Photosensitive resin composition
Patent Information
- Application Number
- JP2023508841
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-02-25
- Filing Date
- 2022-02-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-02-25
AI Technical Summary
Conventional negative photosensitive resins containing polyamic acid have high solubility in alkaline aqueous developers, leading to difficulties in controlling dissolution rates and achieving desired relief patterns, and tend to swell during development, causing stress and peeling of the formed relief pattern from the substrate, while those developed in organic solvents face challenges in achieving low dielectric loss tangents and high tensile elongation.
A photosensitive resin composition comprising a reaction product of an aromatic diamine compound with a photopolymerizable group and a tetracarboxylic acid derivative having three or more aromatic rings, which can be developed using an organic solvent, resulting in a cured film with low dielectric loss tangent and high tensile elongation.
The composition enables effective development in organic solvents, achieving a cured film with improved mechanical properties and reduced transmission loss, thereby enhancing the reliability and stability of the relief pattern.
Smart Images

Figure 2022202098000001 
Figure 2022202098000002 
Figure 2022202098000003
Abstract
Description
Photosensitive resin composition
[0001] The present invention relates to a photosensitive resin composition, a resin film obtained from the composition, a photosensitive resist film using the composition, a method for producing a substrate having a cured relief pattern, a substrate having a cured relief pattern, and a semiconductor device having a cured relief pattern.
[0002] Polyimide resins, which have excellent heat resistance, electrical properties, and mechanical properties, have been used as insulating materials for electronic components and passivation films, surface protective films, interlayer insulating films, and the like for semiconductor devices. Among these polyimide resins, those provided in the form of photosensitive polyimide precursors can easily form heat-resistant relief pattern coatings by applying the precursor, exposing it to light, developing it, and subjecting it to a thermal imidization treatment through curing. Such photosensitive polyimide precursors have the advantage of enabling significant process reduction compared to conventional non-photosensitive polyimide resins.
[0003] Patent Documents 1 and 2 propose photosensitive resin compositions containing polyamic acid or polyimide using diamines having a (meth)acryloyloxy group.
[0004] JP 2000-347404 A JP 2012-516927 A
[0005] In recent years, semiconductor devices have become increasingly sensitive to the need to transmit and process large amounts of information at high speed, leading to the trend toward higher frequencies for electrical signals. Because high-frequency electrical signals are prone to attenuation, low transmission loss is essential. Therefore, resins used in semiconductor devices are required to have a low dielectric dissipation factor. On the other hand, resins with low dielectric dissipation factors tend to be brittle, and may be unable to adapt to the thermal expansion of adjacent materials during heat treatment processes such as solder reflow, resulting in breakage or reduced interlayer adhesion. Therefore, resins used in semiconductor devices are required to have a high tensile elongation.
[0006] Furthermore, when forming a cured relief pattern, development is performed using a developer, and an alkaline aqueous developer or an organic solvent developer is generally used. Photosensitive resins for obtaining a cured relief pattern can be divided into positive-type resins, in which the photosensitive resin in the exposed areas dissolves in the developer after exposure and development, leaving the photosensitive resin in the unexposed areas, and negative-type resins, in which the photosensitive resin in the unexposed areas dissolves in the developer, leaving the photosensitive resin in the exposed areas. Negative-type resins have inferior resolution compared to positive-type resins, but are easily thickened and film-formed, and are highly reliable, making them suitable for the manufacture of semiconductor devices requiring such features. However, conventional negative-type photosensitive resins containing polyamic acid have extremely high solubility in alkaline aqueous developer, making it difficult to control the dissolution rate and potentially making it difficult to obtain a desired relief pattern. Furthermore, negative-type photosensitive resins containing polyamic acid have a high affinity for alkaline aqueous developer, which means they tend to swell during development, leading to problems such as the stress generated during drying that causes the formed relief pattern to peel off from the substrate. For this reason, organic solvent development is suitable for negative photosensitive resins containing polyamic acid, as it is relatively easy to control the dissolution rate and there is little risk of substrate peeling.
[0007] Therefore, there is a need for a photosensitive resin composition that can be developed in an organic solvent and that provides a cured film with a low dielectric tangent and high tensile elongation. However, the photosensitive resin compositions described in Patent Documents 1 and 2 do not satisfy all of these properties.
[0008] In view of the above circumstances, an object of the present invention is to provide a photosensitive resin composition that can be developed in an organic solvent and that produces a cured film having a low dielectric tangent and high tensile elongation; a resin film obtained from the composition; a photosensitive resist film using the composition; a method for producing a substrate having a cured relief pattern; a substrate having a cured relief pattern; and a semiconductor device having a cured relief pattern.
[0009] As a result of extensive research to achieve the above object, the present inventors have found that by incorporating into a photosensitive resin composition a reaction product of an aromatic diamine compound having a photopolymerizable group and a tetracarboxylic acid derivative having three or more aromatic rings, it is possible to obtain a photosensitive resin composition that can be developed in an organic solvent and that provides a cured film having a low dielectric tangent and high tensile elongation, thereby completing the present invention.
[0010] [1] A photosensitive resin composition comprising a reaction product of an aromatic diamine compound having a photopolymerizable group and a tetracarboxylic acid derivative having three or more aromatic rings, and a solvent. [2] The photosensitive resin composition according to [1], wherein the reaction product is a polyamic acid or a polyimide obtained by dehydrating and ring-closing a polyamic acid. [3] The photosensitive resin composition according to [2], wherein the polyamic acid has at least a structural unit represented by the following formula (1), and the polyimide has at least a structural unit represented by the following formula (2): [In formula (1), Ar 1 represents a divalent organic group having a photopolymerizable group and an aromatic ring, and Ar 2 represents a tetravalent organic group having three or more aromatic rings. [In formula (2), Ar 3 represents a divalent organic group having a photopolymerizable group and an aromatic ring, and Ar 4 represents a tetravalent organic group having three or more aromatic rings.] [4] Ar in the formula (1) 2 and Ar in the formula (2) 4 is a tetravalent organic group represented by the following formula (3): [In formula (3), X 1 and X 2 R each independently represents a direct bond, an ether bond, an ester bond, an amide bond, a urethane bond, a urea bond, a thioether bond or a sulfonyl bond. 1 and R 2 each independently represents an optionally substituted alkyl group having 1 to 6 carbon atoms; Y represents a divalent organic group represented by the following formula (3-1) or (3-2); n1 and n2 each independently represent an integer of 0 to 3. R 1If there are multiple R 1 may be the same or different. 2 If there are multiple R 2 may be the same or different. * represents a bond.] [In formula (3-1), Z 1 represents a direct bond, an ether bond, an ester bond, an amide bond, a urethane bond, a urea bond, a thioether bond, or a sulfonyl bond. 3 and R 4 each independently represents an optionally substituted hydrocarbon group having 1 to 6 carbon atoms; m1 represents an integer of 0 to 3; n3 and n4 each independently represent an integer of 0 to 4; Z 1 If there are multiple Z 1 may be the same or different. When n4 is plural, the plural n4 may be the same or different. 3 If there are multiple R 3 may be the same or different. 4 If there are multiple R 4 may be the same or different. * represents a bond. In formula (3-2), Z 2 R represents a divalent organic group represented by the following formula (4) or (5): 5 and R 6 each independently represents an optionally substituted hydrocarbon group having 1 to 6 carbon atoms; n5 and n6 each independently represent an integer of 0 to 4. R 5 If there are multiple R 5 may be the same or different. 6 If there are multiple R 6 may be the same or different. * represents a bond.] [In formula (4), R 7 and R 8 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms which may be substituted with a halogen atom. * represents a bond. In formula (5), R 9 and R 10each independently represents an optionally substituted alkylene group having 1 to 6 carbon atoms or an optionally substituted arylene group having 6 to 10 carbon atoms. * represents a bond.] [5] Ar in the formula (1) 1 and Ar in the formula (2) 3 is a divalent organic group represented by the following formula (6): [In formula (6), Z 3 represents an ether bond, an ester bond, an amide bond, a urethane bond or a urea bond; Z 4 represents a direct bond, an ester bond or an amide bond. 5 represents a direct bond, an ether bond, an ester bond, an amide bond, a urethane bond, a urea bond, a thioether bond, or a sulfonyl bond. m2 represents an integer of 0 or 1. R 11 represents a direct bond or an alkylene group having 2 to 6 carbon atoms which may be substituted with a hydroxyl group; R 12 represents a hydrogen atom or a methyl group. * represents a bond.] [6] Z in the formula (6) 3 and Z 4 [7] The photosensitive resin composition according to [5], wherein R in the formula (6) is an ester bond. 11is a 1,2-ethylene group. [8] The photosensitive resin composition according to any one of [1] to [7], further comprising a photoradical polymerization initiator. [9] The photosensitive resin composition according to any one of [1] to [8], further comprising a crosslinkable compound.
[10] The photosensitive resin composition according to any one of [1] to [9], which is used to form an insulating film.
[11] The photosensitive resin composition according to any one of [1] to
[10] , which is a negative photosensitive resin composition.
[12] A resin film, which is a fired product of a coating film of the photosensitive resin composition according to any one of [1] to
[11] .
[13] The resin film according to
[12] , which is an insulating film.
[14] A photosensitive resist film, which has a substrate film, a photosensitive resin layer formed from the photosensitive resin composition according to any one of [1] to
[11] , and a cover film.
[15] A method for producing a substrate having a cured relief pattern, comprising: (1) applying the photosensitive resin composition according to any one of [1] to
[11] onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer; (3) developing the exposed photosensitive resin layer to form a relief pattern; and (4) heat-treating the relief pattern to form a cured relief pattern.
[16] A method for producing a substrate having a cured relief pattern according to
[15] , wherein the developer used for the development is an organic solvent.
[17] A substrate having a cured relief pattern produced by the method according to
[15] or
[16] .
[18] A semiconductor device comprising a semiconductor element and a cured film provided on or below the semiconductor element, wherein the cured film has a cured relief pattern formed from the photosensitive resin composition according to any one of [1] to
[11] .
[0011] According to the present invention, there are provided a photosensitive resin composition that can be developed in an organic solvent and that produces a cured film having a low dielectric tangent and high tensile elongation; a resin film obtained from the composition; a photosensitive resist film using the composition; a method for producing a substrate having a cured relief pattern; a substrate having a cured relief pattern; and a semiconductor device having a cured relief pattern.
[0012] (Photosensitive Resin Composition) The photosensitive resin composition of the present invention contains at least the reaction product and a solvent, and further contains other components as necessary.
[0013] <Reaction Product> The reaction product is a reaction product of an aromatic diamine compound having a photopolymerizable group and a tetracarboxylic acid derivative having three or more aromatic rings. The reaction product contains, as constituent components, an aromatic diamine compound having a photopolymerizable group and a tetracarboxylic acid derivative having three or more aromatic rings, and may contain, as necessary, other diamine compounds and other tetracarboxylic acid derivatives as constituent components. The reaction product is, for example, a polyamic acid or a polyimide obtained by dehydrating and ring-closing a polyamic acid.
[0014] The reaction product contains an aromatic diamine compound having a photopolymerizable group as a constituent component, which imparts photosensitivity to a resin composition containing the reaction product.The reaction product contains an aromatic diamine compound and a tetracarboxylic acid derivative having three or more aromatic rings as constituent components, which results in a cured film having a low dielectric tangent and a high tensile elongation.
[0015] In the aromatic diamine compound having a photopolymerizable group, the two amino groups may be bonded to one aromatic ring or to each of the two aromatic rings. Examples of the aromatic ring include an aromatic hydrocarbon ring and an aromatic heterocycle. The aromatic diamine compound may have an aromatic ring to which no amino group is bonded.
[0016] Examples of photopolymerizable groups include radically polymerizable groups, cationically polymerizable groups, and anionically polymerizable groups. Among these, radically polymerizable groups are preferred. Examples of radically polymerizable groups include acryloyl groups, methacryloyl groups, propenyl ether groups, vinyl ether groups, and vinyl groups.
[0017] The reaction product preferably contains, as a constituent component, an aromatic diamine compound having three or more aromatic rings as a diamine compound other than the aromatic diamine compound having a photopolymerizable group, in that the resulting cured film has a lower dielectric tangent and a higher tensile elongation.
[0018] The number of aromatic rings in an aromatic diamine compound having three or more aromatic rings is not particularly limited as long as it is three or more, and may be, for example, four or more. The upper limit of the number of aromatic rings is not particularly limited, and may be, for example, eight or less, or six or less.
[0019] Regarding the counting of aromatic rings in "three or more aromatic rings," polycyclic aromatic rings formed by the condensation of two or more aromatic rings, such as naphthalene rings and anthracene rings, are counted as one aromatic ring. Therefore, a naphthalene ring is counted as one aromatic ring. On the other hand, a biphenyl ring is counted as two aromatic rings because it is not a condensed ring. Furthermore, a perylene ring is considered to be a structure formed by the condensation of two naphthalene rings, and is counted as two aromatic rings. Examples of aromatic rings include aromatic hydrocarbon rings and aromatic heterocycles.
[0020] Examples of the tetracarboxylic acid derivative in the "tetracarboxylic acid derivative" include tetracarboxylic acid dianhydrides, tetracarboxylic acid dihalides, tetracarboxylic acid dialkyl esters, and tetracarboxylic acid dialkyl ester dihalides, with tetracarboxylic acid dianhydrides being particularly preferred.
[0021] The tetracarboxylic acid derivative having three or more aromatic rings is preferably an aromatic tetracarboxylic acid derivative having three or more aromatic rings. An aromatic tetracarboxylic acid refers to a compound having four carboxy groups bonded to the same or different aromatic rings.
[0022] The number of aromatic rings in the tetracarboxylic acid derivative having three or more aromatic rings is not particularly limited as long as it is three or more, and may be, for example, four or more. The upper limit of the number of aromatic rings is not particularly limited, and may be, for example, eight or less, or six or less.
[0023] The ratio of the aromatic diamine compound having a photopolymerizable group to all diamine compounds constituting the reaction product is not particularly limited, but from the viewpoint of obtaining sufficient photosensitivity, it is preferably 10 to 100 mol %, more preferably 50 to 100 mol %. The ratio of the aromatic tetracarboxylic acid derivative having three or more aromatic rings to all tetracarboxylic acid derivatives constituting the reaction product is not particularly limited, but from the viewpoint of obtaining the effects of the present invention, it is preferably 20 to 100 mol %, more preferably 50 to 100 mol %.
[0024] The reaction product is preferably a polyamic acid or a polyimide obtained by dehydrating and cyclizing a polyamic acid. From the viewpoint of obtaining a finer relief pattern, a polyimide obtained by dehydrating and cyclizing a polyamic acid is more preferable. Here, the imidization rate of the polyimide does not need to be 100%. The imidization rate may be, for example, 90% or more, 95% or more, or 98% or more.
[0025] The polyamic acid preferably has at least a structural unit represented by the following formula (1): The polyimide preferably has at least a structural unit represented by the following formula (2): [In formula (1), Ar 1 represents a divalent organic group having a photopolymerizable group and an aromatic ring, Ar 2 represents a tetravalent organic group having three or more aromatic rings. [In formula (2), Ar 3 represents a divalent organic group having a photopolymerizable group and an aromatic ring, Ar 4 represents a tetravalent organic group having three or more aromatic rings.
[0026] <<Ar 1 and Ar 3 >> Ar 1 and Ar 3is a divalent organic group having a photopolymerizable group and an aromatic ring, and is not particularly limited as long as it exhibits the effects of the present invention. Note that the divalent organic group having a photopolymerizable group and an aromatic ring is a residue obtained by removing two amino groups from an aromatic diamine compound having a photopolymerizable group. Examples of the photopolymerizable group include the photopolymerizable groups described above.
[0027] Ar 1 and Ar 3 is preferably a divalent organic group represented by the following formula (6): [In formula (6), Z 3 represents an ether bond (—O—), an ester bond (—COO—), an amide bond (—NHCO—), a urethane bond (—NHCOO—) or a urea bond (—NHCONH—), and Z 4 represents a direct bond, an ester bond (—COO—) or an amide bond (—NHCO—). 5 is a direct bond, an ether bond (-O-), an ester bond (-COO-), an amide bond (-NHCO-), a urethane bond (-NHCOO-), a urea bond (-NHCONH-), a thioether bond (-S-), or a sulfonyl bond (-SO 2 m2 represents an integer of 0 to 1. R 11 represents a direct bond or an alkylene group having 2 to 6 carbon atoms which may be substituted with a hydroxyl group; R 12 represents a hydrogen atom or a methyl group. * represents a bond.
[0028] Examples of the alkylene group having 2 to 6 carbon atoms which may be substituted with a hydroxyl group include a 1,1-ethylene group, a 1,2-ethylene group, a 1,2-propylene group, a 1,3-propylene group, a 1,4-butylene group, a 1,2-butylene group, a 2,3-butylene group, a 1,2-pentylene group, a 2,4-pentylene group, a 1,2-hexylene group, a 1,2-cyclopropylene group, a 1,2-cyclobutylene group, a 1,3-cyclobutylene group, a 1,2-cyclopentylene group, a 1,2-cyclohexylene group, and alkylene groups in which at least a portion of the hydrogen atoms have been substituted with a hydroxyl group (for example, a 2-hydroxy-1,3-propylene group).
[0029] Z 3is preferably an ester bond. 4 An ester bond is preferred as R 11 As the alkyl group, a 1,2-ethylene group is preferred.
[0030] Examples of the divalent organic group represented by formula (6) include the following divalent organic groups. In the formula, * represents a bond, and the two bonds are located, for example, at meta positions relative to the substituent having the photopolymerizable group.
[0031] <<Ar 2 and Ar 4 >> Ar in formula (1) 2 and Ar in formula (2) 4 is not particularly limited as long as it is a tetravalent organic group having three or more aromatic rings and exhibiting the effects of the present invention, but from the viewpoint of suitably obtaining the effects of the present invention, it is preferably a divalent organic group represented by the following formula (3): [In formula (3), X 1 and X 2 are each independently a direct bond, an ether bond (-O-), an ester bond (-COO-), an amide bond (-NHCO-), a urethane bond (-NHCOO-), a urea bond (-NHCONH-), a thioether bond (-S-), or a sulfonyl bond (-SO 2 -) represents. 1 and R 2 each independently represents an optionally substituted alkyl group having 1 to 6 carbon atoms; Y represents a divalent organic group represented by the following formula (3-1) or (3-2); n1 and n2 each independently represent an integer of 0 to 3. R 1 If there are multiple R 1 may be the same or different. 2 If there are multiple R 2 may be the same or different. * represents a bond.]
[0032] R 1 and R 2Examples of the optionally substituted alkyl group having 1 to 6 carbon atoms in the formula (I) include alkyl groups having 1 to 6 carbon atoms. Examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, propyl, butyl, pentyl, and hexyl. In this specification, unless otherwise specified, the alkyl group may be linear, branched, or cyclic, or may be a combination of two or more of these. Examples of substituents in the optionally substituted alkyl group having 1 to 6 carbon atoms include halogen atoms, hydroxy groups, mercapto groups, carboxy groups, cyano groups, formyl groups, haloformyl groups, sulfo groups, amino groups, nitro groups, nitroso groups, oxo groups, thioxy groups, and alkoxy groups having 1 to 6 carbon atoms. Note that the "1 to 6 carbon atoms" in the "optionally substituted alkyl group having 1 to 6 carbon atoms" refers to the number of carbon atoms in the "alkyl group" excluding the substituent. The number of substituents is not particularly limited.
[0033] [In formula (3-1), Z 1 is a direct bond, an ether bond (-O-), an ester bond (-COO-), an amide bond (-NHCO-), a urethane bond (-NHCOO-), a urea bond (-NHCONH-), a thioether bond (-S-), or a sulfonyl bond (-SO 2 -) represents. 3 and R 4 each independently represents an optionally substituted hydrocarbon group having 1 to 6 carbon atoms; m1 represents an integer of 0 to 3; n3 and n4 each independently represent an integer of 0 to 4; Z 1 If there are multiple Z 1 may be the same or different. When n4 is plural, the plural n4 may be the same or different. 3 If there are multiple R 3 may be the same or different. 4 If there are multiple R 4 may be the same or different. * represents a bond. In formula (3-2), Z 2R represents a divalent organic group represented by the following formula (4) or (5): 5 and R 6 each independently represents an optionally substituted hydrocarbon group having 1 to 6 carbon atoms; n5 and n6 each independently represent an integer of 0 to 4. R 5 If there are multiple R 5 may be the same or different. 6 If there are multiple R 6 may be the same or different. * represents a bond.]
[0034] R 3 , R 4 , R 5 , and R 6 Examples of the optionally substituted hydrocarbon group having 1 to 6 carbon atoms in the formula (I) include an optionally substituted alkyl group having 1 to 6 carbon atoms and an optionally substituted phenyl group. Examples of the substituent include a halogen atom, a hydroxy group, a mercapto group, a carboxy group, a cyano group, a formyl group, a haloformyl group, a sulfo group, an amino group, a nitro group, a nitroso group, an oxo group, a thioxy group, and an alkoxy group having 1 to 6 carbon atoms. Note that the "1 to 6 carbon atoms" in the "optionally substituted hydrocarbon group having 1 to 6 carbon atoms" refers to the number of carbon atoms in the "hydrocarbon group" excluding the substituent. Furthermore, the number of substituents is not particularly limited.
[0035] R 3 , R 4 , R 5 and R 6 Specific examples of the optionally substituted alkyl group having 1 to 6 carbon atoms in the formula (I) include, for example, R 1 and R 2 Examples of the alkyl group include the alkyl groups having 1 to 6 carbon atoms which may be substituted as exemplified in the description of the above.
[0036] [In formula (4), R 7 and R 8 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms which may be substituted with a halogen atom. * represents a bond. In formula (5), R 9 and R 10each independently represents an optionally substituted alkylene group having 1 to 6 carbon atoms or an optionally substituted arylene group having 6 to 10 carbon atoms. * represents a bond.]
[0037] R 7 and R 8 Examples of the hydrocarbon group having 1 to 6 carbon atoms which may be substituted with a halogen atom in the above formula (I) include an alkyl group having 1 to 6 carbon atoms, a halogenated alkyl group having 1 to 6 carbon atoms, a phenyl group, and a halogenated phenyl group. Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group. Examples of the halogen atom in the halogenated alkyl group having 1 to 6 carbon atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. The halogenation in the halogenated alkyl group having 1 to 6 carbon atoms and the halogenated phenyl group may be partial or complete.
[0038] R 9 and R 10 Examples of the substituent in the optionally substituted alkylene group having 1 to 6 carbon atoms in the formula (I) include a halogen atom, a hydroxy group, a mercapto group, a carboxy group, a cyano group, a formyl group, a haloformyl group, a sulfo group, an amino group, a nitro group, a nitroso group, an oxo group, a thioxy group, and an alkoxy group having 1 to 6 carbon atoms. Examples of the optionally substituted alkylene group having 1 to 6 carbon atoms include an alkylene group having 1 to 6 carbon atoms and a halogenated alkylene group having 1 to 6 carbon atoms. Examples of the alkylene group having 1 to 6 carbon atoms include a methylene group, an ethylene group, a propylene group, and a butylene group. Note that the "1 to 6 carbon atoms" in the "optionally substituted alkylene group having 1 to 6 carbon atoms" refers to the number of carbon atoms in the "alkylene group" excluding the substituent. The number of substituents is not particularly limited.
[0039] R 9 and R 10Examples of the substituent in the optionally substituted arylene group having 6 to 10 carbon atoms in the formula (I) include a halogen atom, an optionally halogenated alkyl group having 1 to 6 carbon atoms, and an optionally halogenated alkoxy group having 1 to 6 carbon atoms. The halogenation may be partial or complete. Examples of the arylene group include a phenylene group and a naphthylene group. The "6 to 10 carbon atoms" in the "optionally substituted arylene group having 6 to 10 carbon atoms" refers to the number of carbon atoms in the "arylene group" excluding the substituent. The number of substituents is not particularly limited.
[0040] Examples of the divalent organic group represented by formula (4) include divalent organic groups represented by the following formulas: In the formula, * represents a bond.
[0041] Examples of the divalent organic group represented by formula (5) include divalent organic groups represented by the following formulas: In the formula, R 13 ~R 15 each independently represents a halogen atom, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom. n13 represents an integer of 0 to 5. n14 and n15 each independently represent an integer of 0 to 4. R 13 If there are multiple R 13 may be the same or different. 14 If there are multiple R 14 may be the same or different. 15 If there are multiple R 15 may be the same or different. * represents a bond.
[0042] R 13 ~R 15Specific examples of the alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom in the formula (I) include an alkyl group having 1 to 6 carbon atoms and a halogenated alkyl group having 1 to 6 carbon atoms. Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group. Examples of the halogen atom in the halogenated alkyl group having 1 to 6 carbon atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. The halogenation in the halogenated alkyl group having 1 to 6 carbon atoms may be partial or complete. R 13 ~R 15 Specific examples of the alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom in the formula (I) include an alkoxy group formed from an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom.
[0043] Ar 2 and Ar 4 Examples of the tetravalent organic group include the tetravalent organic group represented by the following formula: In the formula, * represents a bond.
[0044] <Other Structural Units> The polyamic acid may have a structural unit other than the structural unit represented by formula (1). An example of the other structural unit is a structural unit represented by the following formula (1'). The polyimide may have a structural unit other than the structural unit represented by formula (2). An example of the other structural unit is a structural unit represented by the following formula (2'). [In formula (1'), Ar 1’ represents a divalent organic group having a photopolymerizable group and an aromatic ring or a divalent organic group other than a divalent organic group having a photopolymerizable group and an aromatic ring, Ar 2’ represents a tetravalent organic group having three or more aromatic rings or a tetravalent organic group not having three or more aromatic rings. 1’ is a divalent organic group having a photopolymerizable group and an aromatic ring, and Ar 2’ is a tetravalent organic group having three or more aromatic rings. [In formula (2'), Ar 3’ represents a divalent organic group having a photopolymerizable group and an aromatic ring or a divalent organic group other than a divalent organic group having a photopolymerizable group and an aromatic ring, Ar 4’ represents a tetravalent organic group having three or more aromatic rings or a tetravalent organic group not having three or more aromatic rings. 3’ is a divalent organic group having a photopolymerizable group and an aromatic ring, and Ar 4’ is a tetravalent organic group having three or more aromatic rings.
[0045] Ar 1’ and Ar 2’ Examples of the combinations include the following combinations (i) to (iii): (i): Ar 1’ represents a divalent organic group having a photopolymerizable group and an aromatic ring, Ar 2’ represents a tetravalent organic group having no three or more aromatic rings (ii): Ar 1’ represents a divalent organic group other than a divalent organic group having a photopolymerizable group or an aromatic ring, Ar 2’ represents a tetravalent organic group having no three or more aromatic rings (iii): Ar 1’ represents a divalent organic group other than a divalent organic group having a photopolymerizable group or an aromatic ring, Ar 2’ represents a tetravalent organic group having three or more aromatic rings
[0046] Ar 3’ and Ar 4’ Examples of the combinations include the following combinations (iv) to (vi): (iv): Ar 3’ represents a divalent organic group having a photopolymerizable group and an aromatic ring, Ar 4’ represents a tetravalent organic group having no three or more aromatic rings (v): Ar 3’ represents a divalent organic group other than a divalent organic group having a photopolymerizable group or an aromatic ring, Ar 4’ represents a tetravalent organic group having no three or more aromatic rings (vi): Ar 3’ represents a divalent organic group other than a divalent organic group having a photopolymerizable group or an aromatic ring, Ar 4’represents a tetravalent organic group having three or more aromatic rings
[0047] <<Ar 1’ and Ar 3’ >> Ar 1’ and Ar 3’ Examples of the divalent organic group having a photopolymerizable group and an aromatic ring in 1 and Ar 3 Examples of the divalent organic group having a photopolymerizable group and an aromatic ring are those exemplified in the description of Ar. 1’ and Ar 3’ The divalent organic group other than the photopolymerizable group and the divalent organic group having an aromatic ring in (1) is not particularly limited, but a divalent organic group having three or more aromatic rings is preferred in that a lower dielectric tangent and a higher tensile elongation can be obtained in the resulting cured film. The divalent organic group having three or more aromatic rings is not particularly limited, but is preferably a divalent organic group represented by the following formula (13): [In formula (13), X 21 and X 22 are each independently a direct bond, an ether bond (-O-), an ester bond (-COO-), an amide bond (-NHCO-), a urethane bond (-NHCOO-), a urea bond (-NHCONH-), a thioether bond (-S-), or a sulfonyl bond (-SO 2 -) represents. 21 and R 22 Y each independently represents an optionally substituted alkyl group having 1 to 6 carbon atoms. 20 represents a divalent organic group represented by the following formula (13-1) or (13-2), and n21 and n22 each independently represent an integer of 0 to 4. 21 If there are multiple R 21 may be the same or different. 22 If there are multiple R 22 may be the same or different. * represents a bond.]
[0048] R 21 and R 22 Specific examples of the optionally substituted alkyl group having 1 to 6 carbon atoms in R 1 and R2 Examples of the alkyl group include the alkyl groups having 1 to 6 carbon atoms which may be substituted, as exemplified in the description of the alkyl group having 1 to 6 carbon atoms. Note that the "1 to 6 carbon atoms" in the "alkyl group having 1 to 6 carbon atoms which may be substituted" refers to the number of carbon atoms in the "alkyl group" excluding the substituents. The number of substituents is not particularly limited.
[0049] [In formula (13-1), Z 21 is a direct bond, an ether bond (-O-), an ester bond (-COO-), an amide bond (-NHCO-), a urethane bond (-NHCOO-), a urea bond (-NHCONH-), a thioether bond (-S-), or a sulfonyl bond (-SO 2 -) represents. 23 and R 24 each independently represents an optionally substituted hydrocarbon group having 1 to 6 carbon atoms; m21 represents an integer of 0 to 3; n23 and n24 each independently represents an integer of 0 to 4. Z 21 If there are multiple Z 21 may be the same or different. When n24 is plural, the plural n24 may be the same or different. R 23 If there are multiple R 23 may be the same or different. 24 If there are multiple R 24 may be the same or different. * represents a bond. In formula (13-2), Z 22 R represents a divalent organic group represented by the following formula (14) or (15). 25 and R 26 each independently represents an optionally substituted hydrocarbon group having 1 to 6 carbon atoms; n25 and n26 each independently represent an integer of 0 to 4. R 25 If there are multiple R 25 may be the same or different. 26 If there are multiple R 26 may be the same or different. * represents a bond.]
[0050] R 23 , R 24 , R 25 , and R26 Specific examples of the optionally substituted hydrocarbon group having 1 to 6 carbon atoms in R 3 , R 4 , R 5 , and R 6 Examples of the hydrocarbon group include the optionally substituted hydrocarbon groups having 1 to 6 carbon atoms exemplified in the description of (1). Note that the "carbon number of 1 to 6" in the "optionally substituted hydrocarbon group having 1 to 6 carbon atoms" refers to the number of carbon atoms in the "hydrocarbon group" excluding the substituents. In addition, the number of substituents is not particularly limited.
[0051] R 23 , R 24 , R 25 and R 26 Specific examples of the optionally substituted alkyl group having 1 to 6 carbon atoms in the formula (I) include, for example, R 1 and R 2 Examples of the alkyl group include the alkyl groups having 1 to 6 carbon atoms which may be substituted as exemplified in the description of the above.
[0052] [In formula (14), R 27 and R 28 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms which may be substituted with a halogen atom. * represents a bond. In formula (15), R 29 and R 30 each independently represents an optionally substituted alkylene group having 1 to 6 carbon atoms or an optionally substituted arylene group having 6 to 10 carbon atoms. * represents a bond.]
[0053] R 27 and R 28 Specific examples of the hydrocarbon group having 1 to 6 carbon atoms which may be substituted with a halogen atom in R 7 and R 8 Examples of the hydrocarbon groups include those having 1 to 6 carbon atoms which may be substituted with a halogen atom as exemplified in the description of (1).
[0054] R 29 and R 30 Specific examples of the optionally substituted alkylene group having 1 to 6 carbon atoms in R 9 and R10 Examples of the alkylene group include the alkylene groups having 1 to 6 carbon atoms which may be substituted, as exemplified in the description of the group 1 to 6. The "1 to 6 carbon atoms" in the "alkylene group having 1 to 6 carbon atoms which may be substituted" refers to the number of carbon atoms in the "alkylene group" excluding the substituents. The number of substituents is not particularly limited.
[0055] R 29 and R 30 Specific examples of the optionally substituted arylene group having 6 to 10 carbon atoms in R 9 and R 10 Examples of the arylene group include the optionally substituted arylene groups having 6 to 10 carbon atoms exemplified in the description of 1. Note that the "6 to 10 carbon atoms" in the "optionally substituted arylene group having 6 to 10 carbon atoms" refers to the number of carbon atoms in the "arylene group" excluding the substituents. In addition, the number of substituents is not particularly limited.
[0056] Examples of the divalent organic group represented by formula (14) include divalent organic groups represented by the following formulas: In the formula, * represents a bond.
[0057] Examples of the divalent organic group represented by formula (15) include divalent organic groups represented by the following formulas: In the formula, R 33 ~R 35 each independently represents a halogen atom, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom. n33 represents an integer of 0 to 5. n34 and n35 each independently represent an integer of 0 to 4. R 33 If there are multiple R 33 may be the same or different. 34 If there are multiple R 34 may be the same or different. 35 If there are multiple R 35 may be the same or different. * represents a bond.
[0058] R 33 ~R35 Specific examples of the alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom in R 13 ~R 15 Examples of the alkyl groups include those having 1 to 6 carbon atoms which may be substituted with a halogen atom as exemplified in the description of R. 33 ~R 35 Specific examples of the alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom in the formula (I) include an alkoxy group formed from an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom.
[0059] Ar 1’ and Ar 3’ Examples of the group include divalent organic groups represented by the following formula: In the formula, * represents a bond.
[0060] Other Ar 1’ and Ar 3’ Examples of the group include divalent organic groups represented by the following formula: In the formula, * represents a bond.
[0061] <<Ar 2’ and Ar 4’ >> Ar 2’ and Ar 4’ Examples of the tetravalent organic group having three or more aromatic rings in 2 and Ar 4 Examples of the tetravalent organic groups having three or more aromatic rings include those exemplified in the description of Ar. 2’ and Ar 4’ Examples of the tetravalent organic group not having three or more aromatic rings in the above formula include a tetravalent organic group having one or two aromatic rings and a tetravalent organic group not having an aromatic ring. The tetravalent organic group having one or two aromatic rings is derived, for example, from an aromatic tetracarboxylic dianhydride derivative. Furthermore, the tetravalent organic group not having an aromatic ring is derived, for example, from an aliphatic tetracarboxylic anhydride derivative. Such a tetravalent organic group is not particularly limited, but examples include the following tetravalent organic groups. In the formula, * represents a bond.
[0062] The proportion of the structural unit represented by formula (1) in all structural units of the polyamic acid is not particularly limited, but from the viewpoint of obtaining sufficient photosensitivity, it is preferably 10 to 100 mol %, more preferably 50 to 100 mol %. Note that the structural unit is also a repeating unit. When the polyamic acid has a structural unit represented by formula (1'), the proportion of the structural unit represented by formula (1') in all structural units of the polyamic acid is not particularly limited, but is preferably 1 to 90 mol %, more preferably 1 to 50 mol %.
[0063] When the imidization rate of the polyimide is not 100%, the polyimide may have a structural unit represented by formula (1) in addition to the structural unit represented by formula (2). The total proportion of the structural units represented by formula (1) and the structural units represented by formula (2) in all structural units of the polyimide is not particularly limited, but from the viewpoint of obtaining sufficient photosensitivity, it is preferably 10 to 100 mol%, more preferably 50 to 100 mol%. When the polyimide has at least one of the structural units represented by formula (1') and the structural unit represented by formula (2'), the total proportion of the structural units represented by formula (1') and the structural units represented by formula (2') in all structural units of the polyimide is not particularly limited, but is preferably 1 to 90 mol%, more preferably 1 to 50 mol%.
[0064] The weight-average molecular weight of the reaction product is not particularly limited, but the weight-average molecular weight measured in terms of polystyrene by gel permeation chromatography (hereinafter abbreviated as GPC in this specification) is preferably 5,000 to 100,0000, more preferably 7,000 to 50,000, still more preferably 10,000 to 50,000, and particularly preferably 10,000 to 40,000.
[0065] <Method for producing reaction product> The reaction product is obtained by reacting an aromatic diamine compound having a photopolymerizable group, a tetracarboxylic acid derivative having three or more aromatic rings, and, if necessary, other diamine compounds and other tetracarboxylic acid derivatives.
[0066] The method for producing the reaction product is not particularly limited, and examples thereof include known methods for producing polyamic acid or polyimide by reacting a diamine compound with a tetracarboxylic acid derivative. Polyamic acid and polyimide can be synthesized by known methods such as those described in WO 2013 / 157586.
[0067] The reaction product is produced, for example, by reacting a diamine component containing an aromatic diamine compound having a photopolymerizable group with a tetracarboxylic acid derivative component having three or more aromatic rings in a solvent (condensation polymerization).
[0068] Specific examples of the solvent include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylpropionamide, N,N-dimethylisobutyric acid amide, dimethyl sulfoxide, and 1,3-dimethyl-2-imidazolidinone. When the polymer has high solubility in the solvent, methyl ethyl ketone, cyclohexanone, cyclopentanone, 4-hydroxy-4-methyl-2-pentanone, or solvents represented by the following formulas [D-1] to [D-3] can be used. (In formula [D-1], D 1 represents an alkyl group having 1 to 3 carbon atoms, and in formula [D-2], D 2 represents an alkyl group having 1 to 3 carbon atoms, and in formula [D-3], D 3 represents an alkyl group having 1 to 4 carbon atoms.
[0069] These solvents may be used alone or in combination. Furthermore, even if a solvent does not dissolve the reaction product, it may be mixed with the above-mentioned solvent to the extent that the reaction product does not precipitate.
[0070] When the diamine component and the tetracarboxylic acid derivative component are reacted in a solvent, the reaction can be carried out at any concentration, preferably 1 to 50% by mass, and more preferably 5 to 30% by mass. The reaction can be carried out at a high concentration initially, with additional solvent added later. In the reaction, the ratio of the total number of moles of the diamine component to the total number of moles of the tetracarboxylic acid derivative component is preferably 0.8 to 1.2. As with a typical condensation polymerization reaction, the closer this molar ratio is to 1.0, the higher the molecular weight of the reaction product produced.
[0071] When reacting the diamine component with the tetracarboxylic acid derivative component, a thermal polymerization inhibitor may be added to the reaction system to prevent polymerization of the photopolymerizable group. Examples of thermal polymerization inhibitors include hydroquinone, 4-methoxyphenol, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-cresol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt. The amount of the thermal polymerization inhibitor used is not particularly limited.
[0072] Polyimide can be obtained by dehydrating and cyclizing the polyamic acid, which is the reaction product obtained in the above reaction. Methods for obtaining polyimide include thermal imidization, in which a solution of the polyamic acid, which is the reaction product obtained in the above reaction, is heated as is, or chemical imidization, in which a catalyst is added to a solution of polyamic acid. When thermal imidization is performed in a solution, the temperature is 100 to 400°C, preferably 120 to 250°C, and it is preferable to perform the imidization while removing water produced by the imidization reaction from the system.
[0073] The chemical imidization can be carried out by adding a basic catalyst and an acid anhydride to a solution of the polyamic acid obtained by the reaction and stirring at -20 to 250°C, preferably 0 to 180°C. The amount of the basic catalyst is 0.1 to 30 molar times, preferably 0.2 to 20 molar times, the amount of the amic acid groups, and the amount of the acid anhydride is 1 to 50 molar times, preferably 1.5 to 30 molar times, the amount of the amic acid groups. Examples of basic catalysts include pyridine, triethylamine, trimethylamine, tributylamine, and trioctylamine. Of these, triethylamine is preferred because it is less likely to produce polyisoimide as a by-product. Examples of acid anhydrides include acetic anhydride, trimellitic anhydride, and pyromellitic anhydride. Of these, acetic anhydride is preferred because it facilitates purification after the reaction. The imidization rate (the ratio of ring-closed repeating units to all repeating units in the polyimide precursor, also known as the ring-closure rate) during chemical imidization can be controlled by adjusting the catalyst amount, reaction temperature, and reaction time.
[0074] When recovering the produced imidized product from the imidization reaction solution, the reaction solution may be poured into a solvent to cause precipitation. Examples of solvents used for precipitation include methanol, ethanol, isopropyl alcohol, acetone, hexane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, toluene, benzene, and water. The polymer precipitated by pouring into the solvent can be recovered by filtration and then dried at room temperature or by heating under normal or reduced pressure.
[0075] The polyimide has repeating units that are partially or entirely ring-closed, and the imidization rate in the polyimide is preferably 20 to 99%, more preferably 30 to 99%, and even more preferably 50 to 99%.
[0076] The polyimide may be end-capped. The method for end-capping is not particularly limited, and for example, a conventionally known method using a monoamine or an acid anhydride can be used.
[0077] <Solvent> As the solvent contained in the photosensitive resin composition, it is preferable to use an organic solvent from the viewpoint of solubility in the reaction product. Specific examples of the solvent include N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylpropionamide, N,N-dimethylisobutyric acid amide, dimethyl sulfoxide, diethylene glycol dimethyl ether, cyclopentanone, cyclohexanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethylurea, 1,3-dimethyl-2-imidazolinone, N-cyclohexyl-2-pyrrolidone, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, methyl 2-hydroxyisobutyrate, ethyl lactate, and solvents represented by the following formulas [D-1] to [D-3]. These may be used alone or in combination of two or more. (In formula [D-1], D 1 represents an alkyl group having 1 to 3 carbon atoms, and in formula [D-2], D 2 represents an alkyl group having 1 to 3 carbon atoms, and in formula [D-3], D 3 represents an alkyl group having 1 to 4 carbon atoms.
[0078] The solvent can be used in an amount of, for example, 30 parts by mass to 1500 parts by mass, preferably 100 parts by mass to 1000 parts by mass, relative to 100 parts by mass of the reaction product, depending on the desired coating film thickness and viscosity of the photosensitive resin composition.
[0079] <Other Components> In an embodiment, the photosensitive resin composition may further contain other components in addition to the reaction product and the solvent. Examples of the other components include a photoradical polymerization initiator (also referred to as a "photoradical initiator"), a crosslinking compound (also referred to as a "crosslinking agent"), a thermosetting agent, other resin components, a filler, a sensitizer, an adhesion aid, a thermal polymerization inhibitor, an azole compound, and a hindered phenol compound.
[0080] <<Photoradical Polymerization Initiator>> The photoradical polymerization initiator is not particularly limited as long as it is a compound that absorbs light from a light source used for photocuring. Examples of the photoradical polymerization initiator include tert-butylperoxy-iso-butylate, 2,5-dimethyl-2,5-bis(benzoyldioxy)hexane, 1,4-bis[α-(tert-butyldioxy)-iso-propoxy]benzene, di-tert-butylperoxide, 2,5-dimethyl-2,5-bis(tert-butyldioxy)hexene hydroperoxide, α-(iso-propylphenyl)-iso-propyl hydroperoxide, tert-butyl hydroperoxide, 1,1-bis(tert-butyldioxy)-3,3,5-trimethylcyclohexane, butyl-4,4-bis(tert-butyldioxy)valerate, cyclohexanone peroxide, 2,2',5,5'-tetra(tert-butylperoxy)- ... Organic peroxides such as 3,3'-bis(tert-butylperoxycarbonyl)benzophenone, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, 3,3',4,4'-tetra(tert-amylperoxycarbonyl)benzophenone, 3,3',4,4'-tetra(tert-hexylperoxycarbonyl)benzophenone, 3,3'-bis(tert-butylperoxycarbonyl)-4,4'-dicarboxybenzophenone, tert-butylperoxybenzoate, and di-tert-butyldiperoxyisophthalate; quinones such as 9,10-anthraquinone, 1-chloroanthraquinone, 2-chloroanthraquinone, octamethylanthraquinone, and 1,2-benzanthraquinone; benzoin derivatives such as benzoin methyl, benzoin ethyl ether, α-methylbenzoin, and α-phenylbenzoin;2,2-Dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-[4-{4-(2-hydroxy-2-methyl-propionyl)benzyl}-phenyl]-2-methyl-propan-1-one, phenylglyoxylic acid methyl ester, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)phenyl alkylphenone compounds such as bis(2,4,6-trimethylbenzoyl)-1-butanone and 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one; acylphosphine oxide compounds such as bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide; and oxime ester compounds such as 2-(O-benzoyloxime)-1-[4-(phenylthio)phenyl]-1,2-octanedione and 1-(O-acetyloxime)-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone.
[0081] The photoradical polymerization initiator is commercially available, for example, IRGACURE [registered trademark] 651, 184, 2959, 127, 907, 369, 379EG, 819, 819DW, 1800, 1870, 784, OXE01, OXE02, OXE03, OXE04, 250, 1173, MBF, TPO, 4265, TPO (all manufactured by BASF), KAYACURE [registered trademark] DETX-S, MBP, DMBI, EPA, OA (all manufactured by Nippon Kayaku Co., Ltd.), VICURE-10, VICURE-55 (all manufactured by Stauffer Co., Ltd.), ESACURE Examples of such photo-radical polymerization initiators include KIP150, TZT, 1001, KTO46, KB1, KL200, KS300, EB3, Triazine-PMS, Triazine A, and Triazine B (all manufactured by Nippon SiberHegner Co., Ltd.), ADEKA OPTOMER N-1717, N-1414, and N-1606, ADEKA ARCLES N-1919T, NCI-831E, NCI-930, and NCI-730 (all manufactured by ADEKA Corporation). These photo-radical polymerization initiators may be used alone or in combination of two or more.
[0082] The content of the photoradical polymerization initiator is not particularly limited, but is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the reaction product, and more preferably 0.5 to 15 parts by mass from the viewpoint of photosensitivity characteristics. When the photoradical polymerization initiator is contained in an amount of 0.1 part by mass or more relative to 100 parts by mass of the reaction product, the photosensitivity of the photosensitive resin composition tends to be improved, while when the photoradical polymerization initiator is contained in an amount of 20 parts by mass or less, the thick-film curability of the photosensitive resin composition tends to be improved.
[0083] <<Crosslinkable Compound>> In an embodiment, in order to improve the resolution of the relief pattern, a monomer having a photoradical polymerizable unsaturated bond (crosslinkable compound) may be optionally contained in the photosensitive resin composition.Such a crosslinkable compound is preferably a (meth)acrylic compound that undergoes a radical polymerization reaction with a photoradical polymerization initiator, and includes, but is not limited to, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, ethylene glycol or polyethylene glycol mono- or di(meth)acrylate, propylene glycol or polypropylene glycol mono- or di(meth)acrylate, glycerol mono-, di- or tri(meth)acrylate, 1,4-butanediol, di(meth)acrylate of 1,6-hexanediol, di(meth)acrylate of 1,9-nonanediol, di(meth)acrylate of 1,10-decanediol, di(meth)acrylate of neopentyl glycol, cyclohexane di(meth)acrylate, di(meth)acrylate of cyclohexanedimethanol, di(meth)acrylate of tricyclodecanedimethanol, di(meth)acrylate of dioxane glycol, mono- or di(meth)acrylate of bisphenol A, bisphenol Di(meth)acrylate of bisphenol F, di(meth)acrylate of hydrogenated bisphenol A, benzene trimethacrylate, di(meth)acrylate of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, di(meth)acrylate of tris(2-hydroxyethyl)isocyanurate, isobornyl (meth)acrylate, acrylamide and its derivatives, methacrylamide and its derivatives, trimethylolpropane tri(meth)acrylate, di- or tri(meth)acrylate of glycerol, pentaerythritol Examples of such compounds include di-, tri-, or tetra(meth)acrylates of tungsten, and ethylene oxide or propylene oxide adducts of these compounds, 2-isocyanate ethyl (meth)acrylate or isocyanate-containing (meth)acrylates, and compounds obtained by adding a blocking agent such as methyl ethyl ketone oxime, ε-caprolactam, γ-caprolactam, 3,5-dimethylpyrazole, diethyl malonate, ethanol, isopropanol, n-butanol, or 1-methoxy-2-propanol to these compounds. These compounds may be used alone or in combination of two or more.In this specification, (meth)acrylate means acrylate and methacrylate.
[0084] The content of the crosslinkable compound is not particularly limited, but is preferably 1 to 100 parts by mass, and more preferably 1 to 50 parts by mass, per 100 parts by mass of the reaction product.
[0085] <<Thermal Curing Agent>> Examples of the thermal curing agent include hexamethoxymethylmelamine, tetramethoxymethylglycoluril, tetramethoxymethylbenzoguanamine, 1,3,4,6-tetrakis(methoxymethyl)glycoluril, 1,3,4,6-tetrakis(butoxymethyl)glycoluril, 1,3,4,6-tetrakis(hydroxymethyl)glycoluril, 1,3-bis(hydroxymethyl)urea, 1,1,3,3-tetrakis(butoxymethyl)urea, and 1,1,3,3-tetrakis(methoxymethyl)urea. The content of the thermal curing agent in the photosensitive resin composition is not particularly limited.
[0086] <<Filler>> Examples of the filler include inorganic fillers, and specific examples include sols of silica, aluminum nitride, boron nitride, zirconia, alumina, etc. The content of the filler in the photosensitive resin composition is not particularly limited.
[0087] <<Other Resin Components>> In an embodiment, the photosensitive resin composition may further contain a resin component other than the reaction product. Examples of resin components that can be contained in the photosensitive resin composition include polyoxazole, polyoxazole precursor, phenolic resin, polyamide, epoxy resin, siloxane resin, and acrylic resin. The content of these resin components is not particularly limited, but is preferably in the range of 0.01 to 20 parts by mass per 100 parts by mass of the reaction product.
[0088] <<Sensitizer>> In an embodiment, a sensitizer can be optionally blended into the photosensitive resin composition to improve photosensitivity. Examples of sensitizers include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, and p-dimethylaminocinnamylideneindano. p-dimethylaminobenzylidene indanone, 2-(p-dimethylaminophenylbiphenylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetyl
[0039] Examples of the methylaminobenzoate include methylaminobenzoate, ... These may be used alone or in combination.
[0089] The content of the sensitizer is not particularly limited, but is preferably 0.1 to 25 parts by mass per 100 parts by mass of the reaction product.
[0090] <<Adhesion Aid>> In an embodiment, in order to improve the adhesion between a film formed using the photosensitive resin composition and a substrate, an adhesion aid can be optionally blended into the photosensitive resin composition. Examples of the adhesion aid include γ-aminopropyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, 3-(meth)acryloxypropyldimethoxymethylsilane, 3-(meth)acryloxypropyltrimethoxysilane, dimethoxymethyl-3-piperidinopropylsilane, diethoxy-3-glycidoxypropylmethylsilane, N-(3-diethoxymethylsilylpropyl)succinimide, N-[3-(triethoxysilyl)propyl]furan, and the like. Examples of the adhesive agent include silane coupling agents such as thalamic acid, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propylamido)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propylamido)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propyl succinic anhydride and N-phenylaminopropyltrimethoxysilane, and aluminum-based adhesion promoters such as aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate) and ethylacetoacetate aluminum diisopropylate.
[0091] Among these adhesion aids, it is more preferable to use a silane coupling agent in terms of adhesive strength.
[0092] The content of the adhesive aid is not particularly limited, but is preferably in the range of 0.5 to 25 parts by mass per 100 parts by mass of the reaction product.
[0093] <<Thermal Polymerization Inhibitor>> In an embodiment, a thermal polymerization inhibitor can be optionally blended to improve the stability of the viscosity and photosensitivity of the photosensitive resin composition, particularly during storage in a solvent-containing solution. Examples of the thermal polymerization inhibitor include hydroquinone, 4-methoxyphenol, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-cresol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt.
[0094] The content of the thermal polymerization inhibitor is not particularly limited, but is preferably in the range of 0.005 to 12 parts by mass per 100 parts by mass of the reaction product.
[0095] <<Azole Compounds>> For example, when a substrate made of copper or a copper alloy is used, an azole compound can be optionally blended into the photosensitive resin composition to suppress discoloration of the substrate. Examples of the azole compound include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-t-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-benzotriazole, and the like. benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)benzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxy-1H-benzotriazole, 5-carboxy-1H-benzotriazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, 1-methyl-1H-tetrazole, etc. Particularly preferred are tolyltriazole, 5-methyl-1H-benzotriazole, and 4-methyl-1H-benzotriazole. These azole compounds may be used alone or in combination of two or more.
[0096] The content of the azole compound is not particularly limited, but is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the reaction product, and more preferably 0.5 to 5 parts by mass from the viewpoint of photosensitivity characteristics. When the content of the azole compound relative to 100 parts by mass of the reaction product is 0.1 part by mass or more, discoloration of the copper or copper alloy surface is suppressed when the photosensitive resin composition is formed on copper or a copper alloy, while when the content is 20 parts by mass or less, excellent photosensitivity is achieved, which is preferable.
[0097] <<Hindered Phenol Compound>> In an embodiment, a hindered phenol compound can be optionally blended into the photosensitive resin composition to suppress discoloration on copper. Examples of the hindered phenol compound include 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thio-bis(3-methyl-6-t-butylphenol), 4,4'-butylidene-bis(3-methyl-6-t-butylphenol), and 4,4'-butylidene-bis(3-methyl-6-t-butylphenol). N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 2,2'-methylene- Bis(4-methyl-6-t-butylphenol), 2,2'-methylene-bis(4-ethyl-6-t-butylphenol), pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4- isopropylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-s-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4- t-butyl-3-hydroxy-2,5,6-trimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H ,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl) Examples of the hydroxybenzoates include, but are not limited to, 1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione. Among these, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione is particularly preferred.
[0098] The content of the hindered phenol compound is not particularly limited, but is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the reaction product, and more preferably 0.5 to 10 parts by mass from the viewpoint of photosensitivity characteristics. When the content of the hindered phenol compound relative to 100 parts by mass of the reaction product is 0.1 part by mass or more, for example, when the photosensitive resin composition is formed on copper or a copper alloy, discoloration and corrosion of the copper or copper alloy are prevented, while when the content is 20 parts by mass or less, excellent photosensitivity is achieved, which is preferable.
[0099] The photosensitive resin composition can be suitably used as a negative photosensitive resin composition for producing a cured relief pattern, which will be described later.
[0100] (Resin Film) The resin film of the present invention is a baked product of a coating film of the photosensitive resin composition of the present invention. Examples of coating methods include those conventionally used for coating photosensitive resin compositions, such as coating with a spin coater, bar coater, blade coater, curtain coater, or screen printer, and spray coating with a spray coater. Various methods can be selected for the baking method used to obtain the baked product, including, for example, using a hot plate, an oven, or a temperature-programmable heating oven. Baking can be performed, for example, at 130°C to 250°C for 30 minutes to 5 hours. Air may be used as the atmospheric gas during heat curing, or an inert gas such as nitrogen or argon can also be used. The thickness of the resin film is not particularly limited, but is preferably 1 μm to 100 μm, and more preferably 2 μm to 50 μm. The resin film is, for example, an insulating film.
[0101] (Photosensitive Resist Film) The photosensitive resin composition of the present invention can be used for a photosensitive resist film (so-called dry film resist). The photosensitive resist film has a substrate film, a photosensitive resin layer (photosensitive resin film) formed from the photosensitive resin composition of the present invention, and a cover film. Usually, the photosensitive resin layer and the cover film are laminated in this order on the substrate film.
[0102] The photosensitive resist film can be produced, for example, by applying a photosensitive resin composition to a substrate film, drying the composition to form a photosensitive resin layer, and then laminating a cover film on the photosensitive resin layer. The application method can be a conventional method used to apply a photosensitive resin composition, such as using a spin coater, bar coater, blade coater, curtain coater, or screen printer, or spray coating with a spray coater. Drying can be performed, for example, at 20°C to 200°C for 1 minute to 1 hour. The thickness of the resulting photosensitive resin layer is not particularly limited, but is preferably 1 μm to 100 μm, and more preferably 2 μm to 50 μm.
[0103] Known materials can be used for the base film, such as a thermoplastic resin film. Examples of such thermoplastic resins include polyesters such as polyethylene terephthalate. The thickness of the base film is preferably 2 μm to 150 μm. Known materials can be used for the cover film, such as a polyethylene film or a polypropylene film. The cover film is preferably a film that has a lower adhesive strength with the photosensitive resin layer than the base film. The thickness of the cover film is preferably 2 μm to 150 μm, more preferably 2 μm to 100 μm, and particularly preferably 5 μm to 50 μm. The base film and the cover film may be made of the same film material, or different films may be used.
[0104] (Method for manufacturing a substrate having a cured relief pattern) The method for manufacturing a substrate having a cured relief pattern of the present invention includes the steps of: (1) applying the photosensitive resin composition of the present invention onto a substrate to form a photosensitive resin layer (photosensitive resin film) on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; and (4) heat-treating the relief pattern to form a cured relief pattern.
[0105] Each step will be described below.
[0106] (1) Step of applying the photosensitive resin composition of the present invention onto a substrate to form a photosensitive resin layer on the substrate In this step, the photosensitive resin composition of the present invention is applied onto a substrate, and then dried as necessary to form a photosensitive resin layer. As the application method, a method conventionally used for applying a photosensitive resin composition can be used, such as a method of applying using a spin coater, bar coater, blade coater, curtain coater, screen printing machine, etc., or a method of spray application using a spray coater, etc.
[0107] If necessary, the coating film made of the photosensitive resin composition can be dried, and examples of the drying method include air drying, heat drying using an oven or a hot plate, vacuum drying, etc. Specifically, when air drying or heat drying is performed, drying can be carried out under conditions of 20°C to 200°C for 1 minute to 1 hour. In this manner, a photosensitive resin layer can be formed on the substrate.
[0108] (2) Step of Exposing the Photosensitive Resin Layer In this step, the photosensitive resin layer formed in step (1) above is exposed to an ultraviolet light source or the like using an exposure device such as a contact aligner, mirror projection, or stepper, either directly or through a patterned photomask or reticle. Examples of light sources used for exposure include g-line, h-line, i-line, ghi-line broadband, and KrF excimer laser. The exposure dose is 25 mJ / cm. 2 ~2000mJ / cm 2 is desirable.
[0109] Thereafter, post-exposure baking (PEB) and / or pre-development baking may be performed at any combination of temperature and time, as necessary, for the purpose of improving photosensitivity, etc. The baking conditions are preferably in the range of a temperature of 50°C to 200°C and a time of 10 seconds to 600 seconds, but are not limited to these ranges as long as they do not impair the properties of the photosensitive resin composition.
[0110] (3) Step of Developing the Exposed Photosensitive Resin Layer to Form a Relief Pattern In this step, the unexposed portions of the exposed photosensitive resin layer are developed and removed. The development method for developing the exposed (irradiated) photosensitive resin layer can be any of the conventional photoresist development methods, such as the rotary spray method, the paddle method, and the immersion method accompanied by ultrasonic treatment. After development, rinsing may be performed to remove the developer. Furthermore, post-development baking may be performed at any temperature and time combination, as needed, for purposes such as adjusting the shape of the relief pattern. The developer used for development is preferably an organic solvent. Examples of preferred organic solvents include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, γ-butyrolactone, and α-acetyl-γ-butyrolactone. Two or more of each solvent, for example, a combination of several solvents, may also be used. The rinse solution used for rinsing is preferably an organic solvent that is miscible with the developer and has low solubility in the photosensitive resin composition. Examples of preferred rinse solutions include methanol, ethanol, isopropyl alcohol, ethyl lactate, propylene glycol methyl ether acetate, toluene, and xylene. Two or more of each solvent, for example, a combination of several types, can also be used.
[0111] (4) Step of Heating the Relief Pattern to Form a Cured Relief Pattern In this step, the relief pattern obtained by the development described above is heated to convert it into a cured relief pattern. When the reaction product is a polyamic acid, this heating causes thermal imidization, resulting in a cured relief pattern containing polyimide. Various methods can be selected for heat curing, such as using a hot plate, an oven, or a temperature-programmable heating oven. Heating can be performed, for example, at 130°C to 250°C for 30 minutes to 5 hours. The atmospheric gas used during heat curing may be air, or an inert gas such as nitrogen or argon.
[0112] The thickness of the cured relief pattern is not particularly limited, but is preferably 1 μm to 100 μm, and more preferably 2 μm to 50 μm.
[0113] (Semiconductor Device) In an embodiment, a semiconductor device is also provided, comprising a semiconductor element and a cured film provided on or below the semiconductor element. The cured film is a cured relief pattern formed from the photosensitive resin composition of the present invention. The cured relief pattern can be obtained, for example, by steps (1) to (4) in the above-described method for manufacturing a substrate having a cured relief pattern. The present invention is also applicable to a method for manufacturing a semiconductor device that uses a semiconductor element as a substrate and includes the above-described method for manufacturing a substrate having a cured relief pattern as part of its processes. The semiconductor device of the present invention can be manufactured by forming a cured relief pattern as a surface protective film, an interlayer insulating film, an insulating film for rewiring, a protective film for a flip-chip device, or a protective film for a semiconductor device having a bump structure, and combining this with a known method for manufacturing a semiconductor device.
[0114] (Display Device) In an embodiment, a display device is provided that includes a display element and a cured film provided on the display element, the cured film having the above-described cured relief pattern. Here, the cured relief pattern may be laminated in direct contact with the display element, or may be laminated with another layer sandwiched therebetween. Examples of the cured film include surface protection films, insulating films, and planarizing films for TFT (Thin Film Transistor) liquid crystal display elements and color filter elements, protrusions for MVA (Multi-Domain Vertical Alignment) liquid crystal display devices, and partition walls for cathodes of organic EL (Electro-Luminescence) elements.
[0115] The photosensitive resin composition of the present invention is useful not only for application to the semiconductor devices described above, but also for applications such as an interlayer insulating film for a multilayer circuit, a cover coat for a flexible copper-clad board, a solder resist film, and a liquid crystal alignment film.
[0116] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples.
[0117] The weight average molecular weights (Mw) shown in the following synthesis examples are the results of measurement by gel permeation chromatography (hereinafter abbreviated as GPC in this specification). For the measurement, a GPC device (HLC-8320GPC (manufactured by Tosoh Corporation)) was used, and the measurement conditions were as follows: Column: Shodex (registered trademark) KD-805 / Shodex (registered trademark) KD-803 (manufactured by Showa Denko K.K.) Column temperature: 50°C Flow rate: 1 mL / min Eluent: N,N-dimethylformamide (DMF), lithium bromide monohydrate (30 mM) / phosphoric acid (30 mM) / tetrahydrofuran (1%) Standard sample: polyethylene oxide
[0118] The chemical imidization ratio shown in the synthesis examples below was calculated by the following method. 100 mg of polyimide powder was placed in an NMR sample tube (NMR sampling tube standard, φ5 (Kusano Scientific Co., Ltd.)), and deuterated dimethyl sulfoxide (DMSO-d6, 0.05% TMS (tetramethylsilane) mixture) (0.53 ml) was added. Complete dissolution was achieved by applying ultrasound. This solution was subjected to 500 MHz proton NMR measurement using an NMR measurement device (JNM-ECA500) (JEOL Ltd.). The chemical imidization ratio was calculated by the following formula, using a proton derived from a structure that remains unchanged before and after imidization as the reference proton, and the integrated value of the peak of this proton and the integrated value of the proton peak derived from the NH group of the amic acid that appears around 9.5 ppm to 11.0 ppm. Chemical imidization rate (%)=(1−α×x / y)×100 In the above formula, x is the integrated value of the proton peak derived from the NH group of the amic acid, y is the integrated value of the peak of the reference proton, and α is the ratio of the number of reference protons to one NH group proton of the amic acid in the case of polyamic acid (imidization rate 0%).
[0119] Synthesis Example 1 Synthesis of Polyamic Acid (P-1) 11.00 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 0.05 g of 2,6-di-tert-butyl-p-cresol, and 33.14 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 21.45 g of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride and 42.68 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 1 hour and then at 60° C. for 93 hours. The resulting polyamic acid had a repeating unit structure represented by the following (P-1), and its weight average molecular weight (Mw) measured by GPC in terms of polystyrene was 22,868.
[0120] Synthesis Example 2 Synthesis of Polyamic Acid (P-2) 9.85 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 12.84 g of 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, 0.04 g of 2,6-di-tert-butyl-p-cresol, and 53.04 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 37.25 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride and 86.91 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 50° C. for 89 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-2), and had a weight average molecular weight (Mw) of 25,273 as measured by GPC in terms of polystyrene.
[0121] Synthesis Example 3 Synthesis of Polyamic Acid (P-3) 10.18 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 11.26 g of 1,4-bis(4-aminophenoxy)benzene, 0.04 g of 2,6-di-tert-butyl-p-cresol, and 50.13 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 38.49 g of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride and 89.82 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 50° C. for 89 hours. The resulting polyamic acid had a repeating unit structure represented by the following (P-3), and its weight average molecular weight (Mw) measured by GPC in terms of polystyrene was 26,998.
[0122] Synthesis Example 4 Synthesis of Polyamic Acid (P-4) 13.73 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 9.14 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.06 g of 2,6-di-tert-butyl-p-cresol, and 53.50 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 37.08 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride and 86.53 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 2 hours and then at 50° C. for 88 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-4), and had a weight average molecular weight (Mw) of 24,973 as measured by GPC in terms of polystyrene.
[0123] Synthesis Example 5 Synthesis of Polyamic Acid (P-5) 9.47 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 14.70 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.04 g of 2,6-di-tert-butyl-p-cresol, and 56.49 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 35.79 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride and 83.51 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 50° C. for 89 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-5), and had a weight average molecular weight (Mw) of 27,852 as measured by GPC in terms of polystyrene.
[0124] Synthesis Example 6 Synthesis of Polyamic Acid (P-6) 3.59 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 13.01 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.01 g of 2,6-di-tert-butyl-p-cresol, and 66.47 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 23.33 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride and 93.33 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 50° C. for 95 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-6), and had a weight average molecular weight (Mw) of 56,737 as converted into polystyrene by GPC.
[0125] Synthesis Example 7 Synthesis of Polyamic Acid (P-7) 1.16 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 16.22 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.01 g of 2,6-di-tert-butyl-p-cresol, and 69.53 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature in air, and then 22.62 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride and 90.47 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 50° C. for 95 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-7), and had a weight average molecular weight (Mw) of 58,225 as measured by GPC in terms of polystyrene.
[0126] Synthesis Example 8 Synthesis of Polyamic Acid (P-8) 9.71 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 13.54 g of 4,4′-bis(4-aminophenoxy)biphenyl, 0.04 g of 2,6-di-tert-butyl-p-cresol, and 54.34 g of N-ethyl-2-pyrrolidone were stirred at room temperature in air to dissolve, and then 36.72 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride and 85.67 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 50° C. for 92 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-8), and had a weight average molecular weight (Mw) of 33,012 as measured by GPC in terms of polystyrene.
[0127] Synthesis Example 9 Synthesis of Polyamic Acid (P-9) 6.22 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 10.18 g of bis[4-(4-aminophenoxy)phenyl]sulfone, 0.03 g of 2,6-di-tert-butyl-p-cresol, and 65.70 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature in air, and then 23.52 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride and 94.08 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 2 hours and then at 50° C. for 92 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-9), and had a weight average molecular weight (Mw) of 31,175 as measured by GPC in terms of polystyrene.
[0128] Synthesis Example 10 Synthesis of Polyamic Acid (P-10) 6.62 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 13.34 g of 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene (BPF-AN, manufactured by JFE Chemical Corporation), and 79.86 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 25.04 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride and 25.14 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 40° C. for 42 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-10), and had a weight average molecular weight (Mw) of 25,249 as measured by GPC in terms of polystyrene.
[0129] Synthesis Example 11 Synthesis of Polyamic Acid (P-11) 7.94 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 10.46 g of bis(4-aminophenyl) terephthalate, 0.05 g of 4-methoxyphenol, and 87.05 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 29.98 g of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride and 58.04 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 50° C. for 74 hours. The resulting polyamic acid had a repeating unit structure represented by the following (P-11), and had a weight average molecular weight (Mw) of 29,792 as measured by GPC in terms of polystyrene.
[0130] Synthesis Example 12 Synthesis of Polyamic Acid (P-12) 7.94 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 10.46 g of 1,4-phenylenebis(4-aminobenzoate), 0.05 g of 4-methoxyphenol, and 87.05 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 29.98 g of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride and 58.04 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 50° C. for 74 hours. The resulting polyamic acid had a repeating unit structure represented by the following (P-12), and had a weight average molecular weight (Mw) of 24,660 as measured by GPC relative to polystyrene standards.
[0131] Synthesis Example 13 Synthesis of Polyamic Acid (P-13) 10.95 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 17.01 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.05 g of 2,6-di-tert-butyl-p-cresol, and 112.00 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 32.00 g of hydroquinone diphthalic anhydride (HQDA, manufactured by Air Water Inc.) and 28.00 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 2 hours and then at 40° C. for 39 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-13), and had a weight average molecular weight (Mw) of 21,092 as measured by GPC in terms of polystyrene.
[0132] Synthesis Example 14 Synthesis of Polyamic Acid (P-14) 8.63 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 13.41 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.04 g of 2,6-di-tert-butyl-p-cresol, and 88.32 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature in air, and then 37.92 g of bis-(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)propane-2,2-diylbis(2-methyl-4,1-phenylene) and 51.68 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 2 hours and then at 40° C. for 39 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-14), and had a weight average molecular weight (Mw) of 16,379 as measured by GPC in terms of polystyrene.
[0133] Synthesis Example 15 Synthesis of Polyamic Acid (P-15) 6.23 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 9.68 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and 63.64 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 29.09 g of 9,9-bis[4-(3,4-dicarboxyphenoxy)phenylfluorenedioic anhydride (BPF-PA, manufactured by JFE Chemical Corporation) and 41.36 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 40° C. for 42 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-15), and had a weight average molecular weight (Mw) of 24,559 as measured by GPC in terms of polystyrene.
[0134] Synthesis Example 16 Synthesis of Polyamic Acid (P-16) 5.29 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 10.36 g of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 0.04 g of 4-methoxyphenol, and 65.87 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 24.68 g of 9,9-bis[4-(3,4-dicarboxyphenoxy)phenylfluorenedioic anhydride (BPF-PA, manufactured by JFE Chemical Corporation) and 28.23 g of N-ethyl-2-pyrrolidone were added to the system, and the mixture was stirred at room temperature for 4 hours and then at 50° C. for 26.5 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-16), and had a weight average molecular weight (Mw) of 28,330 as measured by GPC in terms of polystyrene.
[0135] Synthesis Example 17 Synthesis of Polyamic Acid (P-17) 6.181 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 9.60 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.04 g of 4-methoxyphenol, and 79.65 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature in air, and then 24.0 g of 5-isobenzofurancarboxylic acid, 1,3-dihydro-1,3-dioxo-cyclohexylidene-4,1-phenylene ester (BPZ-TME, manufactured by Honshu Chemical Industry Co., Ltd.) and 39.82 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 1 hour and then at 50° C. for 63 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-17), and had a weight average molecular weight (Mw) of 13,550 as measured by GPC in terms of polystyrene.
[0136] Synthesis Example 18 Synthesis of Polyamic Acid (P-18) 8.65 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 13.44 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.053 g of 4-methoxyphenol, and 105.62 g of N-ethyl-2-pyrrolidone were dissolved by stirring under air at room temperature, and then 15.0 g of p-phenylenebis(trimellitate anhydride) (TAHQ, manufactured by Manac Corporation), 15.67 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride, and 52.81 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 1 hour and then at 50° C. for 40 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-18), and had a weight average molecular weight (Mw) of 36,287 as converted into polystyrene by GPC.
[0137] Synthesis Example 19 Synthesis of Polyamic Acid (P-19) 8.65 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 13.44 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.054 g of 4-methoxyphenol, and 107.24 g of N-ethyl-2-pyrrolidone were dissolved by stirring under air at room temperature, and then 9.0 g of p-phenylenebis(trimellitate anhydride) (TAHQ, manufactured by Manac Corporation), 22.49 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride, and 53.62 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 1 hour and then at 50° C. for 40 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-19), and had a weight average molecular weight (Mw) of 34,006 as measured by GPC in terms of polystyrene.
[0138] Synthesis Example 20 Synthesis of Polyamic Acid (P-20) 7.418 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 11.52 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.047 g of 4-methoxyphenol, and 126.47 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 15.0 g of p-biphenylenebis(trimellitic acid monoester anhydride) (BP-TME, manufactured by Honshu Chemical Co., Ltd.), 13.44 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride, and 63.23 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 1 hour and then at 50° C. for 40 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-20), and had a weight average molecular weight (Mw) of 28,962 as measured by GPC in terms of polystyrene.
[0139] Synthesis Example 21 Synthesis of Polyamic Acid (P-21) 7.418 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 11.52 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 0.047 g of 4-methoxyphenol, and 126.47 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature in air, and then 9.0 g of p-biphenylenebis(trimellitic acid monoester anhydride) (BP-TME, manufactured by Honshu Chemical Co., Ltd.), 19.28 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride, and 63.23 g of N-ethyl-2-pyrrolidone were added to the system, and the mixture was stirred at room temperature for 1 hour and then at 50° C. for 40 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-21), and had a weight average molecular weight (Mw) of 26,182 as measured by GPC in terms of polystyrene.
[0140] Synthesis Example 22: Synthesis of Solvent-Soluble Polyimide (P-22) 80.42 g of N-ethyl-2-pyrrolidone, 3.66 g of acetic anhydride, and 0.61 g of triethylamine were added to 40.21 g of the polyamic acid (P-16) obtained in Synthesis Example 16. The mixture was stirred in air at room temperature for 30 minutes, followed by stirring at 60°C for 3 hours. This solution was slowly added to 437.15 g of stirring methanol, and the mixture was stirred for 10 minutes. The resulting precipitate was filtered off. The precipitate was washed with 874.30 g of methanol and then dried under reduced pressure at 80°C to obtain a solvent-soluble polyimide powder having the repeating unit structure represented by the following formula (P-22). The chemical imidization rate was 95.3%.
[0141] Synthesis Example 23 Synthesis of Solvent-Soluble Polyimide (P-23) 9.51 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 18.66 g of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 0.06 g of 4-methoxyphenol, and 98.06 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 23.99 g of 4,4′-(hexafluoroisopropylidene)diphthalic anhydride, 7.87 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride, and 42.03 g of N-ethyl-2-pyrrolidone were added to the system, and the mixture was stirred at room temperature for 2 hours and then at 50° C. for 24 hours. The weight average molecular weight (Mw) measured by GPC in terms of polystyrene was 29,468. To 50.00 g of the resulting polyamic acid, 100.00 g of N-ethyl-2-pyrrolidone, 5.51 g of acetic anhydride, and 0.91 g of triethylamine were added, and the mixture was stirred in air at room temperature for 30 minutes, followed by stirring at 60°C for 3 hours. This solution was slowly added to 547.47 g of stirring methanol, and the mixture was stirred for 10 minutes. The resulting precipitate was filtered off. The precipitate was washed with 1094.94 g of methanol and then dried under reduced pressure at 80°C to obtain a solvent-soluble polyimide powder having the repeating unit structure represented by the following (P-23). The chemical imidization rate was 95.3%.
[0142] Synthesis Example 24 Synthesis of Solvent-Soluble Polyimide (P-24) 9.25 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 18.15 g of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 0.06 g of 4-methoxyphenol, and 97.52 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 15.55 g of 4,4′-(hexafluoroisopropylidene)diphthalic anhydride, 16.76 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride, and 41.79 g of N-ethyl-2-pyrrolidone were added to the system, and the mixture was stirred at room temperature for 2 hours and then at 50° C. for 24 hours. The weight average molecular weight (Mw) measured by GPC in terms of polystyrene was 30,055. To 50.00 g of the resulting polyamic acid, 100.00 g of N-ethyl-2-pyrrolidone, 5.39 g of acetic anhydride, and 0.89 g of triethylamine were added, and the mixture was stirred in air at room temperature for 30 minutes, followed by stirring at 60°C for 3 hours. This solution was slowly added to 546.97 g of stirring methanol, and the mixture was stirred for 10 minutes. The resulting precipitate was filtered off. The precipitate was washed with 1093.94 g of methanol and then dried under reduced pressure at 80°C to obtain a solvent-soluble polyimide powder having the repeating unit structure represented by the following (P-24). The chemical imidization rate was 95.3%.
[0143] Comparative Synthesis Example 1 Synthesis of Polyamic Acid (P-25) 30.00 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 0.13 g of 2,6-di-tert-butyl-p-cresol, and 90.38 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 24.51 g of pyromellitic anhydride and 37.11 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 13 hours and then at 80° C. for 51 hours. The resulting polyamic acid had a repeating unit structure represented by the following (P-25), and had a weight average molecular weight (Mw) of 10,579 as measured by GPC in terms of polystyrene.
[0144] Comparative Synthesis Example 2 Synthesis of Polyamic Acid (P-26) 42.28 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 0.09 g of 4-methoxyphenol, and 144.42 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature in air, and then 46.13 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride and 61.89 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 1 hour and then at 80° C. for 75 hours. A polyamic acid having the repeating unit structure represented by the following (P-26) was obtained.
[0145] Comparative Synthesis Example 3 Synthesis of Polyamic Acid (P-27) 31.71 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 0.09 g of 4-methoxyphenol, and 137.13 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 52.24 g of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride and 58.77 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 3 hours and then at 80°C for 75 hours. A polyamic acid having the repeating unit structure represented by the following (P-27) was obtained.
[0146] Comparative Synthesis Example 4 Synthesis of Polyamic Acid (P-28) 18.00 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 0.08 g of 2,6-di-tert-butyl-p-cresol, and 54.23 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 13.22 g of 1,2,3,4-cyclobutanetetracarboxylic acid dianhydride and 30.40 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 62 hours and then at 40° C. for 34 hours. The resulting polyamic acid had a repeating unit structure represented by the following (P-28), and had a weight average molecular weight (Mw) of 42,930 as measured by GPC relative to polystyrene standards.
[0147] Comparative Synthesis Example 5 Synthesis of Polyamic Acid (P-29) 15.00 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 0.06 g of 2,6-di-tert-butyl-p-cresol, and 45.19 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 17.21 g of 1,1′-bicyclohexane-3,3′,4,4′-tetracarboxylic acid-3,3′,4,4′-dianhydride (BPDA-H, manufactured by Iwatani Industrial Gases Corporation) and 30.12 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 62 hours and then at 40° C. for 34 hours. The resulting polyamic acid had a repeating unit structure represented by the following formula (P-29), and had a weight average molecular weight (Mw) of 45,136 as converted into polystyrene by GPC.
[0148] Comparative Synthesis Example 6 Synthesis of Solvent-Soluble Polyimide (P-30) 8.60 g of 2-(methacryloyloxy)ethyl 3,5-diaminobenzoate (BEM-S, manufactured by Wako Pure Chemical Industries, Ltd.), 16.85 g of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 0.05 g of 4-methoxyphenol, and 148.85 g of N-ethyl-2-pyrrolidone were dissolved by stirring at room temperature under air, and then 27.72 g of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride and 63.79 g of N-ethyl-2-pyrrolidone were added to the system, followed by stirring at room temperature for 1 hour and then at 50°C for 87 hours. The weight average molecular weight (Mw) of the resulting polyamic acid, measured in terms of polystyrene by GPC, was 27,335. To 60.00 g of the resulting polyamic acid, 60.00 g of N-ethyl-2-pyrrolidone, 4.49 g of acetic anhydride, and 0.58 g of pyridine were added, and the mixture was stirred in air at room temperature for 30 minutes, followed by stirring at 50°C for 3 hours. This solution was slowly added to 437.76 g of stirring methanol, and the mixture was stirred for 10 minutes. The resulting precipitate was filtered off. The precipitate was washed with 875.52 g of methanol and then dried under reduced pressure at 60°C to obtain a solvent-soluble polyimide powder having the repeating unit structure represented by the following formula (P-30). The chemical imidization rate was 93.2%.
[0149] Example 1 27.75 g of a solution (solids concentration: 30% by weight) containing the polyamic acid (P-1) obtained in Synthesis Example 1, 1.67 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.42 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.17 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and then filtered using a polypropylene filter with a pore size of 5 μm to prepare a solution of a negative photosensitive resin composition.
[0150] Example 2 32.24 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-2) obtained in Synthesis Example 2, 1.93 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.48 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert- 0.15 g of (butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Japan Ltd., and 0.19 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0151] Example 3 33.16 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-2) obtained in Synthesis Example 2, 1.93 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.48 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.48 g of IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)phenyl) as a photopolymerizable copolymer were mixed. 0.15 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.19 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0152] Example 4 22.08 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-3) obtained in Synthesis Example 3, 1.32 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.33 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzoyl)) were mixed together. A solution of a negative photosensitive resin composition was prepared by mixing and dissolving 0.10 g of (dibenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.), 0.13 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) and 11.04 g of N-ethyl-2-pyrrolidone, and then filtering the solution using a polypropylene filter having a pore size of 5 μm.
[0153] Example 5 32.49 g of a solution (solid content concentration: 30% by weight) containing the polyamic acid (P-3) obtained in Synthesis Example 3, 0.97 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.49 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.49 g of IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzoyl)) as a photopolymerizable copolymer were mixed. A solution of a negative photosensitive resin composition was prepared by mixing and dissolving 0.15 g of (acryloxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Japan Ltd., 0.19 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.), and 0.71 g of N-ethyl-2-pyrrolidone, and then filtering the solution using a polypropylene filter having a pore size of 5 μm.
[0154] Example 6 33.16 g of a solution (solid content concentration: 30% by weight) containing the polyamic acid (P-4) obtained in Synthesis Example 4, 0.99 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.50 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl)methyl) as a photopolymerizable copolymer were mixed. 0.15 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.20 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0155] Example 7 29.96 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-5) obtained in Synthesis Example 5, 1.80 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.45 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzoyl)) were mixed together. A solution of a negative photosensitive resin composition was prepared by mixing and dissolving 0.13 g of (dibenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.), 0.18 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) and 2.48 g of N-ethyl-2-pyrrolidone, and then filtering the solution using a polypropylene filter having a pore size of 5 μm.
[0156] Example 8 23.89 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-5) obtained in Synthesis Example 5, 0.72 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.36 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzoyl)) were mixed together. A solution of a negative photosensitive resin composition was prepared by mixing and dissolving 0.11 g of (acryloxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.), 0.14 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) and 4.78 g of N-ethyl-2-pyrrolidone, and then filtering the solution using a polypropylene filter having a pore size of 5 μm.
[0157] Example 9 37.84 g of a solution (solid content: 20% by weight) containing the polyamic acid (P-6) obtained in Synthesis Example 6, 1.51 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.38 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.38 g of IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)propanol) as a photopolymerizable copolymer were mixed together. A solution of a negative photosensitive resin composition was prepared by mixing and dissolving 0.11 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.15 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) and then filtering the solution using a polypropylene filter having a pore size of 5 μm.
[0158] Example 10 37.84 g of a solution (solid content: 20% by weight) containing the polyamic acid (P-7) obtained in Synthesis Example 7, 1.51 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.38 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert- 0.11 g of (butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Japan Ltd., and 0.15 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0159] Example 11 22.08 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-8) obtained in Synthesis Example 8, 1.32 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.33 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzoyl)) were mixed together. A solution of a negative photosensitive resin composition was prepared by mixing and dissolving 0.10 g of (dibenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.), 0.13 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) and 11.04 g of N-ethyl-2-pyrrolidone, and then filtering the solution using a polypropylene filter having a pore size of 5 μm.
[0160] Example 12 31.50 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-8) obtained in Synthesis Example 8, 0.95 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.47 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.47 g of IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzoyl)) as a photopolymerizable copolymer were mixed. A solution of a negative photosensitive resin composition was prepared by mixing and dissolving 0.14 g of (acryloxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Japan Ltd., 0.19 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.), and 1.75 g of N-ethyl-2-pyrrolidone, and then filtering the solution using a polypropylene filter having a pore size of 5 μm.
[0161] Example 13 33.11 g of a solution (solid content: 20% by weight) containing the polyamic acid (P-9) obtained in Synthesis Example 9, 1.32 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.33 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert- 0.10 g of (butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Japan Ltd., and 0.13 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0162] Example 14 20.75 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-10) obtained in Synthesis Example 10, 1.25 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.31 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.31 g of IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzoyl)methyl) as a photopolymerizable copolymer were mixed together. A solution of a negative photosensitive resin composition was prepared by mixing and dissolving 0.09 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.), 0.12 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) and 2.47 g of N-ethyl-2-pyrrolidone, and then filtering the solution using a polypropylene filter having a pore size of 5 μm.
[0163] Example 15 23.66 g of a solution (solid content: 25% by weight) containing the polyamic acid (P-11) obtained in Synthesis Example 11, 0.99 g of N-ethyl-2-pyrrolidone, 0.59 g of NK ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.30 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl)methyl) as a photopolymerizable copolymer were mixed. 0.09 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.12 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0164] Example 16 24.78 g of a solution (solid content: 25% by weight) containing the polyamic acid (P-12) obtained in Synthesis Example 12, 0.62 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.31 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl) 0.09 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.12 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0165] Example 17 27.64 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-13) obtained in Synthesis Example 13, 1.66 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.41 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert- 0.12 g of (butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Japan Ltd., and 0.17 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0166] Example 18 28.42 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-13) obtained in Synthesis Example 13, 0.85 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.43 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.43 g of IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)phenyl) as a photopolymerizable copolymer were mixed. 0.13 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.17 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0167] Example 19 27.64 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-14) obtained in Synthesis Example 14, 1.66 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.41 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert- 0.12 g of (butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Japan Ltd., and 0.17 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0168] Example 20 28.42 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-14) obtained in Synthesis Example 14, 0.85 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.43 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl) 0.13 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.17 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0169] Example 21 21.40 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-15) obtained in Synthesis Example 15, 1.28 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.32 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzoyl)) were mixed together. A solution of a negative photosensitive resin composition was prepared by mixing and dissolving 0.10 g of (dibenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.), 0.13 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) and 1.77 g of N-ethyl-2-pyrrolidone, and then filtering the solution using a polypropylene filter having a pore size of 5 μm.
[0170] Example 22 37.81 g of a solution (solid content: 30% by weight) containing the polyamic acid (P-16) obtained in Synthesis Example 16, 2.27 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.57 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl) 0.17 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.23 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0171] Example 23 65.34 g of a solution (solid content: 25% by weight) containing the polyamic acid (P-17) obtained in Synthesis Example 17, 3.27 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.82 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.82 g of IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert- 0.25 g of (butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Japan Ltd., and 0.33 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0172] Example 24 38.23 g of a solution (solid content: 25% by weight) containing the polyamic acid (P-18) obtained in Synthesis Example 18, 0.96 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.48 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl) 0.14 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.19 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0173] Example 25 38.23 g of a solution (solid content: 25% by weight) containing the polyamic acid (P-19) obtained in Synthesis Example 19, 0.96 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.48 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl) 0.14 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.19 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0174] Example 26 38.57 g of a solution (solid content: 20% by weight) containing the polyamic acid (P-20) obtained in Synthesis Example 20, 0.77 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.39 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl) 0.12 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.15 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0175] Example 27 38.57 g of a solution (solid content: 20% by weight) containing the polyamic acid (P-21) obtained in Synthesis Example 21, 0.77 g of NK Ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.39 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl) 0.12 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.15 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0176] Example 28 11.02 g of the powder of the solvent-soluble polyimide (P-22) obtained in Synthesis Example 22, 25.71 g of N-ethyl-2-pyrrolidone, 2.20 g of NK ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.55 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl) 0.17 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.22 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0177] Example 29 10.89 g of the powder of the solvent-soluble polyimide (P-23) obtained in Synthesis Example 23, 26.00 g of N-ethyl-2-pyrrolidone, 2.18 g of NK ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.54 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl)methyl) as a photopolymer were mixed together. 0.16 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.22 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0178] Example 30 10.89 g of the powder of the solvent-soluble polyimide (P-24) obtained in Synthesis Example 24, 26.00 g of N-ethyl-2-pyrrolidone, 2.18 g of NK ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.54 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl)methyl) as a photopolymerizable copolymer were mixed together. 0.16 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.22 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0179] Comparative Example 1 27.75 g of a solution (solids concentration: 30% by weight) containing the polyamic acid (P-25) obtained in Comparative Synthesis Example 1, 1.67 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.42 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.17 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and then filtered using a polypropylene filter with a pore size of 5 μm to prepare a solution of a negative photosensitive resin composition.
[0180] Comparative Example 2 26.17 g of a solution (solids concentration: 30% by weight) containing the polyamic acid (P-26) obtained in Comparative Synthesis Example 2, 1.57 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.39 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.16 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the mixture was filtered using a polypropylene filter having a pore size of 5 μm to prepare a solution of a negative photosensitive resin composition.
[0181] Comparative Example 3 25.08 g of a solution (solids concentration: 30% by weight) containing the polyamic acid (P-27) obtained in Comparative Synthesis Example 3, 1.50 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.38 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.15 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and then filtered using a polypropylene filter with a pore size of 5 μm to prepare a solution of a negative photosensitive resin composition.
[0182] Comparative Example 4 27.96 g of a solution (solids concentration: 27 wt %) containing the polyamic acid (P-28) obtained in Comparative Synthesis Example 4, 1.51 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.38 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.15 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the mixture was filtered using a polypropylene filter having a pore size of 5 μm to prepare a solution of a negative photosensitive resin composition.
[0183] Comparative Example 5 27.75 g of a solution (solids concentration: 30% by weight) containing the polyamic acid (P-29) obtained in Comparative Synthesis Example 5, 1.67 g of NK Ester A-200 (polyethylene glycol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.42 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and 0.17 g of KBM-5103 (3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the mixture was filtered using a polypropylene filter having a pore size of 5 μm to prepare a solution of a negative photosensitive resin composition.
[0184] Comparative Example 6 9.14 g of the powder of the solvent-soluble polyimide (P-30) obtained in Comparative Synthesis Example 6, 16.98 g of N-ethyl-2-pyrrolidone, 1.83 g of NK ester A-DOD-N (1,10-decanediol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent, 0.46 g of IRGACURE [registered trademark] OXE01 (1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], manufactured by BASF Japan Ltd.) as a photoradical initiator, and IRGANOX [registered trademark] 3114 (1,3,5-tris(3,5-di-tert-butyl)methyl)methyl) as a photopolymerizable copolymer were mixed. 0.14 g of (1H,3H,5H)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by BASF Japan Ltd.) and 0.18 g of KBM-5103 (3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and dissolved, and the solution was filtered using a polypropylene filter having a pore size of 5 μm, to prepare a solution of a negative photosensitive resin composition.
[0185] [Photosensitivity Evaluation] The negative photosensitive resin compositions prepared in Examples 1 to 30 and Comparative Examples 1 to 6 were applied to 8-inch silicon wafers using a spin coater (CLEAN TRACK ACT-8, manufactured by Tokyo Electron Limited) and baked at 115°C for 180 seconds or 270 seconds to form photosensitive resin films with a thickness of 5 to 15 μm on the wafers. Next, the films were exposed using an i-line stepper (NSR-2205i12D, manufactured by Nikon Corporation). Furthermore, using an automatic developing apparatus (AD-1200, manufactured by Mikasa Co., Ltd.), the films were spray-developed for 20 to 240 seconds using cyclopentanone as a developer, and then spray-rinsed with propylene glycol monomethyl ether acetate (PGMEA) as a rinse for 10 seconds. The film thickness immediately after film formation and the film thickness at 0 mJ / cm 2 (unexposed area) and 300 mJ / cm 2 The film thickness of the exposed area after development was measured using an interference film thickness meter (Lambda Ace VM-2110, manufactured by SCREEN Co., Ltd.) to compare the film thickness of the exposed area with that of the unexposed area. The film thickness measurement results are shown in Table 1.
[0186]
[0187] From the results in Table 1, the negative photosensitive resin compositions of Examples 1 to 30 had a low photoirradiation rate in the unexposed area (0 mJ / cm ) after development. 2 ) photosensitive resin film is sufficiently dissolved (developed), and the exposed area (300 mJ / cm 2 ) remained without dissolving (development). In other words, a clear difference in solubility (dissolution contrast) of the photosensitive resin film was obtained between the exposed and unexposed areas, and therefore the composition can be suitably used as a negative photosensitive resin composition for a relief pattern creation process in which development is carried out using a general-purpose organic solvent such as cyclopentanone. On the other hand, the photosensitive resin compositions of Comparative Examples 1, 2, 4, and 5 remained without dissolving (development) in the unexposed areas (0 mJ / cm 2 ) remained without being sufficiently dissolved (developed). In other words, no clear dissolution contrast was obtained between the exposed and unexposed areas, and the composition is unsuitable as a negative-tone photosensitive resin composition for a relief pattern formation process in which development is carried out using a general-purpose organic solvent such as cyclopentanone.
[0188] [Evaluation of Electrical Properties] The negative photosensitive resin compositions prepared in Examples 1 to 30 and Comparative Examples 1 to 6 were spin-coated onto a 4-inch silicon wafer covered with 20 μm-thick aluminum foil, and baked on a hot plate at 115° C. for 180 seconds or 270 seconds to form a photosensitive resin film on the aluminum foil. Next, an i-line aligner (PLA-501, manufactured by Canon Inc.) was used to apply 500 mJ / cm to the wafer. 2 After the entire surface was exposed to light with a 1000 W exposure lamp, the foil was baked in a nitrogen atmosphere at 160°C for 1 hour and then at 230°C for 1 hour. The baked aluminum foil was then immersed in 6N hydrochloric acid to dissolve the aluminum foil, thereby obtaining a film. The obtained film was then dried under reduced pressure at 80°C for 2 hours and left to stand for 24 hours in an environment at a temperature of approximately 25°C and a humidity of approximately 42%, after which the dielectric loss tangent at 1 GHz was measured using a cavity resonator (TMR-1A, manufactured by Keycom Corporation). The measurement conditions for the dielectric loss tangent were as follows: Measurement method: Perturbation cavity resonator method Vector network analyzer: FieldFox N9926A (manufactured by Keysight Technologies, Inc.) Cavity resonator: TMR-1A (manufactured by Keycom Corporation) Cavity volume: 1192822 mm 3 Measurement frequency: approximately 1 GHz Sample tube: PTFE, inner diameter: 3 mm, length: approximately 30 mm (manufactured by Keycom Co., Ltd.)
[0189] [Mechanical Property Evaluation] The negative photosensitive resin compositions prepared in Examples 1 to 30 and Comparative Examples 1 to 6 were spin-coated onto an aluminum wafer having a thickness of 100 nm, and baked on a hot plate at 115°C for 180 seconds or 270 seconds to form a photosensitive resin film on the aluminum wafer. Next, an i-line aligner (PLA-501, manufactured by Canon Inc.) was used to apply 500 mJ / cm 2After the entire surface was exposed to light, the wafer was baked in a nitrogen atmosphere at 160°C for 1 hour and then at 230°C for 1 hour. The photosensitive resin film was then cut at 5 mm intervals using a dicing saw (DAD323, manufactured by Disco Corporation). The aluminum wafer was then immersed in 6N hydrochloric acid to dissolve the aluminum, yielding a 5 mm wide film. The tensile elongation of the resulting film was then measured using a benchtop precision universal testing machine (Autograph AGS-10kNX, manufactured by Shimadzu Corporation). The tensile elongation measurement conditions were as follows: Tabletop precision universal testing machine: Autograph AGS-10kNX (manufactured by Shimadzu Corporation) Film width: 5 mm Grip distance: 25 mm A tensile elongation of 50% means that the film can be stretched to 1.5 times its original length, or in other words, the film breaks when the grip distance is 1.5 times its original length (37.5 mm).
[0190] The measurement results of the dielectric loss tangent and tensile elongation are shown in Table 2.
[0191]
[0192] The results in Table 2 show that the films obtained from the negative photosensitive resin compositions of Examples 1 to 30 had dielectric loss tangent values at 1 GHz that were lower than those of Comparative Examples 1 to 5. Furthermore, the films obtained from the negative photosensitive resin compositions of Examples 1 to 30 had improved tensile elongation values than those of Comparative Examples 1 to 6. That is, the negative photosensitive resin compositions of Examples 1 to 30 are capable of producing relief patterns and simultaneously have the features of low dielectric loss tangent and high tensile elongation, and therefore can be suitably used in the production of electronic materials that require excellent electrical and mechanical properties.
Claims
1. A photosensitive resin composition comprising a reaction product of an aromatic diamine compound having a photopolymerizable group and a tetracarboxylic acid derivative having three or more aromatic rings, and a solvent, the reaction product is a polyamic acid or a polyimide obtained by dehydrating and ring-closing a polyamic acid, The polyamic acid has at least a structural unit represented by the following formula (1): The polyimide has at least a structural unit represented by the following formula (2): Ar 2 in the formula (1) and Ar 4 in the formula (2) are tetravalent organic groups represented by the following formula (3): Ar 1 in the formula (1) and Ar 3 in the formula (2) are divalent organic groups represented by the following formula (6): Photosensitive resin composition. 【Chemistry 1】 [In formula (1), Ar 1 represents a divalent organic group having a photopolymerizable group and an aromatic ring, and Ar 2 represents a tetravalent organic group having three or more aromatic rings.] 【Chemistry 2】 [In formula (2), Ar 3 represents a divalent organic group having a photopolymerizable group and an aromatic ring, and Ar 4 represents a tetravalent organic group having three or more aromatic rings.] 【Chemistry 3】 [In formula (3), X 1 and X 2 each independently represent a direct bond, an ether bond, an ester bond, a urethane bond, a urea bond, a thioether bond or a sulfonyl bond. R 1 and R 2 each independently represent an alkyl group having 1 to 6 carbon atoms which may be substituted. Y represents a divalent organic group represented by the following formula (3-1) or (3-2). n1 and n2 each independently represent an integer of 0 to 3. When there are multiple R 1 s, the multiple R 1 s may be the same or different. When there are multiple R 2 s, the multiple R 2 s may be the same or different. * represents a bond.] 【Chemistry 4】 [In formula (3-1), Z 1 represents a direct bond, an ether bond, an ester bond, a urethane bond, a urea bond, a thioether bond, or a sulfonyl bond. R 3 and R 4 each independently represent a hydrocarbon group having 1 to 6 carbon atoms which may be substituted. m1 represents an integer of 0 to 3. n3 and n4 each independently represent an integer of 0 to 4. When there are multiple Z 1 s, the multiple Z 1 s may be the same or different. When there are multiple n4 s, the multiple n4 s may be the same or different. When there are multiple R 3 s, the multiple R 3 s may be the same or different. When there are multiple R 4 s, the multiple R 4 s may be the same or different. * represents a bond. In formula (3-2), Z 2 represents a divalent organic group represented by the following formula (4) or (5). R 5 and R 6 each independently represent an optionally substituted hydrocarbon group having 1 to 6 carbon atoms. n5 and n6 each independently represent an integer of 0 to 4. When there are multiple R 5 s, the multiple R 5 s may be the same or different. When there are multiple R 6 s, the multiple R 6 s may be the same or different. * represents a bond.] 【Chemistry 5】 In formula (4), R 7 and R 8 each independently represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms which may be substituted with a halogen atom; * represents a bond. In formula (5), R 9 and R 10 each independently represent an optionally substituted alkylene group having 1 to 6 carbon atoms or an optionally substituted arylene group having 6 to 10 carbon atoms. * represents a bond.] 【Chemistry 6】 [In formula (6), Z 3 represents an ether bond, an ester bond, an amide bond, a urethane bond or a urea bond, Z 4 represents a direct bond, an ester bond or an amide bond, Z 5 represents a direct bond, an ether bond, an ester bond, an amide bond, a urethane bond, a urea bond, a thioether bond or a sulfonyl bond, m2 represents an integer of 0 or 1, R 11 represents a direct bond or an alkylene group having 2 to 6 carbon atoms which may be substituted with a hydroxyl group, and R 12 represents a hydrogen atom or a methyl group. * represents a bond.]
2. Z in the formula (6) 3 and Z 4 The photosensitive resin composition according to claim 1 , wherein is an ester bond.
3. R in the formula (6) 11 The photosensitive resin composition according to claim 1 or 2, wherein is a 1,2-ethylene group.
4. The photosensitive resin composition according to any one of claims 1 to 3, further comprising a photoradical polymerization initiator.
5. The photosensitive resin composition according to any one of claims 1 to 4, further comprising a crosslinkable compound.
6. The photosensitive resin composition according to any one of claims 1 to 5, which is used for forming an insulating film.
7. The photosensitive resin composition according to any one of claims 1 to 6, which is a negative type photosensitive resin composition.
8. A resin film which is a fired product of a coating film of the photosensitive resin composition according to any one of claims 1 to 7.
9. The resin film according to claim 8 , which is an insulating film.
10. A photosensitive resist film comprising a base film, a photosensitive resin layer formed from the photosensitive resin composition according to any one of claims 1 to 7, and a cover film.
11. (1) applying the photosensitive resin composition according to any one of claims 1 to 7 onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; (4) heat treating the relief pattern to form a hardened relief pattern; A method for producing a substrate having a cured relief pattern comprising:
12. The method for producing a substrate having a cured relief pattern according to claim 11 , wherein the developer used in the development is an organic solvent.
13. 13. A substrate with a cured relief pattern produced by the method of claim 11 or 12.
14. A semiconductor device comprising a semiconductor element and a cured film provided on an upper or lower part of the semiconductor element, the cured film being a cured relief pattern formed from the photosensitive resin composition according to any one of claims 1 to 7.