Homoepitaxial thin film, its manufacturing method and manufacturing device

JPWO2024075690A5Active Publication Date: 2024-10-03SHINCRON KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024505340
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-05
Filing Date
2023-10-02
Publication Date
2024-10-03
Estimated Expiration
2043-10-02

AI Technical Summary

Technical Problem

Existing methods for forming thin films of lithium niobate (LN) and lithium tantalate (LT) single crystals face challenges such as damage from grinding processes, high manufacturing costs, and compromised structural integrity due to high-energy ion implantation, with conventional epitaxial growth technologies not applicable to these materials without causing reoxidation.

Method used

A low-temperature high-frequency sputtering method is used to deposit a homoepitaxial thin film on LN or LT single crystals, employing specific Euler angles and controlled ion impacts to maintain crystallinity and avoid reoxidation, utilizing a specialized manufacturing apparatus with features like a rotating susceptor and shielding to promote uniform deposition.

Benefits of technology

The method enables the formation of a homoepitaxial thin film on LN or LT single crystals without damaging the crystal structure, maintaining their properties and avoiding reoxidation, thus improving manufacturing efficiency and reducing costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

In order to form a homoepitaxial thin film on a surface of a substrate (2) having a surface of a LiNbO3 single crystal or a LiTaO3 single crystal, the same composition as that of the single crystal is deposited on the surface of the substrate having a surface of a LiNbO3 single crystal or a LiTaO3 single crystal by a high-frequency sputtering method. The manufacturing apparatus (1) has a chamber (11) and a high-frequency power supply that supplies high-frequency power to a target (121) placed inside the chamber, and a sputtering electrode (12) is placed so that the surface normal (PL1) of the target is offset from the substrate at the film formation position and is inclined at an angle of 15 to 75 degrees with respect to the surface normal (PL2) of the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a homoepitaxial thin film, and a method and apparatus for producing the same. [Background technology]

[0002] Lithium niobate (LiNbO3, hereafter also referred to as LN) and lithium tantalate (LiTaO3, hereafter also referred to as LT), which are oxide single crystals, are materials that have excellent piezoelectric and electro-optical effects. In recent years, composite substrates in which single crystal LN or single crystal LT is bonded to a silicon substrate or a sapphire substrate as a supporting substrate to form a thin plate of single crystal LN or single crystal LT have attracted attention from the viewpoint of improving the performance of communication and optical control elements that use both materials. Thin plates of single crystal LN or single crystal LT on these composite substrates are produced by top-down processing such as grinding.

[0003] Grinding techniques include, for example, chemical mechanical polishing (CMP) and ion beam trimming. Typically, CMP is used for grinding thickness and surface flattening on the order of micrometers, while ion beam trimming is used for grinding on the order of nanometers. However, the excellent physical properties of single crystal structures are related to the crystal structure and composition of the surface layer in many device products, but since single crystal LN and single crystal LT are difficult-to-etch materials, there is a risk that these grinding processes will cause atomic-level damage such as defects and changes in composition in the surface layer. In addition, a trimming method using a gas cluster ion beam is an example of a low-damage grinding method, but there is a problem that the grinding speed is slow, which increases the manufacturing cost (see Patent Document 1).

[0004] In addition, as a method for obtaining thin single crystal LN or single crystal LT using a method other than the above grinding technique, there is a method of ion implantation of light elements and dividing and transferring the ion-implanted single crystal by heat treatment (Patent Document 2). However, the cost of dosing a large amount of high-energy ions is that the structural integrity inside the divided single crystal is damaged, and the inherent properties of the material may deteriorate. In such cases, there is a method of recovering the damage inside the crystal by additional heat treatment, but this requires adjustment of the heat treatment conditions depending on the form of the final product, which causes problems such as a complicated manufacturing process.

[0005] Incidentally, in the case of silicon single crystals used in many semiconductor devices, the structural integrity of the surface layer of a silicon single crystal is restored by forming a new thin film layer through epitaxial growth using vapor phase growth on a substrate that contains a type of defect in the surface layer that cannot be overlooked in terms of the performance required for device products (see Patent Document 3). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2020-43214 A [Patent Document 2] International Publication No. 2009 / 081651 [Patent Document 3] JP 2010-177355 A Summary of the Invention [Problem to be solved by the invention]

[0007] As with silicon single crystals, epitaxial growth technology is expected for LN single crystals and LT single crystals that can recover the functionality of the single crystal surface layer that tends to be lost during the thin plate formation process, but no such technology has existed until now. This is because LN single crystals and LT single crystals used in many devices are subjected to reduction reaction treatment within the range that does not impair crystallinity in order to prevent static electricity during the manufacturing process and to eliminate product defects due to residual charges. In general, when epitaxial growth is performed, the substrate is heated to about 600°C to 1100°C to obtain sufficient crystallinity.

[0008] However, when such temperatures are applied to LN single crystals and LT single crystals that have been subjected to reduction reaction, oxygen atoms in the process atmosphere diffuse to the substrate side, causing reoxidation, and the charge suppression ability that the substrate originally possesses deteriorates. Therefore, epitaxial growth on LN single crystals and LT single crystals is preferably deposited by a low-temperature process, and it is difficult to obtain a sufficiently crystallized epitaxial thin film under such conditions.

[0009] The problem to be solved by the present invention is to form a homoepitaxial thin film on a surface of a substrate having an LN single crystal or an LT single crystal surface. [Means for solving the problem]

[0010] The present invention, which aims to solve the above problems, provides a method for producing a homoepitaxial thin film by depositing the same composition as that of a LiNbO3 single crystal or LiTaO3 single crystal on a surface of a substrate having the surface by a high-frequency sputtering method. Here, the substrate itself may be a LiNbO3 single crystal or LiTaO3 single crystal substrate, or only the surface may be a LiNbO3 single crystal or LiTaO3 single crystal substrate.

[0011] In the above invention, the Euler angles (φ, θ, ψ) of the LiNbO3 single crystal plane may be (0°±5°, 0°±5°, 0°±5°), (90°±5°, 90°±5°, 0°±5°), (180°±5°, 90°±5°, 0°±5°), (0°±5°, -95° to 260°, 0°±5°), or a crystallographically equivalent plane orientation thereto.

[0012] In the above invention, the Euler angles (φ, θ, ψ) of the LiTaO3 single crystal plane may be (90°±5°, 90°±5°, 0°±5°), (0°±5°, -95° to 140°, 0°±5°), or a crystallographically equivalent plane orientation thereto.

[0013] In the above invention, the temperature of the substrate may be set to less than 450° C., preferably less than 350° C., and more preferably less than 250° C., and epitaxial growth may be performed by the radio frequency sputtering method.

[0014] In the above invention, a DC voltage may be applied to the substrate to cause epitaxial growth by the radio frequency sputtering method.

[0015] In the above invention, argon gas and oxygen gas may be used as process gases and epitaxial growth may be performed by the radio frequency sputtering method.

[0016] In the above invention, epitaxial growth may be performed by the radio frequency sputtering method so as to reduce the impact of positive ions or negative ions on the substrate.

[0017] In the above invention, the single crystal may be subjected to a reduction reaction treatment.

[0018] The above problems can also be solved by a homoepitaxial thin film manufacturing apparatus that uses the homoepitaxial thin film manufacturing method according to the above invention.

[0019] In order to solve the above problems, the present invention provides an apparatus for producing a homoepitaxial thin film, comprising a chamber and a high frequency power supply for supplying high frequency power to a target placed inside the chamber, and depositing, by a sputtering method, a composition identical to that of a LiNbO3 single crystal or a LiTaO3 single crystal placed inside the chamber on a substrate having the single crystal.

[0020] In the above invention, a sputtering electrode may be provided in which a surface normal of the target is offset with respect to a substrate at a film formation position.

[0021] In the above invention, the sputtering electrode may be disposed such that a surface normal of the target is inclined at an angle of 15 to 75° with respect to a surface normal of the substrate.

[0022] In the above invention, the apparatus may further comprise a shielding plate disposed in front of the target inside the chamber so as to shield a plane where a surface normal of the target intersects with the surface of the substrate.

[0023] In the above invention, the device may further include a heater provided on a rear surface side of the substrate for heating the substrate.

[0024] In the above invention, the device may further comprise a rotation shaft that is electrically floating with respect to surrounding components and rotates the substrate from a rear surface side of the substrate.

[0025] In the above invention, the rotor may further include a high-frequency matching box connected to the rotating shaft and capable of adjusting a reactance of the rotating shaft.

[0026] In the above invention, the electric motor may further include a DC power supply connected to the rotating shaft and configured to apply a DC voltage to the rotating shaft.

[0027] In the above invention, the chamber may further include, in front of the target, a porous metal plate which can be grounded or to which a DC voltage can be applied, and a porous quartz plate which covers the porous metal plate.

[0028] In the above invention, the apparatus may further include a conductive susceptor for holding the single crystal substrate, and heat may be supplied to the substrate from the heater via the susceptor.

[0029] In the above invention, the apparatus may further include a conductive susceptor for holding the single crystal substrate, and a DC voltage may be applied to the substrate from the DC power supply via the susceptor.

[0030] The present invention, which has been made to solve the above problems, is a homoepitaxial thin film formed on the surface of a LiNbO3 single crystal or a LiTaO3 single crystal and made of the same composition as the single crystal.

[0031] In the above invention, the Euler angles (φ, θ, ψ) of the LiNbO3 single crystal plane may be (0°±5°, 0°±5°, 0°±5°), (90°±5°, 90°±5°, 0°±5°), (180°±5°, 90°±5°, 0°±5°), (0°±5°, -95° to 260°, 0°±5°), or a crystallographically equivalent plane orientation thereto.

[0032] In the above invention, the Euler angles (φ, θ, ψ) of the LiTaO3 single crystal plane may be (90°±5°, 90°±5°, 0°±5°), (0°±5°, -95° to 140°, 0°±5°), or a crystallographically equivalent plane orientation thereto.

[0033] In the above invention, the single crystal may be subjected to a reduction reaction treatment. Effect of the Invention

[0034] According to the present invention, a homoepitaxial thin film can be formed on the surface of a substrate having a surface of an LN single crystal or an LT single crystal. [Brief description of the drawings]

[0035] [Figure 1] FIG. 1 is a diagram showing an embodiment of a homoepitaxial thin film manufacturing apparatus of the present invention. [Diagram 2]1 is a cross-sectional view showing an embodiment of a homoepitaxial thin film of the present invention. [Diagram 3] 1 is a graph showing the results of X-ray diffraction of a LiNbO3 single crystal and a homoepitaxial thin film (X-ray diffraction apparatus (Rigaku Smart Lab), out-of-plane crystallinity evaluation: ω-2θ measurement). [Figure 4] FIG. 1 shows the results of X-ray diffraction of a LiNbO3 single crystal and a homoepitaxial thin film (X-ray diffraction apparatus (Rigaku Smart Lab), in-plane crystallinity evaluation: pole measurement LiNbO3(012)). [Diagram 5] 1 shows the results of X-ray diffraction of a LiNbO3 single crystal and a homoepitaxial thin film. [Figure 6] 1 shows the results of X-ray diffraction of a LiNbO3 single crystal and a homoepitaxial thin film. [Figure 7] 1 shows the results of X-ray diffraction of a LiNbO3 single crystal and a homoepitaxial thin film. [Figure 8] FIG. 2 is a diagram showing X-ray diffraction results of 250 nm homoepitaxial thin films deposited on substrates having various crystal plane orientations, which were formed using the homoepitaxial thin film manufacturing apparatus of FIG. [Figure 9] FIG. 1 shows a transmission electron microscope image and a selected area electron diffraction image of a LiNbO3 single crystal and a homoepitaxial thin film (part 1). [Figure 10] FIG. 2 shows a transmission electron microscope image and a selected area electron diffraction image of a LiNbO3 single crystal and a homoepitaxial thin film (part 2). [Figure 11] FIG. 3 shows a transmission electron microscope image and a selected area electron diffraction image of a LiNbO3 single crystal and a homoepitaxial thin film (part 3). [Figure 12] 1 is a graph (spectrophotometer (Agilent Cary7000)) showing the optical absorptance in the visible range before and after deposition of a homoepitaxial thin film of a reduced LiNbO3 single crystal. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] 1 is a cross-sectional view showing one embodiment of the homoepitaxial thin film manufacturing apparatus 1 according to the present invention. The homoepitaxial thin film manufacturing apparatus 1 of this embodiment is a sputtering apparatus that deposits the same composition as that of an LN single crystal or an LT single crystal on the surface of the substrate having the surface of the single crystal by radio frequency sputtering.

[0037] That is, in the homoepitaxial thin film manufacturing apparatus 1 of this embodiment, high frequency power is applied to a target made of sintered LN powder or sintered LT powder to form plasma, and positive ions accelerated by a negative DC bias generated on the surface of the target collide with the target, so that particles sputtered from the target surface are used as the material for the homoepitaxial thin film. The substrate 2 has a surface of LiNbO3 single crystal or LiTaO3 single crystal, and the LiNbO3 single crystal or LiTaO3 single crystal may be subjected to a reduction reaction treatment.

[0038] As shown in FIG. 1, the homoepitaxial thin film manufacturing apparatus 1 includes a chamber 11 that can be set to a predetermined vacuum level, and a sputtering electrode provided in the chamber 11. 12 and a susceptor also provided in the chamber 11. 13 And, it is equipped with.

[0039] The chamber 11 according to this embodiment includes a film formation chamber 111 facing a target 121 attached to a sputtering electrode 12 and a substrate 2 mounted on a susceptor 13. The film formation chamber 111 can be set to a predetermined vacuum level by an exhaust device 113 provided at an exhaust port 112 of the chamber 11.

[0040] The sputtering electrode 12 of this embodiment supplies high-frequency power to the target 121 attached to the tip. The frequency of this high-frequency power is not limited, but may include a frequency of 13.56 MHz. The target 121 is an LN target or an LT target, but may contain a certain proportion of Li2O, and the molar ratio of LiNbO3 (or LiTaO3):Li2O includes a range of 100:0 to 50:50.

[0041] The susceptor 13 of this embodiment is made of a conductive material, and can hold the substrate 2 and rotate at a predetermined rotation speed by a drive unit 132 connected to a rotation shaft 131. The susceptor 13 may be provided with a counterbore (a recess corresponding to the outer shape of the substrate 2) so that deposition processing can be performed on multiple substrates 2 in one processing. The material constituting the susceptor 13 is not particularly limited, and examples thereof include inconel, silicon carbide, graphite, and silicon. The conductivity of the susceptor 13 does not necessarily have to be exhibited at room temperature, and may be exhibited when the substrate 2 is heated at less than 450°C.

[0042] Further, a heater 133 for heating the substrate 2 to a predetermined temperature is provided below the susceptor 13. The heating method of the heater 133 is not limited, but examples include a resistance heating method using graphite or silicon carbide as a resistor, and an optical heating method using a halogen lamp. If a homoepitaxial thin film is deposited by high-frequency sputtering while maintaining the substrate 2 at a temperature below 450° C., it is possible to prevent reoxidation of the LN single crystal or LT single crystal that has been subjected to a reduction reaction while promoting the epitaxial growth of the deposited thin film.

[0043] The rotating shaft 131 of the susceptor 13 is maintained in an electrically floating state. By electrically floating the rotating shaft 131, adjustments can be made to alleviate the impact of positive ions. By depositing a thin film while rotating the substrate 2 in an electrically floating state, it is possible to deposit a thin film uniformly over the entire surface of the substrate 2 while satisfying the requirement to alleviate the impact of negative ions.

[0044] The homoepitaxial thin film manufacturing apparatus 1 of this embodiment includes a high-frequency matching box 134 that is connected to the rotating shaft 131 of the susceptor 13 and can adjust the reactance of the electrically floating rotating shaft 131. The reactance here corresponds to the capacitance and inductance in the high-frequency matching box 134. The adjustment by the high-frequency matching box 134 is performed by diagnosing the state of electrical coupling of the substrate 2 with the high-frequency plasma by measuring the DC voltage generated in the high-frequency matching box 134 during deposition.

[0045] Here, when the DC voltage indicates a negative maximum value, it indicates that the capacitive substrate sheath and capacitance are in a series resonance state, and positive ions are attracted to the substrate 2, causing reverse sputtering. In contrast, when the DC voltage indicates a positive maximum value, it corresponds to a parallel resonance state between the substrate 2 and the floating capacitance of the high-frequency matching device 134 including the rotating shaft 131, and negative charged particles are attracted to the substrate 2. In the case of this embodiment, by adjusting and maintaining the reactance to the latter value, it is possible to suppress re-evaporation of Li atoms deposited on the substrate 2 due to reverse sputtering, and to promote epitaxial growth of the deposited thin film.

[0046] The homoepitaxial thin film manufacturing apparatus 1 of this embodiment further includes a DC power supply 135 that is connected to the rotating shaft 131 and applies a DC voltage to the electrically floating rotating shaft 131. The DC power supply 135 may apply either a negative voltage or a positive voltage, but it is preferable to apply a positive voltage from the viewpoint of promoting epitaxial growth of the deposited thin film.

[0047] The target 121 in this embodiment is arranged so as not to directly face the substrate 2. That is, as shown in FIG. 1, the target 121 is arranged offset with respect to the rotation axis 131, and the surface normal PL1 of the target 121 is provided so as to have an inclination α of 15° to 75° with respect to the substrate normal PL2 of the substrate 2. The DC negative bias generated on the surface of the target 121 accelerates the negative ions in the plasma and causes the negative ions to be emitted along the surface normal L1 of the target 121. Therefore, by not facing the substrate 2 and the target 121, it is possible to prevent the negative ions from directly colliding with the substrate 2, and to alleviate the impact of the negative ions. This can promote the epitaxial growth of the deposited thin film.

[0048] The homoepitaxial thin film manufacturing apparatus 1 of this embodiment includes a shielding plate 122 that reduces the impact of negative ions emitted from the target 121 along the surface normal PL1 of the target 121. The shielding plate 122 of this embodiment is disposed in front of the target 121 so as to shield the surface where the surface normal PL1 of the target 121 intersects with the surface of the substrate 2. This makes it possible to suppress the negative ions emitted along the surface normal PL1 of the target 121 from impacting the substrate 2, and further promotes the epitaxial growth of the deposited thin film.

[0049] The homoepitaxial thin film manufacturing apparatus of this embodiment includes a perforated metal plate 123 and a perforated quartz plate 124. As shown in FIG. 1, the perforated metal plate 123 and the perforated quartz plate 124 of this embodiment are provided on the inner wall of the film forming chamber 111 in front of the target 121, and the perforated quartz plate 124 is disposed in front of the perforated metal plate 123. The perforated metal plate 123 is electrically coupled to the plasma and provides electrons to the plasma. At that time, the potential of the perforated metal plate 123 may be ground, or a controlled negative potential may be supplied to provide electrons more actively. In addition, in order to increase the efficiency of the power consumed in the actual sputtering phenomenon among the high frequency power input to the target 121, the perforated metal plate 123 may be stacked in multiple sheets to increase the surface area. The perforated quartz plate 124 prevents the deposition of sputter particles on the perforated metal plate 123 and maintains a constant supply of electrons. The porous quartz plate 124 also has the function of preventing reverse deposition onto the substrate 2 of the material of the porous metal plate 123 that is sputtered when a negative potential is applied.

[0050] The homoepitaxial thin film manufacturing apparatus of this embodiment further includes a gas supply device 125, which supplies argon gas and oxygen gas to the film formation chamber 111 as process gases during film formation. EXAMPLES

[0051] 2 is a cross-sectional view showing an embodiment of a homoepitaxial thin film according to the present invention. In the illustrated example, a homoepitaxial thin film 22 is formed on an LN single crystal 21. Deposition using the homoepitaxial thin film manufacturing apparatus 1 of the present embodiment described above was performed with LN as the target 121, a heating temperature of the substrate 2 by the heater 133 of 300° C., a sputtering rate of 0.2 angstroms / second, and a flow rate ratio of argon gas and oxygen gas of 50:50.

[0052] 3 to 7 are graphs showing the results of X-ray diffraction of a 250 nm homoepitaxial thin film formed using the homoepitaxial thin film manufacturing apparatus 1 of this embodiment. The X-ray diffraction apparatus used was a Smart Lab manufactured by Rigaku Corporation, and the out-of-plane crystallinity was evaluated by measuring ω-2θ.

[0053] Figure 3 is a graph showing the results of X-ray diffraction on a Z-cut surface (Euler angles (0°, 0°, 0°)), and the lower figure is an enlarged view of the peak portion of the upper figure. As shown in Figure 3, the diffraction peak of the homoepitaxial thin film was confirmed at a 2θ position slightly lower than the diffraction peak of the substrate of this example.

[0054] FIG. 4 is a graph showing the X-ray diffraction results of an X-cut surface (Euler angles (90°, 90°, 0°)), and the lower figure is an enlarged view of the peak portion of the upper figure. As shown in FIG. 4, similar to the result of the Z-cut surface in FIG. 3, a diffraction peak of the homoepitaxial thin film was confirmed at a 2θ position slightly lower than the diffraction peak of the substrate of this example.

[0055] Figures 5 to 7 show a rotated Y-cut surface (with Euler angles of (0°, -49°, 0°), (0°, 154°, 0°), and (0°, -37°, 0°) respectively), and as shown in each figure, no unnecessary diffraction peaks are observed in the direction perpendicular to the surface of substrate 2, suggesting the presence of a homoepitaxial thin film.

[0056] Fig. 8 shows the X-ray diffraction results of homoepitaxial thin films of 250 nm deposited on substrates having various crystal plane orientations, which were formed using the homoepitaxial thin film manufacturing apparatus 1 of this embodiment. The X-ray diffraction apparatus used was a Rigaku Smart Lab, and the in-plane crystallinity evaluation was performed using the pole measurement LiNbO3 (012) plane. As shown in Fig. 8, diffraction patterns with symmetry corresponding to each single crystal were confirmed, and it was possible to identify the thin films as having the same crystal structure as the substrate, i.e., homoepitaxial thin films.

[0057] 9 to 11 are diagrams showing transmission electron microscope (TEM) images and selected area electron diffraction (SAED) images of a homoepitaxial thin film of 250 nm formed using the homoepitaxial thin film manufacturing apparatus 1 of this embodiment. In each of the diagrams of Figs. 9 to 11, the selected area electron diffraction images shown in the lower diagrams are images of the substrate and thin film portions indicated by circles in the upper diagrams, respectively. Fig. 9 shows an X-cut surface, Fig. 10 shows a 41Y-cut surface, and Fig. 11 shows a 127Y-cut surface, respectively. In the selected area electron diffraction images of Figs. 9 to 11, the thin film shows a diffraction pattern equivalent to that of the substrate, so that it was directly confirmed that homoepitaxial thin films having a single crystal structure equivalent to that of the substrate were deposited on substrates having various crystal plane orientations.

[0058] FIG. 12 is a graph showing the optical absorptance in the visible region before and after deposition of a homoepitaxial thin film of a reduced LN single crystal, where the dashed line shows the optical absorptance before deposition and the solid line shows the optical absorptance after deposition. The spectrophotometer used was an Agilent Cary7000. As shown in FIG. 12, there is almost no difference in the optical absorptance profile before and after deposition of the homoepitaxial thin film. In addition, since the LN single crystal that has not been subjected to a reduction treatment does not have optical absorptance, the homoepitaxial thin film deposited in this embodiment shows that reoxidation does not occur on the substrate. [Explanation of symbols]

[0059] 1. Homoepitaxial thin film manufacturing equipment 11…Chamber 111...Deposition chamber 112…Exhaust port 113…Exhaust system 12...Sputter electrode 121…Target 122...Shielding plate 123...Porous metal plate 124...Porous quartz plate 125...Gas supply equipment 13…Susceptor 131...Rotation axis 132...Drive unit 133…Heater 134...High frequency matching box 135…DC power supply PL1: Target surface normal PL2: Substrate surface normal α: Angle between the target surface normal and the substrate surface normal

Claims

1. LiNbO 3 Single crystal or LiTaO 3 A method for producing a homoepitaxial thin film, comprising depositing a composition identical to that of the single crystal on a surface of a substrate having a single crystal by a radio frequency sputtering method, comprising: A method for producing a homoepitaxial thin film, comprising setting the temperature of the substrate to less than 450° C. and epitaxially growing the thin film by the high frequency sputtering method.

2. LiNbO 3 Single crystal or LiTaO 3 A method for producing a homoepitaxial thin film, comprising depositing a composition identical to that of the single crystal on a surface of a substrate having a single crystal by a radio frequency sputtering method, comprising: A method for producing a homoepitaxial thin film, comprising applying a DC voltage to the substrate and epitaxially growing the thin film by the radio frequency sputtering method.

3. The LiNbO 3 3. The method for producing a homoepitaxial thin film according to claim 1 or 2, wherein the single crystal plane has Euler angles (φ, θ, ψ) of (0°±5°, 0°±5°, 0°±5°), (90°±5°, 90°±5°, 0°±5°), (180°±5°, 90°±5°, 0°±5°), (0°±5°, -95° to 260°, 0°±5°), or a plane orientation crystallographically equivalent thereto.

4. The LiTaO 3 3. The method for producing a homoepitaxial thin film according to claim 1 or 2, wherein the Euler angles (φ, θ, ψ) of the single crystal plane are (90°±5°, 90°±5°, 0°±5°), (0°±5°, -95° to 140°, 0°±5°), or a plane orientation crystallographically equivalent thereto.

5. 3. The method for producing a homoepitaxial thin film according to claim 1, wherein argon gas and oxygen gas are used as process gases and epitaxial growth is carried out by the high frequency sputtering method.

6. 3. The method for producing a homoepitaxial thin film according to claim 1, wherein epitaxial growth is carried out by the high frequency sputtering method so as to reduce impact of positive ions or negative ions on the substrate.

7. 3. The method for producing a homoepitaxial thin film according to claim 1, wherein the single crystal is subjected to a reduction reaction treatment.

8. 3. An apparatus for producing a homoepitaxial thin film, which employs the method for producing a homoepitaxial thin film according to claim 1 or 2.

9. a chamber; and a high frequency power source that supplies high frequency power to a target disposed inside the chamber; LiNbO disposed in the chamber 3 Single crystal or LiTaO 3 An apparatus for producing a homoepitaxial thin film, which deposits a composition identical to that of a single crystal on a substrate having a single crystal surface by a sputtering method, comprising: The homoepitaxial thin film manufacturing apparatus further comprises a shielding plate arranged in front of the target inside the chamber so as to shield a plane where a surface normal of the target intersects with a surface of the substrate.

10. a chamber; and a high frequency power source that supplies high frequency power to a target disposed inside the chamber; LiNbO disposed in the chamber 3 Single crystal or LiTaO 3 An apparatus for producing a homoepitaxial thin film, which deposits a composition identical to that of a single crystal on a substrate having a single crystal surface by a sputtering method, comprising: The homoepitaxial thin film manufacturing apparatus further comprises, in front of the target inside the chamber, a porous metal plate which can be grounded or to which a DC voltage can be applied, and a porous quartz plate which covers the porous metal plate.

11. 10. The homoepitaxial thin film manufacturing apparatus according to claim 9, further comprising a sputtering electrode in which a surface normal of the target is offset with respect to the substrate at a film formation position.

12. 12. The homoepitaxial thin film manufacturing apparatus according to claim 11, wherein the sputtering electrode is disposed such that a surface normal of the target is inclined at an angle of 15 to 75 degrees with respect to a surface normal of the substrate.

13. 13. The homoepitaxial thin film manufacturing apparatus according to claim 9, further comprising a heater provided on a rear side of the substrate for heating the substrate.

14. The substrate holder further includes a conductive susceptor for holding the substrate.

14. The homoepitaxial thin film manufacturing apparatus according to claim 13, wherein heat is supplied to the substrate from the heater via the susceptor.