Jelly roll type electrode assembly, method for manufacturing a jelly roll type electrode assembly, and secondary battery containing the same

The jelly roll type electrode assembly with a heated flexible film supports the core to address core deformation, improving battery safety and lifespan by preventing internal short circuits and membrane damage.

JP7948515B2Active Publication Date: 2026-11-11LG ENERGY SOLUTION LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2025539464
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-08-22
Filing Date
2024-08-22
Publication Date
2026-11-11
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

Cylindrical batteries face issues with core deformation due to electrode contraction and expansion, leading to battery life degradation, separator membrane damage, and internal short circuits, especially with multiple tabs or silicon-based active materials.

Method used

A jelly roll type electrode assembly with a flexible film inserted into the core, heated to a certain tensile strength, supporting the core to maintain its shape and prevent internal short circuits.

Benefits of technology

The flexible film maintains the core's shape, preventing damage to electrodes and separator membranes, enhancing battery safety and lifespan by preventing internal short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948515000002
    Figure 0007948515000002
  • Figure 0007948515000003
    Figure 0007948515000003
  • Figure 0007948515000004
    Figure 0007948515000004
Patent Text Reader

Abstract

The present invention relates to a jelly-roll type electrode assembly, a method for manufacturing the jelly-roll type electrode assembly, and a secondary battery including the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a jelly roll type electrode assembly, a method for manufacturing a jelly roll type electrode assembly, and a secondary battery including the same. More specifically, the present invention relates to a jelly roll type electrode assembly comprising a flexible film heated by a heating means inserted into the hollow core portion of the jelly roll type electrode assembly, a method for manufacturing a jelly roll type electrode assembly, and a cylindrical secondary battery including the same. [Background technology]

[0002] In the case of cylindrical batteries, a long electrode of a predetermined width is wound into a roll to manufacture an electrode assembly in the form of a jelly roll. Cylindrical batteries manufactured by inserting such a jelly roll electrode assembly into a battery case undergo repeated contraction and expansion of the electrodes during charging and discharging. In particular, if a tab is located in the core of the jelly roll electrode assembly, or if a silicon-based active material is added to the negative electrode, increasing the degree of contraction and expansion of the electrode assembly, the pressure acting on the core of the electrode assembly will increase significantly.

[0003] On the other hand, the core of the cylindrical battery is the space where the winding core used for winding the jelly roll type electrode assembly is located, and there is a space used in the assembly process of the cylindrical battery, such as the process of inserting the jelly roll type electrode assembly into the battery case and the welding process, i.e., a hollow space in the core.

[0004] Recently, with the increasing demand for low-resistance / high-capacity designs, jelly roll electrode assemblies are increasingly being constructed with multiple tabs or containing silicon-based active materials. Consequently, the possibility of deformation of the electrode assembly located in the core increases due to the contraction / expansion of the electrode assembly. In particular, core deformation, i.e., the collapse of the hollow core, can lead to a deterioration of battery life. Furthermore, if the separator membrane located between the negative and positive electrodes is damaged, the negative and positive electrodes can come into direct contact, causing internal short circuits, heat generation, and ignition.

[0005] To solve the problems of battery life degradation, separation membrane damage, and internal short circuits caused by deformation of such electrode assemblies, it is necessary to develop a technology that can support the hollow core of the affected region in a way that maintains its original shape and suppresses the occurrence of internal short circuits. [Overview of the project] [Problems that the invention aims to solve]

[0006] The present invention aims to provide a jelly roll type electrode assembly with a modified design, a method for manufacturing a jelly roll type electrode assembly, and a secondary battery containing the same.

[0007] However, the problems that this invention aims to solve are not limited to those mentioned above, and other problems not mentioned will be clearly understandable to those skilled in the art from the following description. [Means for solving the problem]

[0008] One embodiment of the present invention is a jelly roll type electrode assembly in which a first separation membrane, a negative electrode, a second separation membrane, and a positive electrode are sequentially laminated and wound together, wherein the core portion of the jelly roll type electrode assembly includes a flexible film disposed between the first separation membrane and the second separation membrane, the longitudinal length of the flexible film being 100% or more and 150% or less of the circumference of the inner surface of the jelly roll type electrode assembly, the flexible film being heated by a heating means inserted into the hollow of the core portion of the jelly roll type electrode assembly, and the tensile strength of the heated flexible film being 18 kgf / mm² 2 (176.4N / mm 2 ) or more 25kgf / mm 2 (245N / mm 2 The following is provided: a jelly roll type electrode assembly.

[0009] Another embodiment of the present invention is a method for manufacturing a jelly roll type electrode assembly in which a first separation membrane, a negative electrode, a second separation membrane, and a positive electrode are sequentially laminated and wound, comprising: (a) winding the first separation membrane and the second separation membrane; (b) inserting a flexible film between the first separation membrane and the second separation membrane; (c) inserting the negative electrode; (d) inserting the positive electrode; and (e) heating the jelly roll type electrode assembly with a heating means inserted into the hollow core portion, wherein the longitudinal length of the flexible film is 100% or more and 150% or less based on 100% of the circumference of the inner surface of the jelly roll type electrode assembly, and the tensile strength of the heated flexible film is 18 kgf / mm². 2 (176.4N / mm 2 ) or more 25kgf / mm 2 (245N / mm 2 The present invention provides a method for manufacturing a jelly roll type electrode assembly and a jelly roll type electrode assembly manufactured by the said manufacturing method.

[0010] Another embodiment of the present invention provides a secondary battery comprising the jelly roll-type electrode assembly and a battery case for housing the electrode assembly. [Effects of the Invention]

[0011] A jelly roll-type electrode assembly according to one embodiment of the present invention, after being heated by a heating means inserted into the hollow of the core, includes a flexible film having a certain level of rigidity. This supports the hollow of the core so that it maintains its original shape against deformation of the electrode assembly due to contraction / expansion of the electrodes during battery charging and discharging, thereby preventing damage to the positive electrode and separator film, and preventing internal short circuits between the positive and negative electrodes, thus improving the safety and lifespan characteristics of the battery.

[0012] A method for manufacturing a jelly roll type electrode assembly according to one embodiment of the present invention allows for the simpler manufacture of a jelly roll type electrode assembly containing a flexible film having a certain level of rigidity after heating, and the rigidity of the flexible film before heating is suitable for a continuous process using existing roll-to-roll process equipment, thereby ensuring productivity and economic efficiency.

[0013] Furthermore, the secondary battery according to the present invention prevents damage to the positive electrode and separator membrane, and prevents internal short circuits between the positive and negative electrodes, thereby improving the safety and lifespan characteristics of the battery. This is achieved by supporting the core portion's hollow structure so that it maintains its original shape even when the electrode assembly deforms due to the contraction / expansion of the electrodes during charging and discharging.

[0014] The effects of the present invention are not limited to those described above, and effects not mentioned will be clearly understandable to those skilled in the art from this specification and the accompanying drawings. [Brief explanation of the drawing]

[0015] [Figure 1] This figure shows a jelly roll type electrode assembly including a flexible film according to one embodiment of the present invention. [Figure 2] This is a schematic diagram showing a method for manufacturing a jelly roll-type electrode assembly containing a flexible film according to one embodiment of the present invention. [Figure 3] This is a CT image showing the long-term cycle evaluation results of the jelly roll type electrode assemblies according to Example 1 and Example 2. [Figure 4] This is a CT image showing the long-term cycle evaluation results of the jelly roll type electrode assemblies according to Example 1 and Example 2. [Figure 5] This is a CT image showing the long-term cycle evaluation results of the jelly roll type electrode assemblies used in Comparative Examples 1 to 3. [Figure 6] This is a CT image showing the long-term cycle evaluation results of the jelly roll type electrode assemblies used in Comparative Examples 1 to 3. [Figure 7]These are CT images showing the long-term cycle evaluation results of the jelly-roll type electrode assemblies according to Comparative Examples 1 to 3. [Mode for Carrying Out the Invention]

[0016] Throughout this specification, when a part is referred to as "comprising" a constituent element, unless otherwise specified, this does not exclude other constituent elements, and means that the part may further include other constituent elements.

[0017] Throughout this specification, when a member is described as being located "on" another member, this includes not only the case where the member is in contact with the other member, but also the case where still another member exists between the two members.

[0018] Throughout this specification, the term "flexible film" refers to a film having a certain level of rigidity required for easy winding of a jelly-roll type electrode assembly, that is, rigidity equal to or higher than a specific numerical value, and has a tensile strength of 16 kgf / mm 2 (156.8 N / mm 2 ) or less.

[0019] In one embodiment of the present invention, in a jelly-roll type electrode assembly in which a first separator, a negative electrode, a second separator, and a positive electrode are sequentially laminated and wound, the core portion of the jelly-roll type electrode assembly includes a flexible film disposed between the first separator and the second separator, the length of the flexible film in the longitudinal direction is 100% or more and 150% or less based on 100% of the circumferential length of the inner peripheral surface of the jelly-roll type electrode assembly, and the flexible film is heated by a heating unit inserted into the hollow of the core portion of the jelly-roll type electrode assembly, and the tensile strength of the heated flexible film is 18 kgf / mm 2 (176.4 N / mm 2 ) or more and 25 kgf / mm 2 (245 N / mm 2 ) or less.

[0020] A jelly roll type electrode assembly according to one embodiment of the present invention includes a flexible film having a certain level of rigidity in the hollow of the core after being heated by an insertion means. This allows the hollow of the core to maintain its original shape against deformation of the electrode assembly due to contraction / expansion of the electrodes during battery charging and discharging, thereby preventing damage to the positive electrode and separator film, and preventing internal short circuits between the positive and negative electrodes, thus improving the safety and lifespan characteristics of the battery.

[0021] According to one embodiment of the present invention, the core portion of the jelly roll type electrode assembly may include a flexible film disposed between the first separation membrane and the second separation membrane. Here, the "core portion" is a region that includes a hollow located on the winding shaft of the electrode assembly and a part of the laminated structure of the wound electrode assembly, and may mean the region from one longitudinal end of the negative electrode located at the innermost part of the electrode assembly to the ends of the first separation membrane and the second separation membrane. The core portion may also mean a region within three turns from one longitudinal end of the negative electrode.

[0022] According to one embodiment of the present invention, the core portion of the jelly roll type electrode assembly may not include the positive electrode and the negative electrode. In other words, the core portion of the jelly roll type electrode assembly may be a region comprising a first separation membrane, a flexible film, and a second separation membrane.

[0023] According to one embodiment of the present invention, one and the other surfaces of the flexible film may not be in direct contact with the negative electrode or the positive electrode. In other words, one and the other surfaces of the flexible film may be in direct contact with the separation membrane, and the separation membrane may be a first separation membrane and a second separation membrane.

[0024] In this case, even when the flexible film is included in the core of the jelly roll-type electrode assembly, problems such as a decrease in charge / discharge capacity due to a reduction in the area of ​​the negative electrode that receives lithium ions, or inhibition of electrolyte impregnation, can be minimized.

[0025] According to one embodiment of the present invention, the core portion of the jelly roll type electrode assembly includes a flexible film disposed between the first separation membrane and the second separation membrane, and may include a first region having a laminated structure of the first separation membrane and the second separation membrane, and a second region having a laminated structure of the first separation membrane, the flexible film, and the second separation membrane.

[0026] Figure 1 shows a jelly roll type electrode assembly including a flexible film according to one embodiment of the present invention, and Figure 2 is a schematic diagram of a method for manufacturing a jelly roll type electrode assembly including a flexible film according to one embodiment of the present invention.

[0027] Referring to Figures 1 and 2, the core portion of the jelly roll electrode assembly may include a first region having a laminated structure of a first separation membrane and a second separation membrane, and a second region having a laminated structure of a first separation membrane, a flexible film, and a second separation membrane. Specifically, the core portion of the jelly roll electrode assembly may include a flexible film disposed between the first separation membrane and the second separation membrane, thereby including a first region having a laminated structure of a first separation membrane and a second separation membrane, and a second region having a laminated structure of a first separation membrane, a flexible film, and a second separation membrane. More specifically, the longitudinal length of the first region is L1, the longitudinal length of the second region is L2, and the core portion C represents a region having a longitudinal length of the sum of the longitudinal lengths L1 of the first region and L2 of the second region, i.e., L1 + L2, and L3 = 0.

[0028] In this case, one end of the flexible film and the negative electrode in the longitudinal direction are in contact with each other, and as will be described later, the step difference may be minimized by adjusting the thickness range of the flexible film. That is, the formation of a step difference due to the thickness difference between the flexible film and the negative electrode, and the occurrence of local problems such as lithium deposition in the step-forming region can be minimized.

[0029] According to one embodiment of the present invention, the longitudinal length of the first region may be 1 turn or more and 1.7 turns or less. Specifically, the longitudinal length L1 of the first region may be 1.1 turns or more, 1.2 turns or more, or 1.3 turns or more, and may be 1.6 turns or less, 1.5 turns or less, or 1.4 turns or less.

[0030] Here, "Turn" refers to the length required to wind the separation membrane included in the electrode assembly 360° from a reference point, and the length may be determined by the outer diameter of the core used to wind the electrode assembly, the thickness of the first separation membrane, the flexible film, and the second separation membrane, and the number of turns of the first separation membrane, the flexible film, and the second separation membrane located on the inside. For example, "Turn" may refer to the length required to wind the first separation membrane 360° from its longitudinal end in the direction in which the jelly roll type electrode assembly is wound.

[0031] When the longitudinal length range of the first region described above is met, the electrode assembly can be wound more easily by adjusting the separation distance between one longitudinal end of the separation membrane and one longitudinal end of the flexible film. When the longitudinal length of the first region is less than one turn, the tension for continuous winding may not be sufficient when winding using a winding core.

[0032] According to one embodiment of the present invention, the core portion of the jelly roll type electrode assembly may further include a third region having a laminated structure of a first separation membrane and a second separation membrane. Specifically, the core portion of the jelly roll type electrode assembly may include a first region having a laminated structure of a first separation membrane and a second separation membrane, a second region having a laminated structure of a first separation membrane, a flexible film, and a second separation membrane, and a third region having a laminated structure of a first separation membrane and a second separation membrane. More specifically, the longitudinal length of the first region may be L1, the longitudinal length of the second region may be L2, and the longitudinal length of the third region may be L3. The core portion C represents a region having a longitudinal length of the sum of the longitudinal lengths L1 of the first region, L2 of the second region, and L3 of the third region, i.e., L1 + L2 + L3, and L3 may be > 0.

[0033] In this case, the longitudinal ends of the flexible film and the negative electrode do not come into contact with each other, and as will be described later, by adjusting the separation distance between the longitudinal ends of the flexible film and the negative electrode, damage to the separation membrane caused by the ends of the electrode or flexible film can be minimized even when the electrode assembly shrinks or expands.

[0034] According to one embodiment of the present invention, the longitudinal length of the flexible film may be 100% or more and 150% or less, based on 100% of the circumference of the inner surface of the jelly roll type electrode assembly. Specifically, the longitudinal length of the flexible film may be 105% or more, 110% or more, 115% or more, or 120% or more, based on 100% of the circumference of the inner surface of the jelly roll type electrode assembly, and may be 145% or less, 140% or less, 135% or less, or 130% or less.

[0035] Here, the "circumference of the inner surface" refers to a virtual circumference whose radius is the maximum value of the distance from the winding shaft of the electrode assembly to the innermost layer that is in contact with the hollow of the electrode assembly, and its length may be determined by the outer diameter of the winding core used to wind the electrode assembly. For example, the circumference of the inner surface may be approximately 10 mm.

[0036] According to one embodiment of the present invention, the longitudinal length of the flexible film may be between 0.9 turns and 1.4 turns. Specifically, the distance between one end of the flexible film in the longitudinal direction and one end of the negative electrode in the longitudinal direction is between 1 turn and 1.1 turns and may be between 1.3 turns and 1.2 turns. Referring to Figure 2, the longitudinal length of the flexible film may be the same as the longitudinal length L2 of the second region.

[0037] When the longitudinal length of the flexible film meets the aforementioned range, the core support effect by the heated flexible film is superior, minimizing the reduction in battery capacity and energy density and preventing deterioration of electrochemical properties.

[0038] According to one embodiment of the present invention, the separation distance between one end of the flexible film in the longitudinal direction and one end of the negative electrode in the longitudinal direction may be 0.5 turns or less. Specifically, the separation distance between one end of the flexible film in the longitudinal direction and one end of the negative electrode in the longitudinal direction may be 0.4 turns or less or 0.3 turns or less. Referring to Figure 2, the separation distance between one end of the flexible film in the longitudinal direction and one end of the negative electrode in the longitudinal direction may be the same as the longitudinal length L3 of the third region.

[0039] In this case, one end of the flexible film and the negative electrode in the longitudinal direction may be in contact with each other, and by adjusting the thickness of the flexible film and the negative electrode, the step difference caused by the difference in thickness between the electrode and the flexible film can be minimized.

[0040] According to one embodiment of the present invention, the separation distance between one end of the flexible film in the longitudinal direction and one end of the negative electrode in the longitudinal direction may be 0.3 turns or more and 0.7 turns or less. Specifically, the separation distance between one end of the flexible film in the longitudinal direction and one end of the negative electrode in the longitudinal direction may be 0.4 turns or more or 0.5 turns or more, and may be 0.6 turns or less or 0.5 turns or less. Referring to Figure 2, the separation distance between one end of the flexible film in the longitudinal direction and one end of the negative electrode in the longitudinal direction may be the same as the longitudinal length L3 of the third region.

[0041] In this case, one longitudinal end of the flexible film and one longitudinal end of the negative electrode do not need to be in contact with each other, and by adjusting the separation distance between the longitudinal end of the flexible film and the longitudinal end of the negative electrode, damage to the separation membrane by the ends of the electrode or flexible film can be minimized even when the electrode assembly shrinks or expands.

[0042] According to one embodiment of the present invention, the flexible film may further include a fixing member on at least one surface. Specifically, the fixing member is for minimizing the sliding of the flexible film, and can be an adhesive or adhesive tape. When the fixing member is further included, damage to the separation membrane by the electrodes or the edges of the flexible film can be minimized even when the electrode assembly shrinks / expands or the flexible film slides.

[0043] According to one embodiment of the present invention, the flexible film may be heated by a heating means inserted into the hollow of the core portion of the jelly roll-type electrode assembly.

[0044] According to one embodiment of the present invention, the tensile strength of the flexible film before heating is 9 kgf / mm². 2 (88.2 N / mm 2 ) or more 16kgf / mm 2 (156.8 N / mm 2 ) or less. Specifically, the tensile strength of the flexible film before heating is 10 kgf / mm². 2(98N / mm 2 ) or more, 11kgf / mm 2 (107.8 N / mm 2 ) or more or 12 kgf / mm 2 (117.6 N / mm 2 ) may be greater than or equal to 15 kgf / mm² 2 (147N / mm 2 ) or less, 14kgf / mm 2 (137.2 N / mm 2 ) or less or 13 kgf / mm 2 (127.4 N / mm 2 The following are also acceptable:

[0045] According to one embodiment of the present invention, the tensile strength of the flexible film can be increased after heating. Specifically, the tensile strength of the flexible film can be increased by modification of the flexible film after one or both sides are heated, and the rate of increase in tensile strength may vary depending on the degree of heating of the flexible film, i.e., the heating area, heating temperature, and heating time.

[0046] According to one embodiment of the present invention, the tensile strength of the heated flexible film may be 150% or more and 200% or less, based on the tensile strength of 100% before heating. Specifically, the tensile strength of the heated flexible film may be 160% or more, 170% or more, or 180% or more, and may be 190% or less, 180% or less, or 170% or less, based on the tensile strength of 100% before heating.

[0047] According to one embodiment of the present invention, the tensile strength of the heated flexible film is 18 kgf / mm². 2 (176.4N / mm 2 ) or more 25kgf / mm 2 (245N / mm 2 ) or less. Specifically, the tensile strength of the heated flexible film is 19 kgf / mm². 2 (186.2 N / mm 2 ) or more, 20 kgf / mm 2 (196N / mm 2 ) or above or 21 kgf / mm 2(205.8 N / mm 2 ) or more, 24 kgf / mm 2 (235.2 N / mm 2 ) or less, 23kgf / mm 2 (225.4 N / mm 2 ) or less or 22 kgf / mm 2 (215.6 N / mm 2 The following are also acceptable:

[0048] Here, the tensile strength of the flexible film can be measured by preparing a sample of the heated flexible film sample measuring 20 mm × 100 mm and 10 μm in thickness, and measuring it using a Universal Testing Machine (UTM) at room temperature and a speed of 2 cm / min.

[0049] If the rigidity of the flexible film before heating meets the aforementioned range, the rigidity of the jelly roll-type electrode assembly including the flexible film becomes more suitable for the roll-to-roll process, thereby improving the productivity and economic efficiency of the jelly roll-type electrode assembly.

[0050] When the tensile strength of the heated flexible film meets the aforementioned range, the core support effect of the heated flexible film is superior, and productivity and economic efficiency can be ensured by enabling the electrode assembly to be produced in a continuous process using existing roll-to-roll process equipment.

[0051] According to one embodiment of the present invention, the heating means may be a reforming pin. Specifically, referring to Figure 2(c), the heating means may be a reforming pin 200 that pushes a separation membrane (not shown) located in the hollow H of the core of the jelly roll type electrode assembly 100 toward the inner circumferential surface of the core of the jelly roll type electrode assembly 100 to form a cylindrical hollow.

[0052] A pair of winding cores can be used in the winding process of the jelly roll type electrode assembly. After winding the electrode assembly into a jelly roll shape using the winding cores, the electrode assembly is separated from the winding cores. In the hollow core of the jelly roll type electrode assembly, a separation membrane exists that crosses the hollow in a shape corresponding to the distance between the pair of winding cores used for winding. In order to remove the separation membrane that crosses the hollow and restore the central part of the electrode assembly to its original shape, the central part must be tidied up after the winding process of the electrode assembly by a separate reforming process using reforming pins.

[0053] If the heating means is a reform pin, the subsequent process can be facilitated and the productivity of the electrode assembly can be improved by removing the separation film that crosses the hollow of the core of the jelly roll type electrode assembly after winding, and the degree of heating of the flexible film, i.e., the heating area, heating temperature and heating time, can be adjusted to a specific range to ensure that the heated flexible film has a certain level of rigidity.

[0054] According to one embodiment of the present invention, the heating can be performed on one surface of the flexible film. Specifically, the heating can be performed on the entire surface of the flexible film.

[0055] According to one embodiment of the present invention, the heating can be performed at a temperature of 50°C to 80°C for a period of 5 seconds to 15 seconds.

[0056] By adjusting the degree of heating of the flexible film, i.e., the heating area, heating temperature, and heating time, to a specific range, a jelly roll-type electrode assembly containing a flexible film having a certain level of rigidity can be manufactured.

[0057] According to one embodiment of the present invention, the heating can be carried out at a temperature of 55°C or higher, 60°C or higher, or 65°C or higher, and may also be carried out at a temperature of 75°C or lower, 70°C or lower, or 65°C or lower. For example, the heating can be carried out at a temperature of 60°C.

[0058] According to one embodiment of the present invention, the heating can be carried out for a time of 5 seconds or more and 15 seconds or less. Specifically, the heating can be carried out for a time of 6 seconds or more, 7 seconds or more, 8 seconds or more, or 9 seconds or more, and may be carried out for a time of 14 seconds or less, 13 seconds or less, 12 seconds or less, or 11 seconds or less. For example, the heating can be carried out for a time of 10 seconds.

[0059] When the aforementioned heating time and temperature conditions are met, a jelly roll-type electrode assembly containing a flexible film with a certain level of rigidity can be manufactured more easily, and the core support effect by the heated flexible film can be improved.

[0060] On the other hand, if the heating is excessive, shrinkage of the separation membrane may occur, and if the heating is insufficient, the increase in rigidity of the heated flexible film may not be sufficient, resulting in poor support for the core.

[0061] According to one embodiment of the present invention, the core portion of the jelly roll type electrode assembly may have a longitudinal length of 2 turns or more and 3 turns or less. Specifically, the core portion of the jelly roll type electrode assembly may have a longitudinal length of 2.1 turns or more, 2.2 turns or more, 2.3 turns or more, 2.4 turns or more, or 2.5 turns or more, and may have a longitudinal length of 2.9 turns or less, 2.8 turns or less, 2.7 turns or less, 2.6 turns or less, or 2.5 turns or less.

[0062] Referring to Figure 2, the longitudinal length of the core portion may be the same as the sum of the longitudinal length L1 of the first region and the longitudinal length L2 of the second region, or the sum of the longitudinal length L1 of the first region, the longitudinal length L2 of the second region, and the longitudinal length L3 of the third region.

[0063] Here, "Turn" refers to the length required to wind the separation membrane included in the electrode assembly 360° from a reference point, and the length can be determined by the outer diameter of the core used to wind the electrode assembly, the thickness of the first separation membrane, the flexible film, and the second separation membrane, and the number of turns of the first separation membrane, the flexible film, and the second separation membrane located on the inside. For example, "Turn" may refer to the length required to wind the first separation membrane 360° from its longitudinal end in the direction in which the jelly roll type electrode assembly is wound.

[0064] When the longitudinal length of the core portion satisfies the aforementioned range, sufficient space can be secured for the arrangement of the flexible film, and the core portion support effect by the heated flexible film can be further improved.

[0065] According to one embodiment of the present invention, the widthwise length of the flexible film may be 95% or more and 105% or less, based on 100% of the widthwise length of the jelly roll type electrode assembly. Specifically, the widthwise length of the flexible film may be 96% or more, 97% or more, 98% or more, 99% or more, or 100% or more, based on 100% of the widthwise length of the jelly roll type electrode assembly, and may be 104% or less, 103% or less, 102% or less, 101% or less, or 100% or less.

[0066] When the length of the flexible film in the width direction satisfies the range described above, the length of the flexible film can correspond to the length of the jelly roll type electrode assembly in the width direction, which is advantageous for supporting the core portion of the jelly roll type electrode assembly and provides excellent protection against deformation of the core portion.

[0067] If the widthwise length of the flexible film is too small, the effect of preventing deformation of the core may be inferior. On the other hand, if the flexible film is too exposed in the widthwise direction of the jelly roll type electrode assembly, the defect rate may increase during the process of inserting it into the battery case, and local problems such as lithium deposition due to step formation may occur.

[0068] According to one embodiment of the present invention, the flexible film may include at least one selected from polypropylene, polyethylene, polyester, and polyamide. Specifically, the flexible film may include at least one selected from polypropylene (PP), polyethylene (PE), polyethylene terephthalate (PET), and polyamide (PA). For example, the flexible film may include polypropylene (PP).

[0069] When the material of the flexible film is of the type described above, the rigidity of the heated flexible film is sufficient to support the core portion of the jelly roll type electrode assembly, and the rigidity of the flexible film before heating is more suitable for the roll-to-roll process, thereby improving the productivity and economic efficiency of the jelly roll type electrode assembly.

[0070] According to one embodiment of the present invention, the thickness of the flexible film may be 5% or more and 20% or less based on 100% of the thickness of the negative electrode. Specifically, the thickness of the flexible film may be 6% or more, 7% or more, 8% or more, 9% or more, or 10% or more based on 100% of the thickness of the negative electrode, and may be 19% or less, 18% or less, 17% or less, 16% or less, or 15% or less.

[0071] If the thickness of the flexible film meets the aforementioned range, the step difference can be minimized by adjusting the thickness range of the flexible film. In other words, the occurrence of local problems such as step formation due to the thickness difference between the flexible film and the negative electrode, and lithium deposition in the step-forming region can be minimized.

[0072] According to one embodiment of the present invention, the thickness of the flexible film may be 10 μm or more and 50 μm or less. Specifically, the thickness of the flexible film may be 15 μm or more, 20 μm or more, or 25 μm or more, and may be 45 μm or less, 40 μm or less, or 35 μm or less.

[0073] When the thickness of the flexible film meets the aforementioned range, the rigidity of the heated flexible film is sufficient to support the core portion of the jelly roll type electrode assembly, and the rigidity of the flexible film before heating is more suitable for the roll-to-roll process, thereby improving the productivity and economic efficiency of the jelly roll type electrode assembly.

[0074] According to one embodiment of the present invention, the positive electrode includes a positive electrode current collector and a positive electrode active material layer provided on at least one surface of the positive electrode current collector, wherein the positive electrode current collector and the positive electrode active material layer may have longitudinal ends at the same position. In other words, one longitudinal end of the positive electrode may be in the form of a free edge.

[0075] This reduces the area of ​​the blank portion of the positive electrode current collector, thereby ensuring cost-effectiveness. Furthermore, since the slitting process can be performed after forming the active material layer on the electrode, the roll-to-roll process, including the slitting and winding processes, can be carried out more efficiently.

[0076] Here, "same position" means that the ends in the longitudinal direction are identical, and this may include cases where the ends are formed at substantially the same position due to process errors that may occur in processes such as slitting.

[0077] According to one embodiment of the present invention, the positive electrode current collector includes a positive electrode surfaced portion on which a positive electrode active material is applied and a positive electrode blank portion on which the positive electrode active material is not applied, and a tab may be included on the positive electrode blank portion. Specifically, the positive electrode current collector may include a positive electrode blank portion and may include a positive electrode tab formed on the positive electrode blank portion.

[0078] According to one embodiment of the present invention, the positive electrode current collector is not particularly limited as long as it is conductive without causing a chemical change in the battery. Specifically, the positive electrode current collector can be stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treatment of carbon, nickel, titanium, silver, etc. That is, the positive electrode current collector can be provided in the form of surface-treated stainless steel, aluminum foil, etc.

[0079] Furthermore, the positive electrode current collector typically has a thickness of 5 μm to 30 μm, and fine irregularities can be formed on the surface of the current collector to enhance the adhesion of the positive electrode active material. For example, it can be used in a variety of forms such as films, sheets, foils, nets, porous materials, foams, and nonwoven fabrics.

[0080] According to one embodiment of the present invention, the positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound with the chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (0 ≤ x ≤ 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-y M y Ni-site type lithium nickel oxide represented as O2 (where M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, satisfying 0.01 ≤ y ≤ 0.3); chemical formula LiMn 2-z M zLithium manganese composite oxides represented as O2 (where M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, satisfying 0.01 ≤ z ≤ 0.1) or Li2Mn3MO8 (where M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); LiMn2O4 in which part of the Li in the chemical formula is substituted with an alkaline earth metal ion, etc., can be mentioned, but are not limited to these. The positive electrode may also be Li-metal.

[0081] According to one embodiment of the present invention, the positive electrode active material layer may further include a positive electrode conductive material and a positive electrode binder. The positive electrode conductive material is used to impart conductivity to the electrode and can be used in any battery without particular limitation as long as it has electronic conductivity without causing a chemical change. Specifically, the positive electrode conductive material can be graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, Phanese black, lamp black, thermal black, or carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, or silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more can be used.

[0082] Furthermore, the positive electrode binder plays a role in improving the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one or more of these can be used individually or in mixtures of two or more.

[0083] According to one embodiment of the present invention, the negative electrode may include a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector. Specifically, the negative electrode may include a negative electrode current collector and a negative electrode active material layer formed on one or both sides of the negative electrode current collector, and containing negative electrode active material. In other words, the negative electrode active material layer may be formed on the negative electrode surface portion of the negative electrode current collector, and the surface without the negative electrode active material layer may be described as the negative electrode blank portion.

[0084] According to one embodiment of the present invention, the negative electrode current collector includes a negative electrode surface portion on which a negative electrode active material layer is formed, and a negative electrode surface portion on which a negative electrode active material layer is not formed, and a tab may be included on the negative electrode surface portion. Specifically, the negative electrode current collector may include a negative electrode surface portion, and a negative electrode tab may be included on the negative electrode surface portion. Therefore, the manufactured electrode assembly may include one or more negative electrode tabs.

[0085] According to one embodiment of the present invention, the negative electrode active material layer may include a negative electrode active material comprising one or more materials selected from the group consisting of silicon-based materials and carbon-based materials. The negative electrode active material layer may further include a negative electrode conductive material and a negative electrode binder, and the negative electrode active material, negative electrode conductive material, and negative electrode binder may be any material used in the field without limitation.

[0086] According to one embodiment of the present invention, the negative electrode current collector can be any material that is conductive without causing a chemical change in the battery, and is not particularly limited. For example, the negative electrode current collector can be made of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treatment of carbon, nickel, titanium, silver, etc. Specifically, transition metals that readily adsorb carbon, such as copper and nickel, can be used as the negative electrode current collector. The thickness of the negative electrode current collector may be 5 μm or more and 30 μm or less, but the thickness of the negative electrode current collector is not limited thereto.

[0087] According to one embodiment of the present invention, the negative electrode binder may contain at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which the hydrogen atoms of these substances are substituted with Li, Na, or Ca, and may also contain a variety of copolymers thereof.

[0088] According to one embodiment of the present invention, the negative electrode conductive material is not particularly limited as long as it is conductive without causing a chemical change in the battery, and for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Kechen black, channel black, Phanase black, lamp black, and thermal black; conductive fiber such as carbon fiber or metal fiber; conductive tube such as carbon nanotube; metal powder such as fluorocarbon, aluminum, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives can be used.

[0089] According to one embodiment of the present invention, the jelly roll electrode assembly may include a plurality of separation membranes. For example, the jelly roll electrode assembly may have a structure in which separation membranes / negative electrode / separation membrane / positive electrode are stacked in that order. The separation membranes separate the negative electrode and the positive electrode and provide a passage for lithium ions to move. Any separation membrane commonly used in secondary batteries can be used without special limitations, and those with low resistance to electrolyte ion movement while having excellent electrolyte content are particularly preferred. Specifically, porous polymer films, such as ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers, or porous polymer films made from polyolefin polymers or laminated structures of two or more layers thereof can be used. Alternatively, ordinary porous nonwoven fabrics, such as nonwoven fabrics made from high-melting-point glass fibers or polyethylene terephthalate fibers, can also be used. Furthermore, the separation membrane may be made by coating the substrate layer with a slurry containing ceramic components or polymer substances to ensure heat resistance or mechanical strength, using the aforementioned separation membrane material as the substrate layer. It can be selectively used as a single-layer or multi-layer structure. The thickness of the separation membrane may be 10 μm or more and 20 μm or less, but is not limited thereto.

[0090] Another embodiment of the present invention is a method for manufacturing a jelly roll type electrode assembly in which a first separation membrane, a negative electrode, a second separation membrane, and a positive electrode are sequentially laminated and wound, comprising: (a) winding the first separation membrane and the second separation membrane; (b) inserting a flexible film between the first separation membrane and the second separation membrane; (c) inserting the negative electrode; (d) inserting the positive electrode; and (e) heating the jelly roll type electrode assembly with a heating means inserted into the hollow core portion, wherein the longitudinal length of the flexible film is 100% or more and 150% or less based on 100% of the circumference of the inner surface of the jelly roll type electrode assembly, and the tensile strength of the flexible film is 18 kgf / mm². 2 (176.4N / mm 2 ) or more 25kgf / mm 2 (245N / mm 2 The present invention provides a method for manufacturing a jelly roll type electrode assembly and a jelly roll type electrode assembly manufactured by the said manufacturing method.

[0091] A method for manufacturing a jelly roll type electrode assembly according to one embodiment of the present invention allows for the simpler production of a jelly roll type electrode assembly containing a flexible film having a certain level of rigidity after heating, and the rigidity of the flexible film before heating is suitable for a continuous process using existing roll-to-roll process equipment, thereby ensuring productivity and economic efficiency.

[0092] Furthermore, the jelly roll-type electrode assembly manufactured by the above manufacturing method includes a flexible film in the core that has a certain level of rigidity after heating. This allows the hollow core to maintain its original shape against deformation of the electrode assembly due to contraction / expansion of the electrodes during battery charging and discharging, thereby preventing damage to the positive electrode and separator film, and preventing internal short circuits between the positive and negative electrodes. This improves the safety and lifespan characteristics of the battery.

[0093] According to one embodiment of the present invention, the longitudinal length of the flexible film may be 100% or more and 150% or less, based on 100% of the circumference of the inner surface of the jelly roll type electrode assembly. Specifically, the longitudinal length of the flexible film may be 105% or more, 110% or more, 115% or more, or 120% or more, based on 100% of the circumference of the inner surface of the jelly roll type electrode assembly, and may be 145% or less, 140% or less, 135% or less, or 130% or less.

[0094] When the longitudinal length of the flexible film meets the aforementioned range, the core support effect by the heated flexible film is superior, minimizing the reduction in battery capacity and energy density and preventing deterioration of electrochemical properties.

[0095] According to one embodiment of the present invention, the tensile strength of the heated flexible film is 18 kgf / mm². 2 (176.4N / mm 2 ) or more 25kgf / mm 2 (245N / mm 2 ) or less. Specifically, the tensile strength of the flexible film is 19 kgf / mm². 2 (186.2 N / mm 2 ) or more, 20 kgf / mm 2 (196N / mm 2 ) or above or 21 kgf / mm 2 (205.8 N / mm 2 ) or more, 24 kgf / mm 2 (235.2 N / mm 2 ) or less, 23kgf / mm 2 (225.4 N / mm 2 ) or less or 22 kgf / mm 2 (215.6 N / mm 2 The following are also acceptable:

[0096] When the tensile strength of the heated flexible film meets the aforementioned range, the core support effect of the heated flexible film is superior, and productivity and economic efficiency can be ensured by enabling the electrode assembly to be produced in a continuous process using existing roll-to-roll process equipment.

[0097] Here, the meaning of the circumference of the core portion and the inner surface, the physical properties of the flexible film, i.e., the tensile strength of the flexible film before heating, the rate of increase in tensile strength, and the method for measuring the tensile strength of the flexible film may be the same as those described above for the jelly roll type electrode assembly. Furthermore, the meaning of the first to third regions included in the core portion, the length L1 of the first region, the length L2 of the second region, the length L3 of the third region, and the longitudinal length L1+L2+L3 of the core portion may be the same as those described above for the jelly roll type electrode assembly.

[0098] According to one embodiment of the present invention, the method for manufacturing the jelly roll type electrode assembly may be carried out using a roll-to-roll method. Specifically, steps (a) to (d) above can be carried out using a roll-to-roll processing method in which a number of flexible metal foils or the like are moved between rollers during processing.

[0099] Here, the roll-to-roll method may also mean a method in which a roll winding a flexible, thin metal sheet-like electrode current collector is unwound to supply the electrode current collector, an electrode slurry containing electrode active material is applied to at least one surface of the electrode current collector, dried to form an electrode active material layer, and then the processed electrode current collector is rewound and recovered by another roll.

[0100] Furthermore, the term "feedback" may also refer to a series of feeding and winding processes performed during the manufacturing stage of a roll-to-roll electrode assembly, i.e., a part of the winding process. Specifically, it refers to the process of feeding a film or electrode to be further wound between multiple separation films that have been wound onto a core for a portion of their longitudinal length from one end in the longitudinal direction, or onto one surface of multiple separation films that have been partially wound onto a core. It also refers to the process of manufacturing an electrode assembly by continuously winding the film or electrode fed back together with the multiple separation films that have been partially wound, and may include a slitting process to cut off a portion of the longitudinal length as needed.

[0101] A method for manufacturing a jelly roll type electrode assembly according to one embodiment of the present invention allows for the continuous production of a jelly roll type electrode assembly containing the heated flexible film using existing roll-to-roll process equipment. In other words, the method for manufacturing the jelly roll type electrode assembly allows step (b) to be carried out after step (a) and before step (c), so that the entire process can be carried out by a roll-to-roll process used in the field.

[0102] In other words, the method for manufacturing a jelly roll type electrode assembly according to one embodiment of the present invention ensures productivity and economic efficiency by enabling the continuous production of a jelly roll type electrode assembly containing a flexible film having a certain level of rigidity after heating, using existing roll-to-roll process equipment.

[0103] According to one embodiment of the present invention, the method for manufacturing the jelly roll type electrode assembly may include a step of heating the jelly roll type electrode assembly with a heating means inserted into the hollow core portion. Specifically, the heating means may be a reforming pin, and the reforming pin may be the one described above for the jelly roll type electrode assembly.

[0104] According to one embodiment of the present invention, the reform pin may, after being inserted into the hollow of the electrode assembly, repeatedly move forward and backward to push out and remove the separation membrane that crosses the hollow of the core portion to the innermost layer in contact with the hollow of the electrode assembly.

[0105] According to one embodiment of the present invention, the diameter of the reform pin may be 70% or more and 90% or less, based on 100% of the diameter of the hollow core portion. Specifically, the diameter of the reform pin may be 75% or more, 80% or more, or 85% or more, or 85% or less, 80% or less, or 75% or less, based on 100% of the diameter of the hollow core portion.

[0106] If the diameter of the reform pins is within the range described above, the degree of heating of the flexible film, i.e., the heating area, heating temperature, and heating time, can be adjusted to a specific range to ensure a certain level of rigidity of the heated flexible film, and the protrusion of the separation membrane can be prevented when the reform pins are removed.

[0107] According to one embodiment of the present invention, the length of the reform pin may be 100% or more of the widthwise length of the jelly roll-type electrode assembly.

[0108] When the length of the reform pins satisfies the range described above, the length of the reform pins can correspond to the widthwise length of the jelly roll-type electrode assembly, and the process of removing the separation membrane that crosses the hollow core of the electrode assembly and heating can be carried out more uniformly over the entire widthwise length of the electrode assembly.

[0109] According to one embodiment of the present invention, the heating can be performed at a temperature of 50°C to 80°C for a period of 5 seconds to 15 seconds.

[0110] According to one embodiment of the present invention, the heating can be carried out at a temperature of 55°C or higher, 60°C or higher, or 65°C or higher, and may also be carried out at a temperature of 75°C or lower, 70°C or lower, or 65°C or lower. For example, the heating can be carried out at a temperature of 60°C.

[0111] According to one embodiment of the present invention, the heating can be carried out for a time of 5 seconds or more and 15 seconds or less. Specifically, the heating can be carried out for a time of 6 seconds or more, 7 seconds or more, 8 seconds or more, or 9 seconds or more, and can be carried out for a time of 14 seconds or less, 13 seconds or less, 12 seconds or less, or 11 seconds or less. For example, the heating can be carried out for a time of 10 seconds.

[0112] When the aforementioned heating time and temperature conditions are met, a jelly roll-type electrode assembly containing a flexible film with a certain level of rigidity can be manufactured more easily, and the support effect of the heated flexible film on the core can be improved.

[0113] On the other hand, if the heating is excessive, shrinkage of the separation membrane may occur, and if the heating is insufficient, the increase in rigidity of the heated flexible film may not be sufficient, resulting in poor support for the core.

[0114] Figure 2 is a schematic diagram of a method for manufacturing a jelly roll type electrode assembly including a flexible film according to one embodiment of the present invention.

[0115] Referring to Figure 2, step (a) may involve winding the first and second separation membranes. After winding the first and second separation membranes to a predetermined length using a winding core, step (b) can be carried out.

[0116] In other words, a flexible film can be inserted between the first and second separation membranes, which have been wound to a predetermined length. Therefore, the core portion of the jelly roll type electrode assembly does not include the positive electrode and the negative electrode, and one side and the other side of the flexible film may not be in direct contact with the negative electrode or the positive electrode. Here, the widthwise length, material, and thickness of the flexible film to be inserted may be the same as those described above for the jelly roll type electrode assembly.

[0117] In step (b) above, the flexible film may have a predetermined length, and the core portion of the jelly roll-type electrode assembly including the flexible film may also have a predetermined length.

[0118] Next, steps (c) and (d) can be carried out in order.

[0119] According to one embodiment of the present invention, step (c) involves introducing the negative electrode, and more specifically, the negative electrode may be introduced between the first separation membrane and the second separation membrane.

[0120] The longitudinal ends of the flexible film and the negative electrode do not come into contact with each other, and by adjusting the separation distance between the longitudinal end of the flexible film and the longitudinal end of the negative electrode, damage to the separation membrane by the ends of the electrode or flexible film can be minimized even when the electrode assembly shrinks or expands.

[0121] On the other hand, when one end of the flexible film and the negative electrode in the longitudinal direction are in contact with each other, the thickness range of the flexible film can be adjusted to minimize the step difference, thereby minimizing the occurrence of local problems such as lithium deposition in the step-forming region.

[0122] Next, step (e) can be carried out after steps (a) to (d). Specifically, after the jelly roll-type electrode assembly is wound up, it can be heated by a heating means inserted into the hollow of the core. More specifically, if the heating means is a reforming pin, the step of removing the separation membrane that crosses the hollow of the core of the electrode assembly and the heating can be carried out simultaneously.

[0123] A method for manufacturing a jelly roll type electrode assembly according to one embodiment of the present invention allows for the simpler manufacture of a jelly roll type electrode assembly containing a flexible film having a certain level of rigidity after heating, and the rigidity of the flexible film before heating is suitable for a continuous process using existing roll-to-roll process equipment, thereby ensuring productivity and economic efficiency.

[0124] One embodiment of the present invention provides a jelly roll type electrode assembly manufactured by the method for manufacturing a jelly roll type electrode assembly described above.

[0125] A jelly roll-type electrode assembly according to one embodiment of the present invention includes a flexible film in the core portion that has a certain level of rigidity after heating. This allows the hollow core portion to maintain its original shape against deformation of the electrode assembly due to contraction / expansion of the electrodes during battery charging and discharging, thereby preventing damage to the positive electrode and separator film, and preventing internal short circuits between the positive and negative electrodes. This improves the safety and lifespan characteristics of the battery.

[0126] One embodiment of the present invention provides a secondary battery including the jelly roll-type electrode assembly and a battery case for housing the electrode assembly. Specifically, the secondary battery may include the electrode assembly according to the above-described embodiment and the battery case for housing the electrode assembly.

[0127] The secondary battery according to the present invention prevents damage to the positive electrode and separator membrane, and prevents internal short circuits between the positive and negative electrodes, thereby improving the safety and lifespan characteristics of the battery, by supporting the hollow core portion to maintain its original shape despite deformation of the electrode assembly due to the contraction / expansion of the electrodes during charging and discharging of the battery.

[0128] According to one embodiment of the present invention, the battery case may be cylindrical. Specifically, the battery case may be cylindrical, rectangular, or pouch-shaped, depending on the application, but is not limited thereto.

[0129] According to one embodiment of the present invention, the inside of the battery case may contain an electrolyte. Specifically, the electrolyte may include, but is not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, or molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries. Specifically, the electrolyte may contain a non-aqueous organic solvent and a metal salt.

[0130] According to one embodiment of the present invention, as the non-aqueous organic solvent, for example, aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethyl carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, ethyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, and ethyl propionate can be used.

[0131] According to one embodiment of the present invention, the metal salt may be a lithium salt. The lithium salt is a substance that is easily soluble in the non-aqueous electrolyte, and for example, as the anion of the lithium salt, F - , Cl - , I - , NO3 - , N(CN) 2- , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - one or more selected from the group consisting of can be used.

[0132] According to one embodiment of the present invention, the electrolyte may further contain, in addition to the electrolyte components, one or more additives for the purpose of improving the battery life characteristics, suppressing the decrease in battery capacity, and improving the battery discharge capacity, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphate triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride.

[0133] One embodiment of the present invention provides a battery module and a battery pack including the secondary battery as a unit cell. Since the battery module and battery pack include the secondary battery which has improved high capacity, high battery safety, and life characteristics, they can be used as a power source for medium to large devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.

[0134] Modes for carrying out the invention

[0135] The present invention will be described in detail below based on examples. However, the examples of the present invention can be modified into various other forms, and the scope of the present invention should not be construed as being limited to the examples described below. The examples herein are provided to give a more complete explanation of the present invention to a person of average skill in the art.

[0136] Examples

[0137] Example 1

[0138] Manufacturing of electrode assemblies

[0139] Li(Ni) is used as the positive electrode material. 0.93 Co 0.01 Mn 0.03 Al0.03 A cathode active material slurry was prepared by adding O2, CNTs as the cathode conductive material, and polyvinylidene fluoride (PVdF) as the binder to N-methyl-2-pyrrolidone (NMP) in a weight ratio of 98.2:0.8:1.0. The cathode active material slurry was coated onto an aluminum current collector with a thickness of 15 μm and a width of 64 mm, and then dried and rolled to form a cathode active material layer, thereby preparing a cathode with a thickness of 175 μm.

[0140] Next, as the negative electrode active material, natural graphite (C, average particle size 10 μm, manufactured by POSCO Chemical Co., Ltd.) and SiO (average particle size (D) 50 A negative electrode active material composition was prepared by mixing carbon black (5 μm):5 μm each in a weight ratio of 95:5 (SiO5 wt%) with a mixture of styrene-butadiene rubber (SBR) and carboxymethylcellulose (CMC) in a weight ratio of 98:1:1 as the conductive material for the negative electrode active material, and as the first binder. Then, 7.8 g of distilled water was added to 5 g of the negative electrode active material composition and stirred to produce a negative electrode active material slurry. The negative electrode active material slurry was applied to a copper (Cu) metal thin film, which was a negative electrode current collector with a thickness of 10 μm and a width of 65 mm, and dried (drying temperature 120°C, 1 minute) to form a negative electrode with an average thickness of 185 μm. Here, the temperature of the circulating air was 60°C.

[0141] Subsequently, a flexible film made of polypropylene (PP) material with a width of 65 mm, a length of 15 mm, and a thickness of 50 μm was prepared, along with two separation membranes made of polyethylene (PE) material with a thickness of 13 μm, which served as the first and second separation membranes. A sample measuring 20 mm × 100 mm and 10 μm thick was then prepared from the flexible film. The tensile strength measured using a Universal Testing Machine (UTM) at room temperature and a speed of 2 cm / min was 11 kgf / mm². 2 (107.8 N / mm 2 ) was.

[0142] Subsequently, the first and second separation membranes were arranged in order and wound up using a 3.4 mm diameter core. Then, the flexible film was placed between the first and second separation membranes and wound up further. After the entire flexible film had been wound up, the negative electrode and positive electrode were placed in order at a distance of 6 mm from the flexible film and wound up. At the end where winding was complete, a PET sealing tape was attached and finished to wrap around the outer circumferential surfaces of the upper and lower ends of the jelly roll to produce a jelly roll type electrode assembly. Here, the circumference of the inner surface of the jelly roll type electrode assembly was approximately 12 mm, and the length from the longitudinal end of the negative electrode to the longitudinal end of the first separation membrane was approximately 15 mm.

[0143] Subsequently, a 2.5 mm diameter reforming pin equipped with a heater was inserted into the hollow of the electrode assembly. The separation film crossing the hollow of the core was then pushed out and removed to the innermost layer in contact with the hollow of the electrode assembly by repeatedly moving it forward and backward. The heater on the reforming pin was adjusted to 60°C, and the reforming was performed for 10 seconds. After preparing a sample of the heated flexible film measuring 20 mm × 100 mm and 10 μm thick, the tensile strength measured on a Universal Testing Machine (UTM) at room temperature and a speed of 2 cm / min was 18 kgf / mm². 2 (176.4N / mm 2 ) was.

[0144] Manufacturing of rechargeable batteries

[0145] After inserting the aforementioned jelly roll electrode assembly into a cylindrical battery case, ethylene carbonate (EC):ethyl methyl carbonate (EMC):dimethyl carbonate (DMC) are mixed in a volume ratio of 20:50:30 to obtain a LiPF6 solution of 1.3 M (mol / dm³). 3 A rechargeable battery was manufactured by pouring an electrolyte solution dissolved to the desired state (as shown in the diagram) into the cylindrical battery case, and then sealing it with a cap assembly.

[0146] Example 2

[0147] A jelly roll-type electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that a polyethylene (PE) film was used as the flexible film.

[0148] Here, after preparing a sample of polyethylene (PE) film with dimensions of 20 mm x 100 mm and a thickness of 10 μm, the tensile strength measured using a Universal Testing Machine (UTM) at room temperature and a speed of 2 cm / min was 15 kgf / mm². 2 (147N / mm 2 The tensile strength of the heated flexible film is 25 kgf / mm². 2 (245N / mm 2 ) was.

[0149] Comparative Example 1

[0150] A jelly roll-type electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that a flexible film was not included.

[0151] Comparative Example 2

[0152] A jelly roll-type electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that a PI (polyimide) film was used as the flexible film. Here, after preparing a sample of the PI film measuring 20 mm × 100 mm and 10 μm in thickness, the tensile strength measured on a Universal Testing Machine (UTM) at room temperature and a speed of 2 cm / min was 5 kgf / mm². 2 (49N / mm 2 The tensile strength of the heated flexible film is 10 kgf / mm². 2 (98N / mm 2 ) was.

[0153] Comparative Example 3

[0154] A jelly roll-type electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that a film with a longitudinal length of 30 mm was used as the flexible film.

[0155] Experimental example

[0156] Experimental Example 1: Evaluation of Cycle Safety

[0157] The secondary batteries manufactured in the above examples and comparative examples were subjected to a cycle test using an electrochemical charger and discharger at 25°C under conditions of 4.2–2.85 V 0.5 C / 0.5 C. After 50 cycles, the core portion was examined by computed tomography (CT) to check for core deformation, thereby evaluating cycle safety. The resulting images are shown in Figures 3 to 7, respectively.

[0158] Experimental Example 2: Lifespan Evaluation

[0159] In the above examples and comparative examples, the lifespan of secondary batteries was evaluated using an electrochemical charger / discharger, and the capacity retention rate was assessed. The secondary batteries underwent cycle testing at 4.2–2.85 V 1 C / 1 C, and during the test, the capacity retention rate was measured by charging / discharging at 0.2 C / 0.2 C (4.2–2.85 V) every 100 cycles. The results are shown in Table 1.

[0160] Life retention rate (%) = {(Discharge capacity in the Nth cycle) / (Discharge capacity in the first cycle)} × 100 Experimental Example 3: Measurement and Evaluation of Resistance Increase Rate

[0161] In Experimental Example 2, during the test, the capacity retention rate was measured by charging / discharging at 0.2 C / 0.2 C (4.2-2.85 V) every 100 cycles. Then, the resistance was measured by discharging with a 0.5 C pulse using SOC50, and the resistance increase rate was compared and analyzed. The results are shown in Table 1 below.

[0162] [Table 1]

[0163] Referring to Table 1 and Figures 3 to 7, it was confirmed that the secondary battery according to one embodiment of the present invention includes a flexible film in the core, and that the core deformation is improved by increasing the rigidity of the flexible film through heating using reform pins after the assembly of the jelly roll type electrode assembly. Furthermore, it was confirmed that the secondary batteries according to Examples 1 and 2 can achieve the design capacity and improve lifespan and resistance characteristics. On the other hand, as in Comparative Examples 1 to 3, the flexible film is not included, or the tensile strength remains at 18 kgf / mm² even after heating. 2 (176.4N / mm 2 )We confirmed that when using a film with low rigidity, core deformation occurs, increasing the internal resistance of the battery and degrading its lifespan characteristics. We also confirmed that if the longitudinal length of the flexible film increases excessively, the longitudinal length of the electrodes decreases, reducing both the design capacity and the actual discharge capacity.

[0164] Therefore, a jelly roll type electrode assembly and a secondary battery containing the same, according to one embodiment of the present invention, are heated by a heating means inserted into the hollow of the core portion and then include a flexible film having a certain level of rigidity. This allows the hollow of the core portion to maintain its original shape against deformation of the electrode assembly due to contraction / expansion of the electrodes during charging and discharging of the battery, thereby preventing damage to the positive electrode and the separator film, and preventing internal short circuits between the positive and negative electrodes. Thus, the safety and lifespan characteristics of the battery can be improved.

[0165] The above detailed description is illustrative of the present invention. Furthermore, the foregoing merely illustrates preferred embodiments of the present invention, and as stated above, the present invention can be used in a variety of other combinations, modifications, and environments, and can be modified or altered within the scope of the concept of the invention disclosed herein, within the scope equivalent to the foregoing disclosure, and / or within the scope of the art or knowledge. Therefore, the above detailed description of the invention is not intended to limit the present invention to the disclosed embodiments. Furthermore, the appended claims should be interpreted as including other embodiments as well. [Industrial applicability]

[0166] A jelly roll-type electrode assembly and a secondary battery containing the same, according to one embodiment of the present invention, are heated by a heating means inserted into the hollow of the core portion and then include a flexible film having a certain level of rigidity. This allows the hollow of the core portion to maintain its original shape against deformation of the electrode assembly due to contraction / expansion of the electrodes during charging and discharging of the battery, thereby preventing damage to the positive electrode and the separator film, and preventing internal short circuits between the positive and negative electrodes. Thus, the safety and lifespan characteristics of the battery can be improved. [Explanation of symbols]

[0167] 10 First separation membrane 20 negative electrode 30 Second separation membrane 40 positive electrode 50 Flexible film 100 Jelly Roll Type Electrode Assembly 200 Remodeling Pins L1 is the longitudinal length of the first region. L2 is the longitudinal length of the second region. L3 is the longitudinal length of the third region. C Core H Core section is hollow

Claims

1. A jelly roll type electrode assembly in which a first separation membrane, a negative electrode, a second separation membrane, and a positive electrode are sequentially stacked and wound together, The core portion of the jelly roll-type electrode assembly includes a flexible film disposed between the first separation membrane and the second separation membrane. The longitudinal length of the flexible film is 100% or more and 150% or less, based on 100% of the circumference of the inner surface of the jelly roll-type electrode assembly. The flexible film is heated, The tensile strength of the heated flexible film is 18 kgf / mm². 2 (176.4N / mm 2 ) or more 25kgf / mm 2 (245 N / mm 2 The following is a jelly roll-type electrode assembly.

2. The jelly roll type electrode assembly according to claim 1, wherein the core portion of the jelly roll type electrode assembly has a longitudinal length of 2 turns or more and 3 turns or less.

3. The jelly roll type electrode assembly according to claim 1, wherein the core portion of the jelly roll type electrode assembly does not include the positive electrode and the negative electrode.

4. The jelly roll type electrode assembly according to claim 1, wherein one side and the other side of the flexible film are not in direct contact with the negative electrode or the positive electrode.

5. The jelly roll type electrode assembly according to claim 1, wherein the length of the flexible film in the width direction is 95% or more and 105% or less, based on 100% of the length of the jelly roll type electrode assembly in the width direction.

6. The jelly roll type electrode assembly according to claim 1, wherein the thickness of the flexible film is 5% or more and 20% or less based on 100% of the thickness of the negative electrode.

7. The jelly roll type electrode assembly according to claim 1, wherein the thickness of the flexible film is 10 μm or more and 50 μm or less.

8. The positive electrode includes a positive electrode current collector and a positive electrode active material layer provided on at least one surface of the positive electrode current collector. The jelly roll type electrode assembly according to claim 1, wherein the positive electrode current collector and the positive electrode active material layer have longitudinal ends at the same position.

9. A method for manufacturing a jelly roll type electrode assembly in which a first separation membrane, a negative electrode, a second separation membrane, and a positive electrode are sequentially stacked and wound together, (a) The step of winding up the first separation membrane and the second separation membrane, (b) The step of inserting a flexible film between the first separation membrane and the second separation membrane, (c) The step of introducing the negative electrode, (d) The step of bringing the positive electrode into place, (e) Heating by a heating means inserted into the hollow core of the jelly roll-type electrode assembly, Includes, The longitudinal length of the flexible film is 100% or more and 150% or less, based on 100% of the circumference of the inner surface of the jelly roll-type electrode assembly. The tensile strength of the heated flexible film is 18 kgf / mm². 2 (176.4N / mm 2 ) or more 25kgf / mm 2 (245 N / mm 2 The method for manufacturing a jelly roll-type electrode assembly is as follows:

10. The method for manufacturing a jelly roll type electrode assembly according to claim 9, wherein the heating means is a reform pin.

11. The method for manufacturing a jelly roll type electrode assembly according to claim 10, wherein the diameter of the reform pin is 70% or more and 90% or less, based on 100% of the diameter of the hollow part of the core.

12. The method for manufacturing a jelly roll type electrode assembly according to claim 9, wherein the heating is carried out at a temperature of 50°C or higher and 80°C or lower for a period of 5 seconds or higher and 15 seconds or lower.

13. A jelly roll type electrode assembly according to any one of claims 1 to 8, A secondary battery comprising a battery case for housing the aforementioned jelly roll-type electrode assembly.

14. The secondary battery according to claim 13, wherein the battery case is cylindrical.

Citation Information

Patent Citations

  • Nonaqueous secondary battery

    JP2005174793A

  • Method for manufacturing battery with wound electrode body

    JP2010055753A

  • battery

    JP2012009249A

  • Cylindrical rechargeable battery

    JP2014507762A

  • Electrode assembly and secondary battery therewith the electrode assembly and battery pack therewith the secondary battery

    KR1020200070895A