Ion-conducting polymer and separation membrane containing the same
The novel ion-conducting polymer with quaternary ammonium and ether bonds addresses the limitations of existing ion exchange membranes by enhancing ionic conductivity and mechanical strength, enabling effective use in green technologies.
Patent Information
- Application Number
- JP2025009417
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-07-01
- Filing Date
- 2025-01-22
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-01-22
AI Technical Summary
Existing ion exchange membranes lack sufficient ionic conductivity, mechanical strength, and chemical stability, limiting their effectiveness in applications requiring high efficiency and durability.
A novel ion-conducting polymer with repeating units represented by Chemical Formula 1, synthesized through mild acidic conditions, incorporating quaternary ammonium groups and ether bonds, enhances ionic conductivity and mechanical strength.
The ion-conducting polymer exhibits ionic conductivity of 40 mS/cm to 80 mS/cm and improves the durability of separation membranes, suitable for green technologies like electric vehicles and solar power generation.
Smart Images

Figure 0007949072000001 
Figure 0007949072000002 
Figure 0007949072000003
Abstract
Description
Technical Field
[0001] The present disclosure relates to an ion-conductive polymer and a separation membrane comprising the same.
Background Art
[0002] A separation membrane is generally a barrier present between two different substances, which can selectively allow specific substances to pass through. Separation membranes are classified into various types according to their properties, materials, forms and the like. In the case of an ion exchange membrane, it corresponds to a non-porous membrane, a symmetric membrane, a single membrane, a homogeneous membrane, a hydrophilic membrane, a charged membrane, a liquid separation membrane, and the like.
[0003] An ion exchange membrane is a membrane having an ion exchange function for specific ions, and is a type of high-efficiency separation membrane. When an ion exchange membrane is introduced into an electrolyte solution and an electric current is passed therethrough, functional groups having positive or negative charges on the pore walls of the membrane draw only specific ions having opposite charges into the pores of the membrane to achieve electrical neutrality. The specific ions bound to the functional groups of the membrane pass through the membrane by continuously repeating binding and dissociation with the functional groups.
[0004] Ion exchange membranes are classified into cation exchange membranes (CEM), anion exchange membranes (AEM), and bipolar exchange membranes (BEM) according to their properties. A cation exchange membrane is a membrane that allows only cations to pass through with anions as fixed charges. An anion exchange membrane is a membrane that allows only anions to pass through with cations as fixed charges. A bipolar exchange membrane is in a form in which a cation exchange membrane and an anion exchange membrane are bonded to both side surfaces, and selectively permeates both cations and anions.
[0005] Ion exchange membranes can be used in various fields such as water treatment, chemistry, and energy. Because ion exchange membranes need to selectively allow different specific charges to pass through, they require low electrical resistance and high ionic conductivity. Furthermore, for long-term continuous use, ion exchange membranes must possess excellent mechanical strength and chemical stability. [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] Korean Published Patent Publication No. 2018-0100079 [Overview of the project] [Problems that the invention aims to solve]
[0007] One of the objectives of this disclosure is to provide an ion-conducting polymer having improved ion conductivity.
[0008] One of the objectives of this disclosure is to provide a separation membrane having improved ionic conductivity. [Means for solving the problem]
[0009] The ion-conducting polymer according to the exemplary embodiments of this disclosure has repeating units represented by the following chemical formula 1. [ka] In chemical formula 1, A + is a quaternary ammonium, B - is an anion, a is an integer from 1 to 3, R 1 R is an organic group with 1 to 10 carbon atoms. 2 H or an organic group with 1 to 10 carbon atoms, R 3 is an organic group having 1 to 20 carbon atoms that contains at least one alkylene group or arylene group, and Ar is a benzene ring.
[0010] In an exemplary embodiment, B -may be a monovalent or divalent anion.
[0011] In an exemplary embodiment, the B - may be a halide anion.
[0012] In an exemplary embodiment, the B - may be a bromide anion (Br - ).
[0013] In an exemplary embodiment, the R 1 may be a methyl group (-CH3).
[0014] In an exemplary embodiment, the R may be an organic group having 1 to 8 carbon atoms.
[0015] In an exemplary embodiment, the R
[0007] may be an organic group having 4 to 16 carbon atoms.
[0016] In an exemplary embodiment, the repeating unit represented by Chemical Formula 1 may include at least one of the repeating units represented by Chemical Formula 1-1 to Chemical Formula 1-5 below. [Chemical Formula] [Chemical Formula] [Chemical Formula] [Chemical Formula] [Chemical Formula]
[0017] In an exemplary embodiment, the OH - ionic conductivity of the ion-conductive polymer at 25°C may be 40 mS / cm to 80 mS / cm.
[0018] In the exemplary embodiments of the present disclosure, a monomer having a benzene ring substituted with at least one alkoxy group is prepared. The monomer is reacted with an aldehyde under mild acidic conditions to obtain a precursor polymer. A quaternary ammonium group is introduced into the precursor polymer to synthesize an ion-conducting polymer having repeating units represented by the following chemical formula 1. [ka]
[0019] In chemical formula 1, A + is a quaternary ammonium, B - is an anion, a is an integer from 1 to 3, R 1 R is an organic group with 1 to 10 carbon atoms. 2 H or an organic group with 1 to 10 carbon atoms, R 3 is an organic group having 1 to 20 carbon atoms that contains at least one alkylene group or arylene group, and Ar is a benzene ring.
[0020] The separation membrane according to the exemplary embodiment contains the aforementioned ion-conducting polymer.
[0021] An apparatus according to an exemplary embodiment includes a positive electrode, a negative electrode opposite to the positive electrode, and the separation membrane.
[0022] In exemplary embodiments, the apparatus may include a water electrolyzer, a CO2 electrolyzer, a fuel cell, an electrolytic battery, a vanadium flow battery, and the like. [Effects of the Invention]
[0023] The ion-conducting polymers according to the exemplary embodiments of this disclosure can exhibit excellent ionic conductivity.
[0024] The separation membrane according to the exemplary embodiments of this disclosure can exhibit excellent ionic conductivity by including the ion-conducting polymer.
[0025] The ion-conducting polymers and separation membranes of this disclosure can be widely applied to green technology fields such as electric vehicles, battery charging stations, and solar and wind power generation using batteries.
[0026] Furthermore, the ion-conducting polymers and separation membranes of this disclosure can be used in environmentally friendly electric vehicles, hybrid vehicles, and the like, with the aim of preventing climate change by suppressing air pollution and greenhouse gas emissions. [Modes for carrying out the invention]
[0027] Embodiments of the present disclosure provide an ion-conducting polymer having repeating units comprising a quaternary ammonium and at least one ether group.
[0028] The aforementioned ion-conducting polymer can have its stability and ion conductivity improved by containing a quaternary ammonium compound.
[0029] The ion-conducting polymer, by containing an ether group, can be synthesized under mild acidic conditions.
[0030] The ion-conducting polymer can improve its physicochemical durability by including a main chain composed of carbon-carbon bonds (CC bonds).
[0031] The following describes the present disclosure in detail. However, this is illustrative only, and the present disclosure is not limited to the specific embodiments described herein.
[0032] The ion-conducting polymer according to the exemplary embodiments of this disclosure has repeating units represented by the following chemical formula 1.
[0033] [ka]
[0034] In an exemplary embodiment, A + A may be a quaternary ammonium compound. In an exemplary embodiment, A + A may be a substituent containing at least one methyl group. For example, A + It may be a quaternary ammonium compound.
[0035] In this disclosure, ammonium may also include ammonium compounds in which two different substituents bonded to a nitrogen atom are linked together to form a ring structure. For example, A + This may include trimethylammonium, triethylammonium, tripropylammonium, tributylammonium, imidazolium, piperidinium, quinuclidinium, and others.
[0036] In an exemplary embodiment, B - B may be an anion. In an exemplary embodiment, B - This can be a monovalent or divalent anion. For example, B - If it is a divalent anion, then the two A located on different chains + is one B - They can bond together to form a cross-linked structure.
[0037] In an exemplary embodiment, B - This may be a halogen anion. For example, the above B - is a chloride anion (Cl - ), bromine anion (Br - ), iodine anion (I - ), hydroxide ion (OH - ), sulfate anion (SO4 2- ), carbonate anion (CO3 2- ), bicarbonate anion (HCO3)- ), carboxylate anion (RCO2 - ) is also acceptable.
[0038] In the exemplary embodiment, a may be an integer from 1 to 3. For example, a may be 1 or 3.
[0039] In an exemplary embodiment, the R 1 This may be an organic group having 1 to 10 carbon atoms.
[0040] In exemplary embodiments, the organic group may be a substituent containing only carbon and hydrogen, or it may be a substituent containing one or more atoms other than carbon and hydrogen. For example, the atoms other than carbon and hydrogen may be nitrogen (N), oxygen (O), phosphorus (P), sulfur (S), etc.
[0041] In an exemplary embodiment, the R 1 R may be an organic group having 1 to 6 carbon atoms. For example, the R 1 It may also be a methyl group (-CH3).
[0042] In exemplary embodiments, the ion-conducting polymer having the repeating unit represented by chemical formula 1 may include an ether bond in the benzene ring. The inclusion of an ether bond in the benzene ring places the benzene ring in an electron-rich state. This allows the synthesis of the ion-conducting polymer to be carried out under relatively mild acid conditions, rather than under superacid conditions such as triflic acid.
[0043] According to exemplary embodiments, the pKa of the mild acid may be -7 or higher.
[0044] For example, the mild acid may be methanesulfonic acid, trifluoroacetic acid, nitric acid, sulfuric acid, hydrochloric acid, etc.
[0045] In an exemplary embodiment, the R 2 This may be H or an organic group having 1 to 10 carbon atoms.
[0046] In exemplary embodiments, the organic group may be a hydrocarbon group or a hydrocarbon group containing one or more heteroatoms. The heteroatoms may be, for example, nitrogen (N), oxygen (O), phosphorus (P), or sulfur (S).
[0047] For example, the R 2 R may be an organic group having 1 to 8 carbon atoms. Alternatively, the above R 2 This may be an organic group having 1 to 6 carbon atoms.
[0048] In an exemplary embodiment, the R 2 This may be further substituted with an electron-withdrawing group (EWG). Examples of electron-withdrawing groups include nitro groups, trifluoromethyl groups, cyano groups, fluoro groups, and acyl groups. This makes the synthesis of ion-conducting polymers easier.
[0049] In an exemplary embodiment, the R 3 This may be an organic group having 1 to 20 carbon atoms that contains at least one alkylene group or an arylene group. For example, the R 3 R may be an organic group having 4 to 16 carbon atoms. Alternatively, the above R 3 R may be an organic group having 6 to 14 carbon atoms. Alternatively, the above R 3 This may be an organic group having 8 to 12 carbon atoms.
[0050] When a quaternary ammonium ion is directly linked to a benzene ring, the ammonium functional group undergoes a bimolecular nucleophilic substitution (S) reaction. N It can be decomposed by a 2-reaction or Hofmann elimination reaction. N When reaction 2 occurs, the ammonium functional group becomes OH - It can react with and decompose into an alcohol functional group and a tertiary amine. When the Hoffmann elimination reaction occurs, the β-hydrogen atom of the ammonium functional group becomes OH - The ammonium functional group may be attacked, forming a double bond, and decomposition of the ammonium functional group may occur. When the ammonium functional group decomposes, the mechanical strength and ionic conductivity of the ion-conducting polymer may decrease significantly.
[0051] In this disclosure, quaternary ammonium ions are R 3 Because it is linked to the benzene ring via OH, the electron-withdrawing inductive effect and resonance effect of the benzene ring are reduced, - This reduces the attack caused by [unspecified factor]. This prevents the decomposition of ammonium functional groups.
[0052] In an exemplary embodiment, the R 3 The mixture may contain both aromatic and aliphatic chains. This can further improve the mechanical strength of the ion-conducting polymer.
[0053] In exemplary embodiments, the Ar may be a benzene ring.
[0054] In exemplary embodiments, the repeating unit represented by chemical formula 1 may include at least one of the repeating units represented by the following chemical formulas 1-1 to 1-5.
[0055] [ka] [ka] [ka] [ka] [ka]
[0056] In an exemplary embodiment, the OH of the ion-conducting polymer at 25°C - The ionic conductivity may be 40 mS / cm to 80 mS / cm. For example, the OH of the ionic conductive polymer at 25°C - The ionic conductivity may be 43 mS / cm to 70 mS / cm, or 45 mS / cm to 65 mS / cm, or 46 mS / cm to 63 mS / cm, or 47 mS / cm to 60 mS / cm.
[0057] One embodiment of the present disclosure provides a method for producing an ion-conducting polymer.
[0058] First, prepare a monomer having a benzene ring substituted with at least one alkoxy group.
[0059] The alkoxy group is -(OR) of the chemical formula 1. 1 ) a This is also acceptable. Here, a may be an integer from 1 to 3.
[0060] A benzene ring has its terminals substituted with halogens. 3 It may also be combined with this.
[0061] Next, the monomer is reacted with an aldehyde under mild acidic conditions to obtain a precursor polymer.
[0062] When the monomer is reacted with an aldehyde under mild acidic conditions (primary polymerization), a precursor polymer containing the benzene ring in the main chain is obtained.
[0063] Primary polymerization can be carried out in the presence of a mild acid. The mild acids mentioned above can be used as the mild acid. For example, an acid with a pKa of -7 or higher can be used.
[0064] As mentioned above, when an ether bond (alkoxy group) is included in a benzene ring, the benzene ring is placed in an electron-rich state. This allows the synthesis of ionic conductive polymers to be carried out under relatively mild acid conditions, rather than under superacid conditions such as triflic acid.
[0065] The aforementioned aldehyde is R 2 -It contains CHO, and after primary polymerization, R 2 This will result in a structure in which it is linked to the main chain of the precursor polymer.
[0066] In some embodiments, R 2 It may be further substituted with an electron-withdrawing group. In this case, the reactivity of the aldehyde can be increased, making the formation of the precursor polymer easier.
[0067] Next, a quaternary ammonium group is introduced into the precursor polymer to synthesize an ion-conducting polymer having repeating units represented by the chemical formula 1.
[0068] Quaternary ammonium groups can be introduced into the side chains of benzene rings to exhibit ionic conductivity.
[0069] According to embodiments of this disclosure, a separation membrane containing the ion-conducting polymer is provided.
[0070] In an exemplary embodiment, the separation membrane can be manufactured by laminating ion-conducting polymer membranes having repeating units represented by the chemical formula 1.
[0071] According to embodiments of the present disclosure, an apparatus including the separation membrane is provided. The apparatus may include a positive electrode, a negative electrode opposite to the positive electrode, and the separation membrane. Exemplary embodiments of the apparatus may include a water electrolyzer, a CO2 electrolyzer, a fuel cell, an electrolytic cell, a vanadium flow cell, and the like.
[0072] Examples are presented below to aid in understanding the present invention. These examples are merely illustrative of the present invention and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the examples are possible within the scope of the present invention and the technical concept, and that such variations and modifications naturally fall within the scope of the appended claims.
[0073] Manufacturing Example 1: Manufacturing of Monomers (1) Manufacturing of monomer 1 (A-1) 50 mL of dichloromethane, 5 g of anisole (46 mmol), and 6.78 g of aluminum chloride (51 mmol) were added to a 100 mL two-necked round-bottom flask, and the mixture was stirred in an ice bath to prepare a mixed solution.
[0074] 6-bromohexanoyl chloride (10.4 g, 49 mmol) was added to the prepared mixed solution using a syringe pump over 2 hours, and then 85 mL of 1 M hydrochloric acid aqueous solution was added. After the reaction was complete, the aqueous solution layer was removed using a separatory funnel and washed with 1 M sodium hydroxide aqueous solution. After washing, the aqueous solution layer was removed, and the organic solvent layer was dried over anhydrous magnesium sulfate. The organic solvent was then removed using a vacuum concentrator to obtain a solid.
[0075] Triethylsilane (16.1 g, 139 mmol), trifluoroacetic acid (5.3 g, 46 mmol), and the aforementioned solid were placed in a 100 mL round-bottom flask. A reflux condenser was attached to the round-bottom flask, and the mixture was stirred at 85°C for 24 hours. After stirring, the mixture was cooled in an ice bath, and 53 mL of 1 M aqueous sodium hydroxide solution was added. After the reaction was complete, the aqueous solution layer was removed using a separatory funnel, the organic solvent layer was dried over anhydrous magnesium sulfate, and purified by column chromatography to produce 11.1 g of monomer 1(A-1) represented by the following chemical formula 2-1. [ka]
[0076] (2) Manufacturing of monomer 2 (A-2) A mixed solution was prepared by adding 30 mL of dichloromethane, 3 g of 1,3,5-trimethoxybenzene, and 2.85 g of aluminum chloride to a 100 mL two-necked round-bottom flask and stirring in an ice bath.
[0077] 6-bromohexanoyl chloride (4.57 g, 21 mmol) was added to the prepared mixed solution using a syringe pump over 2 hours, and then 45 mL of 1 M hydrochloric acid aqueous solution was added. After the reaction was complete, the aqueous solution layer was removed using a separatory funnel and washed with 1 M sodium hydroxide aqueous solution. After washing, the aqueous solution layer was removed, and the organic solvent layer was dried over anhydrous magnesium sulfate. The organic solvent was then removed using a vacuum concentrator to obtain a solid.
[0078] Triethylsilane (6.1 g, 52 mmol), trifluoroacetic acid (1.98 g, 17 mmol), and the aforementioned solid were placed in a 100 mL round-bottom flask. A reflux condenser was attached to the round-bottom flask, and the mixture was stirred at 85°C for 24 hours. After stirring, the mixture was cooled in an ice bath, and 53 mL of 1 M aqueous sodium hydroxide solution was added. After the reaction was complete, the aqueous solution layer was removed using a separatory funnel, the organic solvent layer was dried over anhydrous magnesium sulfate, and purified by column chromatography to produce 3.65 g of monomer 2(A-2) represented by the following chemical formula 2-2. [ka]
[0079] (3) Manufacturing of monomer 3 (A-3) 75 mL of dichloromethane, 5 g of 4-methoxybiphenyl, and 3.98 g of aluminum chloride were added to a 100 mL two-necked round-bottom flask, and the mixture was stirred in an ice bath to prepare a mixed solution.
[0080] 6-bromohexanoyl chloride (6.08 g, 28 mmol) was added to the prepared mixed solution using a syringe pump over 2 hours, and then 50 mL of 1 M hydrochloric acid aqueous solution was added. After the reaction was complete, the aqueous solution layer was removed using a separatory funnel and washed with 1 M sodium hydroxide aqueous solution. After washing, the aqueous solution layer was removed, and the organic solvent layer was dried with anhydrous magnesium sulfate. The organic solvent was then removed using a vacuum concentrator to obtain a solid.
[0081] Triethylsilane (12.6 g, 109 mmol), trifluoroacetic acid (6.2 g, 54 mmol), and the aforementioned solid were placed in a 100 mL round-bottom flask. A reflux condenser was attached to the round-bottom flask, and the mixture was stirred at 85°C for 24 hours. After stirring, the mixture was cooled in an ice bath, and 60 mL of 1 M sodium hydroxide aqueous solution was added. After the reaction was complete, the aqueous solution layer was removed using a separatory funnel, the organic solvent layer was dried over anhydrous magnesium sulfate, and purified by column chromatography to produce 6.20 g of monomer 3(A-3) represented by the following chemical formulas 2-3. [ka]
[0082] Manufacturing Example 2: Polymer Manufacturing (1) Production of polymer 1 (B-1) 14.8 mL of chloroform, 1.8 mL of methanesulfonic acid, 0.24 g of paraformaldehyde (equivalent to 8 mmol of formaldehyde), and the aforementioned A-1 (2 g, 7 mmol) were placed in a 25 mL round-bottom flask. A reflux condenser was attached to the round-bottom flask and refluxed at 85°C for 2 hours. After refluxing, the mixture was cooled to room temperature (25°C) and added to 200 mL of methanol to precipitate the solid. The precipitated solid was filtered, washed twice with 50 mL of methanol, and then dried in an oven to produce 1.9 g of polymer 1 (B-1) represented by the following chemical formula 3-1. [ka]
[0083] (2) Production of polymer 2 (B-2) 12.0 mL of chloroform, 1.5 mL of methanesulfonic acid, paraformaldehyde (0.20 g, equivalent to 7 mmol of formaldehyde), and the aforementioned A-2 (2 g, 6 mmol) were placed in a 25 mL round-bottom flask. A reflux condenser was attached to the round-bottom flask and refluxed at 85°C for 2 hours. After refluxing, the mixture was cooled to room temperature (25°C), and 200 mL of methanol was added to precipitate the solid. The precipitated solid was filtered, washed twice with 50 mL of methanol, and then dried in an oven to produce 1.6 g of polymer 2(B-2) represented by the following chemical formula 3-2. [ka]
[0084] (3) Production of polymer 3 (B-3) 14.8 mL of chloroform, 1.8 mL of methanesulfonic acid, 0.77 g of benzaldehyde, and 2 g of A-1 (7 mmol) were added to a 25 mL round-bottom flask. A reflux condenser was attached to the round-bottom flask and refluxed at 85°C for 2 hours. After refluxing, the flask was cooled to room temperature (25°C), and 200 mL of methanol was added to precipitate the solid. The precipitated solid was filtered, washed twice with 50 mL of methanol, and then dried in an oven to produce 2.3 g of polymer 3(B-3) represented by the following chemical formula 3-3. [ka]
[0085] (4) Production of polymer 4 (B-4) 14.8 mL of chloroform, 1.8 mL of methanesulfonic acid, 1.09 g of 4-nitrobenzaldehyde (7 mmol), and the aforementioned A-1 (2 g, 7 mmol) were placed in a 25 mL round-bottom flask. A reflux condenser was attached to the round-bottom flask and refluxed at 85°C for 2 hours. After refluxing, the mixture was cooled to room temperature (25°C), and 200 mL of methanol was added to precipitate the solid. The precipitated solid was filtered, washed twice with 50 mL of methanol, and then dried in an oven to produce 3.0 g of polymer 4 (B-4) represented by the following chemical formulas 3-4. [ka]
[0086] (5) Production of polymer 5 (B-5) 11.5 mL of chloroform, 1.44 mL of methanesulfonic acid, 0.61 g of paraformaldehyde (equivalent to 20 mmol of formaldehyde), and the aforementioned A-3 (2 g, 6 mmol) were placed in a 25 mL round-bottom flask. A reflux condenser was attached to the round-bottom flask and refluxed at 85°C for 2 hours. After refluxing, the mixture was cooled to room temperature (25°C), and 200 mL of methanol was added to precipitate the solid. The precipitated solid was filtered, washed twice with 50 mL of methanol, and then dried in an oven to produce 1.7 g of polymer 5 (B-5) represented by the following chemical formula 3-5.
[0087] [ka]
[0088] Manufacturing Example 3: Manufacturing of Separation Membranes Example 1 1.45 mL of N-methylpyrrolidone and 0.25 g of B-1 were added to a 20 mL glass vial and stirred at room temperature (25°C). After B-1 was completely dissolved, 0.17 g of N,N-dimethylcyclohexylamine was added and the mixture was stirred at 80°C for 24 hours. After stirring, the mixture was cooled to room temperature (25°C), the cooled solution was poured into a Petri dish, and the mixture was dried in an 80°C oven for 24 hours to produce a separation membrane (C-1) formed from a polymer having repeating units represented by chemical formula 1-1. For C-1 mentioned above 1 H-nuclear magnetic resonance spectroscopy ( 1 H-Nuclear Magnetic Resonance, 1 The results of the 1H-NMR (H-NMR) analysis are shown below. 1 H-NMR (DMSO-d6, ppm):7.3(br,2H),4.0(br,2H),3.8(br,3H),3.6-3.2(br,9H),2.6-2.5(br,2H),2.0-1.0(br,18H)
[0089] Example 2 2.12 mL of N-methylpyrrolidone and 0.25 g of B-2 were added to a 20 mL glass vial and stirred at room temperature (25°C). After B-2 was completely dissolved, 0.28 g of trimethylamine aqueous solution (28% by weight) was added and the mixture was stirred at 80°C for 24 hours. After stirring, the mixture was cooled to room temperature (25°C), the cooled solution was poured into a petri dish, and the mixture was dried in an oven at 80°C for 24 hours to produce a separation membrane (C-2) formed from a polymer having repeating units represented by chemical formula 1-2. For C-2 mentioned above 1 The results of the 1H nuclear magnetic resonance spectroscopy analysis are shown below. 1 H-NMR(DMSO-d6,ppm):3.9(br,2H),3.8(br,9H),3.3-3.2(br,11H),2.7-2.6(br,2H),2.0-1.0(br,8H)
[0090] Example 3 1.38 mL of N-methylpyrrolidone and 0.25 g of B-3 were added to a 20 mL glass vial and stirred at room temperature (25°C). After B-3 was completely dissolved, 0.10 g of 1-methylimidazole was added and the mixture was stirred at 80°C for 24 hours. After stirring, the mixture was cooled to room temperature (25°C), the cooled solution was poured into a petri dish, and the mixture was dried in an 80°C oven for 24 hours to produce a separation membrane (C-3) formed from a polymer having repeating units represented by chemical formula 1-3. For C-3 mentioned above 1 The results of the 1H nuclear magnetic resonance spectroscopy analysis are shown below. 1 H-NMR(DMSO-d6,ppm):8.92(br,1H),7.9-7.0(br,9H),5.48(br,1H),5.01(br,2H),3.9-3.7(br,6H),2.64(br,2H),2.1-1.2(br,8H)
[0091] Example 4 1.83 mL of N-methylpyrrolidone and 0.25 g of B-4 were placed in a 20 mL glass vial and stirred at room temperature (25°C). After B-4 was completely dissolved, 0.21 g of trimethylamine aqueous solution (28% by weight) was added and the mixture was stirred at 80°C for 24 hours. After stirring, the mixture was cooled to room temperature (25°C), the cooled solution was poured into a petri dish, and the mixture was dried in an 80°C oven for 24 hours to produce a separation membrane (C-4) formed from a polymer having repeating units represented by chemical formulas 1-4. For C-4 mentioned above 1 The results of the 1H nuclear magnetic resonance spectroscopy analysis are shown below. 1 H-NMR(DMSO-d6,ppm):8.16(br,2H),7.5-7.0(br,4H),5.50(br,1H),3.78(br,3H),3.5-3.0(br,11H),2.66(br,2H),1.8-1.2(br,8H)
[0092] Example 5 1.44 mL of N-methylpyrrolidone, 1.44 g of dimethyl sulfoxide, and 0.25 g of B-5 were added to a 20 mL glass vial and stirred at room temperature (25°C). After B-5 was completely dissolved, 0.1 g of N-methylpiperidine was added and the mixture was stirred at 80°C for 24 hours. After stirring, the mixture was cooled to room temperature (25°C), the cooled solution was poured into a petri dish, and the mixture was dried in an 80°C oven for 24 hours to produce a separation membrane (C-5) formed from a polymer having repeating units represented by chemical formulas 1-5. For C-5 mentioned above 1 The results of the 1H nuclear magnetic resonance spectroscopy analysis are shown below. 1 H-NMR(DMSO-d6,ppm):7.8-7.0(br,6H),4.0-3.8(br,5H),3.4-3.0(br,9H),2.63(br,2H),2.0-1.0(br,14H)
[0093] Comparative Example 1 We used Sustainion® X37-50 Grade RT product from Dioxide Materials.
[0094] Comparative Example 2 We used Sustainion® X37-50 Grade T product from Dioxide Materials.
[0095] Experimental example: Evaluation of the ionic conductivity of a separation membrane. The membrane samples from Examples 1 to 5 and Comparative Examples 1 to 2 were cut to a size of 1 cm x 3 cm and fixed between the Pt electrodes of a Conductivity Clamp (BT-110, Scribner).
[0096] The ionic conductivity (σ) of the anion exchange membrane was measured under the conditions of OH at room temperature (25°C) and tertiary distilled water. -The evaluation was performed in the following manner. Film resistance (R) was measured using a 4-point probe method with an impedance analyzer (VSP-3e, Biologics) in the frequency range of 0.1 kHz to 1 MHz. The thickness (T) of the film sample was measured using a micrometer.
[0097] The ionic conductivity (σ) was calculated using Equation 1 below. The results are shown in Table 1 below.
[0098]
number
[0099] In Equation 1, R is the film resistance (Ω) and A is the cross-sectional area (cm²) of the film sample. 2 ), L is the distance between electrodes (cm), W is the width of the membrane sample (cm), and T is the thickness of the membrane sample (cm).
[0100] [Table 1]
[0101] Table 1 shows the OH of Examples 1 to 5. - The ionic conductivity is as follows: OH - This confirms that it is superior to ionic conductivity.
Claims
1. An ionic conductive polymer having repeating units represented by the following chemical formula 1. 【Chemistry 1】 (In chemical formula 1, A + is a quaternary ammonium, B - is an anion, a is an integer from 1 to 3, R 1 R is an organic group having 1 to 10 carbon atoms. 2 H or an organic group having 1 to 10 carbon atoms, R 3 (where is an organic group having 1 to 20 carbon atoms containing at least one alkylene group or arylene group, and Ar is a benzene ring.)
2. B - The ion-conducting polymer according to claim 1, wherein is a monovalent or divalent anion.
3. B - The ion-conducting polymer according to claim 1, wherein is a halogen anion.
4. the aforementioned B - is a bromide anion (Br - ), the ion-conductive polymer according to claim 3.
5. The aforementioned R 1 is a methyl group (-CH 3 The ion-conducting polymer according to claim 1, which is the same as the one described in claim 1.
6. The aforementioned R 2 The ion-conducting polymer according to claim 1, wherein is an organic group having 1 to 8 carbon atoms.
7. The aforementioned R 3 The ion-conducting polymer according to claim 1, wherein is an organic group having 4 to 16 carbon atoms.
8. The ion-conducting polymer according to claim 1, wherein the repeating unit represented by chemical formula 1 includes at least one of the repeating units represented by the following chemical formulas 1-1 to 1-5. 【Chemistry 2】 【Transformation 3】 【Chemistry 4】 【Transformation 5】 【Transformation 6】
9. The OH of the ionic conductive polymer at 25°C - The ion-conducting polymer according to claim 1, wherein the ion conductivity is 40 mS / cm to 80 mS / cm.
10. The steps include preparing a monomer having a benzene ring substituted with at least one alkoxy group, The steps include: reacting the monomer with an aldehyde under mild acidic conditions to obtain a precursor polymer; A method for producing an ion-conducting polymer, comprising the step of introducing a quaternary ammonium group into the precursor polymer to synthesize an ion-conducting polymer having repeating units represented by the following chemical formula 1. 【Transformation 7】 (In chemical formula 1, A + is a quaternary ammonium, B - is an anion, a is an integer from 1 to 3, R 1 R is an organic group having 1 to 10 carbon atoms. 2 H or an organic group having 1 to 10 carbon atoms, R 3 (where is an organic group having 1 to 20 carbon atoms containing at least one alkylene group or arylene group, and Ar is a benzene ring.)
11. A separation membrane comprising the ion-conducting polymer described in claim 1.
12. Positive electrode and, A negative electrode opposite the positive electrode, An apparatus comprising the separation membrane described in claim 11.
13. The aforementioned apparatus includes a water electrolysis device and a CO2 electrolysis device. 2 The apparatus according to claim 12, comprising an electrolytic device, a fuel cell, an electrolytic battery, or a vanadium flow battery.
Citation Information
Patent Citations
Spiro polymer electrolyte material and preparation method and application thereof
CN115093523A
Poly (4-aryl) piperidine polymer, preparation method and anion exchange membrane prepared from poly (4-aryl) piperidine polymer
CN117700657A
Anion exchange membrane with high ionic conductivity as well as preparation method and application of anion exchange membrane
CN118240159A
Sparingly water-soluble anion conductive resin
JP2013107916A
Anion exchange membrane and method for preparing the same
KR1020200023822A