrical battery case was then sealed with a cap assembly to manufacture a secondary battery.
[0080] Comparative Example 1 and Comparative Example 2 An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that the longitudinal lengths of the negative electrode active material layer and the plain negative electrode, which extend from the longitudinal end of the positive electrode and are further wound up, were adjusted according to the conditions shown in Table 1 below.
[0081] [Table 1]
[0082] Experimental example Experimental Example 1 - Cycle Stability Evaluation The secondary batteries manufactured in Example 1, Comparative Example 1, and Comparative Example 2 were each subjected to 3 cycles of charging at 4.2V-2.5V, 0.2C, and discharging at 0.2C, respectively, to prepare activated secondary batteries with a State of Charge (SOC) of 30%. Subsequently, these activated secondary batteries were subjected to 200 cycles under the conditions of 4.3V-2.85V, 0.5C / 1C, and 55°C to prepare secondary batteries with advanced cycles. The core portions of the activated secondary batteries and the cyclic-advanced secondary batteries were subjected to computed tomography (CT) to check for the presence or absence of core impingement, and the short-term cycle stability was evaluated. The images are shown in Figure 4.
[0083] Experimental Example 2 - Evaluation of Negative Electrode Sliding Computed tomography was performed on the core portion of the secondary batteries manufactured in Example 1, Comparative Example 1, and Comparative Example 2. The angular change between the initial position of the longitudinal end of the negative electrode and the position of the longitudinal end of the negative electrode after a cycle was measured with respect to the winding shaft of the electrode assembly. The angular change was remeasured every 200 cycles, and the results are shown in Figure 6 below.
[0084] Experimental Example 3 - Core Impingement Evaluation Secondary batteries were prepared using the method described below in Example 1, Comparative Example 1, and Comparative Example 2. These batteries were then activated by charging them to 4.2V-2.5V, 0.2C, and discharging them at 0.2C for three cycles until their State of Charge (SOC) reached 30%. The core of the activated secondary batteries was scanned using computed tomography, and the presence or absence of core impingement was evaluated according to the evaluation method described below. The presence or absence of core impingement was re-evaluated every 200 cycles, and the results are shown in Figure 6 below.
[0085] Figure 5 schematically illustrates the method for evaluating whether or not core impingement occurs. Specifically, Figure 5(a) schematically illustrates the method for evaluating whether or not core impingement occurs when deformation occurs in the negative electrode, and Figure 5(b) schematically illustrates the method for evaluating whether or not core impingement occurs when deformation does not occur in the negative electrode.
[0086] 1) On the first surface of the positive electrode 300, extend the straight line connecting the longitudinal end 310 of the positive electrode and a point 5 mm away from the end to draw the first extension line E1.
[0087] 2-1) If deformation occurs in the negative electrode In the core portion of the electrode assembly, on the surface of the negative electrode 100 facing the first surface of the positive electrode, a straight line is drawn by extending a straight line connecting two points where the curvature direction changes within a distance of 5 mm from the longitudinal end 310 of the positive electrode, to draw a second extension line E2.
[0088] 2-2) When no deformation has occurred in the negative electrode In the core portion of the electrode assembly, on the surface of the negative electrode 100 facing the first surface of the positive electrode, a straight line is drawn by extending a line connecting two points that are 5 mm apart from the longitudinal end 310 of the positive electrode, thereby drawing a second extension line E2.
[0089] 3) Core impingement was evaluated as having occurred if the angle from the first extension line E1 to the second extension line E2, counterclockwise from the intersection of the first extension line E1 and the second extension line E2, exceeded 25°.
[0090] On the other hand, the method for evaluating the presence or absence of core impingement can be applied by, when an unknown secondary battery is obtained, evaluating the presence or absence of core impingement at the time of initial acquisition, re-evaluating the presence or absence of core impingement every 200 cycles, and comparing and analyzing it with the core impingement conditions of the secondary battery according to the embodiment of the present invention.
[0091] Referring to Table 1 and Figures 4-6, the secondary battery manufactured in Example 1 was confirmed not to exhibit core impingement in the cycle stability evaluation. However, the secondary batteries manufactured in Comparative Examples 1 and 2 were both confirmed to exhibit core impingement. Specifically, the secondary batteries manufactured in Comparative Examples 1 and 2 did not exhibit core impingement after activation, but core impingement was confirmed to occur after 200 cycles at a high temperature of 55°C.
[0092] Referring to Figure 6, the secondary battery manufactured in Example 1 showed relatively high negative electrode core sliding of 5° or more, even though the angular change between the initial position of the longitudinal end of the negative electrode and the position of the longitudinal end of the negative electrode after 200 cycles gradually decreased with respect to the winding shaft of the electrode assembly. In contrast, the secondary battery manufactured in Comparative Example 2 showed inhibited negative electrode core sliding, exhibiting relatively low negative electrode core sliding of 5° or less even after 400 cycles. Furthermore, the secondary battery manufactured in Comparative Example 2 showed a significant increase in the angle between the positive and negative electrodes after 200 cycles, and after 400 cycles, the angle between the positive and negative electrodes was 25° or more, confirming that core impingement occurred.
[0093] As a result, it was confirmed that the secondary battery according to Example 1, in which the amount of negative electrode material inserted into the core was adjusted to a specific range, showed a significant reduction in the frequency and extent of damage to the negative electrode and separation membrane caused by the longitudinal end of the positive electrode, i.e., core impingement due to shrinkage / expansion of the electrode assembly, compared to the secondary batteries according to Comparative Examples 1 and 2, especially when a negative electrode in tab was included. Specifically, it was confirmed that the secondary batteries according to Comparative Examples 1 and 2 had inferior battery stability and life characteristics compared to the secondary battery according to Example 1, in which the longitudinal length of the negative electrode active material layer exceeded 0.5 turns from the longitudinal end of the positive electrode, i.e., 60% or more relative to 100% of the circumference of the inner surface of the electrode assembly, or the weight of the negative electrode active material layer exceeded 110% relative to 100% of the weight of the plain negative electrode, and the amount of negative electrode material inserted into the core was within a specific range.
[0094] In other words, the electrode assembly according to one embodiment of the present invention can adjust the amount of negative electrode inserted into the core to facilitate the sliding of the negative electrode during battery charging and discharging, and can reduce the relative sliding of the positive electrode end relative to the negative electrode. A secondary battery according to one embodiment of the present invention, including this assembly, can prevent damage to the negative electrode and separator membrane due to relative sliding of the positive electrode end, and can prevent internal short circuits between the positive and negative electrodes, thereby improving battery stability and life characteristics.
[0095] The above detailed description is illustrative of the present invention. Furthermore, the foregoing is merely an illustration of preferred embodiments of the present invention, and as stated above, the present invention can be used in a variety of other combinations, modifications, and environments, and can be changed or modified within the scope of the concepts of the present invention disclosed herein, the scope equivalent to the foregoing disclosures, and / or within the scope of the art or knowledge of the art. Accordingly, the above detailed description of the invention is not intended to limit the present invention by the disclosed embodiments. Furthermore, the appended claims should be construed to include other embodiments as well. [Explanation of symbols]
[0096] C... core H ···Hollow core section 100...Negative electrode 101...Negative electrode current collector 102,103...Negative electrode active material layer 10...Negative electrode active material layer section 11... Negative end surface area 12 ···Negative electrode blank area 20,20'...Separation membrane 300...Positive electrode 301...Positive electrode current collector 302,303...Cathode active material layer 310 ··· Longitudinal end of the positive electrode 40 ··· Protective tape 50 ···Negative electrode tab L1 ···Length in the longitudinal direction of the negative electrode active material layer L1' ···Length of the area with a negative terminal face in the longitudinal direction L2 ···Length of the plain area on the negative terminal E1 ···First extension E2...Second extension 60 ···Battery case 1...electrode assembly 2...Secondary battery
Claims
1. In the core portion of an electrode assembly in which a negative electrode, a separator membrane, and a positive electrode are stacked and wound in order, The negative electrode includes a negative electrode current collector and a negative electrode active material layer portion which includes a negative electrode active material layer provided on at least one surface of the negative electrode current collector; and a negative electrode plain portion which includes a negative electrode current collector on which the negative electrode active material layer is not provided. The longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode is 0.5 turns or less from the longitudinal end of the positive electrode. The weight of the negative electrode active material layer extending from the longitudinal end of the positive electrode is An electrode assembly having a weight of 70% or more and less than 110% of the weight of the plain negative electrode portion extending from the end of the negative electrode active material layer portion, based on 100% of the weight of the plain negative electrode portion.
2. The electrode assembly according to claim 1, wherein the longitudinal length of the negative electrode extending from the longitudinal end of the positive electrode is 1.5 turns or more and 2.5 turns or less from the longitudinal end of the positive electrode.
3. The longitudinal length of the negative electrode active material layer extending from the longitudinal end of the positive electrode is The electrode assembly according to claim 2, wherein the length of the plain negative electrode portion extending from the end of the negative electrode active material layer is 35% or less, based on 100% of the longitudinal length of the plain negative electrode portion.
4. The electrode assembly according to claim 1, wherein the longitudinal length of the negative electrode extending from the longitudinal end of the positive electrode is 0.5 turns or more and 1 turn or less from the longitudinal end of the positive electrode.
5. The negative electrode active material layer portion is The electrode assembly according to claim 1, comprising one surface of the negative electrode current collector on which the negative electrode active material layer is provided, and an end face portion including the other surface on which the negative electrode current collector is directly exposed and on which the negative electrode active material layer is not provided.
6. The electrode assembly according to claim 1, wherein the longitudinal length of the negative electrode active material layer portion extending from the longitudinal end of the positive electrode is 5 mm or more and less than 7 mm.
7. Using the winding shaft of the electrode assembly as a reference, The electrode assembly according to claim 1, wherein the angle between the initial position of the longitudinal end of the negative electrode and the position of the longitudinal end of the negative electrode after being charged and discharged 200 or more times at 40°C or higher is 5° or more.
8. The electrode assembly according to claim 7, wherein the initial position of the longitudinal end of the negative electrode is measured after activation.
9. The positive electrode includes a first surface which is in the winding axis direction of the electrode assembly and a second surface which is the opposite surface of the first surface. On the first surface of the positive electrode, a first extension line drawn by extending a straight line connecting two points within a distance of 5 mm from the longitudinal end of the positive electrode where the curvature direction changes; and The electrode assembly according to claim 1, wherein, on the surface of the negative electrode facing the first surface of the positive electrode, the second extension line drawn by extending a straight line connecting two points separated by a distance of 5 mm from the longitudinal end of the positive electrode forms an angle of 25° or less.
10. In the core portion of the electrode assembly, The electrode assembly according to claim 1, wherein the positive electrode includes a positive electrode current collector; and a positive electrode active material layer provided on at least one surface of the positive electrode current collector and having its longitudinal end at the same position as the positive electrode current collector.
11. In the core portion of the electrode assembly, The electrode assembly according to claim 1, wherein the plain negative electrode portion further includes a negative electrode tab provided on one surface of the negative electrode current collector.
12. An electrode assembly according to any one of claims 1 to 11; and Battery case for housing the electrode assembly Rechargeable batteries, including those mentioned above.
13. The secondary battery according to claim 12, wherein the battery case is cylindrical.
Citation Information
Patent Citations
Battery having spiral electrode body
JP1999111327A
Nonaqueous electrolyte secondary battery
JP2000021452A
Battery having spiral electrode body and its manufacture
JP2000077091A
Wound type battery
JP2001273881A
Wound electrode body and nonaqueous electrolyte secondary battery
JP2003217668A