Phase shift mask blank, phase shift mask, and methods for manufacturing same

JPWO2023199668A5Active Publication Date: 2024-11-15NIKON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024514852
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-10
Filing Date
2023-03-10
Publication Date
2024-11-15
Estimated Expiration
2043-03-10

AI Technical Summary

Technical Problem

Current MoSi phase shift masks have long etching times using wet processes, leading to difficulties in controlling the phase shift amount, increased etchant consumption, and decreased throughput, while also affecting the quality of phase shift masks.

Method used

A phase shift mask blank with a substrate and a first layer comprising zirconium (Zr) and silicon (Si) and nitrogen (N), which provides a transmittance of 4% or more and 40% or less for a 180° phase shift at 365 nm, and is manufactured using a stacked layer structure with an inclination angle of 55° or more and 90° or less, improving pattern accuracy and reducing etching time.

Benefits of technology

The ZrSi phase shift mask blanks achieve faster etching, reduced etchant consumption, and improved pattern accuracy, enhancing the quality and throughput of phase shift masks by optimizing the phase shift layer's transmittance and inclination angle.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This phase shift mask blank has: a substrate; and a first layer that is deposited on the substrate. The first layer contains zirconium (Zr), silicon (Si), and nitrogen (N). The transmittance of the first layer at a thickness at which a 180° phase shift is imparted to light having a wavelength of 365 nm is 4-40%.
Need to check novelty before this filing date? Find Prior Art

Description

Phase shift mask blanks, phase shift masks, and methods for manufacturing the same

[0001] The present invention relates to a phase shift mask blank, a phase shift mask, and a method for manufacturing the same. This invention claims priority from Japanese Patent Application No. 2022-067715, filed on April 15, 2022, and the contents of that application are incorporated herein by reference in designated states where incorporation by reference of documents is permitted.

[0002] A phase shift mask is known in which a phase shift layer made of chromium oxide nitride is formed on a transparent substrate (see Patent Document 1). Improvements in the quality of phase shift masks have been desired.

[0003] Currently, MoSi films with an i-line (365 nm) transmittance of 5% are used as silicide-based phase shift films. To improve the phase shift effect, films with even higher transmittance have been proposed, and by increasing the nitrogen content, transmittance of up to 10% can be achieved. However, the long wet etching time required for MoSi films is a problem. Extended etching time accelerates glass etching, making it difficult to control the amount of phase shift. Furthermore, this leads to increased etchant consumption and reduced throughput.

[0004] JP 2011-013283 A

[0005] According to a first aspect, there is provided a phase shift mask blank comprising a substrate and a first layer formed on the substrate, the first layer containing zirconium (Zr), silicon (Si) and nitrogen (N), and the first layer having a transmittance per film thickness that imparts a phase shift of 180° to light with a wavelength of 365 nm of 4% or more and 40% or less.

[0006] According to a second aspect, there is provided a phase shift mask blank comprising a substrate and a first layer formed on the substrate, wherein the first layer is a laminate having four or more layers of a metal silicide nitride containing zirconium (Zr) and silicon (Si), and wherein the transmittance per film thickness of the first layer that imparts a phase shift of 180° to light having a wavelength of 365 nm is 4% or more and 40% or less.

[0007] According to a third aspect, there is provided a phase shift mask blank comprising a substrate and a first layer formed on the substrate, the first layer being a stack having four or more layers of a metal silicide nitride containing zirconium (Zr) and silicon (Si), and the tilt angle of the first layer being 55° or more and 90° or less.

[0008] According to a fourth aspect, there is provided a phase shift mask having a desired pattern formed on the phase shift mask blank of any one of the first to third aspects.

[0009] According to a fifth aspect, there is provided a method for manufacturing a phase shift mask blank, comprising a film formation step of forming a first layer on a substrate, in which a nitride layer of a metal silicide containing zirconium and silicon is formed on the substrate four or more times to form the first layer.

[0010] According to a sixth aspect, there is provided a method for manufacturing a phase shift mask, which is the method for manufacturing a phase shift mask blank of the fifth aspect, further comprising a pattern formation step of forming a desired pattern.

[0011] 1 is a schematic cross-sectional view showing an example of a phase shift mask blank according to an embodiment; FIG. 2 is a schematic cross-sectional view showing another example of a phase shift mask blank according to an embodiment; FIG. 3 is a schematic cross-sectional view of a phase shift mask according to an embodiment; FIG. 4 is a schematic view of an exposure apparatus used in an exposure method according to an embodiment; FIG. 5 is a schematic view of an example of an apparatus for manufacturing a phase shift mask blank according to an embodiment; FIG. 6 is a graph showing the transmittance of a ZrSi phase shift mask blank according to an example at a film thickness at which light having a wavelength of 300 to 600 nm gives a phase shift of 180°; FIG. 7 is a graph showing the transmittance of a MoSi phase shift mask blank according to a comparative example at a film thickness at which light having a wavelength of 300 to 600 nm gives a phase shift of 180°; and FIG. 8 is a graph showing the sputtering gas introduction rate (Sputter gas ratio: N) of the ZrSi phase shift mask blank according to an example and the MoSi phase shift mask blank according to a comparative example. 2 / (Ar+N 2 1 is a graph showing the relationship between the sputtering gas introduction rate (N) of the ZrSi phase shift mask blanks in the examples and the MoSi phase shift mask blanks in the comparative examples and the sputtering gas introduction rate (N) of the ZrSi phase shift mask blanks in the examples and the MoSi phase shift mask blanks in the comparative examples. 2 / (Ar+N 2 1 is a graph showing the relationship between the sputtering gas introduction rate (Sputter gas ratio: N) and the refractive index (Refractive index: n) of the ZrSi phase shift mask blanks in the examples and the MoSi phase shift mask blanks in the comparative examples. 2 / (Ar+N 2 1 is a graph showing the relationship between the cross-section tilt angle and the sputtering gas introduction rate (Sputter gas ratio: N) of the ZrSi phase shift mask blanks in the examples and the MoSi phase shift mask blanks in the comparative examples. 2 / (Ar+N 21 is a graph showing the relationship between the extinction coefficient (k) and the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 2 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 3 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 4 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 5 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 6 ...8 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 9 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 10 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 11 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 12 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 13 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 14 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 15 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 16 is a graph showing the relationship between the surface roughness (SEM) of a ZrSi phase shift mask blank in an example. 17 is a graph showing the relationship between the surface roughness (

[0012] An embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described below. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be practiced with appropriate modifications within the scope of its gist.

[0013] [Phase Shift Mask Blanks 100] A phase shift mask blank 100 of this embodiment shown in Figure 1 will be described. Phase shift mask blanks 100 include a substrate 10 and a phase shift layer 20 formed on a surface (substrate surface) 10a of substrate 10. A phase shift mask 300 (see Figure 3) can be manufactured from phase shift mask blanks 100 by forming a predetermined pattern 50 in phase shift layer 20. Phase shift masks 300 are used in manufacturing display devices such as FPDs (Flat Panel Displays) and semiconductor devices such as LSIs (Large Scale Integration).

[0014] The substrate 10 may be made of, for example, synthetic quartz glass. However, the material of the substrate 10 is not limited to synthetic quartz glass. The substrate 10 may be made of any material that sufficiently transmits exposure light from an exposure tool in which the phase shift mask 300 is used.

[0015] The phase shift layer 20 contains zirconium (Zr), silicon (Si), and nitrogen (N). As shown in FIG. 3 , in the phase shift mask 300, a portion of the phase shift layer 20 is removed from the substrate surface 10 a by wet etching, and the removed portion forms a predetermined pattern 50 on the surface of the phase shift layer 20. The pattern 50 (removed portion, recess) is defined by the side surface 21 of the phase shift layer 20 exposed by the wet etching and the exposed substrate surface 10 a. FIG. 3 shows a cross section of the phase shift layer 20 perpendicular to the substrate surface 10 a. In the cross section shown in FIG. 3 , the closer the inclination angle θ of the side surface 21 of the phase shift layer 20 defining the pattern 50 from the substrate surface 10 a to 90°, the higher the accuracy of the pattern 50 formed in the phase shift mask 300. The tilt angle θ is the angle between the side surface 21 defining the pattern 50 (recess) of the phase shift layer 20 and the substrate surface 10a in a cross section of the phase shift layer 20 perpendicular to the substrate surface 10a, including the phase shift layer 20. Therefore, the closer the tilt angle θ is to 90°, the more preferable. Specifically, the tilt angle θ is preferably 45° to 90°, with a lower limit of 60° being more preferable and 70° being even more preferable. The upper limit may be 85° or 75°. FIG. 3 shows a state where θ = 90°. The inventors have found that by forming the phase shift layer 20 from multiple layers, the tilt angle θ in the phase shift mask 300 manufactured from the phase shift mask blank 100 increases (approaching 90°), improving the pattern accuracy of the phase shift mask 300. Therefore, the phase shift layer 20 of this embodiment is preferably composed of multiple layers, and can be, for example, a stack of 4 to 10 layers. The lower limit is 5 layers, and more preferably 6 layers. By stacking the phase shift layer 20 in this manner, the tilt angle θ can be increased, and the amount of side etching can be reduced, thereby improving pattern accuracy. Although the phase shift layer 20 in Figures 1 to 5 is depicted as a single layer (one layer), it is actually depicted as a laminate of multiple layers.

[0016] The phase shift layer 20 may contain no elements other than Zr, Si, and N, or may contain small amounts of impurities that do not affect the effect.

[0017] Furthermore, the phase shift layer 20 of the phase shift mask blank of this embodiment has a high refractive index. A higher refractive index allows for a thinner thickness of the phase shift layer 20, calculated by the following equation: d=λ / (2(n−1)) (d: thickness of the phase shift layer 20, λ: wavelength of the exposure light, n: refractive index of the phase shift layer 20 at wavelength λ). By reducing the thickness required for film formation, a more uniform film can be formed on the substrate 10. Furthermore, if the thickness of the phase shift layer 20 can be reduced, the amount of side etching (described later) can be reduced, allowing for the formation of a pattern 50 closer to the design dimensions (improved pattern accuracy).

[0018] The refractive index of the phase shift layer 20 of this embodiment for light with a wavelength of 365 nm may be, for example, 2.70 to 2.90, with a more preferable lower limit being 2.75, and even more preferably 2.80. By providing such a high refractive index, it is possible to reduce the film thickness when the phase shift amount is 180°.

[0019] The extinction coefficient of the phase shift layer 20 of this embodiment for light with a wavelength of 365 nm may be, for example, 0.13 to 0.80, and the upper limit of the extinction coefficient is more preferably 0.70, more preferably 0.60, and even more preferably 0.50.

[0020] The phase shift layer 20 functions as a phase shifter that locally changes the phase of the exposure light irradiated in the exposure process using the phase shift mask 300. Therefore, the phase shift layer 20 needs to transmit the exposure light to a certain extent. The transmittance of the phase shift layer 20 to the exposure light (e.g., light with a wavelength of 330 nm to 470 nm) is preferably 3% or more and 85% or less. Typical exposure light used in the exposure process using the phase shift mask 300 includes, for example, deep ultraviolet (DUV, wavelengths: 302 nm, 313 nm, 334 nm), i-line (wavelength: 365 nm), h-line (wavelength: 405 nm), and g-line (wavelength: 436 nm). These can be used as monochromatic light or composite light.

[0021] Here, the phase shift layer 20 may have a transmittance of 4% to 40% for 365 nm light at a thickness that provides a 180° phase shift for 365 nm light, with the lower limit being preferably 5%, more preferably 8%. The upper limit is preferably 38%, more preferably 37%. The phase shift layer 20 may have a transmittance of 5% to 50% for 405 nm light at a thickness that provides a 180° phase shift for 405 nm light, with the lower limit being preferably 7%, more preferably 8%. The upper limit is preferably 49%, more preferably 48%. The phase shift layer 20 may have a transmittance of 8% to 65% for 436 nm light at a thickness that provides a 180° phase shift for 436 nm light, with the lower limit being preferably 9%, more preferably 10%. The upper limit is preferably 63%, more preferably 60%.

[0022] Phase shift layer 20 preferably changes (shifts) the phase of exposure light irradiated by about 180° in the exposure step using phase shift mask 300 (phase shift amount: about 180°). That is, phase shift layer 20 preferably shifts the phase of exposure light (e.g., light with a wavelength of 330 nm to 470 nm) passing through it by 160° to 200° (180°±20°), 170° to 190° (180°±10°), or 175° to 185° (180°±5°).

[0023] The phase shift amount can be adjusted by changing the refractive index and thickness (film thickness) of the phase shift layer 20 to match the wavelength of the light (exposure light) transmitted through the phase shift mask 300. The thickness of the phase shift layer 20 can be designed to achieve a phase shift amount of approximately 180°, taking into account the characteristics of the phase shift layer 20, such as the refractive index, and the wavelength of the transmitted light (exposure light). That is, the thickness d of the phase shift layer 20 can be designed based on the formula: d = λ / (2(n-1)) (d: thickness of the phase shift layer 20, λ: wavelength of the exposure light, n: refractive index of the phase shift layer 20 at wavelength λ). The thickness of the phase shift layer 20 is preferably, for example, 90 nm to 125 nm, with a more preferred lower limit of 94 nm and even more preferred 96 nm. A more preferred upper limit of the thickness of the phase shift layer 20 is 116 nm and even more preferred 110 nm. By setting the film thickness in this range, the etching time required to achieve a 180° phase shift is shortened, reducing damage to the glass.

[0024] The phase shift mask blank 100 is manufactured using a method described below. For example, the phase shift mask blank 100 may be manufactured by depositing the phase shift layer 20 on the substrate 10 using reactive sputtering, which will be described in the examples below.

[0025] [Phase Shift Mask Blanks 200] Phase shift mask blanks 200 shown in Figure 2 will be described. Phase shift mask blanks 200 include substrate 10, phase shift layer 20 formed on substrate surface 10a, and etching mask layer (chromium compound layer) 30 containing a chromium compound formed on phase shift layer 20. Except for having etching mask layer 30, the configuration of phase shift mask blanks 200 is the same as that of phase shift mask blanks 100 shown in Figure 1. Phase shift mask blanks 200 shown in Figure 2 exhibits the same effects as phase shift mask blanks 100, and further exhibits the effects described below by having etching mask layer 30.

[0026] As with the phase shift mask blank 100, a phase shift mask 300 (see FIG. 3) can be manufactured from the phase shift mask blank 200 by forming a predetermined pattern 50 in the phase shift layer 20. When forming the predetermined pattern 50 in the phase shift layer 20 by wet etching, a photoresist layer 40 is formed on the phase shift mask blank 200 (see FIG. 4A). The phase shift layer (ZrSiN-based layer) 20 here has low adhesion to the photoresist layer 40. For this reason, if the photoresist layer 40 were formed directly on the phase shift layer 20, there is a risk that the photoresist layer 40 would peel off during wet etching. Therefore, in the phase shift mask blank 200, an etching mask layer 30 that has adhesion to both the photoresist layer 40 and the phase shift layer 20 is provided, thereby preventing the photoresist layer 40 from peeling off during wet etching.

[0027] The material of the etching mask layer 30 is not particularly limited, and any material that enhances adhesion between the photoresist layer 40 and the phase shift layer 20 may be used. For example, chromium compounds such as chromium nitride and chromium oxide may be used. Furthermore, in the manufacture of the phase shift mask 300, the photoresist layer 40 is exposed to light with a wavelength of 350 nm to 450 nm. Therefore, the etching mask layer 30 provided below the photoresist layer 40 preferably has a low reflectance for light with a wavelength of 350 nm to 450 nm, and also functions as an anti-reflection layer. Chromium oxide is more preferable as an anti-reflection layer. By suppressing the reflection of the exposure light, multiple reflections of the exposure light within the photoresist layer 40 are suppressed, improving the pattern accuracy of the phase shift mask 300. For example, the reflectance of the etching mask layer 30 for light with a wavelength of 413 nm is preferably 15% or less. The etching mask layer 30 may be a single layer or may be formed from multiple layers. If the etching mask layer 30 is formed from multiple layers, it is preferable that the layer directly below the photoresist layer 40 has a low reflectance for the exposure light. For example, the etching mask layer 30 may be composed of a chromium nitride layer 31 formed on the phase shift layer 20 and a chromium oxide layer 32 formed on the chromium nitride layer 31. The chromium oxide layer 32 can suppress the reflectance of light with a wavelength of 413 nm to, for example, about 11%.

[0028] The thickness of the etching mask layer 30 is not particularly limited and can be adjusted as appropriate, for example, to 10 nm to 120 nm. When the etching mask layer 30 is composed of a chromium nitride layer 31 and a chromium oxide layer 32, the thickness of the etching mask layer 30 is preferably 80 to 120 nm, and the ratio of the thickness of the chromium nitride layer 31 to the thickness of the chromium oxide layer 32 is preferably 6:4 (3:2) to 8:2 (4:1). If the etching mask layer 30 is too thin, the etching time becomes short, making it difficult to control the CD (critical dimension) in the phase shift layer plane (i.e., control the line width of the pattern 50). Furthermore, if the etching mask layer 30 is too thick, the amount of side etching increases, making it difficult to obtain the designed pattern dimensions. When the phase shift layer 20 is wet-etched using the etching mask layer 30 (see FIG. 4D ), the phase shift layer 20 is isotropically etched by the etching solution. Therefore, the phase shift layer 20 is etched not only in the direction perpendicular to the substrate 10 but also in the lateral direction perpendicular to the vertical direction. This phenomenon in which etching progresses in the lateral direction is called side etching. Therefore, if the etching mask layer 30 is too thick or if the phase shift layer 20 is too thick as described above, there is a risk that the etching will be wider than the desired pattern width.

[0029] There are no particular limitations on the method for manufacturing phase shift mask blank 200, and a general-purpose method can be used. For example, phase shift mask blank 200 may be manufactured by depositing phase shift layer 20 and etching mask layer 30 on substrate 10 using reactive sputtering, which will be described later in FIG. 6 and in the Examples.

[0030] 6 is a schematic diagram showing a manufacturing apparatus 600 for manufacturing phase shift mask blanks 100 and 200 according to this embodiment, and is a diagram showing the interior of manufacturing apparatus 600 as viewed from above. Film formation apparatus 600 shown in Fig. 6 is an in-line sputtering apparatus, and includes a load chamber 601 for loading substrate 10 for manufacturing phase shift mask blanks 100 and 200, a first sputtering chamber 602, a buffer chamber 603, a second sputtering chamber 604, and an unloading chamber 605 for unloading manufactured phase shift layer 20.

[0031] The substrate tray P is a frame-shaped tray on which the substrate 10 for forming the phase shift layer 20 can be placed, and the substrate 10 is placed with its outer edge supported. The substrate 10 is placed on the substrate tray P so that the surface on which the phase shift layer 20 (ZrSiN-based layer), the light-shielding film serving as the etching mask layer 30 (chromium compound layer), and the anti-reflection film are to be formed faces downward (facing downward). In the film formation apparatus 600, as will be described later, the substrate tray P on which the substrate 10 is placed is transported to the position of the buffer chamber 603 in the direction indicated by the solid arrow Q in FIG. 6 while maintaining the surface of the substrate 10 facing the target. This forms a first phase shift layer 20 (ZrSiN-based layer) on the surface of the substrate 10, thereby producing a phase shift mask blank 100 having a single phase shift layer 20.

[0032] As indicated by solid arrow Q, after first phase shift layer 20 is formed, substrate tray P is further repeatedly transported between load chamber 601 and buffer chamber 603, thereby manufacturing phase shift mask blanks 100 having phase shift layers 20 consisting of layers equal to the number of transports. Note that whether transporting from load chamber 601 to buffer chamber 603 or transporting from buffer chamber 603 to load chamber 601, a ZrSiN-based layer can be formed in the same manner.

[0033] After the phase shift mask blank 100 is manufactured, the substrate tray P is further transported from the buffer chamber 603 to the position of the unloading chamber 605, as shown by the dotted arrow R, whereby an etching mask layer 30 (chromium compound layer) is formed on the phase shift layer 20, and the phase shift mask blank 200 is manufactured.

[0034] Loading chamber 601, first sputtering chamber 602, buffer chamber 603, second sputtering chamber 604, and unloading chamber 605 are each separated by a shutter (not shown). Loading chamber 601, first sputtering chamber 602, buffer chamber 603, second sputtering chamber 604, and unloading chamber 605 are each connected to an exhaust device (not shown), and the inside of each chamber is evacuated.

[0035] A first target 606 (ZrSi) is provided inside first sputtering chamber 602, and a second target 607 (Cr) is provided inside second sputtering chamber 604. DC power supplies (not shown) are provided in first sputtering chamber 602 and second sputtering chamber 604, respectively, and supply power to first target 606 (ZrSi) and second target 607 (Cr), respectively.

[0036] The first sputtering chamber 602 is provided with a first gas inlet 608 for introducing a sputtering gas into the first sputtering chamber 602. The first target 606 is a sputtering target for forming a ZrSiN-based layer and is formed of a material containing zirconium (Zr) and silicon (Si). Specifically, the first target 606 is formed of a material selected from zirconium, zirconium oxide, zirconium nitride, zirconium carbide, silicon, silicon oxide, silicon nitride, silicon carbide, etc. For example, to form a ZrSiN film, a mixed gas of a nitrogen-containing gas and an inert gas (such as argon gas) is introduced through the first gas inlet 608.

[0037] The second sputtering chamber 604 is provided with a second gas inlet 609 for introducing a sputtering gas into the second sputtering chamber 604. The second target 607 is a sputtering target for forming a chromium compound layer and is made of a material containing chromium. Specifically, the second target 607 is made of a material selected from chromium, chromium oxide, chromium nitride, chromium carbide, etc. For example, to form a CrCN film as a light-shielding film, a mixed gas of a gas containing nitrogen or oxygen and an inert gas (such as argon gas) is introduced through the second gas inlet 609.

[0038] When the substrate 10 is transferred to the first sputtering chamber 602, a first phase shift layer 20 (ZrSiN-based layer) is formed on the surface of the substrate 10 by sputtering in the first sputtering chamber 602. Furthermore, the substrate 10 on which the first phase shift layer 20 has been formed may be transferred between the buffer chamber 603 and the load chamber 601 multiple times, and multiple sputtering processes may be performed in the first sputtering chamber 602, thereby forming a laminate of the phase shift layer 20. The substrate 10 is then transferred to the second sputtering chamber 604. In the second sputtering chamber 604, an etching layer 30 (chromium compound layer) is formed on the surface of the phase shift layer 20 by sputtering. Similar to the ZrSiN layer, the chromium compound layer may also be transferred between the buffer chamber 603 and the load chamber 605 multiple times, and multiple sputtering processes may be performed in the second sputtering chamber 604, thereby forming a laminate of the etching layer 30. In this manner, a ZrSiN layer and a chromium compound layer are formed in this order on the surface of the substrate 10, and a phase shift mask blank 200 is manufactured.

[0039] The materials of the first and second targets 606, 607 and the types of gases introduced from the first and second gas inlets 608, 609 are appropriately selected depending on the materials and compositions of the chromium compound layer and the ZrSiN layer. The sputtering method may be any of DC sputtering, RF sputtering, ion beam sputtering, etc.

[0040] [Phase Shift Mask] A phase shift mask 300 shown in FIG. 3 will now be described. Phase shift mask 300 has substrate 10 and phase shift layer 20 formed on surface 10a of substrate 10, with a predetermined pattern 50 formed in phase shift layer 20. Except for the formation of predetermined pattern 50 in phase shift layer 20, the configuration of phase shift mask 300 is the same as phase shift mask blank 100 shown in FIG. 1. In a cross section of phase shift layer 20 perpendicular to substrate surface 10a, the inclination angle θ of side surface 21 of phase shift layer 20 that defines pattern 50 from substrate surface 10a is preferably 45° to 90°. Furthermore, by stacking phase shift layer 20, the inclination angle θ can be made closer to a right angle, which in turn reduces the amount of side etching and improves pattern accuracy.

[0041] There are no particular limitations on the method for manufacturing phase shift mask 300, and a general-purpose method can be used. For example, phase shift mask 300 may be manufactured using reactive sputtering and wet etching (see FIG. 4), which will be described in the examples below.

[0042] [Exposure Method] Next, we will explain an exposure method using phase shift mask 300 manufactured from phase shift mask blanks 100 and 200. The exposure method using phase shift mask 300 can be carried out as a photolithography process using an exposure apparatus in the manufacture of devices such as semiconductors and liquid crystal panels.

[0043] As shown in Figure 5, the exposure apparatus 500 used in the exposure method includes a light source LS, an illumination optical system 502, a mask stage 503 that holds the phase shift mask 300, a projection optical system 504, a substrate stage 505 that holds a photosensitive substrate 515 that is the object to be exposed, and a drive mechanism 506 that moves the substrate stage 505 in a horizontal plane.

[0044] First, a phase shift mask 300 is placed on a mask stage 503 of an exposure apparatus 500. A photosensitive substrate 515 coated with photoresist is placed on a substrate stage 505. Exposure light is then emitted from a light source LS. The emitted exposure light enters an illumination optical system 502, where it is adjusted to a predetermined luminous flux, and is then irradiated onto a phase shift mask 300 held on a mask stage 503. The light that passes through the phase shift mask 300 has the same pattern as the device pattern 50 drawn on the phase shift mask 300, and this pattern is irradiated via a projection optical system 504 onto a predetermined position on a photosensitive substrate 515 held on a substrate stage 505. As a result, the photosensitive substrate 515 is exposed to the device pattern of the phase shift mask 300 at a predetermined magnification.

[0045] Phase shift mask 300 manufactured from phase shift mask blanks 100 and 200 has high pattern accuracy. Therefore, by performing exposure using phase shift mask 300, it is possible to reduce circuit pattern defects in the exposure process and efficiently manufacture highly integrated devices.

[0046] The phase shift mask blanks and phase shift masks will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples and comparative examples.

[0047] Phase shift mask blanks having five types of ZrSiN phase shift layers 20 with different nitrogen introduction ratios were manufactured as Examples 1 to 5. Furthermore, phase shift mask blanks having two types of MoSiN phase shift layers 20 with different nitrogen introduction ratios were manufactured as comparative examples.

[0048] [Production of Phase Shift Mask Blank 100] A circular parallel plate made of quartz glass was prepared as the substrate 10 (size: diameter 3 inches, thickness 0.5 mm). A DC magnetron sputtering device was used, and a ZrSi alloy was used as the sputtering target. Ar—N 2Reactive sputtering was performed while introducing the mixed gas, and a ZrSiN film was formed on the substrate 10. Thereafter, reactive sputtering using the same ZrSi alloy target as above was repeated five times to form a ZrSiN-based phase shift layer 20 consisting of a total of six layers, and phase shift mask blanks 100 were manufactured (Examples 1 to 5). The composition (atomic ratio) of the ZrSi alloy target was Zr:Si=1:2. The film formation conditions were a total mixed gas pressure of 0.32 Pa, N in the mixed gas (sputtering gas), 2 Introduction ratio: 24% in Example 1, 26% in Example 2, 28% in Example 3, 30% in Example 4, and 60% in Example 5. The DC output was 1.5 kW in all Examples 1 to 5.

[0049] Comparative Example: A MoSi alloy target (atomic ratio: Mo:Si=1:4) was used as the sputtering target, and Ar—N was introduced at the introduction ratio shown in Table 2. 2 Reactive sputtering was performed once (single layer) while introducing the mixed gas. 2 The incorporation ratio was 30% in Comparative Example 1 and 36% in Comparative Example 2. MoSiN-based phase shift layer 20 was formed under the above conditions to produce phase shift mask blanks.

[0050] [Production of Phase Shift Mask Blanks 200] A DC magnetron sputtering apparatus was used on the phase shift mask blanks 100 of each Example and Comparative Example, and a Cr target was used as the sputtering target, and Ar—N 2 Reactive sputtering was performed while introducing the mixed gas, followed by Ar—O 2Reactive sputtering was performed while introducing the mixed gas. This resulted in an etching mask layer 30 composed of a chromium nitride layer 31 and a chromium oxide layer 32 being formed on the phase shift mask blank 100, producing a phase shift mask blank 200 (FIG. 2). The etching mask layer 30 was formed to a thickness within the range of 90±7 nm (thickness of the chromium nitride layer 31:thickness of the chromium oxide layer 32 = 7:3). Next, a positive ultraviolet resist (GRX-M237, manufactured by Nagase ChemteX) was applied by spin coating onto the phase shift mask blank 200 to form a photoresist layer 40 (FIG. 4(A)). The thickness of the photoresist layer 40 was 660 nm.

[0051] [Evaluation of Physical Properties of Phase Shift Layer 20] Measurement of Refractive Index and Extinction Coefficient, and Simulation of Transmittance The refractive index and extinction coefficient of the phase shift layer 20 of each Example and Comparative Example were measured by ellipsometry. The results are shown in Table 1 and FIGS. 10 and 12. Furthermore, for the phase shift layer 20 of each Example and Comparative Example, the film thicknesses that provide a 180° phase shift at each of the three wavelengths (365 nm, 405 nm, and 436 nm) were determined from the refractive index measurements, and the transmittance of the phase shift layer 20 at each film thickness was calculated by simulation. The results are shown in Table 1 and FIGS. 7 and 8. The simulation was performed using the simulation software "TFCalc." Based on the refractive index and extinction coefficient measurements at the i-line (365 nm) obtained by ellipsometry, the film thicknesses that provide a 180° phase shift at each of the three wavelengths (365 nm, 405 nm, and 436 nm) were used to calculate the transmittance of the phase shift layer 20 at each film thickness. Here, the transmittance refers to the external transmittance taking reflection into consideration.

[0052] [Fabrication of Phase Shift Mask 300] A pattern 50 was formed in phase shift layer 20 of each example and comparative example to fabricate phase shift mask 300 shown in Fig. 3. First, a DC magnetron sputtering device was used, and a Cr target was used as the sputtering target, and Ar-N 2 Reactive sputtering was performed while introducing the mixed gas, followed by Ar—O 2Reactive sputtering was performed while introducing the mixed gas. This resulted in an etching mask layer 30 composed of a chromium nitride layer 31 and a chromium oxide layer 32 being formed on the phase shift mask blank 100, producing a phase shift mask blank 200 (FIG. 2). The etching mask layer 30 was formed to a thickness within the range of 90±7 nm (thickness of the chromium nitride layer 31:thickness of the chromium oxide layer 32=7:3). Next, a positive ultraviolet resist (GRX-M237, manufactured by Nagase ChemteX) was applied by spin coating onto the phase shift mask blank 200 to form a photoresist layer 40 (FIG. 4(A)). The thickness of the photoresist layer 40 was 660 nm.

[0053] Using a mask aligner (PLA-501, manufactured by Canon) with a high-pressure mercury lamp, the photoresist layer 40 was exposed using a light-shielding mask in which openings corresponding to the pattern 50 were formed. As a result, the portions of the photoresist layer 40 corresponding to the pattern 50 were exposed. Next, the exposed phase shift mask blanks 200 were immersed in an organic alkaline developer (1.83% tetramethylammonium hydroxide, manufactured by Tama Chemicals Co., Ltd.). As a result, the exposed portions of the photoresist layer 40 were dissolved and removed, and openings corresponding to the pattern 50 were formed ( FIG. 4(B) ).

[0054] Next, using the photoresist layer 40 with openings corresponding to the pattern 50 as a mask, the etching mask layer 30 was wet-etched using an etching solution containing ceric ammonium nitrate and nitric acid (PureEtchCR101, manufactured by Hayashi Pure Chemical Industries, Ltd.). The etching solution temperature was 23±3°C, and the etching time was 80 seconds. As a result, the exposed portions of the etching mask layer 30 that were not covered by the photoresist layer 40 were removed ( FIG. 4(C) ).

[0055] Next, using the photoresist layer 40 with openings corresponding to the pattern 50 and the etching mask layer 30 as a mask, the phase shift layer 20 was wet-etched using an etching solution containing ammonium fluoride (ADEKA Chelmica WGM-155, manufactured by ADEKA). The etching solution temperature was set to 23±3°C, and 20% over-etching was performed to remove the exposed phase shift layer 20 uniformly and completely. Here, 20% over-etching means that the time required to penetrate the phase shift film 20 is defined as the reference time, and etching is performed for 120% of the reference time. As a result, a pattern 50 was formed in the phase shift layer 20 (FIG. 4(D)).

[0056] Finally, a stripping process was carried out to remove the photoresist layer 40 and the etching mask layer 30. Through the above steps, a phase shift mask 300 shown in Fig. 4(E) was obtained from the phase shift mask blank.

[0057]

[0058] As shown in Table 1 and FIG. 12 , even when the nitrogen introduction ratios were the same, the extinction coefficients of the ZrSi layers in Examples 1 to 5 were lower than the extinction coefficients of the MoSi layers in Comparative Examples 1 and 2. The larger the extinction coefficient, the smaller the transmittance. Therefore, as shown in Table 1 and FIGS. 7 and 8 , increasing the nitrogen introduction ratio of the ZrSi phase shift layers in Examples 1 to 5 and the MoSi phase shift layers in Comparative Examples 1 and 2 increased the transmittance (365 nm) of all phase shift layers. Furthermore, even when the nitrogen introduction ratios were the same, the ZrSi phase shift layer in Example 4 had a higher transmittance (365 nm) than the MoSi phase shift layer in Comparative Example 1.

[0059] 9 , the etching rates of the ZrSi phase shift layers in Examples 1 to 5 were faster than the etching rates of the MoSi phase shift layers in Comparative Examples 1 and 2. In addition, since the refractive index of the ZrSi phase shift layers in Examples 1 to 5 was higher than the refractive index of the MoSi phase shift layers in Comparative Examples 1 and 2, the film thickness of the ZrSi phase shift layers in Examples 1 to 5 at a phase of 180° was thinner than the film thickness of the MoSi phase shift layers in Comparative Examples 1 and 2.

[0060] In the process of manufacturing the phase shift mask 300, cross-sections of the patterns 50 formed in each example and each comparative example were observed. The cross-sections were observed in the state before the etching mask layer 30 and the photoresist layer 40 were removed (the state shown in FIG. 4(D)). FIG. 13 shows SEM images of cross sections perpendicular to the substrate surface 10a of each example and each comparative example. From FIG. 13, the inclination angle θ of the side surface 21 of the phase shift layer 20 from the substrate surface 10a was measured for each example and each comparative example. The results are shown in Table 1 and FIG. 13.

[0061] 13, it can be seen that the tilt angles of the ZrSi layers in Examples 1 to 5 are larger than the tilt angles of the MoSi layers in Comparative Examples 1 and 2. It can also be seen that in Comparative Example 2, the substrate 10 is also etched due to the long etching time. Furthermore, as shown in Table 1 and FIG. 11, even though the nitrogen introduction ratios were the same, the tilt angle of the ZrSi layer in Example 4 was larger than the tilt angle of the MoSi layer in Comparative Example 1.

[0062] Furthermore, the tilt angle of the phase shift layer 20 of this embodiment, which is over-etched by 20% using an etching solution containing ammonium fluoride (ADEKA Chelmica WGM-155, manufactured by ADEKA Corporation, etching solution temperature 23±3° C.), is preferably 55° or more and 90° or less. The lower limit is preferably 58°, more preferably 60°, and even more preferably 65°.

[0063] During the manufacturing process of the phase shift mask 300, cross-sectional observations were performed on the patterns 50 formed on the ZrSiN phase shift layers 20, which were formed into four, six, and eight layers, respectively. The nitrogen introduction ratio during the deposition of the ZrSiN film was 28%, the same as in Example 3. The cross-sectional observations were performed before the etching mask layer 30 and the photoresist layer 40 were removed (the state shown in FIG. 4(D)). FIG. 14 shows SEM images of cross sections perpendicular to the substrate surface 10a for phase shift masks having (A) four, (B) six, and (C) eight shift layers 20, as well as sketches based on the SEM images. FIG. 14(B) shows phase shift masks formed under the same conditions as in Example 3, but etched for a longer time than in Example 3. The side surfaces 21 of the phase shift layers 20 in FIGS. 14(A) to 14(C) confirm that the phase shift layers 20 are stacked.

[0064] The phase shift mask blanks according to this embodiment have a shorter etching time and a higher refractive index than MoSi phase shift mask blanks, and therefore can have a thinner film thickness when the phase shift amount is 180°, and the pattern accuracy can be improved by reducing the amount of side etching.

[0065] 10 Substrate 20 Phase shift layer 30 Etching mask layer 31 Chromium nitride layer 32 Chromium oxide layer 40 Photoresist layer 50 Pattern 100, 200 Phase shift mask blank 300 Phase shift mask 500 Exposure apparatus LS Light source 502 Illumination optical system 504 Projection optical system 503 Mask stage 505 Substrate stage 600 Film forming apparatus 600 P Substrate tray Q Solid arrow R Dotted arrow 601 Loading chamber 602 First sputtering chamber 603 Buffer chamber 604 Second sputtering chamber 605 Unloading chamber 606 First target (ZrSi) 607 Second target (Cr) 608 First gas inlet 609 Second gas inlet

Claims

1. A phase shift mask blank, comprising: A substrate; a first layer deposited on the substrate; The first layer includes zirconium (Zr), silicon (Si), and nitrogen (N); the first layer has a transmittance per film thickness that gives a phase shift of 180° to light having a wavelength of 365 nm of 4% or more and 40% or less; The refractive index of the first layer with respect to light having a wavelength of 365 nm is 2.70 or more and 2.90 or less. Phase shift mask blanks.

2. A phase shift mask blank, comprising: A substrate; a first layer deposited on the substrate; the first layer is a stack having four or more layers of a metal silicide nitride containing zirconium (Zr) and silicon (Si); the first layer has a transmittance per film thickness that gives a phase shift of 180° to light having a wavelength of 365 nm of 4% or more and 40% or less; The refractive index of the first layer with respect to light having a wavelength of 365 nm is 2.70 or more and 2.90 or less. Phase shift mask blanks.

3. A phase shift mask blank, comprising: A substrate; a first layer deposited on the substrate; the first layer is a stack having four or more layers of a metal silicide nitride containing zirconium (Zr) and silicon (Si); The inclination angle of the first layer is equal to or greater than 55° and equal to or less than 90°, The refractive index of the first layer with respect to light having a wavelength of 365 nm is 2.70 or more and 2.90 or less. Phase shift mask blanks.

4. 4. The phase shift mask blank according to claim 1, wherein the first layer has a transmittance per film thickness that gives a phase shift of 180° to light having a wavelength of 365 nm of 4% or more and 40% or less.

5. 4. The phase shift mask blank according to claim 3, wherein the tilt angle is an angle when the first layer is over-etched by 20% under conditions of an etching solution of ADEKA CHELMIC WGM-155 and a temperature of the etching solution of 23±3° C.

6. The thickness of the first layer that gives a phase shift of 180° to light having a wavelength of 365 nm is calculated by the following formula (1): d=365 / (2(n-1)) (d: film thickness, n: refractive index) 3. The phase shift mask blank according to claim 1.

7. A phase shift mask blank described in any one of claims 1 to 3, wherein the first layer is substantially free of elements other than Zr, Si, and N.

8. A phase shift mask blank described in any one of claims 1 to 3, wherein the film thickness of the first layer is 90 nm or more and 125 nm or less.

9. 4. A phase shift mask having a desired pattern formed on the phase shift mask blank according to claim 1.

10. A method for producing a phase shift mask blank, comprising the steps of: A deposition step of depositing a first layer on a substrate, In the film-forming step, a nitride layer of a metal silicide containing zirconium and silicon is formed four or more times on the substrate to form a first layer.

11. The method for producing a phase shift mask blank according to claim 10 , wherein in the film forming step, the nitride layer of the metal silicide is formed six or more times on the substrate.

12. A method for manufacturing a phase shift mask, comprising the steps of: The method for producing a phase shift mask blank according to claim 10 or 11 further comprises a pattern forming step of forming a desired pattern. A method for manufacturing a phase shift mask.