Hot stamping component and method of manufacturing the same

The hot stamping part with a zinc-manganese oxide layer and controlled post-treatment layer addresses surface oxidation and manufacturing costs, ensuring improved formability and corrosion resistance in high-strength steel parts.

KR1020260161384APending Publication Date: 2026-11-09HYUNDAE STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020250057751
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-04-30
Publication Date
2026-11-09

AI Technical Summary

Technical Problem

High-strength steel used in hot stamping processes faces challenges such as material fracture, springback, surface oxidation leading to degraded paintability and corrosion resistance, and increased manufacturing costs due to post-treatment processes like shot peening.

Method used

A hot stamping part comprising a steel plate with a zinc-manganese oxide layer and a post-treatment layer, where the oxide layer has a specific thickness and network structure, and a method involving controlled application of a Si-based post-treatment agent to form a uniform layer, enhancing corrosion resistance and paintability.

Benefits of technology

The solution provides hot stamping parts with improved formability, corrosion resistance, and reduced manufacturing costs by preventing surface oxidation and enhancing paint adhesion during the hot stamping process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PAT00003_ABST
    Figure PAT00003_ABST
Patent Text Reader

Abstract

The present invention relates to a substrate comprising, on a plating layer, carbon (C) 0.15 wt% or more and 0.50 wt% or less, silicon (Si) 0.02 wt% or more and 1.00 wt% or less, manganese (Mn) 0.3 wt% or more and 2.0 wt% or less, phosphorus (P) 0 or more and 0.1 wt% or less, sulfur (S) 0 or more and 0.01 wt% or less, titanium (Ti) 0.001 wt% or more and 0.1 wt% or less, niobium (Nb) 0.001 or more and 0.1 wt% or less, chromium (Cr) 0.05 wt% or more and 1.5 wt% or less, boron (B) 0.0001 wt% or more and 0.01 wt% or less, nitrogen (N) 0 or more and 0.01 wt% or less, calcium (Ca) 0.0001 wt% or more and 0.01 wt% or less, and the remainder being iron (Fe) and other unavoidable impurities. A hot stamping part is provided, comprising: a steel plate; a plating layer disposed on the base steel plate; a post-treatment layer disposed on the plating layer; and a Zn-Mn-based oxide layer disposed on the plating layer and disposed in the same layer as the post-treatment layer, wherein the average width of the Zn-Mn-based oxide layer is 10㎛ or more and 30㎛ or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a hot stamping part having excellent formability during hot stamping and a method for manufacturing the same. Background Technology

[0002] With the recent tightening of environmental regulations and safety standards in the automotive industry, the application of high-strength steel for vehicle lightweighting and stability is increasing. While high-strength steel can secure high strength-to-weight ratio characteristics, it can be difficult to form products with complex and precise shapes due to material fracture or springback phenomena occurring during processing.

[0003] Hot stamping is a method to address these issues, and as interest in it grows, research on materials for hot stamping is also actively underway. For example, as disclosed in Korean Patent Publication No. 10-2018-0095757, hot stamping is a forming technology that manufactures high-strength parts by heating a steel plate for hot stamping to a high temperature and then forming and rapidly cooling it simultaneously within a press mold.

[0004] Meanwhile, steel sheets for hot stamping have a problem in that the surface of the steel sheet can oxidize and form scale when heated, which degrades the surface characteristics and paintability of the product and also results in corrosion resistance being inferior to that of plated materials. Therefore, separate processes such as shot blasting or shot peening are required to remove scale after product forming. Alternatively, to prevent the above problems, a method has been used in which an Al-based plating layer is used to suppress the oxidation reaction on the surface of the steel sheet and induce the formation of an Al passivation film to increase the corrosion resistance of the steel sheet. However, in the case of such Al-plated materials, although heat resistance is excellent, there is a problem in that corrosion resistance is inferior compared to Zn-plated materials and manufacturing costs increase.

[0005] However, the paint adhesion and appearance of Zn-based hot stamping steel sheets can be significantly degraded due to the oxidation of Zn that occurs during hot stamping heat treatment. To solve this, post-treatment processes such as shot peening have been introduced, but this results in additional costs and processes, leading to a decrease in productivity. Prior art literature

[0006] (Patent Document 0001) KR 2018-0095757 A The problem to be solved

[0007] The present invention aims to solve various problems, including the problems mentioned above, and can provide a hot stamping part with excellent formability during hot stamping and a method for manufacturing the same.

[0008] However, these tasks are exemplary and do not limit the scope of the invention. means of solving the problem

[0009] According to one aspect of the present invention, a substrate comprising carbon (C) 0.15 wt% or more and 0.50 wt% or less, silicon (Si) 0.02 wt% or more and 1.00 wt% or less, manganese (Mn) 0.3 wt% or more and 2.0 wt% or less, phosphorus (P) 0 or more and 0.1 wt% or less, sulfur (S) 0 or more and 0.01 wt% or less, titanium (Ti) 0.001 wt% or more and 0.1 wt% or less, niobium (Nb) 0.001 or more and 0.1 wt% or less, chromium (Cr) 0.05 wt% or more and 1.5 wt% or less, boron (B) 0.0001 wt% or more and 0.01 wt% or less, nitrogen (N) 0 or more and 0.01 wt% or less, calcium (Ca) 0.0001 wt% or more and 0.01 wt% or less, and the remainder being iron (Fe) and other unavoidable impurities A hot stamping part is provided, comprising: a steel plate; a plating layer disposed on the base steel plate; a post-treatment layer disposed on the plating layer; and a Zn-Mn-based oxide layer disposed on the plating layer and disposed in the same layer as the post-treatment layer, wherein the average width of the Zn-Mn-based oxide layer is 10㎛ or more and 30㎛ or less.

[0010] According to one embodiment, a phosphate may be attached to the surface of the Zn-Mn-based oxide layer.

[0011] According to one embodiment, the Zn-Mn-based oxide layer may have a network structure.

[0012] According to one embodiment, the average thickness of the post-processing layer may be 0.5㎛ or more and 2.0㎛ or less.

[0013] According to one embodiment, the post-treatment layer may comprise silicon (Si) at 15 wt% or more and 50 wt% or less, zinc (Zn) at 0 wt% or more and 15 wt% or less, iron (Fe) at 0 wt% or more and 15 wt% or less, manganese (Mn) at 0 wt% or more and 15 wt% or less, oxygen (O) at 10 wt% or more and 80 wt% or less, and aluminum at 0 wt% or more and 15 wt% or less.

[0014] According to one embodiment, the average thickness of the Zn-Mn-based oxide layer may be thicker than the average thickness of the post-treatment layer.

[0015] According to one embodiment, the average thickness of the Zn-Mn-based oxide layer may be at least twice the average thickness of the post-treatment layer.

[0016] According to one embodiment, the hot stamping part may further include a coating layer located on the post-treatment layer and the Zn-Mn-based oxide layer.

[0017] According to one aspect of the present invention, a method for manufacturing a hot stamping part is provided, comprising: a step of preparing a hot stamping steel plate having a zinc-based plating layer formed thereon; a step of forming a post-treatment layer by applying a Si-based post-treatment agent on the plating layer; a step of heating the hot stamping steel plate having the plating layer and the post-treatment layer formed thereon; a step of transporting the heated hot stamping steel plate; and a step of forming and cooling the transported hot stamping steel plate; wherein, in the step of forming the post-treatment layer, the production speed ratio (R) of the steel plate when applying the post-treatment agent satisfies the following Equation 1.

[0018] [Equation 1]

[0019] 0.85 ≤ R ≤ 2.0 (where R = V A / V B am.)

[0020] (At this time, V A is the driving speed of the applicator roll (unit: rpm), and V B is the steel plate production speed (unit: mpm).

[0021] According to one embodiment, in the step of forming the post-treatment layer, the driving speed of the applicator roll applying the post-treatment agent may be 60 rpm or less.

[0022] According to one embodiment, in the step of forming the post-treatment layer, the post-treatment agent may comprise a silane-based solid content of 5% by weight or more and 20% by weight or less, a binder of 1% by weight or more and 10% by weight or less, formic acid of 1% by weight or more and 10% by weight or less, and a solvent of 60% by weight or more and 80% by weight or less.

[0023] According to one embodiment, in the step of forming the post-treatment layer, the silane-based solid may include at least one of trimethoxymethylsilane, tetraethoxysilane, and triethoxy-[3-(oxiranylmethoxy)propyl]silane.

[0024] According to one embodiment, in the step of forming the post-treatment layer, the amount of the post-treatment agent attached is 1300 mg / m² per piece. 2 to 2000 mg / m² 2 It could be.

[0025] According to one embodiment, in the step of forming the post-treatment layer, the production speed of the steel plate forming the post-treatment layer may be 30 mpm or more and 150 mpm or less.

[0026] According to one embodiment, in the step of heating the steel plate for hot stamping, a network of cracks may be formed in the post-treatment layer, and a Zn-Mn-based oxide layer may be formed in the portion where the cracks are formed.

[0027] According to one embodiment, the method for manufacturing the hot stamping part may further include a phosphate treatment step to attach a phosphate to the Zn-Mn-based oxide layer.

[0028] According to one embodiment, the average thickness of the post-processing layer may be 0.5㎛ or more and 2.0㎛ or less.

[0029] Other aspects, features, and advantages other than those described above will become clear from the following specific details, claims, and drawings for implementing the invention. Effects of the invention

[0030] According to one embodiment of the present invention as described above, a hot stamping part having excellent formability during hot stamping and a method for manufacturing the same can be provided. Of course, the scope of the present invention is not limited by such effects. Brief explanation of the drawing

[0031] FIG. 1 is a flowchart schematically illustrating a method for manufacturing a steel plate for hot stamping according to one embodiment of the present invention. FIG. 2 is a flowchart schematically illustrating a method for manufacturing a hot stamping part using the hot stamping steel plate of FIG. 1. Figure 3 is an SEM image showing a cross-section of a hot-stamped part after the hot-stamping process. FIG. 4 is an SEM image showing the surface of a hot stamping part according to one embodiment of the present invention. Figure 5 is an image showing the results of the EDITIONal Spectroscopic Analysis (EDS) of the SEM image in Figure 4. Figure 6 shows SEM images of surface cracks in the post-treatment layer according to the amount of post-treatment agent applied. Figure 7 is an SEM image showing the surface of a hot stamping part after phosphate treatment. FIGS. 8A and FIGS. 8B are surface images showing the evaluation of coating adhesion of experimental examples of the present invention. Specific details for implementing the invention

[0032] The present invention will be described in detail below. However, in describing the present invention, if it is determined that a detailed description of related known technologies or configurations may unnecessarily obscure the essence of the present invention, such detailed description will be omitted.

[0033] In the following embodiments, terms such as first, second, etc. are used not in a limiting sense, but for the purpose of distinguishing one component from another component.

[0034] In the following examples, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0035] In the following embodiments, when various components such as layers, films, regions, and plates are described as being "on" another component, this includes not only cases where they are "directly on" another component, but also cases where another component is interposed between them.

[0036] In the drawings, the size of components may be exaggerated or reduced for convenience of explanation. For example, the size and thickness of each component shown in the drawings are depicted arbitrarily for convenience of explanation, and therefore the present invention is not necessarily limited to what is illustrated.

[0037] In the following embodiments, terms such as "include" or "have" mean that the features or components described in the specification are present, and do not preclude the possibility that one or more other features or components may be added.

[0038] In this specification, "A and / or B" indicates the case where it is A, B, or both A and B. Additionally, in this specification, "at least one of A and B" indicates the case where it is A, B, or both A and B.

[0039] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.

[0040] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0041] FIG. 1 is a flowchart schematically illustrating a method for manufacturing a steel plate for hot stamping according to one embodiment of the present invention, and FIG. 2 is a flowchart schematically illustrating a method for manufacturing a hot stamping part using the steel plate for hot stamping of FIG. 1.

[0042] Referring to FIG. 1, a method for manufacturing a steel sheet for hot stamping according to one embodiment of the present invention may include a hot rolling step (S110), a cold rolling step (S120), an annealing heat treatment step (S130), a plating layer forming step (S140), and a post-treatment step (S150).

[0043] In a method for manufacturing a steel plate for hot stamping according to one embodiment of the present invention, the semi-finished product subject to hot rolling may be a slab. The slab in the semi-finished product state can be obtained through a continuous casting process after obtaining molten steel of a predetermined composition through a steelmaking process.

[0044] In one embodiment, the slab comprises carbon (C) 0.15 wt% or more and 0.50 wt% or less, silicon (Si) 0.02 wt% or more and 1.00 wt% or less, manganese (Mn) 0.30 wt% or more and 2.0 wt% or less, phosphorus (P) greater than 0 and 0.1 wt% or less, sulfur (S) greater than 0 and 0.01 wt% or less, titanium (Ti) 0.001 wt% or more and 0.1 wt% or less, niobium (Nb) 0.001 wt% or more and 0.1 wt% or less, chromium (Cr) 0.05 wt% or more and 1.5 wt% or less, boron (B) 0.0001 wt% or more and 0.01 wt% or less, nitrogen (N) greater than 0 and 0.01 wt% or less, calcium (Ca) 0.0001 wt% or more and 0.01 wt% or less, and the remainder being iron (Fe) and other unavoidable It may contain impurities.

[0045] The melting method for manufacturing the slab described above is not limited, and known methods such as blast furnaces, converters, and electric furnaces may be adopted. For example, the slab can be manufactured for continuous casting by extracting iron from raw materials such as iron ore, steel scrap (hereinafter referred to as scrap), and direct reduced iron.

[0046] The following explains the reason why the numerical range of the components included in the base steel plate is limited.

[0047] Carbon (C)

[0048] Carbon is an element that increases the strength of steel and stabilizes austenite. In one embodiment, the carbon content in the base steel sheet may be 0.15 wt% or more and 0.50 wt% or less. If the carbon content in the base steel sheet is less than 0.15 wt%, the strength is reduced, and if the carbon content in the base steel sheet is more than 0.50 wt%, weldability may be reduced.

[0049] Silicon (Si)

[0050] Silicon has an excellent effect on increasing strength, homogenizes the hot stamping structure, and finely disperses ferrite. In one embodiment, the silicon content in the base steel sheet may be 0.02 wt% or more and 1.00 wt% or less. If the silicon content in the base steel sheet is less than 0.02 wt%, the effect on increasing strength is negligible, and if the silicon content in the base steel sheet exceeds 1.00 wt%, the plating quality may deteriorate.

[0051] Manganese (Mn)

[0052] Manganese is an element that increases the strength of steel and stabilizes austenite. In one embodiment, the manganese content in the base steel sheet may be 0.30 wt% or more and 2.0 wt% or less. If the manganese content in the base steel sheet is less than 0.30 wt%, the strength is reduced, and if the manganese content in the base steel sheet is more than 2.0 wt%, the formability and bendability may be reduced.

[0053] Ph(P)

[0054] Phosphorus can reduce weldability and increase the brittleness of the steel sheet. In one embodiment, the phosphorus content in the base steel sheet may be greater than 0 and less than or equal to 0.1 weight%. If the phosphorus content in the base steel sheet exceeds 0.1 weight%, the brittleness may increase, making processing difficult.

[0055] Yellow (S)

[0056] Sulfur can reduce weldability and increase the brittleness of the steel sheet. In one embodiment, the sulfur content in the base steel sheet may be greater than 0 and less than or equal to 0.01 weight%. If the sulfur content in the base steel sheet exceeds 0.01 weight%, the brittleness may increase, making processing difficult.

[0057] Titanium (Ti)

[0058] Titanium can effectively contribute to grain refinement by forming precipitates at high temperatures. In one embodiment, the titanium content in the base steel sheet may be 0.001 wt% or more and 0.1 wt% or less. When titanium is included within the above content range, continuous casting defects and precipitate coarsening can be prevented, the physical properties of the steel can be easily secured, and defects such as crack formation on the surface of the steel can be prevented. If the titanium content is less than 0.001 wt%, it is difficult to sufficiently achieve the grain refinement effect; on the other hand, if the titanium content exceeds 0.1 wt%, precipitates coarsen, which may result in a decrease in elongation and bendability.

[0059] Niobium (Nb)

[0060] Niobium is a powerful carbide-forming element that has a grain refinement effect, such as a reduction in martensite packet size, and has the effect of improving hardenability and increasing the strength of the steel sheet. In one embodiment, the niobium in the base steel sheet may be 0.001 wt% or more and 0.1 wt% or less. When niobium is included in the above range, the grain refinement effect of the steel is excellent during the hot rolling and cold rolling processes, preventing cracking of the slab and brittle fracture of the product during steelmaking / continuous casting, and minimizing the formation of coarse precipitates during steelmaking.

[0061] Chrome (Cr)

[0062] Chromium has a grain refinement effect and improves hardenability and increases the strength of the steel sheet. In one embodiment, the chromium content in the base steel sheet may be 0.05 wt% or more and 1.5 wt% or less. If the chromium content in the base steel sheet is less than 0.05 wt%, sufficient strength cannot be secured, and if the chromium content in the base steel sheet exceeds 1.5 wt%, the toughness of the steel sheet decreases and the manufacturing cost of the steel sheet may increase.

[0063] Boron (B)

[0064] Boron has the effect of improving hardenability and increasing the strength of the steel sheet. In one embodiment, the boron content in the base steel sheet may be 0.0005 wt% or more and 0.005 wt% or less. If the boron content in the base steel sheet is less than 0.0005 wt%, the hardenability may not be sufficient, and if the boron content in the base steel sheet exceeds 0.005 wt%, intergranular brittleness may occur.

[0065] Nitrogen (N)

[0066] Nitrogen is an impurity element that can form coarse nitrides in steel, thereby reducing the toughness of the steel. In one embodiment, the nitrogen content in the base steel sheet may be greater than 0 and less than or equal to 0.01 weight%. If the nitrogen content exceeds 0.01 weight%, it may form coarse nitrides, thereby reducing the toughness of the steel or causing blowholes during spot welding. Additionally, if boron (B) is included in the steel, nitrogen combines with boron to reduce the amount of dissolved boron, thereby deteriorating quenchability; therefore, it is desirable to keep the nitrogen content at 0.01% or less. However, although there is no lower limit for the nitrogen content, removing an excessive amount of nitrogen from the steel would increase manufacturing costs, so it is set to greater than 0.

[0067] Calcium (Ca)

[0068] Calcium is an element that forms sulfides and / or oxides within steel, and it can improve weldability by suppressing the formation of coarse inclusions within the steel. In one embodiment, the calcium content in the base steel plate may be 0.0001 wt% or more and 0.01 wt% or less. When the calcium content in the base steel plate falls within the above range, the occurrence of cracks during spot welding can be effectively suppressed. If the calcium content in the base steel plate exceeds 0.01 wt%, excessive inclusions are generated, making it prone to cracking during spot welding.

[0069] It will be understood by anyone with ordinary knowledge in the technical field to which this invention pertains that, in addition to the components described above, various components (including impurities) included in steel sheets for hot stamping may be included as components of the steel sheets for hot stamping according to the present invention. Combinations of commonly known components and their applications naturally fall within the scope of the rights of this invention.

[0070] Hot rolling step (S110)

[0071] The slab may be reheated for hot rolling prior to the hot rolling step (S110). By reheating the slab, components segregated during casting can be redissolved. The slab reheating temperature (SRT) may be 1150°C to 1350°C. If the slab reheating temperature (SRT) is lower than 1150°C, components segregated during casting may not be sufficiently redissolved, making it difficult to achieve a significant homogenization effect of the alloying elements. On the other hand, if the slab reheating temperature (SRT) is higher than 1350°C, the austenite crystal grain size increases, making it difficult to secure strength, and the manufacturing cost of the steel sheet may increase due to the excessive heating process.

[0072] In the hot rolling step (S110), the reheated slab may be hot rolled at a predetermined finishing delivery temperature (FDT). In one embodiment, the finishing delivery temperature (FDT) may be 800°C to 1000°C. If the finishing delivery temperature (FDT) is lower than 800°C, it is difficult to ensure workability of the steel sheet due to the occurrence of a mixed grain structure caused by rolling in an abnormal region, workability may be reduced due to microstructural non-uniformity, and problems with sheet throughput may occur during hot rolling due to rapid phase changes. On the other hand, if the finishing delivery temperature (FDT) is higher than 1000°C, the austenite grains may coarsen. In addition, there is a risk that the performance of the final part may deteriorate due to the coarsening of TiC precipitates.

[0073] Hot-rolled steel sheets can be coiled after cooling to a predetermined coiling temperature (CT). In one embodiment, the coiling temperature (CT) may be 550°C to 750°C. The coiling temperature (CT) affects the redistribution of carbon (C). If the coiling temperature (CT) is below 550°C, the low-temperature phase fraction increases due to overcooling, which increases strength and may lead to increased rolling load during cold rolling, and may cause a rapid decrease in ductility. On the other hand, if the coiling temperature (CT) exceeds 750°C, deterioration in formability and strength may occur due to abnormal or excessive grain growth.

[0074] Cold rolling step (S120)

[0075] A cold rolling step (S120) may be performed after the hot rolling step (S110). In the cold rolling step (S120), the coiled steel sheet may be uncoiled, pickled, and then cold rolled. At this time, the pickling may be performed for the purpose of removing scale from the coiled steel sheet, that is, the hot-rolled coil produced through the hot rolling process.

[0076] In the cold rolling step (S120), the hot-rolled plate can be cold-rolled to a thickness of 1.0 mm to 2.5 mm. In one embodiment, to impart rollability, the plate temperature (e.g., the temperature of the pre-annealed plate or the hot-rolled plate) may be raised to proceed with warm rolling.

[0077] The reduction rate in the cold rolling step (S120) may be 40% to 70%. If the reduction rate satisfies the above conditions, it is advantageous to induce a texture, and the development of the {111} / / ND texture may be facilitated during subsequent recrystallization heat treatment. If the reduction rate in the cold rolling step (S120) is less than 40%, the {111} / / ND texture may not develop sufficiently, resulting in inferior formability, and if the reduction rate exceeds 70%, the cold rolling load may increase and productivity may decrease.

[0078] Annealing heat treatment step (S130)

[0079] An annealing heat treatment step (S130) may be performed after the cold rolling step (S120). At this time, the annealing heat treatment step (S130) may be referred to as the final annealing step. In the annealing heat treatment step (S130), a cold-rolled annealed sheet may be manufactured by cold-rolling annealing the cold-rolled sheet. The annealing heat treatment step (S130) may be omitted depending on the characteristic requirements of the final product and the step conditions.

[0080] The annealing heat treatment step (S130) can be performed at a temperature that derives the optimal grain size considering mechanical properties.

[0081] In one embodiment, the annealing heat treatment step (S130) may include a step of raising the temperature of the cold-rolled sheet to an annealing temperature of 800°C to 850°C, which is higher than the recrystallization temperature, and a step of cooling the annealed cold-rolled sheet.

[0082] If the annealing temperature is below 800℃, recrystallization may not occur sufficiently, and if the annealing temperature exceeds 850℃, abnormal grain growth may occur, such as a rapid increase in the amount of bainite due to the formation of excessive austenite, and a non-uniform microstructure according to thickness may develop, which may degrade the material properties of the steel sheet. In this case, the heating rate may be 3℃ / s or more and 8℃ / s or less.

[0083] In the aforementioned annealing temperature range, the holding time may be 5 to 70 seconds. If the holding time is less than 5 seconds, grain growth may not occur sufficiently, and the elongation may decrease. On the other hand, if the holding time exceeds 70 seconds, productivity may decrease, and the manufacturing cost may increase.

[0084] The annealing heat treatment step (S130) may be performed in an atmosphere containing a mixed gas to prevent excessive oxidation and nitriding of the surface. By performing the annealing heat treatment step (S130) in an atmosphere containing a mixed gas, a cold-rolled annealed plate with excellent surface condition can be obtained. As an example, the annealing heat treatment step (S130) may be performed in a reducing atmosphere composed of 5% to 30% hydrogen and 70% to 90% nitrogen.

[0085] The steel sheet heated through annealing heat treatment may undergo a cooling step at a predetermined cooling rate in a temperature range of 430°C to 510°C. For example, the cooling rate may be 5°C / s to 30°C / s.

[0086] plating layer formation step (S140)

[0087] In the plating layer formation step (S140), a plating layer can be formed on a cold-rolled annealed plate (i.e., a base steel plate) to manufacture a plated steel plate for hot stamping. In one embodiment, the plating layer may be a zinc-based plating layer. In the plating layer formation step (S140), the cold-rolled annealed plate may be immersed in a plating bath containing a plating solution to form a plating layer on the surface of the cold-rolled annealed plate.

[0088] Specifically, the plating layer formation step (S140) may include a step of forming a molten plating layer on the surface of a steel plate by immersing the steel plate in a plating bath having a temperature of 630°C to 700°C, and a cooling step of forming a plating layer by cooling the steel plate on which the molten plating layer is formed. At this time, the plating bath may include Si, Fe, Al, Mn, Cr, Mg, Ti, Zn, Sb, Sn, Cu, Ni, Co, In, and / or Bi as additive elements, but is not limited thereto. For example, the plating bath may include less than 0.3 weight% aluminum (Al), less than 0.1 weight% iron (Fe), the remainder zinc, and other unavoidable components.

[0089] The thickness of the cold-rolled annealed sheet (i.e., the base steel sheet) on which the plating layer is formed can be between 1.0 mm and 2.5 mm. The thickness of the base steel sheet may be related to the primary heating temperature and the resulting heating time during the hot stamping process described later. If the thickness of the base steel sheet is less than 1.0 mm, it is difficult to secure the heat treatment time during the hot stamping process, and if the thickness of the base steel sheet exceeds 2.5 mm, forming may not be easy during the hot stamping process.

[0090] In one embodiment, the plating deposition amount in the plating layer formation step (S140) is 30 g / m² per side. 2 Up to 100 g / m² 2 It can be controlled to satisfy. The plating deposition amount is 30 g / m² 2 If applied at a thickness less than 100 g / m², corrosion resistance decreases, and the plating thickness is 100 g / m² 2 If it exceeds [value], the increase in zinc scattering during the hot stamping process leads to increased contamination during the heating process and may result in the formation of an uneven plating layer. Additionally, liquid metal embrittlement (LME) may occur during the hot stamping forming stage, which can degrade the toughness and / or ductility of the hot stamped part.

[0091] Through the above processes, the steel sheet for hot stamping according to one embodiment of the present invention may be a hot-dip galvanized steel sheet (e.g., GI steel sheet).

[0092] As an optional embodiment, the plating layer formation step (S140) may include a plating layer alloying step. In this case, an alloyed hot-dip galvanized steel sheet (e.g., GA steel sheet) can be manufactured by alloying the steel sheet on which the plating layer is formed. In one embodiment, in the plating layer alloying step, an alloying heat treatment may be performed by maintaining the temperature at 500°C or higher and 600°C or lower for a time of 10 seconds or more and 60 seconds or less.

[0093] In one embodiment, the plating layer alloying step can be performed continuously after the plating layer formation step (S140). That is, a separate cooling step may not be performed between the plating layer alloying step and the plating layer formation step (S140).

[0094] Under the above conditions, when alloying heat treatment is performed, the plating layer grows stably, and the adhesion of the plating layer can be excellent.

[0095] The hot stamping steel sheet with the plating layer formed in this way may optionally undergo a shot spinning process to remove zinc oxide formed on the surface of the plating layer.

[0096] Post-processing step (S150)

[0097] After the plating layer formation step (S140), a post-treatment step (S150) may be performed. In the post-treatment step (S150), a post-treatment agent is applied to the steel plate on which the plating layer has been formed to form a pre-post-treatment layer, and the steel plate is dried to produce a post-treated steel plate.

[0098] In one embodiment, the post-treatment agent may be an inorganic or organic post-treatment agent. Specifically, the post-treatment agent may be a Si-based inorganic post-treatment agent, an Al-based inorganic post-treatment agent, or a Ca-based inorganic post-treatment agent. In the present invention, by using an inorganic post-treatment agent, the problem of reduced durability caused by chain breakage due to heating during the hot stamping process can be improved when using an organic post-treatment agent containing carbon (C) chains.

[0099] The post-treatment agent according to the present embodiment may use a Si-based post-treatment agent. The Si-based post-treatment agent may comprise a silane-based solid content of 5% by weight or more and 20% by weight or less, a binder of 1% by weight or more and 10% by weight or less, formic acid of 1% by weight or more and 10% by weight or less, a solvent of 60% by weight or more and 80% by weight or less, and other additives. As an example, the silane-based solid content may comprise at least one of trimethoxymethylsilane, tetraethoxysilane, and triethoxy-[3-(oxiranylmethoxy)propyl]silane. Additionally, the binder may comprise 3-(triethoxysilyl)-1-propanamine.

[0100] As described above, by using a post-treatment material having the component ratio within the aforementioned range to form a film such as a post-treatment layer on the surface of the steel plate for hot stamping, i.e., the plating layer, prior to the hot stamping heat treatment process, the oxidation of zinc occurring during the heat treatment process prior to hot stamping can be suppressed, thereby ensuring the corrosion resistance and paintability of the plating layer. That is, by forming a film such as a post-treatment layer on the plating layer on the surface of the steel plate for hot stamping, cracks may be formed in the post-treatment layer during the manufacturing process of the hot stamping part, and paint adhesion can be improved due to the network Zn-Mn-based oxide layer growing from the cracks. However, in the hot stamping steel plate for securing strength according to one embodiment of the present invention, it is difficult to form a uniform thickness of the post-treatment layer due to the difference in flatness between the center and the edge portions during the manufacturing process, and therefore, it was difficult to form a post-treatment layer of a predetermined thickness or more.

[0101] Accordingly, in the manufacturing method according to one embodiment of the present invention, the amount of post-treatment agent applied can be improved by controlling the production speed ratio (R) of the steel plate when applying the post-treatment agent in the post-treatment step (S150). This will be explained in detail through Equation 1 described below.

[0102] In the post-treatment step (S150), the Si-based post-treatment agent can be applied to the hot stamping steel plate (i.e., the plating layer) with a thickness of about 0.5 μm or more to form a pre-post-treatment layer. This can be controlled by a combination of applying a post-treatment attachment roller coater equipment within the range of 110~130% of the post-treatment speed of the APR automotive exterior steel plate, a range of 30~40% of the post-treatment speed of the PUR automotive exterior steel plate, and a pressure within ±300N range during post-treatment of the NIP automotive exterior steel plate. The Si-based post-treatment agent of the present invention must be applied with such an amount to ensure the formability of the hot stamping part according to one embodiment of the present invention described later.

[0103] More specifically, when the Si-based post-treatment agent is applied to the steel plate (i.e., plating layer) in the post-treatment step (S150), the production speed ratio (R) of the steel plate can satisfy the following Equation 1.

[0104] [Equation 1]

[0105] 0.85 ≤ R ≤ 2.0 (where R = V A / V B am.)

[0106] (At this time, V A is the driving speed of the applicator roll (unit: rpm), and V B is the steel plate production speed (unit: mpm).

[0107] In Equation 1, the driving speed (V) of the applicator roll A ) can be expressed by the following Equation 1, and the steel plate production speed (V B ) can be expressed by the following relationship 2.

[0108] [Relationship 1]

[0109] V A = rx 2π x N

[0110] [Relationship 2]

[0111] V B = L / m

[0112] In the above equation 1, r is the radius of the applicator roll, and N is the rotational speed per minute of the applicator roll. In the above equation 2, L / m is the distance traveled per minute (unit: m) of the steel plate.

[0113] In the above Equation 1, if the production speed ratio (R) of the steel plate satisfies a range of 0.85 or higher and 2.0 or lower, the thickness of the post-treatment layer can be easily controlled within the scope of the present invention during the process of applying a post-treatment agent to the steel plate (i.e., the plating layer). When Equation 1 is satisfied, the production speed ratio (R) of the steel plate can be interpreted as being faster than in the conventional method; in other words, this means that the driving speed (V) of the applicator roll A It may mean that the driving speed of the applicator roll (V) has increased. A ) is generally proportional to the thickness of the post-treatment layer, and if the driving speed of the applicator roll becomes faster, more post-treatment agent can be applied to the steel plate (i.e., the plating layer), so the amount of post-treatment agent applied may increase.

[0114] In one embodiment, the driving speed (V) of the applicator roll A ) may be 300 rpm or less, and preferably may be controlled within a range of 24 rpm or more and 300 rpm or less. In addition, the steel plate production speed (V B ) can be controlled within a range of 30 mpm or more and 150 mpm or less.

[0115] In one embodiment, the amount of post-treatment agent applied is 1,300 mg / m² per side. 2 It may be higher, preferably 1,300 mg / m² 2 Above 2,000 mg / m² 2 It may be less than or equal to 1,300 mg / m² of post-treatment agent application amount. 2 If it is less than that, the thickness of the post-treatment layer cannot be sufficiently secured, and the application amount of the post-treatment agent is 2,000 mg / m² 2 If exceeded, the thickness of the post-treatment layer becomes too thick, leading to cracking and delamination due to increased internal stress, and there is a problem of reduced processability during hot stamping.

[0116] The above post-treatment agent may be applied to a steel plate on which a plating layer is formed to form a pre-post-treatment layer, and then a drying step may be performed. The drying step may, for example, be performed at a temperature of 70°C to 150°C, specifically 90°C to 120°C, for 1 to 10 seconds, specifically 3 to 8 seconds. By forming the pre-post-treatment layer on the steel plate on which the plating layer is formed under the aforementioned conditions, excellent paintability is secured, which may be advantageous in terms of rust prevention by preventing exposure to the external environment.

[0117] After that, hot stamping parts can be manufactured by using the above-mentioned post-treated hot stamping steel plate and undergoing a hot stamping process.

[0118] Referring to FIG. 2, a method for manufacturing a hot stamping part according to one embodiment may include a heating step (S210), a transfer step (S220), a forming and cooling step (S230), a phosphate treatment step (S240), and a painting step (S250).

[0119] Heating step (S210)

[0120] In one embodiment, a steel plate (or blank) for hot stamping may be heated in the heating step (S210). At this time, the steel plate for hot stamping may be manufactured through the method for manufacturing a steel plate for hot stamping described above.

[0121] In some embodiments, the heating step (S210) may include a multi-stage heating step and / or a crack heating step. The multi-stage heating step may be a step of heating the steel plate in stages, and the crack heating step may be a step of heating the multi-stage heated steel plate to a uniform temperature. In the multi-stage heating step, the steel plate may be heated in stages as it passes through a plurality of sections provided within the furnace. Among the plurality of sections provided within the furnace, there may be multiple sections where the multi-stage heating step is performed, and the temperature may be set for each section so that the steel plate is heated in stages from the inlet of the furnace into which the steel plate is fed to the outlet of the furnace from which the steel plate is ejected. A crack heating step may be performed after the multi-stage heating step. In the crack heating step, the multi-stage heated steel plate may be heat-treated as it passes through a section of the furnace set to a temperature of approximately Ac3 to approximately 910 °C. Additionally, among the plurality of sections provided within the furnace, there may be at least one section where the crack heating step is performed.

[0122] In one embodiment, in the heating step (S210), a steel sheet for hot stamping can be heat-treated in a heating furnace having a dew point of -30°C or higher and 20°C or lower. Since additional equipment is required to set the dew point to less than -30°C, a problem of increased process costs may occur. If the dew point exceeds 20°C, hydrogen embrittlement of the material may occur due to the influx of hydrogen during hot stamping.

[0123] In the heating step (S210), a steel plate coated with a post-treatment agent can be introduced into a heating furnace and heated. The steel plate for hot stamping can be heated to a target heating temperature in the heating furnace to ensure the material of the steel plate and to prevent the vaporization of the zinc-based plating layer. The heating temperature in the heating furnace is 830°C to 950°C and can be maintained at that temperature for 240 seconds to 400 seconds. If the temperature of the heating furnace is below 830°C, it may be difficult to secure strength because a martensite structure cannot be formed after hot stamping. In addition, if the temperature of the heating furnace exceeds 950°C, a coarse structure may be formed after hot stamping, which may reduce strength.

[0124] During the heating step (S210), the average heating rate of the steel plate in the range where the temperature of the steel plate for hot stamping reaches the target heating temperature from approximately 700°C may be 1.5°C / sec to 7°C / sec. When the average heating rate is 1.5°C / sec to 7°C / sec, the components between the plating layer and the post-treatment layer mutually diffuse, and at the same time, the material properties of the steel plate and the plating layer can be secured. If the heating rate is less than 1.5°C / sec, there are problems of insufficient material properties of the steel plate and reduced productivity, and if the heating rate exceeds 7°C / sec, it is difficult to secure the target plating layer structure due to over-alloying of the plating layer.

[0125] In one embodiment, during the process of performing the heating step (S210), the components of the pre-post-treatment layer containing the post-treatment agent and the plating layer may mutually diffuse to form a mutual diffusion layer at the boundary between the pre-post-treatment layer and the plating layer. The mutual diffusion layer may include Si, Mn, O, Fe, Zn, and SiO.

[0126] Transfer step (S220)

[0127] A transfer step (S220) may be performed after the heating step (S210). The transfer step (S220) may be a step of transferring the heated hot stamping steel plate from the heating furnace to the press mold. At this time, during the transfer step (S220), the heated hot stamping steel plate may be cooled at ambient temperature (or room temperature). That is, the heated hot stamping steel plate may be air-cooled during transfer. In one embodiment, the time taken to remove the heated hot stamping steel plate from the heating furnace and transfer it to the press mold, i.e., the air-cooling time, may be about 5 seconds or more and 20 seconds or less.

[0128] Molding and cooling step (S230)

[0129] After the transfer step (S220), the molding and cooling step (S230) may be performed.

[0130] The forming and cooling step (S230) may be a step of forming a molded body by pressing the transferred hot stamping steel plate with a press mold and simultaneously cooling the transferred hot stamping steel plate. Specifically, in the forming and cooling step (S230), the hot stamping steel plate may be formed into the shape of a hot stamping part by pressing it with a press mold, and at the same time, cooling of the hot stamping steel plate may be achieved as the press mold and the hot stamping steel plate come into contact.

[0131] In one embodiment, the forming start temperature may be 600°C or higher and 800°C or lower. If the forming start temperature is less than 600°C, the forming start temperature is too low, which may reduce the formability of the steel sheet for hot stamping, and the manufactured hot stamping part may not have the target structure and physical properties. On the other hand, if the forming start temperature exceeds 800°C, wrinkles, bends, and / or cracks of a level of about 10 μm or more may occur on the surface of the manufactured hot stamping part due to the Liquid Metal Embrittlement (LME) phenomenon. In addition, the plating layer may adhere to the mold. Therefore, when the forming start temperature satisfies 600°C or higher and 800°C or lower, the formability of the steel sheet for hot stamping may be improved, the manufactured hot stamping part may have the target structure and physical properties, and the occurrence of wrinkles and cracks on the surface of the manufactured hot stamping part may be minimized.

[0132] Cooling of the hot stamping steel plate can be achieved as the press mold presses the hot stamping steel plate and the press mold comes into contact with the hot stamping steel plate. Specifically, the hot stamping steel plate can be cooled simultaneously with forming the hot stamping steel plate into the shape of a hot stamping part in the press mold. The press mold may be equipped with a cooling channel through which a refrigerant circulates. The formed body (e.g., hot stamping steel plate) can be rapidly cooled by the circulation of the refrigerant supplied through the cooling channel provided in the mold. At this time, in order to prevent the spring back phenomenon of the plate material and maintain the desired shape, rapid cooling can be performed while applying pressure with the mold closed.

[0133] In one embodiment, the cooling rate may be 25°C / s or higher. Additionally, the cooling time for the hot stamping steel sheet in the press may be 3 seconds or more and 20 seconds or less. If the cooling rate is too low (less than 25°C / s) or the cooling time is too short (less than 3 seconds), the martensite structure may not be properly formed, and the desired material property standards may not be satisfied. On the other hand, if the cooling time exceeds 20 seconds, productivity may decrease.

[0134] During the process of undergoing the aforementioned heating step (S210) and / or forming and cooling step (S230), network-like cracks may occur in the post-treatment layer formed on the surface of the hot-stamping steel sheet. A network-like Zn-Mn oxide layer may be formed in the areas where cracks have occurred in the post-treatment layer. The Zn-Mn oxide layer is a portion to which phosphate adheres through the phosphate treatment described later, thereby improving paint adhesion. Therefore, in order for sufficient phosphate to be generated, it is important to control the grid width of the network-like Zn-Mn oxide layer to be greater than a predetermined amount.

[0135] Phosphate treatment step (S240) and painting step (S250)

[0136] After the molding and cooling step (S230), a phosphate treatment step (S240) and a painting step (S250) may be performed.

[0137] The phosphate treatment step (S240) may be a step of applying a phosphate to the surface of a hot-stamped part on which a post-treatment layer has been formed to perform a coating treatment. The phosphate applied to the surface of the hot-stamped part may adhere to the Zn-Mn-based oxide layer grown in the cracks of the post-treatment layer. The phosphate may serve to improve surface roughness by forming fine protrusions on the surface of the Zn-Mn-based oxide layer. This can improve adhesion with the coating layer in the subsequent coating step (S250).

[0138] Hot stamping parts

[0139] FIG. 3 is an SEM image showing a cross-section of a hot stamped part after a hot stamping process, and FIG. 4 is an SEM image showing the surface of a hot stamped part according to an embodiment of the present invention. FIG. 5 is an image showing the result of EDS analysis of the SEM image of FIG. 4. The images in FIG. 4 and FIG. 5 are surface images of a hot stamped part prior to the phosphate treatment step (S240) and the coating step (S250).

[0140] Referring to FIG. 3, a hot stamping part (1) according to one embodiment of the present invention comprises a base steel plate (not shown), a plating layer (20) disposed on the base steel plate, and a surface layer (30) disposed on the plating layer (20). The surface layer (30) includes a post-treatment layer (32) disposed in contact with the plating layer (20) and a Zn-Mn-based oxide layer (34) disposed in the same layer as the post-treatment layer (32).

[0141] The base steel plate of the hot stamping part (1) contains carbon (C) 0.15 wt% or more and 0.50 wt% or less, silicon (Si) 0.02 wt% or more and 1.00 wt% or less, manganese (Mn) 0.30 wt% or more and 2.0 wt% or less, phosphorus (P) greater than 0 and 0.1 wt% or less, sulfur (S) greater than 0 and 0.01 wt% or less, titanium (Ti) 0.001 wt% or more and 0.1 wt% or less, niobium (Nb) 0.001 wt% or more and 0.1 wt% or less, chromium (Cr) 0.05 wt% or more and 1.5 wt% or less, boron (B) 0.0001 wt% or more and 0.01 wt% or less, nitrogen (N) greater than 0 and 0.01 wt% or less, calcium (Ca) 0.0001 wt% or more and 0.01 wt% or less, and the remainder of It may contain iron (Fe) and other unavoidable impurities.

[0142] The composition of the base steel plate of the hot stamping part (1) may be similar to the composition of the hot stamping steel plate prior to the hot stamping process described with reference to FIG. 1, but the structure may be different. The structure of the base steel plate after the hot stamping process of the present invention undergoes a phase transformation and may, for example, contain 90% or more of martensite and less than 10% of the remainder, other unavoidable structures and other precipitates. In the following, redundant content regarding the steel composition is omitted.

[0143] The plating layer (20) can be provided on one side or both sides of the base steel plate.

[0144] In one embodiment, the plating layer (20) may be a zinc-based plating layer. That is, the hot stamping steel sheet having a zinc-based plating layer to form a hot stamping part (1) may be, for example, a hot-dip galvanized steel sheet or an alloyed hot-dip galvanized steel sheet. The plating layer (20) may contain iron (Fe) 10 wt% or more and 70 wt% or less, aluminum (Al) greater than 0 and 0.3 wt% or less, manganese (Mn) greater than 0 and 1 wt% or less, silicon (Si) greater than 0 and 1 wt% or less, and the remainder being zinc (Zn) and other impurities.

[0145] In one embodiment, the plating adhesion amount of the plating layer (20) is 30 g / m² per side. 2 Up to 100g / m² 2 It may be. The amount of plating deposited on the plating layer (20) is related to the thickness of the plating layer (20). If the thickness of the plating layer (20) is too thin, it is difficult to ensure sufficient corrosion resistance, and if the plating layer (20) is too thick, the amount of zinc scattering increases during the hot stamping process, and liquid metal embrittlement (LME) may occur during molding, and productivity may also decrease. Therefore, the thickness of the plating layer (20) may be about 10㎛ to 50㎛.

[0146] The surface layer (30) may include a post-treatment layer (32) and a Zn-Mn-based oxide layer (34). The post-treatment layer (32) and the Zn-Mn-based oxide layer (34) are disposed on the plating layer (20) and may be disposed in contact with the plating layer (20). A network-like crack may be formed on the plating layer (20) in the post-treatment layer (32), and the Zn-Mn-based oxide layer (34) may be located within the crack. Figure 5 shows the results of an elemental analysis (EDS) based on the SEM image of Figure 4. The SEM image on the left side of the table in Figure 5 shows a post-treatment agent application amount of 1,500 mg / m² 2 This is the result formed by the above. As shown in FIG. 5, a Si-based post-treatment layer (32) is disposed on the plating layer (20), and it can be seen that a network-like Zn-Mn-based oxide layer (34) is formed in the cracks of the post-treatment layer (32).

[0147] The post-treatment layer (32) can be formed through the aforementioned post-treatment step (S150). The post-treatment layer (32) may include an inorganic post-treatment agent. The inorganic post-treatment agent may be, for example, a Si-based inorganic post-treatment agent, an Al-based inorganic post-treatment agent, or a Ca-based inorganic post-treatment agent.

[0148] For example, when a post-treatment layer (32) is formed using a Si-based inorganic post-treatment agent, the post-treatment layer (32) of the hot stamping part (1) may further include an oxide such as SiO, in which Si, etc. is oxidized compared to the pre-post-treatment layer, and components diffused from the base material (10) and the plating layer (20). For example, the components diffused from the base material (10) and the plating layer (20) may include at least one of O, Mn, Zn, Al, and Fe. For example, the post-treatment layer (32) may include silicon (Si) at 20 wt% or more and 90 wt% or less, zinc (Zn) at 0 wt% or more and 15 wt% or less, iron (Fe) at 0 wt% or more and 15 wt% or less, manganese (Mn) at 0 wt% or more and 15 wt% or less, and oxygen (O) at 10 wt% or more and 80 wt% or less.

[0149] The post-treatment layer (32) is formed on the plating layer (20) to suppress and minimize the formation of a Zn oxide layer, which lowers paint adhesion, by combining the Zn component of the plating layer (20) with oxygen. In this way, the post-treatment layer (32) suppresses the formation of Zn oxide that inhibits binding with the paint layer and induces the formation of a phosphate-attached Zn-Mn oxide layer (34) that improves binding with the paint layer, thereby ultimately improving the paint adhesion of the hot stamping part (1).

[0150] In one embodiment, the average thickness (h1) of the post-treatment layer (32) may be 0.5 μm or more and 3 μm or less, or 0.5 μm or more and 1 μm or less. If the average thickness (h1) of the post-treatment layer (32) is less than 0.5 μm, the thickness of the post-treatment layer is not sufficiently secured, and thus the adhesion of the coating is reduced. If the average thickness of the post-treatment layer (32) exceeds 3 μm, the thickness of the post-treatment layer becomes too thick, causing cracking and peeling due to increased internal stress, and there is a problem of reduced processability during hot stamping molding.

[0151] A Zn-Mn oxide layer (34) can be disposed on the plating layer (20) together with the post-treatment layer (32) and may have a network shape. The Zn-Mn oxide layer (34) can be disposed in contact with the post-treatment layer (32) and the plating layer (20). Referring to FIG. 3, the Zn-Mn oxide layer (34) can be disposed to be in contact with the post-treatment layer (32) on the side and in contact with the plating layer (20) on the bottom. The Zn-Mn oxide layer (34) can grow in the portion where a network crack occurs in the post-treatment layer (32) during the hot stamping heat treatment process. That is, during the hot stamping heat treatment process, a crack occurs in the post-treatment layer (32), and the zinc and manganese of the plating layer (20) exposed to the outside in the portion where the crack occurred are oxidized to form a Zn-Mn oxide layer (34) on the plating layer (20).

[0152] In one embodiment, the average width (W in FIG. 4) of the network-like Zn-Mn oxide layer (34) may be 10 μm or more, preferably 10 μm or more and 30 μm or less. Since the Zn-Mn oxide layer (34) plays an important role in the plating adhesion with the plating layer as described below, it is preferable that the width of the Zn-Mn oxide layer (34) be 10 μm or more. Since the Zn-Mn oxide layer (34) can grow on the cracks of the post-treatment layer (32) as described above, the width of the Zn-Mn oxide layer (34) may be generally the same as the width of the cracks of the post-treatment layer (32). Although the upper limit of the width of the Zn-Mn oxide layer (34) is not particularly limited, it is preferable that the width of the Zn-Mn oxide layer (34) be formed to be 30 μm or less, taking into account the thickness of the post-treatment layer (32).

[0153] In one embodiment, as shown in FIG. 3, the average thickness (h2) of the Zn-Mn oxide layer (34) may be thicker than the average thickness (h1) of the post-treatment layer (32). Additionally, the average thickness (h2) of the Zn-Mn oxide layer (34) may be at least twice the average thickness (h1) of the post-treatment layer (32). For example, the average thickness (h2) of the Zn-Mn oxide layer (34) may be 0.1 μm or more and 10.0 μm or less. Thus, the fact that the thickness (h2) of the Zn-Mn oxide layer (34) is thicker than the thickness (h1) of the post-treatment layer (32) may mean that the Zn-Mn oxide layer (34) protrudes upward above the post-treatment layer (32). In this way, when the Zn-Mn oxide layer (34) protrudes above the post-treatment layer (32), surface roughness may be formed on the surface layer (30) due to the height difference between them. Additionally, since the Zn-Mn oxide layer (34) has phosphate attached to its surface through phosphate treatment to improve the adhesion of the coating layer, it may be more advantageous for the coating adhesion to protrude above the post-treatment layer (32).

[0154] Phosphate can be attached to the surface of the Zn-Mn-based oxide layer (34). Phosphate can be formed through the aforementioned phosphate treatment. By attaching phosphate to the surface of the Zn-Mn-based oxide layer (34), fine protrusions can be formed on the surface of the Zn-Mn-based oxide layer, thereby improving surface roughness. Through this, the adhesion between the hot stamping part (1) and the paint layer can be improved during the process of forming a paint layer on the hot stamping part (1).

[0155] In one embodiment, the paint adhesion between the hot stamping part (1) and the paint layer may be ISO Class 1 or lower and ASTM Class 4B or higher.

[0156] The tensile strength of a hot stamping part (1) according to one embodiment of the present invention having a structural composition as described above may be 1300 MPa or more and 2000 MPa or less. In addition, the yield strength of a hot stamping part (1) according to one embodiment of the present invention may be 900 MPa or more and 1500 MPa or less. In addition, the elongation of a hot stamping part (1) according to one embodiment of the present invention may be 4% or more and 10% or less.

[0157] Hereinafter, the structure and operation of the present invention will be explained in more detail through preferred embodiments of the present invention. However, these are presented as preferred examples of the present invention and should not be interpreted in any way as limiting the present invention.

[0158] Experimental Example

[0159] The present invention will be explained in more detail below through experimental examples. However, the following experimental examples are intended to explain the present invention more specifically, and the scope of the present invention is not limited by the following experimental examples. The following experimental examples may be appropriately modified or changed by those skilled in the art within the scope of the present invention.

[0160] Figure 6 shows SEM images of surface cracks in the post-treatment layer according to the amount of post-treatment agent applied.

[0161] Referring to FIG. 6, specimen (A) has a post-treatment agent application amount of 800 mg / m² 2 This is the result of applying it, and specimen (B) had a post-treatment agent application amount of 1,200 mg / m² 2 This is the result of application, and specimen (C) had a post-treatment agent application amount of 1,500 mg / m² 2 This is the result of applying the method. Specimens (A) and (B) are comparative examples in which the amount of post-treatment agent applied falls outside the scope of the present invention, and Specimens (C) is an example in which the amount of post-treatment agent applied is controlled within the scope of the present invention. In Specimens (A) and (B), cracks occurred in the post-treatment layer, but it can be confirmed that the width of the cracks was formed much narrower than in Specimens (C). In Specimens (A), the average width of the cracks was 1 μm or less, and in Specimens (B), the average width of the cracks was measured to be 5 μm or less. As such, in the case of Specimens (A) and (B) in which the amount of post-treatment agent applied falls below the scope of the present invention, the average width of the cracks occurring in the post-treatment layer is formed very narrowly, and thus the width of the Zn-Mn-based oxide layer growing through the cracks is also formed narrowly. If the width of the Zn-Mn-based oxide layer does not satisfy the scope of the present invention, it may be difficult to secure sufficient paint adhesion.

[0162] Figure 7 is an SEM image showing the surface of a hot stamping part after phosphate treatment.

[0163] Specimens (B') and (C') in Fig. 7 are specimens (B) and (C) in Fig. 6 that have undergone phosphate treatment. It can be confirmed that phosphate is attached to the surface of the surface layer in specimens (B') and (C') of Fig. 7 through phosphate treatment. Phosphate can be attached to the surface of the Zn-Mn-based oxide layer among the surface layers.

[0164] Specimen (B') has a post-treatment agent application amount of 1,200 mg / m² 2As it fell below the scope of the present invention, the width of the Zn-Mn-based oxide layer was 5㎛ or less, thus failing to satisfy the scope of the present invention. On the other hand, specimen (C') had a post-treatment agent application amount of 1,500 mg / m² 2 As the scope of the present invention was satisfied, the width of the Zn-Mn oxide layer was 10 μm or more, satisfying the scope of the present invention. As a result, as shown in the SEM image, it can be confirmed that more phosphate is attached to the surface of specimen (C') compared to the surface of specimen (B'). In this way, the greater the amount of phosphate attached to the surface layer, the greater the surface roughness of the surface layer, and thereby the adhesion of the coating can be improved.

[0166] Evaluation Method

[0167] To prepare the specimens of the examples, a cold-rolled steel sheet having a thickness of 1 mm and containing 0.30 wt% carbon (C), 0.20 wt% silicon (Si), 1.5 wt% manganese (Mn), 0.012 wt% phosphorus (P), 0.002 wt% sulfur (S), 0.05 wt% titanium (Ti), 0.01 wt% niobium (Nb), 0.08 wt% chromium (Cr), 0.002 wt% boron (B), 0.001 wt% calcium (Ca), and the remainder being iron (Fe) and other unavoidable impurities is immersed in an alkaline solution at 50°C for 30 minutes, and then washed with water to remove foreign substances and oil from the surface to prepare the specimen. After annealing the specimen, a plating layer is formed on the surface. The annealing treatment is carried out in a reducing atmosphere composed of 10% to 30% hydrogen and 70% to 90% nitrogen, and the annealing heat treatment temperature is 820℃.

[0168] For plating, the annealed specimen is cooled to the plating bath temperature, immersed in the bath for 2 seconds, and then lifted out. After nitrogen wiping, the plating thickness on one side is 50 g / m² per side. 2The plating bath is cooled to room temperature at a cooling rate of 5°C / sec to 30°C / sec to solidify. At this time, the plating bath temperature is set to 630°C to 700°C. The composition of the plating layer may include iron (Fe) 10 wt% or more and 70 wt% or less, aluminum (Al) greater than 0 and 0.3 wt% or less, manganese (Mn) greater than 0 and 1 wt% or less, silicon (Si) greater than 0 and 1 wt% or less, and the remainder being zinc (Zn) and other impurities, and a zinc-based plating layer is formed by the above process. After that, the alloying of the plating layer is carried out at an alloying temperature of 500°C to 650°C.

[0169] Subsequently, a post-treatment agent is applied onto the plating layer to form a post-treatment layer. The aforementioned Si-based post-treatment agent may be used. At this time, the application amount of the post-treatment agent is 1300 mg / m² per side. 2 , 1400 mg / m 2 , 1500 mg / m 2 The production rate ratio (R) values ​​for Equation 1 were controlled to be 0.85, 1.2, and 1.5, respectively. The thickness of the post-treatment layer formed under these conditions was measured to be 0.5㎛, 0.6㎛, and 0.8㎛, respectively. Accordingly, the average grid width of the network-like Zn-Mn oxide layer was formed to be 10㎛ or more.

[0170] After manufacturing a steel plate for hot stamping under the above conditions, it was maintained at a heat treatment temperature of 870°C for 360 seconds for the hot stamping process. Subsequently, the heated steel plate for hot stamping was hot stamped using a press die to produce a specimen. The forming start temperature was set to 600°C to 800°C, and the average cooling rate was set to 25°C / s or higher.

[0171] After hot stamping, phosphate treatment was performed on the surface of the formed body (i.e., the hot stamped part). After the phosphate treatment, a coating treatment was performed to evaluate paintability.

[0172] In the case of comparative examples, all other conditions were manufactured identically, but at least one of the following conditions was manufactured to be outside the scope of the present invention: the amount of post-treatment agent attached, the production speed ratio (R) according to Equation 1, and the thickness of the post-treatment layer.

[0173] <Method for Evaluating Coat Adhesion>

[0174] In the present invention, a cross-hatch cutter test was performed as a method to evaluate paint adhesion. For the cross-hatch cutter test, a cross-hatch pattern is first formed on the upper surface of a painted specimen using a cutter knife. The cross-hatch area is finished with a brush, and a tape is attached to the cross-hatch area and then peeled off. At this time, the painted area that is peeled off along with the adhesive surface of the tape during the peeling process is evaluated according to ISO and / or ASTM standards. ISO class indicates that ISO class 0 has the best paint adhesion and ISO class 5 has the worst paint adhesion. ASTM class indicates that ASTM class 5B has the best paint adhesion and ASTM class 0B has the worst paint adhesion. In the present invention, ISO Class 1 or lower and ASTM Class 4B or higher were evaluated as having excellent paint adhesion.

[0175] division Production rate ratio (R) Post-treatment agent adhesion amount (mg / m²) 2 ) Post-treatment layer thickness (㎛) Zn-Mn oxide layer width (㎛) Coating Adhesion (ISO / ASTM) Comparative Example 1 0.5 700 0.35 ≤2 Class 4 / Class 1B Comparative Example 2 0.6 800 0.37 ≤2 Class 4 / Class 1B Comparative Example 3 0.7 1000 0.4 ≤4 Class 3 / Class 2B Comparative Example 4 0.8 1250 0.45 ≤6 Class 3 / Class 2B Example 1 0.85 1300 0.5 ≥10 Class 1 / Class 4B Example 2 1.2 1400 0.6 ≥11 Class 1 / Class 4B Example 3 1.5 1500 0.8 ≥13 Class 0 / Class 5B

[0177] Referring to Table 1 above, for Comparative Example 1 and Comparative Example 2, the production rate ratio (R) according to Equation 1 is 0.5 and 0.6, respectively, and the amount of post-treatment agent attached is 700 mg / m², respectively. 2 , 800 mg / m 2Therefore, the scope of the present invention was not satisfied. Accordingly, the thickness of the post-treatment layer was 0.35㎛ and 0.37㎛, respectively, and the width of the Zn-Mn oxide layer was 2㎛ or less, falling below the scope of the present invention. As a result, it can be confirmed that Comparative Example 1 and Comparative Example 2 were found to be very inferior in the coating adhesion evaluation, as ISO Class 4 and ASTM Class 1B.

[0178] In the case of Comparative Examples 3 and 4, the production rate ratio (R) according to Equation 1 was 0.7 and 0.8, respectively, and the amount of post-treatment agent attached was 1000 mg / m², respectively. 2 , 1250 mg / m 2 Therefore, the scope of the present invention was not satisfied. Accordingly, the thickness of the post-treatment layer was 0.4㎛ and 0.45㎛, respectively, and the width of the Zn-Mn oxide layer was 6㎛ or less, falling below the scope of the present invention. As a result, it can be confirmed that Comparative Examples 3 and 4 were inferior to ISO Class 3 and ASTM Class 2B in the coating adhesion evaluation.

[0179] On the other hand, in the case of Examples 1 to 3 of the present invention, the production rate ratio (R) according to Equation 1 is 0.85, 1.2, and 1.5, respectively, and the amount of post-treatment agent attached is 1300 mg / m², respectively. 2 , 1400 mg / m 2 , 1500 mg / m 2 Therefore, the scope of the present invention was satisfied. Accordingly, the thickness of the post-treatment layer was 0.5㎛, 0.6㎛, and 0.8㎛, respectively, and the width of the Zn-Mn oxide layer was 10㎛ or more. As a result, it can be confirmed that Examples 1 to 3 showed excellent results in the coating adhesion evaluation as ISO Class 1 and ASTM Class 4B, or ISO Class 0 and ASTM Class 5B.

[0180] Figures 8a and 8b are images showing the results of the paint adhesion evaluation for Comparative Example 4 and Example 1 of Table 1, respectively. Figure 8a is Comparative Example 4, where the thickness of the post-treatment layer and the resulting width of the Zn-Mn oxide layer fell below the range of the present invention. As described above, the paint adhesion evaluation was ISO Class 3 and ASTM Class 2B, and the experimental results also confirmed that the paint peeled off significantly. On the other hand, Figure 68b is Example 1, where the thickness of the post-treatment layer and the resulting width of the Zn-Mn oxide layer satisfied the range of the present invention. As described above, the paint adhesion evaluation was ISO Class 1 and ASTM Class 4B, and the experimental results also confirmed that paint peeling did not occur at all.

[0181] The embodiments of the present invention are merely illustrative, and those skilled in the art will understand that various modifications and equivalent alternative embodiments are possible therefrom. Accordingly, the true scope of technical protection of the present invention should be determined by the technical spirit of the appended claims. Explanation of the symbols

[0183] 1: Hot stamping parts 20: Plating layer 30: Surface layer 32: Post-processing layer 34: Zn-Mn oxide layer

Claims

Claim 1 A base steel sheet comprising carbon (C) 0.15 wt% or more and 0.50 wt% or less, silicon (Si) 0.02 wt% or more and 1.00 wt% or less, manganese (Mn) 0.3 wt% or more and 2.0 wt% or less, phosphorus (P) 0 or more and 0.1 wt% or less, sulfur (S) 0 or more and 0.01 wt% or less, titanium (Ti) 0.001 wt% or more and 0.1 wt% or less, niobium (Nb) 0.001 or more and 0.1 wt% or less, chromium (Cr) 0.05 wt% or more and 1.5 wt% or less, boron (B) 0.0001 wt% or more and 0.01 wt% or less, nitrogen (N) 0 or more and 0.01 wt% or less, calcium (Ca) 0.0001 wt% or more and 0.01 wt% or less, and the remainder being iron (Fe) and other unavoidable impurities; said base steel sheet A hot stamping part comprising: a plating layer disposed on top; a post-treatment layer disposed on top of the plating layer; and a Zn-Mn-based oxide layer disposed on top of the plating layer and disposed on the same layer as the post-treatment layer, wherein the average width of the Zn-Mn-based oxide layer is 10 μm or more and 30 μm or less. Claim 2 A hot stamping part according to claim 1, wherein a phosphate is attached to the surface of the Zn-Mn-based oxide layer. Claim 3 In paragraph 2, the hot stamping part having a network structure in the Zn-Mn-based oxide layer. Claim 4 A hot stamping part according to claim 1, wherein the average thickness of the post-treatment layer is 0.5㎛ or more and 2.0㎛ or less. Claim 5 A hot stamping part according to claim 1, wherein the post-treatment layer comprises silicon (Si) at 15 wt% or more and 50 wt% or less, zinc (Zn) at 0 wt% or more and 15 wt% or less, iron (Fe) at 0 wt% or more and 15 wt% or less, manganese (Mn) at 0 wt% or more and 15 wt% or less, oxygen (O) at 10 wt% or more and 80 wt% or less, and aluminum at 0 wt% or more and 15 wt% or less. Claim 6 A hot stamping part according to claim 1, wherein the average thickness of the Zn-Mn-based oxide layer is thicker than the average thickness of the post-treatment layer. Claim 7 A hot stamping part according to claim 6, wherein the average thickness of the Zn-Mn-based oxide layer is at least twice the average thickness of the post-treatment layer. Claim 8 In claim 1, the hot stamping part further comprises a coating layer located on the post-treatment layer and the Zn-Mn-based oxide layer. Claim 9 A method for manufacturing a hot stamping part, comprising: a step of preparing a hot stamping steel plate having a zinc-based plating layer formed thereon; a step of forming a post-treatment layer by applying a Si-based post-treatment agent onto the plating layer; a step of heating the hot stamping steel plate having the plating layer and the post-treatment layer formed thereon; a step of transporting the heated hot stamping steel plate; and a step of forming and cooling the transported hot stamping steel plate; wherein, in the step of forming the post-treatment layer, the production speed ratio (R) of the steel plate when applying the post-treatment agent satisfies the following Equation 1. [Equation 1] 0.85 ≤ R ≤ 2.0 (where R = V A / V B is.)(At this time, V A is the driving speed of the applicator roll (unit: rpm), and V B is the steel plate production speed (unit: mpm). Claim 10 A method for manufacturing a hot stamping part according to claim 9, wherein, in the step of forming the post-treatment layer, the driving speed of the applicator roll applying the post-treatment agent is 60 rpm or less. Claim 11 A method for manufacturing a hot stamping part according to claim 9, wherein, in the step of forming the post-treatment layer, the post-treatment agent comprises a silane-based solid content of 5% by weight or more and 20% by weight or less, a binder of 1% by weight or more and 10% by weight or less, formic acid of 1% by weight or more and 10% by weight or less, and a solvent of 60% by weight or more and 80% by weight or less. Claim 12 A method for manufacturing a hot stamping part according to claim 11, wherein, in the step of forming the post-treatment layer, the silane-based solid comprises at least one of trimethoxymethylsilane, tetraethoxysilane, and triethoxy-[3-(oxiranylmethoxy)propyl]silane. Claim 13 In claim 9, in the step of forming the post-treatment layer, the amount of the post-treatment agent attached is 1300 mg / m² per piece. 2 to 2000 mg / m² 2 Method for manufacturing a hot stamping part. Claim 14 A method for manufacturing a hot stamping part according to claim 9, wherein, in the step of forming the post-treatment layer, the production speed of the steel plate forming the post-treatment layer is 30 mpm or more and 150 mpm or less. Claim 15 A method for manufacturing a hot stamping part according to claim 9, wherein, in the step of heating the steel plate for hot stamping, a network of cracks is formed in the post-treatment layer and a Zn-Mn oxide layer is formed in the portion where the cracks are formed. Claim 16 In claim 15, the method for manufacturing the hot stamping part further comprises a phosphate treatment step to attach a phosphate to the Zn-Mn-based oxide layer. Claim 17 A method for manufacturing a hot stamping part according to claim 9, wherein the average thickness of the post-treatment layer is 0.5㎛ or more and 2.0㎛ or less.