Detergent composition including vinyl-alcohol-based copolymer
Patent Information
- Application Number
- JP2024517301
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2023-04-24
- Filing Date
- 2023-04-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional vinyl alcohol copolymers used in detergents exhibit insufficient washing performance when used as additives, necessitating the development of a biodegradable detergent composition with enhanced anti-resoiling ability.
A detergent composition containing a vinyl alcohol copolymer with specific structural units, including a vinyl carboxylate-derived unit and a vinylamine-derived unit, is formulated, with a weight average molecular weight of 1,000 to 1,000,000, and a mass ratio of structural units optimized for improved biodegradability and re-stain prevention.
The composition achieves excellent re-stain prevention and improved biodegradability, enhancing the washing performance and environmental sustainability of detergents.
Smart Images

Figure 2023210565000001 
Figure 2023210565000002 
Figure 2023210565000003
Abstract
Description
Detergent composition containing vinyl alcohol copolymer
[0001] The present disclosure relates to a detergent composition containing a vinyl alcohol copolymer that is biodegradable and has excellent anti-redeposition properties.
[0002] Various types of polymers have been proposed for polyvinyl alcohol, modified polyvinyl alcohol, and copolymers of vinyl alcohol. Polyvinyl alcohol is biodegradable and has excellent processability, so it has been used in a variety of applications, such as films.
[0003] For example, Patent Document 1 discloses a copolymer of vinyl alcohol with N-vinyl-2-caprolactam, N-vinylacetamide, ethyl vinyl ether, or the like.
[0004] Japanese Patent Application Laid-Open No. 2004-137361
[0005] The present inventors have been studying the use of a vinyl alcohol copolymer having a structural unit derived from vinyl alcohol as a detergent additive. However, the vinyl alcohol copolymer described in Patent Document 1 has a problem in that when used as an additive to a detergent composition, the washing performance is insufficient.
[0006] The present disclosure has been made in consideration of the above-mentioned drawbacks, and aims to provide a detergent composition containing a vinyl alcohol copolymer that is biodegradable and has good anti-soil redeposition properties.
[0007] That is, the detergent composition containing the vinyl alcohol-based copolymer of the present disclosure is a detergent composition containing a vinyl alcohol-based copolymer having a structural unit (A) of the following general formula (1) and a structural unit (B) of the following general formula (2):
[0008] (In general formula (1), R 1 is a hydrogen atom or —C(═O)—R x Represents R x represents a hydrogen atom or an organic group having 1 to 10 carbon atoms.
[0009] (In general formula (2), R 2is a hydrogen atom or —C(═O)—R x R represents one or more selected from x represents a hydrogen atom or one or more organic groups having 1 to 10 carbon atoms.
[0010] The detergent composition of the present disclosure further comprises a vinyl alcohol copolymer having a structural unit (A) of the following general formula (1) and a structural unit (B) of the following general formula (2) in an amount of 0.1 to 15 mass % based on the total amount of the detergent composition:
[0011] (In general formula (1), R 1 is a hydrogen atom or —C(═O)—R x Represents R x represents a hydrogen atom or an organic group having 1 to 10 carbon atoms.
[0012] (In general formula (2), R 2 is a hydrogen atom or —C(═O)—R x Represents R x represents a hydrogen atom or an organic group having 1 to 10 carbon atoms.) The detergent composition further comprises a surfactant in an amount of 10 to 60% by mass based on the total amount of the detergent composition.
[0013] The vinyl alcohol copolymer preferably has a weight average molecular weight of 1,000 to 1,000,000.
[0014] In the vinyl alcohol copolymer, the mass ratio of the structural unit (A) to the structural unit (B) is preferably 1-99 / 1-99.
[0015] In the vinyl alcohol copolymer, the content of the structural unit (E) other than the structural unit (A) and the structural unit (B) is preferably 0 to 50% by mass relative to 100% by mass of the total amount of the structural units (A), (B), and (E).
[0016] The vinyl alcohol copolymer has a structure in which the —C═O—R x The ratio of R 1 It is preferably 20 mol % or less relative to 100 mol % of the total amount of groups.
[0017] The vinyl alcohol copolymer has a structure in which the —C═O—R x The ratio of R 2 It is preferably 99 mol % or less relative to 100 mol % of the total amount of groups.
[0018] The present invention also relates to a vinyl alcohol copolymer having the structural unit (A), the structural unit (B), and a structural unit (C) represented by the following general formula (4): (In the general formula (4), X represents a hydrocarbon group having 1 to 6 carbon atoms. R 3 represents a hydrocarbon group having 2 to 6 carbon atoms. m represents an integer of 1 or 2. n represents an integer of 1 to 200. However, the asterisk represents an atom contained in another structural unit of the same type or a different type to which the structural unit (C) represented by general formula (4) is bonded.
[0019] In the vinyl alcohol copolymer, the content of the structural unit (E1) other than the structural unit (A), the structural unit (B), and the structural unit (C) is preferably 0 to 10% by mass relative to 100% by mass of the total amount of the structural units (A), (B), (C), and (E1).
[0020] According to the present disclosure, it is possible to provide a detergent composition containing a vinyl alcohol copolymer that is biodegradable and has excellent anti-redeposition properties.
[0021]
[0023] The following detailed description of preferred embodiments of the present disclosure is merely exemplary in nature and is in no way intended to limit the present disclosure, its application, or its uses.
[0022] In the following description, unless otherwise specified, "%" means "% by mass", "parts" means "parts by mass", and the range "A to B" means A or more and B or less. In addition, in this disclosure, "(meth)acrylate" means "acrylate" or "methacrylate", and "(meth)acrylic" means "acrylic" or "methacrylic".
[0023] [Vinyl Alcohol-Based Copolymer] The vinyl alcohol-based copolymer of the present disclosure is a copolymer having a structural unit (A) represented by the following general formula (1) and a structural unit (B) represented by the following general formula (2).
[0024] (In general formula (1), R 1 is a hydrogen atom or —C(═O)—R x Represents R x represents a hydrogen atom or an organic group having 1 to 10 carbon atoms.
[0025] (In general formula (2), R 2 The group is a hydrogen atom or -C(=O)-R x Represents R x represents a hydrogen atom or an organic group having 1 to 10 carbon atoms.
[0026] R in the structural unit (A) represented by the general formula (1) of the present disclosure 1 is a hydrogen atom or —C(═O)—R x This represents R in the structural unit (A) present in plural numbers in the copolymer. 1 may all be the same or different. x represents a hydrogen atom or an organic group having 1 to 10 carbon atoms, but in the copolymer, R x If there are multiple instances of R x may all be the same or different. The monomer (A), which is a precursor of the structural unit (A) represented by the general formula (1), is a vinyl carboxylate compound such as vinyl acetate. The vinyl carboxylate compound can be represented by the general formula (5) described below. After copolymerizing the vinyl carboxylate compound with another monomer, there is a step of hydrolysis, and upon hydrolysis (saponification), the R 1 becomes a hydrogen atom, and if it remains without being hydrolyzed, it becomes -C(=O)-R x Therefore, in many cases, the R 1 is a hydrogen atom and -C(=O)-R x When both groups are present, the —C(═O)—R x The number of groups is often small. 1When the total amount of groups is 100 mol%, -C(=O)-R x The residual amount of —C(═O)—R groups is preferably 20 mol % or less, more preferably 10 mol % or less, and even more preferably 5 mol % or less. x The remaining amount of the R 1 -C(=O)-R in x If the amount of the remaining group is within the above range, biodegradability is also improved, which is preferable.
[0027] R in the general formula (1) of the present disclosure x is not particularly limited as long as it is a hydrogen atom or an organic group having 1 to 10 carbon atoms. x When R is an organic group having 1 to 10 carbon atoms, it may be a saturated or unsaturated chain hydrocarbon, and may be linear or branched. It may also contain an aromatic group or a heteroatom. Specific examples of organic groups having 1 to 10 carbon atoms include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, heptyl, octyl, nonyl, and decyl; alkenyl groups such as vinyl, allyl, 1-butenyl, 2-butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, and decenyl; and aryl groups such as phenyl, naphthyl, and benzyl. The organic group is preferably an alkyl group. Among these, R x is preferably a hydrogen atom or a methyl group, since this improves the polymerization reactivity with a vinylamine derivative or the like represented by general formula (3) described later, and facilitates hydrolysis of the protecting group by a hydrolysis (saponification) treatment carried out after the copolymerization reaction.
[0028] The monomer (B), which is a precursor of the structural unit (B) represented by the general formula (2), is a vinylamine derivative. The vinylamine derivative can be represented by the following general formula (3).
[0029] R in general formula (3) x is R in general formula (2) xExamples of vinylamine derivatives include amide compounds of vinylamine with a carboxylic acid having 1 to 10 carbon atoms, such as N-vinylformamide and N-vinylacetamide. Preferred are N-vinylformamide and N-vinylacetamide.
[0030] After copolymerization of a vinylamine derivative with another monomer, there is a step of hydrolysis, and when hydrolysis (saponification) occurs, the R 2 becomes a hydrogen atom, and if it remains without being hydrolyzed, it becomes -C(=O)-R x Therefore, in many cases, the R 2 is a hydrogen atom and -C(=O)-R x The —NH—C(═O)—R group of the structural unit B is present. x Since the group is an amide bond, acid or alkali hydrolysis takes time. Therefore, by controlling the degree of hydrolysis, -NH-C(=O)-R x group and -NH obtained by hydrolysis 2 From the viewpoint of biodegradability of the polymer, the amount of -NH-C(=O)-R x group and -NH 2 There is no limitation on the ratio of the groups. Under the conditions for alkaline hydrolysis of the structural unit A, the hydrolysis of the structural unit B is slow. x Even when both are present, -C=O-R x The number of groups is often small. 2 When the total amount of groups is 100 mol%, -C=O-R x When hydrolyzed with an alkali, the remaining amount of —C═O—R groups is preferably 99 mol % or less, more preferably 95 mol % or less, even more preferably 90 mol % or less, still more preferably 80 mol % or less, and particularly preferably 75 mol % or less. x The remaining amount of the R group may be 20 mol % or less, 5 mol % or less, or 0 mol %. 2 -C=O-R in x It is preferable that the residual amount of the group is within the above range, since hydrophilicity is improved.x represents R in the general formula (1). x The same as R in the general formula (2). 2 is a hydrogen atom or -C(=O)CH 3 A protecting group is preferably a group, since it improves the polymerization reactivity of the vinylamine compound corresponding to the monomer that is the precursor of the structural unit (B) represented by the general formula (1) and facilitates hydrolysis of the protecting group by a hydrolysis (saponification) treatment carried out after the copolymerization reaction.
[0031] The mass ratio of the structural unit (A) to the structural unit (B) in the vinyl alcohol-based copolymer of the present invention is preferably 1 to 99 / 1 to 99. It is more preferably 1 to 98 / 2 to 99, even more preferably 1 to 97 / 3 to 99, even more preferably 50 to 97 / 3 to 50, and particularly preferably 70 to 97 / 3 to 30. When the mass ratio of the structural unit (A) to the structural unit (B) in the vinyl alcohol-based copolymer of the present disclosure is within the above-mentioned range, anti-soil redeposition ability is improved, which is preferable. Furthermore, it is preferable that the mol % of the structural unit (A) is 50 mol % or more, preferably 70 mol % or more, more preferably 80 mol % or more, and even more preferably 90 mol %, based on the number of moles of all structural units constituting the polymer, because biodegradability is improved.
[0032] The vinyl alcohol-based copolymer of the present disclosure may have a structural unit (E) other than the structural units (A) and (B). The structural unit (E) is a structural unit derived from a monomer (E) other than the monomer (A) and the monomer (B). When the vinyl alcohol-based copolymer of the present disclosure contains a structural unit (E) other than the structural units (A) and (B), the content of the structural unit (E) is preferably 0 to 50% by mass, where the total amount of the structural units (A), (B), and (E) constituting the vinyl alcohol-based copolymer of the present disclosure is 100% by mass. The content is more preferably 0 to 30% by mass, even more preferably 0 to 20% by mass, even more preferably 0 to 10% by mass, particularly preferably 0 to 5% by mass, and most preferably 0% by mass.
[0033] Examples of the monomer (E) include the monomer (C) represented by the general formula (6) described later and other polymerizable monomers (E1) described later.
[0034] The vinyl alcohol copolymer of the present disclosure may have a structural unit (C) of the following general formula (4) in addition to the structural unit (A) and the structural unit (B). (In the general formula (4), X represents a hydrocarbon group having 1 to 6 carbon atoms. R 3 represents a hydrocarbon group having 2 to 6 carbon atoms. m represents an integer of 1 or 2. n represents an integer of 1 to 200. However, the asterisk represents an atom contained in another structural unit of the same or different type to which the structural unit (C) represented by general formula (4) is bonded.) A vinyl alcohol copolymer having the structural unit (A) represented by general formula (1), the structural unit (B) represented by general formula (2), and the structural unit (C) represented by general formula (4) also constitutes one aspect of the present invention.
[0035] X in the structural unit (C) represented by the general formula (4) of the present disclosure is one or more hydrocarbon groups selected from hydrocarbon groups having 1 to 6 carbon atoms, and R 3 represents a hydrocarbon group having 2 to 6 carbon atoms, m is an integer of 1 or 2, and n is an integer of 1 to 200, and is not particularly limited.
[0036] When X is a hydrocarbon group having 1 to 6 carbon atoms, the hydrocarbon group may be a linear and / or branched hydrocarbon group. Specific examples of the hydrocarbon group having 1 to 6 carbon atoms include a methylene group, an ethylene group, an n-propylene group, an isopropylene group, an n-butylene group, an isobutylene group, an n-pentyl group, a neopentyl group, an isopentyl group, and an n-hexyl group. A preferred form of X is a hydrocarbon group having 2 to 4 carbon atoms, and more preferred forms are an ethylene group, an n-propylene group, and an n-butylene group. An ethylene group or an n-butylene group is even more preferred. Furthermore, when m is 2, an ethylene group is preferred. When X is an ethylene group or an n-butylene group, this is preferred from the viewpoints of the availability and polymerizability of the raw material vinyl ether before addition of alkylene oxide.
[0037] R in the structural unit (C) represented by the general formula (4) of the present disclosure3 represents a hydrocarbon group having 2 to 6 carbon atoms, and n is not particularly limited as long as it is an integer of 1 to 200. 3 may be a linear and / or branched hydrocarbon group. More preferably, it is a hydrocarbon group having 2 to 4 carbon atoms, even more preferably a hydrocarbon group having 2 to 3 carbon atoms, and most preferably a hydrocarbon group having 2 carbon atoms. Specific examples include an ethylene group, a propylene group, and a butylene group. Among these, one or more groups selected from an ethylene group and a propylene group are preferred because they can impart hydrophilicity to the alkylene oxide polymer having a hydrophobic group of the present disclosure. Similarly, from the viewpoint of imparting hydrophilicity to the vinyl alcohol copolymer of the present disclosure, R 3 is more preferably an ethylene group, which is a hydrocarbon group having two carbon atoms.
[0038] Furthermore, n in the structural unit (C) represented by the general formula (4) of the present disclosure is more preferably 1 to 150, even more preferably 1 to 100, even more preferably 1 to 50, still more preferably 1 to 30, and particularly preferably 1 to 20. When n in the structural unit (C) represented by the general formula (4) is within the above-mentioned range, this is preferred in that the polyalkylene oxide chain improves the effect of dispersing particulate soils such as mud.
[0039] The vinyl alcohol-based copolymer of the present disclosure may have a structural unit (E1) other than the structural units (A) to (C). The structural unit (E1) is a structural unit derived from a polymerizable monomer (E1) other than the monomer (A), the monomer (B), and the monomer (C) represented by general formula (6) described later. Specific examples of the other polymerizable monomer (E1) include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, fumaric acid, and citraconic acid; vinyl ethers such as ethylene glycol monovinyl ether and hydroxybutyl vinyl ether; unsaturated alcohols having 3 to 10 carbon atoms such as (meth)allyl alcohol and isoprenyl alcohol; unsaturated alcohol alkylene oxide adducts obtained by adding 1 to 300 moles of alkylene oxide having 2 to 18 carbon atoms to unsaturated alcohols having 3 to 10 carbon atoms such as (meth)allyl alcohol and isoprenyl alcohol; esters of (meth)acrylic acid such as methoxy(poly)oxyethylene glycol (meth)acrylate and methoxy(poly)ethylene glycol (poly)propylene glycol with alkoxy(poly)alkylene glycol obtained by adding 1 to 500 moles of alkylene oxide having 2 to 18 carbon atoms to alcohols or amines having 1 to 30 carbon atoms; hydroxyethyl (meth)acrylate, ... hydroxyalkyl (meth)acrylates such as hydroxypropyl (meth)acrylate and hydroxybutyl (meth)acrylate; alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, octyl (meth)acrylate and cyclohexyl (meth)acrylate; aromatic (meth)acrylates such as phenoxy (meth)acrylate and benzyl (meth)acrylate; maleic (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, octyl (meth)acrylate and cyclohexyl (meth)acrylate; half esters and diesters of unsaturated dicarboxylic acid monomers such as maleic anhydride, fumaric acid, itaconic acid, and citraconic acid with alcohols having 1 to 30 carbon atoms; half amides and diamides of the above unsaturated dicarboxylic acid monomers with amines having 1 to 30 carbon atoms; half esters and diesters of alkyl (poly) alkylene glycols obtained by adding 1 to 500 moles of alkylene oxides having 2 to 18 carbon atoms to the above alcohols or amines with the above unsaturated dicarboxylic acid monomers;Half esters and diesters of the above unsaturated dicarboxylic acid monomers with glycols having 2 to 18 carbon atoms or polyalkylene glycols having 2 to 500 moles of these glycols added; half amides of maleamic acid with glycols having 2 to 18 carbon atoms or polyalkylene glycols having 2 to 500 moles of these glycols added; triethylene glycol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, (poly)ethylene glycol (poly)propylene glycol (Poly)alkylene glycol di(meth)acrylates such as hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane di(meth)acrylate, and other polyfunctional (meth)acrylates; (poly)alkylene glycol dimaleates such as triethylene glycol dimaleate and polyethylene glycol dimaleate; vinyl sulfonate, (meth)allyl sulfonate, 2-(meth)acryloxyethyl sulfonate, 3-(meth)acryloxypropyl unsaturated sulfonic acids such as phenyl sulfonate, 3-(meth)acryloxy-2-hydroxypropyl sulfonate, 3-(meth)acryloxy-2-hydroxypropyl sulfophenyl ether, 3-(meth)acryloxy-2-hydroxypropyloxysulfobenzoate, 4-(meth)acryloxybutyl sulfonate, (meth)acrylamidomethyl sulfonic acid, (meth)acrylamidoethyl sulfonic acid, 2-methylpropanesulfonic acid (meth)acrylamide, and styrenesulfonic acid, as well as their monovalent metal salts, divalent metal salts, and ammonium salts and organic amine salts; amides of unsaturated monocarboxylic acids and amines having 1 to 30 carbon atoms, such as methyl(meth)acrylamide; vinyl aromatics such as styrene, α-methylstyrene, vinyltoluene, and p-methylstyrene; alkanediol mono(meth)acrylates such as 1,4-butanediol mono(meth)acrylate, 1,5-pentanediol mono(meth)acrylate, and 1,6-hexanediol mono(meth)acrylate; dienes such as butadiene, isoprene, 2-methyl-1,3-butadiene, and 2-chloro-1,3-butadiene;Unsaturated amides such as (meth)acrylamide, (meth)acrylalkylamide, N-methylol (meth)acrylamide, and N,N-dimethyl (meth)acrylamide; unsaturated cyanides such as (meth)acrylonitrile and α-chloroacrylonitrile; unsaturated amines such as aminoethyl (meth)acrylate, methylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, dibutylaminoethyl (meth)acrylate, and vinylpyridine; divinyl aromatics such as divinylbenzene; cyanurates such as triallyl cyanurate; polydimethylsiloxane propyl Suitable siloxane derivatives include propylaminomaleamic acid, polydimethylsiloxane aminopropyleneaminomaleamic acid, polydimethylsiloxane-bis-(propylaminomaleamic acid), polydimethylsiloxane-bis-(dipropyleneaminomaleamic acid), polydimethylsiloxane-(1-propyl-3-acrylate), polydimethylsiloxane-(1-propyl-3-methacrylate), polydimethylsiloxane-bis-(1-propyl-3-acrylate), and polydimethylsiloxane-bis-(1-propyl-3-methacrylate), and these can be used alone or in combination of two or more.
[0040] In one embodiment, the vinyl alcohol-based copolymer of the present disclosure preferably has a mass ratio of the structural unit (A), the structural unit (B), and the structural unit (C) of 1 to 98 / 1 to 98 / 1 to 98. It is more preferably 19 to 89 / 1 to 71 / 10 to 80, even more preferably 25 to 83 / 2 to 60 / 15 to 73, still more preferably 30 to 75 / 2 to 30 / 20 to 60, and particularly preferably 40 to 60 / 2 to 20 / 30 to 55. When the mass ratio of the structural unit (A), the structural unit (B), and the structural unit (C) contained in the vinyl alcohol-based copolymer of the present disclosure is within the above-mentioned range, anti-soil redeposition ability and biodegradability are improved, which is preferable.
[0041] When the vinyl alcohol-based copolymer of the present disclosure contains a structural unit (E1) other than the structural units (A) to (C), the content of the structural unit (E1) is preferably 0 to 10 mass%, more preferably 0 to 5 mass%, even more preferably 0 to 1 mass%, and most preferably 0 mass%, when the total amount of the structural units (A) to (C) and the structural unit (E1) constituting the vinyl alcohol-based copolymer of the present disclosure is taken as 100 mass%.
[0042] The weight-average molecular weight of the vinyl alcohol-based copolymer of the present disclosure is not particularly limited as long as it is 1,000 to 1,000,000. It is preferably 3,000 to 500,000, more preferably 5,000 to 200,000, even more preferably 7,000 to 100,000, even more preferably 8,000 to 50,000, particularly preferably 9,000 to 30,000, and most preferably 10,000 to 20,000. It is preferable for the weight-average molecular weight of the vinyl alcohol-based copolymer of the present disclosure to be within the above-mentioned range, as this copolymer has biodegradability and exhibits excellent anti-redeposition properties. The weight-average molecular weight of the vinyl alcohol-based copolymer can be measured by the method described in the Examples.
[0043] [Method for Producing Vinyl Alcohol-Based Copolymer] <Polymerization Conditions> The method for producing the vinyl alcohol-based copolymer of the present disclosure is not particularly limited, and the copolymer can be produced by copolymerizing a monomer component containing a monomer (A) represented by the following general formula (5) and a monomer (B) represented by the above general formula (3).
[0044] (In general formula (5), R 1 is -C(=O)-R x It is. x is a hydrogen atom or an organic group having 1 to 10 carbon atoms.) When the vinyl alcohol copolymer has the structural unit (C) of the general formula (4), it is preferable to use a monomer (C) represented by the following general formula (6) as the monomer component.
[0045] (In general formula (6), X represents a hydrocarbon group having 1 to 6 carbon atoms. R 3represents a hydrocarbon group having 2 to 6 carbon atoms. m represents an integer of 1 or 2. n represents an integer of 1 to 200.
[0046] R in the monomer (A) represented by the general formula (5) 1 is -C(=O)-R x and R x is not particularly limited as long as it is a hydrogen atom or an organic group having 1 to 10 carbon atoms. 1 is the same as R 1 R in x R in the general formula (1) x The same as R in the general formula (5). x is preferably a hydrogen atom or a methyl group, since this improves the polymerization reactivity of the vinyl carboxylate compound corresponding to the monomer that is the precursor of the structural unit (A) represented by the general formula (1) and facilitates hydrolysis of the protecting group in the hydrolysis (saponification) treatment carried out after the copolymerization reaction.
[0047] R of the monomer (B) represented by the general formula (3) x is not particularly limited as long as it is a hydrogen atom or an organic group having 1 to 10 carbon atoms. x The same as R in the general formula (3). x is preferably a hydrogen atom or a methyl group, since this improves the polymerization reactivity of the vinylamide compound corresponding to the monomer that is the precursor of the structural unit (B) represented by the general formula (2) and facilitates hydrolysis of the protecting group by the hydrolysis (saponification) treatment carried out after the copolymerization reaction.
[0048] R of the monomer (C) represented by the general formula (6) 3 is a hydrocarbon group having 2 to 6 carbon atoms, m is an integer of 1 or 2, and n is not particularly limited as long as it is an integer of 1 to 200. Regarding preferred embodiments, etc., R in the structural unit (C) represented by the general formula (4) 3, m, and n are the same. The monomer (C) represented by the general formula (6) can be produced by adding an alkylene oxide having 2 to 6 carbon atoms to a hydroxyvinyl ether such as 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, or diethylene glycol monovinyl ether. Among these, 2-hydroxyethyl vinyl ether and diethylene glycol monovinyl ether are preferred in terms of raw material availability and polymerizability. The method for producing a vinyl alcohol copolymer of the present disclosure includes a hydrolysis step in addition to a copolymerization step of monomer components including the monomer (A) represented by the general formula (5) and the monomer (B) represented by the general formula (3). The order of the copolymerization step and the hydrolysis step is not particularly limited, but considering the stability of the monomer (A) and the monomer (B), it is preferable to carry out the hydrolysis step after the copolymerization step in a state in which the monomers contain protecting groups. In one embodiment, the vinyl alcohol-based copolymer of the present disclosure is preferably prepared by copolymerizing a monomer component containing a vinyl carboxylate compound such as vinyl acetate and a vinylamine derivative represented by the general formula (3), followed by hydrolysis (saponification) with a basic substance such as sodium hydroxide or potassium hydroxide.
[0049] When carrying out the polymerization reaction, other polymerizable monomers may be used in addition to the vinyl carboxylate compound such as vinyl acetate and the vinylamine derivative represented by the general formula (3). The other polymerizable monomers are as described above, and specifically, it is preferable to use vinyl ethers such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, fumaric acid, citraconic acid, allyl alcohol, isoprenol, allyl alcohol EO adducts, isoprenol EO adducts, acrylamide, sodium acrylamidopropanesulfonate, sodium 2-hydroxy-3-allyloxypropanesulfonate, hydroxyethyl acrylate, hydroxyethyl methacrylate, ethylene glycol monovinyl ether, diethylene glycol monovinyl ether, and hydroxybutyl vinyl ether, as well as alkylene oxide adducts such as ethylene oxide and propylene oxide.
[0050] In the method for producing a vinyl alcohol copolymer according to the present disclosure, the ratio of the vinyl carboxylate compound such as vinyl acetate and the vinylamine derivative represented by the general formula (3) to the other polymerizable monomers is not particularly limited, and they can be polymerized at any ratio. If the ratio of the other polymerizable monomers is increased, biodegradability tends to decrease.
[0051] <Polymerization Initiator> Polymerization initiators commonly used in the production method can be used. Specific examples include hydrogen peroxide; persulfates such as sodium persulfate, potassium persulfate, and ammonium persulfate; azo compounds such as 2,2'-azobis(2-amidinopropane) hydrochloride, 4,4'-azobis-4-cyanovaleric acid, azobisisobutyronitrile, and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile); and organic peroxides such as benzoyl peroxide, lauroyl peroxide, peracetic acid, di-t-butyl peroxide, and cumene hydroperoxide. Among these polymerization initiators, hydrogen peroxide, persulfates, and 2,2'-azobis(2-amidinopropane) hydrochloride are preferred, with persulfates and 2,2'-azobis(2-amidinopropane) hydrochloride being more preferred. These polymerization initiators may be used alone, or two or more of them may be used in combination.
[0052] <Polymerization Conditions> The polymerization temperature in the production method is determined appropriately depending on the polymerization method, solvent, polymerization initiator, etc. used, but is preferably 25°C or higher. It is more preferably 50°C or higher, even more preferably 60°C or higher, and particularly preferably 80°C or higher. It is also preferably 200°C or lower. It is more preferably 150°C or lower, even more preferably 120°C or lower, and particularly preferably 110°C or lower. The polymerization temperature does not need to be maintained substantially constant during the polymerization reaction. For example, polymerization may be initiated from room temperature, the temperature may be raised to a set temperature over an appropriate heating time or rate, and then the set temperature may be maintained. Alternatively, the temperature may be varied (raised or lowered) over time during the polymerization reaction depending on the method of dropping the monomer components, initiator, etc. The polymerization temperature refers to the temperature of the reaction solution in the polymerization reaction. Any appropriate method or means can be used to measure and control the polymerization temperature. For example, it may be measured using a commonly used device.
[0053] The pressure during the polymerization reaction in the production method is not particularly limited, and any appropriate pressure can be used. For example, the reaction may be carried out under normal pressure (atmospheric pressure), reduced pressure, or increased pressure. The atmosphere in the reaction system may be an air atmosphere or an inert gas atmosphere. When the atmosphere in the reaction system is an inert gas atmosphere, this can be achieved, for example, by replacing the atmosphere in the reaction system with an inert gas such as nitrogen before the start of polymerization. This allows the atmospheric gas in the reaction system (e.g., oxygen gas) to dissolve in the liquid phase and act as a polymerization inhibitor.
[0054] In the above production method, after the addition of all the raw materials has been completed, an aging step may be carried out for the purpose of increasing the polymerization rate, etc. In the above production method, the polymerization time is not particularly limited, but is preferably 20 to 420 minutes.
[0055] <Hydrolysis (Saponification)> The hydrolysis carried out in the production method may be either acidic hydrolysis or basic hydrolysis. Basic hydrolysis is preferred. As a denaturant used in acidic hydrolysis, any compound that acts on a strong acidic state can be used. Examples include hydrochloric acid, bromic acid, hydrofluoric acid, sulfuric acid, nitric acid, phosphoric acid, sulfamic acid, and methanesulfonic acid. However, in terms of the solubility of the hydrolyzate in water, monovalent acids are preferred.
[0056] The modifying agent used in the basic hydrolysis may be any compound that acts as a strong base. Examples include sodium hydroxide, potassium hydroxide, lithium hydroxide, and quaternary ammonium hydroxide. The amount of the modifying agent used is typically 0.05 to 5 times the molar amount of the N-vinylformamide or N-vinylacetamide polymer, relative to the total number of formyl groups and ester groups in the vinyl carboxylate moieties, and is appropriately selected depending on the desired modification rate. The reaction temperature is typically 50 to 110°C, and the reaction time is typically 1 to 8 hours.
[0057] The hydrolysis may be carried out in two steps by hydrolysis (saponification) of the acetyl group (protecting group) of a vinyl carboxylate compound such as vinyl acetate, which is a monomer corresponding to the structural unit (A), and the protecting group in the general formula (3).
[0058] [Detergent composition containing vinyl alcohol-based copolymer] The detergent composition of the present disclosure contains the vinyl alcohol-based copolymer of the present disclosure as an essential component. The content of the vinyl alcohol-based copolymer of the present disclosure in the detergent composition of the present disclosure is not particularly limited, but from the viewpoint of being able to exhibit excellent anti-soil redeposition ability, the content of the vinyl alcohol-based copolymer of the present disclosure is preferably 0.1 to 15 mass% relative to the total amount of the detergent composition of the present disclosure. It is more preferably 0.3 to 10 mass%, and even more preferably 0.5 to 5 mass%.
[0059] Detergent compositions used in detergent applications contain surfactants and additives typically used in detergents. The specific forms of these surfactants and additives are not particularly limited, and conventional knowledge in the detergent field can be appropriately referenced. The detergent composition may be a powder detergent composition or a liquid detergent composition.
[0060] The surfactant is one or more selected from the group consisting of anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants. When two or more surfactants are used in combination, the total amount of the anionic surfactant and the nonionic surfactant is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more, based on the total amount of surfactants.
[0061] Suitable anionic surfactants include alkylbenzenesulfonates, alkyl ether sulfates, alkenyl ether sulfates, alkyl sulfates, alkenyl sulfates, α-olefin sulfonates, α-sulfofatty acid or ester salts, alkanesulfonates, saturated fatty acid salts, unsaturated fatty acid salts, alkyl ether carboxylates, alkenyl ether carboxylates, amino acid surfactants, N-acylamino acid surfactants, alkyl phosphates or salts thereof, alkenyl phosphates or salts thereof, etc. The alkyl and alkenyl groups in these anionic surfactants may be branched with an alkyl group such as a methyl group.
[0062] Suitable nonionic surfactants include polyoxyalkylene alkyl ethers, polyoxyalkylene alkenyl ethers, polyoxyethylene alkylphenyl ethers, higher fatty acid alkanolamides or their alkylene oxide adducts, sucrose fatty acid esters, alkyl glycoxides, fatty acid glycerin monoesters, alkylamine oxides, etc. The alkyl and alkenyl groups in these nonionic surfactants may be branched with an alkyl group such as a methyl group.
[0063] Suitable cationic surfactants include quaternary ammonium salts. Suitable amphoteric surfactants include carboxyl-type amphoteric surfactants and sulfobetaine-type amphoteric surfactants. The alkyl and alkenyl groups in these cationic and amphoteric surfactants may have branched alkyl groups such as methyl groups.
[0064] The blending ratio of the surfactant is not particularly limited as long as it is usually 10 to 60 mass % relative to the total amount of the detergent composition of the present disclosure, and is preferably 15 to 50 mass %, more preferably 20 to 45 mass %, and particularly preferably 25 to 40 mass %. If the blending ratio of the surfactant is too low, there is a risk that the detergent composition will not be able to exhibit sufficient detergency, and if the blending ratio of the surfactant is too high, there is a risk that the economical efficiency will decrease.
[0065] Suitable additives include alkali builders, chelate builders, anti-redeposition agents such as sodium carboxymethyl cellulose to prevent redeposition of contaminants, stain inhibitors such as benzotriazole and ethylene-thiourea, soil release agents, color transfer inhibitors, softeners, alkaline substances for adjusting pH, fragrances, solubilizers, fluorescent agents, colorants, foaming agents, foam stabilizers, glossing agents, disinfectants, bleaching agents, bleaching aids, enzymes, dyes, solvents, etc. In the case of powder detergent compositions, it is also preferable to incorporate zeolite.
[0066] The detergent composition may contain other detergent builders in addition to the polymer composition of the present invention. Examples of other detergent builders include, but are not limited to, alkali builders such as carbonates, bicarbonates, and silicates; chelating builders such as tripolyphosphates, pyrophosphates, Glauber's salt, nitrilotriacetates, ethylenediaminetetraacetates, citrates, (meth)acrylic acid copolymer salts, acrylic acid-maleic acid copolymers, fumarates, and zeolites; and carboxyl derivatives of polysaccharides such as carboxymethylcellulose. Examples of counter salts used for the above builders include alkali metals such as sodium and potassium, ammonium, and amines.
[0067] The total blending ratio of the additives and other detergent builders is usually preferably 0.1 to 50% by mass, more preferably 0.2 to 40% by mass, even more preferably 0.3 to 35% by mass, particularly preferably 0.4 to 30% by mass, and most preferably 0.5 to 20% by mass, relative to 100% by mass of the detergent composition. If the blending ratio of additives / other detergent builders is less than 0.1% by mass, the detergent performance may not be sufficient, while if it exceeds 50% by mass, the cost efficiency may decrease.
[0068] The concept of the detergent composition includes synthetic detergents for household cleaning, detergents for the textile industry and other industrial uses, hard surface cleaners, as well as detergents used only for specific purposes, such as bleaching detergents that enhance the function of one of their components.
[0069] When the detergent composition is a liquid detergent composition, the amount of water contained in the liquid detergent composition is usually preferably 0.1 to 75% by mass, more preferably 0.2 to 70% by mass, even more preferably 0.5 to 65% by mass, still more preferably 0.7 to 60% by mass, particularly preferably 1 to 55% by mass, and most preferably 1.5 to 50% by mass, relative to the total amount of the liquid detergent composition.
[0070] When the detergent composition is a liquid detergent composition, the detergent composition preferably has a kaolin turbidity of 200 mg / L or less, more preferably 150 mg / L or less, even more preferably 120 mg / L or less, particularly preferably 100 mg / L or less, and most preferably 50 mg / L or less.
[0071] The change (difference) in kaolin turbidity between a liquid detergent composition containing the polymer composition of the present invention as a detergent builder and a liquid detergent composition containing no polymer composition is preferably 500 mg / L or less, more preferably 400 mg / L or less, even more preferably 300 mg / L or less, particularly preferably 200 mg / L or less, and most preferably 100 mg / L or less. The kaolin turbidity value is determined by the following method.
[0072] <Method for measuring kaolin turbidity> A uniformly stirred sample (liquid detergent) is placed in a 50 mm square cell with a thickness of 10 mm, and after removing air bubbles, the turbidity (kaolin turbidity: mg / L) at 25°C is measured using a turbidity meter NDH2000 (trade name, manufactured by Nippon Denshoku Industries Co., Ltd.).
[0073] Suitable enzymes that can be incorporated into the detergent composition include proteases, lipases, cellulases, etc. Among these, proteases, alkaline lipases, and alkaline cellulases, which have high activity in alkaline cleaning solutions, are preferred.
[0074] The amount of the enzyme added is preferably 5% by mass or less relative to 100% by mass of the detergent composition. If the amount exceeds 5% by mass, the improvement in detergency may not be observed, and economic efficiency may decrease.
[0075] The detergent composition exhibits excellent cleaning effects with minimal salt deposition even when used in areas with hard water having high concentrations of calcium ions and magnesium ions (e.g., 100 mg / L or more), which is particularly pronounced when the detergent composition contains an anionic surfactant such as LAS.
[0076] The vinyl alcohol copolymer of the present disclosure can be used in water treatment agents, fiber treatment agents, dispersants, etc., in addition to the detergent compositions described above.
[0077] <Water Treatment Agent> The vinyl alcohol copolymer of the present disclosure can be used in a water treatment agent. The water treatment agent may contain other additives, such as polymerized phosphates, phosphonates, anticorrosives, slime control agents, and chelating agents, as needed. The water treatment agent is useful for preventing scale in cooling water circulation systems, boiler water circulation systems, seawater desalination plants, pulp digesters, black liquor concentration pots, and the like. Furthermore, the water treatment agent may contain any appropriate water-soluble polymer as long as it does not affect the performance and effects.
[0078] <Fiber Treatment Agent> The vinyl alcohol-based copolymer of the present disclosure can be used in a fiber treatment agent. The fiber treatment agent contains at least one selected from the group consisting of a dye, a peroxide, and a surfactant, and the vinyl alcohol-based copolymer of the present disclosure. The content of the vinyl alcohol-based copolymer of the present disclosure in the fiber treatment agent is preferably 1 to 100 wt %, more preferably 5 to 100 wt %, based on the total weight of the fiber treatment agent. Furthermore, any appropriate water-soluble polymer may be included within a range that does not affect performance and effects. Below is a formulation example of a fiber treatment agent that is closer to the embodiment. This fiber treatment agent can be used in the scouring, dyeing, bleaching, and soaping processes in fiber treatment. Examples of the dye, peroxide, and surfactant include those typically used in fiber treatment agents.
[0079] The blend ratio of the vinyl alcohol copolymer of the present disclosure and at least one selected from the group consisting of a dye, a peroxide, and a surfactant is preferably 0.1 to 100 parts by weight, calculated as the pure content of the fiber treatment agent, to 1 part by weight of the polymer composition of the present invention, in order to improve the whiteness, color uniformity, and colorfastness of the fiber. The fiber treatment agent can be used with any suitable fiber. Examples of fibers suitable for use with the fiber treatment agent include cellulosic fibers such as cotton and hemp, chemical fibers such as nylon and polyester, animal fibers such as wool and silk, semi-synthetic fibers such as rayon, and woven fabrics and blends thereof. When the fiber treatment agent is used in a scouring process, it is preferable to blend the vinyl alcohol copolymer of the present disclosure with an alkaline agent and a surfactant. When the fiber treatment agent is used in a bleaching process, it is preferable to blend the vinyl alcohol copolymer of the present disclosure with a peroxide and a silicic acid-based agent such as sodium silicate as a decomposition inhibitor for alkaline bleaches.
[0080] <Inorganic Pigment Dispersant> The vinyl alcohol copolymer of the present disclosure can be used as an inorganic pigment dispersant. The inorganic pigment dispersant may contain other additives, such as condensed phosphoric acid and its salts, phosphonic acid and its salts, and polyvinyl alcohol, as needed. The content of the vinyl alcohol copolymer of the present disclosure in the inorganic pigment dispersant is preferably 5 to 100 wt % based on the total inorganic pigment dispersant. Any suitable water-soluble polymer may also be included as long as it does not affect performance and effectiveness. The inorganic pigment dispersant can exhibit excellent performance as a dispersant for inorganic pigments such as heavy or light calcium carbonate and clay used in paper coating. For example, by adding a small amount of the inorganic pigment dispersant to an inorganic pigment and dispersing it in water, a high-concentration inorganic pigment slurry, such as a high-concentration calcium carbonate slurry, can be produced, which has low viscosity, high fluidity, and good stability over time. When the inorganic pigment dispersant is used as a dispersant for an inorganic pigment, the amount of the inorganic pigment dispersant used is preferably 0.05 to 2.0 parts by weight per 100 parts by weight of the inorganic pigment. When the amount of the inorganic pigment dispersant used is within the above range, it is possible to obtain a sufficient dispersing effect, and it is possible to obtain an effect commensurate with the amount added, which can be economically advantageous.
[0081] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass."
[0082] <Molecular weight measurement conditions> Apparatus: HLC-8320GPC manufactured by Tosoh Corporation Detector: RI Column: TSKgel SuperMultiporeHZ-M x 2 + TSK guard column SuperMP(HZ)-M manufactured by Tosoh Corporation Column temperature: 40°C Flow rate: 1.0 ml / min Calibration curve: POLYSTYRENE STANDARD manufactured by Tosoh Corporation Eluent: tetrahydrofuran / triethylamine = 99 / 1 (weight ratio)
[0083] <Production Example 1> A glass reaction vessel equipped with a thermometer, a nitrogen inlet tube, a reflux condenser, and a stirrer tip was charged with 14.57 g of ethanol, 13.52 g of vinyl acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 1.48 g of N-vinylacetamide (hereinafter also referred to as NVA) (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.43 g of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., V-65). The atmosphere inside the reaction vessel was replaced with nitrogen, and the temperature was raised to 60°C with stirring. The reaction solution was further stirred for 18 hours while maintaining it at 60°C. After confirming the consumption of each monomer, the solvent was distilled off under reduced pressure using an evaporator. The weight-average molecular weight of the resulting intermediate 1 was 16,500.
[0084] <Production Example 2> A glass reaction vessel equipped with a thermometer, nitrogen inlet tube, reflux condenser, and stirrer tip was charged with 14.56 g of ethanol, 13.74 g of vinyl acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 1.26 g of N-vinylformamide (hereinafter also referred to as NVF) (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.44 g of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., V-65). The atmosphere inside the reaction vessel was replaced with nitrogen, and the temperature was raised to 60°C with stirring. The reaction solution was further stirred for 18 hours while maintaining it at 60°C. After confirming the consumption of each monomer, the solvent was distilled off under reduced pressure using an evaporator. The weight-average molecular weight of the resulting intermediate 2 was 15,500.
[0085] <Production Example 3> A glass reaction vessel equipped with a thermometer, a nitrogen inlet tube, a reflux condenser, and a stirrer was charged with 18.49 g of ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and the atmosphere inside the reaction vessel was replaced with nitrogen. The temperature was then raised to 60°C while stirring. Next, with stirring, a total of three types of solution were added dropwise from separate dropping nozzles to a polymerization reaction system maintained at a constant temperature of 60°C: 45.79 g of vinyl acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.); an NVF solution consisting of 4.21 g of N-vinylformamide (manufactured by Tokyo Chemical Industry Co., Ltd.) and 16.83 g of ethanol; and an initiator solution consisting of 1.47 g of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., V-65) and 13.21 g of ethanol. The addition of the vinyl acetate, NVF solution, and initiator solution began simultaneously, with the vinyl acetate being added over 180 minutes, and the NVF solution and initiator solution being added over 240 minutes. After the completion of all the dropwise addition, the reaction solution was further aged at 60° C. for 8 hours to complete the polymerization, and then the solvent was distilled off under reduced pressure using an evaporator. The weight average molecular weight of the obtained intermediate 3 was 16,600.
[0086] Examples 1 to 3 5.12 g of intermediate 1 was placed in a glass reaction vessel equipped with a thermometer and a stirrer tip, and dissolved in 20.19 g of methanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). After confirming that intermediate 1 was completely dissolved, 1.19 g of a 4% NaOH-methanol suspension was added so that the concentration was 2 mol % relative to the acyl groups, and the temperature was raised to 50°C while stirring. After 3 hours, it was confirmed that the reaction product had precipitated, and the temperature was returned to room temperature. The solvent was distilled off under reduced pressure using an evaporator from the suspension in which the reaction product had precipitated, yielding polymer (1). Intermediates 2 and 3 were also saponified using the same procedure, yielding polymers (2) and (3).
[0087] Example 3-2 A glass reaction vessel equipped with a thermometer and a stirrer tip was charged with 0.51 g of polymer (3) obtained in Example 3, and 9.54 g of sulfuric acid (1%) was added. The temperature was raised to 80°C with stirring, and the polymer was completely dissolved, followed by stirring for 3 hours. The mixture was then returned to room temperature and neutralized by adding 1.94 g of an aqueous NaOH solution (1 M), to obtain an aqueous solution of polymer (3') obtained by deamidating polymer (3). The hydrolysis rate of polymer (3') after deamidation was 99% for vinyl ester groups and 86% for vinylamide groups.
[0088] Production Example 4 95.5 g of diethylene glycol monovinyl ether (manufactured by Tokyo Chemical Industry Co., Ltd.) and 0.29 g of potassium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were charged into a stainless steel high-pressure reactor equipped with a thermometer, a nitrogen inlet tube, and a stirrer, and the atmosphere inside the reaction vessel was replaced with nitrogen while stirring, and the temperature was raised to 120°C in a nitrogen atmosphere. 254.6 g of ethylene oxide was introduced into the reaction vessel while maintaining the temperature at 120°C under a safe pressure (nitrogen partial pressure in the reactor > ethylene oxide partial pressure). The temperature was further maintained at 120°C for 1 hour to complete the ethylene oxide addition reaction, yielding 350 g of an ethylene oxide adduct (hereinafter referred to as VE-10) in which an average of 8 moles of ethylene oxide had been added to diethylene glycol monovinyl ether.
[0089] Production Example 5 A glass reaction vessel equipped with a thermometer, a nitrogen inlet tube, a reflux condenser, and a stirrer was charged with 13.84 g of ethanol (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) and 19.47 g of VE-10, and the atmosphere inside the reaction vessel was replaced with nitrogen and then heated to 60° C. with stirring. Next, with stirring, a total of three types of initiator solutions were added dropwise from separate dropping nozzles to the polymerization reaction system kept at a constant temperature of 60° C.: an NVF solution consisting of 27.67 g of vinyl acetate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.), 2.86 g of N-vinylformamide (manufactured by Tokyo Chemical Industry Co., Ltd.), and 16.21 g of ethanol; and an initiator solution consisting of 1.00 g of 2,2′-azobis(2,4-dimethylvaleronitrile) (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., V-65), and 18.96 g of ethanol. The vinyl acetate, NVF solution, and initiator solution were added simultaneously, with the vinyl acetate added over 180 minutes and the NVF solution and initiator solution added over 240 minutes. After the entire addition was completed, the reaction solution was maintained at 60°C for an additional 8 hours to mature the mixture. The polymerization was then completed, and the solvent was then removed under reduced pressure using an evaporator. The resulting intermediate 4 had a weight-average molecular weight of 11,100.
[0090] Example 4 8.04 g of intermediate 1 was placed in a glass reaction vessel equipped with a thermometer and a stirrer tip, and dissolved in 32.4 g of methanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). After confirming that intermediate 1 was completely dissolved, 0.75 g of a 5% NaOH-methanol suspension was added, and the temperature was raised to 50°C while stirring. After 3 hours, it was confirmed that the reaction product had precipitated, and the temperature was returned to room temperature. The solvent was distilled off under reduced pressure using an evaporator from the suspension in which the reaction product had precipitated, to obtain polymer (4).
[0091] The proportion of ester groups in the structural unit (a) derived from vinyl acetate and the proportion of amide groups in the structural unit (b) derived from NVA or NVF in the polymers obtained in Examples 1 to 4 are as follows: 1 Measurement was carried out using H-NMR, and the results are shown in Table 1. The above ester group and amide group are groups that were not hydrolyzed.
[0092]
[0093] <Measurement of Anti-Redeposition Ability> A laundry process was performed in which the following washing, rinsing, and drying steps were performed in this order, and the anti-redeposition ability of the fabric was measured. Washing step: The following two types of cotton fabric were used as the laundry items. Cotton fabric (1): Five 5 cm x 5 cm cotton knitted fabrics (manufactured by Tanigashira Shoten) were prepared as cloths for assessing redeposition. Cotton fabric (2): Cotton fabric obtained from Testfabrics was prepared so that the total weight of the cotton fabric (2) and the cotton fabric (1) was 30 g. As surfactants, a 3% aqueous solution of LAS and 0.1% by mass aqueous solutions of the polymers (1) to (4) obtained in the Examples were prepared. 876 g of pure water at 25°C was placed in a 1 L pot for a Tergot-o-meter (manufactured by Daiei Scientific Co., Ltd., product name: TM-4), and then 4.5 g of a 1.5% by mass aqueous solution of sodium bicarbonate was added and stirred. Next, 4.5 g of 3000° DH hard water (prepared from calcium chloride and magnesium chloride, Ca / Mg = 3 (mass ratio)) was added, followed by 7.5 g of a 3% LAS aqueous solution and 7.5 g of a 0.1% aqueous solution of polymers (1) to (4) obtained in the examples, and the mixture was stirred. Next, 0.9 g of ordinary red clay was added and stirred, after which cotton cloths (1) and (2) were added, and washing was performed for 10 minutes at a stirring speed of 120 rpm and 25°C. Rinse process: After the washing process, the washed items were dehydrated for 1.5 minutes, and then 900 mL of 15° DH hard water at 25°C was added and rinsed for 3 minutes at 120 rpm and 25°C. This operation (dehydration and rinsing) was repeated twice. Drying process: After the rinsing process, the washed items were dehydrated for 1.5 minutes, and only cotton cloth (1) was removed, sandwiched between cotton cloths, and dried with an iron. The reflectance (Z value) of the cotton cloth (1) that had been washed as described above and the cotton cloth (1) before the washing treatment was measured using a reflectometer (spectrophotometric colorimeter, manufactured by Nippon Denshoku Industries Co., Ltd., product name: SE6000), and the anti-redeposition rate was calculated using the following formula: Anti-redeposition rate = (Z value of cotton cloth (1) after washing treatment) ÷ (Z value of cotton cloth (1) before washing treatment) × 100 The anti-redeposition rate (2) of the cotton cloth (1) after the washing treatment as described above is shown in Table 2.
[0094] <Biodegradability test> The biodegradability test of the obtained polymer was carried out in accordance with OECD 301F. Preparation of culture medium: Stock culture medium solutions A to D were prepared by the following method. Solution A: Potassium dihydrogen phosphate (KH 2 P.O. 4) 0.850 g, dipotassium hydrogen phosphate (K 2 HPO 4 ) 2.175 g, disodium hydrogen phosphate dodecahydrate (Na 2 HPO 4 ・12H 2 6.7217 g of ammonium chloride (NH 4 Solution B: 0.050 g of calcium chloride dihydrate (CaCl) was weighed into a 50 ml sample bottle, dissolved in an appropriate amount of water, and transferred to a 100 ml measuring flask, and then water was added up to the marked line. 2 ・2H 2 Solution C: Magnesium sulfate heptahydrate (MgSO ) 3.640 g was dissolved in an appropriate amount of water and transferred to a 100 ml measuring flask, and water was added up to the marked line. 4 ・7H 2 Solution D: Iron (III) chloride hexahydrate (FeCl 3 ・6H 2O) 0.025 g was dissolved in an appropriate amount of water and transferred to a 100 ml volumetric flask, and water was added up to the mark. The above stock medium solutions A to D were adjusted to 25°C. 10 ml of A was added to a 1 L volumetric flask using a whole pipette and diluted with approximately 800 ml of water. Then, 1 ml each of B, C, and D was added using a whole pipette and diluted up to the mark with water adjusted to 25°C. Multiple batches of the above medium were prepared according to the amount required for the test. The prepared medium was transferred to a 5 L beaker, mixed, and bubbled for at least 1 hour while stirring. Sludge Solution Preparation: The sludge used for the biodegradability test was obtained from the Minami Suita Sewage Treatment Plant. First, the concentration of the obtained sludge was measured using the following method. The obtained sludge was bubbled while stirring, and 5 ml was taken using a whole pipette and suction filtered using filter paper. Five sheets of filter paper containing sludge were prepared in this manner and dried in a dryer at 105°C for 1 hour. The sludge concentration was calculated from the average weight loss of the five sheets. This sludge was diluted with the culture medium prepared above to prepare a 1000 ppm sludge solution. Preparation of polymer aqueous solution: Polymers (1) to (4) obtained in Examples (1) to (4) were diluted with pure water to obtain a 2% by mass polymer aqueous solution. Furthermore, sodium benzoate was diluted with pure water to obtain a 2% by mass sodium benzoate aqueous solution as a standard substance. BOD test: A pressure sensor-type BOD meter was used to measure BOD. 144.75 g of the culture medium prepared above was weighed into a flask, and 0.75 g of a 2% polymer aqueous solution was added. Note that 0.75 g of pure water was added for the blank measurement, and 0.75 g of a 2% sodium benzoate aqueous solution was added for the standard substance measurement. The pH of the solution was then measured and adjusted to 7.4±0.2 with a 0.1 M aqueous hydrochloric acid solution. 4.5 ml of 1000 ppm sludge solution was then added to prepare a test solution. A stirrer was placed in the flask, and the CO 2 CO in the absorbent holder 21.8 g of absorbent (Yabashiri lime) was placed in the flask and set, and a BOD sensor was attached. The flask with the BOD sensor attached was stirred in a thermostatic bath at 24°C, and the BOD value was calculated from the pressure sensor. Calculation of decomposition rate: The theoretical oxygen demand (ppm) of the polymer was calculated, and the decomposition rate was calculated from the difference between the BOD value of the blank measurement and the BOD value measured using polymers (1) to (4) obtained in the Production Examples. The decomposition rate 28 days after the start of the test was taken as the biodegradation rate. The decomposition rates of the polymers are shown in Table 2. [Formula] Decomposition rate (%) = (biochemical oxygen consumption derived from the polymer) ÷ (theoretical oxygen demand of the polymer) × 100
[0095]
Claims
1. The present invention comprises a vinyl alcohol copolymer having a structural unit (A) represented by the following general formula (1) and a structural unit (B) represented by the following general formula (2), The vinyl alcohol copolymer has a weight average molecular weight of 1,000 to 50,000. [Formula 1] (In general formula (1), R 1 is a hydrogen atom or -C(=O)-R x Represents x represents a hydrogen atom or an organic group having 1 to 10 carbon atoms. [chemical 2] (In general formula (2), R 2 is a hydrogen atom or -C(=O)-R x Represents x represents a hydrogen atom or an organic group having 1 to 10 carbon atoms.
2. The detergent composition contains a vinyl alcohol copolymer having a structural unit (A) represented by the following general formula (1) and a structural unit (B) represented by the following general formula (2) in an amount of 0.1 to 15% by mass based on the total amount of the detergent composition: [C3] (In general formula (1), R 1 is a hydrogen atom, or -C(=O)-R x Represents x represents a hydrogen atom or an organic group having 1 to 10 carbon atoms. [C4] (In general formula (2), R 2 is a hydrogen atom or -C(=O)-R x Represents x represents a hydrogen atom or an organic group having 1 to 10 carbon atoms.) The detergent composition further comprises a surfactant in an amount of 10 to 60 mass % based on the total amount of the detergent composition.
3. The detergent composition according to claim 1, wherein the vinyl alcohol copolymer has, in the molecule, both a structural unit (b) in which R 2 in said general formula (2) is a hydrogen atom and a structural unit (b) in which R 2 is a -C(=O)-R x group.
4. 3. The detergent composition according to claim 1, wherein the vinyl alcohol copolymer has a mass ratio of the structural unit (A) to the structural unit (B) of 1-99 / 1-99.
5. 3. The detergent composition according to claim 1, wherein the content of the structural unit (E) other than the structural unit (A) and the structural unit (B) in the vinyl alcohol-based copolymer is 0 to 50% by mass, relative to 100% by mass of the total amount of the structural units (A), (B) and (E).
6. The vinyl alcohol copolymer is a copolymer having a structure represented by the formula (A) in which the —C═O—R x The ratio of 1 3. The detergent composition according to claim 1, wherein the total amount of the groups is 20 mol % or less, based on 100 mol %.
7. The vinyl alcohol copolymer is a copolymer having a structure represented by the formula (B): x The ratio of 2 3. The detergent composition according to claim 1, wherein the total amount of the groups is 99 mol % or less, based on 100 mol %.