Electrode composites, electrodes, and batteries

The electrode composite with a specific vinylidene fluoride copolymer and carbon-coated active material addresses the issue of high viscosity and thixotropy in LFP/LFMP electrodes, ensuring effective electrode manufacturing and adhesion.

KR1020260161603APending Publication Date: 2026-11-09KUREHA CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267033257
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-29
Filing Date
2025-03-26
Publication Date
2026-11-09

AI Technical Summary

Technical Problem

The use of vinylidene fluoride copolymers with high adhesion strength to current collectors in electrode composites containing lithium iron phosphate (LFP) or lithium iron manganese phosphate (LFMP) results in increased initial viscosity and thixotropy, making it difficult to manufacture electrodes effectively.

Method used

An electrode composite comprising a vinylidene fluoride copolymer with a weight average molecular weight of 1.3 million or less and an adsorption rate of less than 30%, combined with a carbon-coated electrode active material, to maintain low initial viscosity and good handling properties.

Benefits of technology

The composite achieves low initial viscosity and improved handling properties, facilitating the production of electrodes with enhanced adhesion to current collectors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCT00001
    Figure PCT00001
  • Figure PCT00002
    Figure PCT00002
  • Figure PCT00003
    Figure PCT00003
Patent Text Reader

Abstract

The objective is to provide an electrode composite comprising a carbon-coated electrode active material and a vinylidene fluoride copolymer having carboxyl groups, which has low initial viscosity and good handling properties. The electrode composite solving the above objective comprises a vinylidene fluoride copolymer having constituent units derived from vinylidene fluoride and constituent units derived from vinyl compounds having carboxyl groups, and a carbon-coated electrode active material. The amount of carbon coating on the electrode active material is 0.5 mass% or more and 3.0 mass% or less relative to the mass of the electrode active material. When the vinylidene fluoride copolymer is modified with a labeling material composed of 1-bromomethylpyrene and the weight average molecular weight Mw of the carboxyl-containing vinylidene fluoride copolymer that absorbs light of a wavelength of 345 nm is determined, Mw is 1.3 million or less, and the adsorption rate obtained by a predetermined method is greater than 0% and less than 30%.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an electrode composite, an electrode, and a battery. Background Technology

[0002] In forming the composite layer of the electrode of a non-aqueous electrolyte secondary battery, an electrode composite containing a binder and an active material is typically used. As the binder, a vinylidene fluoride polymer is mainly used. High adhesion is required for the binder due to its role of adhering the active material to the current collector. For example, Patent Document 1 describes introducing functional groups such as carboxyl groups into a fluorine-based resin to improve adhesion to the current collector, etc., or to improve solubility in a solvent. Patent Document 2 describes a binder composition comprising vinylidene fluoride and a copolymer of a compound of a specific structure (vinylidene fluoride copolymer), and describes that the vinylidene fluoride copolymer exhibits high adhesion to the current collector.

[0003] Meanwhile, the use of lithium iron phosphate (LFP) as a cathode active material is being considered for the purpose of reducing battery costs. Additionally, the use of lithium iron manganese phosphate (LFMP) as a cathode active material is also being considered as a next-generation material. Prior art literature

[0004] Patent Document 1: Japanese Published Patent Application No. (Hei) 6-172452 Patent Document 2: Japanese Patent Application No. 5797206 The problem to be solved

[0005] In order to increase adhesion to current collectors, etc., it is conceivable to use the vinylidene fluoride copolymer described in the aforementioned Patent Document 1 or Patent Document 2 as an electrode binder in electrode composites (slurries) containing the lithium iron phosphate (LFP) or lithium iron manganese phosphate (LFMP). However, when LFP or LFMP is mixed with a vinylidene fluoride copolymer having high adhesion strength to current collectors, the initial viscosity of the electrode composite increases, and thixotropy tends to increase. Furthermore, it was very difficult to manufacture electrodes with such electrode composites. As the inventors have carefully investigated, it is thought that electrode composites containing LFP or LFMP tend to have higher initial viscosity or higher thixotropy because the vinylidene fluoride copolymer having carboxyl groups interacts with the carbon coating present on the surface of LFP or LFMP.

[0006] The present invention has been made in consideration of the above-mentioned problem. The present invention aims to provide an electrode composite comprising a carbon-coated electrode active material and a vinylidene fluoride copolymer having carboxyl groups, which has low initial viscosity and good handling properties. Furthermore, the invention also aims to provide an electrode and a battery obtained using said electrode composite. means of solving the problem

[0007] [1] The present invention provides an electrode composite comprising a vinylidene fluoride copolymer having a constituent unit derived from vinylidene fluoride and a constituent unit derived from a vinyl compound having a carboxyl group, and a carbon-coated electrode active material, wherein the carbon coating amount of the electrode active material is 0.5 mass% or more and 3.0 mass% or less relative to the mass of the electrode active material, and when the vinylidene fluoride copolymer is modified with a labeling material composed of 1-bromomethylpyrene to determine the weight average molecular weight Mwc of the vinylidene fluoride copolymer containing a carboxyl group that absorbs light of wavelength 345 nm, the weight average molecular weight Mwc is 1.3 million or less, and the vinylidene fluoride copolymer has an adsorption rate of greater than 0% and less than 30% as determined by the following method.

[0008] (Method for determining adsorption rate)

[0009] (i) Prepare a dimethylacetamide solution with a concentration of 1 g / L of vinylidene fluoride copolymer.

[0010] (ii) Gel penetration chromatography is performed on the above dimethylacetamide solution, and the peak area AR1 derived from the above vinylidene fluoride copolymer is calculated by detecting the differential refractive index.

[0011] (iii) 5 g of the above dimethylacetamide solution, with a BET specific surface area of ​​4 m 2 / g or more than 5 m 2 Add 0.8 g of aluminum oxide with a concentration of 1 g or less, stir for 2 hours, and then let stand for 16 hours.

[0012] (iv) After settling, the supernatant of the above dimethylacetamide solution is collected, and solid-liquid separation is performed by centrifugation.

[0013] (v) Gel penetration chromatography is performed on the separated solution, and the peak area AR2 derived from the vinylidene fluoride copolymer is calculated by differential refractive index detection.

[0014] (vi) The adsorption rate is calculated based on the following equation (1). This is done three times, and the average value is taken as the adsorption rate.

[0015] Adsorption rate = (AR1 - AR2) / AR1 × 100

[0016] [2] The present invention provides an electrode composite described in [1] having a weight average molecular weight Mwc of 700,000 or less and an adsorption rate of 20% or less.

[0017] [3] The present invention provides an electrode composite described in [1] or [2], wherein the average particle diameter of the electrode active material is 15 μm or less.

[0018] [4] The present invention provides an electrode composite described in any one of [1] to [3], wherein the carbon coating amount of the electrode active material is 2.5 mass% or less.

[0019] [5] The present invention provides an electrode mixture described in any one of [1] to [4], wherein the vinyl compound is a compound represented by the following general formula (1).

[0020] [Painting 1]

[0021]

[0022] (In general formula (1), R 1 , R 2 , R 3 Each represents independently a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and X represents a hydroxyl group or -Y-COOH (Y represents an atomic group))

[0023] [6] The present invention provides an electrode mixture described in [1] to [4], wherein the vinyl compound is a compound represented by the following general formula (1).

[0024] [Painting 2]

[0025]

[0026] (In general formula (1), R 1 , R 2 , R3 Each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and X represents a hydroxyl group or -Y-COOH (Y represents a divalent group having a molecular weight of 500 or less, containing either an oxygen atom or a nitrogen atom, and also having 1 to 10 atoms in the main chain))

[0027] [7] The present invention provides an electrode comprising a solid component of an electrode mixture described in any one of [1] to [6].

[0028] [8] The present invention provides a battery comprising the electrode described in [7] above. Effects of the invention

[0029] According to the present invention, an electrode composite is provided comprising a carbon-coated electrode active material and a vinylidene fluoride copolymer having carboxyl groups, which has low initial viscosity and good handling properties. Additionally, an electrode and a battery obtained using said electrode composite are also provided. Specific details for implementing the invention

[0030] 1. Electrode composite

[0031] The electrode composite of the present invention is a slurry-type composition comprising a vinylidene fluoride copolymer having a constituent unit derived from vinylidene fluoride and a constituent unit derived from a vinyl compound having a carboxyl group, and a carbon-coated electrode active material (hereinafter also simply referred to as "active material"). The electrode composite may additionally include a conductive agent, a solvent, other additives, etc. When the electrode composite includes a solvent, the vinylidene fluoride copolymer may be dissolved in the solvent or dispersed in the solvent.

[0032] As described above, when an electrode mixture (slurry) is prepared by mixing a vinylidene fluoride copolymer having carboxyl groups with a carbon-coated active material (e.g., LFP, LFMP), the viscosity tends to increase significantly, particularly the initial viscosity tends to increase, and the thixotropy tends to increase as well. In this specification, initial viscosity refers to the viscosity of the slurry immediately after stirring. Generally, LFP, LFMP, etc., are active materials with small particle sizes and are also coated with carbon; they have a large surface area and many functional groups, such as OH groups, exist on the surface. Therefore, the carboxyl groups of the vinylidene fluoride copolymer readily interact with these functional groups, and when a general vinylidene fluoride copolymer is used, the electrode mixture exhibits increased initial viscosity and high thixotropy. In contrast, the electrode composite of the present invention, despite comprising a vinylidene fluoride copolymer having carboxyl groups and a carbon-coated electrode active material as described above, tends to have low initial viscosity and good thixotropy. The reasons for this include the following points.

[0033] The vinylidene fluoride polymer included in the electrode composite of the present invention is a copolymer of vinylidene fluoride, a vinyl compound having a carboxyl group, and, if necessary, another compound, and is an aggregate of multiple polymers. The vinylidene fluoride copolymer (an aggregate of multiple polymers) includes a polymer comprising a constituent unit derived from vinylidene fluoride and a constituent unit derived from a vinyl compound having a carboxyl group (referred to herein as "carboxyl group-containing vinylidene fluoride copolymer" or "carboxyl group-containing copolymer"), and a polymer mainly composed of a constituent unit derived from vinylidene fluoride and not comprising a constituent unit derived from a vinyl compound having a carboxyl group.

[0034] In addition, the weight average molecular weight (Mwc) of the carboxyl group-containing copolymer in the vinylidene fluoride copolymer is 1.3 million or less. That is, the polymerization average molecular weight of the polymer (carboxyl group-containing copolymer) interacting with the active material in the vinylidene fluoride copolymer is relatively small. Therefore, even if the carboxyl group-containing copolymer interacts with the active material, it is difficult to form a robust network, and thus the viscosity of the slurry is unlikely to become excessively high.

[0035] Furthermore, the vinylidene fluoride copolymer included in the electrode composite of the present invention has an adsorption rate for aluminum oxide measured by the method described below that is greater than 0% and less than or equal to 30%. The said adsorption rate represents the ratio of the polymer capable of adsorbing aluminum oxide within the vinylidene fluoride copolymer (an aggregate of multiple polymers). That is, the said adsorption rate corresponds to the ratio of the carboxyl group-containing copolymer within the vinylidene fluoride copolymer. Moreover, since the said adsorption rate is 30% or less, when the vinylidene fluoride copolymer is mixed with an active material, it is difficult to form the aforementioned network, and consequently, it is difficult for excessive thickening of the slurry to occur. Below, the vinylidene fluoride copolymer included in the electrode composite of the present invention, its physical properties, as well as the active material and other components, will be described in detail.

[0036] (Vinylidene fluoride copolymer)

[0037] As described above, the vinylidene fluoride copolymer is a copolymer formed by copolymerizing vinylidene fluoride with at least a vinyl compound having a carboxyl group. The amount of constituent units derived from vinylidene fluoride in the vinylidene fluoride copolymer is 90.00 mol% or more with respect to 100.00 mol% of the total constituent units of the vinylidene fluoride copolymer, and is preferably 95.00 mol% or more and 99.98 mol% or less. If the amount of constituent units derived from vinylidene fluoride is 90.0 mol% or more, it becomes easier to obtain physical properties characteristic of vinylidene fluoride.

[0038] Meanwhile, the amount of constituent units derived from vinyl compounds having carboxyl groups in the above vinylidene fluoride copolymer is preferably 0.01 mol% or more and 0.80 mol% or less, and preferably 0.02 mol% or more and 0.50 mol% or less, based on 100.0 mol% of the total constituent units of the vinylidene fluoride copolymer. If the amount of constituent units derived from vinyl compounds having carboxyl groups is 0.01 mol% or more, the adhesion of the vinylidene fluoride copolymer to the current collector is more likely to increase when an electrode is formed using the electrode mixture. On the other hand, if the amount of constituent units derived from vinyl compounds is 0.80 mol% or less, it becomes more easy to suppress the increase in the initial viscosity of the electrode mixture. The amount of constituent units derived from vinyl compounds having carboxyl groups is neutralization titration or 1 It can be obtained from H-NMR spectra, etc.

[0039] Here, the structure of the vinyl compound is not particularly limited, and any compound having a vinyl group capable of polymerizing with vinylidene fluoride and also having a carboxyl group is acceptable. Additionally, the number of carboxyl groups included in the vinyl compound may be one or two or more. Furthermore, in this specification, an acid anhydride structure composed of two carboxyl groups is also treated as a type of carboxyl group. The vinylidene fluoride copolymer may include only one type of constituent unit derived from the vinyl compound or two or more types. Examples of preferred vinyl compounds include compounds represented by the following general formula (1).

[0040] [Tuesday 3]

[0041]

[0042] In general formula (1), R 1 , R 2 , R 3Each represents independently a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms. Examples of alkyl groups having 1 to 5 carbon atoms include straight-chain or branched-chain alkyl groups, and specific examples thereof include methyl groups, ethyl groups, propyl groups, isopropyl groups, n-butyl groups, sec-butyl groups, isobutyl groups, t-butyl groups, pentyl groups, etc. Among these, methyl groups, ethyl groups, or butyl groups are preferred from the perspective of ease of availability. Furthermore, particularly from the perspective that steric hindrance is unlikely to occur during polymerization with vinylidene fluoride, R 1 , R 2 and R 3 It is more preferable that each be independently a hydrogen atom or a methyl group.

[0043] In addition, in the above general formula (1), X is a hydroxyl group or a group represented by -Y-COOH. Here, Y represents an atomic group, and it is preferable that Y is an atomic group containing either an oxygen atom or a nitrogen atom, more preferable that Y is an atomic group containing either an oxygen atom or a nitrogen atom and having a main chain with 1 or more and 10 or fewer atoms, and more preferable that Y is a divalent atomic group containing either an oxygen atom or a nitrogen atom and also having a main chain with 1 or more and 10 or fewer atoms and a molecular weight of 500 or less.

[0044] The atomic group (Y) may be linear, branched, cyclic, or a combination thereof. Among these, it is preferable that the atomic group (Y) be linear or branched from the perspective that steric hindrance is unlikely to occur during polymerization with vinylidene fluoride.

[0045] The number of atoms in the main chain of the atomic group (Y) may be 1 or more and 10 or less, and 2 or more and 8 or less is preferred. In this specification, the main chain of the atomic group (Y) refers to the longest chain among the chains connecting the carbonyl group of general formula (1) and the carboxyl group of -Y-COOH.

[0046] Here, the atomic group (Y) includes either or both of oxygen atoms and nitrogen atoms (hereinafter collectively referred to as "hetero atoms"). The number of hetero atoms in the atomic group (Y) is preferably 1 to 10, and more preferably 1 to 5. When the atomic group (Y) includes two or more hetero atoms, they may be atoms of the same type or atoms of different types. The hetero atoms may be included in a structure (functional group) or may exist at any position within the atomic group (Y). Examples of structures (functional groups) containing these hetero atoms include ether bonds, ester bonds, carbonyl groups, carboxyl groups, amide groups, hydroxyl groups, etc. Among these, ether bonds, ester groups, carbonyl groups, carboxyl groups, amide groups, and hydroxyl groups are preferred.

[0047] The structure of the atomic group (Y) is not particularly limited and, for example, can be a structure in which a hydrocarbon group such as an alkylene group or an alkyl group is combined with a structure (functional group) containing the above heteroatom. In addition, the molecular weight of the atomic group (Y) may be 500 or less, and from the perspective of polymerization reactivity, it is preferable to be 30 or more and 200 or less.

[0048] Specific examples of compounds represented by the above general formula (1) include (meth)acrylic acid, (meth)acryloyloxyethyl succinic acid, (meth)acryloyloxypropyl succinic acid, 2-carboxyethyl (meth)acrylate, 2-carboxymethyl (meth)acrylate, (meth)acryloyloxyethyl phthalic acid, N-carboxyethyl (meth)acrylamide, and other (meth)acrylamide compounds. Additionally, in this specification, (meth)acrylic refers to methacrylate, acrylate, or a mixture thereof, (meth)acrylate refers to methacrylate, acrylate, or a mixture thereof, and (meth)acryloyl refers to methacryloyl, acryloyl, or a mixture thereof.

[0049] The compounds represented by the above general formula (1) are more preferably acrylic acid, acryloyloxyethyl succinic acid, acryloyloxypropyl succinic acid, 2-carboxyethyl acrylate, and 2-carboxymethyl acrylate in terms of ease of availability and reactivity with vinylidene fluoride.

[0050] However, the above vinyl compound is not limited to the compound represented by general formula (1). Examples of vinyl compounds other than the compound represented by general formula (1) include unsaturated dibasic acids such as maleic acid, fumaric acid, and itaconic acid; unsaturated dibasic acid anhydrides such as maleic anhydride and itaconic anhydride; and unsaturated dibasic acid monoesters such as monomethyl fumarate, monoethyl fumarate, monomethyl maleate, monoethyl maleate, monomethyl citraconic acid, monoethyl citraconic acid, monomethyl phthalate, monoethyl phthalate, monomethyl itaconic acid, and monoethyl itaconic acid.

[0051] In addition, the vinylidene fluoride copolymer may partially contain constituent units derived from vinylidene fluoride and compounds other than the vinyl compound (other compounds), to the extent that it does not impair the purpose and effects of the present invention. The vinylidene fluoride copolymer may contain only one type of constituent unit derived from other compounds, or it may contain two or more types. However, the total amount of constituent units derived from other compounds relative to 100.0 mol% of the total constituent units of the vinylidene fluoride copolymer is preferably 10.0 mol% or less, and more preferably 5.0 mol% or less. The amounts thereof 19 F-NMR spectrum, 1 It is determined from H-NMR spectra and neutralization titrations, etc.

[0052] Examples of other compounds include fluorinated vinyl compounds having a vinyl group and a fluorine atom or a fluorine-containing alkyl group in one molecule. Examples of fluorinated vinyl compounds include vinyl fluoride; trifluoroethylene; tetrafluoroethylene; chlorotrifluoroethylene; hexafluoropropylene; and perfluoroalkyl vinyl ethers represented by perfluoromethyl vinyl ether. Additionally, examples of other compounds include compounds having a vinyl group and not containing fluorine. Examples include unsaturated hydrocarbon compounds such as ethylene and propylene.

[0053] Here, among the vinylidene fluoride copolymers (multiple polymers), the weight average molecular weight Mwc of the polymer having a carboxyl group, i.e., the carboxyl group-containing copolymer, may be 1.3 million or less, but it is preferable to be 10,000 or more and 800,000 or less, more preferable to be 50,000 or more and 700,000 or less, more preferable to be 100,000 or more and 700,000 or less, and even more preferable to be 200,000 or more and 700,000 or less. As described above, if the weight average molecular weight Mwc of the carboxyl group-containing copolymer is 1.3 million or less, it becomes difficult for the slurry viscosity of the electrode mixture to increase excessively.

[0054] In this specification, the weight average molecular weight Mwc of the carboxyl group-containing copolymer is a value measured as follows. A labeling substance (1-bromomethylpyrene) and potassium carbonate are mixed with a vinylidene fluoride copolymer to label the carboxyl group, thereby performing esterification of the carboxyl group. Accordingly, a vinylidene fluoride copolymer modified by pyrene is obtained. Then, a UV-vis detector (detection wavelength is 345 nm) is used, and gel permeation chromatography (GPC) measurement is performed using N,N-dimethylacetamide as the eluent. The weight average molecular weight Mwc is the polystyrene equivalent value of the measured value. Furthermore, the pyrene structure has characteristic absorption in the UV-vis region and strongly absorbs light of wavelength 345 nm. Therefore, by esterifying the carboxyl group with 1-bromomethylpyrene, the polymerization average molecular weight Mwc of the carboxyl group-containing copolymer is determined.

[0055] Meanwhile, the weight average molecular weight Mwa of the vinylidene fluoride copolymer is not particularly limited, but is preferably 50,000 or more, more preferably 200,000 or more and 400,000 or less, and even more preferably 250,000 or more and 300,000 or less. If the weight average molecular weight Mwa of the vinylidene fluoride copolymer is 50,000 or more, the adhesion strength of the vinylidene fluoride copolymer with the active material, etc., or the current collector is likely to increase. On the other hand, if the Mwa is 4,000,000 or less, the viscosity of the slurry does not become too high when the electrode mixture (slurry) is prepared, and the workability is particularly likely to be excellent. In this specification, the weight average molecular weight Mwa of the vinylidene fluoride copolymer is a polystyrene equivalent value in N,N-dimethylacetamide eluent measured by gel permeation chromatography (GPC), and is a value determined by a differential refractive index (RI) detector. Mwa is the average value of three measurements.

[0056] In addition, the above vinylidene fluoride copolymer has an adsorption rate specified by the following method of greater than 0% and less than or equal to 30%, more preferably greater than or equal to 1% and less than or equal to 20%, and even more preferably greater than or equal to 2% and less than or equal to 15%.

[0057] (Method for determining adsorption rate)

[0058] The adsorption rate is determined by performing (i) to (vi) below.

[0059] (i) Prepare a dimethylacetamide (DMAc) solution with a concentration of 1 g / L of vinylidene fluoride copolymer.

[0060] (ii) Gel penetration chromatography (GPC) measurements are performed on the DMAc solution prepared in (i), and the peak area AR1 derived from the vinylidene fluoride copolymer is calculated by differential refractive index detection.

[0061] (iii) 5 g of the DMAc solution prepared in (i), with a BET specific surface area of ​​4 m 2 / g or more than 5 m 2 Add 0.8 g of aluminum oxide with a concentration of 1 g or less, stir for 2 hours, and then let stand for 16 hours.

[0062] (iv) Collect the supernatant of the DMAc solution after settling in (iii), and perform solid-liquid separation by centrifugation.

[0063] (v) GPC measurements are performed on the separated solution obtained in (iv), and the peak area AR2 derived from the vinylidene fluoride copolymer is calculated by differential refractive index detection.

[0064] (vi) From the areas AR1 and AR2 obtained in (ii) and (v) above, the adsorption rate is calculated based on the following equation (1). This is done three times, and the average value is taken as the adsorption rate.

[0065] Adsorption rate = (AR1 - AR2) / AR1 × 100

[0066] As described above, the vinylidene fluoride copolymer comprises the carboxyl group-containing copolymer and a polymer composed mainly of vinylidene fluoride (and other compounds) as constituent units, without including constituent units derived from vinyl compounds. Furthermore, the adsorption rate corresponds to the amount of the carboxyl group-containing copolymer relative to the total amount of polymers constituting the vinylidene fluoride copolymer. In the present invention, since the content ratio of the carboxyl group-containing copolymer in the vinylidene fluoride copolymer is 30% or less, it is difficult to form a robust network based on the active material, and thus it is difficult for the slurry viscosity of the electrode mixture to increase. On the other hand, because the vinylidene fluoride copolymer contains the carboxyl group-containing copolymer, when an electrode is formed using the electrode mixture, the adhesion strength between the vinylidene fluoride copolymer and the current collector, etc., is improved.

[0067] Here, the inherent viscosity of the vinylidene fluoride copolymer is preferably 0.5 dL / g or more and 6.0 dL / g or less, more preferably 0.5 dL / g or more and 5.0 dL / g or less, and even more preferably 0.8 dL / g or more and 4.5 dL / g or less. If the inherent viscosity is 0.5 dL / g or more, the adhesion strength of the vinylidene fluoride copolymer with the active material, etc., or the current collector tends to increase. On the other hand, if the inherent viscosity is 6.0 dL / g or less, the initial viscosity of the electrode mixture does not become too high, so workability is particularly likely to be excellent. Inherent viscosity (η i ) represents the logarithmic viscosity. First, 80 mg of vinylidene fluoride copolymer is dissolved in 20 ml of N,N-dimethylformamide, and the viscosity is measured using a Ubbelohde viscometer in a constant temperature bath at 30°C. Then, it is calculated based on the following formula from the obtained value.

[0068] η i =(1 / C)·ln(η / η0)

[0069] In the above formula, η is the viscosity of the solution, η0 is the viscosity of the solvent N,N-dimethylformamide alone, and C is the concentration of vinylidene fluoride copolymer in the solution, i.e., 0.4 g / dl.

[0070] The amount of vinylidene fluoride copolymer included in the solid content of the electrode mixture (components excluding those that volatilize during the formation of the mixture layer) is preferably 0.2 mass% or more and 20 mass% or less, more preferably 0.2 mass% or more and 10 mass% or less, and even more preferably 0.2 mass% or more and 5 mass% or less. If the amount of vinylidene fluoride copolymer is within this range, it becomes easier to obtain a mixture layer with high strength.

[0071] The above vinylidene fluoride copolymer can be prepared by copolymerizing vinylidene fluoride, the above vinyl compound, and, if necessary, other compounds. Examples of methods for copolymerizing these include suspension polymerization, emulsion polymerization, and solution polymerization, but suspension polymerization is preferred from the view that it reduces impurities.

[0072] In suspension polymerization using water as a dispersion medium, a suspending agent such as methyl cellulose, propoxylated methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyethylene oxide, or gelatin is added and used in a range of 0.005 to 1.0 parts by mass, preferably 0.01 to 0.4 parts by mass, per 100 parts by mass of the total monomers used in copolymerization (vinylidene fluoride, vinyl compounds having carboxyl groups, and other monomers).

[0073] As a polymerization initiator, diisopropyl peroxydicarbonate, dinormal propyl peroxydicarbonate, dinormal heptafluoropropyl peroxydicarbonate, isobutyryl peroxide, di(chlorofluoroacyl)peroxide, di(perfluoroacyl)peroxide, t-butyl peroxypivalate, etc. may be used. The amount used is 0.05 to 10 parts by mass, preferably 0.15 to 5 parts by mass, when the total monomers used in copolymerization (vinylidene fluoride, vinyl compounds having carboxyl groups, and other monomers as needed) are 100 parts by mass.

[0074] In addition, it is also possible to control the degree of polymerization of the obtained vinylidene fluoride copolymer by adding a chain transfer agent such as ethyl acetate, methyl acetate, diethyl carbonate, acetone, ethanol, n-propanol, acetaldehyde, propylaldehyde, ethyl propionate, or carbon tetrachloride. When a chain transfer agent is used, the amount used is typically 0.01 to 5 parts by mass, preferably 0.01 to 3 parts by mass, when the total monomers used in copolymerization (vinylidene fluoride, vinyl compounds having carboxyl groups, and other monomers) are 100 parts by mass.

[0075] In addition, the total amount of monomers used in copolymerization (vinylidene fluoride, vinyl compounds having carboxyl groups, and other monomers) added is typically 1:1 to 1:10, preferably 1:2 to 1:5, in terms of the mass ratio of total monomers to water.

[0076] The polymerization temperature T is the 10-hour half-life temperature T of the polymerization initiator. 10 It is selected appropriately depending on, and usually T 10 -25℃≤T≤T 10 It is selected within the range of +25℃. For example, T of t-butyl peroxypivalate and diisopropyl peroxydicarbonate 10These are 54.6°C and 40.5°C, respectively (refer to the Nichiyu Corporation product catalog). Accordingly, in polymerization using t-butyl peroxypivalate and diisopropyl peroxydicarbonate as polymerization initiators, the polymerization temperature T is appropriately selected within the ranges of 29.6°C ≤ T ≤ 79.6°C and 15.5°C ≤ T ≤ 65.5°C, respectively. The polymerization time is not particularly limited, but considering productivity, it is preferable to be 100 hours or less. The pressure during polymerization is typically performed under pressure, and is preferably 2.0 to 10.0 MPa-G.

[0077] Here, as a method to reduce the weight average molecular weight Mwc of the carboxyl group-containing copolymer to 1.3 million or less, while simultaneously reducing the adsorption rate described above to greater than 0% and less than or equal to 30%, the following two methods may be cited as examples. However, the methods are not limited to these methods. The first method is a method of mixing the entire amount of vinylidene fluoride (and other compounds) and the vinyl compound having carboxyl groups and then starting polymerization. The second method is a method of polymerizing the vinylidene fluoride (and other compounds) to a certain extent, then adding the entire amount of the vinyl compound having carboxyl groups to the reaction system in a short time, and then performing polymerization again. Accordingly, the weight average molecular weight Mwc and the adsorption amount can be set to a desired range.

[0078] (Active material)

[0079] The active material included in the electrode composite of the present invention is carbon-coated, and is a compound having a carbon coating amount of 0.5 mass% or more and 3.0 mass% or less relative to the mass of the active material. The carbon coating amount is determined by separating the active material from the vinylidene fluoride copolymer, heating and dissolving the separated active material in aqua regia, suction filtration using a membrane filter, and calculating the acid-insoluble content (carbon amount) from the residue on the filter. The carbon coating amount is preferably 0.5 mass% or more and 2.7 mass% or less, and more preferably 0.5 mass% or more and 2.5 mass% or less.

[0080] Here, the type of active material is not particularly limited as long as the above carbon coating amount is satisfied, but generally, in olivine-type lithium compounds represented by LiMaPO4 (wherein Ma is one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, Zr), such as the cathode active material LiFePO4 (LFP) or LiFeMnPO4 (LFMP), the surface is often carbon-coated to reduce particle resistance, making it easy to satisfy the above coating rate. As described above, when an electrode composite is prepared by mixing a carbon-coated active material with a general vinylidene fluoride copolymer having carboxyl groups, the initial viscosity tends to increase. In contrast, by combining with the vinylidene fluoride copolymer described above, it is difficult for the initial viscosity of the electrode composite to increase.

[0081] In addition, the above LFP or LFMP has a relatively small average particle diameter. Even when the average particle diameter of the active material in the electrode mixture is small, the initial viscosity of the electrode mixture is typically prone to increasing. However, in the electrode mixture of the present invention, it is difficult to form a robust network structure based on the active material in the above vinylidene fluoride copolymer. Therefore, even if the average particle diameter of the LFP or LFMP is small, it is difficult for the initial viscosity of the electrode mixture to increase. In this specification, the average particle diameter of the active material refers to the particle size accumulation rate of 50% (Dv50) in the volume-based particle size accumulation curve specified in accordance with JISK 1474. The said average particle diameter (Dv50) is preferably 15 μm or less, and more preferably 0.1 μm or more and 15 μm or less. However, the average particle diameter of the active material is not limited to this range.

[0082] The amount of active material included in the electrode mixture is appropriately selected according to the application of the electrode mixture, but it is preferable to be 50 mass% or more and 99.9 mass% or less with respect to the total amount of solids of the electrode mixture. If the amount of active material is within this range, for example, sufficient charge / discharge capacity is obtained, and the battery performance is likely to be good.

[0083] (Challenge Jose)

[0084] The electrode composite may additionally include a conductive agent. The conductive agent included in the electrode composite is not particularly limited as long as it is a compound capable of further enhancing the conductivity between the active materials or between the active materials and the current collector. Examples of conductive agents include acetylene black, ketjen black, carbon black, graphite powder, carbon nanofiber, carbon nanotube, and carbon fiber.

[0085] The amount of conductive additive included in the electrode mixture is appropriately selected according to its type, etc. In terms of improving conductivity and increasing the dispersibility of the conductive additive, it is preferable that the amount be 0.1 mass% or 15 mass% or less with respect to the total amount of solids of the electrode mixture, more preferable that it be 0.1 mass% or more or 7 mass% or less, and even more preferable that it be 0.1 mass% or more or 5 mass% or less.

[0086] (menstruum)

[0087] The electrode composite may contain a solvent. The solvent may be a non-aqueous solvent or water. Additionally, the non-aqueous solvent may be a polar solvent (polar solvent). Examples of the above polar solvents include amide compounds such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; alcohol compounds such as methanol, ethanol, isopropyl alcohol, 2-ethyl-1-hexanol, 1-nonanol, lauryl alcohol, and tripropylene glycol; amine compounds such as o-toluidine, m-toluidine, and p-toluidine; imide compounds such as 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide; lactone compounds such as γ-butyrolactone and δ-butyrolactone; and sulfoxide-sulfone compounds such as dimethyl sulfoxide and sulfolane. Ether compounds such as tetrahydrofuran, diethyl ether, 1,4-dioxane, and diethylene glycol dimethyl ether; ketone compounds such as acetone, 2-butanone, methyl isobutyl ketone, and cyclohexanone are included. The electrode mixture may contain only one of the above solvents, or may contain two or more.

[0088] The total amount of solvent in the electrode mixture is not particularly limited, but typically, it is preferably 10 parts by mass or more and 150 parts by mass or less per 100 parts by mass of the active material described above.

[0089] (Other ingredients)

[0090] The electrode composite may also include a dispersant, an adhesion aid, a thickener, etc., and known compounds may be used for these. Examples of the dispersant include polyvinylpyrrolidone, methyl cellulose, methoxylated methyl cellulose, propoxylated methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyethylene oxide, polypropylene oxide, gelatin, etc. In addition, examples of the adhesion aid include poly(meth)acrylic acid, metal salts of poly(meth)acrylate such as sodium poly(meth)acrylate, carboxymethyl cellulose, etc. The amounts of these are not particularly limited as long as they are within a range that does not impair the purpose and effect of the present invention, but it is preferable that they be 15 mass% or less with respect to the total amount of solids of the electrode composite.

[0091] In addition, the electrode mixture may further include additives such as phosphorus compounds; sulfur compounds; nitrogen compounds such as amine compounds and ammonium compounds; organic acids; organic esters; various silane-based, titanium-based, and aluminum-based coupling agents; vinylidene fluoride polymers other than the vinylidene fluoride copolymer described above; and resins such as polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), and polyacrylonitrile (PAN). These are not particularly limited as long as they do not impair the purpose and effects of the present invention, but it is preferable that they be 15 mass% or less of the total solid content of the electrode mixture.

[0092] (Physical properties of electrode mixtures)

[0093] The viscosity of the electrode composite is not particularly limited as long as it is a viscosity that can prevent dripping, uneven coating, and delayed drying after coating when forming a composite layer by coating the electrode composite, and provides good workability and applicability during the production of the composite layer. The value is measured at 25°C using an E-type viscometer of the electrode composite, and after a holding period of 60 seconds at 25°C using an E-type viscometer, a shear rate of 1 s -1The rotor is rotated, and the value measured 120 seconds after the start of rotor rotation is preferably 2,000 mPa·s or more and 60,000 mPa·s or less, and more preferably 5,000 mPa·s or more and 30,000 mPa·s or less. If the initial viscosity is within this range, the handling properties when forming the composite layer tend to be better.

[0094] In addition, using an E-type viscometer, after a holding period of 60 seconds at 25℃, a shear rate of 40 s -1 The rotor is rotated, and the value measured 30 seconds after the start of rotor rotation is preferably 1,000 mPa·s or more and 5,000 mPa·s or less, and more preferably 1,000 mPa·s or more and 4,000 mPa·s or less. In addition, the shear rate is 40 s -1 Viscosity specified by, and a shear rate of 1 s -1 The ratio of viscosity specified by, i.e. (shear rate 1 s -1 Viscosity / shear rate specified by 40 s -1 The viscosity (specifically defined as) is preferably 2 to 12, and more preferably 3 to 11. If the above ratio is within this range, the handling properties of the electrode composite when forming the composite layer tend to be improved.

[0095] (Method for preparing electrode mixture)

[0096] The above electrode mixture may be prepared by mixing all components at once, or by mixing some components first and then mixing the remaining components later.

[0097] 2. Electrode

[0098] The electrode composite described above can be used to form a composite layer of an electrode of various non-aqueous electrolyte secondary batteries. An electrode of a non-aqueous electrolyte secondary battery comprises, for example, a current collector and a composite layer disposed on said current collector. The electrode composite described above can be used to form said composite layer.

[0099] · Entire house

[0100] The current collector is a terminal for drawing electricity. The material of the current collector is not particularly limited, and metal foils or metal meshes such as aluminum, copper, iron, stainless steel, steel, nickel, and titanium may be used. In addition, a layer containing carbon black, etc., may be formed on the surface of another medium, or the metal foil or metal mesh, etc. may be applied.

[0101] · Combined layer

[0102] The composite layer is a layer formed by applying the aforementioned electrode composite onto a current collector and solidifying it. That is, the composite layer comprises at least the aforementioned vinylidene fluoride-based compound and active material. The composite layer may be formed on only one side of the current collector or may be disposed on both sides.

[0103] The composite layer comprises at least the components included in the electrode composite described above, namely, vinylidene fluoride copolymer and active material, and additionally includes various additives such as conductivity aids, dispersants, adhesion aids, and thickeners as needed. These are the same as those described in the electrode composite.

[0104] Here, the thickness of the composite layer is not particularly limited, but in one example, it is preferably 1 μm or more and 300 μm or less. In addition, the weight per unit area of ​​the composite layer formed on one side of the current collector is not particularly limited and can be any weight per unit area, but in one example, 50 g / m² 2 500 g / m² or more 2 The following is preferable, and 100 g / m² 2 300 g / m² or more 2 The following is more desirable.

[0105] The above composite layer can be formed by performing a process of applying the above-described electrode composite onto a current collector and a process of solidifying it.

[0106] The method of applying the electrode mixture is not particularly limited, and the doctor blade method, reverse roll method, comma bar method, gravure method, air knife method, die coating method, and dip coating method can be applied.

[0107] In addition, after applying the electrode mixture, the solvent is dried by heating at any temperature. In one example, the drying temperature is preferably 60°C or higher and 200°C or lower, and more preferably 80°C or higher and 150°C or lower. Heating may be performed multiple times at different temperatures. In addition, the solvent in the mixture may be dried under atmospheric pressure, pressurized pressure, or reduced pressure, or it may be dried under an environment such as air, nitrogen, or argon. Additional heat treatment may be performed after drying.

[0108] After applying and drying the above electrode mixture, additional press treatment may be performed. By performing press treatment, the electrode density can be improved. In one example, the press pressure is preferably 1 kPa or more and 10 GPa or less.

[0109] 3. Battery

[0110] As described above, the electrode composite can be used for electrodes of various non-aqueous electrolyte secondary batteries, but it can also be used to form other layers of non-aqueous electrolyte secondary batteries.

[0111] Examples

[0112] Specific embodiments of the present invention are described below together with comparative examples, but the present invention is not limited to these.

[0113] 1. Methods for measuring and evaluating various physical properties

[0114] Methods for measuring the inherent viscosity of the vinylidene fluoride copolymer, the weight-average molecular weight Mwa of the vinylidene fluoride copolymer, the weight-average molecular weight Mwc of the carboxyl group-containing copolymer, and the adsorption rate for aluminum oxide are described below. Additionally, methods for measuring the average particle diameter (Dv50) and carbon coating amount of the electrode active material are described below. Furthermore, methods for measuring the slurry viscosity of the electrode mixture are described below.

[0115] (1) Inherent viscosity of vinylidene fluoride copolymer

[0116] The inherent viscosity of the vinylidene fluoride copolymer was measured as follows. First, 80 mg of the vinylidene fluoride copolymer was dissolved in 20 ml of N,N-dimethylformamide, and the viscosity was measured using an Ubérode viscometer in a constant temperature bath at 30°C. Then, based on the obtained value, the inherent viscosity (η) of the vinylidene fluoride copolymer was calculated according to the following formula. i ) produced.

[0117] η i =(1 / C)·ln(η / η0)

[0118] In the above formula, η is the viscosity of the solution, η0 is the viscosity of the solvent N,N-dimethylformamide alone, and C is the concentration of the vinylidene fluoride copolymer in the solution, i.e., 0.4 g / dl.

[0119] (2) Weight average molecular weight Mwa of vinylidene fluoride copolymer

[0120] The weight-average molecular weight Mw1 of the vinylidene fluoride copolymer prepared in each example and comparative example was measured using a differential refractometer (RI). Specifically, GPC (gel penetration) measurements were performed under the following conditions, and Mwa was obtained using a differential refractive index detector. This was performed three times, and the average value was taken as Mwa.

[0121] Separation columns: Shodex KD-807, KD-806M

[0122] Detector: JASCO Corporation RI-4030 (Disparity Refractive Index Detector)

[0123] Eluent: 10 mM LiBr-N, N-dimethylacetamide (DMAc) solution

[0124] Eluent flow rate: 0.5 mL / min

[0125] Column temperature: 40℃

[0126] Standard polymer for calibration curve: TSK standard POLY(STYRENE) (Product of TOSOH CORPORATION)

[0127] (3) Weight average molecular weight Mwc of the carboxyl group-containing copolymer

[0128] To 10 mg of DMAc, 10 mg of the vinylidene fluoride copolymer prepared in each example and comparative example, 2 mg of 1-bromomethylpyrene, and 2 mg of potassium carbonate were added, and the dissolution and reaction were carried out while stirring in a constant temperature shaking bath at 50°C, and the potassium carbonate was removed using a 0.45 μm filter. Accordingly, the carboxyl groups of the carboxyl group-containing copolymer in the vinylidene fluoride copolymer were labeled with 1-bromomethylpyrene.

[0129] The weight-average molecular weight of a carboxyl group-containing copolymer (a polymer that absorbs light at a wavelength of 345 nm) containing a vinylidene fluoride copolymer labeled with 1-bromomethylpyrene was determined using the following UV-vis detector. Except for the detector, the measurement was performed under the same conditions as the above Mwa. The detection wavelength was set to 345 nm, and the weight-average molecular weight Mwc of the carboxyl group-containing copolymer was calculated. This was performed three times, and the average value was taken as Mwc.

[0130] (4) Measurement of the adsorption rate of aluminum oxide

[0131] For the vinylidene fluoride copolymers prepared in each example and comparative example, the adsorption rate for aluminum oxide was determined by the following method. The results are shown in Table 1.

[0132] (i) A dimethylacetamide (DMAc) solution with a concentration of 1 g / L of vinylidene fluoride copolymer was prepared.

[0133] (ii) Gel penetration chromatography (GPC measurement) was performed on the DMAc solution prepared in (i), and the peak area AR1 derived from the vinylidene fluoride copolymer was calculated by differential refractive index detection.

[0134] (iii) 5 g of the DMAc solution prepared in (i), with a BET specific surface area of ​​4 m 2 / g or more than 5 m 2 0.8 g of aluminum oxide with a concentration of 1 g or less was added, stirred for 2 hours, and then left to stand for 16 hours.

[0135] (iv) The supernatant of the DMAc solution was collected after settling in (iii), and solid-liquid separation was performed by centrifugation.

[0136] (v) Gel penetration chromatography was performed on the separated solution, and the peak area AR2 derived from the vinylidene fluoride copolymer was calculated by differential refractive index detection.

[0137] (vi) From the areas AR1 and AR2 obtained in (ii) and (v) above, the adsorption rate was calculated based on the following equation (1). This was performed three times, and the average value was taken as the adsorption rate.

[0138] Adsorption rate = (AR1 - AR2) / AR1 × 100

[0139] (5) Measurement of the average particle diameter of the electrode mixture Dv50

[0140] For 0.01 g of active material, 0.1 g of dispersant (cationic surfactant “SN Wet 366” (manufactured by SAN NOPCO LIMITED)) was added, and the dispersant was fused to the sample. Next, 20 mL of pure water was added and dispersed using an ultrasonic cleaner for about 5 minutes, after which the particle size distribution in the range of 0.1 to 1000 μm was determined using a particle size distribution measuring device (Microtrax product: MT3300EXII). In addition, the dispersion medium was set to pure water, and the refractive index of the dispersion medium was set to 1.333. From the obtained particle size distribution, the particle diameter at which the cumulative frequency is 50% on a volume basis was calculated, and Dv50 was determined.

[0141] (6) Method for determining the carbon coating amount of electrode mixture

[0142] 500 mg of active material was weighed into a beaker, 40 mL of water and aqua regia (3 mL of nitric acid + 9 mL of hydrochloric acid) were added, and after heating and dissolving, the mixture was filtered by suction using a membrane filter, and the acid-insoluble portion (carbon coating amount) was calculated from the remainder.

[0143] (7) Slurry viscosity of electrode mixture

[0144] The slurry viscosity of the electrode mixtures prepared in the examples and comparative examples was measured. The electrode mixture immediately after preparation was introduced into an E-type viscometer (Toki Sangyo Co., Ltd. RE-215 viscometer, rotor 3°×R14). After a holding period of 60 seconds at 25°C in the device, a shear rate of 1 s -1 The rotor was rotated, and the viscosity 120 seconds after the start of rotor rotation was determined as the slurry viscosity.

[0145] In addition, within the above device, after a holding period of 25°C and 60 seconds, a shear rate of 40 s -1 The rotor was rotated, and the viscosity 30 seconds after the start of rotor rotation was determined as the slurry viscosity.

[0146] Also, a specific shear rate 1 s -1 slurry viscosity and shear rate 40 s -1 Viscosity ratio of the slurry viscosity (shear rate 1 s -1 slurry viscosity / shear rate of 40 s -1 The slurry viscosity was specified.

[0147] 2. Preparation of materials

[0148] The following materials were prepared as the materials for the electrode mixtures prepared in the examples and comparative examples.

[0149] (1) Active substance

[0150] ·LFP-A: Carbon coverage: 1.0%, Average particle diameter Dv50: 2 μm)

[0151] ·LFP-B: Carbon coverage: 1.4%, Average particle diameter Dv50: 4 μm)

[0152] ·LFP-C: Carbon coverage: 2.1%, Average particle diameter Dv50: 10 μm)

[0153] ·LFMP: Carbon coating: 2.0%, Average particle diameter Dv50: 1 μm)

[0154] · LCO (Lithium Cobaltate): Carbon coating: 0.0%, Average particle diameter Dv50: 2 μm)

[0155] (2) Vinylidene fluoride copolymer

[0156] ·VDF / APS-1: Prepared in Synthesis Example 1 below

[0157] ·VDF / APS-2: Prepared in Synthesis Example 2 below

[0158] ·VDF / AA-1: Prepared in Synthesis Example 3 below

[0159] ·VDF / AA-2: Prepared in Synthesis Example 4 below

[0160] <Synthesized Example 1>

[0161] 1240 g of ion-exchanged water as a dispersion medium, 0.4 g of METOLOSE SM-100 (manufactured by Shin-Etsu Chemical Co., Ltd.) as a cellulose-based suspending agent, 2.0 g of acryloyloxypropyl succinic acid (APS), 1.40 g of a 50 mass% diisopropyl peroxydicarbonate-HFE-347pc-f solution as a polymerization initiator, 0.8 g of ethyl acetate as a chain transfer agent, and 400 g of vinylidene fluoride were added to an autoclave with a net capacity of 2 liters, and the temperature was raised to 45°C over 2 hours. While maintaining the temperature at 45°C, the reaction was continued until the pressure inside the system was lowered to 1.5 MPa.

[0162] After the polymerization was completed, the polymer slurry was heat-treated at 95°C for 60 minutes, dehydrated, washed with water, and dried again at 80°C for 20 hours to obtain a powder of vinylidene fluoride copolymer (VDF / APS-1), which is a copolymer of vinylidene fluoride (VDF) and acryloyloxypropyl succinic acid (APS). The inherent viscosity, weight average molecular weight Mwa of the vinylidene fluoride copolymer, and the weight average molecular weight Mwc of the carboxyl group-containing copolymer are shown in Table 1 below.

[0163] <Synthesized Example 2>

[0164] 1054.5 g of ion-exchanged water as a dispersion medium, 0.23 g of metholose SM-100 (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.) as a cellulose-based suspending agent, 0.07 g of APS, 3.50 g of a 50 mass% diisopropyl peroxydicarbonate-HFE-347pc-f solution as a polymerization initiator, and 400 g of vinylidene fluoride were added to an autoclave with a net capacity of 2 liters, and the temperature was raised to 26°C over 55 minutes. While maintaining the temperature at 26°C, 0.86 g of an aqueous solution of 5 mass% APS was added over 4.3 hours starting 2 hours after the start of the temperature increase. From the point when the pressure decreased by 0.2 MPaG from the pressure at the end of the temperature increase, the temperature was raised to 55°C over 40 minutes. The reaction was continued while maintaining the temperature at 55℃ until the pressure in the system dropped to 1.3 MPaG.

[0165] By treating the obtained polymer slurry in the same manner as in Synthesis Example 1, a powder of vinylidene fluoride copolymer (VDF / APS-2), which is a copolymer of vinylidene fluoride (VDF) and acryloyloxypropyl succinic acid (APS), was obtained. The inherent viscosity, weight average molecular weight Mwa, and weight average molecular weight Mwc of the vinylidene fluoride copolymer containing the carboxyl group are shown in Table 1 below.

[0166] <Synthesized Example 3>

[0167] 1056 g of ion-exchanged water as a dispersion medium, 0.44 g of metholose SM-100 (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.) as a cellulose-based suspending agent, 9.37 g of acrylic acid (AA), 5.28 g of a 50 mass% tertiary-butyl peroxypivalate-HFE-347pc-f solution as a polymerization initiator, 0.44 g of ethyl acetate as a chain transfer agent, and 440 g of vinylidene fluoride were added to an autoclave with a capacity of 2 liters, and the temperature was raised to 52°C over a period of 110 minutes. While maintaining the temperature at 52°C, the reaction was continued until the pressure inside the system was lowered to 4.7 MPaG.

[0168] By treating the obtained polymer slurry in the same manner as in Synthesis Example 1, a powder of vinylidene fluoride copolymer (VDF / AA-1), which is a copolymer of vinylidene fluoride (VDF) and acrylic acid (AA), was obtained. The inherent viscosity, weight average molecular weight Mwa of the vinylidene fluoride copolymer, and the weight average molecular weight Mwc of the carboxyl group-containing copolymer are shown in Table 1 below.

[0169] <Synthesized Example 4>

[0170] In an autoclave with a net capacity of 2 liters, 1056 g of ion-exchanged water as a dispersion medium, 0.44 g of metholose SM-100 (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.) as a cellulose-based suspending agent, 0.22 g of acrylic acid (AA), 3.08 g of a 50 mass% concentration tertiary-butyl peroxypivalate-HFE-347pc-f solution as a polymerization initiator, 0.44 g of isododecane as a chain transfer agent, and 440 g of vinylidene fluoride were added, and the temperature was raised to 52°C over 110 minutes. While maintaining the temperature at 52°C, 3.74 g of a 1 mass% concentration aqueous AA solution (in terms of solute) was added to maintain the pressure immediately after the end of the heating process. The reaction was continued until the pressure in the system was lowered to 7.18 MPaG.

[0171] By treating the obtained polymer slurry in the same manner as in Synthesis Example 1, a powder of vinylidene fluoride copolymer (VDF / AA-2), which is a copolymer of vinylidene fluoride (VDF) and acrylic acid (AA), was obtained. The inherent viscosity, weight average molecular weight Mwa of the vinylidene fluoride copolymer, and the weight average molecular weight Mwc of the carboxyl group-containing copolymer are shown in Table 1 below.

[0172] (3) Physical properties of vinylidene fluoride copolymer

[0173] The physical properties of the vinylidene fluoride copolymer are shown below.

[0174]

[0175] 3. Preparation of electrode mixture

[0176] Each electrode mixture was prepared using the following method.

[0177] (Example 1)

[0178] LFP-A was used as the electrode active material, VDF / APS-1 as the vinylidene fluoride copolymer (binder), and a carbon nanotube (CNT) NMP dispersion as the conductivity aid. Then, an electrode composite was prepared by mixing these using a planetary rotational mixer, the AWATORI RENTARO ARE310 product of THINKY CORPORATION. The mass ratio of the electrode active material, conductivity aid, and binder in the obtained electrode composite was 100:2:2.5, and the solid content concentration was 55.0 mass%. The slurry viscosity at this time is shown in Table 2.

[0179] (Examples 2–5, Comparative Examples 1–5 and Reference Examples 1, 2)

[0180] As shown in Table 2, the electrode composite was prepared in the same manner as in Example 1, except that the type of electrode active material and the type of vinylidene fluoride copolymer were changed, and in Example 4 and Comparative Example 4, the solid content concentration was changed to 52 mass%.

[0181] (result)

[0182]

[0183] As shown in Table 2 above, when an active material not coated with carbon (LCO) was used, there was no significant difference depending on the difference in the vinylidene fluoride copolymer having carboxyl groups (Reference Examples 1 and 2). In contrast, when an active material coated with carbon was used, even when the same active material was used, the slurry viscosity (particularly the shear rate s) varied depending on the difference in Mwc. -1There was a significant difference in (in the case of), and there was also a significant difference in the viscosity ratio (e.g., comparison between Example 1 and Comparative Example 1). The same applies to the comparison between Examples 2 to 5 and Comparative Examples 2 to 5. Furthermore, if the weight-average molecular weight Mwc of the vinylidene fluoride copolymer is 1.3 million or less and the adsorption rate is greater than 0% and less than or equal to 30%, the initial slurry viscosity (shear rate s -1 The viscosity was 51041 mPa·s or less, and the viscosity ratio was also 11.2 or less (Examples 1-5). That is, there was no significant difference between Reference Example 1 and Reference Example 2.

[0184] The present application claims priority based on Patent Application No. 2024-056555 filed on March 29, 2024. All contents described in the specification of said application are incorporated by reference into the present specification.

[0185] Industrial applicability

[0186] According to the present invention, an electrode composite is provided comprising a carbon-coated electrode active material and a vinylidene fluoride copolymer having carboxyl groups, which has low initial viscosity and good handling properties. The electrode composite is very useful in the field of manufacturing various batteries.

Claims

Claim 1 An electrode composite comprising a vinylidene fluoride copolymer having constituent units derived from vinylidene fluoride and constituent units derived from a vinyl compound having a carboxyl group, and a carbon-coated electrode active material, wherein the carbon coating amount of the electrode active material is 0.5 mass% or more and 3.0 mass% or less relative to the mass of the electrode active material, and when the weight average molecular weight Mwc of the carboxyl-containing vinylidene fluoride copolymer that absorbs light of a wavelength of 345 nm is determined by modifying the vinylidene fluoride copolymer with a labeling material composed of 1-bromomethylpyrene, the weight average molecular weight Mwc is 1.3 million or less, and the vinylidene fluoride copolymer has an adsorption rate greater than 0% and less than or equal to 30% as determined by the following method. (Method for determining adsorption rate) (i) Prepare a dimethylacetamide solution having a concentration of vinylidene fluoride copolymer of 1 g / L. (ii) The dimethylacetamide Gel permeation chromatography is performed on the solution, and the peak area AR1 derived from the vinylidene fluoride copolymer is calculated by differential refractive index detection. (iii) 5 g of the dimethylacetamide solution has a BET specific surface area of ​​4 m² 2 / g or more than 5 m 2 (iv) Add 0.8 g of aluminum oxide at a concentration of 1 / g or less, stir for 2 hours, and then let stand for 16 hours. (iv) After standing, collect the supernatant of the dimethylacetamide solution and perform solid-liquid separation by centrifugation. (v) Perform gel permeation chromatography on the separated solution and calculate the peak area AR2 derived from the vinylidene fluoride copolymer by differential refractive index detection. (vi) Calculate the adsorption rate based on the following equation (1). Perform this three times, and the average value is taken as the adsorption rate. Adsorption rate = (AR1 - AR2) / AR1 × 100 Claim 2 The electrode composite according to claim 1, wherein the weight average molecular weight Mwc is 700,000 or less and the adsorption rate is 20% or less. Claim 3 The electrode composite according to claim 1, wherein the average particle diameter of the electrode active material is 15 μm or less. Claim 4 An electrode composite according to claim 1, wherein the carbon coating amount of the electrode active material is 2.5 mass% or less. Claim 5 An electrode composite according to claim 1, wherein the vinyl compound is a compound represented by the following general formula (1). [Chem 1] (In general formula (1), R 1 , R 2 , R 3 Each represents independently a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and X represents a hydroxyl group or -Y-COOH (Y represents an atomic group) Claim 6 An electrode composite according to claim 1, wherein the vinyl compound is a compound represented by the following general formula (1). [Chem 2] (In general formula (1), R 1 , R 2 , R 3 Each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and X represents a hydroxyl group or -Y-COOH (Y represents a divalent atomic group having a molecular weight of 500 or less, containing either an oxygen atom or a nitrogen atom and having 1 to 10 atoms in the main chain)) Claim 7 An electrode comprising a solid component of the electrode mixture described in any one of claims 1 to 6. Claim 8 A battery comprising the electrode described in paragraph 7.