Soluble core for high-pressure casting and manufacturing method thereof

The soluble core for high-pressure casting, using a low-melting-point water-soluble salt mixture with high heat capacity, addresses the limitations of existing technologies by enabling the production of thick-walled products with complex shapes and facilitating easy core extraction, improving productivity and economics.

JPWO2023167342A5Active Publication Date: 2024-10-31廣川 恭子 +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024504459
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-02-28
Filing Date
2023-02-28
Publication Date
2024-10-31
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

Existing high-pressure casting technologies are limited in producing thick-walled products with complex shapes due to the use of chemical salts with high melting points and low heat capacity, leading to thermal deformation and difficulty in core extraction.

Method used

A soluble core for high-pressure casting is developed using a water-soluble chemical salt mixture with a lower melting point and higher heat capacity, combined with heat-resistant hard powder, allowing for the formation of thick-walled products with complex shapes and enabling core extraction by heating below the melting point.

Benefits of technology

The soluble core allows for the production of thick-walled products with complex internal structures without thermal deformation, facilitating easy core extraction and material reuse, enhancing productivity and economic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023167342000001
    Figure 2023167342000001
Patent Text Reader

Abstract

The present invention pertains to a soluble core for high-pressure casting and a manufacturing method therefor. The manufacturing method of the soluble core for high-pressure casting according to the present invention, that is, a manufacturing method of a core in which a heat-resistant hard ceramic powder is dispersed in a water-soluble chemical salt having a melting point lower by 140 to 260 ˚C than the melting point of a casting metal and a heat capacity of 90 J / (mo·K) or greater, is a very useful technique capable of easily manufacturing a core for high-pressure casting of metals such as aluminum and magnesium, and because the core extraction method enables the core in a cast product to be easily extracted by heating the core at a temperature equal to or lower than the melting point of the casting metal, and the core material can be recycled, the manufacturing method is highly advantageous in terms of productivity and economy.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a soluble core for high pressure casting. of The present invention relates to a manufacturing method and a soluble core manufactured by the manufacturing method, and more particularly to a soluble core for high pressure casting using a low melting point water-soluble chemical salt having a melting point lower than that of a casting alloy. of The present invention relates to a manufacturing method and a soluble core having a complex internal shape manufactured by said manufacturing method. [Background technology]

[0002] Conventionally, core technology is required to manufacture castings with complex internal structures or undercuts. That is, in the case of gravity casting, a collapsible core made of hard sand is generally used, or a technology such as U.S. Patent No. 4,629,708 is used in which a water-soluble chemical salt is used for casting and then dissolved in water or steam.

[0003] In high-pressure casting such as squeeze casting and die casting, U.S. Patent Nos. 3,963,818 and 3,407,864 propose a core technology in which water-soluble chemical salts with high melting points are molded under high pressure. U.S. Patent No. 3,459,253 also discloses a method of molding a core by injecting a slurry that has been heated to over 700°C and melted into a mold.

[0004] Meanwhile, Korean Patent Publication No. 10-2002-0009334 discloses a high-pressure casting core technology using a chemical salt with a lower melting point than the alloy to be cast. However, the casting product manufactured by the above technology is useful for manufacturing die-cast products with a relatively low heat capacity of the casting alloy, such as aluminum or magnesium alloys with a thickness of about 25 mm. However, there are limitations in the application of the above technology to the manufacture of high-pressure casting products, such as molten metal forging and die casting, for thick-walled products with a high heat capacity of 25 mm or more or products with a large change in thickness.

[0005] Therefore, there is a need for a casting manufacturing method that can be effectively applied to the production of die-cast products of products with high heat capacity of casting alloys, can form thick products, and can transfer the die-cast product to the interface of the core without melting or thermally changing the die-cast product. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Republic of Korea Patent Publication No. 10-2002-0009334 (2002.02.01) Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been invented to solve the above-mentioned problems of the prior art, and an object of the present invention is to provide a soluble core for high pressure casting, which is made of a water-soluble chemical salt having a lower melting point and a higher heat capacity than a casting alloy, and can be used to high pressure cast a thick-walled product having a complex shape inside. of A method of manufacture is provided.

[0008] Another object of the present invention is to reduce the melting point of the casting metal by 140 ℃ It has a melting point 260℃ lower than that of the conventional method, and its heat capacity is 90J / ( Mol A core for high pressure casting is manufactured by injecting molten chemical salt containing heat-resistant hard powder uniformly dispersed so that the temperature is equal to or higher than K into a core mold and solidifying it. of A manufacturing method and a casting using a soluble core for high pressure casting manufactured by the above manufacturing method are heated in a temperature range below the melting point where no thermal deformation occurs, and then the core is melted. do The present invention provides a method for extracting cores. [Means for solving the problem]

[0009] In order to achieve the above object, one aspect of the present invention according to a preferred embodiment of the present invention is a soluble core for high pressure casting. of In the manufacturing process, the melting temperature is 390 ℃A step of preparing a water-soluble chemical salt mixture having a temperature of 520°C or less; and a step of uniformly dispersing and blending a heat-resistant hard powder in the water-soluble chemical salt mixture to obtain a heat capacity of 90 J / ( Mol · A process for producing molten chemical salts of K or higher About The soluble core for high pressure casting is then produced by injecting the produced molten chemical salt into a core mold and solidifying it. of It relates to a manufacturing method.

[0010] Cast products manufactured by the conventional technology can only be applied to the production of die-cast products with a relatively low heat capacity of cast alloys such as aluminum and magnesium alloys with a thickness of about 25 mm, and there was a problem that the application of the conventional technology was limited to the production of high-pressure cast products such as molten metal forging and die casting for thick-walled products with a high heat capacity of 25 mm or more and products with drastic changes in product thickness. The fusible core manufactured by high-pressure casting according to the present invention is characterized in that it is possible to mold thick-walled products with a thickness of about 40 mm, and the interface of the core is transferred as it is without melting or thermal changes, which is advantageous for high-pressure casting of thick-walled products with complex shapes embodied inside.

[0011] The water-soluble chemical salt mixture in the present invention may contain at least one selected from the group consisting of chloride-based chemical salts, carbide-based chemical salts, and sulfide-based chemical salts. The chloride-based chemical salts include NaCl, KCl, MnCl, 2, The chemical salts may include, but are not limited to, any one or more selected from the group consisting of CaCl, MgCl2, and LiCl. The carbide-based chemical salts may include, but are not limited to, any one or more selected from the group consisting of K2CO3, Li2CO3, and Na2CO3. The sulfide-based chemical salts may include, but are not limited to, any one or more selected from the group consisting of K2SO4, Na2SO4, and Li2SO4.

[0012] The heat-resistant hard powder in the present invention may contain any one or more selected from the group consisting of TiO2, Al2O3, and ZrSiO4.

[0013] The water-soluble chemical salt mixture of the present invention is 140° C. above the melting point of the casting metal. ℃ According to one embodiment of the present invention, the water-soluble chemical salt mixture is prepared by adjusting the blending ratio of at least one selected from the group consisting of chloride-based chemical salts, carbide-based chemical salts, and sulfide-based chemical salts, so that the melting point of the mixture is 390 to 260°C lower. ℃ It can be made to be ~520℃.

[0014] The cast metal in the present invention may be, but is not limited to, an aluminum alloy or a magnesium alloy.

[0015] The present invention of According to one embodiment, the melting point of the core is 390 ℃ The temperature of the molten metal to be cast is about 520℃ (670 ℃ ~720℃), but the heat capacity of the core is 90J / ( Mol Heat capacity of cast metallic phosphorus aluminum alloy (24.20J / (mol K) ) and the heat capacity of magnesium alloy (24.869 J / (mol K) ) and the thermal conductivity is 2.4×10 -4 ~1.2×10 -3 The thermal conductivity of the steel used in the casting mold is about 1.8×10 -1 Since the thermal conductivity of the core is about 1 / 100 to 1 / 200 of the cal / scm, the filled casting metal begins to cool rapidly in an instant during high-pressure casting. Since the thermal conductivity of the core is lower than that of phosphorus steel, most of the heat in the molten metal is transferred to the mold, and since the heat capacity of the core is high, it takes a lot of time and heat to melt the core. Therefore, when the temperature at which the core melts is reached, a solidified layer of the casting metal is formed at the interface between the core and the casting metal, and after a certain amount of time, a phenomenon occurs in which part of the surface of the core gradually melts, making it possible to form complex internal shapes with the casting metal.

[0016] According to one embodiment of the present invention, a method for extracting a core is to extract a casting that has been high pressure cast using the above-mentioned core by 390°C. ℃3 at temperatures above 520℃ minutes When heated gradually for about 5 minutes, unlike high pressure casting, the heat is transferred to the inside of the core, the core quickly becomes molten, and flows out of the casting, making it easy to remove from the casting. The material removed in this way can be reused as core material.

[0017] The soluble core for high pressure casting according to the present invention is of The manufacturing method may further include a step of placing the manufactured core in a high-pressure casting mold, high-pressure casting molten metal, and then heating the core to a temperature below the melting point of the casting alloy to extract the molten core.

[0018] Another aspect of the present invention relates to a fusible core for high pressure casting manufactured by the above manufacturing method.

[0019] Yet another aspect of the present invention is a method for producing a cast metal having a melting point 140° C. or higher that the melting point of the cast metal includes at least one selected from the group consisting of chloride-based chemical salts, carbide-based chemical salts, and sulfide-based chemical salts. ℃ It is a water-soluble chemical salt mixture with a melting point 260℃ lower than that of conventional ceramics. Heat-resistant hard powder is uniformly dispersed and blended to achieve a heat capacity of 90J / ( Mol The present invention relates to a soluble core for high pressure casting, characterized in that it is formed from a molten chemical salt having a melting point of 1.5 K or higher.

[0020] Yet another aspect of the present invention is to heat a soluble core for high pressure casting to a temperature below the melting point of a product after high pressure casting. After heating, melting and extracting This invention relates to a method for extracting soluble cores for high pressure casting, characterized by washing with water.

[0021] The present invention of Soluble core for high pressure casting according to one embodiment of The manufacturing method is more specifically described as follows. Specifically, the soluble core for high pressure casting in the present invention is made by mixing any one selected from the group consisting of chloride-based chemical salts, carbide-based chemical salts, and sulfide-based chemical salts, and the melting temperature of the water-soluble chemical salt mixture is 390 ℃The heat capacity of the molten chemical salt can be increased to 90 J / ( Mol ·K) or more.

[0022] In the present invention, the blending ratio for producing the water-soluble chemical salt mixture can be changed in various ways, and various embodiments can be used. ℃ ~520℃) and the heat capacity of molten chemical salt is 90J / ( Mol ·K) or higher, so it is not limited to specific ingredients and mixing ratios.

[0023] In accordance with one embodiment of the present invention, the water-soluble chemical salt mixtures are 45.5:33.5:20 KCl:MnCl2:NaCl, 41.6:2.2:8.8:47.4 CaCl2:KCl:MgCl2:NaCl, 60:40 CrCl2:KCl, 25:43.5:31.5 K2CO3:Li2CO3:Na2CO3, 55:45 K2CO3:MgCO3, 18:82 K2S ... The aqueous chemical salt mixtures may include, but are not limited to, O4:Li2SO4, 75:25 K2SO4:Na2SO4, 52.9:27.2:19.8 LiCl:Li2SO4:Li2CO3, 54.8:29:16.1 LiCl:Li2SO4:NaCl, 52.9:19.8:27.2 LiCl:Li2CO3:Li2SO4, and 14:86 CaSO4:LiCl.

[0024] in particular, the Examples of component blend ratios, melting temperatures, and heat capacities using some chloride-based chemical salts, carbide-based chemical salts, and sulfide-based chemical salts will be specifically described with examples shown in the table. Table 1 TIFF2023167342000001.tif96170

[0025] As shown in Table 1 above, the chloride-based chemical salt KCl, MnCl2, and NaCl are mixed in a ratio of 45.5:33.5:20 (Mol%). in When mixed and melted, the melting point is 390°C and the heat capacity is 92J / ( Mol ·K) level.

[0026] In addition, the carbide chemical salt K2CO3, Li2CO3, and Na2CO3 are mixed in a ratio of 25:43.5:31.5 (Mol%), as shown by the symbol CO-397. mixture When melted, its melting point is 397°C and its heat capacity is 102 J / ( Mol ·K).

[0027] In addition, the sulfide chemical salt K2SO4 and Li2SO4 are mixed in a ratio of 18:82 (Mol%), as shown by the symbol SO-520. mixture When melted, its melting point is 520°C and its heat capacity is 108J / ( Mol ·K).

[0028] In addition, when chloride-based chemical salts, sulfide-based chemical salts, carbide-based chemical salts, LiCl, Li2SO4, and Li2CO3 are mixed and melted in a ratio of 52.9:27.2:19.8 (Mol%), as in SC-455, the melting point is about 455°C and the heat capacity is 94 J / ( Mol ·K).

[0029] Similarly, when chloride-based chemical salts, carbide-based chemical salts, sulfide-based chemical salts, LiCl, Li2CO3, and Li2SO4 are mixed and melted in a ratio of 52.9:19.8:27.2 (Mol%), as in CSL-445, the melting point is about 445°C and the heat capacity is 98 J / ( Mol It is possible to produce raw materials for cores for high pressure casting (approximately 1.5K).

[0030] By uniformly dispersing and blending heat-resistant hard ceramic particles such as TiO2, Al2O3, and ZrSiO4, the heat capacity of the material is increased to 90J / ( Mol The molten chemical salt mixture is prepared so that the temperature is 10 K or higher, and then poured into the core mold to solidify. Specifically, the heat-resistant hard ceramic particles such as TiO2, Al2O3, and ZrSiO4 can be more uniformly dispersed, and the hard ceramic powder can be mixed at a temperature of 10 %By adding about 40% (wt%), the heat capacity of the core can be further increased, and the mechanical strength can be improved, resulting in improvements.

[0031] In this way, a solution in which hard ceramic powder is dispersed and mixed can be poured into a core mold and solidified to produce a soluble core for high pressure casting. Effect of the Invention

[0032] Fusible core for high pressure casting according to the present invention of According to the manufacturing method, the casting temperature is 140°C above the melting point of the metal. ℃ It has a melting point 260℃ lower than that of the conventional method, and its heat capacity is 90J / ( Mol The manufacturing method of cores in which heat-resistant hard ceramic powder is dispersed in a water-soluble chemical salt with a temperature of 0.1 K or higher is a very useful technology that can easily manufacture cores for high-pressure casting of metals such as aluminum and magnesium. The core extraction method for castings can also be easily performed by heating at a temperature below the melting point of the casting metal. do This has enormous productive and economic benefits, as it can be extracted and the core material can be recycled.

[0033] In addition, there is an advantage that a thick-walled product having a complex internal shape can be high-pressure cast using a high-pressure casting core made of a water-soluble chemical salt having a lower melting point and higher heat capacity than the casting alloy of the present invention. [Brief description of the drawings]

[0034] [Figure 1] FIG. 1 shows the shape of a core for high pressure casting (symbol CL-460) according to an embodiment of the present invention. [Diagram 2] FIG. 2 shows a front view and a side view of a sample used in an embodiment of the present invention with a high-pressure casting die and a core attached thereto. [Diagram 3] FIG. 3 shows a thermal analysis graph of a soluble core (designated CL-460) according to an embodiment of the present invention. [Figure 4]FIG. 4 is a photograph of a high-pressure casting product using a soluble core (coded CL-460) according to an embodiment of the present invention. [Diagram 5] FIG. 5 shows a photograph of the core after heating and extraction after high pressure casting using a soluble core (code CL-460) according to an embodiment of the present invention. [Figure 6] FIG. 6 shows a photograph of the interface after the core of a high pressure casting product using a soluble core (code CL-460) according to an embodiment of the present invention is heated and extracted. [Figure 7] 7 shows a thermal analysis graph of a soluble core (designated SL-512) according to an embodiment of the present invention. The thermal analysis method used here is Differential Scanning Calorimetry (DSC), which measures the difference in energy input between a sample and a reference material as a function of temperature while changing the temperatures of the sample and the reference material. [Figure 8] FIG. 8 shows a photograph of the interface after the core of a high pressure casting product using a soluble core (code SL-512) according to an embodiment of the present invention is heated and extracted. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0036] The present invention can be modified in various ways and can have various embodiments, but specific embodiments are illustrated in the drawings and specifically described in the detailed description. This is not intended to limit the present invention to the specific embodiments, and should be interpreted as including all modifications and equivalents within the spirit and technical scope of the present invention.

[0037] The terms used in this application are merely used to describe specific embodiments and are not intended to limit the present invention. A singular expression may include a plural expression unless otherwise clearly indicated in the context.

[0038] Unless otherwise defined, all terms used herein, including technical or scientific terms, may have the same meaning as commonly understood by a person having ordinary skill in the art to which the present invention belongs. Terms as defined in commonly used dictionaries may be interpreted to have a meaning consistent with the contextual meaning of the relevant art. Unless expressly defined in this application, they may not be interpreted in an ideal or overly formal sense.

[0039] Specific embodiments of the present invention will now be described with reference to the accompanying drawings. Example 1

[0040] The chloride-based chemical salt, CaCl2, KCl, MgCl2, and NaCl are mixed in the ratio of 41.6:2.2:8.8:47.4 (Mol%), as shown by the symbol CL-460. in When mixed and melted, the melting point is 460°C and the heat capacity is 102J / ( Mol 14 (wt%) of TiO2 hard particles of about 20μm and 30 (wt%) of Al2O3 powder of about 80μm are mixed into this, and the solution heated to about 550℃ is poured into a core mold preheated to 200℃ and allowed to gradually solidify to produce a soluble core.

[0041] The thermal analysis results of the soluble core for high-pressure casting manufactured in this way showed that it started to melt at 460℃ (melting point 456℃) as shown in Figure 3. The core manufactured in this way was attached to a high-pressure casting mold with a casting thickness of about 40mm as shown in Figure 2, and the performance of the core was evaluated by high-pressure die casting using AC4C aluminum alloy. For high-pressure casting, AC4C aluminum alloy heated to 700℃ was used, the gate injection speed of the molten metal was 55m / sec, and the final pressure was 980kg / cm. 2 After casting, the core was extracted by heating the casting at 500°C for about 5 minutes to dissolve the core. do After extraction, it was washed with water.

[0042] Figure 5 shows the core being heated after high pressure casting using the above manufacturing method. doThis is the shape of the extracted casting. It is possible to mold a thick-walled product with a thickness of about 40 mm, and it can be seen that the shape of the core is transferred as it is without any melting changes. As in Figure 6, it can be seen that the casting surface is clean.

[0043] On the other hand, when the melting temperature of the core was 390°C or less, a reaction layer was formed on the boundary surface of the casting, and the core was not suitable for use in high-pressure casting of thick-walled products of about 40 mm. Example 2

[0044] When the sulfide-based chemical salt CaSO4 and the chloride-based chemical salt LiCl are mixed and melted at a ratio of 14:86 (mol%), as in SL-512, the melting point is 512°C and the heat capacity is 96 J / ( Mol ·K) is about 20μm TiO2 hard particles 10 (wt%) and 120μm ZrSiO4 powder The powder is mixed at about 35 wt%, and the solution heated to about 580°C is poured into a core mold preheated to 300°C and allowed to gradually solidify to produce a soluble core. The thermal analysis results of the soluble core for high-pressure casting produced in this way show that the peak due to crystal structure change at 428°C and the peak due to the latent heat of fusion begin at 512°C (melting point 512°C) as shown in Figure 7. Such a core was mounted in a high-pressure casting mold as shown in Figure 2, and the performance of the core was evaluated using a high-pressure die casting method using AC4C aluminum alloy. For high-pressure casting, AC4C aluminum alloy heated to 700°C was used, the gate injection speed of the molten metal was 55m / sec, and the final pressure was 980kg / cm 2 After casting, the core was extracted by heating the casting at 530°C for about 10 minutes to dissolve the core. do After extraction, it was washed with water.

[0045] Figure 8 shows the process of manufacturing a thick-walled product by high-pressure casting, followed by heating the core. do This is a cross section of the extracted casting. It is possible to form a thick-walled product with a thickness of about 40 mm, and it can be seen that the boundary surface of the core is transferred as it is without melting or thermal changes.

[0046] On the other hand, if the melting temperature of the core is 520℃ or higher, it is possible to melt the core without causing thermal changes in the casting. Melt and extract Hard to break, thick-walled product of It was not suitable for use as a core for high pressure casting.

[0047] The present invention has been described in detail above through specific examples. However, these are for the purpose of specifically explaining the present invention, and the present invention is not limited thereto. It is clear that the present invention can be modified or improved by a person having ordinary knowledge in the relevant field within the technical concept of the present invention.

[0048] Any mere variations or modifications of the present invention should belong to the scope of the present invention, and the specific scope of protection of the present invention will be made clear by the appended claims.

Claims

1. A method for producing a soluble core for high pressure casting, comprising the steps of: preparing a water soluble chemical salt mixture having a melting temperature of 390°C to 520°C; a step of uniformly dispersing and blending a heat-resistant hard powder into the water-soluble chemical salt mixture to produce a molten chemical salt having a heat capacity of 90 J / (mol K) or more; The method for producing a soluble core for high pressure casting further includes a step of injecting the produced molten chemical salt into a core form and solidifying it to produce a core.

2. In the method for producing a soluble core for high pressure casting according to claim 1, The water-soluble chemical salt mixture includes at least one selected from the group consisting of chloride-based chemical salts, carbide-based chemical salts, and sulfide-based chemical salts.

3. In the method for producing a soluble core for high pressure casting according to claim 2, The chloride-based chemical salts are NaCl, KCl, MnCl 2 , CaCl, MgCl 2 and LiCl, The carbide-based chemical salt is K 2 CO 3 , Li 2 CO 3 and Na 2 CO 3 At least one selected from the group consisting of: The sulfide-based chemical salt is K 2 SO 4 , Na 2 SO 4 and Li 2 SO 4 A method for producing a soluble core for high pressure casting, comprising at least one selected from the group consisting of:

4. In the method for producing a soluble core for high pressure casting according to claim 2, The water-soluble chemical salt mixture had a mixing ratio (mol%) of 45.5:33.5:20 KCl:MnCl 241.6:2.2:8.8:47.4 NaCl, 41.6:2.2:8.8:47.4 CaCl 2 :KCl:MgCl 2 :NaCl, 60:40 CrCl 2 :KCl, 25:43.5:31.5 K 2 CO 3 :Li 2 CO 3 : Na 2 CO 3 , 55:45 K 2 CO 3 : MgCO 3 , 18:82 K 2 SO 4 :Li 2 SO 4 , 75:25 K 2 SO 4 : Na 2 SO 4 , 52.9:27.2:19.8 LiCl:Li 2 SO 4 :Li 2 CO 3 , 54.8:29:16.1 LiCl:Li 2 SO 4 :NaCl, 52.9:19.8:27.2 LiCl:Li 2 CO 3 :Li 2 SO 4 and CaSO at 14:86 4 1. A method for producing a soluble core for high pressure casting, comprising the steps of:

5. In the method for producing a soluble core for high pressure casting according to claim 1, The heat-resistant hard powder is TiO 2 , Al 2 O 3 and ZrSiO 4 A method for producing a soluble core for high pressure casting, comprising one or more selected from the group consisting of:

6. In the method for producing a soluble core for high pressure casting according to claim 1, The water-soluble chemical salt mixture has a melting point that is 140° C. to 260° C. lower than the melting point of the casting metal.

7. In the method for producing a soluble core for high pressure casting according to claim 1, A method for manufacturing a fusible core for high pressure casting, wherein the casting metal is an aluminum alloy or a magnesium alloy.

8. In the method for producing a soluble core for high pressure casting according to claim 1, The method for producing a soluble core for high pressure casting further comprises the steps of placing the produced core in a formwork for high pressure casting, high pressure casting molten metal, and then heating the core to a temperature below the melting point of the casting alloy to extract the molten core.

9. A soluble core for high pressure casting, characterized in that it is formed from a molten chemical salt having a heat capacity of 90 J / (mol·K) or more, by uniformly dispersing and blending a heat-resistant hard powder in a water-soluble chemical salt mixture having a melting point 140°C to 260°C lower than the melting point of the casting metal, the water-soluble chemical salt mixture including any one selected from the group consisting of chloride-based chemical salts, carbide-based chemical salts, and sulfide-based chemical salts.

10. The soluble core for high pressure casting according to claim 9, The chloride-based chemical salts are NaCl, KCl, MnCl 2 , CaCl, MgCl 2 and LiCl, The carbide-based chemical salt is K 2 CO 3 , Li 2 CO 3 and Na 2 CO 3 At least one selected from the group consisting of: The sulfide-based chemical salt is K 2 SO 4 , Na 2 SO 4 and Li 2 SO 4 A soluble core for high pressure casting, comprising at least one selected from the group consisting of:

11. The soluble core for high pressure casting according to claim 9, The water-soluble chemical salts were mixed in a ratio (mol%) of KCl:MnCl of 45.5:33.5:

20. 2 41.6:2.2:8.8:47.4 NaCl, 41.6:2.2:8.8:47.4 CaCl 2 :KCl:MgCl 2 :NaCl, 60:40 CrCl 2 :KCl, 25:43.5:31.5 K 2 CO 3 :Li 2 CO 3 : Na 2 CO 3 , 55:45 K 2 CO 3 : MgCO 3 , 18:82 K 2 SO 4 :Li 2 SO 4 , 75:25 K 2 SO 4 : Na 2 SO 4 , 52.9:27.2:19.8 LiCl:Li 2 SO 4 :Li 2 CO 3 , 54.8:29:16.1 LiCl:Li 2 SO 4 :NaCl, 52.9:19.8:27.2 LiCl:Li 2 CO 3 :Li 2 SO 4 and CaSO at 14:86 4 1. A soluble core for high pressure casting, characterized in that the soluble chemical salts are selected from the group consisting of a mixture of water soluble chemical salts of LiCl.

12. A method for extracting a soluble core for high pressure casting according to claim 9, comprising heating the soluble core for high pressure casting to a temperature not higher than the melting point of a product after high pressure casting to melt it, extracting it, and then washing it with water.

Citation Information

Patent Citations

  • A method for manufacturing a dissolution type core fora casting, a core and a method for extracting the core

    KR1020020009334A