Piezoelectric laminate, method for manufacturing a piezoelectric laminate, and piezoelectric element

A two-step deposition process for KNN films addresses the challenge of low film stress and high (001) orientation, resulting in a KNN film with spontaneous polarization, enhancing the performance and reliability of piezoelectric elements for sensor applications.

JP7948880B2Active Publication Date: 2026-11-11SUMITOMO CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023052799
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2026-11-11
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Existing KNN films used in piezoelectric materials face challenges in achieving low film stress, high (001) orientation, and spontaneous polarization simultaneously, leading to structural deformation and reduced manufacturing yield in piezoelectric elements.

Method used

A two-step deposition process is employed, where a first KNN layer is formed at a temperature to achieve low film stress and high (001) orientation, followed by a second layer to induce spontaneous polarization, resulting in a KNN film with film stress of 150 MPa or less and relative permittivity of 490 or less.

Benefits of technology

The resulting KNN film achieves low film stress, high (001) orientation, and spontaneous polarization, enabling reliable piezoelectric elements with improved sensitivity and structural integrity, suitable for sensor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948880000005
    Figure 0007948880000005
  • Figure 0007948880000006
    Figure 0007948880000006
  • Figure 0007948880000007
    Figure 0007948880000007
Patent Text Reader

Abstract

To provide a piezoelectric laminate that includes a piezoelectric film that is a spontaneous polarization film, has a relative dielectric constant of 490 or less, and a film stress of 150 MPa or less, and contains potassium, sodium, niobium, and oxygen.SOLUTION: A piezoelectric laminate includes a substrate, a lower electrode film deposited on the substrate, and a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen deposited on the lower electrode film, and in a hysteresis curve showing a correlation between an amount of polarization and an applied electric field obtained by applying an electric field under specified conditions to the piezoelectric film, a median value of a coercive electric field between a coercive electric field EC+ on a positive electric field side and a coercive electric field EC- on a negative electric field side is a positive value, a relative dielectric constant of the piezoelectric film is 490 or less, and a film stress of the piezoelectric film is 150 MPa or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to a piezoelectric laminate, a method for manufacturing a piezoelectric laminate, and a piezoelectric element. [Background technology]

[0002] Piezoelectric materials are widely used in functional electronic components such as sensors and actuators. One of the materials used for piezoelectric materials is a KNN-based ferroelectric containing potassium, sodium, niobium, and oxygen, and laminates having a piezoelectric film (KNN film) fabricated using such piezoelectric materials have been proposed. For example, Patent Document 1 describes a KNN film, which is a spontaneously polarized film that can obtain sufficient piezoelectric displacement without polarization treatment, that is, in a hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field to a KNN film under predetermined conditions, the coercive electric field E on the positive electric field side C + and the negative field side's coercive field E C - A KNN film is disclosed in which the median coercive field between the film and the object is 10.8 kV / cm or higher. Furthermore, Patent Document 1 discloses that the relative permittivity of a KNN film can be reduced by inducing spontaneous polarization in the KNN film.

[0003] Furthermore, piezoelectric films are required to have low film stress (internal stress). For example, Patent Document 2 discloses a technique to reduce the film stress of the KNN film to 1.6 GPa or less by making the lower electrode film that serves as the base for the KNN film out of platinum (Pt) and by controlling the particle size of the crystal grains constituting the lower electrode film to be uniform, thereby reducing the surface irregularities of the lower electrode film and easing the stress at the interface with the KNN film. Patent Document 2 also discloses a technique to control (reduce) the film stress of the KNN film to 1.6 GPa or less by performing heat treatment after the KNN film is fabricated. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 2014-207429 [Patent Document 2] Japanese Patent Publication No. 2011-029591 [Overview of the project] [Problems that the invention aims to solve]

[0005] The KNN film obtained using the technology described in Patent Document 1 is a spontaneously polarized film that can obtain sufficient piezoelectric displacement without polarization treatment, and although it is a film with a low relative permittivity, it has high film stress. On the other hand, the KNN film obtained using the technology described in Patent Document 2 is a film with low film stress, but it is not a spontaneously polarized film.

[0006] The object of this disclosure is to provide a piezoelectric laminate having a piezoelectric film containing potassium, sodium, niobium, and oxygen, which is a spontaneously polarizing film, has a relative permittivity of 490 or less, and a film stress of 150 MPa or less. [Means for solving the problem]

[0007] According to one aspect of this disclosure, circuit board and A lower electrode film formed on the substrate, The lower electrode film comprises a piezoelectric film formed on the lower electrode film, composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field, obtained by applying an electric field to the piezoelectric film under predetermined conditions, the coercive electric field E on the positive electric field side C + and the negative field side's coercive field E C - The median value of the coercive field between is a positive value. The dielectric constant of the piezoelectric film is 490 or less. A piezoelectric laminate and a piezoelectric element are provided, wherein the film stress of the piezoelectric film is 150 MPa or less.

[0008] According to other aspects of this disclosure, A process of forming a lower electrode film on a substrate, The process includes a step of forming a piezoelectric film on the lower electrode film, which is composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen. A method for manufacturing a piezoelectric laminate is provided, in which, in the step of forming the piezoelectric film, first a first piezoelectric film, which is a part of the piezoelectric film, is formed at a first temperature in which the (001) orientation ratio becomes 95% or more and the film stress becomes 100 MPa or less, and then a second piezoelectric film, which is the other part of the piezoelectric film, is formed on the first piezoelectric film at a second temperature in which the second piezoelectric film becomes a spontaneously polarized film. [Effects of the Invention]

[0009] According to this disclosure, a piezoelectric laminate can be provided having a piezoelectric film containing potassium, sodium, niobium, and oxygen, which is a spontaneously polarizing film, has a relative permittivity of 490 or less, and a film stress of 150 MPa or less. [Brief explanation of the drawing]

[0010] [Figure 1] This figure shows an example of a cross-sectional structure of a piezoelectric laminate according to one aspect of the present disclosure. [Figure 2] This figure shows an example of the structure of a simple piezoelectric element according to one aspect of the present disclosure. [Figure 3] This figure shows an example of a schematic configuration of a piezoelectric element according to one aspect of the present disclosure. [Figure 4] This figure shows an example of a schematic configuration of a piezoelectric device module according to one aspect of the present disclosure. [Figure 5] This is the polarization-field hysteresis curve (PE hysteresis curve) for Sample 3. [Figure 6] This is the PE hysteresis curve for sample 9. [Figure 7] (a) is a diagram showing an example of a schematic configuration of a simple unimorph cantilever fabricated using each sample, and (b) is a diagram illustrating a method for measuring piezoelectric displacement. [Figure 8] (a) to (e) are graphs showing the evaluation results regarding the necessity of polarization treatment using a simple piezoelectric element fabricated from Sample 3. [Figure 9] (a) to (e) are graphs showing the evaluation results regarding the necessity of polarization treatment using a simple piezoelectric element fabricated from Sample 9. [Figure 10] (a) and (b) are graphs showing the evaluation results regarding the temperature resistance of spontaneous polarization using a simple piezoelectric element fabricated from Sample 1, respectively. [Figure 11] (a) and (b) are graphs showing the evaluation results regarding the temperature resistance of spontaneous polarization using a simple piezoelectric element fabricated from Sample 2, respectively. [Modes for carrying out the invention]

[0011] <Knowledge gained by the inventors, etc.> In the aforementioned Patent Document 1, when a KNN film is deposited on a substrate such as a silicon (Si) substrate by sputtering, a KNN film that is spontaneously polarized (hereinafter also referred to as "spontaneously polarized KNN film") is realized by depositing the KNN film at a low temperature. The spontaneously polarized KNN film has the advantage that polarization treatment necessary for the KNN film to operate as a piezoelectric film is unnecessary. Laminates having a spontaneously polarized KNN film are particularly advantageous when applied to sensor applications. However, the spontaneously polarized KNN film realized in Patent Document 1 has large film stress. When the temperature during sputtering is low, the film stress generated in the KNN film tends to be compressive stress, and when the temperature during sputtering is high, the film stress generated in the KNN film tends to be tensile stress. If the film stress of the KNN film is large, for example, if the film stress of the KNN film exceeds 150 MPa, large structural deformation will occur when manufacturing piezoelectric elements such as membrane structures and cantilever structures. As a result, the manufactured piezoelectric element will not function correctly. Furthermore, the manufacturing yield of piezoelectric elements and piezoelectric device modules decreases. For this reason, it is required to keep the film stress of the KNN film low, for example, to keep the film stress of the KNN film below 150 MPa.

[0012] The inventors diligently conducted research with the aim of realizing a KNN film that possesses all three previously unrealized characteristics: "being a spontaneously polarized film," "having a low relative permittivity," and "having low film stress." As a result, they obtained the following five findings. (First finding) The film stress of a KNN film obtained by sputter deposition depends heavily on the initial conditions of the KNN film deposition. (Second finding) By first depositing a KNN film as the first layer (initial layer) under temperature conditions that reduce film stress (in the initial stage of film formation), and then depositing a KNN film as the second layer on top of the first layer under temperature conditions that cause the KNN film to spontaneously polarize, the film stress of the entire KNN film (laminated structure of the first and second layers) is greatly relieved, even when the KNN film (second layer) is deposited at a low temperature that would normally generate large film stress. (Third finding) In order to reproducibly obtain a KNN film with a low dielectric constant, it is necessary to increase the (001) orientation of the KNN film. To obtain a KNN film with a high (001) orientation, it is usually necessary to set the film deposition temperature of the KNN film within a predetermined range. By depositing the first layer of KNN film under temperature conditions that increase the (001) orientation in the initial stages of deposition, and then depositing the second layer of KNN film on top of the first layer under temperature conditions that cause the KNN film to become a spontaneously polarized film, a KNN film with a high (001) orientation can be obtained even when the KNN film (second layer) is deposited at a low temperature that would normally decrease the (001) orientation. The (001) orientation of the KNN film refers to the orientation of the crystals constituting the KNN film to the (001) plane orientation, and will be explained in more detail later. (Fourth finding) For example, in order to reproducibly obtain a KNN film with a relative permittivity of 490 or less, the (001) orientation rate of the KNN film must be 90% or higher. By depositing the first layer of KNN film under conditions where the (001) orientation rate is 95% or higher in the initial stage of film formation, a KNN film with a (001) orientation rate of 90% or higher can be obtained even when the second layer of KNN film is subsequently deposited at a low temperature. (Fifth finding) In the initial stages of film formation, a KNN film as the first layer is formed under conditions where the film stress decreases and the (001) orientation rate increases. Subsequently, a KNN film as the second layer is formed on the first layer under temperature conditions where the KNN film becomes a spontaneously polarized film. This makes it possible to realize a KNN film that is a spontaneously polarized film, has a low relative permittivity, and low film stress, that is, a KNN film that possesses all three of the above characteristics.

[0013] Based on the five findings described above, the inventors have discovered that by forming a KNN film as the first layer under temperature conditions in the initial stage of film formation where the film stress is 100 MPa or less and the (001) orientation ratio is 95% or more, and then forming a KNN film as the second layer under temperature conditions where the KNN film becomes a spontaneously polarized film, a KNN film that is a spontaneously polarized film, has a film stress of 150 MPa or less, and a relative permittivity of 490 or less can be obtained.

[0014] This disclosure is based on the problems and knowledge that the inventors have obtained.

[0015] <One aspect of this disclosure> Hereinafter, one aspect of this disclosure will be described with reference to the drawings.

[0016] (1) Structure of the piezoelectric laminate As shown in Figure 1, the piezoelectric laminate (laminated substrate) 10 (hereinafter also referred to as piezoelectric laminate 10) according to this embodiment comprises a substrate 1, a lower electrode film 2 formed on the substrate 1, a piezoelectric film (piezoelectric thin film) 3 formed on the lower electrode film 2, and an upper electrode film 4 formed on the piezoelectric film 3.

[0017] As the substrate 1, a single-crystal silicon (Si) substrate 1a on which a surface oxide film (SiO2 film) 1b such as a thermal oxide film or a CVD (Chemical Vapor Deposition) oxide film is formed, i.e., a Si substrate having a surface oxide film, can be suitably used. Alternatively, as the substrate 1, a Si substrate 1a having an insulating film formed of an insulating material other than SiO2 can be used instead of the surface oxide film 1b. Furthermore, as the substrate 1, a Si substrate 1a with an exposed Si(100) plane or Si(111) plane on its surface, i.e., a Si substrate without a surface oxide film 1b or insulating film, can also be used. Additionally, as the substrate 1, an SOI (Silicon On Insulator) substrate or a quartz glass (SiO2) substrate can be used. The thickness of the single-crystal Si substrate 1a can be, for example, 300 μm to 1000 μm, and the thickness of the surface oxide film 1b can be, for example, 1 nm to 4000 nm.

[0018] The lower electrode film 2 can be formed using, for example, platinum (Pt). The lower electrode film 2 is a polycrystalline film. Hereinafter, a polycrystalline film fabricated using Pt will also be referred to as a Pt film. It is preferable that the (111) plane of the Pt film is parallel to the main surface of the substrate 1 (including cases where the (111) plane is inclined at an angle of ±5° or less with respect to the main surface of the substrate 1), that is, the Pt film is oriented in the (111) plane direction. The orientation of the Pt film in the (111) plane direction means that in the X-ray diffraction pattern obtained by X-ray diffraction (XRD) measured on the surface of the piezoelectric film 3, no peaks other than those attributable to the (111) plane are observed. Thus, it is preferable that the main surface of the lower electrode film 2 (the surface that serves as the base for the piezoelectric film 3) is composed of a Pt(111) plane. The lower electrode film 2 can be fabricated by methods such as sputtering and vapor deposition. In addition to Pt, the lower electrode film 2 can also be formed using various metals such as gold (Au), ruthenium (Ru), or iridium (Ir), alloys mainly composed of these metals, or metal oxides such as strontium ruthenate (SrRuO3, abbreviated as SRO) or lanthanum nickelate (LaNiO3, abbreviated as LNO). When forming the lower electrode film 2 using a metal oxide, it is preferable that the crystals constituting the lower electrode film 2 are preferentially oriented in the (001) plane orientation with respect to the surface of the substrate 1. The lower electrode film 2 can be a single layer film formed using the above-mentioned various metals, alloys mainly composed of the above-mentioned various metals, or metal oxides. The lower electrode film 2 may also be a laminate of a Pt film and a film mainly composed of SRO provided on the Pt film, or a laminate of a Pt film and a film mainly composed of LNO provided on the Pt film. The thickness of the lower electrode film 2 (or the total thickness of each layer if the lower electrode film 2 is a laminate) can be, for example, 100 nm or more and 400 nm or less.

[0019] An adhesion layer 6 may be provided between the substrate 1 and the lower electrode film 2 in order to enhance the adhesion therebetween. The adhesion layer 6 can be, for example, a layer containing zinc (Zn) and oxygen (O) as main components (hereinafter also referred to as "ZnO layer"). The ZnO layer can be formed using, for example, zinc oxide. The composition ratio of Zn and O constituting the ZnO layer preferably satisfies the relationship of Zn:O=1:1, but is not limited thereto, and may have some variation. The ZnO layer is a polycrystalline layer. The ZnO layer preferably has its (0001) plane parallel to the main surface of the substrate 1 (including the case where the (0001) plane is inclined at an angle within ±5° with respect to the main surface of the substrate 1), that is, the ZnO layer is preferably oriented in the (0001) plane orientation. The phrase "the ZnO layer is oriented in the (0001) plane orientation" means that in the X-ray diffraction pattern obtained by XRD measured on the surface of the piezoelectric film 3, the intensity of the peak attributed to the (0002) plane is high. As described above, the main surface of the ZnO layer (the surface serving as the base for the lower electrode film 2) is preferably constituted by the ZnO (0001) plane. The ZnO layer can be formed by a method such as a sputtering method or a vapor deposition method. The thickness of the ZnO layer can be, for example, 1 nm or more and 200 nm or less, preferably 10 nm or more and 50 nm or less. As the adhesion layer 6, for example, a layer containing titanium (Ti), tantalum (Ta), titanium oxide (TiO2), nickel (Ni), ruthenium oxide (RuO2), iridium oxide (IrO2) or the like as a main component may be provided. Such an adhesion layer 6 can also be formed by a method such as a sputtering method or a vapor deposition method, and the thickness of the adhesion layer 6 can be, for example, 1 nm or more and 200 nm or less, preferably 10 nm or more and 50 nm or less. In this specification, the adhesion layer 6 provided between the substrate 1 and the lower electrode film 2 may also be referred to as a lower adhesion layer 6.

[0020] The piezoelectric film 3 is, for example, a film formed from an alkali niobium oxide containing potassium (K), sodium (Na), niobium (Nb), and oxygen (O). That is, the piezoelectric film 3 is a film containing an alkali niobium oxide containing K, Na, Nb, and O as a main component. The piezoelectric film 3 has a composition formula (K 1-x Na x)It can be formed using an alkali niobium oxide represented by NbO3, that is, potassium sodium niobate (KNN). The coefficient x [=Na / (K+Na)] in the above composition formula can be set within a range of 0<x<1, preferably 0.4≦x≦0.8. The piezoelectric film 3 is a KNN polycrystalline film (hereinafter also referred to as KNN film 3). In addition, the crystal structure of KNN is a perovskite structure. That is, the KNN film 3 has a perovskite structure. Further, it is preferable that more than half of the crystals in the crystal group constituting the KNN film 3 have a columnar structure. In this specification, the crystal system of KNN is regarded as a tetragonal crystal system. The KNN film 3 can be formed by a sputtering method. The thickness of the KNN film 3 can be, for example, 0.5 μm to 5 μm, preferably 1 μm to 3 μm.

[0021] The crystals constituting the KNN film 3 are preferentially oriented in the (001) plane orientation with respect to the main surface of the substrate 1 (when the substrate 1 is, for example, a Si substrate 1a having a surface oxide film 1b or an insulating film or the like, the Si substrate 1a). That is, the main surface of the KNN film 3 (the surface serving as the base of the upper electrode film 4) is mainly composed of KNN (001) planes. For example, by directly forming the KNN film 3 on a Pt film (lower electrode film 2) whose main surface is mainly composed of Pt (111) planes, the KNN film 3 whose main surface is mainly composed of KNN (001) planes can be obtained. In this specification, that the crystals constituting the KNN film 3 are oriented in the (001) plane orientation means that the (001) planes of the crystals constituting the KNN film 3 are parallel or substantially parallel to the main surface of the substrate 1. In addition, that the crystals constituting the KNN film 3 are preferentially oriented in the (001) plane orientation means that there are many crystals whose (001) planes are parallel or substantially parallel to the main surface of the substrate 1.

[0022] Furthermore, the alkali niobium oxide that constitutes the KNN film 3 includes lithium (Li), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), bismuth (Bi), antimony (Sb), vanadium (V), indium (In), tantalum (Ta), molybdenum (Mo), tungsten (W), chromium (Cr), Ti, zirconium (Zr), hafnium (Hf), scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), The alkaliniobium oxide may further contain at least one element (dopant) selected from the group consisting of samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), copper (Cu), zinc (Zn), silver (Ag), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), aluminum (Al), silicon (Si), germanium (Ge), tin (Sn), and gallium (Ga). The concentrations of these elements in the alkaliniobium oxide can be, for example, 5 at% or less (if multiple of the above elements are included, the total concentration must be 5 at% or less).

[0023] As will be explained in more detail later, in this embodiment, first, a first KNN film 3a (first piezoelectric film, hereinafter also referred to as "KNN film 3a"), which is a part of the KNN film 3, is deposited at a first temperature at which the orientation ratio becomes 95% or more and the film stress becomes 100 MPa or less. Then, the second KNN film 3b (second piezoelectric film, hereinafter also referred to as "KNN film 3b"), which is the other part of the KNN film 3, is deposited on the KNN film 3a at a second temperature at which the KNN film 3b becomes a spontaneously polarized film. As a result, the KNN film 3 in this embodiment (i.e., the laminate of KNN film 3a and KNN film 3b) possesses all of the features 1 to 3 described later. Furthermore, the KNN film 3 in this embodiment may also possess feature 4 described later.

[0024] The following describes the features 1 to 4 that the KNN film 3 of this embodiment may possess.

[0025] (Feature 1) In the hysteresis curve (PE hysteresis curve) showing the correlation between the polarization amount (P) of the KNN film 3 and the applied electric field (E), obtained by applying an electric field to the KNN film 3 under predetermined conditions, the coercive electric field E on the positive electric field side C + and the negative field side's coercive field E C - It has the characteristic that "the median value of the coercive field between it and the other is a positive value."

[0026] In this embodiment, the PE hysteresis curve is prepared, for example, by depositing an upper electrode film 4 on a KNN film 3 with a thickness of 2 μm, grounding the lower electrode film 2, and applying a triangular wave or sinusoidal (sin wave) electric field of -150 kV / cm to +150 kV / cm (i.e., a triangular wave or sin wave voltage of -30 V to +30 V) to the KNN film 3 via the upper electrode film 4 at a frequency of 1 kHz, measuring the polarization amount of the KNN film 3, and plotting the obtained polarization amount. Furthermore, "coercive field" refers to a polarization amount of 0 μC / cm 2 The two electric field values ​​at which this occurs are, i.e., the intersection points with the x-axis in the PE hysteresis curve. Also, "cooling field E C + "This means that the polarization amount is 0 μC / cm 2 This is the electric field value on the positive electric field side when this occurs. Also, "cooling field E C - "This means that the polarization amount is 0 μC / cm 2 This is the electric field value on the negative electric field side when this occurs. Also, the "median value of the cohesive electric field" is (E C + -E C - It is a value calculated using the formula ) / 2.

[0027] As described above, the KNN film 3 in this embodiment has the characteristic that the median value of the coercive field in the PE hysteresis curve is a positive value. The KNN film 3 having this characteristic is a spontaneously polarized film (spontaneously polarized KNN film) in which the polarization direction is aligned in a certain direction (for example, upward).

[0028] Here, "spontaneously polarized film" refers to a KNN film 3 whose polarization direction spontaneously aligns in a certain direction (without applying an electric field (voltage) through the lower electrode film 2 and upper electrode film 4 even once after film formation). Furthermore, "upward" in this specification refers to the direction from the lower electrode film 2 side to the upper electrode film 4 side. Also, "polarization direction aligned in a certain direction" means that the majority (more than half) of the crystals constituting the KNN film 3 are polarized in a certain direction. For example, "polarization direction aligned upward" means that the polarization direction of the majority of the crystals constituting the KNN film 3 is upward.

[0029] In addition, for KNN films that are not spontaneously polarizing films, the PE hysteresis curve generally becomes a graph symmetrical with respect to the origin, and the coercive field E C + The absolute value of and the coercive field E C - The absolute values ​​of these values ​​are approximately the same. When manufacturing a piezoelectric element 20, such as a sensor device, using a piezoelectric laminate having such a KNN film, it is necessary to perform polarization treatment during the manufacturing process. Polarization treatment is a process in which a large electric field is applied to the KNN film 3 (under heating if necessary) to align the polarization direction of the KNN film 3 to a certain direction (the direction of the applied electric field).

[0030] Because the KNN film 3 is a spontaneously polarizing film, polarization treatment is unnecessary when manufacturing the piezoelectric element 20 described later using the piezoelectric laminate 10 having the KNN film 3 of this embodiment.

[0031] The median coercive field is preferably 10 kV / cm or higher. This allows more of the crystals constituting the KNN film 3 to be polarized in a specific direction (e.g., upward). As a result, the direction of spontaneous polarization occurring in the KNN film 3 (i.e., the polarization direction of the KNN film 3) can be stabilized, and a KNN film 3 that does not require polarization treatment can be reliably obtained.

[0032] The median coercive field is preferably 100 kV / cm or less, more preferably 70 kV / cm or less. This prevents a decrease in the piezoelectric properties (e.g., piezoelectric constant) of the KNN film 3.

[0033] The polarization characteristics of the KNN film 3 are maintained (not lost) even when the KNN film 3 is exposed to high temperatures, for example, when the KNN film 3 is subjected to a thermal history of 400°C or higher. For example, even when the KNN film 3 is exposed to high temperatures during processes such as the deposition of the upper electrode film 4, annealing, formation of the insulating film 8 and metal wiring 9a, 9b described later (for example, deposition of the insulating film 8 by plasma CVD or ALD method, patterning), and mounting (for example, wire bonding, die bonding, solder reflow), the spontaneous polarization generated in the KNN film 3 is maintained. The inventors have confirmed that even when the KNN film 3 is subjected to a thermal history of 500°C, the polarization characteristics of the KNN film 3 are maintained without deterioration. Furthermore, the inventors have confirmed that when the KNN film 3 is subjected to a thermal history of approximately 600°C, although the polarization characteristics of the KNN film 3 deteriorate somewhat, the spontaneous polarization generated in the KNN film 3 is maintained. This makes it possible to suitably apply the piezoelectric element 20 (piezoelectric device module 30), which will be obtained by processing the piezoelectric laminate 10 having the KNN film 3, to sensor applications. In addition, it is possible to avoid a decrease in the performance of the sensor made using the piezoelectric element 20.

[0034] (Feature 2) KNN film 3 also possesses the additional characteristic of having a relative permittivity of 490 or less.

[0035] The relative permittivity of the KNN film 3 is 490 or less, which allows for the application of the piezoelectric element 20 (piezoelectric device module 30), described later, obtained by processing the piezoelectric laminate 10, to sensor applications, resulting in a highly sensitive sensor. Furthermore, the lower the relative permittivity of the KNN film 3, the higher the sensitivity of the sensor fabricated by processing the piezoelectric laminate 10.

[0036] In order to reliably (reliably) exhibit this characteristic, the (001) orientation rate of the KNN film 3 must be 90% or higher. The (001) orientation rate of the KNN film 3 is the orientation rate of the crystals constituting the KNN film 3 toward the (001) plane. "The (001) orientation rate of the KNN film 3 is 90% or higher" means that, for example, 90% or more of the crystals constituting the KNN film 3 are oriented toward the (001) plane with respect to the main plane of the substrate 1. In this specification, "orientation rate" is a value calculated by the following formula (1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurement on the KNN film 3.

[0037] Orientation rate (%) = {(001) peak intensity / ((001) peak intensity + (110) peak intensity)} × 100 ... (1)

[0038] In equation (1) above, the "(001) peak intensity" refers to the intensity of the diffraction peak in the X-ray diffraction pattern obtained by performing XRD measurements on the KNN film 3, which is caused by crystals oriented in the (001) plane orientation among the crystals constituting the KNN film 3 (i.e., crystals whose (001) plane is parallel to the main plane of the substrate 1), and is the intensity of the peak that appears in the range of 2θ from 20° to 23°. If multiple peaks appear in the range of 2θ from 20° to 23°, it is the intensity of the highest peak. Furthermore, in equation (1) above, the "(110) peak intensity" refers to the intensity of the diffraction peak in the X-ray diffraction pattern obtained by performing XRD measurements on the KNN film 3, which is caused by crystals oriented in the (110) plane orientation among the crystals constituting the KNN film 3 (i.e., crystals whose (110) plane is parallel to the main plane of the substrate 1), and is the intensity of the peak that appears in the range of 2θ from 30° to 33°. If multiple peaks appear within the range of 30° to 33° for 2θ, the intensity of the highest peak is used.

[0039] (Feature 3) KNN film 3 also possesses the additional characteristic of having a film stress of 150 MPa or less.

[0040] The film stress of the KNN film 3 is 150 MPa or less, which suppresses large structural deformation when processing the piezoelectric laminate 10 to fabricate piezoelectric elements 20 such as membrane structures and cantilever structures, as described later. As a result, the piezoelectric elements 20 (piezoelectric device module 30 described later) obtained by processing the piezoelectric laminate 10 can be operated normally.

[0041] (Feature 4) The KNN film 3 may further possess the characteristic that, "when a negative voltage (AC) is continuously applied to the upper electrode film 4 such that a unipolar AC electric field of 300 kV / cm is generated between the lower electrode film 2 and the upper electrode film 4 (i.e., on the KNN film 3), the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of its initial value exceeds 10 million."

[0042] For example, in the case of a piezoelectric laminate 10 having a KNN film 3 with a thickness of 2 μm, when a unipolar triangular wave or sinusoidal AC voltage with amplitude in the range of 0V to -60V is continuously applied to the upper electrode film 4 (via the KNN film 3) at a frequency of 300 Hz, with the lower electrode film 2 grounded, so that the direction of the electric field applied to the KNN film 3 does not reverse (so that the direction of the electric field is unidirectional), the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of the initial value exceeds 10 million.

[0043] In this specification, "unipolar electric field" means an electric field that is unidirectional even if the magnitude of the voltage applied to the KNN film 3 via the upper electrode film 4 fluctuates periodically within the range of, for example, 0V to -60V. In this specification, "the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of its initial value when a negative voltage is continuously applied to the upper electrode film 4 to generate a unipolar AC electric field of 300kV / cm in the KNN film 3" is also referred to as "number of application cycles."

[0044] When an AC voltage is applied to the KNN film 3 via the upper electrode film 4, the KNN film 3 deforms. The higher the applied voltage, the greater the deformation of the KNN film 3. The KNN film 3 in this embodiment may have the characteristic that even when repeatedly subjected to large deformations due to the continuous application of large AC voltages, the piezoelectric displacement does not decrease easily, that is, it has excellent AC stress resistance.

[0045] In the piezoelectric laminate 10 obtained by the novel method described above, a KNN film 3a with a high (001) orientation and low film stress, for example, a KNN film 3a with a (001) orientation of 95% or more and a film stress of 100 MPa or less, is interposed between the lower electrode film 2 and the KNN film 3b. As a result, the KNN film 3 in this embodiment (a laminate of KNN film 3a and KNN film 3b) can have even better AC stress resistance compared to the case where the KNN film 3a is not interposed. This is thought to be because the interposition of the KNN film 3a significantly improves the adhesion between the lower electrode film 2 and the KNN film 3. Thus, the fact that the number of applied cycles can be increased to more than 10 million by interposing the KNN film 3a, that is, that the AC stress resistance of the KNN film 3 can be increased, is a novel finding discovered for the first time as a result of the inventors' diligent research.

[0046] The KNN film 3 has excellent AC stress resistance, which makes it possible to improve the reliability of the piezoelectric element 20 (piezoelectric device module 30), described later, obtained by processing the piezoelectric laminate 10.

[0047] The inventors have confirmed that in a piezoelectric laminate 10 in which a KNN film 3a having a (001) orientation ratio of 95% or more and a film stress of 100 MPa or less is interposed between the lower electrode film 2 and the KNN film 3b, when a negative voltage is continuously applied to the KNN film 3 via the upper electrode film 4 so that a unipolar AC electric field of 300 kV / cm is generated in the KNN film 3, the piezoelectric displacement of the KNN film 3 can be maintained at 80% or more of the initial value even after the number of application cycles exceeds 10 million, and even 50 million or more.

[0048] In contrast, if the KNN film 3a is not present, that is, if the KNN film 3 is not composed of a laminate of KNN film 3a and KNN film 3b, then when a large AC voltage is continuously applied to the KNN film 3 via the upper electrode film 4, causing the KNN film 3 to deform continuously and significantly, a phenomenon occurs where the KNN film 3 gradually peels off from the lower electrode film 2. As a result, the piezoelectric displacement of the KNN film 3 tends to decrease.

[0049] The inventors have confirmed that in a piezoelectric laminate in which the KNN film 3a is not interposed between the lower electrode film 2 and the KNN film 3b, when a negative voltage is continuously applied to the KNN film via the upper electrode film 4 so that a unipolar AC electric field of 300 kV / cm is generated in the KNN film, the piezoelectric displacement of the KNN film decreases to less than 80% of the initial value before the number of application cycles reaches 10 million.

[0050] As described above, the KNN film 3 in this embodiment can have all of the features 1 to 3 described above, preferably all of the features 1 to 4 described above. By having all of the features 1 to 3 described above, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 having the KNN film 3 can be suitably applied to sensor applications. Furthermore, by having all of the features 1 to 4 described above, the piezoelectric element 20 (piezoelectric device module 30) can be more suitably applied to sensor applications.

[0051] Furthermore, in this embodiment, when forming the KNN film 3, first, the KNN film 3a is formed at a first temperature where the (001) orientation ratio is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is formed on the KNN film 3a at a second temperature where the KNN film 3b becomes a spontaneously polarized film. Therefore, the KNN film 3 in this embodiment has a laminated structure consisting of a KNN film 3a as a first layer (initial layer) formed at the first temperature and a KNN film 3b as a second layer formed at the second temperature.

[0052] Spontaneous polarization does not occur in the KNN film 3a deposited at the first temperature. In other words, KNN film 3a is not a spontaneously polarized film. For this reason, as the ratio of the thickness of KNN film 3a to the total thickness of KNN film 3 (the sum of the thickness of KNN film 3a and KNN film 3b) increases, the above-mentioned characteristic 1 tends to become less likely to occur. In other words, it tends to become less likely to generate spontaneous polarization in KNN film 3. Therefore, it is preferable to keep the thickness of KNN film 3a to the minimum necessary to relax the film stress of KNN film 3 and keep the overall film stress of KNN film 3 below 150 MPa. The thickness of KNN film 3a is not strictly limited, but for example, it is preferable to have a thickness of 20% or less of the total thickness of KNN film 3. This ensures that a KNN film 3 possessing the above-mentioned characteristic 1, i.e., a spontaneously polarized KNN film 3, is reliably obtained.

[0053] The upper electrode film 4 is mainly composed of various metals such as Pt, Au, Al, and Cu, or alloys thereof. The upper electrode film 4 can be fabricated by methods such as sputtering, vapor deposition, plating, and metal paste. The upper electrode film 4 does not significantly affect the crystal structure of the KNN film 3, unlike the lower electrode film 2. Therefore, the material, crystal structure, and fabrication method of the upper electrode film 4 are not particularly limited. In addition, an adhesion layer 7 mainly composed of RuO2, IrO2, Ti, Ta, TiO2, Ni, etc. may be provided between the KNN film 3 and the upper electrode film 4 to improve their adhesion. The thickness of the upper electrode film 4 can be, for example, 50 nm to 5000 nm, preferably 50 nm to 300 nm, and if an adhesion layer 7 is provided, the thickness of the adhesion layer 7 can be, for example, 1 nm to 200 nm, preferably 5 nm to 50 nm. In this specification, the adhesion layer 7 provided between the KNN film 3 and the upper electrode film 4 may also be referred to as the upper adhesion layer 7.

[0054] (2) Method for manufacturing piezoelectric laminates, piezoelectric elements, and piezoelectric device modules The manufacturing methods for the piezoelectric laminate 10, piezoelectric element, and piezoelectric device module described above will now be explained.

[0055] (Formation of the lower adhesion layer and lower electrode film) First, a substrate 1 is prepared, and a lower adhesion layer 6 (e.g., a ZnO layer) and a lower electrode film 2 (e.g., a Pt film) are deposited on one of the main surfaces of the substrate 1 in that order, for example by sputtering. Alternatively, a substrate 1 may be prepared with the lower adhesion layer 6 and the lower electrode film 2 already deposited on one of the main surfaces.

[0056] The following are examples of conditions for forming the ZnO layer as the lower adhesion layer 6. The film formation time for the lower adhesion layer 6 is adjusted as appropriate according to the target thickness of the lower adhesion layer 6. Target: ZnO sintered body Temperature (substrate temperature): 200°C or higher and 700°C or lower, preferably 300°C or higher and 700°C or lower, more preferably 500°C or higher and 700°C or lower. Discharge power density: 2W / cm² 2 More than 6W / cm 2 Preferably 3 W / cm 2 More than 5W / cm 2 below Atmosphere: A mixed gas atmosphere consisting of argon (Ar) gas and oxygen (O2) gas (hereinafter also referred to as "Ar / O2 mixed gas atmosphere"). Ratio of partial pressure of Ar gas to O2 gas (partial pressure of Ar gas / partial pressure of O2 gas): 5 / 1 to 30 / 1, preferably 7 / 1 to 20 / 1, more preferably 10 / 1 to 15 / 1 Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 1 nm to 200 nm, preferably 10 nm to 50 nm

[0057] In this specification, numerical ranges such as "5 / 1 to 30 / 1" mean that the lower and upper limits are included within that range. The same applies to other numerical ranges.

[0058] The following are examples of conditions for forming the Ti layer, etc., as the lower adhesion layer 6. Target: Ti plates, etc. Temperature (substrate temperature): 100°C to 500°C, preferably 200°C to 400°C Atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Other conditions can be the same as those for when the ZnO layer is provided.

[0059] The following are examples of conditions for forming the Pt film as the lower electrode film 2. The film formation time for the lower electrode film 2 is adjusted as appropriate according to the target thickness of the lower electrode film 2. Target: Pt board Temperature (substrate temperature): 200°C to 600°C, preferably 300°C to 500°C Discharge power density: 1W / cm² 2 More than 5W / cm 2 Preferably 2 W / cm 2 More than 4W / cm 2 below Atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 100nm to 400nm

[0060] (KNN film deposition) After the lower adhesion layer 6 and the lower electrode film 2 have been formed, a KNN film 3 is then formed on the lower electrode film 2 by a sputtering method such as RF magnetron sputtering. The composition of the KNN film 3 can be adjusted, for example, by controlling the composition of the target used during sputtering. The target can be made by mixing K2CO3 powder, Na2CO3 powder, Nb2O5 powder, etc., and firing them. The composition of the target can be controlled by adjusting the mixing ratio of K2CO3 powder, Na2CO3 powder, Nb2O5 powder, etc. When forming a KNN film 3 containing the above-mentioned elements such as Cu and Mn, a target can be used in which Cu powder (or CuO powder) or Mn powder (or MnO powder), etc., are mixed in a predetermined ratio in addition to the above-mentioned powders.

[0061] The KNN film 3 is fabricated in two stages by changing the temperature conditions. Specifically, first (at the beginning of film fabrication), KNN film 3a is fabricated at the first temperature, and then KNN film 3b is fabricated at the second temperature.

[0062] The first temperature is the temperature at which the (001) orientation ratio of the KNN film 3a becomes 95% or higher and the film stress becomes 100 MPa or lower. For example, the first temperature is the temperature at which the (001) orientation ratio of the KNN film 3a becomes 95% or higher when a KNN film 3a with a thickness of 2 μm (±10%) is fabricated at the first temperature. Also, the first temperature is the temperature at which the film stress of the KNN film 3a becomes 100 MPa or lower when a KNN film 3a with a thickness of 2 μm (±10%) is fabricated at the first temperature.

[0063] The second temperature is the temperature at which the KNN film 3b becomes a spontaneously polarized film, that is, the temperature at which the median value of the coercive field in the PE hysteresis curve becomes a positive value. The second temperature is, for example, the temperature at which the KNN film 3b becomes a spontaneously polarized film when a KNN film 3b with a thickness of 2 μm (±10%) is fabricated at the second temperature.

[0064] The first and second temperatures depend somewhat on the sputtering deposition apparatus and deposition conditions, but in the sputtering deposition of the KNN film 3 in this embodiment, the second temperature is usually lower than the first temperature (first temperature > second temperature). For example, the first temperature can be in the range of 550°C to 600°C, and the second temperature can be in the range of 400°C to 500°C.

[0065] Other conditions besides temperature when forming KNN film 3 (KNN film 3a, KNN film 3b) include the following examples for both film formation at the first temperature and film formation at the second temperature. Discharge power density: 2.7 W / cm² 2 More than 4.1W / cm 2 Preferably, 2.8 W / cm² 2 More than 3.8W / cm 2 below Atmosphere: An atmosphere containing at least Ar gas, preferably an Ar / O2 mixed gas atmosphere. Ambient pressure: 0.03 Pa or more and 0.5 Pa or less, preferably 0.04 Pa or more and 0.4 Pa or less Ratio of partial pressure of O2 gas to Ar gas (O2 gas partial pressure / Ar gas partial pressure): 0 to 1 / 20, preferably 0 to 1 / 30 Film formation rate: 0.5 μm / hr to 4 μm / hr, preferably 0.5 μm / hr to 2 μm / hr Total thickness of KNN film: 0.5 μm or more and 5 μm or less, preferably 1 μm or more and 3 μm or less

[0066] Note that "the O2 gas partial pressure / Ar gas partial pressure is 0 (zero)" means the state where the O2 gas partial pressure is 0, i.e., the atmosphere is one with only Ar gas. Also, "total thickness of the KNN film" is the sum of the thickness of the KNN film 3a deposited at the first temperature and the KNN film 3b deposited at the second temperature. Furthermore, the deposition times for KNN films 3a and 3b are adjusted as appropriate according to the target thickness of KNN films 3a and 3b. As mentioned above, it is preferable that the thickness of KNN film 3a be the minimum necessary to reduce the film stress in KNN film 3b during deposition at the second temperature and to reduce the overall film stress of KNN film 3 to 150 MPa or less. For this reason, it is preferable to adjust the deposition time for KNN film 3a (deposition time at the first temperature) so that the thickness of KNN film 3a is 20% or less of the total thickness of KNN film 3.

[0067] As described above, first, the KNN film 3a is deposited at a first temperature where the (001) orientation rate is 95% or higher and the film stress is 100 MPa or less. Then, the KNN film 3b is deposited on the KNN film 3a at a second temperature where the KNN film 3b becomes a spontaneously polarized film. Even if the second temperature is low enough that the (001) orientation rate decreases or large film stress is generated in the KNN film 3b, the overall (001) orientation rate of the KNN film 3 after the deposition of the KNN film 3b can be made 90% or higher, and the overall film stress of the KNN film 3 can be greatly relieved. As a result, while the KNN film 3 becomes a spontaneously polarized film, the relative permittivity of the entire KNN film 3 can be reproducibly reduced to 490 or less, and the overall film stress of the KNN film 3 can be reduced to 150 MPa or less. In other words, by depositing the KNN film 3 (KNN film 3a and KNN film 3b) in two stages by changing the temperature under the above conditions, a KNN film 3 possessing all of the above characteristics 1 to 3 can be obtained. Furthermore, by fabricating the KNN film 3 in two stages by changing the temperature under the above conditions, that is, by providing a KNN film 3a with a high (001) orientation and low film stress, a KNN film 3 possessing all of the above-mentioned features 1 to 4 can also be obtained.

[0068] (Formation of the upper adhesion layer and upper electrode film) Once the deposition of the KNN film 3 is complete, the upper adhesion layer 7 (e.g., a RuO2 layer) and the upper electrode film 4 (e.g., a Pt film) are deposited on the KNN film 3 in that order, for example by sputtering.

[0069] The following are examples of conditions for forming the RuO2 layer or the like as the upper adhesion layer 7. The film formation time for the upper adhesion layer 7 is adjusted as appropriate according to the target thickness of the upper adhesion layer 7. Target: Ru boards, etc. Temperature (substrate temperature): Room temperature (25℃) or higher and 500℃ or lower Discharge power density: 0.3 W / cm² 2 More than 2W / cm 2 Preferably 0.5 W / cm² 2 More than 1W / cm 2 below Atmosphere: Ar / O2 mixed gas atmosphere Ratio of partial pressure of Ar gas to O2 gas (partial pressure of Ar gas / partial pressure of O2 gas): 3 / 5 to 1 / 1, preferably 3 / 4 to 1 / 1 Ambient pressure: 0.1 Pa to 1.0 Pa, preferably 0.2 Pa to 0.7 Pa Thickness: 1 nm to 200 nm, preferably 5 nm to 50 nm

[0070] The following are examples of conditions for forming the Pt film or the like as the upper electrode film 4. The film formation time for the upper electrode film 4 is adjusted as appropriate according to the target thickness of the upper electrode film 4. Target: Pt boards, etc. Temperature (substrate temperature): Room temperature (25℃) or higher and 500℃ or lower Discharge power density: 1W / cm² 2 More than 5W / cm 2 Preferably 2 W / cm 2 More than 4W / cm 2 below Atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 50 nm to 5000 nm, preferably 50 nm to 300 nm

[0071] As described above, by sequentially forming the lower adhesion layer 6, lower electrode film 2, KNN film 3 (KNN films 3a, 3b), upper adhesion layer 7, and upper electrode film 4, a piezoelectric laminate 10 as shown in Figure 1 is obtained.

[0072] (Fabrication of piezoelectric elements) After fabricating a piezoelectric laminate 10 as shown in Figure 1, the piezoelectric laminate 10 is processed to form an element having a KNN film 3 (also referred to as a piezoelectric element 20).

[0073] Specifically, first, the upper electrode film 4 (including the upper adhesion layer 7) and the KNN film 3 are individually patterned by dry etching using, for example, Ar gas or a reactive gas. In the patterning process, the upper electrode film 4 (including the upper adhesion layer 7) and the KNN film 3 are shaped into predetermined forms, while a portion of the lower electrode film 2 is exposed. In addition, a photoresist can be used as an etching mask in the patterning process. Figure 2 shows the piezoelectric laminate 10, i.e., the piezoelectric element 20, after the patterning process is completed. The piezoelectric element 20 shown in Figure 2 is also referred to as a simple piezoelectric element.

[0074] After fabricating a simple piezoelectric element as shown in Figure 2, the lower electrode film 2 and the lower adhesion layer 6 are patterned by dry etching using, for example, Ar gas or a reactive gas, thereby shaping the lower electrode film 2 and the lower adhesion layer 6 into predetermined shapes. In this patterning process, a photoresist can be used as an etching mask.

[0075] Once the patterning of the lower electrode film 2 and the lower adhesion layer 6 is complete, the insulating film 8 and metal wiring 9a and 9b are provided. Specifically, first, a layer made of insulating material is provided from the upper electrode film 4 to the substrate 1 so as to cover the side surface of the KNN film 3. Then, the insulating film 8 is provided by patterning the insulating material layer using dry etching with a reactive gas such as Ar gas or CF4 gas, or by wet etching. The insulating film 8 can be formed using oxides such as silicon oxide (SiO2), aluminum oxide (Al2O3), or tantalum oxide (Ta2O5). The insulating film 8 may be a single layer or a laminate of multiple layers. The insulating film 8 can be provided by methods such as CVD or sputtering.

[0076] After providing the insulating film 8, a layer made of a metal-containing material (metal wiring layer) is provided. Then, the metal wiring layer is patterned by dry etching using Ar gas or a reactive gas, or by wet etching, to form metal wirings 9a and 9b. Metal wiring 9a is formed (patterned) so that it is connected to (in contact with) the lower electrode film 2 but not connected to (not in contact with) the upper electrode film 4, while metal wiring 9b is formed so that it is connected to the upper electrode film 4 but not connected to the lower electrode film 2. Metal wirings 9a and 9b can be formed using various metals such as Au, Al, Ti, Cr, etc., or alloys mainly composed of these metals. Metal wirings 9a and 9b may be single-layer films or laminates of multiple layers. Metal wirings 9a and 9b (metal wiring layer) can be provided by methods such as sputtering, vapor deposition, plating, or metal paste.

[0077] Furthermore, a portion of the substrate 1 is removed from its back side (the side opposite to the side on which the lower electrode film 2, etc., is formed, out of the two main surfaces of the substrate 1) by Deep-RIE or wet etching. This yields a piezoelectric element 20 such as a membrane structure or a cantilever structure, for example, a membrane-type MEMS piezoelectric element 20 as shown in Figure 3.

[0078] Furthermore, the etching conditions for pattern processing when forming the insulating film 8 and metal wiring 9a, 9b, and the etching conditions for the substrate 1 when processing the piezoelectric laminate 10 into the piezoelectric element 20, can be general etching conditions used in semiconductor device manufacturing processes, as long as they do not degrade the insulating properties of the KNN film 3.

[0079] (Fabrication of piezoelectric device modules) By connecting the voltage detection means 11a to the obtained piezoelectric element 20, a device module 30 having a KNN film 3 (hereinafter also referred to as piezoelectric device module 30) is obtained. Figure 4 shows a schematic configuration diagram of the piezoelectric device module 30 according to this embodiment. The piezoelectric device module 30 comprises at least a piezoelectric element 20 and a voltage detection means 11a connected to the piezoelectric element 20. The voltage detection means 11a is a means for detecting the voltage generated between the lower electrode film 2 and the upper electrode film 4 (between electrodes). Various known means can be used as the voltage detection means 11a.

[0080] By connecting the voltage detection means 11a between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can function as a sensor. When the KNN film 3 deforms in response to a change in some physical quantity, a voltage is generated between the lower electrode film 2 and the upper electrode film 4 due to this deformation. By detecting this voltage with the voltage detection means 11a, the magnitude of the physical quantity applied to the KNN film 3 can be measured. In this case, examples of applications for the piezoelectric device module 30 include angular velocity sensors, ultrasonic sensors, pressure sensors, and acceleration sensors.

[0081] (3) Effects According to this embodiment, one or more of the following effects can be obtained.

[0082] (a) KNN film 3 possesses all three characteristics: the median value of the coercive field in the PE hysteresis curve is positive (characteristic 1 above), the relative permittivity is 490 or less (characteristic 2 above), and the film stress is 150 MPa or less (characteristic 3 above). In other words, KNN film 3 is a spontaneously polarizing film, yet it has low film stress and low relative permittivity.

[0083] Because the KNN film 3 is a spontaneously polarizing film, polarization treatment of the KNN film 3 is unnecessary when fabricating the piezoelectric laminate 10 to create the piezoelectric element 20 (piezoelectric device module 30). The elimination of polarization treatment simplifies the manufacturing process of the piezoelectric element 20 (piezoelectric device module 30) obtained by fabricating the piezoelectric laminate 10.

[0084] Because the relative permittivity of the KNN film 3 is 490 or less, a highly sensitive sensor can be obtained when the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 is applied to a sensor application.

[0085] The film stress of the KNN film 3 is 150 MPa or less, which suppresses large structural deformation when processing the piezoelectric laminate 10 to fabricate piezoelectric elements 20 (piezoelectric device modules 30) such as membrane structures and cantilever structures. This allows the piezoelectric elements 20 (piezoelectric device modules 30) obtained by processing the piezoelectric laminate 10 to operate normally. For example, it becomes possible to ensure that the piezoelectric elements 20 (piezoelectric device modules 30) function reliably as sensors.

[0086] Thus, because the KNN film 3 possesses all of the above-mentioned features 1 to 3, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 can be suitably applied to sensor applications.

[0087] (b) The presence of a KNN film 3a with a high orientation and low film stress between the lower electrode film 2 and the KNN film 3b allows the KNN film 3 to further possess the characteristic of having more than 10 million applied cycles (characteristic 4 above), in addition to the characteristics 1 to 3 above. In other words, the KNN film 3 is a spontaneously polarizing film, yet it has low film stress, a low relative permittivity, and excellent AC stress resistance.

[0088] The KNN film 3 has excellent AC stress resistance, meaning that even if the KNN film 3 undergoes repeated large deformations, the amount of piezoelectric displacement does not decrease easily, which makes it possible to improve the reliability of the piezoelectric element 20 (piezoelectric device module 30).

[0089] Thus, because the KNN film 3 possesses all of the above-mentioned features 1 to 4, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 can be more suitably applied to sensor applications.

[0090] (c) The polarization characteristics of the KNN film 3 in this embodiment are maintained even when the KNN film 3 is exposed to high temperatures. For example, even if the KNN film 3 is exposed to high temperatures when the upper electrode film 4 is fabricated, annealed, the insulating film 8 and metal wiring 9a, 9b are formed, and the mounting process is carried out after the KNN film 3 is fabricated, the spontaneous polarization generated in the KNN film 3 is maintained. This makes it possible to more suitably apply the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 to sensor applications. In addition, it is possible to avoid a decrease in the performance of the sensor made using the piezoelectric element 20 (piezoelectric device module 30).

[0091] (d) By having a median coercive field of 10 kV / cm or more, the direction of spontaneous polarization generated in the KNN film 3 can be stabilized, and a KNN film 3 that does not require polarization treatment can be reliably obtained. In addition, by having a median coercive field of 10 kV / cm or more, even if a reverse electric field (an electric field that reverses the polarization direction which is aligned in a certain direction) is mistakenly applied to the KNN film 3 during the fabrication of the piezoelectric laminate 10, piezoelectric element 20, and piezoelectric device module 30, or when using the piezoelectric element 20 (piezoelectric device module 30), the initial polarization direction (the direction in which it was spontaneously polarized) can be maintained.

[0092] (e) When forming the KNN film 3, first, the KNN film 3a is formed at a first temperature in which the (001) orientation ratio becomes 95% or more and the film stress becomes 100 MPa or less, and then the KNN film 3b is formed on the KNN film 3a at a second temperature in which the KNN film 3b becomes a spontaneously polarized film, thereby making it possible to obtain a KNN film 3 that has all of the above features 1 to 3, preferably all of the above features 1 to 4.

[0093] <Other embodiments> The above describes in detail one aspect of this disclosure. However, this disclosure is not limited to the above-described aspect and can be modified in various ways without departing from its essence. Furthermore, these aspects can be combined in any way.

[0094] The above-described embodiment explains an example in which the piezoelectric device module 30 functions as a sensor, but it is not limited to this. That is, the piezoelectric device module 30 may also function as an actuator. In this case, the piezoelectric device module 30 comprises at least a piezoelectric element 20 obtained by molding the piezoelectric laminate 10 described above into a predetermined shape, and a voltage application means 11b (see Figure 4) connected to the piezoelectric element 20. The voltage application means 11b is a means for applying a voltage between the lower electrode film 2 and the upper electrode film 4 (between electrodes). Various known means can be used as the voltage application means 11b. By connecting the voltage application means 11b between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can be made to function as an actuator. By applying a voltage between the lower electrode film 2 and the upper electrode film 4 using the voltage application means 11b, the KNN film 3 can be deformed. This deformation operation can activate various components connected to the piezoelectric device module 30. In this case, examples of applications for the piezoelectric device module 30 include inkjet printer heads, MEMS mirrors for optical scanners, and transducers for ultrasonic generators.

[0095] For example, when forming the piezoelectric laminate 10 into a piezoelectric element 20, the piezoelectric device module 30 manufactured using the piezoelectric laminate 10 (piezoelectric element 20) can be applied to a desired application such as a sensor, insofar as the substrate 1 can be replaced with another substrate. [Examples]

[0096] The following describes experimental results that support the effects of the above-described embodiment.

[0097] [Experiment 1] We conducted experiments to confirm the applicable temperatures for the first and second temperatures when forming the KNN film.

[0098] (Preparation of samples A-G) As the substrate, a Si substrate was prepared with a surface orientation of (100), a thickness of 610 μm, a diameter of 6 inches (also referred to as "φ6 inches"), and a thermal oxide film (thickness 200 nm) formed on the surface. Then, on the thermal oxide film of this Si substrate, a ZnO layer (thickness 25 nm) as the lower adhesion layer, a Pt film (preferentially oriented in the (111) plane orientation relative to the substrate surface, thickness 200 nm) as the lower electrode film, a KNN film (thickness 2 μm) as the piezoelectric film, a RuO2 layer (thickness 10 nm) as the upper adhesion layer, and a Pt film (thickness 100 nm) as the upper electrode film were fabricated in this order to create piezoelectric laminates, samples A to G. In samples A to G, the lower adhesion layer, lower electrode film, KNN film, upper adhesion layer, and upper electrode film were all fabricated by RF magnetron sputtering.

[0099] The conditions for forming the ZnO layer as the lower adhesion layer were as follows: Target: ZnO sintered body Substrate temperature: 500℃ Discharge power density: 4W / cm² 2 Atmosphere: Ar / O2 mixed gas atmosphere Atmospheric pressure: 0.3 Pa Ar gas partial pressure / O2 gas partial pressure: 10 / 1 Deposition time: 3 minutes (thickness 25 nm)

[0100] The conditions for forming the Pt film as the lower electrode film were as follows: Target: Pt board Substrate temperature: 500℃ Discharge power density: 2W / cm² 2 Atmosphere: Ar gas atmosphere Atmospheric pressure: 0.3 Pa Film deposition time: 14 minutes (thickness 200 nm)

[0101] The conditions for depositing the KNN film were as follows: Target: KNN sintered body Discharge power density: 3W / cm² 2 Atmosphere: Ar / O2 mixed gas atmosphere Atmospheric pressure: 0.1 Pa O2 gas partial pressure / Ar gas partial pressure: 1 / 20 Film formation temperature: A specified temperature within the range of 300°C to 650°C. Film deposition time: 60 minutes (thickness 2000 nm (2 μm))

[0102] The conditions for forming the RuO2 layer as the upper adhesion layer were as follows: Target: Ru board Substrate temperature: Room temperature (25℃) Discharge power density: 0.5 W / cm² 2 Atmosphere: Ar / O2 mixed gas atmosphere Atmospheric pressure: 0.3 Pa Ar gas partial pressure / O2 gas partial pressure: 1 / 1 Film deposition time: 6 minutes (thickness 10 nm)

[0103] The conditions for depositing the Pt film as the upper electrode film were as follows: Target: Pt board Substrate temperature: Room temperature (25℃) Discharge power density: 2W / cm² 2 Atmosphere: Ar gas atmosphere Atmospheric pressure: 0.3 Pa Film deposition time: 7 minutes (thickness 100 nm)

[0104] Samples A through G were prepared under the same conditions as described above, except for the KNN film deposition temperature. The KNN film deposition temperatures for samples A through G are shown in Table 1 below.

[0105] <Rating> For samples A through G, the (001) orientation ratio of the KNN film, the film stress of the KNN film, and the median coercive field were evaluated.

[0106] ((001) Evaluation of orientation ratio) The (001) orientation rate of the KNN film was evaluated by calculating it using the above formula (1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurements on the KNN film. The XRD measurements were performed after the KNN film was fabricated but before the upper adhesion layer and upper electrode film were fabricated. The calculation results of the (001) orientation rate are shown in Table 1 below. In Table 1, "orientation rate" refers to the (001) orientation rate of the KNN film.

[0107] (Evaluation of membrane stress) The stress of a thin film on a substrate can be calculated by measuring the amount of substrate warping caused by the thin film, specifically the radius of curvature of the substrate warp, as shown in equation (2) below. Therefore, in this evaluation, first, after depositing the lower adhesion layer, lower electrode film, and KNN film, the radius of curvature R of the substrate (Si substrate) of each sample was measured before depositing the upper adhesion layer and upper electrode film. Then, the film stress of the KNN film of each sample was calculated using equation (2) below. In this evaluation, the radius of curvature R of the Si substrate was calculated by measuring the warp shape of the Si substrate after depositing the lower adhesion layer, lower electrode film, and KNN film using a laser displacement meter.

[0108] TIFF0007948880000001.tif17170

[0109] In equation (2) above, σ is the stress of the thin film (KNN film), and E s / (1-νs ) is the biaxial elastic modulus (Pa) of the substrate, h is the substrate thickness (m), R is the radius of curvature of the substrate warp (m), and t is the thickness of the KNN film (m). In samples A to G, since a Si substrate was used, the value of the biaxial elastic modulus was set to 30.3. In addition, the film stress (σ) of the KNN film was calculated assuming that the Si substrate was sufficiently flat. Furthermore, in samples A to G, a lower adhesion layer (ZnO layer) and a lower electrode film (Pt film) were fabricated, but the thickness of the lower adhesion layer (25 nm) and the lower electrode film (200 nm) are sufficiently small compared to the thickness of the KNN film (2 μm). For this reason, the film stress of the KNN film was calculated by ignoring the effects of the lower adhesion layer and the lower electrode film.

[0110] The calculated membrane stresses for KNN membranes of samples A to G are shown in Table 1 below. In Table 1, "compression" means that the membrane stress is compressive, and "tensile" means that the membrane stress is tensile.

[0111] (Evaluation of the median value of the coercive field) The median value of the coercive field was evaluated as follows. First, piezoelectric laminates of samples A to G were fabricated, and then the upper electrode film (including the upper adhesion layer) and the KNN film were individually patterned by dry etching using Ar gas. In the patterning process, a photoresist was used as the etching mask, and the upper electrode film was formed to a size of φ0.5 mm while a portion of the lower electrode film was exposed to fabricate a simple piezoelectric element as shown in Figure 2. Using each of the simple piezoelectric elements fabricated from samples A to G, PE hysteresis curves were prepared. Specifically, with the lower electrode film grounded, a triangular wave or sine wave electric field of -150 kV / cm to +150 kV / cm was applied to the KNN film via the upper electrode film at a frequency of 1 kHz, the polarization of the KNN film was measured, and the PE hysteresis curve was prepared by plotting the obtained polarization amount with the applied electric field. An Agzact (DBLI) device was used to prepare the PE hysteresis curves. From each PE hysteresis curve, the coercive field E C + and coercive field E C - Obtain the value, and then the coelectric field EC + and coercive field E C - From the value of the coercive field, the median (=(E) C + -E C - The formula ) / 2) was calculated. The results of calculating the median cohesive field for samples A to G are shown in Table 1 below. Note that "median" in Table 1 refers to the median cohesive field.

[0112] [Table 1]

[0113] In sample A, the crystal structure of the KNN film did not become a perovskite structure. Therefore, in the X-ray diffraction pattern obtained by XRD measurement, no peaks were observed within the range of 2θ = 20° to 23°, and as a result, the (001) orientation rate could not be calculated. Furthermore, because the crystal structure of the KNN film was not a perovskite structure, the breakdown voltage characteristics of the KNN film were low, and it was not possible to apply a triangular wave or sinus wave electric field of -150kV / cm to +150kV / cm at a frequency of 1kHz to the KNN film via the upper electrode film when preparing the PE hysteresis curve. Therefore, it was not possible to prepare the PE hysteresis curve, and as a result, the median value of the coercive field could not be measured. From these findings, it can be confirmed that the film deposition temperature for sample A is not applicable to either the first or second temperature.

[0114] In samples B to D, the film stress exceeds 100 MPa. This confirms that the film deposition temperatures for samples B to D are not applicable to the first temperature. On the other hand, in samples B to D, the median coercive field is 10 kV / cm or higher. This confirms that the film deposition temperatures for samples B to D, i.e., the temperature range of 400°C to 500°C, are the temperatures at which the KNN film becomes a spontaneously polarized film, and are applicable to the second temperature.

[0115] In samples E and F, the (001) orientation ratio is 95% or higher, and the film stress is 100 MPa or less. From this, it can be confirmed that the film deposition temperature of samples E and F, i.e., the temperature range of 550°C to 600°C, is applicable to the first temperature. On the other hand, in samples E and F, the median coercive field is 0 kV / cm. In other words, the KNN films in samples E and F are not spontaneously polarized films. From this, it can be confirmed that the film deposition temperature of samples E and F is not applicable to the second temperature.

[0116] In sample G, the (001) orientation ratio is less than 95%, and the film stress is greater than 100 MPa. Furthermore, the median coercive field value for sample G is 0 kV / cm. From these findings, it can be confirmed that the film deposition temperature for sample G is not applicable to either the first or second temperature.

[0117] [Experiment 2] We conducted an experiment to confirm the effect of depositing KNN films in two stages at different temperatures.

[0118] (Preparation of samples 1-16) As the substrate, a Si substrate was prepared with a surface orientation of (100), a thickness of 610 μm, a diameter of 6 inches, and a thermal oxide film (thickness 200 nm) formed on the surface. Then, on the thermal oxide film of this Si substrate, a ZnO layer (thickness 25 nm) as the lower adhesion layer, a Pt film (preferentially oriented in the (111) plane orientation relative to the substrate surface, thickness 200 nm) as the lower electrode film, a KNN film (thickness 2 μm) as the piezoelectric film, a RuO2 layer (thickness 10 nm) as the upper adhesion layer, and a Pt film (thickness 100 nm) as the upper electrode film were fabricated in this order to create piezoelectric laminates, samples 1 to 16. The lower adhesion layer, lower electrode film, KNN film, upper adhesion layer, and upper electrode film were all fabricated by RF magnetron sputtering.

[0119] In samples 1-14, the KNN film was deposited in two stages by changing the temperature conditions. Specifically, the first KNN film was deposited at the first temperature, and then the second KNN film was deposited on top of the first KNN film at a second temperature different from the first temperature. The first and second temperatures for depositing the KNN films in samples 1-14 are as shown in Table 2 below, with a deposition time of 6 minutes (thickness 200 nm) at the first temperature and a deposition time of 54 minutes (thickness 1800 nm) at the second temperature. In samples 15 and 16, the KNN film was deposited at a predetermined temperature without changing the temperature conditions. The temperature for depositing the KNN films in samples 15 and 16 is as shown in the "Second Temperature" column of Table 2 below, with a deposition time of 60 minutes (thickness 2000 nm). The conditions for depositing the KNN film, other than the deposition temperature and time, and the deposition conditions for each film (each layer) other than the KNN film, were the same as those in Experiment 1 described above. Samples 1 to 16 were prepared under the same conditions as described above, except for the deposition temperature (first temperature, second temperature) of the KNN film.

[0120] <Rating> For samples 1 to 16, the median coercive field, relative permittivity of the KNN film, film stress of the KNN film, and AC stress resistance were evaluated for each sample. Furthermore, the necessity of polarization treatment was evaluated using simple piezoelectric elements fabricated from samples 3 and 9. Additionally, the temperature resistance of spontaneous polarization in the KNN film was evaluated using simple piezoelectric elements fabricated from samples 1, 2, and 8. Finally, the heat resistance performance of the piezoelectric elements was evaluated using simple piezoelectric elements fabricated from samples 3 and 9.

[0121] (Evaluation of the median value of the coercive field) Using samples 1 to 16, simple piezoelectric elements were fabricated as shown in Figure 2, using the same method as described in the evaluation of the median coercive field in Experiment 1 above. Then, PE hysteresis curves were fabricated for each of the simple piezoelectric elements fabricated from samples 1 to 16. The PE hysteresis curves were fabricated using the same conditions, methods, and apparatus as described in the evaluation of the median coercive field in Experiment 1 above. The PE hysteresis curves for sample 3 and sample 9 are shown in Figures 5 and 6, respectively. Furthermore, the coercive field E was calculated from each PE hysteresis curve. C + and coercive field E C - The values ​​were obtained, and the median coercive field was calculated. The results of calculating the median coercive field for samples 1 to 16 are shown in Table 2 below. Note that "median" in Table 2 refers to the median coercive field.

[0122] (Evaluation regarding relative permittivity) Using samples 1 to 16, simple piezoelectric elements as shown in Figure 2 were fabricated using the same method as described in the evaluation of the median coercive field in Experiment 1 above. Then, using each simple piezoelectric element fabricated from samples 1 to 16, the lower electrode film and upper electrode film were connected to an LCR meter, and the capacitance was measured under conditions of ±1V and 1kHz. Measured capacitance, upper electrode film area (0.625mm²) 2 The relative permittivity of the KNN film in each sample was calculated using the values ​​of ( ), and the thickness of the KNN film (2 μm). The relative permittivity of samples 1 to 16 is shown in Table 2 below.

[0123] (Evaluation of membrane stress) For samples 1 to 16, the film stress of the KNN film was evaluated using the same method as described in the evaluation of film stress in Experiment 1 above. In samples 1 to 16, a lower adhesion layer and a lower electrode film were also fabricated, but as with samples A to G, the thickness of the lower adhesion layer and the lower electrode film was sufficiently small compared to the thickness of the KNN film. Therefore, the influence of the lower adhesion layer and the lower electrode film was ignored when calculating the film stress of the KNN film. The calculation results of the film stress of the KNN films for samples 1 to 16 are shown in Table 2 below. "Compression" and "Tension" in Table 2 have the same meaning as "Compression" and "Tension" in Table 1.

[0124] (Assessment of AC stress tolerance) AC stress resistance was evaluated by measuring the AC stress lifetime. The AC stress lifetime was evaluated as follows: First, small strips measuring 20 mm in length and 2.5 mm in width were cut from each of the samples 1 to 16. Then, as shown in Figure 7(a), one end of each small piece obtained from samples 1 to 16 was fixed in the longitudinal direction with a clamp, and a voltage application means (not shown) was connected between the lower electrode film and the upper electrode film to create a simple unimorph cantilever. Then, using the voltage application means, a negative voltage was continuously applied to the KNN film via the upper electrode film so that a unipolar AC electric field of 300 kV / cm was generated between the lower electrode film and the upper electrode film (i.e., on the KNN film). Specifically, with the lower electrode film grounded, a unipolar sinusoidal AC voltage oscillating in the range of 0 V to -60 V was continuously applied to the KNN film via the upper electrode film at a frequency of 300 Hz, and the KNN film (thickness 2 μm) of each small piece was continuously deformed. The deformation of the KNN film causes the entire cantilever to flex and extend (vibrate), and the tip of the cantilever continuously reciprocates in the vertical direction. The displacement Δ (piezoelectric displacement) of the tip of the cantilever at this time was measured by irradiating the tip of the cantilever with laser light L from a laser Doppler displacement meter, as shown in Figure 7(b). In this evaluation, the displacement Δ was measured every 1 million applied cycles. The number of applied cycles at which the displacement Δ fell to 80% or less of the initial value was defined as the AC stress lifetime. If the displacement Δ remained above 80% of the initial value after 50 million applied cycles, the measurement was stopped, and the AC stress lifetime measurement result was set to over 50 million cycles (>50 million cycles). The measurement results are shown in Table 2 below.

[0125] Note that in Figures 7(a) and 7(b), for the sake of clarity, the lower and upper adhesion layers are omitted from the illustration, and the laminate of the first KNN film and the second KNN film is shown as a single KNN film.

[0126] [Table 2]

[0127] In samples 1 to 6, the median coercive field is positive, the relative permittivity is 490 or less, and the film stress is 150 MPa or less. In other words, from samples 1 to 6, it can be seen that when forming a KNN film, by first forming the first KNN film at a first temperature where the (001) orientation is 95% or more and the film stress is 100 MPa or less, and then forming the second KNN film on the first KNN film at a second temperature where the second KNN film becomes a spontaneously polarized film, a KNN film possessing all three characteristics can be obtained: a median coercive field that is positive (characteristic 1 above), a relative permittivity of 490 or less (characteristic 2 above), and a film stress of 150 MPa or less (characteristic 3 above).

[0128] In sample 7, where the second temperature was 300°C, it was not possible to calculate the (001) orientation ratio or measure the median coercive field. This is thought to be because the crystal structure of the second KNN film did not become a perovskite structure. In samples 8-10, the median coercive field was 0 in all cases. This is thought to be because the second temperature in samples 8-10 was above 500°C (600°C, 650°C). From this, it can be confirmed that if the second temperature is not the temperature at which the second KNN film becomes a spontaneously polarized film, a spontaneously polarized KNN film, i.e., a KNN film possessing the above-mentioned characteristic 1, cannot be obtained. In samples 11 and 12, the relative permittivity was above 490 in both cases, and the film stress was above 150 MPa. This is thought to be because the first temperature in samples 11 and 12 was above 600°C (650°C). Also, in samples 13 and 14, the film stress was above 150 MPa in both cases. This is likely because, in samples 13 and 14, the first temperature was less than 550°C (500°C). From samples 11 to 14, it can be confirmed that if the first temperature is not the temperature at which the (001) orientation ratio of the first KNN film becomes 95% or higher and the film stress becomes 100 MPa or less, a KNN film with a relative permittivity of 490 or less and a film stress of 150 MPa or less, i.e., a KNN film possessing the above-mentioned characteristics 2 and 3, cannot be obtained.

[0129] Furthermore, in samples 1-6 and 8-10, the number of applied cycles until the displacement Δ fell to 80% or less of the initial value exceeded 50 million, indicating excellent AC stress resistance. This is thought to be due to the presence of a first KNN film with a high (001) orientation and low film stress (for example, a first KNN film with a (001) orientation of 95% or more and a film stress of 100 MPa or less) interposed between the lower electrode film and the second KNN film.

[0130] In particular, in samples 1 to 6, the median coercive field is a positive value, the relative permittivity is 490 or less, the film stress is 150 MPa or less, and the number of applied cycles exceeds 10 million (50 million or more). Thus, it can be confirmed that samples 1 to 6 possess the additional characteristic of excellent AC stress resistance (characteristic 4 above) in addition to the characteristics 1 to 3 above. From samples 1 to 6, it can be confirmed that when forming a KNN film, a KNN film possessing all of the above characteristics 1 to 4 can be obtained by first forming the first KNN film at a first temperature where the (001) orientation ratio is 95% or more and the film stress is 100 MPa or less, and then forming the second KNN film on the first KNN film at a predetermined second temperature higher than the first temperature.

[0131] In contrast, in sample 7, it was not possible to apply a large enough voltage to generate a unipolar AC electric field of 300 kV / cm to the KNN film, and therefore the number of application cycles could not be measured. This is thought to be because the crystal structure of the second KNN film did not become a perovskite structure, resulting in low voltage resistance of the KNN film. Furthermore, in samples 11 to 16, the number of application cycles until the displacement Δ fell below 80% of the initial value was less than 10 million, indicating low AC stress resistance. This is thought to be because, in samples 11 to 14, the first KNN film was not fabricated at a temperature at which the (001) orientation ratio was 95% or higher and the film stress was 100 MPa or lower; in other words, the (001) orientation ratio of the first KNN film was low and the film stress was high. Furthermore, in samples 15 and 16, the KNN film is not constructed as a laminate of a first KNN film and a second KNN film. Specifically, this is thought to be because there is no KNN film with a high (001) orientation and low film stress (for example, a KNN film with a (001) orientation of 95% or more and a film stress of 100 MPa or less) interposed between the lower electrode film and the KNN film.

[0132] In addition, when forming the KNN film, the film formation time at the first temperature was set to 6 minutes for samples 1 to 14, but this is not limited to this. The inventors have confirmed that if the film formation time at the first temperature is in the range of 1 minute to 12 minutes, the same results as described above can be obtained. In forming the KNN film, it has been confirmed that the optimal value for the film formation time at the first temperature, i.e., the thickness of the KNN film formed at the first temperature, may have a certain range.

[0133] (Regarding the evaluation of membrane stress) In experiments 1 and 2 described above, the film stress of the KNN film was calculated from the amount of warpage of the substrate (Si substrate), i.e., the radius of curvature of the substrate's warpage, but this is not the only method. The film stress of the KNN film can also be determined in the state of a piezoelectric element (piezoelectric device module) in which a MEMS structure has been fabricated by processing a piezoelectric laminate, by comparing the MEMS simulation with the actual shape of the object.

[0134] (Evaluation regarding the necessity of polarization treatment) Using simple piezoelectric elements fabricated from piezoelectric laminates of Sample 3, where the median coercive field is a positive value, and Sample 9, where the median coercive field is zero (0), we confirmed whether the KNN films in Samples 3 and 9 were spontaneously polarizing films, that is, we evaluated whether polarization treatment was necessary.

[0135] In piezoelectric films such as KNN films, the polarization directions are aligned in a specific direction, causing piezoelectric deformation when an electric field is applied in that polarization direction. Therefore, by applying a low voltage (electric field) to an unpolarized KNN film and checking whether the KNN film deforms, it is possible to determine whether the KNN film is a spontaneously polarized film, i.e., whether polarization treatment is necessary.

[0136] The necessity of polarization treatment was confirmed by performing the following measurements (a) to (e) in order. The graphs obtained from measurements (a) to (e) are shown in Figures 8(a) to (e) and Figures 9(a) to (e). Figures 8(a) to (e) are graphs of Sample 3, and Figures 9(a) to (e) are graphs of Sample 9, respectively.

[0137] <Measurement (a)> First, using the simple piezoelectric elements fabricated from samples 3 and 9, a sine wave voltage of -2V to +2V (a sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1kHz, with the lower electrode film grounded. The displacement of the KNN film (surface of the upper electrode film) was measured (measurement (a)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The graphs obtained from measurement (a) are shown in Figures 8(a) and 9(a), respectively.

[0138] <Measurement (b)> After measurement (a) was completed, with the lower electrode film grounded, a sine wave voltage of 0V to -30V (a sine wave electric field of 0kV / cm to -300kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1kHz, and the displacement of the KNN film (surface of the upper electrode film) was measured (measurement (b)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The application of a voltage of -30V in measurement (b) corresponds to the performance of a process to align the polarization in the upward direction (hereinafter also referred to as "upward polarization process"). The graphs obtained in measurement (b) are shown in Figure 8(b) and Figure 9(b), respectively.

[0139] <Measurement (c)> After measurement (b) was completed, with the lower electrode film grounded again, a sine wave voltage of -2V to +2V (a sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1kHz, and the displacement of the KNN film (surface of the upper electrode film) was measured (measurement (c)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The graphs obtained in measurement (c) are shown in Figure 8(c) and Figure 9(c), respectively.

[0140] <Measurement (d)> After measurement (c) was completed, with the lower electrode film grounded, a sine wave voltage of 0V to +30V (a sine wave electric field of 0kV / cm to +300kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1kHz, and the displacement of the KNN film (surface of the upper electrode film) was measured (measurement (d)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The application of a voltage of +30V in measurement (d) corresponds to the performance of a process to align the polarization in the downward direction (hereinafter also referred to as "downward polarization process"). The graphs obtained in measurement (d) are shown in Figure 8(d) and Figure 9(d), respectively.

[0141] <Measurement (e)> After measurement (d) was completed, with the lower electrode film grounded again, a sine wave voltage of -2V to +2V (a sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1kHz, and the displacement of the KNN film (surface of the upper electrode film) was measured (measurement (e)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The graphs obtained in measurement (e) are shown in Figure 8(e) and Figure 9(e), respectively.

[0142] In the simplified piezoelectric element of Sample 3, a clear piezoelectric displacement can be observed in the graph shown in Figure 8(a). It can also be confirmed that the piezoelectric displacement in the graph shown in Figure 8(c) is the same as the piezoelectric displacement in the graph shown in Figure 8(a). From these, it can be seen that the KNN film in Sample 3 has its polarization direction aligned upward even in its initial state without polarization treatment. In other words, it can be seen that the KNN film in Sample 3 is a spontaneously polarized film. Furthermore, it can be seen that the piezoelectric displacement in the graph shown in Figure 8(e) is the same as the piezoelectric displacement in the graphs shown in Figures 8(a) and 8(c). From this, it can be seen that the initial polarization state (upward polarization) is maintained even after performing a treatment corresponding to a downward polarization treatment (measurement (d)), which is the opposite direction to the treatment corresponding to an upward polarization treatment (measurement (b)). From these, it can be seen that the spontaneous polarization generated in the KNN film of Sample 3 is maintained even after applying a large voltage (regardless of whether it is in the forward or reverse direction). In other words, it can be seen that polarization treatment is unnecessary in Sample 3.

[0143] On the other hand, in the simple piezoelectric element of sample 9, no clear piezoelectric displacement was observed in the graph shown in Figure 9(a), but piezoelectric displacement was observed in the graph shown in Figure 9(c). From this, it can be seen that in sample 9, the polarization direction of the KNN film was aligned upward (forward) by performing the polarization treatment (measurement (b)) in the upward direction. Furthermore, in Figure 9(e), piezoelectric displacement was observed in the opposite direction to the piezoelectric displacement in Figure 9(c). From this, it can be seen that the polarization direction of the KNN film was aligned downward by performing the polarization treatment (measurement (d)) in the opposite direction to the polarization treatment (measurement (b)). From these findings, it can be seen that the KNN film in sample 9 does not exhibit spontaneous polarization, and that this KNN film has the property that after a large voltage is applied (regardless of whether it is in the forward or reverse direction), the polarization direction aligns with the direction of the applied voltage. The properties of the KNN film in Sample 9 are typical of KNN films (piezoelectric films) that require polarization treatment. In other words, it can be seen that polarization treatment is necessary for Sample 9.

[0144] (Evaluation of temperature tolerance of spontaneous polarization) We evaluated the temperature resistance of spontaneous polarization generated in the KNN film using simple piezoelectric elements fabricated from the piezoelectric laminates of Samples 1 and 2.

[0145] First, using a simple piezoelectric element fabricated from Sample 1, with the lower electrode film grounded, a sine wave voltage of -2V to +2V (a sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1kHz. The displacement of the KNN film (surface of the upper electrode film) was measured, and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in Figure 10(a). Subsequently, the simple piezoelectric element was placed in an air atmosphere at 400°C for 2 hours. After that, again with the lower electrode film grounded, a sine wave voltage of -2V to +2V (a sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1kHz. The displacement of the KNN film (surface of the upper electrode film) was measured, and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in Figure 10(b).

[0146] Furthermore, using the simplified piezoelectric element fabricated from Sample 2, with the lower electrode film grounded, a sine wave voltage of -2V to +2V (a sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1kHz, and the displacement of the KNN film (surface of the upper electrode film) was measured. A graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in Figure 11(a). Subsequently, the simplified piezoelectric element was placed in an air atmosphere at 500°C for 2 hours. After that, again with the lower electrode film grounded, a sine wave voltage of -2V to +2V (a sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1kHz, and the displacement of the KNN film (surface of the upper electrode film) was measured. A graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in Figure 11(b).

[0147] Figures 10(a) and 10(b) show that the piezoelectric displacement of the KNN film remains almost unchanged before and after exposure to a 400°C atmosphere. Furthermore, Figures 11(a) and 11(b) show that the piezoelectric displacement of the KNN film remains almost unchanged before and after exposure to a 500°C atmosphere. These results indicate that the polarization characteristics of the KNN film, a spontaneously polarized film fabricated by the method of this disclosure, are maintained even after the KNN film is subjected to a thermal history of 400°C and even 500°C.

[0148] Furthermore, the KNN film of sample 8 was subjected to polarization treatment, and the temperature resistance of the polarization generated in the KNN film of sample 8 was evaluated. Specifically, a simple piezoelectric element was prepared from sample 8, and polarization treatment in the downward direction (i.e., measurement (b) described above) was performed. Then, using the same method as for samples 1 and 2, the displacement of the KNN film was observed before and after exposure to a 400°C or 500°C atmosphere. As a result, it was confirmed that in sample 8, the piezoelectric displacement of the KNN film changed before and after exposure to a 400°C or 500°C atmosphere. Specifically, in sample 8, a clear piezoelectric displacement was observed before exposure to a 400°C or 500°C atmosphere, but no clear piezoelectric displacement was observed after exposure to a 400°C or 500°C atmosphere. In other words, it was confirmed that no polarization occurred in the KNN film of sample 8 after exposure to a 400°C or 500°C atmosphere.

[0149] (Evaluation of the heat resistance performance of piezoelectric elements) The thermal resistance performance of piezoelectric elements (membrane-type MEMS devices) fabricated from the piezoelectric laminates of Samples 3 and 9 was evaluated.

[0150] First, piezoelectric element chips were fabricated as follows. Piezoelectric laminates of samples 3 and 9 were prepared, and an insulating film was provided from the upper electrode film to the lower electrode film so as to cover a portion of the side surface of the KNN film of each sample. In this experiment, a laminate of aluminum oxide (Al2O3) with a thickness of 5 nm and silicon oxide (SiO2) with a thickness of 500 nm provided on the Al2O3 layer was provided as the insulating film. Then, a pattern was formed on the insulating film by dry etching using CF4 gas. Subsequently, a laminate of a Ti layer with a thickness of 10 nm and an Au layer with a thickness of 300 nm provided on the Ti layer was provided as the metal wiring layer. Then, a pattern was formed on the metal wiring layer by wet etching to form metal wiring of a predetermined pattern. In addition, a portion of the Si substrate was removed from the back side of the Si substrate by deep-RIE etching to form a membrane structure. Finally, the piezoelectric laminates (each sample) were divided into chips to fabricate multiple piezoelectric element chips as shown in Figure 3.

[0151] Next, polarization treatment was performed on the piezoelectric element chip fabricated using the piezoelectric laminate of Sample 9, which did not exhibit spontaneous polarization, by applying a DC voltage of -30V to the KNN film through the upper electrode film via probing. Polarization treatment was not performed on the piezoelectric element chip fabricated using the piezoelectric laminate of Sample 3, which exhibited spontaneous polarization.

[0152] Then, the obtained piezoelectric element chips were mounted in a package (bonding and wire bonding). To evaluate the heat resistance performance of the fabricated piezoelectric element chips, heat treatment temperatures (hereinafter also referred to as "PKG temperature") during package mounting were set to 200°C and 300°C.

[0153] This piezoelectric element (membrane-type MEMS device) deforms in the membrane structure in response to the sound pressure of ultrasound, generating a voltage from the KNN film. In other words, this piezoelectric element functions as an ultrasonic sensor. Ultrasound was applied to each fabricated piezoelectric element chip to evaluate its sensitivity to ultrasound (i.e., sensor sensitivity, hereinafter also referred to as "ultrasonic sensitivity"). The evaluation results are shown in Table 3 below. In the "Ultrasonic Sensitivity" column of Table 3, "Pass" means that the piezoelectric element operated normally after package mounting, and "Fail" means that the piezoelectric element did not operate normally after package mounting.

[0154] [Table 3]

[0155] The piezoelectric element fabricated using the piezoelectric laminate of Sample 3 operated normally regardless of the package temperature.

[0156] On the other hand, the piezoelectric element fabricated using the piezoelectric laminate of Sample 9 and subjected to polarization treatment functioned normally at a package temperature of 200°C, but did not function normally at a package temperature of 300°C. This indicates that the ultrasonic sensitivity deteriorates in piezoelectric elements subjected to a thermal history of 300°C after polarization treatment. This is presumed to be because the polarization direction of the KNN film, which was aligned by the polarization treatment, became disordered when exposed to high temperatures. From these findings, it can be seen that piezoelectric elements fabricated using spontaneously polarized KNN films have higher heat resistance than piezoelectric elements that have undergone polarization treatment. This demonstrates that piezoelectric elements have high heat resistance and high reliability.

[0157] <Preferred aspects of this disclosure> The following are preferred embodiments of this disclosure.

[0158] (Note 1) According to one aspect of this disclosure, circuit board and A lower electrode film formed on the substrate, The lower electrode film comprises a piezoelectric film formed on the lower electrode film, composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field, obtained by applying an electric field to the piezoelectric film under predetermined conditions, the coercive electric field E on the positive electric field side C + and the negative field side's coercive field E C - The median value of the coercive field between is a positive value. The dielectric constant of the piezoelectric film is 490 or less. The film stress of the piezoelectric film is 150 MPa or less. A piezoelectric laminate is provided.

[0159] (Note 2) A piezoelectric laminate as described in Appendix 1, preferably, In the hysteresis curve, the coercive field E when the thickness of the piezoelectric film is 2 μm. C + and the aforementioned coercive field E C - The median value of the coercive field between the two points is 10 kV / cm or more.

[0160] (Note 3) A piezoelectric laminate as described in Appendix 1 or 2, preferably, When a negative voltage is continuously applied to the upper electrode film such that a unipolar alternating electric field of 300 kV / cm is generated between the lower electrode film and the upper electrode film provided on the piezoelectric film, the number of voltage application cycles until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of the initial value exceeds 10 million.

[0161] (Note 4) A piezoelectric laminate according to any one of the appendices 1 to 3, preferably, The piezoelectric film contains, as a dopant, at least one element selected from copper and manganese at a concentration of 0.1 at% to 2.0 at%.

[0162] (Note 5) A piezoelectric laminate according to any one of the appendices 1 to 4, preferably, A layer containing zinc and oxygen is provided between the substrate and the piezoelectric film.

[0163] (Note 6) According to other aspects of this disclosure, A process of forming a lower electrode film on a substrate, The process includes a step of forming a piezoelectric film on the lower electrode film, which is composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen. In the process of forming the piezoelectric film, first, a first piezoelectric film, which is a part of the piezoelectric film, is formed at a first temperature at which the (001) orientation ratio becomes 95% or more and the film stress becomes 100 MPa or less, and then, a second piezoelectric film, which is the other part of the piezoelectric film, is formed on the first piezoelectric film at a second temperature at which the second piezoelectric film becomes a spontaneously polarized film. A method for manufacturing a piezoelectric laminate is provided.

[0164] (Note 7) The method described in Appendix 6, preferably, The thickness of the first piezoelectric film is 20% or less of the total thickness of the piezoelectric film.

[0165] (Note 8) The method described in Appendix 6 or 7, preferably, The first temperature is the temperature at which, when the first piezoelectric film with a thickness of 2 μm is fabricated, the (001) orientation ratio of the first piezoelectric film becomes 95% or more.

[0166] (Note 9) A method according to any one of the appendices 6 to 8, preferably, The first temperature is the temperature at which, when the first piezoelectric film with a thickness of 2 μm is fabricated, the film stress of the first piezoelectric film becomes 100 MPa or less.

[0167] (Note 10) A method according to any one of the appendices 6 to 9, preferably, The process further includes a step of providing a layer containing zinc and oxygen on the substrate before performing the step of forming the piezoelectric film, In the step of forming the piezoelectric film, the piezoelectric film is formed on the layer containing zinc and oxygen.

[0168] (Note 11) According to yet another aspect of this disclosure, circuit board and A lower electrode film formed on the substrate, A piezoelectric film is formed on the lower electrode film and is composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen. The system comprises an upper electrode film formed on the piezoelectric film, In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field, obtained by applying an electric field to the piezoelectric film under predetermined conditions, the coercive electric field E on the positive electric field side C + and the negative field side's coercive field E C - The median value of the coercive field between is a positive value. The dielectric constant of the piezoelectric film is 490 or less. The film stress of the piezoelectric film is 150 MPa or less. A piezoelectric element or piezoelectric device module is provided.

[0169] (Note 12) According to yet another aspect of this disclosure, A piezoelectric element or piezoelectric device module that utilizes the polarization characteristics of a piezoelectric film, In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field, obtained by applying an electric field under predetermined conditions, the coercive electric field E on the positive electric field side C + and the negative field side's coercive field E C - A piezoelectric film is installed in which the median value of the coercive field between it and the object is a positive value. The sensor sensitivity does not deteriorate even when subjected to a heat history of 300°C (the sensor sensitivity is maintained). A piezoelectric element or piezoelectric device module is provided.

[0170] (Appendix 13) According to still another aspect of the present disclosure, a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, In a hysteresis curve showing the correlation between the polarization amount and the applied electric field, obtained by applying an electric field to the piezoelectric film under predetermined conditions, the coercive electric field E on the positive electric field side C + and the coercive electric field E on the negative electric field side C - the median value of the coercive electric fields between them is a positive value, the relative permittivity is 490 or less, and the film stress is 150 MPa or less, the piezoelectric film is provided.

[0171] (Appendix 14) According to still another aspect of the present disclosure, In a hysteresis curve showing the correlation between the polarization amount and the applied electric field, obtained by applying an electric field under predetermined conditions, the coercive electric field E on the positive electric field side C + and the coercive electric field E on the negative electric field side C - the median value of the coercive electric fields between them is a positive value, and the polarization characteristics are maintained even when a thermal history of 400°C or higher is applied, the piezoelectric film is provided.

[0172] (Appendix 15) The piezoelectric film, piezoelectric element, or piezoelectric device module according to any one of Appendices 11 to 14, wherein preferably, When a negative voltage is continuously applied to the upper electrode film (the upper electrode film provided on the piezoelectric film) such that a unipolar alternating electric field of 300 kV / cm is generated between the lower electrode film and the upper electrode film (across the piezoelectric film), the number of voltage application cycles until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of the initial value exceeds 10 million. [Description of Symbols]

[0173] 1 Substrate 2 Lower electrode film 3 Piezoelectric film 4 Upper electrode film 6. Lower adhesion layer 10 Piezoelectric laminate 20 Piezoelectric elements 30 Piezoelectric device modules

Claims

1. circuit board and A lower electrode film formed on the substrate, The lower electrode film comprises a piezoelectric film formed on the lower electrode film, composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field, obtained by applying an electric field to the piezoelectric film under predetermined conditions, the coercive electric field E on the positive electric field side C + and the cohesive field E on the negative field side C - The median value of the coercive field between is a positive value. The dielectric constant of the piezoelectric film is 490 or less. A piezoelectric laminate in which the film stress of the piezoelectric film is 150 MPa or less.

2. The piezoelectric laminate according to claim 1, wherein when a negative AC voltage is continuously applied to the upper electrode film such that a unipolar AC electric field of 300 kV / cm is generated between the lower electrode film and the upper electrode film provided on the piezoelectric film, the number of voltage application cycles until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of the initial value is more than 10 million.

3. The piezoelectric laminate according to claim 1 or 2, wherein the piezoelectric film contains, as a dopant, at least one element selected from copper and manganese at a concentration of 0.1 at% to 2.0 at%.

4. A process of forming a lower electrode film on a substrate, The process includes a step of forming a piezoelectric film on the lower electrode film, which is composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen. A method for manufacturing a piezoelectric laminate, comprising the steps of first forming a piezoelectric film, in which a first piezoelectric film, which is a part of the piezoelectric film, is formed at a first temperature in which the orientation ratio becomes 95% or more and the film stress becomes 100 MPa or less, and then a second piezoelectric film, which is the other part of the piezoelectric film, is formed on the first piezoelectric film at a second temperature in which the second piezoelectric film becomes a spontaneously polarized film.

5. circuit board and A lower electrode film formed on the substrate, A piezoelectric film formed on the lower electrode film, comprising an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, The system comprises an upper electrode film formed on the piezoelectric film, In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field, obtained by applying an electric field to the piezoelectric film under predetermined conditions, the coercive electric field E on the positive electric field side C + and the cohesive field E on the negative field side C - The median value of the coercive field between is a positive value. The dielectric constant of the piezoelectric film is 490 or less. A piezoelectric element in which the film stress of the piezoelectric film is 150 MPa or less.

6. The piezoelectric element according to claim 5, wherein when a negative AC voltage is continuously applied to the upper electrode film such that a unipolar electric field of 300 kV / cm is generated between the lower electrode film and the upper electrode film, the number of voltage application cycles until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of the initial value is more than 10 million.

Citation Information

Patent Citations

  • Piezoelectric thin film element and manufacturing method of piezoelectric thin film element, and piezoelectric thin film device

    JP2011029591A

  • Piezoelectric thin-film device, piezoelectric sensor, and vibration power generator

    JP2014207429A

  • Piezoelectric elements, piezoelectric actuators, hard disk drives, inkjet printers, and piezoelectric sensors

    JP2015529963A

  • Piezoelectric thin film-attached laminate board, piezoelectric thin-film device and manufacturing method thereof

    JP2017076730A

  • Piezoelectric laminate, piezoelectric element, and manufacturing method of piezoelectric laminate

    JP2021012909A