Method for depositing film
Patent Information
- Application Number
- JP2024549468
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2023-12-26
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2043-12-26
AI Technical Summary
Existing methods struggle to adjust film stress of silicon films while maintaining desired optical properties, such as refractive index and extinction coefficient, which are crucial for precise alignment and etching processes in semiconductor manufacturing.
A two-step sputtering process is employed to form a silicon film with a columnar structure, where the first silicon film has a lower density and the second silicon film has a higher density, allowing for adjustment of film stress while maintaining optical properties by varying the partial pressure of the sputtering gas and bias power.
This approach enables precise control of film stress and optical properties, reducing particle contamination and ensuring uniform film thickness distribution, thereby enhancing the accuracy and reliability of the film formation process.
Abstract
Description
Film forming method
[0001] The present invention relates to a film formation method, and more particularly to a method for forming a silicon film that can be used as a hard mask or the like.
[0002] In the manufacturing process of semiconductor devices, when dry etching an insulating film (e.g., a silicon oxide film) formed on the surface of a substrate made of a silicon wafer, a hard mask is formed to limit the etching area, and a silicon film is sometimes used as the hard mask in this process (see, for example, Patent Document 1). Such silicon films are required to have a film density that provides strong etching resistance, and also to have a film stress within a predetermined range to prevent deformation of the etched shape during dry etching.
[0003] On the other hand, when patterning a resist layer coated on a silicon film using an exposure device, alignment with a wiring pattern already formed as an underlying layer may be required. Such alignment is typically performed by detecting alignment marks formed at predetermined positions on the substrate using a laser beam. With the recent trend toward finer wiring patterns, laser beams with smaller spot diameters are increasingly being used to enable high-precision alignment. Therefore, the silicon film is also required to have optical properties in which the refractive index (n value) and extinction coefficient (k value) at a predetermined film thickness are each within a predetermined range.
[0004] Here, for example, in consideration of productivity, it is conceivable to use a sputtering device to form the silicon film. In this case, a rare gas is introduced into a vacuum chamber in which a silicon target and a film-forming target are arranged opposite each other, and DC or AC power with a negative potential is applied to the target to sputter the target, thereby forming a silicon film with a predetermined thickness. In this case, it is generally known that the film stress or optical properties can be individually adjusted within a predetermined range by adjusting sputtering conditions such as the partial pressure of the sputtering gas during film formation, the power applied to the target, and the bias power to the substrate. However, it has not been possible to adjust the film stress while maintaining the optical properties, for example.
[0005] Patent No. 6952866
[0006] In view of the above, an object of the present invention is to provide a method for forming a silicon film that allows adjustment of film stress while maintaining optical properties.
[0007] The present inventors have conducted extensive research and have come to the following discovery. Specifically, when sputtering a silicon target to form a (single) silicon film with a predetermined thickness, adjusting sputtering conditions such as the partial pressure of the sputtering gas during film formation, the power input to the target, and the bias power applied to the substrate so as to maintain the film stress within a predetermined range does not result in the desired optical properties (specifically, the refractive index and extinction coefficient). Here, for example, if the optical properties required for the above-mentioned alignment are a refractive index (n value) in the range of 4 to 5 and an extinction coefficient (k value) in the range of 0.3 to 0.6, it was found that the desired optical properties can be easily obtained by growing the silicon film in a columnar structure and adjusting the film density at that time by changing the sputtering conditions. Therefore, without considering the film stress, first find sputtering conditions that maintain the optical properties within a predetermined range, and then use the silicon film formed under these sputtering conditions as the main silicon film. The inventors then discovered that if the underlayer of the main silicon film is grown under sputtering conditions that create a density difference in the film, specifically, if the film density is lower than that of the main silicon film when the film is grown in a columnar structure, the film stress can be adjusted while maintaining the optical properties in accordance with the density difference in the film.
[0008] In order to solve the above problems, the present invention provides a film formation method in which a silicon target and an object to be film-formed are placed in a vacuum chamber, a sputtering gas is introduced into the vacuum chamber in a vacuum atmosphere, and power is applied to the target to form a silicon film on the surface of the object to be film-formed by a sputtering method, wherein the silicon film formation is carried out in two steps: a first step of forming a first silicon film having a columnar structure, and a second step of forming a second silicon film having a columnar structure and a higher film density than the first silicon film.
[0009] Based on the above, it was confirmed that the film stress can be adjusted according to the difference in film density between the first silicon film and the second silicon film while maintaining optical properties. During film formation, silicon films are also formed on components present in the vacuum chamber, such as adhesion shields, and the second silicon film, which has a higher film density, is formed on the surface layer. Therefore, when silicon film formation is repeated, the number of particles that peel off from the surface layer of the component and float in the vacuum chamber is reduced, thereby minimizing the number of particles that adhere to the film formation target after film formation. Furthermore, it was confirmed that the film can be formed with good film thickness distribution within the substrate surface, and that the film can be formed with almost no difference in film thickness distribution between the film formation targets when film formation is repeated on multiple film formation targets.
[0010] In the present invention, the partial pressure of the sputtering gas in the vacuum chamber in the first step is set to a reference partial pressure, and the partial pressure of the sputtering gas in the second step is set to be lower than the reference partial pressure. By changing the partial pressure of the sputtering gas in the first and second steps, the film density of the first and second silicon films can be changed, which is advantageous because the first and second silicon films can be successively deposited with a density difference in a single vacuum chamber. In this case, the ratio of the partial pressure in the second step to the first step is set to a range of 0.1 to 0.7. A partial pressure ratio less than 0.1 results in a high-density thin film with an excessively high refractive index (n value) and extinction coefficient (k value), while a partial pressure ratio greater than 0.7 results in a low-density thin film with an excessively low refractive index (n value) and extinction coefficient (k value).
[0011] Furthermore, in the present invention, the ratio of the thickness of the first silicon film to the thickness of the silicon film may be set in the range of 0.3 to 0.8, which is advantageous in that the film stress can be easily adjusted without changing the optical characteristics at a predetermined film thickness.
[0012] When bias power is applied to the film-forming target during the sputtering process to form the silicon film on the surface of the film-forming target, the bias power in the first and second steps can be set to a range of 20 W to 100 W. This allows the film density of each of the first and second silicon films to be adjusted, and the film stress can be adjusted over a wider range. Note that if the bias power is lower than 20 W, the controllability (tracking ability) of the power supply is poor, which may result in unstable film-forming conditions. On the other hand, if the bias power is higher than 100 W, the resulting thin film will be too high in density, resulting in an excessively high refractive index (n value) and extinction coefficient (k value).
[0013] 1A and 1B are schematic diagrams showing the configuration of a sputtering apparatus as a silicon film forming apparatus of the present embodiment. (a) and (b) are diagrams explaining the silicon film forming process. (b) are SEM images of a silicon film formed under predetermined conditions. (c) are graphs showing experimental results of a silicon film formed by the film forming method of the present embodiment. (d) are graphs showing experimental results of a silicon film formed by the film forming method of the present embodiment.
[0014] Hereinafter, with reference to the drawings, an embodiment of the silicon film forming method of the present invention will be described using as an example a silicon wafer (hereinafter referred to as "substrate Sw") on which a film is to be formed, with a silicon oxide film formed to a predetermined thickness on one side thereof, a silicon target made of a predetermined purity, and argon gas as the sputtering gas to form a silicon film on the surface of the substrate Sw by a sputtering method. In the following, terms indicating directions such as up and down are based on FIG.
[0015] Referring to FIG. 1 , SM denotes a magnetron sputtering apparatus capable of implementing the film formation method of this embodiment. The sputtering apparatus SM includes an earthed vacuum chamber 1. A vacuum pump 12 is connected to the vacuum chamber 1 via an exhaust pipe 11, and the inside of the vacuum chamber 1 can be evacuated to a predetermined pressure (vacuum level). A gas pipe 13 is connected to the sidewall of the vacuum chamber 1, and a mass flow controller 14 is installed in the gas pipe 13, which is connected to an argon gas source (not shown). Argon gas, the flow rate of which is controlled by the mass flow controller 14, can be introduced into the vacuum chamber 1.
[0016] A stage 2 is provided within the vacuum chamber 1. The stage 2 includes a base 21 disposed on the inside bottom surface of the vacuum chamber 1 via an insulator 21a, and a chuck plate 22 made of, for example, aluminum nitride or boron nitride, mounted on the base 21. An electrode 22a for electrostatic chucking is incorporated in the chuck plate 22, and by applying electricity to the electrode 22a from a chuck power supply (not shown), the substrate Sw placed with its film-forming surface facing upward can be electrostatically attracted (held). At this time, the substrate Sw is in an electrically floating state. Although not specifically shown or described, the chuck plate 22 is provided with a heating / cooling mechanism for the substrate Sw, which can adjust the substrate Sw to a predetermined temperature during film formation.
[0017] The vacuum chamber 1 is also provided with a cathode unit Uc. The cathode unit Uc includes a target 3 and a magnet unit 4 disposed above the target 3 to apply a leakage magnetic field to the space between the target 3 and the substrate Sw. A backing plate 31 is bonded to the side of the target 3 facing away from the sputtering surface 3a. When the peripheral portion of the backing plate 31 is attached to the upper wall of the vacuum chamber 1 via an insulating member 32, the target 3 and the substrate Sw are concentrically positioned opposite each other within the vacuum chamber 1 in a vacuum atmosphere. The target 3 is connected to the output of a sputtering power supply Ps, allowing, for example, DC power with a negative potential to be applied in pulses. A stainless steel or aluminum shield plate 5 is also provided within the vacuum chamber 1, surrounding the space between the substrate Sw and the target 3 to prevent sputter particles from adhering to the inner wall of the vacuum chamber 1. The adhesion prevention plate 5 is composed of an upper adhesion prevention plate 51 suspended from the upper wall of the vacuum chamber 1 and a lower adhesion prevention plate 52 that can be moved up and down by a lifting mechanism Du equipped with a cylinder and a motor.
[0018] A cylindrical block body 6 with a truncated cone-shaped profile is provided within the vacuum chamber 1 and positioned around the stage 2. The block body 6 is made of a metal such as aluminum or copper and is installed via an insulator 61 installed inside the bottom surface of the vacuum chamber 1. When the block body 6 is installed, the top of the block body 6 is flush with or located below the upper surface (film formation surface) of the substrate Sw held by the stage 2, and at least a portion of its outer cylindrical surface directly faces the plasma atmosphere formed in the vacuum chamber 1. Note that the shape of the block body 6 is not limited to this, and it does not need to completely surround the periphery of the stage 2. For example, the block body 6 can be configured by arranging multiple plates with arc-shaped profiles on the same circumference. An output 71 from a DC power supply 7 is also connected to the block body 6. During film formation, a positive potential is appropriately applied from the DC power supply 7 so that the block body 6 functions as an anode. An output 81 from an AC power supply 8 is also connected to the stage 2, allowing a predetermined range of bias power to be applied to the substrate Sw during film formation. The film forming method of this embodiment for forming a silicon film to a predetermined thickness on a substrate Sw using the sputtering apparatus SM will be described below.
[0019] The substrate Sw is placed on the stage 2 with the film-forming surface facing up and electrostatically attracted, and then the vacuum chamber 1 is evacuated. When the pressure inside the vacuum chamber 1 reaches a predetermined pressure, argon gas is introduced into the vacuum chamber 1 at a predetermined flow rate under the control of the mass flow controller 14 while maintaining a constant effective pumping speed. A sputtering power supply Ps applies pulsed DC power with a negative potential to the target 3. The argon gas flow rate is set to a range of 100 sccm to 1000 sccm (the partial pressure of the argon gas inside the vacuum chamber 1 is 0.3 Pa to 8.0 Pa), and the applied power is set to a range of 1.0 kW to 5.0 kW. If the argon gas flow rate is less than 100 sccm, a high-density thin film is formed, resulting in excessively high refractive index (n value) and extinction coefficient (k value). However, if the flow rate is greater than 1000 sccm, the sputtering rate becomes too slow, resulting in poor productivity. Furthermore, if the input power is less than 1.0 kW, the sputtering rate becomes too slow, resulting in poor productivity, while if it is more than 5.0 kW, the resulting thin film will be too dense, resulting in an excessively high refractive index (n value) and extinction coefficient (k value).
[0020] During film formation by sputtering the target 3, a positive potential (e.g., in the range of 0 V to 100 V, preferably 30 V) may be applied to the block body 6 by the DC power supply 7, and bias power (in the range of 20 W to 100 W) may be applied to the substrate Sw by the AC power supply 8. If the bias power is lower than 20 W, the controllability (tracking ability) of the power supply may be poor, and the film formation conditions may become unstable. On the other hand, if it is higher than 100 W, a high-density thin film may be formed, with an excessively high refractive index (n value) and extinction coefficient (k value). As a result, a plasma atmosphere is formed in the space between the substrate Sw and the target 3, and the target 3 is sputtered by argon gas ions in the plasma. Sputtered particles are scattered from the target 3 according to a predetermined cosine law, and a silicon film (hereinafter referred to as the "first silicon film Sf1") with a columnar structure and a relatively low film density is formed (first step), as shown in FIG. 2(a) . In this case, the film thickness of the first silicon film Sf1 is determined based on the film thickness of the silicon film Sf to be formed, and the sputtering time for forming the first silicon film Sf1 is set based on the film thickness and the sputtering rate corresponding to the power input to the target 3.
[0021] Next, when the preset sputtering time is reached, the mass flow controller 14 is controlled to change the flow rate of argon gas while maintaining the power supplied to the target 3. The argon gas flow rate at this time is set to a range of 20 sccm to 80 sccm (the partial pressure of the argon gas in the vacuum chamber 1 is 0.08 Pa to 0.2 Pa). In other words, the ratio of the partial pressure in the second step to that in the first step is set to a range of 0.1 to 0.7. In this case, if the partial pressure ratio is less than 0.1, a high-density thin film is formed, with an excessively high refractive index (n value) and extinction coefficient (k value). Conversely, if the partial pressure ratio is greater than 0.7, a low-density thin film is formed, with an excessively low refractive index (n value) and extinction coefficient (k value). As a result, as shown in FIG. 2(b), a dense silicon film (hereinafter referred to as the "second silicon film Sf2") having a similar columnar structure and a higher film density than the first silicon film Sf1 is formed (laminate) (second step). The sputtering time is set so as to reach the film thickness of the silicon film Sf. It has been confirmed that if the ratio of the film thickness of the first silicon film Sf1 to the silicon film Sf is set in the range of 0.3 to 0.8, the film stress can be changed without changing the optical characteristics at a predetermined film thickness. In this case, it has been confirmed that if the ratio of the film thickness of the first silicon film Sf1 to the silicon film Sf is set in the range of 0.3 to 0.7, the optical characteristics at a predetermined film thickness can be more suitably set.
[0022] According to the above embodiment, it has been confirmed that the film stress can be adjusted according to the difference in film density between the first silicon film Sf1 and the second silicon film Sf2 grown in a columnar structure while maintaining the optical properties. Furthermore, during the deposition of the silicon film Sf, a silicon film is also formed on the inner surface of the deposition shield 5, and at this time, the second silicon film Sf2, which has a higher film density, is formed on the surface layer. Therefore, when the silicon film Sf is repeatedly deposited, the number of particles that peel off from the surface layer of the deposition shield 5 and float in the vacuum chamber 1 is reduced, thereby minimizing the number of particles that adhere to the surface of the substrate Sw after deposition. Furthermore, it has been confirmed that the film can be deposited with good film thickness distribution within the surface of the substrate Sw, and that the film can be deposited with almost no difference in film thickness distribution between substrates Sw when the film is repeatedly deposited on multiple substrates Sw.
[0023] To confirm the above-described effects, the following experiment was conducted using the sputtering apparatus SM. In this experiment, a silicon oxide film with a thickness of 100 nm was formed on one side of a silicon wafer used as the substrate Sw, and a silicon film with a thickness of 50 nm was formed on the surface of the silicon oxide film. First, as a preliminary experiment, the pulsed power input to the target 3 was appropriately set to a frequency of 150 kHz and a range of 1 kW to 10 kW, and the argon gas flow rate was appropriately set to a range of 20 sccm to 1000 sccm (the argon partial pressure in the vacuum chamber 1 at this time was in the range of 0.08 to 8 Pa). Silicon films with a thickness of 25 nm were formed on multiple substrates Sw, and sputtering conditions were confirmed that resulted in a refractive index (n value) in the range of 4 to 5 and an extinction coefficient (k value) in the range of 0.3 to 0.6. Although not specifically illustrated or explained, SEM images of the silicon film after film formation confirmed that silicon films having refractive indexes and extinction coefficients both within the above ranges grew in a columnar structure, and that the film density changed depending on the flow rate of argon gas.
[0024] Next, the pulsed power input to the target 3 was set to a frequency of 150 kHz and 4 kW, and the argon gas flow rate was appropriately changed within a range of 30 sccm to 300 sccm. A first silicon film Sf1 was formed as a base layer on a plurality of substrates Sw to a thickness of 25 nm. Then, a second silicon film Sf2 was formed on the surface of the first silicon film Sf1 to a thickness of 25 nm. The sputtering conditions for forming the second silicon film Sf2 were set to a frequency of 150 kHz and 4 kW input to the target 3, and an argon gas flow rate of 70 sccm (hereinafter referred to as "sputtering condition 1"), based on the sputtering conditions confirmed in the above preliminary experiment. According to this, it was confirmed that when the argon gas flow rate was less than 100 sccm, the film stress decreased, and the film stress (MPa) changed depending on the argon gas flow rate. It was also confirmed that the refractive index and extinction coefficient were maintained within the above ranges.
[0025] 3 shows SEM images of the first silicon film Sf1 deposited under sputtering conditions 1 and 2, in which the pulsed power applied to the target 3 was set to a frequency of 150 kHz and 4 kW, and the argon gas flow rate was set to 240 sccm (hereinafter referred to as "sputtering condition 2"). The images show that the first silicon film Sf1 and the second silicon film Sf2 were successively deposited to a thickness of 25 nm under sputtering conditions 1 and 2. The images show that the first silicon film Sf1 and the second silicon film Sf2 each grew to have a columnar structure, with the film density of the first silicon film Sf1 being lower than that of the second silicon film Sf2. It was also confirmed that a similar trend was observed when the power applied to the target 3 was changed while the argon gas flow rate was kept constant.
[0026] Next, an experiment was conducted in which the sputtering time when depositing the first silicon film Sf1 and the second silicon film Sf2 under sputtering conditions 1 and 2 was changed to change the ratio of the film thickness of the first silicon film Sf1 to the film thickness (50 nm) of the entire silicon film Sf. As shown in FIGS. 4(a) and 4(b), it was confirmed that within a film thickness ratio range of 10% to 80%, the refractive index (n value) was in the range of 4 to 5 and the extinction coefficient (k value) was in the range of 0.3 to 0.6, i.e., predetermined optical characteristics were maintained. Furthermore, as shown in FIG. 4(c), it was confirmed that changing the film thickness ratio can change the film stress, and in particular, within a film thickness ratio range of 30% to 80%, it was possible to achieve a small film stress within the range of ±200 MPa. Next, when the first silicon film Sf1 and the second silicon film Sf2 were successively deposited to a film thickness of 25 nm under sputtering conditions 1 and 2, the bias power supplied from the AC power source 8 to the substrate Sw was varied within a range of 40 W to 100 W. As shown in FIG. 5, this shows that the film stress changes in response to the bias power while maintaining predetermined optical characteristics.
[0027] Although the embodiments of the present invention have been described above, various modifications are possible without departing from the scope of the technical concept of the present invention. In the above embodiments, a silicon film was used as an example, but the present invention can also be applied to a stacked film (e.g., a film containing silicon as the main component and containing nitrogen and oxygen) that has a columnar structure and allows film stress to be adjusted by creating density differences while maintaining optical properties. Furthermore, in the above embodiments, the first and second steps are performed consecutively in the same vacuum chamber 1, but the present invention is not limited to this and can also be performed in separate vacuum chambers.
[0028] SM...sputtering device, Sw...substrate (object to be film-formed), Sf...silicon film, Sf1...first silicon film, Sf2...second silicon film, 1...vacuum chamber, 14...mass flow controller (for adjusting the partial pressure of the sputtering gas), 3...silicon target, Ps...sputtering power supply.
Claims
1. A method for depositing a silicon film on a surface of an object by sputtering, comprising: placing a silicon target and an object to be deposited in a vacuum chamber; introducing sputtering gas into the vacuum chamber in a vacuum atmosphere; and applying power to the target, wherein the deposition of the silicon film is carried out in a first process, in which a first silicon film having a columnar structure is deposited; and a second silicon film having a columnar structure and a higher film density than the first silicon film.
2. A film forming method according to claim 1, wherein the partial pressure of the sputtering gas in the vacuum chamber in said first step is set to a reference partial pressure, and the partial pressure of the sputtering gas in said second step is set to be lower than the reference partial pressure.
3. A film forming method according to claim 1, wherein the ratio of the thickness of said first silicon film to that of said silicon film is set in the range of 0.3 to 0.
8.
4. A method for forming a film according to any one of claims 1 to 3, in which a bias power is applied to an object to be film-formed while the silicon film is formed on the surface of the object by a sputtering method, the bias power being set in the range of 20 W to 100 W in the first and second steps.
Citation Information
Patent Citations
Energy device and its manufacturing method
JP2005183364A
Density modulated thin film electrodes, methods of making same, and applications of same
US20160226065A1
Low stress polysilicon film and method for producing same
US6465045B1