Polyurethane water-based dispersions and water-based paints
A polyurethane water-based dispersion with aromatic polyester polyol, carbodiimide, and polyalkylene glycol enhances adhesion and anti-blocking properties, addressing the challenges of polyurethane coatings on resin substrates.
Patent Information
- Application Number
- KR1020267028047
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-15
- Filing Date
- 2025-02-12
- Publication Date
- 2026-11-09
Smart Images

Figure PCT00001 
Figure PCT00002 
Figure PCT00003
Abstract
Description
Technology Field
[0001] An embodiment of the present invention relates to a polyurethane water-based dispersion and an aqueous paint containing the same. Background Technology
[0002] Polyurethane water-based dispersions formed by dispersing a polyurethane resin in a water-based dispersion medium are widely used in paints, inks, adhesives, etc. For example, Patent Document 1 discloses a water-based polyurethane resin composition in which a urethane prepolymer, comprising polyester glycol, an organic diisocyanate, and a chain extender having a free carboxyl group as constituent components, is cross-linked with water, and also discloses a primer composition comprising the composition and a carbodiimide compound.
[0003] Patent Document 2 discloses that a carbodiimide compound is incorporated as an aqueous crosslinking agent together with a polyurethane resin in an aqueous ink layer constituting a laminated film. Prior art literature
[0004] Japanese Published Patent Application No. 2002-302526 Japanese Published Patent Application No. 2021-066031 The problem to be solved
[0005] When a polyurethane water-based dispersion is used as a coating applied to the surface of a resin, such as a polyester resin, it is required that the coating film exhibit good adhesion to the resin substrate. Furthermore, when used as a primer, for example, the coating film requires adhesion to the resin substrate as well as adhesion to the topcoat layer applied through the primer. Thus, for polyurethane water-based dispersions, good adhesion of the coating film to the resin is required. In addition, for polyurethane water-based dispersions, it is desirable to have low tack, that is, anti-blocking properties, when applied to a substrate to form a coating film. Here, anti-blocking properties refer to the performance in which the surfaces of the coating films are difficult to adhere to each other and easy to peel off when substrates with formed coating films are laminated.
[0006] As described above, it is known that a carbodiimide compound is incorporated into a polyurethane water-based dispersion in the past, but, for example, in the one described in Patent Document 1, the amount of carbodiimide compound incorporated was small, so it was not necessarily satisfactory in terms of adhesion to the resin.
[0007] The embodiments of the present invention aim to provide a polyurethane water-based dispersion capable of improving the adhesion and anti-blocking properties of a coating film to a resin, and a water-based paint using the same. means of solving the problem
[0008] The present invention includes embodiments shown below.
[0009] [1] A polyurethane water dispersion formed by dispersing a polyurethane resin (A) containing an aromatic polyester polyol as a component in a water dispersion medium,
[0010] The above polyurethane water-based dispersion comprises a carbodiimide group-containing compound (B), and
[0011] The above polyurethane resin (A) has a carboxyl group, and the acid value of the above polyurethane resin (A) is 5 to 25 mgKOH / g, and
[0012] A polyurethane aqueous dispersion comprising 120 to 300 moles of carbodiimide groups of the carbodiimide group-containing compound (B) for every 100 moles of carboxyl groups of the polyurethane resin (A).
[0013] [2] The above polyurethane resin (A) is a polyurethane water-based dispersion described in [1], which further comprises polyalkylene glycol as a component.
[0014] [3] A polyurethane aqueous dispersion described in [2], wherein the amount of the polyalkylene glycol is 5 to 15 parts by mass per 100 parts by mass of the polyurethane resin (A).
[0015] [4] A polyurethane water-based dispersion described in any one of [1] to [3], wherein the above polyurethane resin (A) further comprises an aromatic ring-containing polyisocyanate as a component.
[0016] [5] A water-based paint comprising a polyurethane water-based dispersion as described in any one of [1] ~ [4].
[0017] [6] A water-based paint used as a primer, as described in [5]. Effects of the invention
[0018] According to an embodiment of the present invention, the adhesion and anti-blocking properties of the coating film to the resin can be improved. Specific details for implementing the invention
[0019] The polyurethane water-based dispersion related to the present embodiment (hereinafter simply referred to as a water-based dispersion) comprises a polyurethane resin (A), a carbodiimide group-containing compound (B), and a water-based dispersion medium (C).
[0020] [Polyurethane Resin (A)]
[0021] Polyurethane resin (A) is obtained by reacting a polyol with a polyisocyanate and is a polymer having urethane bonds within the molecule. In the present embodiment, an aromatic polyester polyol is used as a constituent component of the polyurethane resin (A). By doing so, the effect of improving adhesion to a polyester resin substrate can be enhanced. In the present specification, "included as a constituent component" means using it as a raw material (monomer) for synthesizing the polyurethane resin (A), and the polyurethane resin (A) has a structure derived therefrom.
[0022] Aromatic polyester polyols are polyester polyols having an aromatic ring within the molecule. Polyester polyols are obtained by a condensation reaction between a polycarboxylic acid and a polyhydroxyl group-containing compound, and at least one of the polycarboxylic acid and the polyhydroxyl group-containing compound must contain an aromatic ring.
[0023] As for the polycarboxylic acid, a dicarboxylic acid is preferred, and examples include aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, and aliphatic dicarboxylic acids such as adipic acid, succinic acid, sebacic acid, azelaic acid, maleic acid, and fumaric acid. Any one of these may be used, or two or more may be used in combination.
[0024] As a compound containing a polyhydroxyl group, a diol is preferred, and examples include aliphatic diols such as ethylene glycol, diethylene glycol, propylene glycol, butylene glycol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, and aromatic diols such as bisphenol A, bisphenol F, and their alkylene oxide adducts. Any one of these may be used, or two or more may be used in combination.
[0025] The molecular weight of the aromatic polyester polyol is not particularly limited, and for example, the number average molecular weight (Mn) may be 500 to 5000, 800 to 4000, or 1000 to 3000.
[0026] In this specification, the number average molecular weight (Mn) is a value calculated by measuring by the GPC method (gel permeation chromatography) and using a calibration curve based on standard polystyrene. Specifically, as the conditions for GPC, the column can be measured as "TSKgel G4000HXL + TSKgel G3000HXL + TSKgel G2000HXL + TSKgel G1000HXL + TSKgel G1000HXL" manufactured by Toso Co., Ltd., mobile phase: THF (tetrahydrofuran), mobile phase flow rate: 1.0 mL / min, column temperature: 40 ℃, sample injection volume: 50 μL, and sample concentration: 0.2 mass%.
[0027] The amount of aromatic polyester polyol in the polyol constituting the polyurethane resin (A) is not particularly limited, but, for example, it is preferably 60 to 99 mass% with respect to 100 mass% of polyol, more preferably 70 to 97 mass%, more preferably 75 to 95 mass%, and even more preferably 80 to 90 mass%.
[0028] In this specification, regarding the amount of each component constituting the polyol, the polyol 100 mass% used as a standard is calculated by taking the carboxyl group as an acid when the polyol includes the carboxyl group-containing polyol described below. The amount of the carboxyl group-containing polyol is calculated in the same way by taking the carboxyl group as an acid.
[0029] In this embodiment, the polyurethane resin (A) has a carboxyl group, and thus can form a cross-linked structure by reacting with a carbodiimide group-containing compound (B) when the aqueous dispersion is heated and dried. In this specification, unless specifically mentioned otherwise, the carboxyl group is a concept that includes not only the acid form (-COOH) but also the salt form, i.e., the carboxylate group (-COOX, where X is a cation that forms a salt with a carboxylic acid), and the acid form and the salt form may be mixed.
[0030] Examples of salts of carboxylate groups include alkali metal salts such as sodium salts and potassium salts, alkaline earth metal salts such as magnesium salts and calcium salts, ammonium salts, amine salts (primary amine salts, secondary amine salts, tertiary amine salts), and quaternary ammonium salts. Among these, it is preferable to use a salt of a volatile base such as an ammonium salt or an amine salt. If it is a volatile base, the carboxyl group is easily converted into an acidic form by evaporation during the heating and drying of the aqueous dispersion, and the reactivity with the carbodiimide group-containing compound (B) is improved, thereby enhancing the effect of improving the adhesion of the coating film to the resin.
[0031] In this embodiment, the acid value of the polyurethane resin (A) is 5 to 25 mgKOH / g. Since the acid value is 5 mgKOH / g or higher, it becomes easier to emulsify the polyurethane resin (A) into a water-based dispersion medium. Since the acid value is 25 mgKOH / g or lower, the adhesion of the coating film to the resin can be improved. The acid value of the polyurethane resin (A) is more preferably 7 to 20 mgKOH / g, and even more preferably 10 to 15 mgKOH / g.
[0032] In the present specification, the acid value can be obtained from the amount of KOH (mg) required to neutralize the carboxyl groups contained in 1 g of polyurethane resin (A) in accordance with JIS K0070-1992.
[0033] In order to introduce carboxyl groups into the polyurethane resin (A), it is preferable to use a carboxyl group-containing polyol along with an aromatic polyester polyol in the polyol used to synthesize the polyurethane resin (A). That is, it is preferable that the polyurethane resin (A) includes a carboxyl group-containing polyol as a component.
[0034] Examples of carboxyl group-containing polyols include carboxylic acid-containing compounds such as dimethylolpropionic acid, 2,2-dimethylolbutyric acid, 2,2-dimethylolvaleric acid, dihydroxymaleic acid, 2,6-dihydroxybenzoic acid, and tartaric acid, as well as derivatives thereof and salts thereof. Any one of these may be used, or two or more may be used in combination.
[0035] The amount of carboxyl group-containing polyol in the polyol is not particularly limited and, for example, may be 0.5 to 15 mass%, 1 to 10 mass%, or 2 to 7 mass% with respect to 100 mass% of the polyol.
[0036] As a polyol used to synthesize the polyurethane resin (A), polyalkylene glycol may additionally be used. That is, it is preferable that the polyurethane resin (A) additionally include polyalkylene glycol as a component. By including polyalkylene glycol, for example, when a polyurethane aqueous dispersion is used as a primer, the adhesion to the top layer can be improved when the resin constituting the top layer includes polyalkylene glycol as a component.
[0037] Examples of polyalkylene glycols include polyethylene glycol, polytrimethylene glycol, polypropylene glycol, polytetramethylene glycol, polybutylene glycol, and copolymers using two or more of the constituent monomers thereof. The molecular weight of the polyalkylene glycol is not particularly limited, and for example, the number average molecular weight (Mn) may be 500 to 5000, 800 to 4000, or 1000 to 3000.
[0038] The amount of polyalkylene glycol in the polyurethane resin (A) (i.e., the amount of structure derived from polyalkylene glycol) is preferably 5 to 15 parts by mass per 100 parts by mass of the polyurethane resin (A), more preferably 7 to 13 parts by mass, and even more preferably 8 to 10 parts by mass. The amount of polyalkylene glycol in the polyol is not particularly limited and, for example, may be 3 to 25 parts by mass, 5 to 20 parts by mass, or 10 to 15 parts by mass per 100 parts by mass of the polyol.
[0039] As a polyol used to synthesize a polyurethane resin (A), a polyol having three or more functional groups may be used. As a polyol having three or more functional groups, low molecular weight polyhydric alcohols (preferably trihydric alcohols) such as trimethylolpropane, glycerin, and pentaerythritol are preferably exemplified. The amount of such polyol with three or more functional groups is not particularly limited and, for example, may be 0.1 to 5 mass%, 0.2 to 3 mass%, or 0.3 to 1 mass% with respect to 100 mass% of the polyol.
[0040] Polyols other than those mentioned above may be used for synthesizing polyurethane resin (A). Examples of such other polyols include polymer polyols such as aliphatic polyester polyols, polycarbonate polyols, polyether polyols other than polyalkylene glycol, and polybutadiene polyols. Other polyols may also include low molecular weight diols such as ethylene glycol, propylene glycol, propanediol, butanediol, pentanediol, 3-methyl-1,5-pentanediol, hexanediol, neopentyl glycol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, bisphenol A, bisphenol F, bisphenol S, and hydrogenated bisphenol A. Any one of these other polyols may be used, or two or more may be used in combination.
[0041] The amount of polyol constituting the polyurethane resin (A) (i.e., the amount of structure derived from the polyol) is not particularly limited, and for example, 70 to 90 parts by mass may be added, or 75 to 85 parts by mass may be added, for every 100 parts by mass of the polyurethane resin (A).
[0042] Examples of polyisocyanates used to synthesize polyurethane resin (A) include aromatic polyisocyanates, aromatic aliphatic polyisocyanates, aliphatic polyisocyanates, and alicyclic polyisocyanates.
[0043] Examples of aromatic polyisocyanates include diphenylmethane diisocyanate (MDI), polymeric MDI, tolylene diisocyanate (TDI), naphthalene diisocyanate, and their modified forms such as isocyanurate, adduct, biuret, allophanate, and carbodiimide.
[0044] Examples of aromatic aliphatic polyisocyanates include xylylene diisocyanate (XDI), ω,ω'-diisocyanate-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanate-1-methylethyl)benzene and their modified forms such as isocyanurates, adducts, biurets, allophanates, and carbodiimides.
[0045] Examples of aliphatic polyisocyanates include tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate (HDI), 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, and their modified forms such as isocyanurate, adduct, biuret, allophanate, and carbodiimide.
[0046] Examples of cycloaliphatic polyisocyanates include isophorone diisocyanate (IPDI), dicyclohexylmethane 4,4'-diisocyanate (hydrogenated MDI), hydrogenated xylylene diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, and their modified forms such as isocyanurates, adducts, biurets, allophanates, and carbodiimides.
[0047] These polyisocyanates may be used in any one type, or two or more types may be used in combination.
[0048] As for the polyisocyanate, among the above, it is preferable to use an aromatic ring-containing polyisocyanate, such as an aromatic polyisocyanate or an aromatic aliphatic polyisocyanate, in order to have an excellent effect of improving anti-blocking properties, and more preferably, an aromatic aliphatic polyisocyanate is used. The amount of aromatic ring-containing polyisocyanate relative to 100 mass% of polyisocyanate is not particularly limited and, for example, may be 50 mass% or more, 70 mass% or more, 90 mass% or more, or 100 mass%.
[0049] The amount of polyisocyanate constituting the polyurethane resin (A) (i.e., the amount of structure derived from polyisocyanate) is not particularly limited, and for example, 10 to 30 parts by mass may be added per 100 parts by mass of the polyurethane resin (A), or 15 to 25 parts by mass may be added.
[0050] In one embodiment, the following (A1) and (A2) may be used as polyurethane resins (A).
[0051] (A1) An anionic polyurethane resin formed by reacting a polyol containing an aromatic polyester polyol and a carboxyl group-containing polyol with a polyisocyanate to synthesize an isocyanate group-containing urethane prepolymer, and then extending the chain of the urethane prepolymer using a chain extender.
[0052] (A2) A hydroxyl group-containing anionic polyurethane resin obtained by reacting a polyol containing an aromatic polyester polyol and a carboxyl group-containing polyol with a polyisocyanate.
[0053] [Carbodiimide group-containing compound (B)]
[0054] The carbodiimide group-containing compound (B) is a compound containing a carbodiimide group (-N=C=N-) within its molecule and reacts with the carboxyl group of the polyurethane resin (A).
[0055] Examples of carbodiimide group-containing compounds (B) include carbodiimide group-containing compounds used as aqueous crosslinking agents. Preferably, it is a polycarbodiimide that is a polymer having carbodiimide groups in its molecule, and more preferably, it is an aqueous polycarbodiimide in which a hydrophilic segment is introduced to a polycarbodiimide having multiple carbodiimide groups in its molecule. Examples of such aqueous polycarbodiimides include, for instance, "Carbodilite V-02," "Carbodilite V-02-L2," "Carbodilite SV-02," "Carbodilite V-04," and "Carbodilite V-10" as water-soluble types, and "Carbodilite E-02" and "Carbodilite E-05" as emulsion / dispersion types (all manufactured by Nisshinbo Chemical Co., Ltd.).
[0056] The NCN equivalent of a carbodiimide group-containing compound is not particularly limited and, for example, may be 300 to 600 or 350 to 500. Here, the NCN equivalent refers to the chemical formula weight per mole of carbodiimide group.
[0057] [Aqueous dispersion medium (C)]
[0058] An aqueous dispersion medium is a dispersion medium containing water, and may be a medium of water or a mixture of water and a hydrophilic organic solvent. From the perspective of dispersion stability of an aqueous dispersion, water is preferred for the aqueous dispersion medium, and while an organic solvent may be included, it is preferable that it be in a small amount. In one embodiment, the aqueous dispersion medium preferably contains 70 mass% or more of water, more preferably 80 mass% or more of water, and even more preferably 90 mass% or more of water, and may contain 100 mass% of water. That is, in the aqueous dispersion medium, the water / hydrophilic organic solvent ratio is preferably 70 / 30 to 100 / 0 by mass, more preferably 80 / 20 to 100 / 0, and even more preferably 90 / 10 to 100 / 0.
[0059] Various organic solvents that are soluble in water are used as hydrophilic organic solvents, such as lower monohydric alcohols like methanol, ethanol, and propanol, polyhydric alcohols like ethylene glycol and glycerin, and non-protonic polar solvents like N-methylpyrrolidone, dimethyl sulfoxide, dimethylformamide, and acetonitrile.
[0060] [Polyurethane Water-based Dispersion]
[0061] The polyurethane water-based dispersion is a water-based dispersion formed by dispersing a polyurethane resin (A) in a water-based dispersion medium (C), and includes a carbodiimide group-containing compound (B). By incorporating the carbodiimide group-containing compound (B) into the water-based dispersion of the polyurethane resin (A) in this way, the adhesion of the coating film to the resin can be improved.
[0062] In this embodiment, the amount of the carbodiimide group-containing compound (B) in the aqueous dispersion is set as follows. That is, the aqueous dispersion contains 120 to 300 moles of carbodiimide groups of the carbodiimide group-containing compound (B) for every 100 moles of carboxyl groups of the polyurethane resin (A).
[0063] As described above, after making the acid value of the polyurethane resin (A) relatively small, the number of moles of carbodiimide groups is set to an excess amount relative to the number of moles of carboxyl groups (specifically, a molar ratio of 1.2 times or more), so that carbodiimide groups remain in the coating film after curing. The adhesion of the coating film to the resin can be improved by these remaining carbodiimide groups, and in particular, the adhesion to the top layer can be improved. It is thought that the remaining carbodiimide groups contribute to the adhesion to the acrylate resin included in the top layer, but this is not limited thereto. In addition, the anti-blocking properties can be improved by having 300 moles or less of carbodiimide groups. The amount of carbodiimide groups per 100 moles of carboxyl groups is more preferably 130 to 280 moles, more preferably 150 to 250 moles, and even more preferably 180 to 220 moles.
[0064] The content of polyurethane resin (A) in the polyurethane water-based dispersion is not particularly limited and, for example, may be 5 to 50 mass%, 7 to 40 mass%, 10 to 30 mass%, or 15 to 25 mass% with respect to the total mass of the water-based dispersion.
[0065] The particle size of the polyurethane resin (A) in the polyurethane water-based dispersion is not particularly limited, and, for example, the average particle size may be 0.001 to 0.5 μm. Here, the average particle size is the 50% cumulative particle size (d50) measured using the "Microtrac UPA-UZ152" manufactured by Nikkiso Co., Ltd.
[0066] The polyurethane aqueous dispersion may include other components as long as the effect is not impaired. The other components may be included in the resin particles as the dispersion, or they may be included in a state separately dispersed or dissolved in the aqueous dispersion medium. For example, in the polyurethane aqueous dispersion, the resin particles as the dispersion may consist only of polyurethane resin (A), but may also consist of other components together with the polyurethane resin (A). Additionally, the polyurethane aqueous dispersion may include a surfactant for dispersing the polyurethane resin (A) in the aqueous dispersion medium (C). Furthermore, the carbodiimide group-containing compound (B) may be included in the resin particles, but in the case of the above-mentioned aqueous polycarbodiimide, it may be included in a state separately dispersed or dissolved in the aqueous dispersion medium.
[0067] [Method for manufacturing an aqueous dispersion]
[0068] The method for manufacturing the polyurethane water-based dispersion related to the present embodiment is not particularly limited. In one embodiment, the water-based dispersion containing the anionic polyurethane resin of (A1) may be manufactured by the following processes (a1) to (a5).
[0069] Process (a1): A process for synthesizing an isocyanate-containing urethane prepolymer by reacting a polyol containing an aromatic polyester polyol and a carboxyl group-containing polyol with a polyisocyanate.
[0070] Process (a2): A process for neutralizing the carboxyl groups of an isocyanate-containing urethane prepolymer.
[0071] Process (a3): A process of dispersing an isocyanate group-containing urethane prepolymer in an aqueous dispersion medium.
[0072] Process (a4): A process of extending the chain of an isocyanate-containing urethane prepolymer using a chain extender.
[0073] Process (a5): A process of mixing a carbodiimide group-containing compound (B) into an aqueous dispersion containing an anionic polyurethane resin after chain elongation.
[0074] In the above process (a1), the polyisocyanate may be used such that the isocyanate group is stoichiometrically in excess of the amount of hydroxyl group contained in the polyol, for example, the equivalent ratio of the hydroxyl group to the isocyanate group (NCO / OH) is 1.05 to 1.70 (more preferably 1.10 to 1.60).
[0075] In addition, in process (a1), the reaction between the polyol and the polyisocyanate may be carried out without an organic solvent, or in an organic solvent that does not have active hydrogen groups, such as methyl ethyl ketone or acetone.
[0076] In the above process (a2), bases that neutralize the carboxyl group may include, for example, non-volatile bases such as sodium hydroxide and potassium hydroxide, tertiary amines such as trimethylamine, triethylamine, dimethyl ethanolamine, methyl diethanolamine, and triethanolamine, and volatile bases such as ammonia.
[0077] In the above process (a3), the method of dispersing the urethane prepolymer in the aqueous dispersion medium is not particularly limited, and examples include (i) a method of adding the urethane prepolymer or its solution while stirring the aqueous dispersion medium with a homogenizer or homomixer, etc., and (ii) a method of adding the aqueous dispersion medium while stirring the urethane prepolymer or its solution with a homogenizer or homomixer, etc.
[0078] In the above process (a4), the chain extender is not particularly limited and may be water, for example, polyhydrazide compounds such as aliphatic polyamine compounds (e.g., ethylenediamine, trimethylenediamine, propylenediamine, diethylenetriamine, triethylenetetramine), aromatic polyamine compounds (e.g., metaxylylenediamine, tolylenediamine, diaminodiphenylmethane), alicyclic polyamine compounds (e.g., piperazine, isophoronediamine), and polyhydrazide compounds (e.g., hydrazine, adipic acid dihydrazide).
[0079] The neutralization of process (a2), the dispersion of process (a3), and the chain extension of process (a4) may be carried out in this order, but two or more processes may be carried out simultaneously. For example, when ammonia water is used for the neutralization of the carboxyl group, dispersion into an aqueous dispersion medium may be carried out simultaneously with the neutralization, and chain extension with water may also be carried out. Additionally, when the reaction between the polyol and the polyisocyanate in process (a1) is carried out in an organic solvent, the organic solvent may be removed after dispersion into an aqueous dispersion medium in process (a4).
[0080] In one embodiment, the aqueous dispersion containing the anionic polyurethane resin of (A2) may be manufactured by the following processes (b1) to (b4).
[0081] Process (b1): A process for synthesizing a hydroxyl group-containing polyurethane resin by reacting a polyol containing an aromatic polyester polyol and a carboxyl group-containing polyol with a polyisocyanate.
[0082] Process (b2): A process for neutralizing the anionic groups of a hydroxyl group-containing polyurethane resin.
[0083] Process (b3): A process of dispersing a hydroxyl group-containing polyurethane resin in an aqueous dispersion medium.
[0084] Process (b4): A process of mixing a carbodiimide group-containing compound (B) into an aqueous dispersion containing a hydroxyl group-containing polyurethane resin.
[0085] In the above process (b1), the polyol is used such that the hydroxyl group is stoichiometrically in excess of the isocyanate group contained in the polyisocyanate, for example, the equivalent ratio of the hydroxyl group to the isocyanate group (NCO / OH) is 0.70 to 0.95 (more preferably 0.75 to 0.90).
[0086] The neutralization of process (b2) and the dispersion of process (b3) may be carried out in this order, but may also be carried out simultaneously. For example, when ammonia water is used for the neutralization of the carboxyl group, the dispersion into an aqueous dispersion medium may be carried out simultaneously with the neutralization. Additionally, when the reaction between the polyol and the polyisocyanate in process (b1) is carried out in an organic solvent, the organic solvent may be removed after dispersion into an aqueous dispersion medium in process (b3).
[0087] [Water-based paint]
[0088] The aqueous paint related to the present embodiment comprises the above-described polyurethane aqueous dispersion, and thus comprises an aqueous dispersion medium (C), a polyurethane resin (A) dispersed in the aqueous dispersion medium, and a carbodiimide group-containing compound (B). The aqueous paint can be applied to various substrates such as resin substrates or metal substrates, but since the aqueous dispersion has excellent adhesion of the coating film to the resin as described above, it is preferably used as an aqueous paint for application to a substrate whose surface is made of resin. More preferably, it is an aqueous paint for application to a polyester resin substrate such as a PET film. Here, the substrate may be a film or a plate-shaped substrate, and the shape, such as thickness, is not particularly limited.
[0089] In one embodiment, the water-based paint may be a primer paint used as a primer. For example, it may be used as a primer layer of a laminate formed by applying the water-based paint related to this embodiment onto a resin substrate, such as a polyester resin substrate, to form a coating film, and then applying a UV-curing resin (UV-curing resin) as a topcoat layer onto the coating film to form a UV-curing resin layer. An optical film may be cited as an example of an application for the laminate. The coating film formed by the water-based paint related to this embodiment has excellent adhesion to the resin substrate, such as a polyester resin, as well as excellent adhesion to the UV-curing resin. Therefore, it is preferred for use as such a primer.
[0090] The UV-curing resin constituting the top layer is not particularly limited, and examples include acrylate resins such as epoxy acrylate, urethane acrylate, and polyester acrylate. In one embodiment, a UV-curing resin containing polyalkylene glycol as a component may be used.
[0091] In the water-based paint, other water-based resins that are generally used as film-forming components of water-based paints may be used in combination with the polyurethane resin (A), or not used in combination. Examples of other water-based resins include water-soluble or water-dispersible acrylic resins, water-soluble or water-dispersible polyester resins, water-soluble or water-dispersible alkyd resins, water-soluble or water-dispersible cellulose resins, etc.
[0092] The content of the polyurethane resin (A) and the carbodiimide group-containing compound (B) in the water-based paint is not particularly limited, and for example, with respect to 100 mass% of the total resin solid content included in the water-based paint, the sum of both may be 20 to 100 mass% or 50 to 100 mass%.
[0093] Water-based paints may also be formulated with various additives that are generally incorporated into water-based paints, provided that their effects are not impaired. Examples of such additives include pigments, ultraviolet absorbers, light stabilizers, surface modifiers, inorganic fillers, organic fillers, dispersion aids, preservatives, rust inhibitors, antioxidants, silane coupling agents, defoaming agents, viscosity modifiers, antistatic agents, crosslinking agents, organic solvents, etc.
[0094] Examples
[0095] The present invention will be described in more detail below based on examples and comparative examples, but the invention is not limited thereto.
[0096] The details of each component used in the examples are as follows.
[0097] [Polyol]
[0098] · Aromatic polyester polyol 1: number of functional groups 2, number average molecular weight 1000, solid content 70 mass%, diluent solvent MEK. The synthesis method is as follows.
[0099] 16.2 parts by mass of succinic anhydride and 83.8 parts by mass of bisphenol A ethylene oxide adduct ("Nyupol BPE-20NK" manufactured by Sanyo Chemical Industry Co., Ltd.) were added to a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank, and a nitrogen gas inlet tube, and the temperature was raised to 250°C while stirring under a nitrogen stream. The reaction was carried out until the acid value became 5 mgKOH / g or less (2.92 parts by mass of distilled water), and after cooling to 70°C, 41.61 parts by mass of methyl ethyl ketone were added to obtain aromatic polyester polyol 1.
[0100] · Aromatic polyester polyol 2: number of functional groups 2, number average molecular weight 2000, solid content 70 mass%, diluent solvent MEK. The synthesis method is as follows.
[0101] 19.9 parts by mass of succinic anhydride and 80.1 parts by mass of bisphenol A ethylene oxide adduct ("Nyupol BPE-20NK" manufactured by Sanyo Chemical Industry Co., Ltd.) were added to a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank, and a nitrogen gas inlet tube, and the temperature was raised to 250°C while stirring under a nitrogen stream. The reaction was carried out until the acid value became 5 mgKOH / g or less (3.58 parts by mass of distilled water), and after cooling to 70°C, 41.32 parts by mass of methyl ethyl ketone were added to obtain aromatic polyester polyol 2.
[0102] · Aromatic polyester polyol 3: number of functional groups 2, number average molecular weight 1000, solid content 70 mass%, diluent solvent MEK. The synthesis method is as follows.
[0103] 40.9 parts by mass of isophthalic acid, 19.89 parts by mass of adipic acid, 25.14 parts by mass of neopentyl glycol, and 14.07 parts by mass of ethylene glycol were added to a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank, and a nitrogen gas inlet tube, and the temperature was raised to 250 °C while stirring under a nitrogen stream. The reaction was carried out until the acid value became 5 mgKOH / g or less (13.76 parts by mass of distilled water), and after cooling to 70 °C, 36.96 parts by mass of methyl ethyl ketone were added to obtain aromatic polyester polyol 3.
[0104] · Aliphatic polyester polyol: Number of functional groups 2, number average molecular weight 1000, solid content 100 mass%. The synthesis method is as follows.
[0105] 53.1 parts by mass of adipic acid and 46.9 parts by mass of neopentyl glycol were added to a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank, and a nitrogen gas inlet tube, and the temperature was raised to 250 °C while stirring under a nitrogen stream. The reaction was carried out until the acid value became 5 mgKOH / g or less (13.08 parts by mass of distilled water), and an aliphatic polyester polyol was obtained.
[0106] · Dimethylolpropionic acid: 2,2-bis(hydroxymethyl)propionic acid, number of functional groups 2
[0107] · 2,2-Dimethylolbutyric acid: 2,2-Bis(hydroxymethyl)butyric acid, number of functional groups 2
[0108] · Trimethylolpropane: Number of functional groups 3
[0109] · PEG1000: Polyethylene glycol, number of functional groups 2, number average molecular weight 1000, manufactured by Daiichi Kogyo Pharmaceutical "PEG 1000"
[0110] [Polyisocyanate]
[0111] · XDI : Xylylene diisocyanate (number of functional groups: 2)
[0112] · TDI : Tolylene diisocyanate (number of functional groups: 2)
[0113] · HDI : Hexamethylene diisocyanate (number of functional groups: 2)
[0114] [Carbodiimide group-containing compounds]
[0115] · Water-soluble polycarbodiimide 1: "Carbodilite SV-02" manufactured by Nisshinbo Chemical Co., Ltd., solid content 40 mass%, NCN equivalent 430
[0116] · Water-soluble polycarbodiimide 2: "Carbodilite V-02-L2" manufactured by Nisshinbo Chemical Co., Ltd., solid content 40 mass%, NCN equivalent 385
[0117] The evaluation method for polyurethane water-based dispersions is as follows.
[0118] [Adhesion 1 and 2]
[0119] A polyurethane water-based dispersion was used as a primer paint, and the adhesion of the coating film to the resin (especially the adhesion between the primer layer and the UV-cured resin layer) was evaluated by the following method in a three-layer stacked state of PET film / primer layer / UV-cured resin layer.
[0120] A polyethylene terephthalate (PET) film ("Lumirror T-60" manufactured by Toray Corp.) was used as a substrate, and the surface of the substrate was degreased with isopropyl alcohol. Subsequently, a formulation of the following polyurethane water-based dispersion was applied using a bar coater to a dry film thickness of 1 μm, and dried at 180°C for 1 minute to obtain a test specimen X having a polyurethane resin coating film formed thereon.
[0121] · Prescription solution of polyurethane water-based dispersion:
[0122] A formulation solution was prepared by adding 0.1 mass% of a wetting agent ("Neocol SW-C" manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd.) to an aqueous dispersion in which water was added to the polyurethane aqueous dispersion of each example or comparative example so that the solid content was 10 mass%, with respect to 100 mass% of the aqueous dispersion.
[0123] A UV-curing resin formulation was applied to the coating film of test specimen X using a bar coater to a film thickness of 12 μm. Subsequently, a high-pressure mercury lamp was applied to the surface coated with the UV-curing resin formulation at 600 mJ / cm². 2 Test specimen Y was obtained by irradiating with ultraviolet light. Using test specimen Y as a sample, a 1 mm cross-cut test was performed in accordance with JIS K5400-8.5:1990, and the adhesion between the PET film, the primer layer, and the UV-cured resin layer was calculated by the following formula.
[0124] Adhesion (%) = 100 - (Number of peeled cells)
[0125] The details of the UV curing resin formulation are as follows.
[0126] · UV-curing resin formulation with adhesion 1:
[0127] 3 parts by mass of a photopolymerization initiator ("Irgacure 184" manufactured by Chiba Specialty Chemicals Co., Ltd.) added to 100 parts by mass of the epoxy acrylate obtained in the following synthesis example.
[0128] 39 parts by mass of bisphenol A type epoxy resin ("YD-901" manufactured by Nittetsu Chemical & Materials Co., Ltd.), 6 parts by mass of acrylic acid, 0.05 parts by mass of hydroquinone monomethyl ether as a polymerization inhibitor, and 0.35 parts by mass of tetrabutylammonium bromide were added to a flask, and the mixture was reacted under conditions of 100 to 105°C until the acid value was 5 mgKOH / g or less. 55 parts by mass of a diluted monomer ("New Frontier OPPE" manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd.) was added to obtain an epoxy acrylate.
[0129] · UV-curing resin formulation with adhesion level 2:
[0130] 3 parts by mass of a photopolymerization initiator ("Irgacure 184" manufactured by Chiba Specialty Chemicals Co., Ltd.) added to 100 parts by mass of urethane acrylate obtained in the following synthesis example.
[0131] 20 parts by mass of TDI were placed in a flask, 60 parts by mass of PEG1000 were added while stirring, and the temperature was raised to 80°C and the reaction was carried out until the free isocyanate content reached 5.8 mass%. Subsequently, 0.05 parts by mass of hydroquinone monomethyl ether as a polymerization inhibitor was added, followed by the addition of 20 parts by mass of 2-hydroxyethyl acrylate, and the reaction was carried out at 70 to 80°C until the residual isocyanate concentration became less than 0.1 mass% to produce urethane acrylate.
[0132] [My Blocking]
[0133] The anti-blocking properties of the polyurethane water-based dispersion were evaluated by the following method. Two test specimens X (3×5 cm) for the above adhesion evaluation were used, overlapped with the coated surface facing inward, a weight (1000 g) was placed on top, and left to stand for 20 hours at a temperature of 40 ℃ and a humidity of 95 %. After 20 hours, they were cooled to room temperature, and the two test specimens X were peeled off by hand to observe the appearance. If there was no zipping and no change in appearance upon peeling, it was evaluated as “A” (Good); if there was zipping and no change in appearance upon peeling, it was evaluated as “B” (Good); and if one coating film peeled off and adhered to the other, it was evaluated as “C” (Poor).
[0134] [Example 1]
[0135] In a four-necked flask equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen blower, 92.51 parts by mass of aromatic polyester polyol, 1 part by mass of 3.0 parts by mass of dimethylolpropionic acid, 0.5 parts by mass of trimethylolpropane, 9.82 parts by mass of PEG1000, and 100 parts by mass of methyl ethyl ketone were added and thoroughly mixed and dissolved. Subsequently, 21.92 parts by mass of XDI was added as a polyisocyanate, and the mixture was reacted at 70 to 75 °C for 300 minutes to obtain a methyl ethyl ketone solution of an isocyanate group-containing urethane prepolymer. In the obtained urethane prepolymer solution, the content of free isocyanate groups relative to the solid content was 1.2 mass%. The obtained urethane prepolymer solution was cooled to 60°C and, while stirring with a homogenizer, emulsified and dispersed by slowly adding a solution mixed with 3.46 parts by mass of 25 mass% ammonia water and 350 parts by mass of water. Subsequently, the emulsion was stirred at 40°C for 1 hour to complete the chain extension reaction with water. Methyl ethyl ketone was removed by distillation under reduced pressure, thereby obtaining an aqueous dispersion of a polyurethane resin with a solid content of 25 mass%. To the obtained aqueous dispersion, 48.09 parts by mass of water-soluble polycarbodiimide 1 was added and stirred to obtain the polyurethane aqueous dispersion of Example 1. In the obtained polyurethane aqueous dispersion, the acid value of the polyurethane resin was 12.5 mgKOH / g. In addition, the amount of carbodiimide groups relative to 100 moles of carboxyl groups of the polyurethane resin was 200 moles.
[0136] [Examples 2–13 and Comparative Examples 1–5]
[0137] The types and amounts (parts by mass) of the polyol, polyisocyanate, neutralizing agent, and carbodiimide group-containing compound were changed as shown in Tables 1 to 3 below, and otherwise kept the same as in Example 1, thereby obtaining polyurethane water-based dispersions of Examples 2 to 13 and Comparative Examples 1 to 5. However, regarding Comparative Example 3, emulsification dispersion could not be achieved, and therefore, no carbodiimide group-containing compound was added, and no polyurethane water-based dispersion was obtained.
[0138] Adhesion 1 and 2 and anti-blocking properties were evaluated for the polyurethane water-based dispersions of Examples 1 to 13 and Comparative Examples 1 to 5 (except for Comparative Example 3). The results are shown in Tables 1 to 3.
[0139] Meanwhile, in Tables 1 to 3, the amount of aromatic polyester polyol is the amount of solids that are the active ingredients, and the number in parentheses is the amount including solvent. The amount of carbodiimide group-containing compound is the amount of each component including solvent, and the number in parentheses is the amount of solids that are the active ingredients. "Solid content of polyurethane resin" is the solid content (mass%) of polyurethane resin in the aqueous dispersion before the addition of the carbodiimide group-containing compound.
[0140]
[0141]
[0142]
[0143] The results are as shown in Tables 1 to 3. In Comparative Example 1, the anti-blocking properties were inferior because the polyol did not contain aromatic polyester polyol.
[0144] In Comparative Example 2, the acid value of the polyurethane resin was excessively high, so the adhesion was poor despite the excessive addition of a carbodiimide group-containing compound. In Comparative Example 3, an attempt was made to prepare the polyurethane resin so that its acid value was 4.2 mgKOH / g, which is lower than the set value, but the amount of carboxyl group-containing polyol was excessively low, so the urethane prepolymer could not be emulsified.
[0145] In Comparative Example 4, the anti-blocking properties were poor because the amount of carbodiimide groups relative to carboxyl groups was excessively large. Conversely, in Comparative Example 5, the adhesion properties were poor because the amount of carbodiimide groups relative to carboxyl groups was excessively small.
[0146] In contrast, Examples 1 to 13 exhibited excellent adhesion as well as excellent anti-blocking properties. When comparing Example 1 with Example 5 and Example 6, regarding the polyisocyanate, the aromatic ring-containing polyisocyanate showed a tendency to exhibit better anti-blocking properties than the aliphatic polyisocyanate. Furthermore, when comparing Example 1 with Example 12, including polyalkylene glycol as the polyol showed a tendency to improve adhesion to the UV-cured resin layer, particularly urethane acrylate. When comparing Example 1 with Example 13, regarding the neutralizing agent, ammonia showed a tendency to exhibit better adhesion than tertiary amine (triethylamine).
[0147] In addition, the various numerical ranges described in the specification may each have their upper and lower limits arbitrarily combined, and all such combinations are described in this specification as preferred numerical ranges. Furthermore, the description of a numerical range "X ~ Y" means X or greater and Y or less.
[0148] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments may be implemented in various other forms, and various omissions, substitutions, and modifications may be made within the scope of not departing from the essence of the invention. These embodiments and the omissions, substitutions, and modifications thereof are included within the scope of the invention described in the claims and the scope of equivalents, just as they are included in the scope or essence of the invention.
Claims
Claim 1 A polyurethane aqueous dispersion comprising a polyurethane resin (A) containing an aromatic polyester polyol as a constituent component, dispersed in an aqueous dispersion medium, wherein the polyurethane aqueous dispersion comprises a carbodiimide group-containing compound (B), wherein the polyurethane resin (A) has a carboxyl group, the acid value of the polyurethane resin (A) is 5 to 25 mgKOH / g, and the carbodiimide group of the carbodiimide group-containing compound (B) is contained in an amount of 120 to 300 moles relative to 100 moles of the carboxyl group of the polyurethane resin (A). Claim 2 In claim 1, the polyurethane resin (A) is a polyurethane aqueous dispersion further comprising polyalkylene glycol as a constituent. Claim 3 A polyurethane aqueous dispersion according to claim 2, wherein the amount of the polyalkylene glycol is 5 to 15 parts by mass per 100 parts by mass of the polyurethane resin (A). Claim 4 A polyurethane aqueous dispersion according to claim 1, wherein the polyurethane resin (A) further comprises an aromatic ring-containing polyisocyanate as a constituent. Claim 5 A water-based paint comprising a polyurethane water-based dispersion described in any one of claims 1 to 4. Claim 6 In claim 5, a water-based paint used as a primer.