Battery
Patent Information
- Application Number
- JP2024511735
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-03-14
AI Technical Summary
Batteries with low-temperature cycle characteristics deteriorate due to insufficient suppression of metallic lithium precipitation on the negative electrode, leading to increased internal resistance and heat generation during charging and discharging.
A battery design featuring strip-shaped electrodes with active material non-coated portions and a specific electrolyte composition, including fluoroethylene carbonate and lithium tetrafluoroborate, to prevent metallic lithium precipitation and maintain low internal resistance.
The battery exhibits improved cycle characteristics in low-temperature environments with reduced gas generation and increased energy density, while maintaining low internal resistance.
Smart Images

Figure 2023189564000001 
Figure 2023189564000002 
Figure 2023189564000003
Abstract
Description
battery
[0001] The present disclosure relates to batteries.
[0002] Patent Document 1 describes a battery including an electrode winding body in which a strip-shaped positive electrode and a strip-shaped negative electrode are stacked and wound with a separator interposed therebetween, and the positive electrode and the negative electrode have uncovered portions that are not covered with an active material layer. Here, the uncovered portions are joined to current collector plates at the ends of the electrode winding body, bent toward the central axis of the wound structure, and overlap each other.
[0003] Patent Document 2 describes that in a secondary battery, when the content of fluoroethylene carbonate (FEC) in the solvent of the nonaqueous electrolyte is set to 2 to 50 volume % and the content of lithium tetrafluoroborate (LiBF4) is set to 0.1 to 1.0 mol / L, the action of FEC can suppress the deposition of metallic lithium that occurs on the surface of the negative electrode, thereby improving cycle characteristics, and the action of LiBF4 can suppress the decomposition of FEC during storage in a charged state, thereby suppressing the generation of gas associated with decomposition.
[0004] International Publication No. 2021 / 020237 Japanese Patent Application Laid-Open No. 2007-294432
[0005] However, a battery having the structure shown in Patent Document 1 generates little heat during charging and discharging due to its low battery resistance. Therefore, if the composition of the electrolyte solution is that shown in Patent Document 2, deposition of metallic lithium on the surface of the negative electrode in a low-temperature environment cannot be sufficiently suppressed, and cycle characteristics in a low-temperature environment may be degraded.
[0006] The present invention has been made in view of the above, and has an object to provide a battery that has excellent cycle characteristics in a low-temperature environment.
[0007] The battery according to the present invention comprises an electrode winding body having a structure in which a strip-shaped positive electrode having a positive electrode foil and a positive electrode active material layer, and a strip-shaped negative electrode having a negative electrode foil and a negative electrode active material layer are stacked with a separator interposed therebetween and wound around a central axis, a positive electrode current collector, a negative electrode current collector, and an electrolyte, all of which are housed in an outer can, wherein the positive electrode foil has a positive electrode active material coated portion coated with the positive electrode active material layer and a positive electrode active material uncoated portion not coated with the positive electrode active material layer, and the negative electrode foil has a negative electrode active material coated portion coated with the negative electrode active material layer and a negative electrode active material uncoated portion not coated with the negative electrode active material layer. The cathode current collector plate and the cathode active material uncoated portion bent toward the central axis are joined together at an overlapping surface of the cathode active material uncoated portion, and the cathode current collector plate and the cathode active material uncoated portion bent toward the central axis are joined together at an overlapping surface of the anode active material uncoated portion, and the electrolyte solution contains 7.7 mass % or more and 11.5 mass % or less of fluoroethylene carbonate, 0.032 mass % or more and 0.048 mass % or less of lithium tetrafluoroborate, and lithium hexafluorophosphate.
[0008] According to the present invention, a battery having excellent cycle characteristics in a low-temperature environment can be provided.
[0009] FIG. 1 is a schematic cross-sectional view of a battery according to this embodiment. FIG. 2 is a diagram showing an example of the structure of the electrode winding body of the battery according to this embodiment before winding. FIG. 3 is a plan view showing an end of the battery according to this embodiment. FIG. 4 is a diagram showing an example of a cross section taken along line IV-IV in FIG. 3. FIG. 5A is a diagram showing a positive electrode current collector plate of the battery according to this embodiment. FIG. 5B is a diagram showing a negative electrode current collector plate of the battery according to this embodiment.
[0010] Hereinafter, embodiments of the present disclosure will be described, but the present disclosure is not limited to these embodiments.
[0011] In this embodiment, a cylindrical lithium ion battery will be described as an example of the battery. However, the battery according to the present invention is not limited to this, and batteries other than lithium ion batteries or batteries other than cylindrical batteries may also be used.
[0012] FIG. 1 is a schematic cross-sectional view of a battery according to this embodiment. As shown in FIG. 1 , the battery 1 according to this embodiment is, for example, a cylindrical lithium-ion battery. The battery 1 includes an outer can 11, insulating plates 12 and 13, a battery lid 14, a gasket 15, an electrode winding 20, and a safety valve mechanism 16. The battery 1 has a structure in which the insulating plates 12 and 13, the electrode winding 20, the safety valve mechanism 16, a positive electrode current collector 30A, and a negative electrode current collector 30B are housed in a space sealed by the outer can 11, the battery lid 14, and the gasket 15, and the space is filled with an electrolyte. The configuration of the battery 1 is not limited thereto, and for example, the outer can 11 may further include a positive temperature coefficient (PTC) element, a reinforcing member, and the like.
[0013] (Outer can) The outer can 11 is a member that houses the electrode winding body 20 and the like. The outer can 11 is a cylindrical container that is open at one end in the Z direction and closed at the other end. That is, the outer can 11 has an open end 11N that is the open end. The outer can 11 is made of, for example, a metal such as iron or aluminum, or an alloy. The surface of the outer can 11 may be plated with a metal such as nickel.
[0014] (Crimping structure) Here, the exterior can 11 has a crimping structure 11R formed at the open end 11N. The crimping structure 11R crimps the battery lid 14 and the safety valve mechanism 16 via a gasket 15. The crimping structure 11R is a so-called crimp structure. This seals the interior of the exterior can 11.
[0015] (Battery Lid) The battery lid 14 is a member that closes the open end 11N of the exterior can 11. The area of the battery lid 14 around the central axis of the battery 1 in the XY plane protrudes in the +Z direction. The area of the battery lid 14 other than the protruding area is in contact with the safety valve mechanism 16. This electrically connects the battery lid 14 to the safety valve mechanism 16. The battery lid 14 contains, for example, the same material as the material from which the exterior can 11 is formed.
[0016] (Gasket) The gasket 15 is a member that seals the gap between the bent portion 11P and the battery lid 14. The gasket 15 is electrically insulating and contains an insulating material. This allows the gap between the bent portion 11P and the battery lid 14 to be sufficiently sealed and prevents direct contact between the outer can 11 and the battery lid 14. The type of insulating material is not particularly limited, but examples include polymeric materials such as polybutylene terephthalate (PBT) and polypropylene (PP), with polybutylene terephthalate being preferred. The surface of the gasket 15 may be coated with asphalt, for example.
[0017] (Safety Valve Mechanism) The safety valve mechanism 16 is a mechanism for preventing the battery from exploding. The safety valve mechanism 16 has a protrusion in the -Z direction, which is in contact with a connection portion 32B of the positive current collector plate 30A (described later). This electrically connects the safety valve mechanism 16 to the positive current collector plate 30A. When the internal pressure of the outer can 11 increases due to gas generation, the safety valve mechanism 16 deforms in the +Z direction, thereby disconnecting the connection with the positive current collector plate 30A and interrupting the current. If the internal pressure of the outer can 11 increases further in this state, the safety valve mechanism 16 opens by itself, releasing the sealed state of the outer can 11 and thereby releasing the internal pressure. This prevents the battery 1 from exploding due to gas.
[0018] (Insulating Plates) The insulating plates 12 and 13 are dish-shaped plates having a thickness in the Z direction and a surface perpendicular to the winding axis of the electrode winding body 20. The insulating plate 12 is provided in the +Z direction of the electrode winding body 20, and the insulating plate 13 is provided in the −Z direction of the electrode winding body 20. That is, the insulating plates 12 and 13 are arranged so as to sandwich the electrode winding body 20 between them. The insulating plate 12 has a slit for passing the strip-shaped portion 32 of the positive current collector plate 30A. Similarly, the insulating plate 13 has a slit for passing the strip-shaped portion 34 of the negative current collector plate 30B.
[0019] (Electrode winding body) Fig. 2 is a diagram showing an example of the structure of the electrode winding body of the battery according to this embodiment before winding. The electrode winding body 20 includes a positive electrode 21, a negative electrode 22, and a separator 23. In the electrode winding body 20, a laminate in which the positive electrode 21 and the negative electrode 22 sandwich the separator 23, as shown in Fig. 2, is spirally wound. Here, the laminate in which the positive electrode 21 and the negative electrode 22 of the electrode winding body 20 sandwich the separator 23 has ends 41, 42 in the Z direction that are parallel to the XY plane. The electrode winding body 20 is housed in an outer can 11 and impregnated with an electrolyte.
[0020] The central axis of the electrode winding body 20 is a through hole. That is, a through hole 26 is provided in the electrode winding body 20. The through hole 26 is a hole for inserting a winding core for assembling the electrode winding body 20 and an electrode rod for welding. In the example according to this embodiment, the through hole 26 is provided with a center pin (not shown). The center pin is made of metal.
[0021] (Positive Electrode) The positive electrode 21 is a strip-shaped member including a positive electrode foil 211, a positive electrode active material layer 212, and an insulating layer 213. The material of the positive electrode foil 211 is, for example, a metal foil containing aluminum or an aluminum alloy, and in the example shown in this embodiment, it is an aluminum foil.
[0022] The positive electrode active material layer 212 is a layer containing a positive electrode active material. The positive electrode active material layer 212 is provided on one or both sides of the positive electrode foil 211. As shown in FIG. 2 , the positive electrode active material layer 212 covers most of the positive electrode foil 211, but the periphery of one end (the end in the +Z direction) in the short axis direction of the band is not covered. Here, the portion of the positive electrode foil 211 that is covered with the positive electrode active material layer 212 is a positive electrode active material coated portion 211A, and the portion of the positive electrode foil 211 that is not covered with the positive electrode active material layer 212 is a positive electrode active material uncoated portion 211B. The positive electrode foil 211 has the positive electrode active material coated portion 211A and the positive electrode active material uncoated portion 211B.
[0023] The positive electrode active material layer 212 includes a positive electrode active material that absorbs and releases lithium. The positive electrode material is preferably a lithium-containing compound, more specifically, a lithium-containing composite oxide, a lithium-containing phosphate compound, or the like. The lithium-containing composite oxide is an oxide containing lithium and one or more elements other than lithium as constituent elements. The lithium-containing composite oxide has, for example, a layered rock salt type or a spinel type crystal structure. The lithium-containing phosphate compound is a phosphate compound containing lithium and one or more elements other than lithium as constituent elements, and has, for example, an olivine type crystal structure.
[0024] The positive electrode active material layer 212 may further include a positive electrode binder. The positive electrode binder may be any material, and may include, for example, one or more of synthetic rubber, polymer compounds, etc. Examples of synthetic rubber include styrene-butadiene rubber, fluorine-based rubber, and ethylene propylene diene. Examples of polymer compounds include polyvinylidene fluoride and polyimide.
[0025] The positive electrode active material layer 212 may further contain a positive electrode conductive agent. The positive electrode conductive agent may be any material, including, for example, carbon. Examples of carbon include graphite, carbon black, acetylene black, and ketjen black. However, the positive electrode conductive agent is not limited to this, and may be any material having conductivity, such as a metal material or a conductive polymer.
[0026] The insulating layer 213 is laminated in a 3 mm-wide section that includes the boundary between the positive electrode active material uncoated portion 211B and the positive electrode active material layer 212. The insulating layer 213 is laminated over the entire surface of the positive electrode active material uncoated portion 211B on the separator 23 side. By providing the insulating layer 213 in this manner, it is possible to prevent the battery 1 from short-circuiting when foreign matter enters between the negative electrode active material layer 222 and the positive electrode active material uncoated portion 211B, and also to absorb the impact when an impact is applied to the battery 1, thereby preventing the positive electrode active material uncoated portion 211B from bending and the negative electrode 22 from short-circuiting.
[0027] (Negative Electrode) The negative electrode 22 is a strip-shaped member including a negative electrode foil 221 and a negative electrode active material layer 222 .
[0028] The material of the negative electrode foil 221 is, for example, a metal foil containing nickel, a nickel alloy, copper, or a copper alloy, and in the example shown in this embodiment, it is copper foil. The surface of the negative electrode foil 221 is roughened at least in the region that comes into contact with the negative electrode active material layer 222. The roughening is achieved, for example, by forming fine particles on the surface of the negative electrode foil 221 using an electrolytic treatment method. This improves the adhesion of the negative electrode active material layer 222 to the negative electrode foil 221 due to a so-called anchor effect.
[0029] The anode active material layer 222 is a layer containing anode active material. The anode active material layer 222 is provided on one or both sides of the anode foil 221. As shown in FIG. 2 , the anode active material layer 222 covers most of the anode foil 221, but the periphery of the other end (the end in the −Z direction) in the minor axis direction of the band is not covered. Here, the portion of the anode foil 221 that is covered with the anode active material layer 222 is the anode active material coated portion 221A, and the portion of the anode foil 221 that is not covered with the anode active material layer 222 is the anode active material uncoated portion 221B. The anode foil 221 has the anode active material coated portion 221A and the anode active material uncoated portion 221B.
[0030] The anode active material layer 222 contains an anode active material that absorbs and desorbs lithium as the anode active material. However, the anode active material layer 222 may further contain one or more of other materials such as an anode binder and an anode conductive agent.
[0031] The negative electrode active material is, for example, a carbon material. In this case, the change in the crystal structure during the absorption and desorption of lithium is very small, so a high energy density can be stably obtained. In addition, the carbon material also functions as a negative electrode conductive agent, improving the conductivity of the negative electrode active material layer 222.
[0032] Examples of carbon materials used as negative electrode active materials include graphitizable carbon, non-graphitizable carbon, and graphite. More specifically, examples of carbon materials include pyrolytic carbons, cokes, glassy carbon fibers, organic polymer compound calcined bodies, activated carbon, and carbon blacks. Examples of cokes include pitch coke, needle coke, and petroleum coke. Organic polymer compound calcined bodies are carbonized by calcining polymer compounds such as phenolic resins and furan resins at an appropriate temperature. When non-graphitizable carbon is used, the interplanar spacing of the (002) plane of the non-graphitizable carbon is preferably 0.37 nm or more and 0.34 nm or less. This range allows for favorable accumulation of lithium between carbon layers. The carbon material is not limited to this, and may be, for example, low-crystalline carbon heat-treated at a temperature of approximately 1000°C or less, or amorphous carbon. The carbon material may be fibrous, spherical, granular, or flaky.
[0033] The amounts of the positive electrode active material and the negative electrode active material are adjusted so that the open circuit voltage (i.e., battery voltage) of the battery 1 when fully charged is 4.25 V or higher. This results in a higher amount of lithium released per unit mass than when the open circuit voltage when fully charged is 4.20 V, even when the same positive electrode active material is used, and therefore a higher energy density can be obtained.
[0034] (Separator) The separator 23 is a film that electrically insulates the positive electrode 21 from the negative electrode 22. The separator 23 is made of, for example, one or more porous films such as synthetic resins and ceramics, or may be a laminate of two or more porous films. Examples of synthetic resins include polytetrafluoroethylene, polypropylene, and polyethylene.
[0035] The separator 23 may include, for example, the porous membrane or a laminate of porous membranes (hereinafter referred to as a substrate layer) described above, and a polymer compound layer provided on one or both sides of the substrate layer. The polymer compound layer may include, for example, a polymer compound such as polyvinylidene fluoride. In this case, the physical strength and chemical stability of the separator 23 can be improved. The polymer compound layer may be formed, for example, by applying a solution of a polymer compound dissolved in an organic solvent to the substrate layer and then drying the substrate layer. Here, the formation of the polymer compound layer may involve immersing the substrate layer in the solution and then drying the substrate layer. The provision of the polymer compound layer improves the adhesion of the separator 23 to the positive electrode 21 and the negative electrode 22, suppressing distortion of the electrode winding body 20 and thereby suppressing decomposition reactions of the electrolyte and leakage of the electrolyte from the substrate layer. This reduces resistance increases even with repeated charge and discharge, and suppresses battery swelling due to gas. The material of the polymer compound layer is not limited to this, and may contain insulating inorganic particles such as aluminum oxide and aluminum nitride.
[0036] In this embodiment, the positive electrode active material uncoated portion 211B is softer than the negative electrode active material uncoated portion 221B, i.e., has a lower Young's modulus. Here, the width of the positive electrode active material uncoated portion 211B is A, the width of the negative electrode active material uncoated portion 221B is B, the length from one end of the positive electrode active material uncoated portion 211B in the +Z direction to the end of the separator 23 in the Z direction is C, and the length from one end of the negative electrode active material uncoated portion 221B in the −Z direction to the end of the separator 23 in the −Z direction is D. In this case, in this embodiment, A > B and C > D, and for example, A = 7 (mm), B = 4 (mm), C = 4.5 (mm), and D = 3 (mm).
[0037] By setting this value, when the active material uncoated portions 211B, 221B are folded simultaneously from both electrode sides with the same pressure, the length in the Z direction from the end of the separator 23 in the +Z direction to the end 41 formed by folding the positive electrode active material uncoated portion 211B can be made to be approximately the same as the length in the Z direction from the end of the separator 23 in the −Z direction to the end 42 formed by folding the negative electrode active material uncoated portion 221B. This allows the folded active material uncoated portions 211B, 221B to be overlapped appropriately.
[0038] (Ends) Fig. 3 is a plan view showing the ends of the battery according to this embodiment. The ends 41, 42 are surfaces formed by bending the active material uncoated portions 211B, 221B. That is, one end 41 of the electrode wound body 20 is an end made up of the positive electrode active material uncoated portion 211B, and the other end 42 of the electrode wound body 20 is an end made up of the negative electrode active material uncoated portion 221B. The ends 41, 42 have flat surfaces that do not affect the bonding with the current collector plates 30A, 30B.
[0039] FIG. 4 is a diagram showing an example of a cross section taken along line IV-IV in FIG. 3. The structure of the end portion 41 will be described in detail below with reference to FIG. 4. As shown in FIG. 4, the end portion 41 has a surface formed by the positive electrode active material uncoated portions 211B bent in the direction of the central axis. With this structure, the radial lines from the central axis (the radius of the electrode winding), i.e., the multiple positive electrode active material uncoated portions 211B on line IV-IV, are stacked in the Z direction. This allows the positive electrode 21 to contact the positive electrode current collector plate 30A over a wide area, thereby reducing battery resistance.
[0040] The end 42 has the same structure as the end 41. That is, as shown in FIG. 4 , the end 42 has a surface on which the anode active material uncoated portions 221B bent in the central axis direction are formed. With this structure, the multiple anode active material uncoated portions 221B radially extending from the central axis are stacked in the Z direction. The anode 22 comes into contact with the anode current collector 30B over a wide area, thereby reducing the battery resistance.
[0041] Grooves 43 shown in FIG. 5B are provided in the end portions 41, 42. The grooves 43 extend from the outer peripheries of the end portions 41, 42 to the through-hole 26 having the central axis. The grooves 43 are provided to prevent the end portions 41, 42 from having an uneven surface due to wrinkles or distortions of the positive electrode active material uncoated portion 211B and the negative electrode active material uncoated portion 221B when the positive electrode active material uncoated portion 211B and the negative electrode active material uncoated portion 221B are bent. This prevents deterioration of the bond between the end portions 41, 42 and the current collector plates, and reduces resistance between the end portions 41, 42 and the current collector plates 30A, 30B.
[0042] More specifically, if the positive electrode active material uncoated portion 211B and the negative electrode active material uncoated portion 221B are folded without previously forming the grooves 43 in the end portions 41, 42, wrinkles and distortions may occur in the positive electrode active material uncoated portion 211B and the negative electrode active material uncoated portion 221B. On the other hand, if the positive electrode active material uncoated portion 211B and the negative electrode active material uncoated portion 221B are folded after previously forming the grooves 43 in the end portions 41, 42, the occurrence of wrinkles during folding can be suppressed. This allows the end portions 41, 42 to have flat surfaces with few irregularities.
[0043] (Positive electrode current collector plate) Figure 5A is a diagram showing the positive electrode current collector plate of the battery according to this embodiment. The material of the positive electrode current collector plate 30A is a metal plate made of, for example, aluminum or an aluminum alloy, or a composite material. As shown in Figure 5A, the positive electrode current collector plate 30A has a sector-shaped portion 31 and a strip-shaped portion 32.
[0044] The sectorial portion 31 is a portion that is connected to the positive electrode active material uncoated portion 211B. Holes 35 are provided in the sectorial portion 31. The sectorial portion 31 is provided between the end portion 41 and the insulating plate 12 in the battery 1. The sectorial portion 31 is welded to the end portion 41 at multiple points. This makes it possible to suppress the internal resistance of the battery. The means for joining the positive electrode current collector plate 30A and the end portion 41 is not particularly limited, and may be laser welding, for example.
[0045] The holes 35 are provided at positions that overlap with the through holes 26 in the Z direction when the end portion 41 is bonded. This structure allows the electrolyte to smoothly penetrate into the electrode wound body 20 when assembling the battery, and also makes it easier to release gas generated when the battery is in an abnormally high temperature state or an overcharged state.
[0046] The strip-shaped portion 32 is provided on a linear portion of the sector-shaped portion 31. The strip-shaped portion 32 includes an insulating portion 32A and a connecting portion 32B. The strip-shaped portion 32 is provided in the battery 1 so as to penetrate the insulating plate 12 in the Z direction. The insulating portion 32A is a portion of the strip-shaped portion 32 whose surface is covered with an insulator. Insulating tape is attached to the insulating portion 32A, or an insulating material is applied to the insulating portion 32A. The insulating portion 32A is provided at the base of the strip-shaped portion 32, i.e., between the connecting portion 32B and the sector-shaped portion 31. The connecting portion 32B is a portion that connects to the safety valve mechanism 16. The connecting portion 32B is provided at the tip of the strip-shaped portion 32. Note that if a center pin is not provided in the through-hole 26, the strip-shaped portion 32 is unlikely to come into contact with a portion at the negative electrode potential, and therefore the insulating portion 32A may not be provided. In this case, the width of the positive electrode 21 and the negative electrode 22 in the Z direction can be increased by an amount corresponding to the thickness of the insulating portion 32A, thereby making it possible to further increase the charge / discharge capacity.
[0047] (Negative electrode current collector plate) Figure 5B is a diagram showing the negative electrode current collector plate of the battery according to this embodiment. The material of the negative electrode current collector plate 30B is a metal plate made of, for example, nickel, a nickel alloy, copper, or a copper alloy, or a composite material. As shown in Figure 5B, the negative electrode current collector plate 30B has a sector-shaped portion 33 and a strip-shaped portion 34.
[0048] The sectorial portion 33 is a portion that is connected to the negative electrode active material uncovered portion 221B. Holes 36 are provided in the sectorial portion 33. The sectorial portion 33 is provided in the battery 1 between the end portion 42 and the insulating plate 13. The negative electrode current collector 30B is joined in the −Z direction of the end portion 42. The sectorial portion 33 is welded to the end portion 42 at multiple points. There are no particular limitations on the means for joining the negative electrode current collector 30B and the end portion 42, and laser welding may be used, for example. This makes it possible to suppress the internal resistance of the battery.
[0049] The holes 36 are provided at positions that overlap with the through holes 26 in the Z direction when the end portions 42 are bonded. This structure allows the electrolyte to smoothly penetrate into the electrode wound body 20 when assembling the battery, and also makes it easier to release gas generated when the battery is in an abnormally high temperature state or an overcharged state.
[0050] The belt-shaped portion 34 is provided on a linear portion of the sector-shaped portion 33. The belt-shaped portion 34 is provided in the battery 1 so as to penetrate the insulating plate 13 in the Z direction. The belt-shaped portion 34 of the negative current collector 30B is shorter than the belt-shaped portion 32 of the positive current collector 30A. The belt-shaped portion 34 is provided with a round projection 37 that is convex in the thickness direction. As a result, during resistance welding in the manufacturing process of the battery 1, the projection 37 melts due to current concentration, allowing the belt-shaped portion 34 to be welded to the closure portion of the outer can 11.
[0051] (Electrolyte) The electrolyte according to this embodiment includes a solvent and a solute. In the following description, the content of the electrolyte components in the battery 1 refers to the content in the electrolyte after the battery 1 is fully discharged. The content of the electrolyte components in the battery 1 can be determined by gas chromatography mass spectrometry or inductively coupled plasma atomic emission spectrometry. The gas chromatograph mass spectrometer used was a 5977B manufactured by Agilent Technologies. The inductively coupled plasma atomic emission spectrometer used was a PS3500DDII manufactured by Hitachi High-Tech Science.
[0052] The solvent includes a non-aqueous solvent such as an organic solvent, for example, a cyclic carbonate such as ethylene carbonate (EC) or dimethyl carbonate (DMC), a chain carbonate, a lactone, a chain carboxylic acid ester, and a nitrile (mononitrile).
[0053] The solvent further contains fluoroethylene carbonate (FEC). By including FEC, when a metallic lithium layer is deposited on the surface of the negative electrode during charging in a low-temperature environment, the metallic lithium layer on the surface of the negative electrode is covered with a film made of a solvent decomposition product, thereby suppressing a deterioration in low-temperature cycle characteristics. This is because the coating can prevent the progression of metallic lithium deposition.
[0054] The content of FEC in Battery 1 is 7.7% by mass or more relative to the electrolyte solution. By setting the content within this range, a coating having a sufficient thickness to cover the metallic lithium layer can be obtained, and therefore, deterioration of low-temperature cycle characteristics can be sufficiently suppressed.
[0055] On the other hand, if FEC is contained in excess, the generation of hydrogen fluoride (HF) is promoted when the temperature of the battery 1 rises. Hydrogen fluoride is generated by reacting with lithium carbonate (Li 2 CO 3 ) may generate large amounts of carbon dioxide and hydrocarbon gases. If a large amount of gas is generated and the internal pressure of the battery rises, the safety valve mechanism will break and the current will be cut off.
[0056] The content of FEC in the battery 1 is 11.5 mass % or less relative to the electrolyte solution. By setting the content in this range, excessive generation of hydrogen fluoride (HF) can be suppressed, and therefore generation of gas can be suppressed.
[0057] The solute is lithium hexafluorophosphate (LiPF 6 ) in an amount of 14% by mass or more and 18% by mass or less.
[0058] The solute is lithium tetrafluoroborate (LiBF 4 LiBF 4 By including the compound (I), a coating is formed on the positive electrode, and contact between the lithium carbonate present in the positive electrode and the hydrogen fluoride in the electrolyte is suppressed, so that the generation of carbon dioxide gas can be further suppressed.
[0059] LiBF in Battery 1 4 The content of is 0.032 mass % or more relative to the electrolyte. By setting it in this range, the generation of carbon dioxide gas can be more sufficiently suppressed.
[0060] On the other hand, LiBF in Battery 1 4 The content of is 0.048 mass % or less relative to the electrolyte solution. By setting the content in this range, it is possible to prevent the coating of the positive electrode from becoming excessively thick, which can prevent an increase in battery resistance.
[0061] The solvent further contains succinonitrile (SN). By including SN, SN captures metal ions in the electrolyte solution, which can prevent short-circuiting of the battery 1. The mechanism by which SN prevents short-circuiting of the battery 1 will be described in detail below with reference to FIG. 4.
[0062] 4 , in the battery 1 according to this embodiment, the positive electrode active material uncoated portion 211B is bent in the central axis direction, and therefore the positive electrode active material coated portion 211A near the end 41 is also pulled in the central axis direction, which may result in a difference in the layer spacing between adjacent positive and negative electrodes. More specifically, at the outermost periphery of the electrode winding 20, the negative electrode 22 is disposed outside the positive electrode 21. Therefore, a local increase in the layer spacing may occur between the upper end 21A of the positive electrode 21 in the outermost peripheral portion of the electrode winding 20 and the upper end 22B of the negative electrode 22 in the outermost peripheral portion of the electrode winding 20. Here, the upper end 21A of the positive electrode 21 refers to the end of the positive electrode active material coated portion 211A and the positive electrode active material layer 212 in the +Z direction, and the +Z upper end 22A of the negative electrode 22 refers to the end of the negative electrode 22, i.e., the negative electrode active material coated portion 221A and the negative electrode active material layer 222 in the +Z direction.
[0063] As a result, the potential of the positive electrode 21 increases, and when the potential of the positive electrode 21 exceeds the dissolution potential of a transition metal (e.g., nickel) in the positive electrode active material, the transition metal in the positive electrode active material dissolves into the electrolyte. If SN is not contained in the electrolyte, metal ions dissolved into the electrolyte may precipitate on the surface of the negative electrode 22. If the precipitate penetrates the separator 23, it may reach the positive electrode 21, causing a short circuit. On the other hand, if SN is contained in the electrolyte, it is thought that SN captures metal ions in the electrolyte and forms a complex containing the metal ions, preventing them from depositing on the surface of the negative electrode 22. From the above, by including SN in the electrolyte, it is possible to prevent metal ions in the electrolyte from depositing on the surface of the negative electrode 22, thereby preventing a short circuit in the battery.
[0064] The SN content of the battery 1 is 0.392 mass % or more relative to the electrolyte solution. By setting the content in this range, the SN can sufficiently capture metal ions in the electrolyte solution, thereby preventing the battery 1 from short-circuiting.
[0065] On the other hand, the SN content of the battery 1 is 0.588 mass % or less with respect to the electrolyte solution. By setting the content within this range, it is possible to prevent the coating on the surface of the negative electrode 22 from becoming excessively thick, which can prevent an increase in battery resistance.
[0066] The solute of the electrolyte is not limited to those listed above, and may be, for example, lithium perchlorate (LiClO 4 ), lithium hexafluoroarsenate (LiAsF 6 ), lithium tetraphenylborate (LiB(C 6 H 5 ) 4 ), lithium methanesulfonate (LiCH 3 SO 3 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), lithium tetrachloroaluminate (LiAlCl 4 ), dilithium hexafluorosilicate (Li 2 SiF 6 ), lithium chloride (LiCl), and lithium bromide (LiBr).
[0067] As described above, the battery 1 according to this embodiment is a battery in which the electrode winding body 20 having a structure in which the strip-shaped positive electrode 21 including the positive electrode foil 211 and the positive electrode active material layer 212, and the strip-shaped negative electrode 22 including the negative electrode foil 221 and the negative electrode active material layer 222 are stacked with the separator 23 interposed therebetween and wound around the central axis, the positive electrode current collector 30A, the negative electrode current collector 30B, and the electrolyte are housed in the outer can 11, in which the positive electrode foil 211 has the positive electrode active material coated portion 211A coated with the positive electrode active material layer 212 and the positive electrode active material uncoated portion 211B not coated with the positive electrode active material layer 212, and the negative electrode foil 221 has the negative electrode active material layer 222 coated with the negative electrode active material layer 222. The cathode active material layer 222 is formed on the cathode current collector 30A and the cathode active material layer 222 is formed on the anode current collector 30B. The cathode active material layer 222 is formed on the anode current collector 30A. The cathode active material layer 222 is formed on the cathode current collector 30A. The cathode active material layer 222 is formed on the anode current collector 30A. The cathode active material layer 222 is formed on the anode current collector 30A. The cathode active material layer 222 is formed on the anode current collector 30A. The cathode active material layer 222 is formed on the anode current collector 30A. The cathode active material layer 222 is formed on the anode current collector 30A. The cathode active material layer 222 is formed on the cathode current collector 30A. The cathode active material layer 222 is formed on the anode current collector 30B. The cathode active material layer 222 is formed on the anode current collector 30A ...A. The cathode active material layer 222 is formed on the anode current collector 30B. The cathode active material layer 222 is formed on the anode current collector 30B. The cathode active material layer 222 is formed on the anode current collector 30A. The cathode active material layer 22 4 ) and lithium hexafluorophosphate (LiPF6).
[0068] As a result, the positive electrode 21 and the negative electrode 22 have active material-uncoated portions 211B and 221B that are not coated with the active material layers 212 and 222. The active material-uncoated portions 211B and 221B are joined to the current collector plates 30A and 30B at the ends 41 and 42 of the electrode winding 20, bent toward the central axis of the wound structure, and overlapped. This reduces the internal resistance of the battery compared to a typical battery in which current extraction leads are welded to each of the positive electrode 21 and the negative electrode 22. This prevents the battery from overheating and reaching high temperatures during discharge, enabling high-rate discharge. Furthermore, by using FEC in an amount within the range disclosed herein, cycle characteristics in low-temperature environments can be improved without excessive gas generation. By using LiBF4 in an amount within the range disclosed herein, gas generation due to decomposition of FEC can be suppressed while suppressing an increase in resistance. This allows cycle characteristics in low-temperature environments to be improved while suppressing gas generation and an increase in resistance.
[0069] In a preferred embodiment, the electrolyte solution further contains 0.392 mass % to 0.588 mass % of succinonitrile (SN), which allows SN to capture metal ions in the electrolyte solution and accumulate them on the surface of negative electrode 22, thereby suppressing an increase in battery resistance and suppressing battery short-circuits due to precipitation of transition metals.
[0070] EXAMPLES Examples will be described below, but the present invention is not limited to the examples described below.
[0071] Table 1 shows the measurement results of the batteries according to Test Examples 1-1 to 1-7.
[0072]
[0073] Test Example 1-1 A battery according to Test Example 1-1 was fabricated by the following method.
[0074] A positive electrode active material was applied to a portion of the surface of the positive electrode foil 211 to provide a positive electrode active material-coated portion 211A and a positive electrode active material-uncoated portion 211B. Similarly, a negative electrode active material was applied to a portion of the surface of the negative electrode foil 221 to provide a negative electrode active material-coated portion 221A and a negative electrode active material-uncoated portion 221B. At this time, notches were provided in portions of the active material-uncoated portions 211B, 221B that corresponded to the central axis.
[0075] Then, the positive electrode 21 and the negative electrode 22, which had been pretreated by drying or the like, were stacked with the separator 23 interposed therebetween, and wound in a spiral shape so as to form a through-hole 26 in the central axis, thereby producing the wound electrode body 20.
[0076] Next, a load was applied locally to the end portions 41, 42 formed by winding the active material uncoated portions 211B, 221B, thereby forming grooves 43. A load was then applied from the outer circumferential direction of the end portions 41, 42 so that the active material uncoated portions 211B, 221B would bend toward the through-hole 26. The same pressure was then applied to the active material uncoated portions 211B, 221B simultaneously from both sides in the Z direction, thereby forming the end portions 41, 42 into flat surfaces. Thereafter, the sector-shaped portion 31 of the positive electrode current collector 30A was laser-welded to the end portion 41, and the sector-shaped portion 33 of the negative electrode current collector 30B was laser-welded to the end portion 42.
[0077] Thereafter, the strip-shaped portions 32 and 34 of the current collectors 30A and 30B were folded, and the insulating plates 12 and 13 were attached to the positive current collector 30A and the negative current collector 30B. The electrode winding body 20 assembled in the above steps was inserted into the outer can 11, and the bottom of the outer can 11 was welded. After the electrolyte was poured into the outer can 11, it was sealed with the gasket 15 and the battery lid 14.
[0078] Here, the battery according to Test Example 1-1 prepared was fully discharged, and then the outer can 11 was pierced and centrifuged to analyze the collected electrolyte solution. As a result, the contents of FEC, LiBF4, and SN were as shown in Table 1. Here, the contents of other components shown in Table 1 of the electrolyte solution according to Test Example 1-1 were 11.4 mass% EC, 59.87 mass% DMC, and 16.2 mass% LiPF6. The analysis of the electrolyte solution was performed using a gas chromatography mass spectrometer.
[0079] (Test Examples 1-2 to 1-7) The batteries according to Test Examples 1-2 to 1-7 were produced by the same operation as in Example 1-1, except that the FEC content of the electrolyte solution was adjusted to the content shown in Table 1. In addition, among the components of the electrolyte solutions according to Test Examples 1-2 to 1-7, the contents of the other components shown in Table 1 were adjusted so that the mass ratio of (EC + FEC):DMC and the molar concentration (mol / kg) of LiPF6 were the same as those of the electrolyte solution according to Test Example 1-1.
[0080] (Evaluation) The number of low-temperature cycles was measured for the batteries according to Test Examples 1-1 to 1-7. The number of low-temperature cycles was defined as the number of charge / discharge cycles at which the charge / discharge capacity of the battery first became less than 40% of that at the initial charge / discharge, and the measurement was carried out under the following conditions. Charging was carried out using the CCCV method until the current became equal to the charge cutoff current. Discharging was carried out using the CC method until the voltage reached the discharge cutoff voltage. Measurement temperature: 0°C Charging voltage: 4.2V Charging current: 6.5A Charging cutoff current: 0.1A Discharging current: 15A Discharging cutoff voltage: 2.5V Rest time between charge and discharge: 30 minutes
[0081] The high-temperature cutoff time was measured for the batteries according to Test Examples 1-1 to 1-7. The high-temperature cutoff time was measured by leaving the battery in an incubator at 80° C. Here, the high-temperature cutoff time was defined as the time from when the battery was placed in the incubator until the safety valve mechanism 16 ruptured.
[0082] For the batteries according to Test Examples 1-1 to 1-7, those that had a low-temperature cycle count of 500 or more and a high-temperature cutoff time of 100 hours or more were rated as passing (evaluation A), and the others were rated as failing (evaluation B).
[0083] (Results) As shown in Table 1, Test Examples 1-2 to 1-6, which are working examples, were judged to have passed the test because the number of low-temperature cycles was 500 or more and the high-temperature cutoff time was 100 or more hours. It can be seen that the batteries according to Test Examples 1-2 to 1-6 can improve the number of low-temperature cycles while suppressing gas generation. On the other hand, Test Example 1-1, which is a comparative example, was judged to have failed the test because the high-temperature cutoff time was 20 hours. It can be seen that the battery according to Test Example 1-1 cannot suppress gas generation because it contains an excessive amount of FEC. Furthermore, Test Example 1-7, which is a comparative example, was judged to have failed the test because it had only 300 low-temperature cycles. It can be seen that the battery according to Test Example 1-7 cannot improve its low-temperature cycle characteristics due to a lack of FEC.
[0084] Table 2 shows the measurement results of the batteries according to Test Examples 2-1 to 2-7.
[0085]
[0086] (Test Examples 2-1 to 2-7) The batteries according to Test Examples 2-1 to 2-7 were produced by the same operation as in Example 1-1, except that the contents of FEC and LiBF4 in the electrolyte were adjusted to the contents shown in Table 2. In addition, among the components of the electrolyte solutions according to Test Examples 2-1 to 2-7, the contents of the other components shown in Table 2 were adjusted so that the mass ratio of (EC + FEC):DMC and the molar concentration (mol / kg) of LiPF6 were the same as those of the electrolyte solution according to Test Example 1-1.
[0087] (Evaluation) The battery resistance was measured for the batteries fabricated in Test Examples 2-1 to 2-7. The battery resistance was determined by measuring the AC impedance of the fabricated batteries at 1 kHz over a voltage range of 3.35 V to 3.55 V. A HIOKI Battery HiTester 3561 was used to measure the battery resistance.
[0088] The storage life of the batteries according to Test Examples 2-1 to 2-7 was measured. The storage life was measured by leaving the fully charged batteries at a high temperature of 60°C. The storage life was defined as the time from when the battery was placed in a constant temperature bath at 60°C until the voltage fell below 4.0 V due to a short circuit.
[0089] For the batteries according to Test Examples 2-1 to 2-7, those having a battery resistance of 6.2 mΩ or less and a storage life of 600 hours or more were rated as passing (evaluation A), and others were rated as failing (evaluation B).
[0090] (Results) As shown in Table 2, Test Examples 2-2 to 2-6, which are working examples, were judged to have passed the test because the battery resistance was 6.2 mΩ or less and the storage life was 600 hours or more. It can be seen that the batteries according to Test Examples 2-2 to 2-6 can improve the storage life while suppressing an increase in battery resistance. On the other hand, Test Example 2-1, which is a comparative example, was judged to have failed the test because the battery resistance was 6.9 mΩ. It can be seen that the battery according to Test Example 2-1 contains an excessive amount of LiBF4, which increases the resistance. Furthermore, Test Example 2-7, which is a comparative example, was judged to have failed the test because the storage life was 400 hours. It can be seen that the battery according to Test Example 2-7 has a short storage life due to a lack of LiBF4.
[0091] Table 3 shows the measurement results of the batteries according to Test Examples 3-1 to 3-7.
[0092]
[0093] (Test Examples 3-1 to 3-7) The batteries according to Test Examples 3-1 to 3-7 were produced by the same operation as in Example 1-1, except that the FEC and SN contents of the electrolyte were adjusted to the contents shown in Table 3. In addition, among the components of the electrolytes according to Test Examples 3-1 to 3-7, the contents of the other components shown in Table 3 were adjusted so that the mass ratio of (EC + FEC):DMC and the molar concentration (mol / kg) of LiPF6 were the same as those of the electrolyte according to Test Example 1-1.
[0094] (Evaluation) The battery resistance and storage life of the fabricated batteries according to Test Examples 3-1 to 3-7 were measured in the same manner as in Test Examples 2-1 to 2-7.
[0095] For the batteries according to Test Examples 3-1 to 3-7, those having a battery resistance of 6.2 mΩ or less and a storage life of 600 hours or more were rated as passing (evaluation A), and others were rated as failing (evaluation B).
[0096] (Results) As shown in Table 3, Test Examples 3-2 to 3-6, which are working examples, were judged to have passed the test because the battery resistance was 6.2 mΩ or less and the storage life was 600 hours or more. It can be seen that the batteries according to Test Examples 3-2 to 3-6 can improve the storage life while suppressing an increase in battery resistance. On the other hand, Test Example 3-1, which is a comparative example, was judged to have failed the test because the battery resistance was 7.4 mΩ. It can be seen that the battery according to Test Example 3-1 has an increased resistance due to the excessive amount of SN contained in the electrolyte. Furthermore, Test Example 3-7, which is a comparative example, was judged to have failed the test because the storage life was 500 hours. It can be seen that the battery according to Test Example 3-7 has a short storage life due to a lack of SN.
[0097] The above-described embodiments are intended to facilitate understanding of the present disclosure and are not intended to limit the present disclosure. The present disclosure may be modified or improved without departing from the spirit thereof, and equivalents thereof are also included in the present disclosure.
[0098] For example, a battery 1 according to another aspect of the present invention includes an electrode winding body 20 having a structure in which a strip-shaped positive electrode 21 including a positive electrode foil 211 and a positive electrode active material layer 212 and a strip-shaped negative electrode 22 including a negative electrode foil 221 and a negative electrode active material layer 222 are stacked and wound with a separator 23 interposed therebetween, a positive electrode current collector 30A, a negative electrode current collector 30B, and an electrolyte, all of which are housed in an outer can 11. The positive electrode foil 211 has a positive electrode active material coated portion 211A coated with the positive electrode active material layer 212 and a positive electrode active material uncoated portion 211B not coated with the positive electrode active material layer 212, and the negative electrode foil 221 has an anode active material coated portion 221A coated with the anode active material layer 222 and a cathode active material uncoated portion 211B not coated with the anode active material layer 222. The positive electrode active material uncoated portion 211B is joined to the positive electrode current collector 30A at one end 41 of the electrode wound body 20, and the negative electrode active material uncoated portion 221B is joined to the negative electrode current collector 30B at the other end 42 of the electrode wound body 20, and at one end 41, an overlapping surface is formed of the positive electrode active material uncoated portion 211B bent toward the central axis of the wound structure, and at the other end 42, an overlapping surface is formed of the negative electrode active material uncoated portion 221B bent toward the central axis of the wound structure, and the electrolyte further contains 0.392 mass % or more and 0.588 mass % or less of succinonitrile (SN). As a result, SN captures metal ions in the electrolyte and prevents them from being deposited on the surface of the negative electrode 22, thereby suppressing an increase in battery resistance and suppressing short circuits in the battery due to the deposition of transition metals.
[0099] REFERENCE SIGNS LIST 1 Battery 11 Outer can 11N Open end 11P Folded portion 11R Crimping structure 12, 13 Insulating plate 14 Battery lid 15 Gasket 16 Safety valve mechanism 20 Electrode wound body 21 Positive electrode 21A Upper end 211 Positive electrode foil 212 Positive electrode active material layer 211A Positive electrode active material coated portion 211B Positive electrode active material uncoated portion 213 Insulating layer 22 Negative electrode 22A Upper end 221 Negative electrode foil 222 Negative electrode active material layer 221A Negative electrode active material coated portion 221B Negative electrode active material uncoated portion 23 Separator 26 Through hole 30A Positive electrode current collector plate 30B Negative electrode current collector plate 31 Fan-shaped portion 32 Strip-shaped portion 32A Insulating portion 32B Connection portion 33 Fan-shaped portion 34 Strip-shaped portion 35, 36 Hole 37 Projection portion 41, 42 End portion 43 Groove
Claims
1. A battery including: an electrode winding body having a structure in which a strip-shaped positive electrode having a positive electrode foil and a positive electrode active material layer, and a strip-shaped negative electrode having a negative electrode foil and a negative electrode active material layer are stacked with a separator interposed therebetween and wound around a central axis; a positive electrode current collector; a negative electrode current collector; and an electrolyte, all of which are housed in an outer can; wherein the positive electrode foil has a positive electrode active material coated portion coated with the positive electrode active material layer and a positive electrode active material uncoated portion not coated with the positive electrode active material layer; the negative electrode foil has a negative electrode active material coated portion coated with the negative electrode active material layer and a negative electrode active material uncoated portion not coated with the negative electrode active material layer; overlapping surfaces of the positive electrode active material uncoated portions bent toward the central axis are joined to the positive electrode current collector; and overlapping surfaces of the negative electrode active material uncoated portions bent toward the central axis are joined to the negative electrode current collector; The battery, wherein the electrolyte solution contains 7.7% by mass or more and 11.5% by mass or less of fluoroethylene carbonate, 0.032% by mass or more and 0.048% by mass or less of lithium tetrafluoroborate, and lithium hexafluorophosphate.
2. The battery according to claim 1, wherein the electrolyte further contains 0.392% by mass or more and 0.588% by mass or less of succinonitrile.