AI Technical Summary
Adhesives used in image sensor modules lack sufficient moisture resistance after thermal curing alone, as existing resin compositions do not effectively maintain adhesive strength in high humidity conditions without UV exposure.
A resin composition comprising a (meth)acrylate compound, polythiol compound, cyclic carbodiimide compound, curing catalyst, and epoxy coupling agent, with the cyclic carbodiimide content being 5% or more, which enhances moisture resistance through suppression of hydrolysis and recombination of polymer chains.
The resin composition achieves high moisture resistance and adhesive strength retention after thermal curing alone, even in high humidity environments, making it suitable for areas with limited UV exposure.
Abstract
Description
Resin composition and adhesive
[0001] The present invention relates to a resinous composition, an adhesive containing the same, a cured product thereof, and a semiconductor device and an electronic component each containing the cured product.
[0002] Adhesives that are temporarily fixed by ultraviolet (UV) irradiation and then fully cured by heat are used in many fields (e.g., Patent Documents 1 and 2), and are particularly popular for image sensor module applications. Image sensor modules are used as camera modules for mobile phones and smartphones. Adhesives used in the manufacture of image sensor modules are also used to prevent moisture from entering electronic components, and therefore are required to exhibit sufficient moisture resistance.
[0003] Patent Document 3 discloses a photo- and thermosetting resin composition that inhibits a decrease in adhesive strength of the cured resin composition in a moisture resistance test and has a sufficiently long pot life, the resin composition comprising (A) an acrylic resin, (B) a polyfunctional nitrogen-containing heterocyclic compound having a specific formula, (C) a latent curing agent, (D) a radical polymerization inhibitor, and (E) an anionic polymerization inhibitor.
[0004] Patent Document 1: JP 2009-51954 A, International Publication No. 2005 / 052021, International Publication No. 2016 / 143777
[0005] As image sensors become larger in the future, adhesives will be increasingly used in locations that are shaded by components and not exposed to ultraviolet light, such as the connection between a support and a substrate, and therefore improvements in the moisture resistance of adhesives after only thermal curing will be required in addition to the moisture resistance of adhesives after UV curing and heat curing. Patent Document 3 describes the suppression of a decrease in adhesive strength in a moisture resistance test of a resin composition after UV curing and heat curing, but does not mention moisture resistance after only thermal curing.
[0006] Therefore, an object of the present invention is to provide a resin composition and an adhesive that have high moisture resistance after thermal curing.
[0007] Specific means for solving the above problems are as follows. A first embodiment of the present invention is the following resin composition. (1) A resin composition comprising: (A) a (meth)acrylate compound; (B) a polythiol compound; (C) a cyclic carbodiimide compound; (D) a curing catalyst; and (E) a coupling agent. (2) The resin composition according to (1) above, in which the content of the (C) cyclic carbodiimide compound is 5 mass% or more relative to the total mass of the resin composition. (3) The resin composition according to (1) or (2) above, in which the (E) coupling agent comprises an epoxy-based coupling agent containing an epoxy group. (4) The resin composition according to any one of (1) to (3), further comprising: (F) a photoinitiator. (5) The resin composition according to any one of (1) to (4), further comprising: (G) an inorganic filler and at least one of (H) a stabilizer.
[0008] A second embodiment of the present invention is (6) an adhesive comprising the resin composition described in any one of (1) to (5) above. A third embodiment of the present invention is (7) a cured product obtained by curing the resin composition described in any one of (1) to (5) above or the adhesive described in (6) above. A fourth embodiment of the present invention is (8) a semiconductor device comprising the cured product described in (7) above. A fifth embodiment of the present invention is an electronic component comprising the semiconductor device described in (8) above.
[0009] According to a first embodiment of the present invention, a resin composition having high moisture resistance after thermal curing can be obtained. Also, according to a second embodiment of the present invention, an adhesive having high moisture resistance after thermal curing can be obtained. Furthermore, according to a third embodiment of the present invention, a cured product having high moisture resistance can be obtained. According to a fourth embodiment of the present invention, a semiconductor device including a cured product having high moisture resistance can be obtained. According to a fifth embodiment of the present invention, an electronic component including a semiconductor device having high moisture resistance can be obtained.
[0010] [Resin Composition] The resin composition according to the first embodiment of the present invention comprises: (A) a (meth)acrylate compound; (B) a polythiol compound; (C) a cyclic carbodiimide compound; (D) a curing catalyst; and (E) a coupling agent. According to this embodiment, a resin composition having high moisture resistance after thermal curing can be obtained.
[0011] (A) (Meth)acrylate Compound The resin composition of this embodiment contains (A) a (meth)acrylate compound (hereinafter also referred to as "component (A)"). The (A) (meth)acrylate compound can impart transparency and appropriate hardness to the cured resin composition. The (meth)acrylate compound as component (A) is not particularly limited as long as it has one or more (meth)acryloyl groups. In consideration of ensuring heat resistance, a compound having two or more (meth)acryloyl groups is preferred, a compound having 2 to 6 (meth)acryloyl groups is more preferred, and a compound having two (meth)acryloyl groups is even more preferred. Furthermore, in order to adjust the viscosity and physical properties of the cured product (such as adhesive strength and flexibility), a compound having one (meth)acryloyl group can also be used in addition to a compound having two (meth)acryloyl groups. From the viewpoint of moisture resistance, it is normally preferable that the component (A) has a structure that does not have a hydrolyzable partial structure such as an ester bond within the molecule. However, in this embodiment, by including the cyclic carbodiimide compound (C), hydrolysis of the ester bond or the like is suppressed and even if the molecular chain is broken by hydrolysis, rebonding is possible, and therefore the component (A) may have an ester bond or the like within the molecule.
[0012] Examples of the (meth)acrylate compound (A) include diacrylate and / or dimethacrylate of tris(2-hydroxyethyl)isocyanurate; tris(2-hydroxyethyl)isocyanurate triacrylate and / or trimethacrylate; trimethylolpropane triacrylate and / or trimethacrylate, or an oligomer thereof; pentaerythritol triacrylate and / or trimethacrylate, or an oligomer thereof; polyacrylate and / or polymethacrylate of dipentaerythritol; tris(acryloxyethyl)isocyanurate; caprolactone-modified tris(acryloxyethyl)isocyanurate; caprolactone-modified tris(methacryloxyethyl)isocyanurate; polyacrylate and / or polymethacrylate of alkyl-modified dipentaerythritol; caprolactone-modified tris(methacryloxyethyl)isocyanurate; Examples of suitable compounds include polyacrylates and / or polymethacrylates of lactone-modified dipentaerythritol, ethoxylated bisphenol A diacrylate and / or ethoxylated bisphenol A dimethacrylate, dihydrocyclopentadiethyl acrylate and / or dihydrocyclopentadiethyl methacrylate, polyester acrylates and / or polyester methacrylates, dimethylol-tricyclodecane diacrylate, poly(meth)acrylates of ditrimethylolpropane, polyurethanes having two or more (meth)acryloyl groups per molecule, polyesters having two or more (meth)acryloyl groups per molecule, phenoxyethyl acrylate, isobornyl acrylate, phenoxydiethylene glycol (meth)acrylate, and 4-tert-butylcyclohexyl acrylate. From the viewpoint of reactivity, it is preferable that component (A) be an acrylate compound and substantially free of methacrylate compounds. As the (meth)acrylate compound (A), any one of the above-mentioned (meth)acrylate compounds may be used alone, or two or more of them may be used in combination.
[0013] From the viewpoint of preparation and dispensability of the resin composition, it is preferable that component (A) has a viscosity of 0.01 to 80 Pa s. In this specification, viscosity refers to a value measured at a measurement temperature of 25°C using a viscometer appropriate for the viscosity range.
[0014] Commercially available products of the component (A) include, for example, polyester acrylate (product name: EBECRYL810) manufactured by Daicel Allnex Corporation, polyester acrylate (product name: M7100) manufactured by Toagosei Co., Ltd., and dimethylol-tricyclodecane diacrylate (product name: Light Acrylate DCP-A) manufactured by Kyoeisha Chemical Co., Ltd. Any one of these components may be used alone, or two or more of them may be used in combination.
[0015] From the viewpoint of adhesive strength of the resin composition, the content of the component (A) is preferably 10 to 70 mass % relative to the total mass of the resin composition, and more preferably 20 to 60 mass %.
[0016] (B) Polythiol Compound The resin composition of this embodiment contains a (B) polythiol compound (hereinafter also referred to as "component (B)"). The (B) polythiol compound imparts elasticity and moisture resistance to the resin composition. The component (B) is not particularly limited as long as it has two or more thiol groups. Originally, from the viewpoint of moisture resistance, it is preferable that the component (B) has a structure that does not have a hydrolyzable partial structure such as an ester bond within the molecule. However, in this embodiment, the component (B) may contain an ester bond within the molecule because the inclusion of a (C) cyclic carbodiimide compound suppresses hydrolysis of ester bonds and the like and allows rebonding even if molecular chains are broken by hydrolysis.
[0017] Examples of polythiol compounds having an ester bond in the molecule include pentaerythritol tetrakis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, trimethylolpropane tris(3-mercaptobutyrate), and trimethylolethane tris(3-mercaptobutyrate).
[0018] Commercially available products of component (B) having an ester bond in the molecule include trimethylolpropane tris(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: TMMP), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate (manufactured by SC Organic Chemical Co., Ltd.: TEMPIC), pentaerythritol tetrakis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: PEMP), and tetraethylene glycol bis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: PEMP). Examples of suitable mercaptobutyrates include dipentaerythritol hexakis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: EGMP-4), dipentaerythritol hexakis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: DPMP), pentaerythritol tetrakis(3-mercaptobutyrate) (manufactured by Showa Denko K.K.: Karenz MT (registered trademark) PE1), and 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by Showa Denko K.K.: Karenz MT (registered trademark) NR1).
[0019] In this embodiment, a polythiol compound (B) that does not have an ester bond in the molecule can also be used. Examples of such a polythiol compound (B) include glycoluril compounds represented by the following general formula (1):
[0020]
[0021] In general formula (1), R 1 , and R 2 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a phenyl group. n is an integer of 0 to 10.
[0022] Furthermore, the component (B) may be a compound represented by the following chemical formula (2) or (3).
[0023]
[0024]
[0025] The compounds represented by chemical formula (2) or chemical formula (3) are more preferred compounds as component (B).
[0026] Furthermore, the polythiol compound (B) that does not have an ester bond or the like in the molecule includes a polythiol compound represented by the general formula (4).
[0027]
[0028] In general formula (4), R 3 , R 4 , R 5 and R 6 are each independently hydrogen or C n H 2n SH (n is 2 to 6). 3 , R 4、 R 5 and R 6 At least one of n H 2nSH (n is 2 to 6). In terms of curability, n in the polythiol compound of component (B) represented by general formula (4) is preferably 2 to 4. Furthermore, in terms of the balance between the physical properties of the cured product and the curing rate, this polythiol compound is more preferably a mercaptopropyl group where n is 3. Component (B) represented by general formula (4) itself has a sufficiently flexible skeleton, so it is effective when it is desired to lower the modulus of elasticity of the cured product. By adding component (B) represented by general formula (4), the modulus of elasticity of the cured product can be controlled, thereby increasing the adhesive strength (particularly peel strength) after curing.
[0029] Commercially available products of component (B) that do not have an ester bond in the molecule include thiol glycoluril derivatives manufactured by Shikoku Chemical Industry Co., Ltd. (product name: TS-G (corresponding to chemical formula (2)), thiol equivalent: 100 g / eq), C3 TS-G (corresponding to chemical formula (3)), thiol equivalent: 114 g / eq)), and thiol compound manufactured by SC Organic Chemical Co., Ltd. (product name: PEPT (corresponding to general formula (4)), thiol equivalent: 124 g / eq)).
[0030] As the component (B), any one of them may be used alone, or two or more of them may be used in combination. A component (B) having an ester bond in the molecule and a component (B) not having an ester bond in the molecule may be used in combination.
[0031] When a polythiol compound having an ester bond in the molecule is used as component (B), the ester bond generates a carboxyl group and a hydroxyl group by hydrolysis. These functional groups react with the cyclic carbodiimide compound (C), and polar groups are formed in the resin composition, thereby improving the adhesive strength under high humidity. In one embodiment, the content of the polythiol compound having an ester bond in the molecule is preferably less than 60 parts by mass, more preferably less than 70 parts by mass, and even more preferably less than 80 parts by mass per 100 parts by mass of component (B).
[0032] In one embodiment, from the viewpoint of long-term humidity resistance reliability, it is preferable that component (B) does not have an ester bond. From the viewpoint of maintaining the shear strength under high humidity conditions for a long period of time after curing, it is preferable that the component (B) contains 70 to 100 parts by mass of a compound that does not have an ester bond per 100 parts by mass of component (B). The content of the polythiol compound that does not have an ester bond in component (B) is more preferably 80 to 100 parts by mass, and even more preferably 90 to 100 parts by mass, per 100 parts by mass of component (B).
[0033] In the resin composition, the ratio [thiol group equivalent number of component (B)] / [(meth)acryloyl group equivalent number of component (A)] is preferably 0.5 to 2.0, more preferably 0.5 to 1.5. In this specification, functional group equivalents such as (meth)acryloyl equivalent and thiol equivalent refer to the molecular weight of a compound per functional group, and functional group equivalent numbers such as (meth)acryloyl group equivalent number and thiol group equivalent number refer to the number of functional groups (equivalent number) per compound mass (charge amount). Theoretically, the thiol equivalent number of component (B) is the molecular weight of component (B) divided by the number of thiol groups in one molecule. The actual thiol equivalent number can be determined, for example, by determining the thiol value by potentiometric measurement. The (meth)acryloyl equivalent of the (A) (meth)acrylate compound is theoretically equal to the molecular weight of the (meth)acrylate compound divided by the number of acryloyl groups (or methacryloyl groups) in one molecule. The actual (meth)acryloyl equivalent can be measured, for example, by NMR. The (meth)acryloyl group equivalent of the (A) component is the number of (meth)acryloyl groups (equivalents) per mass (charged amount) of the (A) component, and is the quotient obtained by dividing the mass (g) of the (A) (meth)acrylate compound by the (meth)acryloyl equivalent of that (meth)acrylate compound (when multiple (meth)acrylate compounds are contained, the sum of such quotients for each (meth)acrylate compound). The thiol group equivalent number of component (B) is the number of thiol groups (equivalent number) per mass (charge amount) of component (B), and is the quotient obtained by dividing the mass (g) of the thiol compound (B) by the thiol equivalent number of that thiol compound (if multiple thiol compounds are contained, the sum of such quotients for each thiol compound). By setting the ratio [thiol group equivalent number of component (B)] / [(meth)acryloyl group equivalent number of component (A)] in the range of 0.5 to 2.0, a certain amount or more of acryloyl groups and thiol groups react, resulting in sufficient formation of molecular crosslinks and making it easier to demonstrate high adhesive strength.
[0034] The resin composition of this embodiment is a resin composition containing a (meth)acrylate compound (A) as a main prepolymer compound. The resin composition of this embodiment may contain other prepolymer compounds, such as an epoxy compound. However, this embodiment does not include embodiments in which the amount of the epoxy compound is greater than the amount of the (meth)acrylate compound (A). For example, embodiments in which the ratio [thiol group equivalents of component (B)] / [epoxy group equivalents of the epoxy compound] is 10.0 or less are not included. Conventionally, cured products of resin compositions rich in a (meth)acrylate compound as a main prepolymer compound have had more serious moisture resistance problems than resin compositions rich in epoxy compounds, especially when hydrolyzable ester bonds are formed in the polymer molecules. The resin composition of this embodiment can produce cured products with high moisture resistance under more stringent moisture resistance conditions, such as those rich in a (meth)acrylate compound. Theoretically, the epoxy equivalent of an epoxy compound is calculated by dividing the molecular weight of the epoxy compound by the number of epoxy groups in one molecule. The actual epoxy equivalent can be determined using the method described in JIS K7236. The epoxy group equivalent number of an epoxy compound is the number of epoxy groups (equivalent number) per mass (charged amount) of the epoxy compound, and is the quotient obtained by dividing the mass (g) of the epoxy compound by the epoxy equivalent of that epoxy compound (when multiple epoxy compounds are contained, the sum of such quotients for each epoxy compound).
[0035] (C) Cyclic Carbodiimide Compound The resin composition of this embodiment contains (C) a cyclic carbodiimide compound (hereinafter also referred to as "component (C)"). The cyclic carbodiimide compound has a cyclic structure. The cyclic structure has one carbodiimide group (-N=C=N-), and the first nitrogen and the second nitrogen are bonded by a bonding group. Each cyclic structure has only one carbodiimide group. The number of atoms in the cyclic structure is preferably 8 to 50, more preferably 10 to 30, and even more preferably 10 to 20. The cyclic carbodiimide compound may have multiple cyclic structures.
[0036] The cyclic carbodiimide compound used in this embodiment is preferably a cyclic carbodiimide compound represented by the following general formula (5).
[0037]
[0038] In general formula (5), Ar 1 ~Ar 4 are each independently an aromatic group. The aromatic group may be substituted with an alkyl group or an aryl group having 1 to 6 carbon atoms. Examples of the aromatic group include a phenylene group and a naphthalenediyl group.
[0039] Ar 1 ~Ar 4 is preferably a phenyl group, since this improves film-forming properties.
[0040] X is a divalent or tetravalent group. When X is divalent, q is 0, and when X is tetravalent, q is 1. X is preferably any one of the following formulae (5-i), (5-ii), (5-iii), (5-iv), (5-v), (5-vi), and (5-vii).
[0041]
[0042]
[0043]
[0044]
[0045] In formula (5-i), n is an integer of 1 to 6. Examples of the group (5-i) include a methylene group, an ethylene group, a 1,3-propylene group, a 1,4-butylene group, a 1,5-pentane group, and a 1,6-hexane group.
[0046] In the formulas (5-ii) to (5-v), m and n each independently represent an integer of 0 to 4. A methylene group where m=0 represents a single bond.
[0047] In addition, in formula (5-vi), R 1 and R 2are each independently an alkyl group or an aryl group having 1 to 6 carbon atoms. Examples of alkyl groups having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, a sec-propyl group, an iso-propyl group, an n-butyl group, a tert-butyl group, a sec-butyl group, an iso-butyl group, an n-pentyl group, a sec-pentyl group, an iso-pentyl group, an n-hexyl group, a sec-hexyl group, and an iso-hexyl group.
[0048] Among the cyclic carbodiimide compounds represented by formula (5), compounds represented by the following general formula (5-0) are preferred.
[0049]
[0050] In the general formula (5-0), X is preferably any one of the above-mentioned (5-i), (5-ii), (5-iii), (5-iv), (5-v), (5-vi), and (5-vii). Y and Z each independently represent a substituent other than an alkyl group having 1 to 6 carbon atoms or a phenyl group. As the substituent other than an alkyl group having 1 to 6 carbon atoms or a phenyl group, a conventionally known substituent can be used, and examples thereof include an alkyl group having 7 or more carbon atoms, an aryl group other than a phenyl group, an alkoxy group, a hydroxy group, an aldehyde group, an acyl group, a carboxyl group, an ester group, a nitro group, an amino group, a sulfo group, a sulfonyloxy group, a halogeno group, a silyl group, a vinyl group, a fluoroalkyl group, a cyano group, an isonitrile group, an amide group, an imide group, and a thiol group.
[0051] Among these, compounds represented by the following chemical formula (5-1) or (5-2) are preferred.
[0052]
[0053]
[0054] [Mechanism of Improvement of Moisture Resistance] The mechanism of improvement of moisture resistance by the (C) cyclic carbodiimide compound is not limited, but is presumed to be as follows. Hydrolyzable partial structures such as ester bonds are contained in some (A) (meth)acrylate compounds and some (B) polythiol compounds. For example, ester bonds are hydrolyzed to produce carboxylic acids and alcohols. As shown below, carbodiimide groups react with carboxylic acids produced by hydrolysis and capture the acid that catalyzes the decomposition reaction, thereby suppressing hydrolysis.
[0055]
[0056] However, in the case of (C) a polycarbodiimide compound that is not a cyclic carbodiimide compound, although the carbodiimide group reacts with a carboxylic acid to inhibit hydrolysis, when heat is subsequently applied, decomposition occurs and an isocyanate gas, which is known to be a highly irritating and sensitizing substance, is generated.
[0057]
[0058] On the other hand, in the case of (C) cyclic carbodiimide compounds, when the carbodiimide groups present in the cyclic skeleton react with carboxylic acid, the bond does not break even when heat is subsequently applied, and the resulting isocyanate remains in the polymer via the skeleton that constitutes the ring. The isocyanate groups form bonds with each other or with thiol groups. This allows polymer chains that are broken by hydrolysis to recombine with other polymer chains, thereby maintaining or strengthening adhesive strength. As a result, it is believed that the moisture resistance improving effect of (C) cyclic carbodiimide compounds is greater than that of polycarbodiimide compounds.
[0059]
[0060] Furthermore, the cyclic carbodiimide compound (C) does not generate isocyanate gas when heated, making it possible to produce a void-free cured film. If there are voids in the cured film, cracks tend to grow and moisture tends to pass through, which can lead to a decrease in reliability, so it is preferable that there are no voids in the cured film.
[0061] The content of the (C) cyclic carbodiimide compound is preferably 5% by mass or more, more preferably 8% by mass or more, and more preferably 10% by mass or more, based on the total mass of the resin composition. The upper limit of the content of the (C) cyclic carbodiimide compound is not particularly limited, but from the viewpoint of viscosity, it is, for example, 60% by mass or less, 50% by mass or less, or 40% by mass or less.
[0062] [Method for Producing Cyclic Carbodiimide Compound] In the present embodiment, the method for producing a cyclic carbodiimide compound is not particularly limited, and the compound can be produced by a conventionally known method (e.g., the methods described in WO 2010 / 071211 and JP 2011-256139 A). Examples of the method include a method for producing the compound from an amine via an isocyanate, a method for producing the compound from an amine via an isothiocyanate, a method for producing the compound from an amine via a triphenylphosphine, a method for producing the compound from an amine via a urea, a method for producing the compound from an amine via a thiourea, a method for producing the compound from a carboxylic acid via an isocyanate, and a method for producing the compound by derivatizing a lactam.
[0063] The cyclic carbodiimide compound may be a commercially available product.
[0064] (D) Curing Catalyst The resin composition of this embodiment contains a (D) curing catalyst (hereinafter also referred to as "component (D)"). The (D) curing catalyst used in this embodiment is not particularly limited as long as it is a curing catalyst for (meth)acrylate compounds, and known curing catalysts can be used, but it is preferably a latent curing catalyst. The latent curing catalyst of component (D) is a compound that is inactive at room temperature but is activated by heating to function as a curing catalyst. Examples of the latent curing catalyst include imidazole compounds that are solid at room temperature; solid-dispersed amine adduct latent curing catalysts such as reaction products of amine compounds and epoxy compounds (amine-epoxy adducts); and reaction products of amine compounds and isocyanate compounds or urea compounds (urea adducts).
[0065] Examples of imidazole compounds that are solid at room temperature include 2-heptadecylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-undecylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4-benzyl-5-hydroxymethylimidazole, 2,4-diamino-6-(2-methylimidazolyl-(1))-ethyl-S-triazine, and 2,4-diamino-6-(2'-methylimidazolyl-(1)')-ethyl-S-triazine. Examples of the methylimidazole include, but are not limited to, isocyanuric acid adducts, 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole-trimellitate, 1-cyanoethyl-2-phenylimidazole-trimellitate, N-(2-methylimidazolyl-1-ethyl)-urea, and N,N'-(2-methylimidazolyl-(1)-ethyl)-adiboyldiamide.
[0066] Examples of epoxy compounds used as one of the raw materials for producing a solid dispersion type amine adduct latent curing catalyst (amine-epoxy adduct) include polyglycidyl ethers obtained by reacting epichlorohydrin with polyhydric phenols such as bisphenol A, bisphenol F, catechol, and resorcinol, or polyhydric alcohols such as glycerin and polyethylene glycol; glycidyl ether esters obtained by reacting epichlorohydrin with hydroxycarboxylic acids such as p-hydroxybenzoic acid and β-hydroxynaphthoic acid; phthalic acid, terephthalic acid, and the like; Examples of epoxy compounds include, but are not limited to, polyglycidyl esters obtained by reacting a polycarboxylic acid such as carboxylic acid with epichlorohydrin; glycidylamine compounds obtained by reacting 4,4'-diaminodiphenylmethane or m-aminophenol with epichlorohydrin; and polyfunctional epoxy compounds such as epoxidized phenol novolac resin, epoxidized cresol novolac resin, and epoxidized polyolefin; and monofunctional epoxy compounds such as butyl glycidyl ether, phenyl glycidyl ether, and glycidyl methacrylate.
[0067] The amine compound used as another raw material for producing the solid dispersion-type amine adduct latent curing catalyst may be any compound as long as it has one or more active hydrogen atoms in the molecule capable of addition reacting with an epoxy group and at least one functional group selected from a primary amino group, a secondary amino group, and a tertiary amino group in the molecule. Examples of such amine compounds include, but are not limited to, aliphatic amines such as diethylenetriamine, triethylenetetramine, n-propylamine, 2-hydroxyethylaminopropylamine, cyclohexylamine, and 4,4'-diamino-dicyclohexylmethane; aromatic amine compounds such as 4,4'-diaminodiphenylmethane and 2-methylaniline; and nitrogen-containing heterocyclic compounds such as 2-ethyl-4-methylimidazole, 2-ethyl-4-methylimidazoline, 2,4-dimethylimidazoline, piperidine, and piperazine.
[0068] Among these, compounds having a tertiary amino group in the molecule are particularly useful as raw materials for providing latent curing catalysts with excellent curing acceleration capabilities. Examples of such compounds include amine compounds such as dimethylaminopropylamine, diethylaminopropylamine, di-n-propylaminopropylamine, dibutylaminopropylamine, dimethylaminoethylamine, diethylaminoethylamine, and N-methylpiperazine, as well as 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, and 2-phenylimidazole. primary or secondary amines having a tertiary amino group in the molecule, such as imidazole compounds such as imidazole; 2-dimethylaminoethanol, 1-methyl-2-dimethylaminoethanol, 1-phenoxymethyl-2-dimethylaminoethanol, 2-diethylaminoethanol, 1-butoxymethyl-2-dimethylaminoethanol, 1-(2-hydroxy-3-phenoxypropyl)-2-methylimidazole, 1-(2-hydroxy-3-phenoxypropyl)-2-ethyl-4 ... 1-(2-hydroxy-3-butoxypropyl)-2-methylimidazole, 1-(2-hydroxy-3-butoxypropyl)-2-ethyl-4-methylimidazole, 1-(2-hydroxy-3-phenoxypropyl)-2-phenylimidazoline, 1-(2-hydroxy-3-butoxypropyl)-2-methylimidazoline, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, N-β-hydroxyethylmorpholine, 2-dimethylaminoethanethiol, 2-mercaptopyridine, 2-benzimidazole Examples of the tertiary amino acid include, but are not limited to, alcohols, phenols, thiols, carboxylic acids, and hydrazides having a tertiary amino group in the molecule, such as thiazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 4-mercaptopyridine, N,N-dimethylaminobenzoic acid, N,N-dimethylglycine, nicotinic acid, isonicotinic acid, picolinic acid, N,N-dimethylglycine hydrazide, N,N-dimethylpropionic acid hydrazide, nicotinic acid hydrazide, and isonicotinic acid hydrazide.
[0069] Further, examples of the isocyanate compound used as another manufacturing raw material for the solid dispersion type amine adduct latent curing catalyst include monofunctional isocyanate compounds such as n-butyl isocyanate, isopropyl isocyanate, phenyl isocyanate, and benzyl isocyanate; polyfunctional isocyanate compounds such as hexamethylene diisocyanate, toluylene diisocyanate, 1,5-naphthalene diisocyanate, diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, xylylene diisocyanate, paraphenylene diisocyanate, 1,3,6-hexamethylene triisocyanate, and bicycloheptane triisocyanate; and terminal isocyanate group-containing compounds obtained by reacting these polyfunctional isocyanate compounds with active hydrogen compounds. Examples of such a terminal isocyanate group-containing compound include, but are not limited to, an addition compound having a terminal isocyanate group obtained by reacting toluylene diisocyanate with trimethylolpropane, and an addition compound having a terminal isocyanate group obtained by reacting toluylene diisocyanate with pentaerythritol.
[0070] Examples of urea compounds include, but are not limited to, urea and thiourea.
[0071] The solid-dispersed latent curing catalyst that can be used in this embodiment is, for example, the above-mentioned combination of two components: (a) an amine compound and an epoxy compound, (b) a combination of three components: these two components and an active hydrogen compound, or (c) a combination of two or three components: an amine compound and an isocyanate compound and / or a urea compound. These can be easily prepared by mixing the components, reacting them at a temperature from room temperature to 200°C, cooling them to solidify them, and then pulverizing them, or by reacting them in a solvent such as methyl ethyl ketone, dioxane, or tetrahydrofuran, removing the solvent, and then pulverizing the solid content.
[0072] Representative examples of commercially available solid dispersion-type latent curing catalysts include amine-epoxy adducts (amine adducts), such as "Amicure PN-23" (product name of Ajinomoto Fine-Techno Co., Ltd.), "Amicure PN-40" (product name of Ajinomoto Fine-Techno Co., Ltd.), "Amicure PN-50" (product name of Ajinomoto Fine-Techno Co., Ltd.), "Hardener X-3661S" (product name of ACS Corporation), "Hardener X-3670S" (product name of ACS Corporation), "Novacure HX-3742" (product name of Asahi Kasei E-materials Co., Ltd.), "Novacure HX-3721" (product name of Asahi Kasei E-materials Co., Ltd.), "Novacure HXA9322HP" (product name of Asahi Kasei E-materials Co., Ltd.), and "FXR1121" (product name of T&K Corporation). Examples of urea adducts include "Fujicure FXE-1000" (product name, T&K TOKA Corporation) and "Fujicure FXR-1030" (product name, T&K TOKA Corporation), but are not limited to these. Component (D) may be used alone or in combination of two or more types.
[0073] The content of the (D) curing catalyst is preferably 0.1 to 40 mass %, more preferably 1 to 20 mass %, relative to the total mass of the resin composition, from the viewpoints of the curing rate and pot life of the resin composition.
[0074] (E) Coupling Agent The resin composition of this embodiment contains (E) a coupling agent (hereinafter also referred to as "component (E)"). The coupling agent has two or more different functional groups in its molecule, one of which is a functional group that chemically bonds with an inorganic material, and the other is a functional group that chemically bonds with an organic material. By including the coupling agent in the resin composition, the adhesion of the resin composition to a substrate or the like is improved.
[0075] In this embodiment, it was found that the presence of (E) a coupling agent is also necessary to improve moisture resistance. The reason for this is thought to be, but is not limited to, the following: When water, heat, ions, vibration / load, etc. are applied to a metal material bond joint, the adhesive strength decreases. Water, in particular, is considered to be an extremely important degradation factor, and when water molecules penetrate and accumulate at the metal / adhesive interface, the effects of other degradation factors such as heat, ions, vibration / load are further accelerated, ultimately leading to failure of the bond joint. In this embodiment, it is thought that the (E) coupling agent inhibits water penetration into the bond interface, improving moisture resistance.
[0076] Examples of (E) coupling agents include, but are not limited to, silane coupling agents, aluminum coupling agents, and titanium coupling agents, depending on the type of functional group that chemically bonds with the inorganic material.
[0077] Examples of coupling agents include, but are not limited to, various coupling agents such as epoxy, amino, vinyl, methacrylic, acrylic, and mercapto coupling agents, depending on the type of functional group that chemically bonds with the organic material. Among these, epoxy coupling agents containing an epoxy group, methacrylic coupling agents containing a methacryloyl group, acrylic coupling agents containing an acryloyl group, and mercapto coupling agents containing a thiol group are preferred because they further improve moisture resistance. In particular, epoxy coupling agents containing an epoxy group are more preferred from the viewpoint of achieving both moisture resistance after thermal curing and UV+thermal curing.
[0078] Specific examples of epoxy-based silane coupling agents include 3-glycidoxypropyltrimethoxysilane (product name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.), 3-glycidoxypropyltriethoxysilane (product name: KBE-403, manufactured by Shin-Etsu Chemical Co., Ltd.), 3-glycidoxypropylmethyldiethoxysilane (product name: KBE-402, manufactured by Shin-Etsu Chemical Co., Ltd.), 3-glycidoxypropylmethyldimethoxysilane (product name: KBM402, manufactured by Shin-Etsu Chemical Co., Ltd.), 8-glycidoxyoctyltrimethoxysilane (product name: KBM-4803, manufactured by Shin-Etsu Chemical Co., Ltd.), and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (product name: Sila-Ace S530, manufactured by JNC Corporation).
[0079] Specific examples of methacrylic silane coupling agents include 3-methacryloxypropyltrimethoxysilane (product name: KBM503, manufactured by Shin-Etsu Chemical Co., Ltd.), 3-methacryloxypropylmethyldimethoxysilane (product name: KBM502, manufactured by Shin-Etsu Chemical Co., Ltd.), 3-methacryloxypropylmethyldiethoxysilane (product name: KBE502, manufactured by Shin-Etsu Chemical Co., Ltd.), and 3-methacryloxypropyltriethoxysilane (product name: KBE503, manufactured by Shin-Etsu Chemical Co., Ltd.).
[0080] A specific example of the acrylic silane coupling agent is 3-acryloxypropyltrimethoxysilane (product name: KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.).
[0081] Specific examples of mercapto-based silane coupling agents include 3-mercaptopropyltrimethoxysilane (product name: KBM803, manufactured by Shin-Etsu Chemical Co., Ltd.) and 3-mercaptopropylmethyldimethoxysilane (product name: KBM802, manufactured by Shin-Etsu Chemical Co., Ltd.).
[0082] The coupling agents may be used alone or in combination of two or more.
[0083] The content of component (E) is preferably 0.1 to 10 mass %, more preferably 0.2 to 7 mass %, and even more preferably 0.3 to 5 mass %, based on the total mass of the resin composition.
[0084] (F) Photoinitiator The resin composition of this embodiment may contain (F) a photoinitiator (hereinafter also referred to as "component (F)") within a range that does not impair the effects of the present invention. In this embodiment, a photoinitiator that generates radicals by UV absorption is preferred.
[0085] Examples of the photoinitiator include alkylphenone-based photoinitiators and acylphosphine oxide-based photoinitiators. Specific examples include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one. The resin composition of this embodiment is photo- and heat-curable, but UV curing can be promoted by using a photoinitiator.
[0086] From the viewpoint of UV curability, the content of the component (F) is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 8 parts by mass, per 100 parts by mass of the (meth)acrylate compound.
[0087] (G) Inorganic Filler The resin composition of this embodiment may contain (G) inorganic filler (hereinafter also referred to as "component (G)") to the extent that the effects of the present invention are not impaired. The inorganic filler is composed of granules formed from an inorganic material. Examples of inorganic materials that can be used include silica, alumina, aluminum nitride, calcium carbonate, aluminum silicate, magnesium silicate, magnesium carbonate, barium sulfate, barium carbonate, lime sulfate, aluminum hydroxide, calcium silicate, potassium titanate, titanium oxide, zinc oxide, silicon carbide, silicon nitride, and boron nitride. Any one of the inorganic fillers may be used alone, or two or more may be used in combination. As the inorganic filler, it is preferable to use a silica filler. As the silica, amorphous silica is preferable.
[0088] The shape of the inorganic filler is not particularly limited, and examples thereof include spherical, flaky, needle-like, irregular, etc. From the viewpoint of flowability, spherical shapes are preferred.
[0089] The average particle size of the inorganic filler is preferably 0.01 to 15 μm, more preferably 0.01 to 10 μm, and the maximum particle size of the inorganic filler is preferably 50 μm or less, more preferably 30 μm or less.
[0090] In this specification, the average particle size is the particle size at an integrated value of 50% in the particle size distribution on a volume basis measured by a laser diffraction / scattering method, and the maximum particle size is the maximum particle size in the particle size distribution on a volume basis measured by a laser diffraction / scattering method.
[0091] The content of the (G) inorganic filler is preferably 0.5 to 80 mass %, more preferably 1 to 70 mass %, based on the total mass of the resin composition.
[0092] (H) Stabilizer The resin composition of this embodiment may contain a (H) stabilizer (hereinafter also referred to as "component (H)") to the extent that the effects of the present invention are not impaired. The (H) stabilizer is added to increase the stability of the resin composition during storage and to suppress the occurrence of polymerization reactions due to unintended radicals or basic components.
[0093] Known (H) stabilizers can be used, such as borate ester compounds, strong acids, and radical scavengers. Specific examples of (H) stabilizers include trimethyl borate, triethyl borate, tri-n-propyl borate, triisopropyl borate, trifluoromethanesulfonic acid, maleic acid, methanesulfonic acid, difluoroacetic acid, trichloroacetic acid, phosphoric acid, dichloroacetic acid, N-nitroso-N-phenylhydroxylamine aluminum, triphenylphosphine, 4-methoxyphenol, and hydroquinone. Among these, preferred (H) stabilizers are at least one selected from maleic acid, methanesulfonic acid, N-nitroso-N-phenylhydroxylamine aluminum, and 4-methoxyphenol. Furthermore, known (H) stabilizers disclosed in JP 2010-117545 A, JP 2008-184514 A, JP 2017-171804 A, and the like can also be used. The stabilizer (H) may be used alone or in combination of two or more.
[0094] The content of component (H) is preferably 0.1 to 5 mass %, more preferably 0.3 to 3 mass %, based on the total mass of the resin composition.
[0095] In a preferred embodiment, the resin composition includes at least one of (G) an inorganic filler and (H) a stabilizer.
[0096] The resin composition may further contain, as necessary, a solvent, carbon black, titanium black, an ion trapping agent, a leveling agent, an antioxidant, an antifoaming agent, a thixotropic agent, a viscosity modifier, a flame retardant, and / or other additives, within a range that does not impair the object of this embodiment.
[0097] The resin composition can be obtained, for example, by stirring, melting, mixing, and / or dispersing components (A) to (E), and optionally components (F), (G), and / or (H), and optionally other additives, simultaneously or separately, while optionally applying heat treatment. The apparatus used for mixing, stirring, dispersing, etc. is not particularly limited. Examples of apparatus that can be used include a Raikai mixer, Henschel mixer, three-roll mill, ball mill, planetary mixer, and bead mill equipped with a stirring and heating device. These apparatuses may also be used in appropriate combinations.
[0098] The resin composition thus obtained has photocurability and thermosetting properties, and can be sufficiently cured by heat alone. When the resin composition is used in an image sensor module, the heat curing temperature of the resin composition is preferably 70 to 90°C.
[0099] The resin composition of the present embodiment can be used, for example, as an adhesive for joining parts together, or as a raw material thereof.
[0100] [Adhesive] The adhesive according to the second embodiment of the present invention includes the resin composition according to the first embodiment, and enables good bonding to engineering plastics, ceramics, and metals.
[0101] [Cured Product of Resin Composition or Adhesive] The cured product of the third embodiment of the present invention is a cured product obtained by curing the resin composition of the first embodiment or the adhesive of the second embodiment described above.
[0102] [Semiconductor device, electronic component] A semiconductor device according to a fourth embodiment of the present invention has high moisture resistance because it includes the cured product according to the third embodiment. An electronic component according to a fifth embodiment of the present invention has high moisture resistance because it includes the semiconductor device according to the fourth embodiment.
[0103] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. In the following examples, parts and % represent parts by mass and % by mass unless otherwise specified.
[0104] [Examples 1 to 9, Comparative Examples 1 to 4] Resin compositions were prepared by mixing predetermined amounts of each component using a three-roll mill according to the formulations shown in Table 1. In Table 1, the amount of each component is expressed in parts by mass (unit: g). The components used in the examples and comparative examples are as follows.
[0105] (A) (meth)acrylate compound (component (A)) (A1): dimethylol-tricyclodecane diacrylate (product name: Light Acrylate DCP-A, manufactured by Kyoeisha Chemical Co., Ltd., acryloyl equivalent: 188 g / eq) (A2): polyester acrylate (product name: M7100, manufactured by Toagosei Co., Ltd., acryloyl equivalent: 152 g / eq) (B) polythiol compound (component (B)) (B1): pentaerythritol tetrakis(3-mercaptopropionate) represented by the following formula (product name: PEMP, manufactured by SC Organic Chemicals, thiol equivalent: 122 g / eq) (B2): Glycoluril derivative represented by formula (3) (product name: C3 TS-G, manufactured by Shikoku Chemicals Corporation, thiol equivalent: 114 g / eq) (B3): 1,3,4,6-tetrakis(2-mercaptoethyl)glycoluril represented by formula (2) (product name: TS-G, manufactured by Shikoku Chemicals Corporation, thiol equivalent: 100 g / eq) (C) Cyclic carbodiimide compound (component (C)) Cyclic carbodiimide compound of formula (5-1) (carbodiimide equivalent: 256 g / eq) (C') Polycarbodiimide compound (product name: Carbodilite V-02B, manufactured by Nisshinbo Chemical Inc., carbodiimide equivalent: 600 g / eq) (D) Curing catalyst (component (D)) (D1): Amine-epoxy adduct latent curing catalyst (product name: Novacure HXA9322HP, manufactured by Asahi Kasei E-materials Corporation) (D2): Amine-epoxy adduct latent curing catalyst (product name: Fujicure FXR1121, manufactured by T&K TOKA Corporation) (E) Coupling agent (component (E)) (E1): 3-glycidoxypropyltrimethoxysilane (product name: KBM-403, Shin-Etsu Chemical Co., Ltd.) (E2): 8-glycidoxyoctyltrimethoxysilane (product name: KBM-4803, Shin-Etsu Chemical Co., Ltd.) (E3): 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (product name: Sila-Ace S530, JNC Corporation) (F) Photoinitiator (component (F)): 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (product name: Omnirad 907, IGM Resins BV) (G) Inorganic filler (component (G)): Silica (product name: SO-E2, Admatechs Co., Ltd.) (H) Stabilizer (component (H)): Triisopropyl borate (product name: TIPB, Tokyo Chemical Industry Co., Ltd.)
[0106] In the examples and comparative examples, the properties of the cured products obtained by curing the resin compositions were measured as follows.
[0107] [Adhesion strength] A resin composition was stencil-printed on a glass plate with a size of φ2 mm and a thickness of 125 μm, and an alumina chip of 3.2 mm × 1.6 mm × 0.45 mm was mounted on the printed resin composition, and the composition was cured under load to prepare test pieces (n = 10). The curing conditions at this time were: in the case of "heat only", 80 ° C / 60 minutes in a blower dryer; in the case of "UV + heat", UV irradiation dose of 2000 mJ / cm from the opposite side (back side) of the alumina chip mounting surface (front side). 2(UV wavelength: 365 nm, LED lamp), and then 80 ° C / 60 minutes in a fan dryer. The alumina chips on this glass plate were poked from the side with a Model-1605HTP strength tester manufactured by Aiko Engineering Co., Ltd., and the shear strength was calculated from the value when the alumina chips peeled off. Next, for Examples 1 to 9 and Comparative Examples 1 to 4, the test pieces after the curing treatment were subjected to a pressure cooker test (hereinafter referred to as PCT) (2 atm, 121 ° C, 100% RH, 20 hours), and the shear strength was calculated in the same manner. Table 1 shows the results (units: N). The PCT test is a reliability test in which the cured resin composition is maintained at 121 ° C, 2 atmospheres, and 100% relative humidity. For each of the heat curing conditions and UV+heat curing conditions, the adhesive strength retention (%) after a pressure cooker test (hereinafter referred to as PCT) relative to the initial adhesive strength was calculated. In the present invention, the adhesive strength retention is preferably 50% or more, more preferably 60% or more. The results are shown in Table 1.
[0108]
[0109] Component (A), (A1) and (A2), are both (meth)acrylate compounds containing an ester bond. Component (B), (B1), is a polythiol compound containing an ester bond, while (B2) and (B3) are polythiol compounds without an ester bond. Examples 1 to 9 and Comparative Examples 1 to 4 all contain (A1), (A2), and (B1), and were investigated under conditions where hydrolysis is likely to occur. It should be noted that the scope of the present invention is not necessarily limited to embodiments in which components (A) and (B) contain an ester bond. Comparison of Examples 1 to 4 and Comparative Example 1 reveals that adding 5% by mass or more of the (C) cyclic carbodiimide compound to the resin composition increased the adhesive strength retention rate after PCT and improved moisture resistance under both heat curing and UV+heat curing conditions. A comparison of Examples 5, 6, and Comparative Example 2 shows that even when two or more types of component (B) were used in combination, the addition of a (C) cyclic carbodiimide compound to the resin composition increased the adhesive strength retention rate after PCT under both heat curing conditions and UV + heat curing conditions, and improved moisture resistance. A comparison of Examples 2 and 7 shows that, regardless of the type of (D) curing catalyst, the addition of a (C) cyclic carbodiimide compound to the resin composition increased the adhesive strength retention rate after PCT under both heat curing conditions and UV + heat curing conditions, and improved moisture resistance. A comparison of Example 2 and Comparative Examples 1 and 3 shows that the (C) cyclic carbodiimide compound improved moisture resistance more than the polycarbodiimide compound under heat curing conditions. Furthermore, under UV + heat curing conditions, the (C) cyclic carbodiimide compound was able to improve moisture resistance, whereas the polycarbodiimide compound was unable to improve moisture resistance. A comparison of Examples 2, 8, and 9 with Comparative Example 4 reveals that the presence of the coupling agent (E) is also necessary to improve moisture resistance.
[0110] The present invention is a photo- and thermosetting resin composition that has high moisture resistance not only after UV and thermosetting, but also after thermosetting alone, and is particularly useful as an adhesive to be applied to locations where UV curing is difficult.
[0111] The disclosures of Japanese Patent Application No. 2021-106245 (filing date: June 28, 2021) and Japanese Patent Application No. 2021-133624 (filing date: August 18, 2021) are incorporated herein by reference in their entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. (A) a (meth)acrylate compound, (B) a polythiol compound, (C) a cyclic carbodiimide compound, (D) a curing catalyst, and (E) Coupling Agent A resin composition comprising:
2. The resin composition according to claim 1, wherein the content of the cyclic carbodiimide compound (C) is 5 mass% or more based on the total mass of the resin composition.
3. The resin composition according to claim 1 , wherein the coupling agent (E) comprises an epoxy-based coupling agent containing an epoxy group.
4. The resin composition according to claim 1 , further comprising (F) a photoinitiator.
5. The resin composition according to claim 1 , further comprising at least one of (G) an inorganic filler and (H) a stabilizer.
6. The resin composition described in claim 4, further comprising at least one of (G) an inorganic filler and (H) a stabilizer.
7. An adhesive comprising the resin composition according to any one of claims 1 to 6.
8. A cured product obtained by curing the resin composition according to any one of claims 1 to 6.
9. A semiconductor device comprising the cured product according to claim 8.
10. An electronic component comprising the semiconductor device according to claim 9.