Seamless steel pipe and method for manufacturing seamless steel pipe

JPWO2024075433A5Active Publication Date: 2024-10-03NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023577095
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-29
Filing Date
2023-08-29
Publication Date
2024-10-03
Estimated Expiration
2043-08-29

AI Technical Summary

Technical Problem

The challenge in deep-sea oil and gas field development is ensuring the fatigue characteristics of circumferential welds in line pipes due to inner diameter differences between steel pipe ends, which can lead to fatigue cracks from repeated stress, especially in risers connected to floating platforms, as current manufacturing methods do not adequately control strength uniformity across the wall thickness.

Method used

A seamless steel pipe with a specific chemical composition and controlled heat treatment process, including quenching and tempering, to uniformly dissolve vanadium-containing particles throughout the wall thickness, ensuring a uniform structure and minimal strength difference between full wall thickness and post-cutting strength.

Benefits of technology

The solution results in a seamless steel pipe with a small strength variation across the thickness, enhancing the fatigue resistance and weld integrity, suitable for deep-sea applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a seamless steel pipe having a small difference between the strength at the entire wall thickness and the strength after cutting. The seamless steel pipe has a predetermined chemical composition, Fn1 represented by the following formula (1) is 0.44 or more, and the grain size number according to ASTM E112-13 (2021) at the center of the wall thickness is 6.0 or more, and in a cross section perpendicular to the tube axial direction, the number density of V-containing particles having a circle equivalent diameter of 10 to 100 nm at a position 2 mm deep from the outer surface of the steel pipe is NDos, the number density of V-containing particles having a circle equivalent diameter of 10 to 100 nm at a position 2 mm deep from the inner surface of the steel pipe is NDis, and the number density of V-containing particles having a circle equivalent diameter of 10 to 100 nm at the center of the wall thickness is NDos / NDc and NDis / NDc are each 0.60 or more. Fn1=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15 (1) The content of each element in formula (1) is substituted for the corresponding element symbol in mass%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a seamless steel pipe and a method for manufacturing a seamless steel pipe. [Background technology]

[0002] In recent years, onshore and shallow-sea oil and gas wells have been depleted, and development of deep-sea oil and gas wells (hereinafter referred to as "deep-sea fields") has become active. For fluid transportation in deep-sea fields, thick-walled line pipes are used to ensure strength against high external pressure and to compensate for the loss of strength caused by high-temperature production fluids.

[0003] WO 2013 / 161567 describes a seamless steel pipe that has high strength and toughness even when it is thick. This seamless steel pipe contains, by mass%, 0.03 to 0.08% C, has a wall thickness of 50 mm or more, has an average grain size of prior austenite grains in the surface layer of less than 80 μm, and has a difference of less than 50 μm between the average grain size of prior austenite grains in the surface layer and the average grain size of prior austenite grains in the center of the wall thickness.

[0004] WO 2015 / 019708 describes a seamless steel pipe for line pipes that has high strength and high toughness with low surface hardness. This seamless steel pipe for line pipes contains, by mass%, C: 0.03-0.10%, Ni: 0.04-2.0%, etc., and in the scale formed on the surface of the steel pipe, metal particles mainly composed of Ni or Cu with an average equivalent circle diameter of 0.1-5 μm are present, and the distance from the boundary between the base material of the steel pipe and the scale to the area where no metal particles are present is 20 μm or more.

[0005] International Publication No. 2017 / 141341 describes a seamless steel pipe that can stably obtain a yield strength of 555 MPa or more and excellent SSC resistance. This seamless steel pipe contains, by mass%, C: 0.02 to 0.15%, etc., a carbon equivalent Ceq of 0.430% or more and less than 0.500%, the size of prior austenite grains in the structure is less than 6.0 in terms of grain size number according to ASTM E112-10, and the Vickers hardness is 250 Hv or less between a position 1 mm from the inner surface and a position 1 mm from the outer surface.

[0006] WO 2017 / 018108 describes a steel pipe for line pipe use with reduced hardness in the surface layer. This steel pipe for line pipe use contains, by mass%, C: 0.02 to 0.11%, etc., and has a structure containing tempered martensite and / or tempered bainite, and further contains ferrite at least one of between the outer surface of the steel pipe and a position 1 mm from the outer surface, and between the inner surface of the steel pipe and a position 1 mm from the inner surface.

[0007] International Publication No. 2018 / 020972 describes a high-strength seamless steel pipe that can stably achieve both high strength and low hardness while ensuring weldability. This high-strength seamless steel pipe contains, by mass%, C: 0.10-0.18%, B: 0.0005-0.005%, etc., and satisfies C+Si / 30+(Mn+Cu+Cr) / 20+Ni / 60+Mo / 15+V / 10+5×B≦0.28. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2013 / 161567 [Patent Document 2] International Publication No. 2015 / 019708 [Patent Document 3] International Publication No. 2017 / 141341 [Patent Document 4] International Publication No. 2017 / 018108 [Patent Document 5] International Publication No. 2018 / 020972 Summary of the Invention [Problem to be solved by the invention]

[0009] As deep-sea field development becomes more active, the use of floating platforms (floating-type platforms) is increasing. Figure 1 is a schematic diagram showing deep-sea field development using a floating-type platform. A line pipe 10 includes a flow line 11 laid along the topography of the seabed surface, and a riser 12 arranged rising from the seabed surface toward the offshore platform PF. In development using a floating-type platform, the line pipe 10 is constantly swaying due to tides and waves. Therefore, it is important to ensure the fatigue properties of the girth weld, especially in the riser 12.

[0010] Line pipes are used by butting the ends of steel pipes together and circumferentially welding the butted parts. Figure 2 is a cross-sectional view that shows a schematic state in which the ends of steel pipes P1 and P2 are butted together. As shown in Figure 2, if there is an inside diameter difference Δ between the ends of steel pipes P1 and P2, fatigue cracks are likely to occur due to repeated stress after circumferential welding. In order to ensure the fatigue properties of the circumferential weld, it is necessary to keep the inside diameter difference Δ small, that is, to keep the inside diameter of the pipe ends within a narrow tolerance when manufacturing the steel pipes.

[0011] As a means of reducing the inner diameter difference Δ, pipe ends may be refined by cutting the inner surface of the pipe end using an NC lathe (inner cutting or boring of the pipe end). In some cases, the outer surface of the pipe end may also be cut at the same time. After cutting, the steel pipe has had its inner surface layer (and in some cases both the inner surface and the outer surface layers) removed. If there is a difference between the strength at full thickness (as manufactured) and the strength after cutting, this is undesirable as it will cause instability in the pipeline design. Meanwhile, the shipping test required by the current mainstream standards is based on full thickness steel pipes, and no evaluation is performed focusing on the strength after cutting.

[0012] An object of the present invention is to provide a seamless steel pipe in which the difference between the strength at the entire wall thickness and the strength in the state after cutting is small, and a method for producing the same. [Means for solving the problem]

[0013] A seamless steel pipe according to an embodiment of the present invention comprises, in mass%, C: 0.030 to 0.100%, Si: 0.05 to 0.50%, Mn: 0.30 to 1.70%, P: 0.020% or less, S: 0.0050% or less, Al: 0.001 to 0.100%, N: 0.0200% or less, Cr: 0.05 to 0.30%, Mo: 0.05 to 0.23%, Cu: The steel has a chemical composition of 0.10-0.50%, Ni: 0.20-0.50%, V: 0.01-0.10%, Nb: 0-0.020%, Ti: 0-0.020%, B: 0-0.0005%, Ca: 0-0.0060%, and the balance: Fe and impurities, and has an Fn1 value of 0.44 or more as represented by the following formula (1), and an ASTM The grain size number according to E112-13(2021) is 6.0 or more, and quantitative analysis is performed using energy dispersive X-ray analysis with V, Nb, Ti, Mo and Al as target elements. Particles with a V content of 30 mass% or more are defined as V-containing particles. In a cross section perpendicular to the tube axial direction, the number density of V-containing particles having a circular equivalent diameter of 10 to 100 nm at a position 2 mm deep from the outer surface of the steel tube is defined as NDos, the number density of V-containing particles having a circular equivalent diameter of 10 to 100 nm at a position 2 mm deep from the inner surface of the steel tube is defined as NDis, and the number density of V-containing particles having a circular equivalent diameter of 10 to 100 nm at the center of the wall thickness is defined as NDos / NDc and NDis / NDc are each 0.60 or more. Fn1=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15 (1) The content of each element in formula (1) is substituted for the corresponding element symbol in mass%.

[0014] A manufacturing method of a seamless steel pipe according to one embodiment of the present invention is a method of manufacturing the above-mentioned seamless steel pipe, and comprises the steps of preparing a mother pipe having the above-mentioned chemical composition, quenching the mother pipe, and tempering the quenched mother pipe, wherein the quenching step includes the steps of heating the mother pipe to a temperature of 600°C or higher at an average heating rate of 5°C / min or less in a temperature range from 400°C to 600°C, heating the mother pipe to the holding temperature at an average heating rate of 10°C / min or more in a temperature range from 600°C to a holding temperature which is a temperature equal to or higher than the Ac3 point, holding the mother pipe at the holding temperature for a period of 10 minutes to 60 minutes, and cooling the mother pipe held at the holding temperature. Effect of the Invention

[0015] According to the present invention, a seamless steel pipe can be obtained in which the difference between the strength at the entire wall thickness and the strength after cutting is small. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic diagram showing deep-sea field development using a floating-type platform. [Diagram 2] FIG. 2 is a cross-sectional view that shows a schematic state in which the ends of two steel pipes are butted together. [Diagram 3] FIG. 3 is a diagram showing a schematic diagram of the position where the arc-shaped test piece was taken. [Figure 4] FIG. 4 is a diagram showing the positions at which round bar test pieces were taken. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Seamless steel pipes are manufactured by applying heat treatments of quenching and tempering after pipe making. In thick-walled steel pipes (for example, steel pipes with a wall thickness of 40.0 mm or more), it is difficult to perform uniform quenching in the wall thickness direction, and the structure in the center of the wall thickness tends to become coarse-grained. According to the Hall-Petch law, the yield strength decreases in a coarse-grained structure, so the strength in the center of the wall thickness tends to be lower than that near the inner and outer surfaces. As a result, there may be a difference between the strength at the entire wall thickness and the strength after cutting.

[0018] Vanadium is an element that contributes greatly to improving hardenability by dissolving in austenite. On the other hand, if vanadium remains in the steel in the form of particles such as carbide (VC) (hereinafter referred to as "V-containing particles"), the effect of improving hardenability is not achieved. Therefore, in order to make the structure of a steel pipe uniform in the wall thickness direction, it is effective to dissolve the V-containing particles uniformly throughout the wall thickness direction and to make the distribution of the V-containing particles uniform in the wall thickness direction. Specifically, it is effective to make the ratio of the number density of the V-containing particles near the inner and outer surfaces to the number density of the V-containing particles in the center of the wall thickness 0.60 or more.

[0019] In order to dissolve the V-containing particles uniformly throughout the thickness direction, it is effective to limit the average heating rate in the temperature range from 400°C to 600°C during quenching heating to 5°C / min or less. This allows sufficient preheating up to the center of the wall thickness of the steel pipe, and promotes uniform dissolution of the V-containing particles during the subsequent heating.

[0020] As a method for dissolving the V-containing particles uniformly throughout the thickness direction, it is possible to hold the material at high temperatures for a long time. However, in this case, the austenite grains become coarse, making it difficult to achieve the required strength. As described above, if the heating rate in the temperature range from 400°C to 600°C is limited, the distribution of the V-containing particles in the thickness direction can be made uniform while suppressing the coarsening of the austenite grains.

[0021] The present invention has been completed based on the above findings. A seamless steel pipe and a manufacturing method thereof according to one embodiment of the present invention will now be described.

[0022] [Seamless steel pipe] [Chemical composition] The seamless steel pipe according to this embodiment has the chemical composition described below. In the following description, "%" for the content of an element means mass %.

[0023] C: 0.030~0.100% Carbon (C) improves the hardenability of steel. On the other hand, if the C content is too high, the weldability of the steel decreases. Therefore, the C content is 0.030 to 0.100%. The lower limit of the C content is preferably 0.040%, more preferably 0.045%, and more preferably 0.050%. The upper limit of the C content is preferably 0.098%, more preferably 0.095%, more preferably 0.090%, and more preferably 0.085%.

[0024] Silicon: 0.05 to 0.50% Silicon (Si) deoxidizes steel. On the other hand, if the Si content is too high, the toughness of the steel decreases. Therefore, the Si content is 0.05 to 0.50%. The lower limit of the Si content is preferably 0.08%, and more preferably 0.10%. The upper limit of the Si content is preferably 0.40%, and more preferably 0.35%.

[0025] Mn: 0.30-1.70% Manganese (Mn) improves the hardenability of steel. On the other hand, if the Mn content is too high, the toughness of the steel decreases. Therefore, the Mn content is 0.30 to 1.70%. The lower limit of the Mn content is preferably 0.50%, more preferably 0.70%, more preferably 0.90%, more preferably 1.00%, and more preferably 1.10%. The upper limit of the Mn content is preferably 1.65%, and more preferably 1.60%.

[0026] P:0.020% or less Phosphorus (P) is an impurity. P reduces the toughness of steel. Therefore, the P content is 0.020% or less. It is preferable that the P content is as low as possible. The P content is preferably 0.018% or less, and more preferably 0.015% or less.

[0027] S: 0.0050% or less Sulfur (S) is an impurity. S reduces the toughness of steel. Therefore, the S content is 0.0050% or less. It is preferable that the S content is as low as possible. The S content is preferably 0.0040% or less, more preferably 0.0030% or less, and even more preferably 0.0020% or less.

[0028] Al: 0.001 to 0.100% Aluminum (Al) deoxidizes steel. Al also forms fine precipitates, contributing to improving the toughness of steel. On the other hand, if the Al content is too high, the precipitates become coarse and the toughness of steel decreases. Therefore, the Al content is 0.001 to 0.100%. The lower limit of the Al content is preferably 0.005%, more preferably 0.010%, and even more preferably 0.015%. The upper limit of the Al content is preferably 0.080%, and even more preferably 0.060%. In this specification, Al means acid-soluble aluminum (sol.Al).

[0029] N: 0.0200% or less Nitrogen (N) is an impurity. If the N content is too high, the toughness of the steel decreases. Therefore, the N content is 0.0200% or less. The upper limit of the N content is preferably 0.0100%, more preferably 0.0080%, and more preferably 0.0060%. On the other hand, excessive restriction of the N content increases the cost. The lower limit of the N content is preferably 0.0005%, more preferably 0.0010%, and more preferably 0.0020%.

[0030] Cr: 0.05~0.30% Chromium (Cr) improves the hardenability and temper softening resistance of steel. On the other hand, if the Cr content is too high, the toughness and weldability of the steel decrease. Therefore, the Cr content is 0.05 to 0.30%. The lower limit of the Cr content is preferably 0.08%, more preferably 0.10%, and further preferably 0.15%. The upper limit of the Cr content is preferably 0.28%, and further preferably 0.25%.

[0031] Mo: 0.05 to 0.23% Molybdenum (Mo) improves the hardenability of steel. On the other hand, if the Mo content is too high, the weldability and toughness of the steel decrease. Therefore, the Mo content is 0.05 to 0.23%. The lower limit of the Mo content is preferably 0.08%, more preferably 0.10%, and further preferably 0.12%. The upper limit of the Mo content is preferably 0.22%, more preferably 0.20%, and further preferably 0.18%.

[0032] Cu: 0.10-0.50% Copper (Cu) improves the hardenability of steel. On the other hand, if the Cu content is too high, the weldability and hot workability of the steel are reduced. Therefore, the Cu content is 0.10 to 0.50%. The lower limit of the Cu content is preferably 0.15%, and more preferably 0.20%. The upper limit of the Cu content is preferably 0.45%, and more preferably 0.40%.

[0033] Ni: 0.20~0.50% Nickel (Ni) improves the hardenability and toughness of steel. On the other hand, if the Ni content is too high, the sulfide stress corrosion cracking resistance of the steel decreases. Therefore, the Ni content is 0.20 to 0.50%. The lower limit of the Ni content is preferably 0.22%, and more preferably 0.25%. The upper limit of the Ni content is preferably 0.45%, and more preferably 0.40%.

[0034] V: 0.01 to 0.10% Vanadium (V) improves the hardenability of steel. V also has the effect of precipitating as fine carbides (VC) to improve the strength of steel. On the other hand, if the V content is too high, the carbides become coarse and the toughness of the steel decreases. Therefore, the V content is 0.01 to 0.10%. The lower limit of the V content is preferably 0.02%, and more preferably 0.03%. The upper limit of the V content is preferably 0.07%, and more preferably 0.06%, and more preferably 0.05%.

[0035] The balance of the chemical composition of the seamless steel pipe according to the present embodiment is Fe and impurities. The impurities referred to here are elements that are mixed in from ores or scraps used as raw materials for steel, or elements that are mixed in from the environment during the manufacturing process, etc.

[0036] [Optional elements] The chemical composition of the seamless steel pipe according to this embodiment may contain, instead of a portion of Fe, one or more elements selected from the group consisting of Group A, Group B, and Group C described below. All of the elements described below are optional elements. In other words, the seamless steel pipe according to this embodiment may not contain a portion or all of these elements. [Group A] Nb: 0 to 0.020%, and Ti: 0 to 0.020% [Group B] B: 0~0.0005% [Group C] Ca: 0 to 0.0060%

[0037] [Group A] One or two selected from the group consisting of Nb: 0-0.020% and Ti: 0-0.020% Niobium (Nb) and titanium (Ti) form fine precipitates to improve the toughness and strength of steel. Therefore, one or both of Nb and Ti may be contained as necessary. This effect can be obtained if even a small amount of either Nb or Ti is contained. On the other hand, if the content of Nb and Ti is too high, the precipitates become coarse and the toughness of the steel decreases. Therefore, the content of each of Nb and Ti is 0.020% or less. The lower limit of the Nb content is preferably 0.001%, more preferably 0.002%, more preferably 0.005%, and further preferably 0.010%. The upper limit of the Nb content is preferably 0.018%, and further preferably 0.015%. The lower limit of the Ti content is preferably 0.001%, more preferably 0.002%, and further preferably 0.004%. The upper limit of the Ti content is preferably 0.015%, and further preferably 0.010%.

[0038] [Group B]B:0~0.0005% Boron (B) improves the hardenability of steel. Therefore, it may be contained as necessary. This effect can be obtained even if even a small amount of B is contained. On the other hand, if the B content is too high, the weldability of the steel decreases. Therefore, the B content is 0.0005% or less. The lower limit of the B content is preferably 0.0001%, and more preferably 0.0002%. The upper limit of the B content is preferably 0.0004%, and more preferably 0.0003%.

[0039] [Group C]Ca:0~0.0060% Calcium (Ca) suppresses the formation of MnS and improves the toughness and hydrogen-induced cracking resistance of steel. Therefore, it may be contained as necessary. This effect can be obtained even if even a small amount of Ca is contained. On the other hand, if the Ca content is too high, the cleanliness of the steel decreases, and the toughness and hydrogen-induced cracking resistance of the steel decrease. Therefore, the Ca content is 0.0060% or less. The lower limit of the Ca content is preferably 0.0001%, more preferably 0.0005%, and further preferably 0.0010%. The upper limit of the Ca content is preferably 0.0055%, more preferably 0.0050%, and further preferably 0.0040%.

[0040] [About Fn1] In the seamless steel pipe according to this embodiment, Fn1, represented by the following formula (1), is 0.44 or more. Fn1=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15 (1) The content of each element in formula (1) is substituted for the corresponding element symbol in mass%.

[0041] Fn1 is the carbon equivalent and is an index of the hardenability of steel. If Fn1 is too small, it is difficult to form a structure with high strength up to the center of the wall thickness. Therefore, Fn1 is 0.44 or more. The lower limit of Fn1 is preferably 0.45, more preferably 0.46. On the other hand, if Fn1 is too large, the weldability may decrease. The upper limit of Fn1 is preferably 0.55, more preferably 0.50, and more preferably 0.48.

[0042] [About Fn2] In the seamless steel pipe according to this embodiment, Fn2 represented by the following formula (2) is preferably 0.070 or less. Fn2=V+Ti+Nb (2) For each element symbol in formula (2), the content of the corresponding element is substituted in mass%. If the corresponding element is not contained, 0 is substituted.

[0043] V, Ti and Nb are all elements that form fine precipitates and increase the strength of steel. If the content of these elements is too high, it may be difficult to make the strength of the steel within the range of the X65 grade of the API standard, and there is a concern that the toughness of the steel after welding may be deteriorated. Therefore, Fn2 is preferably 0.070 or less. The upper limit of Fn2 is more preferably 0.065, and further preferably 0.060. The lower limit of Fn2 is not particularly limited, but is, for example, 0.020, preferably 0.025, more preferably 0.030, and further preferably 0.040.

[0044] [Organization] The seamless steel pipe according to this embodiment has a grain size number according to ASTM E112-13 (2021) of 6.0 or more at the center of the wall thickness. The larger the grain size number, the finer the grains. If the grain size number is too small, the required strength cannot be obtained. The grain size number is preferably 6.5 or more, more preferably 7.0 or more, and more preferably 7.5 or more. On the other hand, if the grain size number is too large, it may be difficult to make the strength of the steel within the range of the X65 grade of the API standard. The upper limit of the grain size number is preferably 10.0, more preferably 9.5, more preferably 9.0, and more preferably 8.5.

[0045] The seamless steel pipe according to the present embodiment preferably has a structure mainly composed of tempered martensite or bainite throughout the entire thickness direction. More specifically, the seamless steel pipe according to the present embodiment preferably has a structure in which the volume fraction of tempered martensite or bainite is 90% or more in both the vicinity of the inner and outer surfaces and the center of the thickness. The volume fraction of tempered martensite or bainite is more preferably 95% or more.

[0046] In the seamless steel pipe according to the present embodiment, the ratio of the number density of V-containing particles near the inner and outer surfaces to the number density of V-containing particles in the wall thickness center is 0.60 or more. More specifically, in the seamless steel pipe according to the present embodiment, quantitative analysis is performed by energy dispersive X-ray analysis using V, Nb, Ti, Mo and Al as target elements, particles with a V content of 30 mass% or more are defined as V-containing particles, and in a cross section perpendicular to the tube axis direction, the number density of V-containing particles having a circle equivalent diameter of 10 to 100 nm at a position at a depth of 2 mm from the outer surface of the steel pipe is defined as NDos, the number density of V-containing particles having a circle equivalent diameter of 10 to 100 nm at a position at a depth of 2 mm from the inner surface of the steel pipe is defined as NDis, and the number density of V-containing particles having a circle equivalent diameter of 10 to 100 nm in the wall thickness center is defined as NDos / NDc and NDis / NDc are each 0.60 or more.

[0047] Vanadium is an element that contributes greatly to improving hardenability by dissolving in austenite. On the other hand, if vanadium remains in the steel in the form of particles such as carbide (VC), the effect of improving hardenability is not exhibited. Therefore, in order to make the structure of the steel pipe uniform in the wall thickness direction, it is preferable to make the distribution of V-containing particles uniform in the wall thickness direction. If each of NDos / NDc and NDis / NDc is 0.60 or more, a uniform structure in the wall thickness direction is obtained. The lower limit of each of NDos / NDc and NDis / NDc is preferably 0.65, more preferably 0.70, and more preferably 0.75. The upper limit of each of NDos / NDc and NDis / NDc is not particularly limited, but is, for example, 1.50, preferably 1.20, more preferably 1.10, more preferably 1.05, and more preferably 1.00.

[0048] NDos, NDis and NDc are measured as follows:

[0049] Test pieces are taken from a position 2 mm deep from the outer surface of the steel pipe, a position 2 mm deep from the inner surface of the steel pipe, and from the center of the wall thickness. The surface perpendicular to the axial direction of the steel pipe is used as the observation surface, and the observation surface of the test piece is mirror-polished and then ultrasonically cleaned in methanol. The cleaned surface is covered with a carbon vapor deposition film. The test piece with its surface covered with the vapor deposition film is immersed in an electrolyte (10% acetylacetone-1% tetramethylammonium chloride-methanol solution) at 20°C and electrolysis is carried out for 10 minutes. The electrolysis conditions are voltage: 100 mV, electrolysis amount: 10 C / cm 2 The evaporated film is peeled off from the electrolyzed test piece. The evaporated film obtained is washed with ethanol, then scooped up with a sheet mesh and dried.

[0050] This vapor-deposited film (replica film) is observed under a transmission electron microscope (TEM). Specifically, the vapor-deposited film is observed at a magnification of 20,000 times and an acceleration voltage of 200 kV. The size and number of the observation fields are not particularly limited, but the total area of ​​the observation fields is preferably 100 μm 2For example, if the observation field is 4.0 μm × 5.0 μm, the number of observation fields shall be 5 or more, and the total area of ​​the observation fields shall be 100 μm 2 That is all.

[0051] In each observation field, particles with a circle-equivalent diameter of 10 to 100 nm are identified. The particles can be identified from the contrast. In this specification, the "particle" is not limited to a circular (spherical) particle, but may be a small piece having an angular shape or an elongated elliptical piece. The circle-equivalent diameter of the precipitate can be determined by image analysis of the observation image in the TEM observation.

[0052] The identified particles are subjected to point analysis by energy dispersive X-ray spectrometry (EDS). The content of elements contained in each particle is determined by the EDS point analysis. In the EDS point analysis, the acceleration voltage is set to 200 kV, and the target elements are quantified as V, Nb, Ti, Mo, and Al. Based on the EDS analysis results for each particle with a circle equivalent diameter of 100 nm or less, particles with a V content of 30% or more by mass are identified as V-containing particles. In other words, particles with a ratio of the mass of V to the total mass of V, Nb, Ti, Mo, and Al of 30% or more are identified as V-containing particles.

[0053] In the above-mentioned analysis method, in addition to using replica samples, C, which is a light element, is difficult to accurately analyze by EDS, so C is excluded from the elements to be analyzed. Therefore, in the above-mentioned analysis method, it is not possible to strictly determine whether the V-containing particles are carbides. On the other hand, in the chemical composition of the seamless steel pipe according to the present embodiment, under the condition that the equivalent circle diameter is 100 nm or less, it is considered that almost all of the V-containing particles identified as above are V carbides (VC) or composite carbides.

[0054] Based on the total number of V-containing particles identified in each observation field and the total area of ​​the observation field, the number density of V-containing particles (particles / μm 2In this embodiment, the number density of the V-containing particles is determined by rounding off the obtained value to one decimal place.

[0055] The equivalent circle diameter of V-containing particles present in the steel pipe is preferably 100 nm or less, that is, it is preferable that no V-containing particles having an equivalent circle diameter of more than 100 nm are present in the steel pipe.

[0056] [Mechanical properties, etc.] The seamless steel pipe according to this embodiment preferably has a yield strength of 450 MPa or more in a pipe axial tensile test (hereinafter referred to as "L-direction tensile test") measured on a round bar test piece (parallel part diameter: 12.7 mm, gauge length: 50.8 mm; hereinafter this test piece will be referred to as "round bar test piece with parallel part diameter of 12.7 mm") specified in ASTM E8 / E8M-21 taken from the center of the wall thickness. The yield strength is a value determined by the 0.5% total elongation method.

[0057] 3 and 4 are diagrams showing the positions where the arc-shaped test specimen and the round bar test specimen are taken, respectively. In a thick-walled steel pipe, the structure in the center of the wall thickness is likely to be coarse grained, and the strength is likely to be lower than that near the inner and outer surfaces. Therefore, there may be a difference between the strength measured on the arc-shaped test specimen S1 (FIG. 3) of the entire wall thickness and the strength measured on the round bar test specimen S2 (FIG. 4) taken from the center of the wall thickness. In this embodiment, the mechanical properties of the seamless steel pipe are evaluated by the strength (yield strength and tensile strength) measured in the L-direction tensile test using a round bar test specimen with a parallel part diameter of 12.7 mm taken from the center of the wall thickness. In the following description, when the terms "yield strength" and "tensile strength" are simply used, they refer to the yield strength and tensile strength measured using this round bar test specimen, respectively.

[0058] The lower limit of the yield strength is more preferably 480 MPa, and even more preferably 500 MPa. However, it may not be preferable for the strength to be too high because of the high cost of welding materials for overmatched joints. The upper limit of the yield strength is preferably 600 MPa, more preferably 580 MPa, and even more preferably 560 MPa.

[0059] The seamless steel pipe according to the present embodiment preferably has a tensile strength of 535 MPa or more. The lower limit of the tensile strength is more preferably 550 MPa, and further preferably 580 MPa. The upper limit of the tensile strength is preferably 760 MPa, more preferably 700 MPa, and further preferably 650 MPa.

[0060] The seamless steel pipe according to the present embodiment preferably has a yield ratio (yield strength / tensile strength) of 0.80 to 0.95. The lower limit of the yield ratio is more preferably 0.83, and further preferably 0.85. The upper limit of the yield ratio is more preferably 0.92, and further preferably 0.90.

[0061] The seamless steel pipe of this embodiment preferably has a difference (hereinafter referred to as "measured strength difference due to test piece shape") between the yield strength in an L-direction tensile test measured on an arc-shaped test piece of full thickness (width: 38.1 mm, gauge length: 50.8 mm) specified in ASTM E8 / E8M-21 and the yield strength in an L-direction tensile test measured on a round bar test piece with a parallel section diameter of 12.7 mm taken from the center of the wall thickness of 10 MPa or less.

[0062] As described above, in a thick steel pipe, the structure in the center of the wall thickness tends to be coarse grained, and the strength tends to be lower than that in the vicinity of the inner and outer surfaces. In this embodiment, the measured strength difference due to the test piece shape is used as an index of the uniformity of the structure in the wall thickness direction. In other words, it is evaluated that the smaller the measured strength difference due to the test piece shape, the more uniform the structure in the wall thickness direction is. The measured strength difference due to the test piece shape is more preferably 8 MPa or less, even more preferably 7 MPa or less, and even more preferably 5 MPa or less.

[0063] The seamless steel pipe according to the present embodiment may be a seamless steel pipe for line pipes. The seamless steel pipe according to the present embodiment can be particularly suitably used as a seamless steel pipe for line pipes.

[0064] The seamless steel pipe according to this embodiment preferably has a wall thickness of 40.0 mm or more. The lower limit of the wall thickness is more preferably 41.0 mm, more preferably 42.0 mm, more preferably 43.0 mm, and more preferably 45.0 mm. The upper limit of the wall thickness is not particularly limited, but is, for example, 55.0 mm, preferably 52.0 mm, and more preferably 50.0 mm.

[0065] [Manufacturing method of seamless steel pipes] An example of a method for producing a seamless steel pipe according to the present embodiment will be described. The method for producing a seamless steel pipe according to the present embodiment includes a step of preparing a mother pipe having the above-mentioned chemical composition, a step of quenching the mother pipe, and a step of tempering the quenched mother pipe.

[0066] A seamless steel pipe having the above-mentioned chemical composition is prepared.

[0067] A seamless steel pipe can be produced, for example, by hot working a billet produced by hot working an ingot, slab, or bloom, or by hot working a billet produced by a continuous casting method. The hot working of the billet can be, for example, piercing and rolling by the Mannesmann method, hot extrusion, hot forging, or hot rolling.

[0068] When manufacturing a mother pipe for a seamless steel pipe, a heat treatment called "direct quenching" may be performed, in which the mother pipe is rapidly cooled (e.g., water-cooled) from the high temperature state after hot pipe making. The manufacturing method according to the present embodiment is applicable to both mother pipes that have been directly quenched and mother pipes that have not been directly quenched. However, it is difficult to obtain a fine-grained structure that is uniform in the wall thickness direction by direct quenching alone. Therefore, in the present embodiment, even if the mother pipe is directly quenched, it is necessary to perform a quenching process described below separately.

[0069] The raw pipe is quenched. Specifically, the raw pipe is heated to a holding temperature in the austenite temperature range, held at the holding temperature for a predetermined holding time, and then cooled.

[0070] More specifically, the quenching process includes the steps of heating the mother tube to a temperature of 600°C or higher at an average heating rate of 5°C / min or less in the temperature range from 400°C to 600°C, heating the mother tube to a holding temperature at an average heating rate of 10°C / min or more in the temperature range from 600°C to a holding temperature that is a temperature equal to or higher than the Ac3 point, holding the mother tube at the holding temperature for a period of 10 minutes to 60 minutes, and cooling the mother tube held at the holding temperature.

[0071] The average heating rate in the temperature range from 400°C to 600°C (hereinafter referred to as the "first heating rate") is 5°C / min or less. By reducing the first heating rate, sufficient preheating can be provided up to the center of the wall thickness of the steel pipe, and uniform solid solution of the V-containing particles can be promoted in the subsequent heating. The heating rate during this period does not need to be constant, and it is sufficient that the average heating rate is 5°C / min or less. The first heating rate is preferably 4°C / min or less. The heating rate in the temperature range up to 400°C is arbitrary.

[0072] The blank tube heated to a temperature of 600° C. or higher is then heated to a holding temperature that is a temperature of the Ac3 point or higher. The lower limit of the holding temperature is preferably 900° C., and more preferably 920° C. The upper limit of the holding temperature is preferably 1100° C., and more preferably 1050° C.

[0073] The average heating rate in the temperature range from 600° C. to the holding temperature (hereinafter referred to as the "second heating rate") is 10° C. / min or more. If the second heating rate is too small, the crystal grains may become coarse during heating.

[0074] The time for which the blank tube is held at the holding temperature is 10 minutes or more and 60 minutes or less. If the holding time is too short, the V-containing particles may not be sufficiently dissolved. On the other hand, if the holding time is too long, the crystal grains become coarse. The upper limit of the holding time is preferably 50 minutes, and more preferably 40 minutes. The lower limit of the holding time is more preferably 15 minutes, and even more preferably 20 minutes.

[0075] The mother pipe that has been held at the holding temperature for a predetermined time is cooled from the holding temperature, preferably by water cooling, at a sufficiently high cooling rate so that the structure of the mother pipe up to the center of the wall thickness becomes a quenched structure (martensite or bainite).

[0076] The quenched raw pipe is then tempered. Specifically, the quenched raw pipe is heated to a predetermined temperature and held there for a predetermined tempering time.

[0077] The tempering is preferably carried out so that the LMP represented by the following formula (3) becomes 18,200 to 19,000. LMP = (T + 273) × (20 + log(t)) (3) In equation (3), T is the tempering temperature (unit: °C), t is the holding time at the tempering temperature (unit: hours), and log(t) is the base 10 logarithm of t.

[0078] The lower limit of the LMP is more preferably 18800, further preferably 18820, and further preferably 18850. The upper limit of the LMP is more preferably 18950, and further preferably 18900.

[0079] The tempering temperature is preferably equal to or lower than the Ac1 point. The upper limit of the tempering temperature is more preferably 700° C., and further preferably 680° C. The lower limit of the tempering temperature is preferably 550° C., and further preferably 600° C.

[0080] The upper limit of the holding time at the tempering temperature is preferably 180 minutes, more preferably 160 minutes, and even more preferably 140 minutes. The lower limit of the holding time at the tempering temperature is preferably 90 minutes, more preferably 100 minutes, and even more preferably 110 minutes.

[0081] The cooling after the holding is preferably air cooling.

[0082] Through the above steps, a seamless steel pipe is manufactured.

[0083] The seamless steel pipe and the manufacturing method thereof according to one embodiment of the present invention have been described above. According to this embodiment, a seamless steel pipe having a small difference in strength between the entire wall thickness and the strength after cutting can be obtained. EXAMPLES

[0084] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0085] Steels having chemical compositions designated A to Y in Table 1 were melted and then subjected to continuous casting to produce round billets.

[0086] [Table 1]

[0087] The produced round billets were pierced and rolled to produce seamless steel pipe blanks having the outer diameter (OD) and wall thickness (WT) shown in Table 2. Each blank was quenched and tempered under the conditions shown in Table 2 to produce steel pipes with test numbers 1 to 25.

[0088] [Table 2]

[0089] "R1" in Table 2 is the first heating rate, i.e., the average heating rate in the temperature range from 400°C to 600°C during heating at the time of quenching. "R2" in Table 2 is the second heating rate, i.e., the average heating rate in the temperature range from 600°C to the holding temperature during heating at the time of quenching.

[0090] [Textural observation] The grain size number of the center of the wall thickness of each steel pipe was measured. Specifically, test pieces were taken from the steel pipes after quenching and before tempering so that the cross section perpendicular to the axial direction of the steel pipe was the test surface. The test pieces were embedded in resin and etched with a saturated aqueous solution of picric acid using the Bechet-Beaujard method to reveal the prior austenite grain boundaries, and the grain size number of the prior austenite grains was measured in accordance with ASTM E112-13 (2021).

[0091] The NDos, NDis, and NDc of each steel pipe, as well as their ratios (NDos / NDc and NDis / NDc) were determined by the method described above. Note that no V-containing particles with a circle equivalent diameter exceeding 100 nm were observed in any of the steel pipes.

[0092] The results of the structure observation are shown in Table 3. Each steel pipe had a structure with a volume fraction of bainite (tempered bainite) of 90% or more in both the vicinity of the inner and outer surfaces and the center of the wall thickness. The volume fraction of the structure was measured as follows. First, a test piece was taken so that the cross section perpendicular to the pipe axis direction was the test surface, and was etched with a nital etching solution to reveal the structure. Then, optical microscope photographs of 500 μm × 500 μm were taken at a position 2 mm deep from the inner and outer surfaces of the steel pipe and at the center of the wall thickness, with the center of the field of view being the center. Lines were drawn vertically and horizontally at 25 μm pitches on each structure photograph, and the number of lattice points on the ferrite structure was counted. The number of lattice points on the ferrite structure was subtracted from the total number of lattice points, and the ratio was calculated as a percentage to determine the volume fraction of bainite (tempered bainite) in each structure photograph (the volume fraction and the area fraction were considered to be equal).

[0093] [Table 3]

[0094] [Mechanical properties] From each steel pipe, an arc-shaped test piece (width: 38.1 mm, gauge length: 50.8 mm) of full thickness as specified in ASTM E8 / E8M-21 and a round bar test piece (parallel part diameter: 12.7 mm, gauge length: 50.8 mm) as specified in ASTM E8 / E8M-21 were taken so that the longitudinal direction was parallel to the pipe axis direction. L-direction tensile tests were conducted using these test pieces. Yield strength (YS), tensile strength (TS) and yield ratio (YR) are shown in Table 4.

[0095] [Table 4]

[0096] As shown in Tables 1 to 4, the steel pipes of test numbers 1 to 9, 24 and 25 had Fn1 of 0.44 or more, NDos / NDc and NDis / NDc of 0.60 or more, and grain size numbers at the center of the wall thickness of 6.0 or more. These steel pipes had yield strengths of 450 MPa or more, and the measured strength differences due to the test specimen shapes were 10 MPa or less.

[0097] In the steel pipes of test numbers 10 to 13, the measured strength difference due to the test piece shape was larger than 10 MPa. In the steel pipes of these test numbers, NDos / NDc and NDis / NDc were both less than 0.60, and it is considered that the structure was not uniform in the wall thickness direction. It is considered that NDos / NDc and NDis / NDc were less than 0.60 because the first heating rate was too large.

[0098] The steel pipes of test numbers 14 to 16 had a yield strength of less than 450 MPa. This is believed to be because the structure of the steel pipes was coarse grained. The reason for the coarse grained structure is believed to be that the quenching holding time was too long.

[0099] The steel pipes of test numbers 17 and 18 had a yield strength of less than 450 MPa. This is believed to be because the value of Fn1 was too small.

[0100] The steel pipe of test number 19 had a yield strength of less than 450 MPa, which is believed to be due to the V content being too low.

[0101] For steel pipes with test numbers 20 and 21, the difference in measured strength due to the test piece shape was greater than 10 MPa. For steel pipes with these test numbers, both NDos / NDc and NDis / NDc were less than 0.60, and it is believed that the structure was not uniform in the wall thickness direction. It is believed that the NDos / NDc and NDis / NDc were less than 0.60 because the quenching holding time was too short.

[0102] The steel pipes of test numbers 22 and 23 had a yield strength of less than 450 MPa. This is believed to be because the steel pipes had coarse grains. The reason for the coarse grains is believed to be that the second heating rate was too slow.

[0103] The above describes the embodiments of the present invention. The above-described embodiments are merely examples for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiments, and the above-described embodiments can be appropriately modified and carried out within the scope of the invention.

Claims

1. In mass percent, C: 0.030-0.100%, Si: 0.05-0.50%, Mn: 0.30-1.70%, P: 0.020% or less, S: 0.0050% or less, Al: 0.001-0.100%, N: 0.0200% or less, Cr: 0.05-0.30%, Mo: 0.05-0.23%, Cu: 0.10-0.50%, Ni: 0.20-0.50%, V: 0.01 to 0.10%, Nb: 0 to 0.020%, Ti: 0 to 0.020%, B: 0 to 0.0005%, Ca: 0-0.0060%, The balance is Fe and impurities, Fn1 represented by the following formula (1) is 0.44 or more, The grain size number according to ASTM E112-13 (2021) at the center of the wall thickness is 6.0 or more; A seamless steel pipe in which quantitative analysis is performed by energy dispersive X-ray analysis with V, Nb, Ti, Mo and Al as target elements, particles having a V content of 30 mass% or more are defined as V-containing particles, NDos is the number density of V-containing particles having a circle-equivalent diameter of 10 to 100 nm at a position 2 mm deep from the outer surface of the steel pipe in a cross section perpendicular to the pipe axis direction, NDis is the number density of V-containing particles having a circle-equivalent diameter of 10 to 100 nm at a position 2 mm deep from the inner surface of the steel pipe, and NDc is the number density of V-containing particles having a circle-equivalent diameter of 10 to 100 nm in a central portion of the wall thickness, and each of NDos / NDc and NDis / NDc is 0.60 or more. Fn1=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15 (1) Each element symbol in formula (1) is substituted with the content of the corresponding element in mass %.

2. The seamless steel pipe according to claim 1, The chemical composition, in mass%, Nb: 0.001-0.020%, Ti: 0.001 to 0.020%, B: 0.0001 to 0.0005%, and Ca: 0.0001-0.0060%, A seamless steel pipe comprising one or more selected from the group consisting of:

3. The seamless steel pipe according to claim 1 or 2, A seamless steel pipe having a yield strength of 450 MPa or more in an axial tensile test measured using a round bar test piece (parallel portion diameter 12.7 mm, rating distance 50.8 mm) specified in ASTM E8 / E8M-21 taken from the center of the wall thickness.

4. The seamless steel pipe according to claim 1 or 2, The seamless steel pipe is a seamless steel pipe for line pipe.

5. The seamless steel pipe according to claim 1 or 2, A seamless steel pipe having a wall thickness of 40.0 mm or more.

6. A method for producing the seamless steel pipe according to claim 1 or 2, preparing a blank tube having the chemical composition; quenching the blank tube; and a step of tempering the quenched mother pipe, The quenching step includes: a step of heating the blank tube to a temperature of 600° C. or higher at an average heating rate of 5° C. / min or less in a temperature range of 400° C. to 600° C.; 3 heating the blank tube to a holding temperature, which is a temperature equal to or higher than the holding temperature point, at an average heating rate of 10° C. / min or more; holding the blank tube at the holding temperature for a period of 10 minutes to 60 minutes; and cooling the mother pipe held at the holding temperature.