Ceramic thermal spray particles and method for forming thermal barrier coating layer

JPWO2023248784A5Active Publication Date: 2024-10-08MITSUBISHI HEAVY IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024528744
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-06
Filing Date
2023-06-06
Publication Date
2024-10-08
Estimated Expiration
2043-06-06

AI Technical Summary

Technical Problem

Current thermal barrier coatings using ceramic spray particles have high thermal conductivity and inadequate thermal cycle durability, which limits their effectiveness in high-temperature applications such as industrial gas turbines.

Method used

The method involves forming ceramic spray particles composed of ZrO2 and Yb2O3 with a standard deviation of 2% to 7% by mass, which are then used to create a thermal barrier coating layer with a metal bonding layer, achieving low thermal conductivity and enhanced thermal cycle durability through specific manufacturing processes like plasma spraying.

Benefits of technology

The resulting thermal barrier coating exhibits low thermal conductivity and improved thermal cycle durability, effectively protecting high-temperature components by maintaining structural integrity and reducing thermal stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023248784000001
    Figure 2023248784000001
Patent Text Reader

Abstract

Ceramic thermal spray particles according to the present invention contain ZrO2 and Yb2O3, wherein the standard deviation of the content of the Yb2O3 is 2-7.0 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Ceramic spray particles and method for forming thermal barrier coating layer

[0001] This disclosure relates to ceramic thermal spray particles and a method for forming a thermal barrier coating layer. This application claims priority to Japanese Patent Application No. 2022-101154, filed on June 23, 2022, the contents of which are incorporated herein by reference.

[0002] Industrial gas turbines are being developed to be more efficient and operate at higher temperatures, and thermal barrier coatings (TBCs) applied to high-temperature components are an important element. Thermal barrier coatings are formed by, for example, plasma spraying of thermal spray materials.

[0003] Ceramic spray particles, which are thermal spray materials, are produced, for example, by a spray dryer. Patent Document 1 discloses a method for producing hollow ceramic powder for thermal spraying, which comprises preparing a raw material containing a stabilizer and a surfactant as a base material of high-purity zirconium oxide (ZrO), adding water to the raw material, dispersing the mixture to homogenize it, and then adding water to prepare a slurry with a raw material / water ratio of 1:1. The prepared slurry is then dropped into an atomizer rotating at high speed to be splashed and formed into particles, which are then swirled in a cyclone while being dried with high-temperature swirling air to evaporate water from the outer periphery of the particles, thereby obtaining hollow ceramic powder. The hollow ceramic powder is then sintered and solidified by heat treatment.

[0004] Japanese Patent No. 3825231

[0005] However, there is a demand for a thermal barrier coating that has a lower thermal conductivity than the thermal barrier coating using the ceramic spray particles produced by the production method described in Patent Document 1. In addition, there is also a demand for the thermal barrier coating to have high thermal cycle durability.

[0006] The present disclosure has been made to solve the above-mentioned problems, and aims to provide ceramic spray particles and a method for forming a thermal barrier coating layer that can form a thermal barrier coating that has low thermal conductivity and excellent thermal cycle durability.

[0007] The ceramic spray particles according to the present disclosure are ZrO 2 and Yb 2 O 3 and a ceramic spray particle containing Yb 2 O 3 The standard deviation of the content is 2% by mass or more and 7.0% by mass or less.

[0008] The method for forming a thermal barrier coating layer according to the present disclosure includes a metal bonding layer forming step of forming a metal bonding layer on a substrate, and a ceramic layer forming step of spraying ceramic spray particles onto the metal bonding layer to form a ceramic layer, the ceramic spray particles being ZrO 2 and Yb 2 O 3 and the Yb in the ceramic spray particles. 2 O 3 The standard deviation of the content is 2% by mass or more and 7.0% by mass or less.

[0009] According to the ceramic spray particles and the method for forming a thermal barrier coating layer according to the present disclosure, a thermal barrier coating having low thermal conductivity and excellent durability against thermal cycles can be formed.

[0010] 1 is a schematic cross-sectional view of a heat-resistant member according to the present disclosure; 2 is a flowchart of a method for forming a thermal barrier coating layer according to the present disclosure; 3 is a flowchart of a method for manufacturing ceramic spray particles according to the present disclosure; 4 is a schematic cross-sectional view of a laser-type thermal cycle testing device; and 5 is a graph showing the relationship between thermal conductivity and Yb of ceramic spray particles. 2 O 3 1 is a graph showing the relationship between the thermal cycle durability and the standard deviation of the Yb 2 O 3 1 is a graph showing the relationship between the thermal cycle durability and the cumulative particle diameter d10 of the ceramic spray particles.

[0011] <Heat-Resistant Member> A heat-resistant member having a thermal barrier coating layer according to the present disclosure formed thereon will now be described. Fig. 1 is a schematic cross-sectional view of a heat-resistant member 10 according to the present disclosure. The heat-resistant member 10 comprises a substrate 21, a metallic bonding layer 22 formed on the substrate 21, and a ceramic layer 23 formed on the metallic bonding layer 22. The thermal barrier coating layer 20 comprises the metallic bonding layer 22 and the ceramic layer 23.

[0012] (Substrate 21) The substrate 21 is a high-temperature heat-resistant alloy substrate used, for example, for buckets. The chemical composition of the substrate 21 includes, for example, in mass %, 20 to 40 mass % Ni, 10 to 30 mass % Cr, 4 to 15 mass % Al, 0.1 to 5 mass % Y, 0.5 to 10 mass % Re, and the remainder Co. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits. Numerical values ​​indicated as "less than" and "greater than" do not include the value in the numerical range.

[0013] (Metallic bonding layer 22) The metallic bonding layer 22 is formed directly on the substrate 21. The metallic bonding layer 22 reduces the difference in thermal expansion coefficient between the substrate 21 and the ceramic layer 23, thereby alleviating thermal stress. This prevents the ceramic layer 23 from peeling off from the metallic bonding layer 22. The metallic bonding layer 22 also prevents high-temperature oxidation and corrosion of the substrate 21. It is preferable to use a material with excellent corrosion resistance and oxidation resistance for the metallic bonding layer 22. The metallic bonding layer 22 is an MCrAlY alloy or the like. The M in the MCrAlY alloy represents a metal element, and indicates, for example, a single metal element such as Ni, Co, or Fe, or two or more of these metal elements.

[0014] (Ceramic Layer) The ceramic layer 23 is made of Yb 2 O 3 Partially stabilized ZrO 2 (hereinafter referred to as YbSZ). 2 O 3 and ZrO 2The ceramic layer 23 made of YbSZ may contain impurities other than those mentioned above. The impurities may be, for example, components mixed in the raw materials or components mixed in during the manufacturing process. The ceramic layer 23 made of YbSZ has excellent crystal stability, and therefore can also suppress the generation of stress due to phase transformation.

[0015] ZrO 2 The content of ZrO is 75 mass % or more based on the total mass of the thermal barrier coating layer 20. 2 The content of ZrO is 80 mass % or more. 2 The content of ZrO is 90 mass % or less. 2 The content is 84 mass % or less.

[0016] Yb 2 O 3 The content of Yb is preferably 10 mass % or more with respect to the total mass of the thermal barrier coating layer 20. 2 O 3 When the content of Yb is 10 mass % or more, the thermal cycle durability of the thermal barrier coating layer 20 is improved. 2 O 3 The content of Yb is 16 mass % or more. 2 O 3 The content of Yb is preferably 25 mass % or less. 2 O 3 If the content of Yb exceeds 25 mass %, the durability of the thermal barrier coating layer 20 may decrease. 2 O 3 The content is 20 mass % or less.

[0017] In the ceramic layer 23, Yb 2 O 3 The standard deviation of the content of Yb is 2 mass% or more and 7.0 mass% or less. 2 O 3 If the standard deviation of the content of Yb is less than 2 mass %, the thermal conductivity of the ceramic layer 23 becomes high, which is not preferable. 2 O 3 If the standard deviation of the content exceeds 7.0 mass %, the thermal cycle durability decreases, which is not preferable.

[0018] The chemical compositions of the metal bonding layer 22 and the ceramic layer 23 can be analyzed using a known method. For example, the heat-resistant member 10 is cut to obtain a specimen for observation, and a cross section of the specimen is randomly analyzed at 10 points using an electron probe microanalyzer. From the obtained Yb and Zr contents (atomic %), the Yb 2 O 3 and ZrO 2 The content of Yb obtained is calculated. 2 O 3 The average value of the content of Yb 2 O 3 The content of ZrO 2 The average content of ZrO 2 At the same time, the content of Yb 2 O 3 and ZrO 2 The standard deviation of can be evaluated similarly.

[0019] The porosity of the ceramic layer 23 is preferably 4% or more and 20% or less. The porosity of the ceramic layer 23 means the area ratio of pores in the ceramic layer 23. The porosity can be determined, for example, by observing a cross section of the ceramic layer 23 at random five fields of view (observation length of approximately 3 mm) using an optical microscope (magnification 100 times) and using an image processing method.

[0020] The thickness of the ceramic layer 23 is preferably 0.1 to 1.5 mm. If the thickness of the ceramic layer 23 is less than 0.1 mm, the heat-shielding properties of the ceramic layer 23 may be insufficient. If the thickness of the ceramic layer 23 exceeds 5 mm, the ceramic layer 23 may peel off easily, and the durability of the ceramic layer 23 may decrease.

[0021] The heat-resistant member 10 has been described above. 2 O 3 ZrO stabilized with 2 By using the ceramic layer 23 as a ceramic material, the crystal stability of the ceramic layer 23 is improved, and even when the ceramic layer 23 is used in a high-temperature component such as a turbine, the crystal phase of the ceramic layer 23 is less likely to change during a thermal cycle, making it possible to prevent cracks and their progression due to phase transformation.

[0022] <Method of Forming Thermal Barrier Coating Layer> A method of forming the thermal barrier coating layer 20 of the present disclosure will now be described. Fig. 2 is a flowchart of the method of forming the thermal barrier coating layer 20. The method of forming the thermal barrier coating layer 20 includes a metallic bonding layer forming step S1 of forming a metallic bonding layer 22 on the substrate 21, and a ceramic layer forming step S2 of forming a ceramic layer 23 by thermally spraying ceramic spray particles on the metallic bonding layer 22 after the metallic bonding layer forming step S1.

[0023] (Metallic bonding layer forming step S1) In the metallic bonding layer forming step S1, a metallic bonding layer 22 is formed on the substrate 21. The method for forming the metallic bonding layer 22 is not particularly limited. The metallic bonding layer 22 can be formed by a low-pressure plasma spraying method, an electron beam physical vapor deposition method, or the like. Note that the substrate 21 on which the metallic bonding layer 22 has been formed in advance may be prepared as the substrate for thermal spraying.

[0024] (Ceramic layer forming step S2) In the ceramic layer forming step S2, the ceramic layer 23 is formed on the metal bonding layer 22. The ceramic layer 23 is formed by spraying ceramic spray particles onto the metal bonding layer 22. The spraying method is not particularly limited, but for example, a low-pressure plasma spraying method can be used.

[0025] (Ceramic spray particles) Next, the ceramic spray particles used in the ceramic layer forming step S2 will be described. The ceramic spray particles of the present disclosure are made of zirconium oxide (ZrO 2 ) and ytterbia (Yb 2 O 3 ) and contains.

[0026] In ceramic spray particles, ZrO 2 The content of ZrO is 75 mass % or more based on the total mass of the ceramic spray particles. 2 The content of ZrO is 80 mass % or more. 2 The content of ZrO is 90 mass % or less. 2 The content is 84 mass % or less.

[0027] Yb 2 O3 The content of Yb is preferably 10 mass % or more based on the total mass of the ceramic spray particles. 2 O 3 When the content of Yb is 10 mass % or more, the durability (thermal cycle durability) of the thermal barrier coating layer 20 is improved. 2 O 3 The content of Yb is 16 mass % or more. 2 O 3 The content of Yb is preferably 25 mass % or less. 2 O 3 If the content of Yb exceeds 25 mass %, the durability of the thermal barrier coating layer 20 may decrease. 2 O 3 The content is 20 mass % or less.

[0028] In ceramic spray particles, Yb 2 O 3 The standard deviation of the content of Yb is 2 mass% or more and 7.0 mass% or less. 2 O 3 If the standard deviation of the content of Yb is less than 2 mass %, the thermal conductivity of the ceramic layer 23 becomes high, which is not preferable. 2 O 3 The standard deviation of the content of Yb is preferably 2.0 mass% or more with respect to the total mass of the ceramic spray particles. 2 O 3 The standard deviation of the content of Yb is 2.3 mass% or more. 2 O 3 The standard deviation of the content of Yb is preferably 5.3 mass% or less. 2 O 3 If the standard deviation of the content exceeds 7.0 mass %, the thermal cycle durability decreases, which is not preferable.

[0029] The in-plane distribution of the chemical composition of ceramic spray particles can be analyzed using a known method. For example, ceramic spray particles are embedded in a resin and then cut. The cut cross section is polished to prepare a specimen for observation. The cross section of the obtained specimen is subjected to point analysis at 10 random locations using an electron probe microanalyzer. From the obtained Yb and Zr contents (atomic %), the Yb 2 O 3 and ZrO 2 The content of Yb obtained is calculated. 2 O 3 The average value of the content of Yb 2 O 3 The content of ZrO 2 The average content of ZrO 2 At the same time, the content of Yb 2 O 3 and ZrO 2 The standard deviation of is evaluated in the same way.

[0030] The cumulative particle size d10 of the ceramic spray particles is preferably 40 μm or more. More preferably, the cumulative particle size d10 of the ceramic spray particles is 45 μm or more. When the cumulative particle size d10 of the ceramic spray particles is 40 μm or more, the porosity of the ceramic layer 23 is improved and the thermal cycle durability of the ceramic layer 23 can be further improved. The cumulative particle size d10 of the ceramic spray particles is preferably 100 μm or less. More preferably, the cumulative particle size d10 of the ceramic spray particles is 51 μm. The cumulative particle size d10 can be measured based on JIS Z 8825:2013. The cumulative particle size d10 refers to the particle size below which 10% of the population lies. The cumulative particle size d10 refers to the particle size that is 10% of the total particle size from the small particle size side on the volume distribution curve.

[0031] The maximum particle size of the ceramic spray particles is preferably 150 μm or less. By setting the maximum particle size of the ceramic spray particles to 150 μm or less, the ceramic spray particles can be easily melted in plasma spraying. The maximum particle size of the ceramic spray particles is the particle size represented by the smallest mesh opening of a metal mesh sieve through which all of the ceramic spray particles can pass.

[0032] The ceramic spray particles of the present disclosure are preferably hollow. If the ceramic spray particles are hollow, the porosity of the ceramic layer 23 is improved, and the heat-shielding properties can be further improved.

[0033] The foregoing has described the disclosed ceramic spray particles and the method for forming the thermal barrier coating layer 20. The disclosed ceramic spray particles and the method for forming the thermal barrier coating layer 20 make it possible to form a thermal barrier coating that has low thermal conductivity and excellent thermal cycle durability.

[0034] <Method for manufacturing ceramic spray particles> Next, a method for manufacturing ceramic spray particles according to the present disclosure will be described. Fig. 3 is a flowchart of the method for manufacturing ceramic spray particles according to the present disclosure. The method for manufacturing ceramic spray particles according to the present disclosure is a method for manufacturing ceramic spray particles by using ZrO 2 Powder and a specified addition ratio of Yb 2 O 3 The method includes a mixing step S11 in which powder and water are mixed to produce a slurry, a powder formation step S12 in which powder is produced from the slurry, a solid solution formation step S13 in which the powder is made into a solid solution, and a classification step S14 in which the powder after the solid solution formation is classified.

[0035] (Mixing step S11) In the mixing step S11, Yb 2 O 3 The standard deviation of the content of ZrO is 2 mass% or more and 7.0 mass% or less. 2 Powder and Yb 2 O 3 The powder and water are mixed to produce a slurry. 2 powder, Yb 2 O 3 It is preferable to add a surfactant to the mixture (powder, and water). By adding a surfactant, the aggregated ZrO 2 powder, Yb 2 O 3 This can promote re-separation of the powder. 2 Powder and Yb 2 O 3The weight ratio of the powder to water is not particularly limited, but is, for example, 1: 1. It is preferable to add water and a binder to the slurry before the powder formation step S12.

[0036] The raw materials can be mixed using, for example, a ball mill, a bead mill, etc. When a bead mill is used, the mixing time is, for example, 8 to 10 hours. If the mixing time is too long, the Yb 2 O 3 The standard deviation of the content of is less than 2 mass %, which increases the thermal conductivity of the ceramic layer 23. If the mixing time is short, the standard deviation exceeds 7 mass %, which decreases the thermal cycle durability of the ceramic layer 23. The mixing conditions vary depending on the mixing device, so it is preferable to adjust them appropriately to suit the device.

[0037] When a bead mill is used, the rotation speed during mixing of the raw materials is, for example, 10 to 30 rpm. The rotation speed can be adjusted appropriately depending on the mixing device.

[0038] (Powder Formation Step S12) In the powder formation step S12, powder is produced from the slurry obtained in the mixing step S11. Specifically, the powder is produced by spray-drying the slurry. The spray-drying method is not particularly limited. For example, in the case of a spin disk method, the disk is rotated at high speed (10,000 rpm), so the slurry is sprayed off while forming spherical shapes. The spherical slurry is dried and rotated by high-temperature swirling air (approximately 200°C). At this time, the slurry is gradually dried from the outside in the dry air and solidifies. Because the raw material particles in the slurry are coarse, water evaporates from the gaps between the raw material particles. This allows for the production of ceramic spray particles with hollow interiors.

[0039] (Solid Solution Formation Step S13) In the solid solution formation step S13, the powder obtained in the powder formation step S12 is solid-solution formed. Specifically, the obtained powder is heat-treated in a heat treatment furnace at 1450°C for 10 hours. The temperature at this time is the set temperature of the heat treatment furnace. This heat treatment results in ZrO 2 and Yb 2 O 3 However, this can be diffused and solid-solved, resulting in strength suitable for thermal spraying.

[0040] (Classification step S14) In the classification step S14, the powder after solid solution formation is classified to obtain ceramic spray particles. In the classification step S14, it is preferable to classify the particles into particles with a particle size of 150 μm or less. That is, it is preferable to set the maximum particle size of the ceramic spray particles to 150 μm or less. If the particle size of the ceramic spray particles exceeds 150 μm, they may not melt well in the plasma spraying process. Furthermore, in the classification step S14, it is preferable to remove small particle diameter ceramic spray particles so that the cumulative particle size d10 is 40 μm or more. The classification method is not particularly limited, and for example, a gyro shifter can be used.

[0041] The method for producing ceramic spray particles according to the present disclosure has been described above. The method for producing ceramic spray particles according to the present disclosure can produce ceramic spray particles that can form a thermal barrier coating having low thermal conductivity and excellent durability against thermal cycles.

[0042] The technical scope of the present invention is not limited to the above-described embodiments, and various modifications can be made without departing from the spirit of the present invention. In addition, the components in the above-described embodiments can be replaced with well-known components as appropriate without departing from the spirit of the present invention.

[0043] Next, examples of the present invention will be described, but the conditions in the examples are merely examples adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to these examples. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.

[0044] Example 1 ZrO 2 and Yb 2 O 3The mass ratio of the water to the surfactant was 84:16:100:1, and mixing was carried out using a bead mill for 8 hours at a rotation speed of 18 rpm to prepare a slurry, to which water and a binder were added in a mass ratio of 50:2. Powder was prepared from the slurry by spray drying, and the obtained powder was heated in a heat treatment furnace at 1450°C for 10 hours. The obtained powder was classified (40 μm to 150 μm) to obtain the ceramic spray particles of Example 1. The ceramic spray particles of Example 1 were embedded in resin and cut. When the cross section was observed, the ceramic spray particles of Example 1 were found to be hollow particles. Measurement by the method described below revealed that the proportion of Yb relative to the total mass of the ceramic spray particles of Example 1 was 1. 2 O 3 The standard deviation of the concentration was ±2.6 mass %, and the 10% cumulative particle size d10 of the ceramic spray particles of Example 1 was 43 μm.

[0045] Example 2 ZrO 2 and Yb 2 O 3 The mass ratio of the water to the surfactant was 84:16:100:1, and mixing was carried out using a bead mill for 8 hours at a rotation speed of 25 rpm to prepare a slurry, to which water and a binder were added in a mass ratio of 50:2. Powder was prepared from the slurry by spray drying, and the obtained powder was heated in a heat treatment furnace at 1450°C for 10 hours. The obtained powder was classified to obtain the ceramic spray particles of Example 2. The ceramic spray particles of Example 2 were embedded in resin and cut. When the cross section was observed, the ceramic spray particles of Example 2 were found to be hollow particles. Measurement by the method described below revealed that the proportion of Yb relative to the total mass of the ceramic spray particles of Example 2 was 1.0%. 2 O 3 The standard deviation of the concentration was ±2.3 mass %, and the 10% cumulative particle size d10 of the ceramic spray particles of Example 2 was 49 μm.

[0046] (Example 3) ZrO 2 and Yb 2 O 3The mass ratio of the water to the surfactant was 84:16:100:1, and mixing was carried out using a bead mill for 8 hours at a rotation speed of 5 rpm to prepare a slurry, to which water and a binder were added in a mass ratio of 50:2. Powder was prepared from the slurry by spray drying, and the obtained powder was heated in a heat treatment furnace at 1450°C for 10 hours. The obtained powder was classified (40 μm to 150 μm) to obtain the ceramic spray particles of Example 2. The ceramic spray particles of Example 3 were embedded in resin and cut. When the cross section was observed, the ceramic spray particles of Example 3 were found to be hollow particles. Measurement by the method described below revealed that the proportion of Yb relative to the total mass of the ceramic spray particles of Example 3 was 1.0%. 2 O 3 The standard deviation of the concentration was ±5.3 mass %, and the 10% cumulative particle size d10 of the ceramic spray particles of Example 3 was 43 μm.

[0047] (Example 4) ZrO 2 and Yb 2 O 3 The mass ratio of the water to the surfactant was 84:16:100:1, and mixing was carried out using a bead mill for 10 hours at a rotation speed of 25 rpm to prepare a slurry, to which water and a binder were added in a mass ratio of 50:2. Powder was prepared from the slurry by spray drying, and the obtained powder was heated in a heat treatment furnace at 1450°C for 10 hours. The obtained powder was classified (40 μm to 150 μm) to obtain the ceramic spray particles of Example 4. The ceramic spray particles of Example 4 were embedded in resin and cut. When the cross section was observed, the ceramic spray particles of Example 4 were found to be hollow particles. Measurement by the method described below revealed that the proportion of Yb relative to the total mass of the ceramic spray particles of Example 4 was 1.0%. 2 O 3 The standard deviation of the concentration was ±2.5 mass %, and the 10% cumulative particle size d10 of the ceramic spray particles of Example 4 was 51 μm.

[0048] (Comparative Example 1) ZrO 2 and Yb 2 O 3The mass ratio of the water to the surfactant was 84:16:100:1, and mixing was carried out using a bead mill for 15 hours at a rotation speed of 10 rpm to prepare a slurry, to which water and a binder were added in a mass ratio of 50:2. Powder was prepared from the slurry by spray drying, and the obtained powder was heated in a heat treatment furnace at 1450°C for 10 hours. The obtained powder was classified (40 μm to 150 μm) to obtain the ceramic spray particles of Comparative Example 1. The ceramic spray particles of Comparative Example 1 were embedded in resin and cut. When the cross section was observed, the ceramic spray particles of Comparative Example 1 were found to be hollow particles. Measurement by the method described below revealed that the proportion of Yb relative to the total mass of the ceramic spray particles of Comparative Example 1 was 1. 2 O 3 The standard deviation of the concentration was ±0.2 mass %, and the 10% cumulative particle size d10 of the ceramic spray particles of Comparative Example 1 was 43 μm.

[0049] (Comparative Example 2) ZrO 2 and Yb 2 O 3 The mass ratio of the water to the surfactant was 84:16:100:1, and mixing was carried out using a bead mill for 15 hours at a rotation speed of 25 rpm to prepare a slurry, to which water and binder were added in a mass ratio of 50:2. Powder was prepared from the slurry by spray drying, and the obtained powder was heated in a heat treatment furnace at 1450°C for 10 hours. The obtained powder was classified (40 μm to 150 μm) to obtain the ceramic spray particles of Comparative Example 2. The ceramic spray particles of Comparative Example 2 were embedded in resin and cut. When the cross section was observed, the ceramic spray particles of Comparative Example 2 were found to be hollow particles. Measurement by the method described below revealed that the proportion of Yb relative to the total mass of the ceramic spray particles of Comparative Example 2 was 1.0%. 2 O 3 The standard deviation of the concentration was ±1.2 mass %, and the 10% cumulative particle size d10 of the ceramic spray particles of Comparative Example 2 was 46 μm.

[0050] (Comparative Example 3) ZrO 2 and Yb 2 O 3The mass ratio of the water to the surfactant was 84:16:100:1, and mixing was carried out using a bead mill for 15 hours at a rotation speed of 25 rpm to prepare a slurry, to which water and a binder were added in a mass ratio of 50:2. Powder was prepared from the slurry by spray drying, and the powder was classified (40 μm to 150 μm) without heat treatment to obtain the ceramic spray particles of Comparative Example 3. The ceramic spray particles of Comparative Example 3 were embedded in resin and cut. When the cross section was observed, the ceramic spray particles of Comparative Example 3 were found to be hollow particles. Measurement by the method described below revealed that the proportion of Yb relative to the total mass of the ceramic spray particles of Comparative Example 3 was 1.0%. 2 O 3 The standard deviation of the concentration was ±7.3 mass %, and the 10% cumulative particle size d10 of the ceramic spray particles of Comparative Example 3 was 50 μm.

[0051] (Formation of Thermal Barrier Coating Layer) The test specimen used was a 5 mm-thick heat-resistant alloy substrate (trade name: IN-738LC) on which a 100 μm-thick metallic bonding layer (Ni: 32 mass %, Cr: 21 mass %, Al: 8 mass %, Y: 0.5 mass %, Co: balance) was formed by low-pressure plasma spraying. Using the ceramic spray particles of Examples 1 to 4 and Comparative Examples 1 to 3 produced above, a ceramic layer (YbSZ layer) was laminated on the metallic bonding layer by atmospheric plasma spraying to form a thermal barrier coating layer. Note that the thickness of the metallic bonding layer (CoNiCrAlY) and the thickness of the ceramic layer (YbSZ) were the same for all samples, at 0.1 mm and 0.5 mm, respectively.

[0052] (Yb ceramic spray particles 2 O 3 For each of the ceramic spray particles in Examples 1 to 4 and Comparative Examples 1 to 3, the standard deviation of the content of Yb 2 O 3 The standard deviation of the Yb and Zr contents was measured. Specifically, it was measured by the following method. The obtained ceramic spray particles were embedded in a resin and cut. The cut cross section was polished, and the polished cross section was subjected to point analysis at 10 random locations using an electron probe microanalyzer. The Yb content was calculated from the Yb and Zr contents (atomic %) obtained by the point analysis. 2 O 3 and ZrO2 The content was calculated and the standard deviation was determined.

[0053] (Cumulative particle size d10 of ceramic spray particles) The particle size distribution of each ceramic spray particle in Examples 1 to 4 and Comparative Examples 1 to 3 was measured using a laser scattering diffraction particle size distribution measuring device (manufactured by Microtrac). The cumulative particle size d10 of each ceramic spray particle in Examples 1 to 4 and Comparative Examples 1 to 3 was obtained from the obtained particle size distribution. The maximum particle size of the ceramic spray particles was measured using a mesh. The maximum particle size of the ceramic spray particles in Examples 1 to 4 and Comparative Examples 1 to 3 was 150 μm.

[0054] (Thermal Conductivity) The thermal conductivity of the thermal barrier coating layers of Examples 1 to 4 and Comparative Examples 1 to 3 was measured by the laser flash method specified in JIS R1611:2010.

[0055] (Thermal Cycle Durability) The thermal cycle durability of the thermal barrier coating layers using the ceramic spray particles of Examples 1 to 4 and Comparative Examples 1 to 3 obtained above was evaluated. FIG. 4 is a schematic cross-sectional view of a laser-type thermal cycle testing device used to evaluate the thermal cycle durability. In the laser-type thermal cycle testing device shown in this figure, a sample 31, which had a thermal barrier coating layer 20 formed on a substrate 21, was placed on a sample holder 32 arranged on a main body 33, with the thermal barrier coating layer 20 facing outward. CO 2 Laser light L was irradiated from the laser device 30 to heat the sample 31 from the side of the thermal barrier coating layer 20. Simultaneously with the heating by the laser device 30, the sample 31 was cooled from its back side by a gas flow F that penetrated the main body 33 and was discharged from the tip of a cooling gas nozzle 34 that was disposed inside the main body 33 at a position facing the back side of the sample 31.

[0056] The heating time was 3 minutes, the cooling time was 3 minutes, and the maximum surface temperature was 900°C. Various maximum surface heating temperatures were set, and the number of thermal cycles until the ceramic layer peeled off was measured. The highest temperature among the surface heating temperatures at which 1000 cycles were completed was determined as the 1000 cycle end temperature. A higher 1000 cycle end temperature indicates higher thermal cycle durability.

[0057] Figure 5 shows the thermal conductivity of the thermal barrier coating layer and the Yb 2 O 3 The horizontal axis of FIG. 5 is the standard deviation of the Yb content in the ceramic spray particles. 2 O 3 The vertical axis represents the standard deviation (± mass%) of the Yb content in the ceramic spray particles. 2 O 3 When the standard deviation of the thermal conductivity was less than 2.0% (Comparative Example 1 and Comparative Example 2), the thermal conductivity tended to be high. It is presumed that the materials were mixed uniformly in Comparative Example 1 and Comparative Example 2 due to the longer stirring time, resulting in a higher thermal conductivity. 2 O 3 When the standard deviation of was 2.0% or more, the thermal conductivity tended to be low. 2 O 3 It is estimated that the large standard deviation (variation) of the temperature makes it easier for heat to be scattered at the interface between different phases, resulting in a decrease in thermal conductivity.

[0058] Figure 6 shows the thermal cycle durability of the thermal barrier coating layer and the Yb 2 O 3 The horizontal axis of FIG. 6 represents the relationship between the standard deviation of Yb in the ceramic spray particles. 2 O 3 The vertical axis of FIG. 6 represents the temperature (°C) at which 1000 cycles are completed. Examples 1 to 4 and Comparative Examples 1 and 2 exhibited sufficient thermal cycle durability, but the temperature at which 1000 cycles are completed in Comparative Example 3 was below 600°C. Comparative Example 3 was characterized by the use of Yb ceramic spray particles. 2 O 3 It is estimated that the thermal cycle durability was low due to the large variation in temperature.

[0059] Fig. 7 is a graph showing the relationship between the thermal cycle durability of the thermal barrier coating layer and the cumulative particle size d10 of the ceramic spray particles. The horizontal axis of Fig. 7 represents the cumulative particle size d10 (µm) of the ceramic spray particles, and the vertical axis of Fig. 7 represents the 1000 cycle turnover temperature (°C). As shown in Fig. 7, the 1000 cycle turnover temperature increased as the cumulative particle size d10 of the ceramic spray particles increased. In particular, when the cumulative particle size d10 was 45 µm or more, high thermal cycle durability of 700°C was observed.

[0060] From the above results, it was confirmed that by using the ceramic spray particles and the method for forming a thermal barrier coating layer disclosed herein, it is possible to form a thermal barrier coating that has low thermal conductivity and excellent thermal cycle durability.

[0061] <Additional Notes> The ceramic spray particles and the method for forming a thermal barrier coating layer described in the above embodiment can be understood as follows.

[0062] (1) The ceramic spray particles according to the first aspect of the present disclosure are ZrO 2 and Yb 2 O 3 and a ceramic spray particle containing the Yb 2 O 3 The standard deviation of the content is 2% by mass or more and 7.0% by mass or less.

[0063] In this way, a thermal barrier coating having low thermal conductivity and excellent durability against thermal cycles can be formed.

[0064] (2) The ceramic spray particles according to a second aspect of the present disclosure are the ceramic spray particles according to (1), which contain, in mass % with respect to the total mass of the ceramic spray particles, Yb 2 O 3 The content is 16 mass % or more.

[0065] This improves the thermal cycle durability of the thermal barrier coating layer 20 .

[0066] (3) The ceramic spray particles according to the third aspect of the present disclosure are the ceramic spray particles of (1) or (2), having an integrated particle size d10 of 40 μm or more.

[0067] By doing so, the thermal cycle durability of the thermal barrier coating layer 20 is further improved.

[0068] (4) The ceramic spray particles according to a fourth aspect of the present disclosure are the ceramic spray particles of (3), in which the cumulative particle diameter d10 is 45 μm or more.

[0069] By doing so, the thermal cycle durability of the thermal barrier coating layer 20 is further improved.

[0070] (5) A method for forming a thermal barrier coating layer according to a fifth aspect of the present disclosure includes a metallic bonding layer forming step S1 of forming a metallic bonding layer on a substrate, and a ceramic layer forming step S2 of spraying ceramic spray particles onto the metallic bonding layer to form a ceramic layer, the ceramic spray particles being ZrO 2 and Yb 2 O 3 and the Yb in the ceramic spray particles. 2 O 3 The standard deviation of the content is 2% by mass or more and 7.0% by mass or less.

[0071] In this way, a thermal barrier coating having low thermal conductivity and excellent durability against thermal cycles can be formed.

[0072] (6) A method for forming a thermal barrier coating layer according to a sixth aspect of the present disclosure is the method for forming a thermal barrier coating layer according to (5), wherein the Yb 2 O 3 The content is 16 mass % or more.

[0073] By doing so, the thermal cycle durability of the thermal barrier coating layer 20 is further improved.

[0074] (7) A seventh aspect of the present disclosure relates to a method for forming a thermal barrier coating layer according to (5) or (6), wherein the cumulative particle size d10 of the ceramic spray particles is 40 μm or more.

[0075] By doing so, the thermal cycle durability of the thermal barrier coating layer 20 is further improved.

[0076] (8) A method for forming a thermal barrier coating layer according to an eighth aspect of the present disclosure is the method for forming a thermal barrier coating layer according to (7), in which the cumulative grain size d10 is 45 μm or more.

[0077] By doing so, the thermal cycle durability of the thermal barrier coating layer 20 is further improved.

[0078] According to the ceramic spray particles and the method for forming a thermal barrier coating layer of the present disclosure, a thermal barrier coating having low thermal conductivity and excellent durability against thermal cycles can be formed.

[0079] S1 metal bonding layer formation process, S2 ceramic layer formation process, S11 mixing process, S12 powder formation process, S13 solid solution formation process, S14 classification process

Claims

1. ZrO 2 and Yb 2 O 3 and a ceramic spray particle containing the Yb 2 O 3 The ceramic spray particles have a standard deviation of the content of 2 mass% or more and 7.0 mass% or less.

2. The Yb in mass% relative to the total mass of the ceramic spray particles 2 O 3 The ceramic spray particles according to claim 1, wherein the content of is 16 mass % or more.

3. Ceramic spray particles according to claim 1 or 2, having a cumulative particle size d10 of 40 μm or more.

4. The ceramic spray particles according to claim 3, wherein the cumulative particle size d10 is 45 μm or more.

5. A method for manufacturing a ceramic substrate, comprising: a metal bonding layer forming step of forming a metal bonding layer on a substrate; and a ceramic layer forming step of spraying ceramic spray particles onto the metal bonding layer to form a ceramic layer, wherein the ceramic spray particles are ZrO 2 and Yb 2 O 3 and the Yb in the ceramic spray particles is 2 O 3 The standard deviation of the content of is 2 mass % or more and 7.0 mass % or less.

6. The Yb in mass% relative to the total mass of the ceramic spray particles 2 O 3 The method for forming a thermal barrier coating layer according to claim 5 , wherein the content of is 16 mass % or more.

7. The method for forming a thermal barrier coating layer according to claim 5 or 6, wherein the cumulative particle size d10 of the ceramic spray particles is 40 μm or more.

8. The method for forming a thermal barrier coating layer according to claim 7, wherein the cumulative grain size d10 is 45 μm or more.