Silicon carbide epitaxial substrate

JPWO2023149166A5Pending Publication Date: 2024-10-10
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023578432
Authority / Receiving Office
JP · JP
Patent Type
Applications
Filing Date
2024-07-18
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

The yield of silicon carbide semiconductor devices is reduced due to defects, particularly blue light-emitting defects exposed on the surface of silicon carbide epitaxial substrates, which are formed from threading dislocations during the polishing process, leading to electrical characteristic deterioration.

Method used

A silicon carbide epitaxial substrate with a controlled polishing process that determines the optimal polishing amount to minimize the areal density of blue light-emitting defects and threading dislocations, ensuring the surface roughness and flatness are maintained within specific limits, thereby reducing the conversion rate of threading dislocations to defects and improving substrate quality.

Benefits of technology

The approach reduces the areal density of blue light-emitting defects and improves the flatness of the substrate, enhancing the yield of silicon carbide semiconductor devices by optimizing the polishing process to balance surface roughness and defect density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023149166000001
    Figure 2023149166000001
Patent Text Reader

Abstract

This silicon carbide epitaxial substrate has a silicon carbide substrate and a silicon carbide epitaxial layer. The silicon carbide substrate has a first main surface. The silicon carbide epitaxial layer is provided on the first main surface. Blue-light-emitting defects are present in the silicon carbide epitaxial layer. The silicon carbide epitaxial layer has a second main surface. The second main surface is on the reverse side from the interface of the silicon carbide substrate and the silicon carbide epitaxial layer. The blue-light-emitting defects are exposed on the second main surface. The ratio of a third surface density to the total value of a first surface density and a second surface density is 0.03% or less, where the first surface density is the surface density of threading screw dislocations in the first main surface, the second surface density is the surface density of threading edge dislocations in the first main surface, and the third surface density is the surface density of blue-light-emitting defects in the second main surface.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon carbide epitaxial substrate

[0001] The present disclosure relates to a silicon carbide epitaxial substrate. This application claims priority to Japanese Patent Application No. 2022-014815, filed February 2, 2022. The entire contents of this Japanese patent application are incorporated herein by reference.

[0002] Japanese Patent Laid-Open Publication No. 2009-292723 (Patent Document 1) discloses a silicon carbide epitaxial substrate having a low threading dislocation density in the silicon carbide substrate.

[0003] JP 2009-292723 A

[0004] A silicon carbide epitaxial substrate according to the present disclosure comprises a silicon carbide substrate and a silicon carbide epitaxial layer. The silicon carbide substrate includes a first main surface. The silicon carbide epitaxial layer is provided on the first main surface. The silicon carbide substrate has threading screw dislocations. The silicon carbide substrate has threading edge dislocations. The silicon carbide epitaxial layer has blue-emitting defects. The silicon carbide epitaxial layer includes a second main surface. The second main surface is located on the opposite side of the interface between the silicon carbide substrate and the silicon carbide epitaxial layer. The blue-emitting defects are exposed at the second main surface. When photoluminescence light generated from blue-emitting defects by irradiating the blue-emitting defects with excitation light is expressed in HSV color space, H is 180° or more and 230° or less, S is 60 or more and 170 or less, and V is 190 or more and 255 or less. When the first main surface is divided into a plurality of square regions with a side length of 10 mm, the plurality of square regions include a plurality of first outer peripheral regions located at the outermost peripheries of the plurality of square regions and a plurality of second outer peripheral regions contacting the plurality of first outer peripheral regions. The average LTIR of the silicon carbide substrate in the plurality of first outer peripheral regions and the plurality of second outer peripheral regions is 0.6 μm or less. When the areal density of threading screw dislocations on the first main surface is defined as a first areal density, the areal density of threading edge dislocations on the first main surface is defined as a second areal density, and the areal density of blue-luminescence defects on the second main surface is defined as a third areal density, the ratio of the third areal density to the sum of the first areal density and the second areal density is 0.03% or less.

[0005] FIG. 1 is a plan view schematic diagram showing the configuration of a silicon carbide epitaxial substrate according to this embodiment. FIG. 2 is a cross-sectional view schematic diagram taken along line II-II in FIG. 1. FIG. 3 is an enlarged cross-sectional view schematic diagram showing region III in FIG. 2. FIG. 4 is a schematic diagram showing the configuration of a color photoluminescence imaging device. FIG. 5 is a plan view schematic diagram showing the measurement region of LTIR. FIG. 6 is a schematic diagram explaining the definition of LTIR. FIG. 7 is a cross-sectional view schematic diagram taken along line VII-VII in FIG. 5. FIG. 8 is a cross-sectional view schematic diagram showing the definition of total thickness variation. FIG. 9 is a flowchart generally showing a method for manufacturing a silicon carbide epitaxial substrate according to this embodiment. FIG. 10 is a cross-sectional view schematic diagram showing the configuration of a silicon carbide wafer. FIG. 11 is an enlarged cross-sectional view schematic diagram showing region XI in FIG. 10. FIG. 12 is a plan view schematic diagram showing the configuration of a polishing apparatus. FIG. 13 is a front view schematic diagram showing the configuration of a polishing apparatus. Fig. 14 is an enlarged schematic cross-sectional view showing the configuration of a dummy wafer during the required polishing amount determining step. Fig. 15 is an enlarged schematic plan view showing the configuration of a dummy wafer during the required polishing amount determining step. Fig. 16 is an enlarged schematic view showing the configuration of a dummy wafer after the required polishing amount determining step. Fig. 17 is an enlarged schematic cross-sectional view showing the configuration of a silicon carbide substrate during the polishing step. Fig. 18 is an enlarged schematic cross-sectional view showing a state in which a silicon carbide epitaxial layer has been formed after polishing the first main surface of the silicon carbide substrate so that the surface roughness is sufficiently small. Fig. 19 is a schematic cross-sectional view showing a state in which the polishing amount due to mechanical polishing in the polishing step is excessively large.

[0006] [Problem to be Solved by the Present Disclosure] An object of the present disclosure is to provide a silicon carbide epitaxial substrate that can improve the yield of silicon carbide semiconductor devices.

[0007] Effect of the Present Disclosure According to the present disclosure, it is possible to provide a silicon carbide epitaxial substrate that can improve the yield of silicon carbide semiconductor devices.

[0008] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described.

[0009] (1) A silicon carbide epitaxial substrate 100 according to the present disclosure includes a silicon carbide substrate 10 and a silicon carbide epitaxial layer 20. The silicon carbide substrate 10 has a first main surface 1. The silicon carbide epitaxial layer 20 is provided on the first main surface 1. The silicon carbide substrate 10 has a threading screw dislocation 81. The silicon carbide substrate 10 has a threading edge dislocation 82. The silicon carbide epitaxial layer 20 has a blue light-emitting defect 83. The silicon carbide epitaxial layer 20 has a second main surface 2. The second main surface 2 is located on the opposite side of the interface 6 between the silicon carbide substrate 10 and the silicon carbide epitaxial layer 20. The blue light-emitting defect 83 is exposed at the second main surface 2. When photoluminescence light generated from blue light-emitting defect 83 by irradiating blue light-emitting defect 83 with excitation light is expressed in HSV color space, H is 180° or more and 230° or less, S is 60 or more and 170 or less, and V is 190 or more and 255 or less. When first main surface 1 is divided into a plurality of square regions 50 with a side length of 10 mm, the plurality of square regions 50 have a plurality of first outer peripheral regions 61 located at the outermost periphery of the plurality of square regions 50 and a plurality of second outer peripheral regions 62 contacting the plurality of first outer peripheral regions 61. The average value of the LTIR of silicon carbide substrate 10 in the plurality of first outer peripheral regions 61 and the plurality of second outer peripheral regions 62 is 0.6 μm or less. If the areal density of threading screw dislocations 81 on the first main surface 1 is defined as the first areal density, the areal density of threading edge dislocations 82 on the first main surface 1 is defined as the second areal density, and the areal density of blue-emitting defects 83 on the second main surface 2 is defined as the third areal density, the ratio of the third areal density to the sum of the first areal density and the second areal density is 0.03% or less.

[0010] (2) According to silicon carbide epitaxial substrate 100 according to (1) above, the variation in the overall thickness of silicon carbide substrate 10 may be 6 μm or less.

[0011] (3) In silicon carbide epitaxial substrate 100 according to (1) or (2) above, the ratio of the third areal density to the sum of the first areal density and the second areal density may be equal to or less than 0.02%.

[0012] (4) In silicon carbide epitaxial substrate 100 according to (3) above, the ratio of the third areal density to the sum of the first areal density and the second areal density may be equal to or less than 0.01%.

[0013] (5) In silicon carbide epitaxial substrate 100 according to any one of (1) to (4) above, the ratio of the third areal density to the first areal density may be equal to or less than 0.2%.

[0014] (6) According to the silicon carbide epitaxial substrate 100 according to any one of (1) to (5) above, the first areal density is 1500 / cm 2 It may be the following:

[0015] (7) According to the silicon carbide epitaxial substrate 100 according to (6) above, the first areal density is 500 particles / cm 2 It may be the following:

[0016] (8) According to the silicon carbide epitaxial substrate 100 according to (7) above, the first areal density is 100 particles / cm 2 It may be the following:

[0017] (9) According to the silicon carbide epitaxial substrate 100 according to any one of (1) to (8) above, the second areal density is 10,000 atoms / cm 2 It may be the following:

[0018] (10) According to the silicon carbide epitaxial substrate 100 according to (9) above, the second areal density is 5000 particles / cm 2 It may be the following:

[0019] (11) According to the silicon carbide epitaxial substrate 100 according to (10) above, the second areal density is 2000 particles / cm 2 It may be the following:

[0020] (12) In silicon carbide epitaxial substrate 100 according to any one of (1) to (11) above, second main surface 2 may have a diameter D of 150 mm or greater.

[0021] (13) According to silicon carbide epitaxial substrate 100 according to any one of (1) to (12) above, silicon carbide substrate 10 may have an electrical resistivity of 10 mΩ·cm or more.

[0022] [Details of the Embodiments of the Present Disclosure] Hereinafter, details of the embodiments of the present disclosure will be described with reference to the drawings. Note that the same or corresponding parts in the following drawings are given the same reference numerals, and their description will not be repeated. In the crystallographic descriptions in this specification, individual orientations are indicated by [ ], collective orientations by < >, individual planes by ( ), and collective planes by {}. Furthermore, for negative indices, in crystallography, a "-" (bar) is placed before the number, but in this specification, a negative sign is placed before the number.

[0023] First, the configuration of the silicon carbide epitaxial substrate according to this embodiment will be described. FIG. 1 is a plan view schematically illustrating the configuration of the silicon carbide epitaxial substrate according to this embodiment. As shown in FIG. 1, the silicon carbide epitaxial substrate 100 has a second main surface 2 and an outer peripheral side surface 9. The second main surface 2 extends along each of a first direction 101 and a second direction 102. The first direction 101 is not particularly limited, but is, for example, the <11-20> direction. The second direction 102 is not particularly limited, but is, for example, the <1-100> direction. The outer peripheral side surface 9 is continuous with the second main surface 2. The silicon carbide epitaxial substrate 100 is made of, for example, hexagonal silicon carbide. The polytype of the hexagonal silicon carbide is, for example, 4H.

[0024] The second main surface 2 is a plane inclined with respect to the {0001} plane. The off-angle of the second main surface 2 with respect to the {0001} plane may be, for example, 8° or less. Specifically, the second main surface 2 may be a plane inclined with an off-angle of 8° or less with respect to the (0001) plane. The second main surface 2 may be a plane inclined with an off-angle of 8° or less with respect to the (000-1) plane. The inclination direction (off-direction) of the second main surface 2 with respect to the {0001} plane is, for example, the <11-20> direction. The off-angle of the second main surface 2 with respect to the {0001} plane is not particularly limited, but may be, for example, 7° or less or 6° or less. The off-angle of the second main surface 2 with respect to the {0001} plane is not particularly limited, but may be, for example, 1° or more or 2° or more.

[0025] 1, the outer peripheral side surface 9 has an orientation flat portion 7 and an arc-shaped portion 8. The arc-shaped portion 8 is continuous with the orientation flat portion 7. As shown in FIG. 1, when viewed from a direction perpendicular to the second main surface 2, the orientation flat portion 7 may extend along a first direction 101.

[0026] The diameter D of the second main surface 2 is, for example, 150 mm or more. The diameter D is not particularly limited, but may be, for example, 200 mm or more, or 250 mm or more. The diameter D is not particularly limited, but may be, for example, 300 mm or less. When viewed in a direction perpendicular to the second main surface 2, the diameter D is the longest linear distance between two different points on the outer peripheral side surface 9.

[0027] Fig. 2 is a cross-sectional schematic view taken along line II-II in Fig. 1. The cross section shown in Fig. 2 is perpendicular to second main surface 2 and parallel to first direction 101. As shown in Fig. 2, silicon carbide epitaxial substrate 100 according to this embodiment has silicon carbide substrate 10 and silicon carbide epitaxial layer 20. Silicon carbide epitaxial layer 20 is provided on silicon carbide substrate 10. Silicon carbide epitaxial layer 20 is in contact with silicon carbide substrate 10. The polytype of silicon carbide substrate 10 is, for example, 4H. Similarly, the polytype of silicon carbide epitaxial layer 20 is, for example, 4H.

[0028] Silicon carbide epitaxial layer 20 forms second main surface 2 of silicon carbide epitaxial substrate 100. Second main surface 2 is located opposite interface 6. Interface 6 is located at the boundary between silicon carbide substrate 10 and silicon carbide epitaxial layer 20. Silicon carbide substrate 10 has first main surface 1 and third main surface 3. At first main surface 1, silicon carbide substrate 10 is in contact with silicon carbide epitaxial layer 20. In other words, silicon carbide epitaxial layer 20 is provided on first main surface 1. Third main surface 3 is located opposite first main surface 1. Second main surface 2 is the front surface of silicon carbide epitaxial substrate 100. Third main surface 3 is the back surface of silicon carbide epitaxial substrate 100.

[0029] The first main surface 1 may have polishing marks. When viewed from a direction perpendicular to the first main surface 1, the polishing marks have an elongated shape. The longitudinal length of the polishing marks is, for example, 10 times or more the lateral length of the polishing marks. The polishing marks may be linear or curved. When viewed from a direction perpendicular to the first main surface 1, the length of the polishing marks is, for example, 0.5 mm or more. The depth of the polishing marks in the direction perpendicular to the first main surface 1 is, for example, 0.5 μm or more. The surface density of the polishing marks on the first main surface 1 is, for example, 1 mark / cm 2 Polishing marks on first main surface 1 can be identified using a laser microscope, a white light interference microscope, or a defect inspection device such as a WASAVI series "SICA 6X" manufactured by Lasertec Corporation. Specifically, when second main surface 2 of silicon carbide epitaxial layer 20 is observed from above, grooves intersecting with linear streaks extending in the <1-100> direction are identified as polishing marks.

[0030] 2 , silicon carbide substrate 10 has a plurality of threading dislocations 80. The plurality of threading dislocations 80 is composed of a plurality of threading screw dislocations 81 and a plurality of threading edge dislocations 82.

[0031] Each of the multiple threading dislocations 80 extends continuously from the third main surface 3 to the first main surface 1. The direction in which each of the multiple threading dislocations 80 extends is a fourth direction 104. The fourth direction 104 is, for example, the <0001> direction. The third direction 103 is a direction perpendicular to the second main surface 2. From another perspective, the third direction 103 is a direction perpendicular to each of the first direction 101 and the second direction 102. The tilt angle θ of the fourth direction 104 with respect to the third direction 103 corresponds to the off-angle of the second main surface 2. Each of the multiple threading dislocations 80 is exposed at the third main surface 3.

[0032] As shown in FIG. 2 , silicon carbide epitaxial layer 20 has a plurality of blue light-emitting defects 83. Each of the plurality of blue light-emitting defects 83 is formed due to a threading dislocation 80. At first main surface 1, each of the plurality of blue light-emitting defects 83 is connected to threading dislocation 80. Each of the plurality of blue light-emitting defects 83 may be connected to a threading screw dislocation 81 or a threading edge dislocation 82. Each of the plurality of blue light-emitting defects 83 extends continuously from interface 6 to second main surface 2. The width of each of the plurality of blue light-emitting defects 83 in first direction 101 increases with increasing distance from interface 6. When viewed from a direction perpendicular to each of first direction 101 and third direction 103, each of the plurality of blue light-emitting defects 83 is, for example, triangular. Each of the plurality of blue light-emitting defects 83 is exposed at second main surface 2.

[0033] 3 is an enlarged schematic cross-sectional view showing region III in FIG. 2 . As shown in FIG. 3 , silicon carbide substrate 10 is composed of normal portion 11 and process-affected portion 12. Normal portion 11 is a portion composed of a normal crystal lattice that has not been damaged by slicing. Process-affected portion 12 is a portion in which the crystal lattice arrangement of silicon carbide substrate 10 has been disturbed by processing damage caused by slicing. Process-affected portion 12 is continuous with normal portion 11. Process-affected portion 12 forms part of first main surface 1 of silicon carbide substrate 10. From another perspective, process-affected portion 12 is in contact with silicon carbide epitaxial layer 20. Process-affected portion 12 is provided in the vicinity of threading dislocations 80.

[0034] Each of the plurality of blue light-emitting defects 83 is formed due to the processing-affected portion 12. From another perspective, each of the plurality of blue light-emitting defects 83 is connected to the processing-affected portion 12. Each of the plurality of blue light-emitting defects 83 is, for example, a triangular defect. Each of the plurality of blue light-emitting defects 83 may include a stacking fault. When viewed in a direction perpendicular to the second main surface 2, the shape of each blue light-emitting defect 83 is, for example, a triangle.

[0035] (Area Density of Threading Screw Dislocations and Threading Edge Dislocations) The area density of threading screw dislocations 81 on the first main surface 1 is referred to as the first area density. The first area density is, for example, 1500 counts / cm 2The first surface density is not particularly limited, but is, for example, 1000 particles / cm 2 It may be 500 particles / cm or less. 2 It may be 100 pieces / cm or less. 2 The first surface density is not particularly limited, but may be, for example, 10 particles / cm 2 It may be 50 pieces / cm or more. 2 It may be more than that.

[0036] The areal density of threading edge dislocations 82 on the first main surface 1 is referred to as the second areal density. The second areal density is, for example, 10,000 pieces / cm 2 The second areal density is not particularly limited, but is, for example, 5000 particles / cm 2 It may be 2000 particles / cm or less. 2 The second areal density is not particularly limited, but may be, for example, 100 particles / cm 2 It may be 500 or more per cm 2 It may be more than that.

[0037] Next, a method for measuring the areal density of each of the threading screw dislocations 81 and the threading edge dislocations 82 will be described.

[0038] The areal density of each of the threading screw dislocations 81 and threading edge dislocations 82 is determined using, for example, molten potassium hydroxide (KOH). Specifically, the silicon carbide epitaxial layer 20 is removed using mechanical polishing or the like. This exposes the first main surface 1 of the silicon carbide substrate 10. The first main surface 1 is etched with the molten KOH. This etches silicon carbide regions near each of the threading screw dislocations 81 and threading edge dislocations 82 exposed at the first main surface 1, forming etch pits at the first main surface 1. The value obtained by dividing the number of etch pits formed at the first main surface 1 by the measured area of ​​the first main surface 1 corresponds to the areal density of each of the threading screw dislocations 81 and threading edge dislocations 82 at the first main surface 1. The temperature of the KOH melt is, for example, approximately 500°C or higher and 550°C or lower. The etching time is approximately 5 minutes or higher and 10 minutes or lower. After etching, the first main surface 1 is observed using a Normarski differential interference contrast microscope.

[0039] When silicon carbide substrate 10 contains basal plane dislocations in addition to threading screw dislocations 81 and threading edge dislocations 82, silicon carbide regions near the basal plane dislocations exposed on first main surface 1 are also etched. Etch pits caused by threading screw dislocations 81, etch pits caused by threading edge dislocations 82, and etch pits caused by basal plane dislocations are distinguished by the following method. Etch pits caused by basal plane dislocations have an elliptical planar shape. Etch pits caused by threading screw dislocations 81 have a round or hexagonal planar shape and a large pit size. Etch pits caused by threading edge dislocations 82 have a round or hexagonal planar shape and a small pit size.

[0040] (Area Density of Blue Light Emitting Defects) The area density of the blue light emitting defects 83 on the second main surface 2 is referred to as a third area density. The third area density is, for example, 2 defects / cm 2 The third surface density is not particularly limited, but is, for example, 1 particle / cm 2 It may be 0.5 pieces / cm or less. 2 The third areal density is not particularly limited, but may be, for example, 0.05 particles / cm 2 or more, or 0.07 particles / cm 2 It may be more than that.

[0041] The ratio of the third areal density to the sum of the first areal density and the second areal density is, for example, 0.03% or less. The ratio of the third areal density to the sum of the first areal density and the second areal density is not particularly limited, but may be, for example, 0.02% or less, or 0.01% or less. The ratio of the third areal density to the sum of the first areal density and the second areal density is not particularly limited, but may be, for example, 0.001% or more, or 0.005% or more.

[0042] The ratio of the third areal density to the first areal density is, for example, 0.2% or less. The ratio of the third areal density to the first areal density may be 0.15% or less, or 0.1% or less. The ratio of the third areal density to the first areal density is not particularly limited, and may be, for example, 0.01% or more, or 0.05% or more.

[0043] The blue light-emitting defect 83 can be identified by a photoluminescence imaging device. FIG. 4 is a schematic diagram showing the configuration of a color photoluminescence imaging device. As the color photoluminescence imaging device, for example, a PL imaging device (SemiScope™ PLI-200) manufactured by Photon Design, Inc. can be used. As shown in FIG. 4, the color photoluminescence imaging device 200 mainly includes an excitation light generation unit 220 and an imaging unit 230.

[0044] The excitation light generation unit 220 has a light source section 221, a light guide section 222, and a filter section 223. The light source section 221 can generate excitation light LE having energy higher than the band gap of hexagonal silicon carbide. The light source section 221 is, for example, a mercury-xenon lamp. The light guide section 222 can guide the light emitted from the light source section 221 so that the light is irradiated onto the second main surface 2 (see FIG. 2 ) of the silicon carbide epitaxial substrate 100. The light guide section 222 has, for example, an optical fiber. As shown in FIG. 4 , the excitation light generation unit 220 may be arranged on both sides of the near-infrared objective lens 233.

[0045] The filter section 223 selectively transmits light having a specific wavelength corresponding to an energy higher than the bandgap of hexagonal silicon carbide. The wavelength corresponding to the bandgap of hexagonal silicon carbide is typically about 390 nm. Therefore, a bandpass filter that specifically transmits light having a wavelength of, for example, about 313 nm is used as the filter section 223. The transmission wavelength range of the filter section 223 may be, for example, 290 nm to 370 nm, 300 nm to 330 nm, or 300 nm to 320 nm.

[0046] Imaging unit 230 mainly includes a control unit 231, a stage 232, a near-infrared objective lens 233, and a color image sensor 235. Control unit 231 controls the displacement operation of stage 232 and the imaging operation by color image sensor 235, and is, for example, a personal computer. Stage 232 supports silicon carbide epitaxial substrate 100 so that second main surface 2 is exposed. Stage 232 is, for example, an XY stage that displaces the position of second main surface 2. Near-infrared objective lens 233 is disposed above second main surface 2. The magnification of near-infrared objective lens 233 is, for example, 4.5 times. Color image sensor 235 receives photoluminescence light emitted from silicon carbide epitaxial substrate 100.

[0047] Next, a method for identifying blue light emission defects 83 will be described. First, excitation light generation unit 220 is used to irradiate second main surface 2 of silicon carbide epitaxial substrate 100 with excitation light LE. This causes photoluminescence light LL to be generated from silicon carbide epitaxial substrate 100. The wavelength of excitation light LE is, for example, 313 nm. The intensity of excitation light LE is, for example, 1 mW / cm. 2 More than 2W / cm 2 The exposure time of the irradiated light is, for example, 0.5 seconds or more and 120 seconds or less, and the measurement temperature is, for example, room temperature (27° C.).

[0048] Next, the photoluminescence light is detected by a color image sensor. Specifically, photoluminescence light LL generated in silicon carbide epitaxial substrate 100 is detected by color image sensor 235. Color image sensor 235 is, for example, a CCD (charge coupled device) image sensor. The type of CCD element is, for example, a back-illuminated deep depletion type. The CCD image sensor is, for example, an excelon (trademark) manufactured by Teledyne. The imaging wavelength range is, for example, 310 nm or more and 1024 nm or less. The element format is, for example, 1024 ch x 1024 ch. The image area is, for example, 13.3 mm x 13.3 mm. The element size is, for example, 13 μm x 13 μm. The number of pixels is, for example, 480 pixels x 640 pixels, and the image size is, for example, 1.9 mm x 2.6 mm.

[0049] The optical characteristics of the blue-light-emitting defect 83 are identified based on the color image obtained from the color image sensor 235. The color of the image of the blue-light-emitting defect 83 obtained from the color image sensor is, for example, blue. Specifically, when the photoluminescence light generated from the blue-light-emitting defect 83 by irradiating the blue-light-emitting defect 83 with excitation light is expressed in the HSV color space, H is 180° or more and 230° or less, S is 60 or more and 170 or less, and V is 190 or more and 255 or less.

[0050] The HSV color space is a color representation method that represents colors using hue, saturation, and value. In the HSV color space, the range of H is 0° to 360°, the range of S is 0 to 255, and the range of V is 0 to 255. S and V are expressed, for example, as decimal numbers.

[0051] (Sagging Degree of Silicon Carbide Substrate) Next, the sagging degree of the peripheral portion of silicon carbide substrate 10 will be described. The sagging degree of silicon carbide substrate 10 can be quantified using an index called LTIR (Local Total Indicated Reading) or total thickness variation (TTV). Each of LTIR and TTV can be measured using, for example, a flatness measuring instrument "Tropel FlatMaster (trademark)" manufactured by Corning Tropel.

[0052] (LTIR of silicon carbide substrate) FIG. 5 is a plan view schematic diagram showing a measurement area for LTIR. As shown in FIG. 5, first main surface 1 of silicon carbide substrate 10 is divided into a plurality of square regions 50. The length of one side of each of the plurality of square regions 50 (first length W1) is 10 mm. Diameter D of first main surface 1 is, for example, 150 mm. First, a 150 mm × 150 mm square circumscribing outer peripheral side surface 9 is assumed. The 150 mm × 150 mm square is divided into 10 mm × 10 mm square regions (15 × 15 = 225).

[0053] When viewed in a direction perpendicular to the first main surface 1, the number of square regions 50 surrounded by the outer peripheral side surface 9 is 145. When viewed in a direction perpendicular to the first main surface 1, the square regions that intersect with the outer peripheral side surface 9 are missing portions and are not complete square regions. Therefore, the square regions that intersect with the outer peripheral side surface 9 are not considered to be square regions 50 that make up the first main surface 1. When viewed in a direction perpendicular to the first main surface 1, one side of each of the multiple square regions 50 is parallel to the extension direction of the orientation flat portion 7.

[0054] The plurality of square regions 50 are composed of a plurality of outer peripheral regions 60 and a plurality of central regions 70. The plurality of outer peripheral regions 60 are composed of a plurality of first outer peripheral regions 61 and a plurality of second outer peripheral regions 62. The plurality of first outer peripheral regions 61 are located on the outermost periphery of the plurality of square regions 50. From another perspective, each of the plurality of first outer peripheral regions 61 is a square region 50 that is in contact with a square region that intersects with the outer peripheral side surface 9. Each of the plurality of second outer peripheral regions 62 is a square region 50 that is in contact with a plurality of first outer peripheral regions 61. Each of the plurality of second outer peripheral regions 62 is located inside the plurality of first outer peripheral regions 61. Each of the plurality of second outer peripheral regions 62 is spaced apart from a square region that intersects with the outer peripheral side surface 9. In FIG. 13 , the hatched regions are the plurality of outer peripheral regions 60.

[0055] The central regions 70 are surrounded by the peripheral regions 60. Each of the central regions 70 is spaced apart from a square region that intersects with the peripheral side surface 9.

[0056] As shown in Figure 5, when the diameter D of the first main surface 1 is 150 mm, the first main surface 1 is divided into 145 square regions 50, each having a side length (first length W1) of 10 mm. LTIR is measured in each of the 145 square regions 50. When the diameter D of the first main surface 1 is 150 mm, the number of outer peripheral regions 60 is 68, and the number of central regions 70 is 77. Of the multiple outer peripheral regions 60, the number of first outer peripheral regions 61 is 36, and the number of second outer peripheral regions 62 is 32.

[0057] Next, the definition of LTIR will be explained. Fig. 6 is a schematic diagram for explaining the definition of LTIR.

[0058] LTIR=|T1|+|T2| (Equation 1) LTIR is measured, for example, by the following procedure. Silicon carbide substrate 10 is prepared before silicon carbide epitaxial layer 20 is formed. Third main surface 3 of silicon carbide substrate 10 is entirely adsorbed onto a flat adsorption surface. Next, an image of first main surface 1 in a certain local region (for example, central region 70 and peripheral region 60) is optically acquired. Next, a least-squares plane L0 of first main surface 1 is found by calculation.

[0059] As shown in Equation 1 and FIG. 6 , LTIR is the sum of the height (first highest point height T1) from the least squares plane L0 to the highest point (first highest point P1) of the first main surface 1 and the height (first lowest point height T2) from the least squares plane L0 to the lowest point (first lowest point P2) of the first main surface 1 when the entire third main surface 3 is attached to a flat attachment surface. The first highest point P1 is the position where the distance between the least squares plane L0 and the first main surface 1 along the direction perpendicular to the least squares plane L0 is the maximum in a region of the first main surface 1 located on the opposite side of the least squares plane L0 from the third main surface 3. The first lowest point P2 is the position where the distance between the least squares plane L0 and the first main surface 1 along the direction perpendicular to the least squares plane L0 is the maximum in a region of the first main surface 1 located on the third main surface 3 side of the least squares plane L0. In other words, LTIR is the distance between a plane (first highest point plane L1) that passes through the first highest point P1 and is parallel to the least squares plane L0, and a plane (first lowest point plane L2) that passes through the first lowest point P2 and is parallel to the least squares plane L0.

[0060] Since silicon carbide epitaxial layer 20 has a substantially uniform thickness within its plane, the LTIR of silicon carbide substrate 10 is substantially the same as the LTIR of silicon carbide epitaxial substrate 100. In other words, the LTIR of silicon carbide epitaxial substrate 100 may be measured instead of the LTIR of silicon carbide substrate 10. When the LTIR of silicon carbide epitaxial substrate 100 is measured, the above procedure is performed on second main surface 2 after third main surface 3 is entirely adsorbed.

[0061] Fig. 7 is a schematic cross-sectional view taken along line VII-VII in Fig. 5. The cross section shown in Fig. 7 is perpendicular to the first main surface 1 and parallel to a first direction 101. As shown in Fig. 7, in the cross-sectional view, the first main surface 1 approaches the third main surface 3 as it approaches the outer peripheral side surface 9. From another perspective, the first outer peripheral region 61 is located between the third main surface 3 and the second outer peripheral region 62 in the third direction 103.

[0062] In a cross-sectional view, central region 70 may be linear. In a cross-sectional view, peripheral region 60 is, for example, curved. From another perspective, the average value of LTIR of silicon carbide substrate 10 in a plurality of peripheral regions 60 is greater than the average value of LTIR of silicon carbide substrate 10 in a plurality of central regions 70.

[0063] In a cross-sectional view, second outer peripheral region 62 has, for example, a curved shape. In a cross-sectional view, first outer peripheral region 61 has, for example, a curved shape. In a cross-sectional view, the curvature of first outer peripheral region 61 is larger than the curvature of second outer peripheral region 62. From another perspective, the average value of LTIR of silicon carbide substrate 10 in the plurality of first outer peripheral regions 61 is larger than the average value of LTIR of silicon carbide substrate 10 in the plurality of second outer peripheral regions 62.

[0064] The average value of the LTIR of silicon carbide substrate 10 in the plurality of peripheral regions 60 is, for example, 0.6 μm or less. The LTIR of silicon carbide substrate 10 in the plurality of peripheral regions 60 is not particularly limited, and may be, for example, 0.4 μm or less, or 0.25 μm or less. The LTIR of silicon carbide substrate 10 in the plurality of peripheral regions 60 is not particularly limited, and may be, for example, 0.01 μm or more, 0.03 μm or more, or 0.05 μm or more.

[0065] (Total Thickness Variation of Silicon Carbide Substrate) Next, the total thickness variation (TTV) will be described. Fig. 8 is a cross-sectional schematic diagram illustrating the definition of the total thickness variation.

[0066] TTV=|T3−T4| (Equation 2) TTV is measured, for example, by the following procedure. First, silicon carbide substrate 10 is prepared before silicon carbide epitaxial layer 20 is formed. Third main surface 3 of silicon carbide substrate 10 is entirely attracted to a flat attracting surface. Next, an entire image of first main surface 1 is optically acquired. As shown in FIG. 8 and Equation 2, TTV is a value obtained by subtracting the height from third main surface 3 to the lowest point (second lowest point P4) of first main surface 1 (second lowest point height T4) from the height from third main surface 3 to the highest point (second highest point P3) of first main surface 1 (second highest point height T3) when third main surface 3 is entirely attracted to the flat attracting surface. In other words, TTV is the value obtained by subtracting the shortest distance between the first principal surface 1 and the third principal surface 3 from the longest distance between the first principal surface 1 and the third principal surface 3 in the direction perpendicular to the third principal surface 3. In other words, TTV is the distance between a plane (second highest point plane L3) that passes through the second highest point P3 and is parallel to the third principal surface 3, and a plane (second lowest point plane L4) that passes through the second lowest point P4 and is parallel to the third principal surface 3.

[0067] Since silicon carbide epitaxial layer 20 has a substantially uniform thickness across its surface, the TTV of silicon carbide substrate 10 is substantially the same as the TTV of silicon carbide epitaxial substrate 100. In other words, the TTV of silicon carbide epitaxial substrate 100 may be measured instead of the TTV of silicon carbide substrate 10. When the TTV of silicon carbide epitaxial substrate 100 is measured, the above procedure is performed on second main surface 2 after third main surface 3 has been entirely adsorbed.

[0068] Silicon carbide substrate 10 according to this embodiment has a total thickness variation (TTV) of, for example, 6 μm or less. The TTV is not particularly limited, but may be, for example, 4 μm or less or 2 μm or less. The TTV is not particularly limited, but may be, for example, 0.1 μm or more or 0.5 μm or more.

[0069] 7 , in silicon carbide substrate 10, second lowest point P4 is located, for example, on the ridge line between first main surface 1 and outer peripheral side surface 9. Second highest point P3 is located, for example, in central region 70.

[0070] (Electrical Resistivity of Silicon Carbide Substrate) The electrical resistivity of silicon carbide substrate 10 is, for example, 10 mΩ·cm or more. The electrical resistivity of silicon carbide substrate 10 is not particularly limited, but may be, for example, 15 mΩ·cm or more, or 18 mΩ·cm or more. The electrical resistivity of silicon carbide substrate 10 is not particularly limited, but is, for example, 25 mΩ·cm or less. The electrical resistivity of silicon carbide substrate 10 can be measured, for example, using an electrical resistivity measuring device "EC-80" manufactured by Napson Corporation. Specifically, the electrical resistivity of silicon carbide substrate 10 is measured after silicon carbide epitaxial layer 20 is removed.

[0071] (Method for Manufacturing Silicon Carbide Epitaxial Substrate) Next, a method for manufacturing silicon carbide epitaxial substrate 100 will be described.

[0072] 9 is a flowchart illustrating a method for manufacturing a silicon carbide epitaxial substrate according to this embodiment. As shown in FIG. 9, the method for manufacturing a silicon carbide epitaxial substrate according to this embodiment mainly includes a silicon carbide wafer preparation step (S10), a required polishing amount determination step (S20), a polishing step (S30), and an epitaxial growth step (S40).

[0073] First, a silicon carbide wafer preparation step (S10) is performed. A silicon carbide crystal of polytype 4H is produced, for example, by sublimation deposition. Next, the silicon carbide crystal is sliced ​​using, for example, a wire saw, to produce a plurality of silicon carbide wafers 90. Each of the plurality of silicon carbide wafers 90 has substantially the same configuration.

[0074] FIG. 10 is a cross-sectional schematic diagram showing the configuration of a silicon carbide wafer 90. As shown in FIG. 10 , the silicon carbide wafer 90 has a fourth main surface 4 and a fifth main surface 5. The fifth main surface 5 is located opposite the fourth main surface 4. The silicon carbide wafer 90 has a plurality of threading dislocations 80. The threading dislocations 80 extend continuously from the fourth main surface 4 to the fifth main surface 5. The threading dislocations 80 are exposed at the fourth main surface 4. The threading dislocations 80 are exposed at the fifth main surface 5. The cross section shown in FIG. 10 is parallel to each of the first direction 101 and the third direction 103, and passes through the fourth main surface 4.

[0075] FIG. 11 is an enlarged schematic view showing region XI in FIG. 10 . As shown in FIG. 11 , silicon carbide wafer 90 is composed of normal portion 11 and process-affected portion 12. Process-affected portion 12 covers normal portion 11. Process-affected portion 12 forms fourth main surface 4. As shown in FIG. 11 , fourth main surface 4 is a surface that is formed by slicing using a wire saw and is not subsequently polished. Fifth main surface 5 may be a surface that has been smoothed by polishing. The thickness of silicon carbide wafer 90 is set to first thickness H1. As described above, silicon carbide wafer 90 is prepared.

[0076] Next, the configuration of the polishing apparatus will be described. Fig. 12 is a schematic plan view showing the configuration of the polishing apparatus. Fig. 13 is a schematic front view showing the configuration of the polishing apparatus. The polishing apparatus 30 is, for example, a mechanical polishing apparatus.

[0077] As shown in FIGS. 12 and 13 , the polishing apparatus 30 mainly includes a polishing head 31, an abrasive supply unit 32, a polishing cloth 34, and a surface plate 35. The polishing head 31 includes a support plate 37, a weight 38, and a support post 39. The weight 38 is positioned on the support plate 37. The support post 39 is positioned on the weight 38. The polishing cloth 34 is fixed to the surface plate 35. For example, the "KV" series of polishing cloths manufactured by Poval Kogyo can be used as the polishing cloth 34. The polishing cloth 34 may be, for example, a nonwoven fabric. The polishing cloth 34 may have a laminated structure. The layering direction of the polishing cloth 34 is, for example, perpendicular to the vertical direction. The vertical direction is the direction from the polishing cloth 34 toward the polishing head 31.

[0078] Next, a required polishing amount determining step (S20) is performed. Of the plurality of silicon carbide wafers 90, one silicon carbide wafer 90 is prepared as a dummy wafer 99. The dummy wafer 99 is a wafer different from the silicon carbide wafer 90 to be polished in the next polishing step (S30).

[0079] As shown in FIGS. 12 and 13, a dummy wafer 99 is attached to the support plate 37 of the polishing head 31. Abrasive 33 is supplied onto the polishing cloth 34. In the abrasive 33, for example, polycrystalline diamond is used as abrasive grains. The particle diameter (D 90 ) is, for example, 0.2 μm or more and 1.5 μm or less. 90 ) means a particle size corresponding to 90% of the cumulative value of the particle size distribution of the abrasive grains. In the abrasive 33, oil-based oil is used as a lubricant. The supply amount of the abrasive 33 is, for example, 5 cm 3 / min or more 50cm 3 / min or less.

[0080] The polishing head 31 and the polishing cloth 34 rotate while the fourth main surface 4 of the dummy wafer 99 is pressed against the polishing cloth 34 by the polishing head 31. The dummy wafer 99 is pressurized using a dead weight method. Specifically, the polishing head 31 presses the dummy wafer 99 against the polishing cloth 34 using the mass of the weight 38. In other words, the support 39 does not have the role of actively pressurizing the dummy wafer 99. Therefore, compared to when the dummy wafer 99 is pressurized by an air cylinder or the like, the dummy wafer 99 can vibrate in the vertical direction during polishing. This causes the frictional resistance experienced by the fourth main surface 4 of the dummy wafer 99 to change locally. The pressure with which the dummy wafer 99 is pressed against the polishing cloth 34 is, for example, 250 g / cm. 2 is.

[0081] 12 , the surface plate 35 to which the polishing cloth 34 is fixed rotates. Specifically, the surface plate 35 to which the polishing cloth 34 is fixed rotates around a first rotation axis 41 in a first rotation direction 111. The first rotation axis 41 passes through, for example, the center of the polishing cloth 34. The rotation speed of the surface plate 35 is, for example, 40 rpm or more and 100 rpm or less. The first rotation direction 111 is, for example, counterclockwise when viewed from above the polishing cloth 34.

[0082] 12 , the polishing head 31 rotates on its axis. Specifically, the polishing head 31 rotates around the second rotation axis 42 in a second rotation direction 112. The second rotation axis 42 passes through the center of the polishing head 31, for example. The rotation speed of the polishing head 31 is, for example, 80 rpm or more and 120 rpm or less. The second rotation direction 112 is, for example, counterclockwise when viewed from above the polishing cloth 34.

[0083] 12 , the polishing head 31 rotates about its axis while oscillating in an oscillation direction 113. The oscillation direction 113 is, for example, the direction from the first rotating shaft 41 to the second rotating shaft 42 when viewed from above the polishing cloth 34. In other words, the oscillation direction 113 is, for example, the radial direction of the polishing cloth 34. When viewed from above the polishing cloth 34, the polishing head 31 oscillates within the polishing cloth 34. The oscillation width of the polishing head 31 is, for example, 0.5 to 0.8 times the diameter of the dummy wafer 99. The oscillation speed of the polishing head 31 is, for example, 10 mm / sec to 30 mm / sec.

[0084] 12 , when the dummy wafer 99 is closest to the first rotation shaft 41, of the points on the outer periphery of the dummy wafer 99, the point closest to the first rotation shaft 41 is the center-side oscillation end 43. The peripheral speed of the surface plate 35 at the center-side oscillation end 43 is at least twice the peripheral speed of the dummy wafer 99 at the center-side oscillation end 43. The peripheral speed of the dummy wafer 99 at the center-side oscillation end 43 is equal to the peripheral speed of the dummy wafer 99 on the outer periphery of the dummy wafer 99.

[0085] 14 is an enlarged schematic cross-sectional view showing the configuration of the dummy wafer 99 during the required polishing amount determining step (S20). The enlarged schematic view shown in FIG. 14 corresponds to the enlarged schematic view shown in FIG.

[0086] In the required polishing amount determination step (S20), polishing is performed so that the frictional force applied to the fourth main surface 4 of the dummy wafer 99 varies locally. Therefore, the portions of the fourth main surface 4 that are easily polished are polished more sharply, like spikes, than the other portions of the fourth main surface 4. Specifically, as shown in FIG. 14 , the portions of the fourth main surface 4 that are near the threading dislocations 80 and that are the work-affected portions 12 are polished more sharply, like spikes, than the other portions of the fourth main surface 4. As a result, voids 84 are formed in the fourth main surface 4. From another perspective, in the required polishing amount determination step (S20), the voids 84 are formed near the threading dislocations 80 and in the work-affected portions 12. The depth of the voids 84 in the third direction 103 is, for example, 10 μm or more and 200 μm or less. The fourth main surface 4 excluding the voids 84 is polished smoothly.

[0087] 15 is an enlarged schematic plan view showing the configuration of a dummy wafer 99 during the required polishing amount determination process. As shown in FIG. 15 , the void 84 may be hexagonal when viewed from a direction perpendicular to the fourth main surface 4. The void 84 may be circular when viewed from a direction perpendicular to the fourth main surface 4. When the void 84 is hexagonal when viewed from a direction perpendicular to the fourth main surface 4, the length of the void 84 (second length W2) when viewed from a direction perpendicular to the fourth main surface 4 is the length of the void 84 in the longitudinal direction when viewed from a direction perpendicular to the fourth main surface 4. When the void 84 is circular when viewed from a direction perpendicular to the fourth main surface 4, the second length W2 of the void 84 is the diameter of the void 84. The second length W2 is, for example, 10 μm or more and 100 μm or less.

[0088] In the required polishing amount determining step (S20), after the dummy wafer 99 has been polished by a predetermined polishing amount, the surface density of the voids 84 on the fourth main surface 4 of the dummy wafer 99 is measured.

[0089] The voids 84 can be identified using, for example, an optical microscope, a laser microscope, or a defect inspection device such as the WASAVI series "SICA 6X" manufactured by Lasertec Corporation. Specifically, the fourth main surface 4 is observed using, for example, an optical microscope. The magnification of the objective lens is, for example, 5x. The field of view of the optical microscope is, for example, 3 mm square. Of the holes detected by observation, holes with a longitudinal length of 10 μm or more and 100 μm or less are identified as voids 84. The surface density of the voids 84 on the fourth main surface 4 is measured by dividing the number of voids 84 on the fourth main surface 4 by the area of ​​the fourth main surface 4.

[0090] In the required polishing amount determination step (S20), polishing and measurement of the surface density of voids 84 are repeated. In the required polishing amount determination step (S20), a threshold value for the surface density of voids 84 (hereinafter also referred to as surface density threshold) is set. If the measured value of the surface density of voids 84 is less than the surface density threshold, the polishing amount polished in the required polishing amount determination step (S20) is measured. The surface density threshold is, for example, 0.3 pieces / cm 2 The surface density threshold is, for example, 0.3 particles / cm 2 It may be the following:

[0091] 16 is an enlarged schematic diagram showing the configuration of the dummy wafer after the required polishing amount determining step. The enlarged schematic diagram shown in FIG. 16 corresponds to the enlarged schematic diagram shown in FIG. 11. The value obtained by subtracting the thickness (second thickness H2) of the dummy wafer 99 after the required polishing amount determining step (S20) from the first thickness H1 of the silicon carbide wafer 90 in the silicon carbide wafer preparing step (S10) is measured as the polishing amount polished in the required polishing amount determining step (S20). The measured polishing amount is determined as the required polishing amount.

[0092] 16, after the required polishing amount determining step (S20), the normal portion 11 is exposed. In other words, after the required polishing amount determining step (S20), the process-affected portion 12 of the dummy wafer 99 is removed.

[0093] Next, the polishing step (S30) is performed. First, a silicon carbide wafer 90 is prepared. The silicon carbide wafer 90 has the same configuration as the dummy wafer 99. The silicon carbide wafer 90 is polished using mechanical polishing. The amount of polishing of the silicon carbide wafer 90 by mechanical polishing is, for example, the required amount of polishing determined in the required amount of polishing determination step (S20). The amount of polishing of the silicon carbide wafer 90 by mechanical polishing may be greater than the required amount of polishing. However, if the amount of polishing of the silicon carbide wafer 90 by mechanical polishing is excessively large, the time required for mechanical polishing increases and the surface density of polishing marks on the fourth main surface 4 of the silicon carbide wafer 90 increases. For this reason, it is preferable that the amount of polishing of the silicon carbide wafer 90 by mechanical polishing is the required amount of polishing.

[0094] The configuration of the mechanical polishing apparatus used for mechanical polishing is different from that of polishing apparatus 30 in that support columns 39 have the role of actively pressurizing silicon carbide wafers 90, but other configurations are the same as those of polishing apparatus 30. Specifically, support columns 39 of the mechanical polishing apparatus have, for example, air cylinders. The polishing conditions for mechanical polishing are the same as the polishing conditions in the required polishing amount determination step (S20).

[0095] Fig. 17 is an enlarged schematic view showing the configuration of silicon carbide substrate 10 in the polishing step (S30). The enlarged schematic view shown in Fig. 17 corresponds to the enlarged schematic view shown in Fig. 11. As shown in Fig. 17, first main surface 1 of silicon carbide substrate 10 is smooth. The position of machine-affected portion 12 in silicon carbide substrate 10 corresponds to the position of void 84 in dummy wafer 99 (see Fig. 16) after the required polishing amount determining step (S20). Silicon carbide substrate 10 has a thickness of second thickness H2.

[0096] Next, chemical mechanical polishing (CMP) is performed on the silicon carbide wafer 90. The amount of polishing by CMP is, for example, 3 μm. The configuration of the CMP apparatus used for CMP differs from the configuration of the polishing apparatus 30 in that the support columns 39 have the role of actively pressurizing the silicon carbide wafer 90, but the other configuration is the same as the configuration of the polishing apparatus 30. Specifically, the support columns 39 of the CMP apparatus have, for example, air cylinders.

[0097] In the polishing agent used in CMP, for example, colloidal silica "PL-3H" manufactured by Fuso Chemical Industries is used as the abrasive grains. For example, dichloroisocyanuric acid Na is used as the oxidizing agent. For example, sucrose is used as the additive. In the polishing agent used in CMP, for example, 4000 cm 3 of water, 1000 cm 3 The polishing agent used in CMP contains 100g of colloidal silica, 50g of oxidizer, and 40g of additive. The amounts of water, colloidal silica, oxidizer, and additive may be changed while maintaining the ratio of each other. The hydrogen ion exponent (pH) of the polishing agent used in CMP is, for example, 2.5 or more and 3.5 or less.

[0098] In the CMP apparatus, for example, a polyurethane suede polishing cloth "Supreme (trademark)" manufactured by Nitta DuPont is used as the polishing cloth. The diameter of the surface plate is, for example, 640 mm. The rotation speed of the surface plate is, for example, 60 rpm. The rotation speed of the polishing head is, for example, 80 rpm. The oscillation speed of the polishing head is, for example, 20 mm / sec. The flow rate of the abrasive is, for example, 200 cm 3 / min. In this manner, silicon carbide substrate 10 is fabricated.

[0099] Next, the epitaxial growth step (S40) is carried out. Silicon carbide epitaxial layer 20 is formed on first main surface 1 of silicon carbide substrate 10. Of the plurality of threading dislocations 80, threading dislocations 80 present in work-affected portion 12 of silicon carbide substrate 10 are converted to form blue light-emitting defects 83. In this manner, silicon carbide epitaxial substrate 100 (see FIG. 3 ) is produced.

[0100] Silicon carbide epitaxial substrate 100 is used as a substrate for a silicon carbide semiconductor device such as a metal oxide semiconductor field effect transistor (MOSFET).

[0101] Next, the effects of silicon carbide epitaxial substrate 100 according to this embodiment will be described.

[0102] When a silicon carbide semiconductor device is fabricated using silicon carbide epitaxial substrate 100, defects exposed on second main surface 2 of silicon carbide epitaxial substrate 100 deteriorate the electrical characteristics of the silicon carbide semiconductor device. This reduces the yield of the silicon carbide semiconductor device. In a detailed investigation into the cause of the above phenomenon, the inventors found that blue light-emitting defects 83 exposed on second main surface 2 particularly affect the deterioration of the electrical characteristics of the silicon carbide semiconductor device.

[0103] Furthermore, the inventors have obtained the following knowledge while investigating the factors behind the formation of blue light-emitting defects 83. Specifically, blue light-emitting defects 83 are formed due to threading dislocations 80 present in work-affected portion 12 of silicon carbide substrate 10. From another perspective, the rate at which threading dislocations 80 are converted to blue light-emitting defects 83 varies depending on the amount of work-affected portion 12 remaining in silicon carbide substrate 10.

[0104] When determining the amount of polishing of silicon carbide substrate 10, it is considered to use the surface roughness of silicon carbide substrate 10 as an index. Polishing of silicon carbide substrate 10 and measurement of the surface roughness are repeated until the surface roughness of silicon carbide substrate 10 becomes a predetermined value or less. However, when polishing is performed so that the surface roughness of first main surface 1 of silicon carbide substrate 10 is sufficiently small, machine-affected portion 12 may not be sufficiently removed. FIG. 18 is an enlarged schematic cross-sectional view showing a state in which silicon carbide epitaxial layer 20 is formed after first main surface 1 of silicon carbide substrate 10 has been polished so that the surface roughness is sufficiently small. The enlarged schematic cross-sectional view shown in FIG. 18 corresponds to the enlarged schematic cross-sectional view shown in FIG. 3.

[0105] The process-affected portion 12 is locally formed deep in the silicon carbide wafer 90 (see FIG. 11 ). Therefore, as shown in FIG. 18 , when the silicon carbide substrate 10 is polished so that the surface roughness of the first main surface 1 is sufficiently small, only the surface layer of the process-affected portion 12 is removed, and the process-affected portion 12 formed deep in the silicon carbide wafer 90 is not removed. From another perspective, when the first main surface 1 is polished so that the surface roughness is sufficiently small, the amount of polishing is excessively small. As a result, the amount of remaining process-affected portion 12 increases. In this case, the number of threading dislocations 80 in the process-affected portion 12 increases. This increases the rate at which the threading dislocations 80 are converted to blue-luminescence defects 83.

[0106] Furthermore, at room temperature, process-affected portions 12 formed deep in silicon carbide wafer 90 do not affect the warpage of silicon carbide wafer 90. For this reason, even when silicon carbide substrate 10 is polished so that the warpage is sufficiently small, process-affected portions 12 formed deep in silicon carbide wafer 90 are not removed. Therefore, the amount of polishing becomes excessively small, similar to when silicon carbide substrate 10 is polished so that the surface roughness is sufficiently small.

[0107] On the other hand, if the polishing amount of mechanical polishing is excessively large, many polishing marks will be formed on first main surface 1 of silicon carbide substrate 10 after mechanical polishing. Therefore, in order to reduce the surface density of polishing marks on first main surface 1, it is necessary to increase the polishing amount by CMP.

[0108] FIG. 19 is a cross-sectional view schematically illustrating a state in which the amount of polishing by mechanical polishing in the polishing step is excessively large. The cross-sectional view shown in FIG. 19 corresponds to the cross-sectional view shown in FIG. 7. As shown in FIG. 19, when the amount of polishing by CMP increases, the outer periphery is more likely to come into contact with the polishing liquid than the inner periphery, resulting in greater sagging of the outer periphery of first main surface 1. Specifically, in a cross-sectional view, for example, the curvature of first outer periphery region 61 and the curvature of second outer periphery region 62 each increase. In a cross-sectional view, central region 70 becomes curved. From another perspective, the LTIR of silicon carbide substrate 10 increases in the multiple outer periphery regions 60. This deteriorates the flatness of silicon carbide epitaxial substrate 100, increasing the number of pattern defects in silicon carbide semiconductor devices fabricated using silicon carbide epitaxial substrate 100. This reduces the yield of silicon carbide semiconductor devices fabricated using silicon carbide epitaxial substrate 100.

[0109] As described above, if the polishing amount is excessively small, the amount of remaining work-affected portions 12 increases, and therefore the rate at which threading dislocations 80 are converted to blue light-emitting defects 83 increases. On the other hand, if the polishing amount is excessively large, the amount of polishing by CMP increases, and therefore the LTIR of silicon carbide substrate 10 in the plurality of outer circumferential regions 60 increases. Therefore, it is necessary to determine an optimal polishing amount in order to reduce the areal density of blue light-emitting defects and reduce the LTIR.

[0110] The inventors conducted extensive research into methods for determining the polishing amount, and as a result, they discovered the following and decided to introduce a required polishing amount determining step (S20) into the method for manufacturing silicon carbide epitaxial substrate 100 according to the present application. Process-affected portion 12 near threading dislocation 80 is more easily removed than other process-affected portions 12 and normal portion 11. Therefore, in the required polishing amount determining step (S20), by polishing so as to locally change the frictional resistance, process-affected portion 12 near threading dislocation 80 is removed deeply. As a result, process-affected portion 12 near threading dislocation 80 is detected as void 84.

[0111] Therefore, by calculating the required polishing amount to reduce the surface density of voids 84 to a predetermined number or less and performing polishing in the polishing step (S30) so that the required polishing amount is achieved, the remaining amount of work-affected portion 12 can be reduced. This reduces the rate at which threading dislocations 80 are converted to blue-luminescent defects 83. From another perspective, the thickness of work-affected portion 12 in third direction 103 can be reduced compared to when the polishing amount is excessively small (see FIGS. 3 and 18 ). Furthermore, since the polishing amount by mechanical polishing in the polishing step (S30) can be prevented from becoming excessively large, the polishing amount by CMP can be reduced. This prevents the LTIR of silicon carbide substrate 10 in outer peripheral region 60 from becoming excessively large.

[0112] In the silicon carbide epitaxial substrate 100 according to the present embodiment, when the areal density of threading screw dislocations 81 on the first main surface 1 of the silicon carbide substrate 10 is defined as the first areal density, the areal density of threading edge dislocations 82 on the first main surface 1 is defined as the second areal density, and the areal density of blue light-emitting defects 83 on the second main surface 2 is defined as the third areal density, the ratio of the third areal density to the sum of the first areal density and the second areal densities is 0.03% or less. This reduces the areal density of blue light-emitting defects 83 on the second main surface 2 of the silicon carbide epitaxial substrate 100. This makes it possible to improve the yield of silicon carbide semiconductor devices fabricated using the silicon carbide epitaxial substrate 100.

[0113] According to silicon carbide epitaxial substrate 100 according to the present embodiment, when first main surface 1 of silicon carbide substrate 10 is divided into a plurality of square regions 50, each having a side length of 10 mm, each of the plurality of square regions 50 has a plurality of first outer peripheral regions 61 located at the outermost periphery of each of the plurality of square regions 50, and a plurality of second outer peripheral regions 62 contacting the plurality of first outer peripheral regions 61. The average value of the LTIR of silicon carbide substrate 10 in the plurality of first outer peripheral regions 61 and the plurality of second outer peripheral regions 62 is 0.6 μm or less. This improves the flatness of outer peripheral region 60 of first main surface 1. This makes it possible to improve the yield of silicon carbide semiconductor devices fabricated using silicon carbide epitaxial substrate 100.

[0114] According to silicon carbide epitaxial substrate 100 according to this embodiment, the variation in overall thickness of silicon carbide substrate 10 is 6 μm or less. This improves the flatness of first main surface 1. This makes it possible to improve the yield of silicon carbide semiconductor devices fabricated using silicon carbide epitaxial substrate 100.

[0115] In silicon carbide epitaxial substrate 100 according to the present embodiment, the ratio of the third areal density to the sum of the first and second areal densities may be equal to or less than 0.02%, thereby further improving the yield of silicon carbide semiconductor devices fabricated using silicon carbide epitaxial substrate 100.

[0116] In silicon carbide epitaxial substrate 100 according to the present embodiment, the ratio of the third areal density to the sum of the first and second areal densities may be equal to or less than 0.01%, thereby further improving the yield of silicon carbide semiconductor devices fabricated using silicon carbide epitaxial substrate 100.

[0117] In silicon carbide epitaxial substrate 100 according to the present embodiment, the ratio of the third areal density to the first areal density is equal to or less than 0.2%, which allows for a further improvement in the yield of silicon carbide semiconductor devices fabricated using silicon carbide epitaxial substrate 100.

[0118] According to the silicon carbide epitaxial substrate 100 according to this embodiment, the first areal density is 1500 particles / cm 2 As a result, the areal density of threading screw dislocations 81 on the first main surface 1 is reduced. Therefore, the areal density of blue light-emitting defects 83 on the second main surface 2 can be further reduced.

[0119] According to the silicon carbide epitaxial substrate 100 according to this embodiment, the first areal density is 500 particles / cm 2 As a result, the areal density of threading screw dislocations 81 on the first main surface 1 is reduced. Therefore, the areal density of blue light-emitting defects 83 on the second main surface 2 can be further reduced.

[0120] According to the silicon carbide epitaxial substrate 100 of this embodiment, the first areal density is 100 particles / cm 2 As a result, the areal density of threading screw dislocations 81 on the first main surface 1 is reduced. Therefore, the areal density of blue light-emitting defects 83 on the second main surface 2 can be further reduced.

[0121] According to the silicon carbide epitaxial substrate 100 according to this embodiment, the second areal density is 10,000 atoms / cm 2 As a result, the surface density of threading edge dislocations 82 on the first main surface 1 is reduced. Therefore, the surface density of blue light-emitting defects 83 on the second main surface 2 can be further reduced.

[0122] According to the silicon carbide epitaxial substrate 100 according to this embodiment, the second areal density is 5000 / cm 2 As a result, the surface density of threading edge dislocations 82 on the first main surface 1 is reduced. Therefore, the surface density of blue light-emitting defects 83 on the second main surface 2 can be further reduced.

[0123] According to the silicon carbide epitaxial substrate 100 according to this embodiment, the second areal density is 2000 / cm 2 As a result, the surface density of threading edge dislocations 82 on the first main surface 1 is reduced. Therefore, the surface density of blue light-emitting defects 83 on the second main surface 2 can be further reduced.

[0124] In silicon carbide epitaxial substrate 100 according to the present embodiment, diameter D of second main surface 2 is 150 mm or more. In this manner, even in the case of silicon carbide epitaxial substrate 100 with a large diameter, the yield of silicon carbide semiconductor devices fabricated using silicon carbide epitaxial substrate 100 can be improved.

[0125] (Examples) (Sample Preparation) Next, tests using samples will be described. First, silicon carbide epitaxial substrates 100 according to Samples 1 to 7 were prepared. Samples 1 and 4 are comparative examples. Samples 2, 3, and 5 to 7 are examples.

[0126] Each of silicon carbide epitaxial substrates 100 according to Samples 1 to 7 was fabricated using the manufacturing method according to the present embodiment. The rotation speed of platen 35 in the required polishing amount determination step (S20) was set to 40 rpm or more and 100 rpm or less. The rotation speed of polishing head 31 was set to 80 rpm or more and 120 rpm or less. The oscillation speed of polishing head 31 was set to 10 mm / sec or more and 30 mm / sec or less. The mechanical polishing conditions in the polishing step (S30) were the same as the polishing conditions in the required polishing amount determination step (S20).

[0127] As shown in Table 1, Samples 1 to 4 were prepared so that the areal densities (first areal density) of threading screw dislocations 81 (TSDs) and the areal densities (second areal density) of threading edge dislocations 82 (TEDs) on first main surface 1 were approximately the same. Specifically, the first areal densities of silicon carbide epitaxial substrates 100 according to Samples 1 to 4 were each 470 / cm 2 , 500 pieces / cm 2 , 540 pieces / cm 2 , 520 pieces / cm 2 The second areal density of silicon carbide epitaxial substrates 100 according to Samples 1 to 4 was 3250 particles / cm 2 , 4000 pieces / cm 2 , 3500 pieces / cm 2 , 4100 pieces / cm 2 It was.

[0128] Samples 5 to 7 were prepared so that the first areal density and the second areal density were different from each other. Specifically, the first areal density of silicon carbide epitaxial substrates 100 according to Samples 5 to 7 was 1340 particles / cm 2 , 870 pieces / cm 2 , 200 pieces / cm 2 The second areal density of silicon carbide epitaxial substrates 100 according to Samples 5 to 7 was 9060 particles / cm 2 , 5620 pieces / cm 2 , 1870 pieces / cm 2 It was.

[0129] In the fabrication of silicon carbide epitaxial substrates 100 according to Samples 1 to 7, the threshold value of the void areal density in the required polishing amount determining step (S20) was changed. As a result, the void areal density after the required polishing amount determining step (S20) changed, as shown in Table 1. Specifically, in Samples 1 to 3, the void areal density was 0.05 / cm 2 0.6 pieces / cm or more 2 In Sample 4, the void areal density threshold was set to have the same void areal density as in Sample 2. In Samples 5 to 7, the void areal density was 0.03 / cm. 2 0.19 pieces / cm or more 2 The required polishing amount was determined for each of Samples 1 to 7 based on the set void surface density threshold.

[0130] As shown in Table 1, in Samples 1 to 4, the first areal density and the second areal density were equivalent, so the calculated polishing amount changed when the threshold value of the void areal density was changed. In Samples 5 to 7, the first areal density and the second areal density were different, so the calculated polishing amount was equivalent even though the threshold value of the void areal density was changed.

[0131] As shown in Table 1, the polishing amount of CMP in the polishing step (S30) was set to 3 μm in Samples 1 to 3 and Samples 5 to 7. In Sample 4, the polishing amount of CMP in the polishing step (S30) was set to 8 μm.

[0132] (Measurement Method) For all samples, the first areal density and the second areal density were each measured using the above-described measurement method. In measuring the first areal density and the second areal density, the first main surface 1 was observed using a Nomarski differential interference microscope. The observation field for etch pits was 0.082 cm × 0.070 cm. The first main surface 1 of the silicon carbide substrate 10 was divided into a plurality of square measurement regions. The size of each of the plurality of square measurement regions was 5 mm × 5 mm. The number of etch pits was determined in each of the plurality of square measurement regions. The value obtained by dividing the number of etch pits in the square measurement region by the area (0.082 cm × 0.070 cm) of the observation field for etch pits was determined as the areal density of threading screw dislocations 81 in the square measurement region.

[0133] The sum of the areal densities of threading screw dislocations 81 in all square measurement regions divided by the number of square measurement regions was defined as the areal density (first areal density) of threading screw dislocations 81 on first main surface 1 of silicon carbide substrate 10. Similarly, the areal density (second areal density) of threading edge dislocations 82 on first main surface 1 of silicon carbide substrate 10 was measured.

[0134] For all samples, the total thickness variation (TTV) of the silicon carbide substrate was measured. Specifically, the TTV was measured by the above-mentioned measurement method using a flatness measuring instrument "Tropel FlatMaster (trademark)" manufactured by Corning Tropel.

[0135] In all samples, the average value of the LTIR of the silicon carbide substrate in the outer circumferential region 60 was measured. Specifically, the LTIR was measured by the above-described measurement method using a flatness measuring instrument "Tropel FlatMaster (trademark)" manufactured by Corning Tropel.

[0136] The third areal density was measured for all samples. Specifically, the third areal density was measured by the above-mentioned measurement method using a PL imaging device "SemiScope (trademark) PLI-200" manufactured by Photon Design Inc. In measuring the third areal density, the magnification of the near-infrared objective lens 233 was set to 4.5 times. The measurement temperature was set to room temperature (27°C).

[0137] The color image sensor 235 was a CCD image sensor. The type of CCD element was a back-illuminated deep depletion type. The CCD image sensor was an "excelon (trademark)" manufactured by Teledyne. The imaging wavelength range was 310 nm or more and 1024 nm or less. The element format was 1024 ch x 1024 ch. The image area was 13.3 mm x 13.3 mm. The element size was 13 μm x 13 μm.

[0138] For all samples, the measured first areal density, second areal density, and third areal density were used to calculate the ratio of the third areal density to the sum of the first areal density and the second areal density, and the ratio of the third areal density to the first areal density.

[0139] (Measurement results)

[0140]

[0141] If the amount of polishing by mechanical polishing is excessively large, polishing marks on first main surface 1 of silicon carbide substrate 10 will increase, and therefore the amount of polishing by CMP must be increased. In this case, the outer periphery is more likely to come into contact with the polishing liquid in CMP than the inner periphery, resulting in greater sagging of the outer periphery of first main surface 1. In other words, both TTV and LTIR increase. On the other hand, according to the method for manufacturing silicon carbide epitaxial substrate 100 of this embodiment, the amount of polishing by mechanical polishing is the required amount of polishing determined in the required amount of polishing determination step (S20). Therefore, it is possible to prevent the amount of polishing by mechanical polishing from becoming excessively large, and to prevent an increase in the amount of polishing by CMP. As a result, it is possible to prevent an increase in both TTV and LTIR.

[0142] As shown in Table 1, when the TTV was compared among Samples 1 to 7, the TTV was 6 μm or less when the amount of polishing by CMP was 3 μm or less. When the LTIR was compared among Samples 1 to 7, the average value of LTIR in the outer circumferential region 60 was 0.6 μm or less when the amount of polishing by CMP was 3 μm or less. These results confirmed that the increase in each of the TTV and LTIR could be suppressed by reducing the amount of polishing by CMP.

[0143] As shown in Table 1, when the ratio of the third areal density to the total value of the first areal density and the second areal density is compared in Samples 1 to 7, the void areal density after the required polishing amount determination step (S20) is 0.3 pieces / cm 2 Similarly, it was confirmed that when the required polishing amount determining step (S20) is performed, the ratio of the third areal density to the total value of the first and second areal densities is 0.03% or less. 2 Similarly, it was confirmed that when the required polishing amount determining step (S20) is performed, the ratio of the third areal density to the total value of the first and second areal densities is 0.02% or less. 2 It has been confirmed that in the following cases, the ratio of the third areal density to the total value of the first areal density and the second areal density is 0.01% or less.

[0144] As shown in Table 1, when the ratio of the third areal density to the first areal density is compared in Samples 1 to 7, the void areal density after the required polishing amount determination step (S20) is 0.3 pieces / cm 2 It has been confirmed that in the following cases, the ratio of the third areal density to the first areal density is 0.2% or less.

[0145] According to the above results, in the method for manufacturing a silicon carbide epitaxial substrate according to this embodiment, the void surface density after the required polishing amount determination step (S20) is 0.3 / cm 2It has been confirmed that in the following cases, silicon carbide substrate 10 has a small LTIR and silicon carbide epitaxial substrate 100 having a small areal density of blue light-emitting defects 83 on second main surface 2 .

[0146] The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present invention is defined by the claims, not by the above-described embodiments, and is intended to include meanings equivalent to the claims and all modifications within the scope thereof.

[0147] 1 First main surface, 2 Second main surface, 3 Third main surface, 4 Fourth main surface, 5 Fifth main surface, 6 Interface, 7 Orientation flat portion, 8 Arc-shaped portion, 9 Outer peripheral side surface, 10 Silicon carbide substrate, 11 Normal portion, 12 Process-affected portion, 20 Silicon carbide epitaxial layer, 30 Polishing apparatus, 31 Polishing head, 32 Abrasive supply portion, 33 Abrasive, 34 Polishing cloth, 35 Surface plate, 37 Support plate, 38 Weight, 39 Support, 41 First rotating shaft, 42 Second rotating shaft, 43 Center-side oscillation end, 50 Square region, 60 Outer peripheral region, 61 First outer peripheral region, 62 Second outer peripheral region, 70 Central region, 80 Threading dislocation, 81 Threading screw dislocation, 82 Threading edge dislocation, 83 Blue luminescence defect, 84 Void, 90 Silicon carbide wafer, 99 dummy wafer, 100 silicon carbide epitaxial substrate, 101 first direction, 102 second direction, 103 third direction, 104 fourth direction, 111 first rotation direction, 112 second rotation direction, 113 oscillation direction, 200 color photoluminescence imaging device, 220 excitation light generation unit, 221 light source unit, 222 light guide unit, 223 filter unit, 230 imaging unit, 231 control unit, 232 stage, 233 near-infrared objective lens, 235 color image sensor, D diameter, H1 first thickness, H2 second thickness, L0 least squares plane, L1 first highest point plane, L2 first lowest point plane, L3 second highest point plane, L4 second lowest point plane, LE excitation light, LL photoluminescence light, P1 first highest point, P2 First lowest point, P3 Second highest point, P4 Second lowest point, T1 First highest point height, T2 First lowest point height, T3 Second highest point height, T4 Second lowest point height, W1 First length, W2 Second length, θ Inclination angle.

Claims

1. a silicon carbide substrate including a first main surface; a silicon carbide epitaxial layer provided on the first main surface, a threading screw dislocation in the silicon carbide substrate; a threading edge dislocation in the silicon carbide substrate; blue light-emitting defects in the silicon carbide epitaxial layer; the silicon carbide epitaxial layer includes a second main surface opposite an interface between the silicon carbide substrate and the silicon carbide epitaxial layer; the blue light-emitting defect is exposed at the second major surface, When photoluminescence light generated from the blue emission defect by irradiating the blue emission defect with excitation light is expressed in an HSV color space, H is 180° or more and 230° or less, S is 60 or more and 170 or less, and V is 190 or more and 255 or less, When the first main surface is divided into a plurality of square regions, each of which has a side length of 10 mm, the plurality of square regions include a plurality of first outer peripheral regions located on the outermost periphery of the plurality of square regions, and a plurality of second outer peripheral regions in contact with the plurality of first outer peripheral regions, an average value of LTIR of the silicon carbide substrate in the plurality of first outer periphery regions and the plurality of second outer periphery regions is 0.6 μm or less; When the areal density of the threading screw dislocations on the first main surface is defined as a first areal density, the areal density of the threading edge dislocations on the first main surface is defined as a second areal density, and the areal density of the blue light-emitting defects on the second main surface is defined as a third areal density, a ratio of the third areal density to a sum of the first areal density and the second areal density is 0.03% or less.

2. The silicon carbide epitaxial substrate according to claim 1 , wherein a total thickness variation of said silicon carbide substrate is 6 μm or less.

3. 3 . The silicon carbide epitaxial substrate according to claim 1 , wherein a ratio of said third areal density to a sum of said first areal density and said second areal density is equal to or less than 0.02%. 4 .

4. 4 . The silicon carbide epitaxial substrate according to claim 3 , wherein a ratio of said third areal density to a sum of said first areal density and said second areal density is equal to or less than 0.01%.

5. 3 . The silicon carbide epitaxial substrate according to claim 1 , wherein a ratio of said third areal density to said first areal density is equal to or less than 0.2%. 4 .

6. The first areal density is 1500 particles / cm 2 3. The silicon carbide epitaxial substrate according to claim 1, wherein:

7. The first areal density is 500 particles / cm 2 7. The silicon carbide epitaxial substrate according to claim 6, wherein:

8. The first surface density is 100 particles / cm 2 8. The silicon carbide epitaxial substrate according to claim 7, wherein:

9. The second surface density is 10,000 particles / cm 2 3. The silicon carbide epitaxial substrate according to claim 1, wherein:

10. The second surface density is 5000 particles / cm 2 10. The silicon carbide epitaxial substrate of claim 9, wherein:

11. The second surface density is 2000 particles / cm 2 11. The silicon carbide epitaxial substrate of claim 10, wherein:

12. 3. The silicon carbide epitaxial substrate according to claim 1, wherein the second main surface has a diameter of 150 mm or more.

13. 3. The silicon carbide epitaxial substrate according to claim 1, wherein the silicon carbide substrate has an electrical resistivity of 10 mΩ·cm or more.