Non-aqueous secondary battery separator and non-aqueous secondary battery
The separator for non-aqueous secondary batteries, with a heat-resistant porous layer containing barium sulfate particles, addresses gas generation and heat resistance issues, enhancing battery safety and productivity.
Patent Information
- Application Number
- KR1020267036204
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-03-20
- Filing Date
- 2020-03-23
- Publication Date
- 2026-11-09
AI Technical Summary
Existing separators for non-aqueous secondary batteries, particularly those with a porous layer containing barium sulfate particles, face challenges in suppressing gas generation and improving heat resistance while maintaining productivity.
A separator design featuring a porous substrate with a heat-resistant porous layer comprising barium sulfate particles of specific size and volume ratio, combined with a binder resin, enhances heat resistance and reduces gas generation, while ensuring high productivity.
The proposed separator effectively suppresses gas generation and improves heat resistance, contributing to the safety and efficiency of non-aqueous secondary batteries.
Smart Images

Figure PAT00001 
Figure PAT00002
Abstract
Description
Technology Field
[0001] The present disclosure relates to a separator for a non-aqueous secondary battery and a non-aqueous secondary battery. Background Technology
[0002] Non-aqueous rechargeable batteries, typified by lithium-ion batteries, are widely used as power sources for portable electronic devices such as laptops, mobile phones, digital cameras, and camcorders. Furthermore, due to their high energy density, the application of non-aqueous rechargeable batteries—represented by lithium-ion batteries—is being considered for power storage and as batteries for electric vehicles. With the widespread adoption of such non-aqueous rechargeable batteries, there is an increasing demand to enhance their safety.
[0003] A separator, which is one of the components constituting a non-aqueous secondary battery, requires heat resistance so that it does not easily rupture even when the inside of the battery becomes high temperature, in order to ensure the safety of the battery. As a separator with enhanced heat resistance, a separator is known that has a porous layer containing inorganic particles on a porous substrate. For example, Patent Document 1 or 2 discloses a separator that has a porous layer containing barium sulfate particles on a porous substrate. Prior art literature
[0004] Japanese Patent No. 5429811 International Publication No. 2014 / 148036 The problem to be solved
[0005] Upon examination by the inventors, it was found that a separator having a porous layer containing barium sulfate particles on a porous substrate is less likely to cause gas generation due to the decomposition of the electrolyte or electrolyte compared to a separator having a porous layer containing magnesium hydroxide or alumina on a porous substrate. Therefore, by further improving the heat resistance of the porous layer containing barium sulfate particles, a separator that significantly contributes to the safety of the battery can be provided. Furthermore, in a separator using barium sulfate particles, it is also important to increase productivity.
[0006] An embodiment of the present disclosure was carried out under the above circumstances.
[0007] One embodiment of the present disclosure aims to provide a separator for a non-aqueous secondary battery that suppresses gas generation inside the battery, has excellent heat resistance, and also has excellent productivity.
[0008] In addition, another embodiment of the present disclosure aims to provide a non-aqueous secondary battery in which gas generation inside the battery is suppressed, heat resistance is excellent, and productivity is improved. means of solving the problem
[0009] Specific means for solving the above problem include the following aspects.
[0010] [1] A separator for a non-aqueous secondary battery, comprising a porous substrate and a heat-resistant porous layer provided on one or both sides of the porous substrate, the layer comprising a binder resin and barium sulfate particles, wherein the average primary particle size of the barium sulfate particles included in the heat-resistant porous layer is 0.01 μm or more and less than 0.30 μm, and the volume ratio of the barium sulfate particles in the heat-resistant porous layer is 30 volume% or more and less than 50 volume%.
[0011] [2] A separator for a non-aqueous secondary battery as described in [1], wherein the binder resin comprises a polyvinylidene fluoride-based resin.
[0012] [3] A separator for a non-aqueous secondary battery described in [2], having a weight average molecular weight of 600,000 to 3,000,000 of the polyvinylidene fluoride resin.
[0013] [4] A separator for a non-aqueous secondary battery as described in any one of [1] to [3], wherein the binder resin comprises at least one selected from the group consisting of all-aromatic polyamide, polyamideimide, poly-N-vinylacetamide, polyacrylamide, copolymerized polyetherpolyamide, polyimide and polyetherimide.
[0014] [5] A separator for a non-aqueous secondary battery described in any one of [1] to [4], having an area shrinkage rate of 30% or less when the separator for a non-aqueous secondary battery is heat-treated at 135°C for 1 hour.
[0015] [6] A separator for a non-aqueous secondary battery described in any one of [1] to [5], having an area shrinkage rate of 45% or less when the separator for a non-aqueous secondary battery is heat-treated at 150°C for 1 hour.
[0016] [7] A separator for a non-aqueous secondary battery described in any one of [1] to [6], wherein the porosity of the heat-resistant porous layer is 30% to 70%.
[0017] [8] The heat-resistant porous layer described above is a separator for a non-aqueous secondary battery described in any one of [1] to [7], having a mass per unit area of 1.0 g / m² to 30.0 g / m² total on both sides.
[0018] [9] A separator for a non-aqueous secondary battery described in any one of [1] to [8], wherein the above heat-resistant porous layer is provided on one side of the porous substrate.
[0019]
[10] A non-aqueous secondary battery having a positive electrode, a negative electrode, and a separator for a non-aqueous secondary battery described in any one of [1] to [9] disposed between the positive electrode and the negative electrode, and obtaining an electromotive force by doping and talping of lithium. Effects of the invention
[0020] According to one embodiment of the present disclosure, a separator for a non-aqueous secondary battery is provided, which suppresses gas generation inside the battery and has excellent heat resistance and also excellent productivity.
[0021] According to another embodiment of the present disclosure, a non-aqueous secondary battery is provided in which gas generation within the battery is suppressed, heat resistance is excellent, and productivity is improved. Specific details for implementing the invention
[0022] Embodiments of the present disclosure are described below. These descriptions and examples are illustrative of embodiments and do not limit the scope of the embodiments.
[0023] In the present disclosure, numerical ranges indicated by "~" represent a range that includes the values described before and after "~" as minimum and maximum values, respectively. In numerical ranges described stepwise in the present disclosure, an upper or lower limit value described in any numerical range may be substituted with an upper or lower limit value of a numerical range described in another stepwise manner. Furthermore, in numerical ranges described in the present disclosure, an upper or lower limit value described in any numerical range may be substituted with a value shown in an example.
[0024] In the present disclosure, the term “process” includes not only independent processes but also cases where the process cannot be clearly distinguished from other processes, provided that the intended purpose of the process is achieved.
[0025] When referring to the amount of each component in the composition in the present disclosure, if there are multiple types of substances corresponding to each component in the composition, it means the total amount of said multiple types of substances present in the composition, unless specifically limited otherwise.
[0026] In the present disclosure, “MD” refers to the elongated direction (i.e., the conveying direction) in a porous substrate and separator manufactured in an elongated form, and is also referred to as the “machine direction.” Additionally, “TD” refers to a direction orthogonal to “MD,” and is also referred to as the “transverse direction.”
[0027] In the present disclosure, the notation “(meth)acrylic” means “acrylic” or “methacrylic”.
[0028] In the present disclosure, the term "monomer unit" of a resin refers to a constituent unit of a resin, which is formed by the polymerization of monomers.
[0029] In the present disclosure, a combination of two or more preferred embodiments is a more preferred embodiment.
[0030] In the present disclosure, the amount of each component in a composition or layer refers to the total amount of a plurality of substances present in the composition, unless specifically limited, where a plurality of substances corresponding to each component exist in the composition.
[0031] Also, in the present disclosure, “mass%” and “weight%” are synonymous, and “parts of mass” and “parts of weight” are synonymous.
[0032] In the present disclosure, a heat-resistant resin refers to a resin having a melting point of 200°C or higher, or a resin having no melting point and a decomposition temperature of 200°C or higher. That is, a heat-resistant resin in the present disclosure is a resin that does not melt or decompose in a temperature range of less than 200°C.
[0033] Separator for Non-Aqueous Secondary Batteries
[0034] A separator for a non-aqueous secondary battery of the present disclosure (also simply referred to as "separator" in the present disclosure) comprises a porous substrate and a heat-resistant porous layer provided on one or both sides of the porous substrate.
[0035] In the separator of the present disclosure, the heat-resistant porous layer comprises a binder resin and barium sulfate particles, the average primary particle size of the barium sulfate particles included in the heat-resistant porous layer is 0.01 μm or more and less than 0.30 μm, and the volume ratio of the barium sulfate particles in the heat-resistant porous layer is 30 volume% or more and less than 50 volume%.
[0036] Compared to magnesium hydroxide or alumina, barium sulfate particles are less likely to decompose the electrolyte or electrolyte, and therefore are less likely to cause gas generation. For this reason, by using barium sulfate particles as an inorganic filler in a heat-resistant porous layer, a separator is obtained that is less likely to cause gas generation and less likely to cause swelling or deformation of the battery.
[0037] In the separator of the present disclosure, the average primary particle size of the barium sulfate particles included in the heat-resistant porous layer is less than 0.30 μm from the perspective of increasing the heat resistance of the heat-resistant porous layer. If the average primary particle size of the barium sulfate particles is less than 0.30 μm, the heat resistance of the heat-resistant porous layer is increased. As for the mechanism, it can be thought that because the particle size of the barium sulfate particles is small, the surface area (specific surface area) of the barium sulfate particles per unit volume increases, and therefore, the contact points between the barium sulfate particles and the binder resin increase, so the shrinkage of the heat-resistant porous layer when exposed to high temperatures is suppressed. In addition, it is presumed that because many barium sulfate particles with small particle sizes are connected to each other, the heat-resistant porous layer becomes less likely to break when exposed to high temperatures.
[0038] From the above perspective, the average primary particle size of the barium sulfate particles is less than 0.30㎛, more preferably 0.28㎛ or less, and more preferably 0.25㎛ or less.
[0039] In the separator of the present disclosure, the average primary particle size of the barium sulfate particles included in the heat-resistant porous layer is 0.01 μm or more, more preferably 0.05 μm or more, and more preferably 0.10 μm or more, from the perspective of suppressing aggregation between particles to form a heat-resistant porous layer with high uniformity.
[0040] Hereinafter, details of the porous substrate and heat-resistant porous layer having of the separator of the present disclosure will be described.
[0041] [Porous substrate]
[0042] In the present disclosure, a porous substrate means a substrate having pores or voids inside.
[0043] Examples of such materials include microporous membranes; porous sheets made of fibrous materials, such as nonwoven fabrics or paper; and composite porous sheets in which one or more other porous layers are laminated onto these microporous membranes or porous sheets. In the present disclosure, microporous membranes are preferred from the viewpoint of thinning and strength of the separator.
[0044] A microporous membrane refers to a membrane that has a large number of micropores within it, structured so that these micropores are interconnected, allowing gas or liquid to pass from one side to the other.
[0045] As for the porous substrate material, a material having electrical insulating properties is preferred, and it may be either an organic material or an inorganic material.
[0046] It is preferable that the porous substrate includes a thermoplastic resin to impart a shutdown function to the porous substrate. The shutdown function refers to a function that prevents thermal runaway of the battery by blocking the movement of ions through the melting of the constituent materials and the blocking of the pores of the porous substrate when the battery temperature rises. As for the thermoplastic resin, a thermoplastic resin with a melting point of less than 200°C is preferred. Examples of thermoplastic resins include polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; among these, polyolefins are preferred.
[0047] As a porous substrate, a microporous membrane comprising a polyolefin (referred to as a "polyolefin microporous membrane" in this disclosure) is preferred. As for the polyolefin microporous membrane, for example, a polyolefin microporous membrane applied to a conventional battery separator may be cited, and among these, it is preferable to select one that possesses sufficient mechanical properties and ion permeability.
[0048] In terms of exhibiting a shutdown function, a polyolefin microporous membrane containing polyethylene is preferred. As for the polyethylene content in the polyolefin microporous membrane, it is preferable to have 95 mass% or more with respect to the total mass of the polyolefin microporous membrane.
[0049] A polyolefin microporous membrane is preferably a microporous membrane containing polypropylene in terms of having heat resistance that prevents it from easily rupturing when exposed to high temperatures.
[0050] From the perspective of providing a shutdown function and heat resistance that prevents easy rupture when exposed to high temperatures, a polyolefin microporous membrane comprising polyethylene and polypropylene is preferred. Examples of such a polyolefin microporous membrane include a microporous membrane in which polyethylene and polypropylene are mixed in a single layer. In the microporous membrane, from the perspective of achieving a balance between the shutdown function and heat resistance, it is preferable to include 95 mass% or more of polyethylene and more than 0 mass% and 5 mass% or less of polypropylene. Furthermore, from the perspective of achieving a balance between the shutdown function and heat resistance, a polyolefin microporous membrane having a laminated structure of two or more layers, wherein at least one layer of the laminated structure comprises polyethylene and at least one layer comprises polypropylene, is also preferred.
[0051] As for the polyolefin included in the polyolefin microporous membrane, a polyolefin having a weight-average molecular weight (Mw) of 100,000 to 5 million is preferred. If the Mw of the polyolefin is 100,000 or higher, sufficient mechanical properties can be imparted to the microporous membrane. On the other hand, if the Mw of the polyolefin is 5 million or lower, the shutdown characteristics of the microporous membrane are good, and the microporous membrane is easy to mold.
[0052] In addition, the weight-average molecular weight is measured by gel permeation chromatography (GPC). Details of the measurement by GPC will be described later.
[0053] Methods for manufacturing a polyolefin microporous membrane include a method of extruding molten polyolefin resin from a T-die to form a sheet, crystallizing the sheet, stretching it, and then heat treating it to form a microporous membrane; and a method of extruding molten polyolefin resin together with a plasticizer such as liquid paraffin from a T-die, cooling the sheet to form a sheet, stretching it, extracting the plasticizer, and then heat treating it to form a microporous membrane.
[0054] Examples of porous sheets made of fibrous materials include nonwoven fabrics, papers, etc., made of polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; heat-resistant resins such as fully aromatic polyamides, polyamideimide, polyimide, polyethersulfone, polysulfone, polyetherketone, and polyetherimide; and fibrous materials such as cellulose.
[0055] Examples of composite porous sheets include a sheet in which a functional layer is laminated onto a porous sheet made of a microporous membrane or a fibrous material. Such a composite porous sheet is desirable in that additional functionality can be added through the functional layer. As for the functional layer, for example, in terms of providing heat resistance, a porous layer made of a heat-resistant resin or a porous layer made of a heat-resistant resin and an inorganic filler can be cited.
[0056] As heat-resistant resins, one or more heat-resistant resins selected from fully aromatic polyamides, polyimides, polyethersulfones, polysulfones, polyetherketones, and polyetherimides may be used.
[0057] Examples of inorganic fillers include metal oxides such as alumina; metal hydroxides such as magnesium hydroxide.
[0058] Methods of composite formation include coating a functional layer onto a microporous membrane or porous sheet, bonding the microporous membrane or porous sheet and the functional layer with an adhesive, and heat-pressing the microporous membrane or porous sheet and the functional layer.
[0059] Various surface treatments may be performed on the surface of the porous substrate to improve wettability with the coating solution for forming a heat-resistant porous layer, provided that the properties of the porous substrate are not damaged. Examples of surface treatments include corona treatment, plasma treatment, flame treatment, and ultraviolet irradiation treatment.
[0060] ~Characteristics of porous substrates~
[0061] From the perspective of increasing the energy density of the battery, the thickness of the porous substrate is preferably 15 μm or less, and more preferably 12 μm or less. From the perspective of the manufacturing yield of the separator and the manufacturing yield of the battery, the thickness of the porous substrate is preferably 4 μm or more, and more preferably 6 μm or more.
[0062] The gully value (JIS P8117:2009) of the porous substrate is preferably 50 seconds / 100mL to 400 seconds / 100mL from the perspective of ion permeability or suppression of short circuits in the battery.
[0063] The porosity of the porous substrate is preferably 20% to 60% from the perspective of obtaining appropriate membrane resistance or shutdown function. The porosity ε(%) of the porous substrate is calculated by the following formula.
[0064] ε={1-(Wa / da+Wb / db+Wc / dc+…+Wn / dn) / t}×100
[0065] Here, the constituent materials of the porous substrate are a, b, c, … , n, the mass of each constituent material is Wa, Wb, Wc, … , Wn (g / cm²), the true density of each constituent material is da, db, dc, … , dn (g / cm³), and the thickness of the porous substrate is t (cm).
[0066] The average pore size of the porous substrate is preferably 20 nm to 100 nm from the perspective of ion permeability or suppression of short circuits in the battery. The average pore size of the porous substrate is measured using a pump phorometer in accordance with ASTM E1294-89.
[0067] The thrust strength of the porous substrate is preferably 200g or more from the perspective of the manufacturing yield of the separator and the manufacturing yield of the battery. The thrust strength of the porous substrate refers to the maximum thrust load (g) measured by performing a thrust test using a Katotecsha KES-G5 hand compression tester under conditions of a radius of curvature of the needle tip of 0.5mm and a thrust speed of 2mm / sec.
[0068] [Heat-resistant porous layer]
[0069] The heat-resistant porous layer in the separator of the present disclosure contains at least a binder resin and barium sulfate particles. The heat-resistant porous layer is a layer having a plurality of micropores and capable of allowing a gas or liquid to pass from one side to the other.
[0070] In the separator of the present disclosure, the heat-resistant porous layer may be located on only one side of the porous substrate or on both sides of the porous substrate. If the heat-resistant porous layer is located on both sides of the porous substrate, the heat resistance of the separator is superior, thereby increasing the safety of the battery. Additionally, curling is less likely to occur in the separator, resulting in excellent handling properties during battery manufacturing. If the heat-resistant porous layer is located on only one side of the porous substrate, the ion permeability of the separator is superior. Furthermore, the overall thickness of the separator can be reduced, allowing for the manufacture of a battery with a higher energy density.
[0071] -Binder Resin-
[0072] The heat-resistant porous layer in the present disclosure contains a binder resin.
[0073] The type of binder resin of the heat-resistant porous layer is not particularly limited, as long as it is capable of binding inorganic particles. The binder resin of the heat-resistant porous layer is preferably a heat-resistant resin (a resin with a melting point of 200°C or higher, or a resin that has no melting point but has a decomposition temperature of 200°C or higher). The binder resin of the heat-resistant porous layer is preferably a resin that is stable with respect to the electrolyte and is also electrochemically stable.
[0074] The binder resin may be used as a single type or in combination of two or more types.
[0075] It is preferable that the binder resin of the heat-resistant porous layer has adhesion to the electrode of the battery, and the type of binder resin may be selected according to the composition of the positive or negative electrode. When the heat-resistant porous layer is present on both sides of the porous substrate, the binder resin of the heat-resistant porous layer on one side and the binder resin of the heat-resistant porous layer on the other side may be the same or different from each other.
[0076] As a binder resin for a heat-resistant porous layer, a polymer having polar functional groups or atomic groups (e.g., hydroxyl groups, carboxyl groups, amino groups, amide groups, carbonyl groups) is preferred.
[0077] Examples of binder resins for a heat-resistant porous layer include, specifically, polyvinylidene fluoride resin, fully aromatic polyamide, polyamideimide, polyimide, polyethersulfone, polysulfone, polyetherketone, polyketone, polyetherimide, poly-N-vinylacetamide, polyacrylamide, copolymerized polyetherpolyamide, fluorinated rubber, acrylic resin, styrene-butadiene copolymer, cellulose, polyvinyl alcohol, etc.
[0078] The binder resin of the heat-resistant porous layer may be a particulate resin, for example, particles of a resin such as polyvinylidene fluoride resin, fluororubber, or styrene-butadiene copolymer. The binder resin of the heat-resistant porous layer may be a water-soluble resin such as cellulose or polyvinyl alcohol. When a particulate resin or a water-soluble resin is used as the binder resin of the heat-resistant porous layer, a coating solution can be prepared by dispersing or dissolving the binder resin in water, and a heat-resistant porous layer can be formed on a porous substrate by a dry coating method using said coating solution.
[0079] As a binder resin for a heat-resistant porous layer, fully aromatic polyamide, polyamideimide, poly-N-vinylacetamide, polyacrylamide, copolymerized polyetherpolyamide, polyimide, or polyetherimide is preferred from the perspective of excellent heat resistance. It is preferable that these resins be heat-resistant resins (resins with a melting point of 200°C or higher, or resins that do not have a melting point but have a decomposition temperature of 200°C or higher).
[0080] Among heat-resistant resins, fully aromatic polyamides (aramids) are preferred from the perspective of durability. The fully aromatic polyamide may be of the meta-type or the para-type. Among the fully aromatic polyamides, the meta-type fully aromatic polyamide is preferred from the perspective of ease of forming a porous layer and excellent redox resistance in electrode reactions. A small amount of aliphatic monomer may be copolymerized in the fully aromatic polyamide.
[0081] As for the all-aromatic polyamide used as the binder resin of the heat-resistant porous layer, specifically, polymetaphenylene isophthalamide or polyparaphenylene terephthalamide is preferred, and polymetaphenylene isophthalamide is more preferred.
[0082] As the binder resin for the heat-resistant porous layer, a polyvinylidene fluoride-based resin (PVDF-based resin) is preferred in terms of adhesion to the electrode.
[0083] PVDF-based resins are suitable as binder resins for heat-resistant porous layers in terms of adhesion to electrodes. By containing PVDF-based resin in the heat-resistant porous layer, the adhesion between the heat-resistant porous layer and the electrode is improved, and as a result, the strength of the battery (cell strength) is enhanced.
[0084] Examples of PVDF-based resins include homopolymers of vinylidene fluoride (i.e., polyvinylidene fluoride); copolymers of vinylidene fluoride with other monomers (polyvinylidene fluoride copolymers); and mixtures of polyvinylidene fluoride and polyvinylidene fluoride copolymers. Examples of monomers copolymerizable with vinylidene fluoride include tetrafluoroethylene, hexafluoropropylene, trifluoroethylene, chlorotrifluoroethylene, trichloroethylene, vinyl fluoride, trifluoroperfluoropropyl ether, ethylene, (meth)acrylic acid, methyl (meth)acrylate, (meth)acrylic acid ester, vinyl acetate, vinyl chloride, acrylonitrile, etc. These monomers may be used individually or in combination of two or more types.
[0085] As for the PVDF-based resin included in the heat-resistant porous layer, a copolymer (VDF-HFP copolymer) containing vinylidene fluoride monomer units (VDF units) and hexafluoropropylene monomer units (HFP units) is more preferable from the perspective of adhesion to the electrode. When the VDF-HFP copolymer is used as the binder resin of the heat-resistant porous layer, it is easy to control the crystallinity and heat resistance of the binder resin within an appropriate range, and it is possible to suppress the heat-resistant porous layer from flowing during the heat press treatment for bonding the separator to the electrode.
[0086] As for the VDF-HFP copolymer included in the heat-resistant porous layer, it may be a copolymer consisting only of VDF units and HFP units, or a copolymer comprising VDF units and HFP units and other monomer units other than VDF units and HFP units. Examples of other monomers include tetrafluoroethylene, trifluoroethylene, chlorotrifluoroethylene, trichloroethylene, vinyl fluoride, etc.
[0087] In the VDF-HFP copolymer, the content of VDF units is preferably 91 mol% or more from the perspective of controlling the crystallinity and heat resistance of the VDF-HFP copolymer to an appropriate range.
[0088] The content of HFP units in the VDF-HFP copolymer is preferably 1 mol% or more, more preferably 2 mol% or more, from the view that it swells appropriately when impregnated with an electrolyte and has excellent adhesion by a wet heat press, and is preferably 7 mol% or less, more preferably 6 mol% or less, from the view that it is difficult to dissolve in an electrolyte.
[0089] The PVDF-based resin included in the heat-resistant porous layer preferably has a weight average molecular weight (Mw) of 600,000 to 3 million. If the Mw of the PVDF-based resin is 600,000 or more, it is easy to obtain a heat-resistant porous layer having mechanical properties capable of withstanding the heat press treatment when bonding the separator to the electrode, and the adhesion between the electrode and the heat-resistant porous layer is improved. From this perspective, the Mw of the PVDF-based resin is more preferably 800,000 or more, and more preferably 1 million or more. On the other hand, if the Mw of the PVDF-based resin is 3 million or less, the viscosity during molding of the heat-resistant porous layer does not become too high, resulting in good moldability and crystal formation, and making it easy for the heat-resistant porous layer to become porous. From this perspective, the Mw of the PVDF-based resin is more preferably 2.5 million or less, and more preferably 2 million or less.
[0090] In addition, the weight-average molecular weight of the binder resin of the heat-resistant porous layer is measured by gel permeation chromatography (GPC). The measurement is performed using the GPC device "GPC-900" manufactured by Nihon Bunkosha, using two TSKgel SUPER AWM-H manufactured by Tososha as columns, using dimethylformamide as the solvent, under conditions of a temperature of 40°C and a flow rate of 10 mL / min, and is obtained as the molecular weight equivalent to polystyrene.
[0091] The PVDF-based resin included in the heat-resistant porous layer preferably has an acid value of 3 mgKOH / g to 20 mgKOH / g.
[0092] The acid value of a PVDF-based resin can be controlled, for example, by introducing carboxyl groups into the PVDF-based resin. The introduction of carboxyl groups into the PVDF-based resin and the amount of introduction can be controlled by using a monomer having a carboxyl group (for example, (meth)acrylic acid, (meth)acrylic acid ester, maleic acid, maleic anhydride, maleic acid ester, and fluorine-substituted derivatives thereof) as a polymerization component of the PVDF-based resin and adjusting the polymerization ratio.
[0093] The fibrillation diameter of the PVDF-based resin included in the heat-resistant porous layer is preferably 10 nm to 1000 nm from the perspective of the cycle characteristics of the battery.
[0094] As a binder resin for a heat-resistant porous layer, PVDF-based resin or all-aromatic polyamide (aramid) is preferred from the perspective that a dramatic effect is obtained by combining it with barium sulfate particles having an average primary particle size of less than 0.30 μm. When PVDF-based resin or all-aromatic polyamide (aramid) is combined with barium sulfate particles having an average primary particle size of less than 0.30 μm, the heat resistance of the heat-resistant porous layer is dramatically increased compared to the case where barium sulfate particles having an average primary particle size of 0.30 μm or more are used.
[0095] Regarding the content ratio of binder resin in the heat-resistant porous layer, from the perspective of imparting heat resistance, it is preferable to have a volume ratio of 70 volume% or less, more preferable to have 65 volume% or less, more preferable to have 63 volume% or less, and particularly preferable to have 60 volume% or less. In addition, regarding the prevention of peeling or detachment of the heat-resistant porous layer from the porous substrate, it is preferable for the content ratio of binder resin to exceed 50 volume%, and more preferable to have 52 volume% or more.
[0096] The heat-resistant porous layer in the separator of the present disclosure may include a resin other than the binder resin.
[0097] Other resins are used for purposes such as improving the adhesion of the heat-resistant porous layer to the electrode, adjusting the ion permeability or membrane resistance of the heat-resistant porous layer, etc.
[0098] Other resins include, for example, fluororubber, styrene-butadiene copolymer, acrylic resin, styrene-acrylic resin, homopolymer or copolymer of vinylnitrile compounds (acrylonitrile, methacrylonitrile, etc.), carboxymethylcellulose, hydroxyalkylcellulose, polyvinyl alcohol, polyvinyl butyral, polyvinylpyrrolidone, polyether (polyethylene oxide, polypropylene oxide, etc.).
[0099] In the separator of the present disclosure, when the heat-resistant porous layer comprises other resins, the total content of other resins other than the binder resin included in the heat-resistant porous layer is preferably 50 mass% or less, more preferably 30 mass% or less, and more preferably 10 mass% or less with respect to the total amount of resins included in the heat-resistant porous layer. The lower limit of the total content of other resins is a value exceeding 0 mass%.
[0100] -Barium Sulfate Particles-
[0101] The separator of the present disclosure contains barium sulfate particles in a heat-resistant porous layer. By selectively including barium sulfate particles among the particles in the heat-resistant porous layer, the generation of gas due to the decomposition of the electrolyte or electrolyte is suppressed.
[0102] The average primary particle size of the barium sulfate particles included in the heat-resistant porous layer is 0.01 μm or more and less than 0.30 μm. As for the lower limit of the average primary particle size, 0.05 μm or more is preferred, and 0.10 μm or more is more preferred. As for the upper limit of the average primary particle size, 0.28 μm or less is preferred, and 0.25 μm or less is more preferred.
[0103] The average primary particle size of the barium sulfate particles is 0.01 μm or larger from the perspective of agglomeration or the agglomeration of the barium sulfate particles. In addition, if the average primary particle size of the barium sulfate particles is less than 0.30 μm, there are fewer convex parts protruding from the surface of the heat-resistant porous layer, and the shrinkage of the heat-resistant porous layer when exposed to high temperatures can be suppressed, resulting in excellent heat resistance.
[0104] The average primary particle size of the filler is determined by measuring the major axes of 100 randomly selected filler particles during observation by scanning electron microscope (SEM) and averaging the 100 major axes. The sample provided for SEM observation is a filler particle that is a material of a heat-resistant porous layer, or a filler particle taken from a separator. There are no restrictions on the method of taking the filler particles from the separator; for example, a method of taking the filler particles by heating the separator to about 800°C to remove the binder resin, or a method of taking the filler particles by immersing the separator in an organic solvent to dissolve the binder resin with the organic solvent.
[0105] When the average primary particle size of the filler is small, or when the filler aggregation is significant and the major axis of the filler cannot be measured, the specific surface area of the filler is measured by the BET method, and assuming the filler is a true sphere, the particle size is calculated from the specific gravity and specific surface area of the filler according to the following formula.
[0106] Average primary particle size (㎛) = 6 ÷ [Specific gravity (g / cm³) × BET specific surface area (m² / g)]
[0107] In addition, for the measurement of specific surface area by the BET method, an inert gas is used as the adsorbate and adsorbed onto the surface of filler particles at the boiling point of liquid nitrogen (-196°C). The amount of gas adsorbed onto the sample is measured as a function of the adsorbate pressure, and the specific surface area of the sample is calculated from the adsorption amount.
[0108] There are no limitations on the shape of the barium sulfate particles, and they may be spherical, elliptical, plate-shaped, needle-shaped, or irregular. For the barium sulfate particles included in the heat-resistant porous layer, it is preferable that they be plate-shaped or spherical particles, or primary particles that are not aggregated, from the perspective of suppressing short circuits in the battery and facilitating dense filling of the filler.
[0109] The volume ratio of barium sulfate particles in the heat-resistant porous layer is 30 volume% or more, 35 volume% or more is preferable, 37 volume% or more is more preferable, and 40 volume% or more is more preferable from the perspective of heat resistance.
[0110] On the other hand, if the volume ratio of barium sulfate particles in the heat-resistant porous layer is too high, the heat-resistant porous layer may become prone to peeling off from the porous substrate. If the heat-resistant porous layer detaches, it becomes a coating defect, which may lead to a decrease in the productivity of the separator. Furthermore, if the volume ratio of barium sulfate particles increases, the surface area of the barium sulfate particles increases, which leads to greater interaction with the binder resin and may result in a higher viscosity of the coating solution used to form the heat-resistant porous layer. If the viscosity of the coating solution is high, coating lines and wrinkles may occur, easily causing a deterioration in the appearance of the coating and potentially leading to a decrease in the productivity of the separator. From this perspective, it is preferable that the volume ratio of barium sulfate particles in the heat-resistant porous layer be less than 50 volume% and 48 volume% or less.
[0111] As for the content ratio (barium sulfate particle / binder resin ratio) of barium sulfate particles and binder resin included in the heat-resistant porous layer, a volume ratio of 32 / 68 to 49 / 51 is preferred, and 36 / 64 to 48 / 52 is more preferred.
[0112] In the separator of the present disclosure, the heat-resistant porous layer may contain other inorganic particles other than barium sulfate particles. However, the volume ratio of other inorganic particles in the heat-resistant porous layer is preferably 20 volume% or less, more preferably 10 volume% or less, more preferably 5 volume% or less, and is particularly preferably not substantially included.
[0113] Other inorganic particles may include, for example, particles of metal hydroxides such as aluminum hydroxide, magnesium hydroxide, calcium hydroxide, chromium hydroxide, zirconium hydroxide, cerium hydroxide, nickel hydroxide, and boron hydroxide; particles of metal oxides such as silica, alumina, titania, zirconia, and magnesium oxide; particles of carbonates such as calcium carbonate and magnesium carbonate; particles of sulfates such as calcium sulfate; and clay minerals such as calcium phosphate, apatite, calcium silicate, and talc. Among other inorganic particles, particles of metal hydroxides or particles of metal oxides are preferred from the perspective of stability with respect to the electrolyte and electrochemical stability. Other inorganic particles may be surface-modified by a silane coupling agent, etc.
[0114] There are no limitations on the shape of other inorganic particles, and they may be spherical, elliptical, plate-shaped, needle-shaped, or irregular. From the perspective of suppressing short circuits in the battery, it is preferable that the other inorganic particles included in the heat-resistant porous layer be spherical or plate-shaped particles, or primary particles that are not aggregated.
[0115] Other inorganic particles may be used as a single type or in combination of two or more types.
[0116] The average primary particle size of other inorganic particles is preferably 0.01㎛ to 5.00㎛. As a lower limit, it is more preferable to have a value of 0.10㎛ or more, and as an upper limit, it is more preferable to have a value of 1.00㎛ or less.
[0117] The heat-resistant porous layer in the separator of the present disclosure may contain an organic filler.
[0118] Examples of organic fillers include particles composed of cross-linked polymers such as cross-linked poly(meth)acrylic acid, cross-linked poly(meth)acrylic acid ester, cross-linked polysilicon, cross-linked polystyrene, cross-linked polydivinylbenzene, styrene-divinylbenzene copolymer crosslinker, melamine resin, phenol resin, benzoguanamine-formaldehyde condensate; and particles composed of heat-resistant polymers such as polysulfone, polyacrylonitrile, aramid, and polyacetal. These organic fillers may be used individually or in combination of two or more types.
[0119] In the separator of the present disclosure, the heat-resistant porous layer may include additives such as a dispersant, a surfactant, a wetting agent, an antifoaming agent, and a pH adjusting agent. The dispersant is added to the coating solution for forming the heat-resistant porous layer for the purpose of improving dispersibility, coating properties, or storage stability. The wetting agent, antifoaming agent, and pH adjusting agent are added to the coating solution for forming the heat-resistant porous layer for the purpose of, for example, improving affinity with the porous substrate, suppressing air ingress into the coating solution, or adjusting the pH.
[0120] ~Characteristics of heat-resistant porous layer~
[0121] From the perspective of the heat resistance or handling properties of the separator, the thickness of the heat-resistant porous layer is preferably 0.5 μm or more on one side, and more preferably 1 μm or more. In addition, from the perspective of the handling properties of the separator or the energy density of the battery, the thickness of the heat-resistant porous layer is preferably 5 μm or less on one side, and more preferably 4 μm or less.
[0122] The thickness of the heat-resistant porous layer is preferably 1 μm or more, and more preferably 2 μm or more, as the sum of the thicknesses of the heat-resistant porous layers on both sides, whether the heat-resistant porous layer is on only one side of the porous substrate or on both sides. In addition, the sum of the thicknesses is preferably 10 μm or less, and more preferably 8 μm or less.
[0123] The mass of the heat-resistant porous layer per unit area, as the sum of the masses of the heat-resistant porous layers on both sides, is preferably 1.0 g / m² or more, more preferably 2.0 g / m² or more, more preferably 3.5 g / m² or more, more preferably 4.0 g / m² or more, and more preferably 4.5 g / m² or more, from the perspective of the heat resistance or handling properties of the separator. In addition, the mass of the heat-resistant porous layer per unit area, as the sum of the masses of the heat-resistant porous layers on both sides, is preferably 30.0 g / m² or less, more preferably 20.0 g / m² or less, more preferably 10.0 g / m² or less, and more preferably 8.0 g / m² or less, from the perspective of the handling properties of the separator or the energy density of the battery.
[0124] When heat-resistant porous layers are present on both sides of a porous substrate, the difference between the mass of one heat-resistant porous layer and the mass of the other heat-resistant porous layer is preferably 20 mass% or less with respect to the total of both sides, from the perspective of suppressing curling of the separator.
[0125] The porosity of the heat-resistant porous layer is preferably 30% or more from the perspective of the ion permeability of the separator, and is preferably 80% or less, more preferably 70% or less, more preferably 60% or less, and more preferably 50% or less from the perspective of the thermal dimensional stability of the separator. The porosity ε(%) of the heat-resistant porous layer is calculated by the following formula.
[0126] ε={1-(Wa / da+Wb / db+Wc / dc+…+Wn / dn) / t}×100
[0127] Here, the constituent materials of the heat-resistant porous layer are a, b, c, … , n, the mass of each constituent material is Wa, Wb, Wc, … , Wn (g / cm²), the true density of each constituent material is da, db, dc, … , dn (g / cm³), and the thickness of the heat-resistant porous layer is t (cm).
[0128] The average pore size of the heat-resistant porous layer is preferably 10 nm to 200 nm. If the average pore size is 10 nm or more, when the electrolyte is impregnated into the heat-resistant porous layer, it is difficult for the pores to become clogged even if the resin contained in the heat-resistant porous layer swells. If the average pore size is 200 nm or less, the uniformity of ion movement is high, and the cycle characteristics and load characteristics of the battery are excellent.
[0129] The average pore size (nm) of the heat-resistant porous layer is calculated by the following formula, assuming that all holes are cylindrical.
[0130] d=4V / S
[0131] In the formula, d represents the average pore diameter of the heat-resistant porous layer, V represents the pore volume per 1 m² of the heat-resistant porous layer, and S represents the pore surface area per 1 m² of the heat-resistant porous layer.
[0132] The volume of pores V per 1 m² of the heat-resistant porous layer is calculated from the porosity of the heat-resistant porous layer.
[0133] The porous surface area S per 1 m² of the heat-resistant porous layer is determined by the following method.
[0134] First, the specific surface area (m² / g) of the porous substrate and the specific surface area (m² / g) of the separator are calculated from the amount of nitrogen gas adsorbed by applying the BET equation to the nitrogen gas adsorption method. The specific surface area (m² / g) of each is multiplied by the mass per unit area (g / m²) to calculate the pore surface area per 1 m² of each. Then, the pore surface area S of the heat-resistant porous layer is calculated by subtracting the pore surface area per 1 m² of the porous substrate from the pore surface area per 1 m² of the separator.
[0135] The peel strength between the porous substrate and the heat-resistant porous layer is preferably 0.1 N / 10 mm or more, more preferably 0.2 N / 10 mm or more, and more preferably 0.3 N / 10 mm or more, in terms of the adhesion strength of the separator to the electrode. In the above view, it is preferable for the peel strength between the porous substrate and the heat-resistant porous layer to be higher, but typically, the peel strength is preferably 2 N / 10 mm or less. When the separator of the present disclosure has heat-resistant porous layers on both sides of the porous substrate, the peel strength between the porous substrate and the heat-resistant porous layer is preferably within the above range on both sides of the porous substrate.
[0136] Characteristics of Separators
[0137] The thickness of the separator of the present disclosure is preferably 10 μm or more and more preferably 12 μm or more from the perspective of the mechanical strength of the separator. In addition, the thickness of the separator is preferably 25 μm or less and more preferably 20 μm or less from the perspective of the energy density of the battery.
[0138] The protrusion strength of the separator of the present disclosure is preferably 250g to 1000g and more preferably 300g to 600g from the perspective of the mechanical strength of the separator or the short-circuit resistance of the battery. The method for measuring the protrusion strength of the separator is the same as the method for measuring the protrusion strength of a porous substrate.
[0139] The porosity of the separator of the present disclosure is preferably 30% to 60% in terms of adhesion to the electrode, handling properties of the separator, ion permeability, or mechanical strength.
[0140] The gully value (JIS P8117:2009) of the separator of the present disclosure is preferably 50 sec / 100mL to 800 sec / 100mL and more preferably 100 sec / 100mL to 400 sec / 100mL in terms of the balance of mechanical strength and ion permeability.
[0141] In the separator of the present disclosure, from the perspective of ion permeability, the value obtained by subtracting the gullibility value of the porous substrate from the gullibility value of the separator is preferably 300 s / 100 mL or less, more preferably 150 s / 100 mL or less, and more preferably 100 s / 100 mL or less. The lower limit of the value obtained by subtracting the gullibility value of the porous substrate from the gullibility value of the separator is not particularly limited, but in the separator of the present disclosure, it is typically 10 s / 100 mL or more.
[0142] The membrane resistance of the separator of the present disclosure is preferably 1 Ω·cm² to 10 Ω·cm² from the perspective of the battery load characteristics. Here, the membrane resistance of the separator refers to the resistance value when the separator is impregnated with an electrolyte, and is a value measured by the AC method at 20°C using 1 mol / L LiBF4-propylene carbonate:ethylene carbonate (mass ratio 1:1) as the electrolyte. The lower the membrane resistance of the separator, the better the ion permeability of the separator.
[0143] The curvature of the separator of the present disclosure is preferably 1.5 to 2.5 in terms of ion permeability.
[0144] The amount of water (based on mass) included in the separator of the present disclosure is preferably 1,000 ppm or less. The lower the amount of water in the separator, the more the reaction between the electrolyte and water is suppressed when the battery is formed, thereby suppressing gas generation within the battery and improving the cycle characteristics of the battery. In this regard, the amount of water included in the separator is more preferably 800 ppm or less, and even more preferably 500 ppm or less.
[0145] The separator of the present disclosure preferably has a shrinkage rate in MD of 30% or less when heat-treated at 135°C for 1 hour, more preferably 20% or less, more preferably 15% or less, more preferably 10% or less, and particularly preferably 0%.
[0146] The separator of the present disclosure preferably has a shrinkage rate at TD of 30% or less when heat-treated at 135°C for 1 hour, more preferably 20% or less, more preferably 15% or less, more preferably 10% or less, and particularly preferably 0%.
[0147] The separator of the present disclosure preferably has an area shrinkage rate of 30% or less when heat-treated at 135°C for 1 hour, more preferably 20% or less, more preferably 15% or less, more preferably 10% or less, and particularly preferably 0%.
[0148] The separator of the present disclosure preferably has a shrinkage rate in MD of 70% or less when heat-treated at 150°C for 1 hour, more preferably 55% or less, more preferably 45% or less, more preferably 20% or less, and more preferably 10%.
[0149] The separator of the present disclosure preferably has a shrinkage rate in TD of 70% or less when heat-treated at 150°C for 1 hour, more preferably 55% or less, more preferably 45% or less, more preferably 20% or less, and more preferably 10%.
[0150] The separator of the present disclosure has an area shrinkage rate of 70% or less when heat-treated at 150°C for 1 hour, more preferably 55% or less, more preferably 45% or less, more preferably 20% or less, and more preferably 10%.
[0151] The area shrinkage rate when the separator is heat-treated at 135°C or 150°C for 1 hour is determined by the following measurement method.
[0152] A separator is cut into a rectangular shape of MD 180 mm × TD 60 mm to serve as a test specimen. On this test specimen, marks are made at locations 20 mm and 170 mm from one end along the line that bisects the length in TD (referred to as Point A and Point B, respectively). Additionally, marks are made at locations 10 mm and 50 mm from one end along the line that bisects the length in MD (referred to as Point C and Point D, respectively). A clip is attached to the marked test specimen (the clip is attached between the end closest to Point A and Point A), and the specimen is suspended in an oven with the internal temperature adjusted to 135°C or 150°C, and heat treatment is performed for 1 hour under no tension. The lengths between A and C and between C and D are measured before and after the heat treatment, and the area shrinkage rate is calculated using the following formula.
[0153] Area shrinkage rate (%) = {1 - (Length of AB after heat treatment ÷ Length of AB before heat treatment) × (Length of CD after heat treatment ÷ Length of CD before heat treatment)} × 100
[0154] The shrinkage rate when the separator of the present disclosure is heat-treated can be controlled, for example, by the content of inorganic particles in the heat-resistant porous layer, the thickness of the heat-resistant porous layer, the porosity of the heat-resistant porous layer, etc.
[0155] The separator of the present disclosure may further have layers other than the porous substrate and the heat-resistant porous layer. Examples of other layers include an adhesive layer provided as the outermost layer for the main purpose of adhesion with the electrode.
[0156] [Method for manufacturing a separator]
[0157] The separator of the present disclosure can be manufactured, for example, by forming a heat-resistant porous layer on a porous substrate using a wet coating method or a dry coating method. In the present disclosure, a wet coating method is a method of solidifying the coating layer in a coagulation liquid, and a dry coating method is a method of solidifying the coating layer by drying it. An example of an embodiment of the wet coating method is described below.
[0158] The wet coating method is a method of coating a porous substrate with a coating solution containing binder resin and barium sulfate particles, immersing the coating layer in a coagulation solution to solidify it, and then removing it from the coagulation solution to perform washing and drying.
[0159] A coating solution for forming a heat-resistant porous layer is prepared by dissolving or dispersing a binder resin and barium sulfate particles in a solvent. If necessary, other components other than the binder resin and barium sulfate particles are dissolved or dispersed in the coating solution.
[0160] The solvent used in the preparation of the coating solution includes a solvent that dissolves the binder resin (hereinafter also referred to as a "good solvent"). Examples of good solvents include polar amide solvents such as N-methylpyrrolidone, dimethylacetamide, and dimethylformamide.
[0161] The solvent used to prepare the coating solution preferably contains a phase-separating agent that induces phase separation, from the perspective of forming a porous layer having a good porous structure. Therefore, the solvent used to prepare the coating solution is preferably a mixed solvent of both solvents and a phase-separating agent. It is preferable to mix the phase-separating agent with both solvents in an amount that can secure a viscosity suitable for the coating. Examples of phase-separating agents include water, methanol, ethanol, propyl alcohol, butyl alcohol, butanediol, ethylene glycol, propylene glycol, tripropylene glycol, etc.
[0162] As a solvent used for preparing a coating solution, from the perspective of forming a good porous structure, a mixed solvent of a solvent and a phase separation agent is preferred, wherein the mixed solvent contains 60 mass% or more of the solvent and 40 mass% or less of the phase separation agent.
[0163] The resin concentration of the coating solution is preferably 1 mass% to 20 mass% in terms of forming a good porous structure. The inorganic particle concentration of the coating solution is preferably 2 mass% to 50 mass% in terms of forming a good porous structure.
[0164] Examples of means for applying a coating solution to a porous substrate include Meyer bars, die coaters, reverse roll coaters, roll coaters, gravure coaters, etc. When forming a heat-resistant porous layer on both sides of a porous substrate, it is desirable from the perspective of productivity to apply the coating solution to both sides of the porous substrate simultaneously.
[0165] The solidification of the coating layer is achieved by immersing a porous substrate forming the coating layer in a coagulation solution to solidify the binder resin while inducing phase separation in the coating layer. In this way, a laminate consisting of a porous substrate and a heat-resistant porous layer is obtained.
[0166] The coagulation solution generally comprises the two solvents and phase separator used in the preparation of the coating solution, and water. For production purposes, it is desirable to match the mixing ratio of the two solvents and the phase separator to the mixing ratio of the mixed solvent used in the preparation of the coating solution. From the perspective of the formation of a porous structure and productivity, it is desirable that the water content in the coagulation solution be 40 mass% to 90 mass%. The temperature of the coagulation solution is, for example, 20°C to 50°C.
[0167] After solidifying the coating layer in the coagulation liquid, the laminate is lifted from the coagulation liquid and washed with water. The coagulation liquid is removed from the laminate by washing. Additionally, water is removed from the laminate by drying. Washing is performed, for example, by conveying the laminate through a water bath. Drying is performed, for example, by conveying the laminate through a high-temperature environment, exposing the laminate to air, or contacting the laminate with a heat roll. The drying temperature is preferably 40°C to 80°C.
[0168] The separator of the present disclosure can also be manufactured by a dry coating method. The dry coating method is a method of forming a heat-resistant porous layer on a porous substrate by coating a coating solution onto a porous substrate and drying the coating layer to volatilize and remove the solvent.
[0169] The separator of the present disclosure can also be manufactured by a method in which a heat-resistant porous layer is produced as an independent sheet, the heat-resistant porous layer is overlapped with a porous substrate, and the layers are combined by heat pressing or an adhesive. As a method for producing a heat-resistant porous layer as an independent sheet, a method of forming a heat-resistant porous layer on a release sheet by applying the wet coating method or dry coating method described above may be cited.
[0170] Non-aqueous secondary batteries
[0171] The non-aqueous secondary battery of the present disclosure is a non-aqueous secondary battery that obtains an electromotive force through doping and taldoping of lithium, and comprises a positive electrode, a negative electrode, and a separator for the non-aqueous secondary battery of the present disclosure. Doping refers to absorption, support, adsorption, or insertion, and refers to the phenomenon in which lithium ions enter the active material of an electrode such as a positive electrode.
[0172] The non-aqueous secondary battery of the present disclosure has a structure in which, for example, a battery element in which a negative electrode and a positive electrode face each other via a separator is enclosed within an outer casing together with an electrolyte. The non-aqueous secondary battery of the present disclosure is suitable for non-aqueous electrolyte secondary batteries, particularly lithium-ion secondary batteries.
[0173] The non-aqueous secondary battery of the present disclosure has excellent safety because the separator of the present disclosure suppresses gas generation inside the battery and has excellent heat resistance.
[0174] Hereinafter, examples of the forms of the positive electrode, negative electrode, electrolyte, and outer casing material provided by the non-aqueous secondary battery of the present disclosure will be described.
[0175] As an example of an embodiment of the positive electrode, a structure in which an active material layer comprising a positive electrode active material and a binder resin is formed on a current collector may be provided. The active material layer may further include a conductivity aid. As for the positive electrode active material, for example, a lithium-containing transition metal oxide may be provided, specifically LiCoO2, LiNiO2, and LiMn 1 / 2 Ni 1 / 2 O2, LiCo 1 / 3 Mn 1 / 3 Ni 1 / 3 O2, LiMn2O4, LiFePO4, LiCo 1 / 2 Ni 1 / 2 O2, LiAl 1 / 4 Ni 3 / 4 Examples include O2. Examples of binder resins include polyvinylidene fluoride resins and styrene-butadiene copolymers. Examples of conductive aids include carbon materials such as acetylene black, Ketjen black, and graphite powder. Examples of current collectors include aluminum foil, titanium foil, and stainless steel foil with a thickness of 5 μm to 20 μm.
[0176] In the non-aqueous secondary battery of the present disclosure, when a polyvinylidene fluoride-based resin is incorporated into the heat-resistant porous layer of the separator of the present disclosure, since the polyvinylidene fluoride-based resin has excellent oxidation resistance, by arranging the heat-resistant porous layer in contact with the positive electrode of the non-aqueous secondary battery, LiMn capable of operating at a high voltage of 4.2 V or higher is used as a positive electrode active material. 1 / 2 Ni 1 / 2 O2, LiCo 1 / 3 Mn 1 / 3 Ni1 / 3 It is easy to apply O2, etc.
[0177] As an example of an embodiment of the negative electrode, a structure in which an active material layer comprising a negative electrode active material and a binder resin is formed on a current collector may be provided. The active material layer may further include a conductive agent. As the negative electrode active material, a material capable of electrochemically absorbing lithium may be provided, specifically, examples include carbon materials; alloys of silicon, tin, aluminum, etc. with lithium; and wood alloys. As the binder resin, examples include polyvinylidene fluoride-based resins and styrene-butadiene copolymers. As the conductive agent, carbon materials such as acetylene black, ketjen black, and graphite powder may be provided. As the current collector, examples include copper foil, nickel foil, and stainless steel foil with a thickness of 5 μm to 20 μm. In addition, instead of the above-mentioned negative electrode, a metallic lithium foil may be used as the negative electrode.
[0178] The electrolyte is a solution in which a lithium salt is dissolved in a non-aqueous solvent. Examples of lithium salts include LiPF6, LiBF4, LiClO4, etc. Examples of non-aqueous solvents include cyclic carbonates such as ethylene carbonate, propylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, and vinylene carbonate; chain carbonates such as dimethyl carbonate, diethyl carbonate, ethylmethyl carbonate, and their fluorine substituents; and cyclic esters such as γ-butyrolactone and γ-valerolactone, etc., and these may be used alone or in combination. As an electrolyte, a solution in which a cyclic carbonate and a chain carbonate are mixed in a mass ratio (cyclic carbonate:chain carbonate) of 20:80 to 40:60 and a lithium salt is dissolved in a solution in the range of 0.5 mol / L to 1.5 mol / L is suitable.
[0179] Examples of exterior materials include metal cans and aluminum laminate film packs. The battery shape may be prismatic, cylindrical, coin-shaped, etc., but the separator of the present disclosure is suitable for any shape.
[0180] A method for manufacturing a non-aqueous secondary battery according to the present disclosure may include a manufacturing method comprising impregnating a separator with an electrolyte and performing a heat press treatment (referred to as "wet heat press" in the present disclosure) to bond it to an electrode; and a manufacturing method comprising not impregnating a separator with an electrolyte and performing a heat press treatment (referred to as "dry heat press" in the present disclosure) to bond it to an electrode.
[0181] The non-aqueous secondary battery of the present disclosure can be manufactured, for example, by manufacturing methods 1 to 3 below, by placing the separator of the present disclosure between the positive electrode and the negative electrode, winding it in the longitudinal direction to produce a wound body, and then using this wound body. The same applies when using a device manufactured by a method of stacking the positive electrode, separator, and negative electrode in this order (so-called stack method) instead of the wound body.
[0182] Manufacturing method 1: After dry heat pressing the electrode and separator onto the coil, the coil is placed in an outer material (e.g., a pack made of aluminum laminate film; hereinafter the same), an electrolyte is injected therein, and the coil is further wet heat pressed from above the outer material to bond the electrode and separator and seal the outer material.
[0183] Manufacturing method 2: A wound body is placed in an outer casing, an electrolyte is injected therein, and the wound body is wet-heat pressed from above the outer casing to bond the electrode and the separator and to seal the outer casing. Before placing the wound body in the outer casing, a room-temperature press (pressure at room temperature) may be performed to temporarily bond the wound body.
[0184] Manufacturing method 3: After attaching the electrode and separator by dry heat pressing on a wound body, the electrode is placed in an outer casing, an electrolyte is injected therein, and the outer casing is sealed.
[0185] As for the conditions for a wet heat press, the press temperature is preferably 70°C to 110°C, and the press pressure is preferably 0.5 MPa to 2 MPa. As for the conditions for a dry heat press, the press temperature is preferably 20°C to 100°C, and the press pressure is preferably 0.5 MPa to 5 MPa. The press time is preferably adjusted according to the press temperature and press pressure, for example, within a range of 0.5 minutes to 60 minutes.
[0186] (Example)
[0187] The separator and non-aqueous secondary battery of the present disclosure will be described in more detail below with reference to examples. The materials, usage amounts, ratios, processing procedures, etc., shown in the following examples may be appropriately modified as long as they do not deviate from the spirit of the present disclosure. Accordingly, the scope of the separator and non-aqueous secondary battery of the present disclosure should not be interpreted as being limited by the specific examples shown below.
[0188] Measurement Methods, Evaluation Methods
[0189] The measurement and evaluation methods applied in the examples and comparative examples are as follows.
[0190] [HFP Content of Polyvinylidene Fluoride Resin]
[0191] The ratio of hexafluoropropylene monomer units (HFP units) in the polyvinylidene fluoride-based resin was determined from the nuclear magnetic resonance (NMR) spectrum. Specifically, 20 mg of polyvinylidene fluoride-based resin was dissolved in 0.6 mL of dimethyl sulfoxide at 100°C, and at 100°C 19 The F-NMR spectrum was measured.
[0192] [Weight Average Molecular Weight of Polyvinylidene Fluoride Resin]
[0193] The weight-average molecular weight (Mw) of the polyvinylidene fluoride-based resin was measured by gel permeation chromatography (GPC). For the molecular weight measurement by GPC, a GPC device "GPC-900" manufactured by Nihon Bunkosha was used, two TSKgel SUPER AWM-H columns manufactured by Tososha were used, dimethylformamide was used as the solvent, and measurements were taken under conditions of a temperature of 40°C and a flow rate of 10 mL / min to obtain the molecular weight equivalent to polystyrene.
[0194] [Average primary particle size of inorganic particles]
[0195] The inorganic filler before being added to the coating solution to form a heat-resistant porous layer was used as a sample.
[0196] For barium sulfate particles with a small average primary diameter (average primary diameter less than 0.3 μm), measuring the major axis of the primary particles using a scanning electron microscope (SEM) was difficult. Therefore, the specific gravity (g / cm³) and BET specific surface area (m² / g) of the barium sulfate particles were measured, and assuming the barium sulfate particles were spherical, the average primary diameter of the barium sulfate particles was calculated according to the following formula. A Micromeritics ASAP2020 was used as the device for measuring the BET specific surface area. The BET specific surface area (m² / g) was determined by the BET multi-point method using a gas adsorption method with nitrogen gas. Nitrogen gas was adsorbed onto the particles at the boiling point temperature of liquid nitrogen (-196°C).
[0197] Average primary particle size (㎛) = 6 ÷ [Specific gravity (g / cm³) × BET specific surface area (m² / g)]
[0198] The average primary particle size of other inorganic particles was obtained by measuring the major axes of 100 randomly selected inorganic particles during observation by SEM and averaging the major axes of the 100.
[0199] [Volume ratio of barium sulfate particles in the heat-resistant porous layer]
[0200] The volume ratio Va(%) of barium sulfate particles in the heat-resistant porous layer was calculated by the following formula.
[0201] Va={(Xa / Da) / (Xa / Da+Xb / Db+Xc / Dc+…+Xn / Dn)}×100
[0202] Here, among the constituent materials of the heat-resistant porous layer, barium sulfate particles are a, and other constituent materials are b, c, … , n, and the mass of each constituent material is Xa, Xb, Xc, … , Xn(g), and the true density of each constituent material is Da, Db, Dc, … , Dn(g / cm³).
[0203] [Thickness of porous substrate and separator]
[0204] Twenty points each of the porous substrate and separator were measured using a contact-type thickness gauge (Mitutoyo Co., LITEMATIC VL-50), and the thickness (μm) of the porous substrate and separator was determined by averaging these measurements. A cylindrical terminal with a diameter of 5 mm was used as the measuring terminal, and the measurement was adjusted so that a load of 0.01 N was applied during the measurement.
[0205] [Thickness of heat-resistant porous layer]
[0206] The thickness of the heat-resistant porous layer (total of both sides, μm) was calculated by subtracting the thickness of the porous substrate (μm) from the thickness of the separator (μm).
[0207] [Mass of heat-resistant porous layer (coating amount)]
[0208] The separator was cut into a 10 cm × 10 cm section to measure its mass, and the mass per unit area (g / m²) of the separator was calculated by dividing the mass by the area. The porous substrate used to manufacture the separator was cut into a 10 cm × 10 cm section to measure its mass, and the mass per unit area (g / m²) of the porous substrate was calculated by dividing the mass by the area. The mass per unit area of the heat-resistant porous layer (total of both sides, g / m²) was calculated by subtracting the mass per unit area of the porous substrate from the mass per unit area of the separator.
[0209] [Porosity of porous substrates]
[0210] The porosity ε(%) of the porous substrate was calculated by the following formula.
[0211] ε={1-Ws / (ds·t)}×100
[0212] Ws: Mass per unit area of the porous substrate (g / m²), ds: True density of the porous substrate (g / cm³), t: Thickness of the porous substrate (cm).
[0213] [Porosity of heat-resistant porous layer]
[0214] The porosity ε(%) of the heat-resistant porous layer was calculated by the following formula.
[0215] ε={1-(Wa / da+Wb / db+Wc / dc+…+Wn / dn) / t}×100
[0216] Here, the constituent materials of the heat-resistant porous layer are a, b, c, … , n, the mass of each constituent material is Wa, Wb, Wc, … , Wn (g / cm²), the true density of each constituent material is da, db, dc, … , dn (g / cm³), and the thickness of the heat-resistant porous layer is t (cm).
[0217] [Gully Value]
[0218] Using a Gulliver-type Denso meter (Toyo Seikisha, G-B2C), the Gulliver values (seconds / 100 mL) of the porous substrate and separator were measured in accordance with JIS P8117:2009.
[0219] [Membrane Resistance]
[0220] A test cell was fabricated by impregnating a separator with 1 mol / L LiBF4-propylene carbonate:ethylene carbonate (mass ratio 1:1) as the electrolyte, placing it between aluminum foil electrodes with lead tabs attached, and sealing it in an aluminum pack. The resistance (Ω·cm²) of this test cell was measured by the AC impedance method (measurement frequency 100 kHz) at a temperature of 20°C.
[0221] [Peel strength between porous substrate and heat-resistant porous layer]
[0222] A T-shaped peel test was performed on the separator. Specifically, an adhesive tape (3M, 12 mm wide) was attached to one surface of the separator (when attaching, the longitudinal direction of the adhesive tape was aligned with the MD of the separator), and the separator, along with the adhesive tape, was cut to a size of 12 mm in length in TD and 70 mm in length in MD. The adhesive tape was peeled off slightly along with the heat-resistant porous layer immediately underneath, and the two separated ends were held in a Tensilon (Orientec, RTC-1210A) to perform a T-shaped peel test. In addition, the adhesive tape was used as a support to peel the heat-resistant porous layer from the porous substrate. The tensile speed of the T-shaped peel test was set to 20 mm / min, and loads (N) were collected at 0.4 mm intervals from 10 mm to 40 mm after the start of measurement, the average was calculated, and converted into a load per 10 mm width (N / 10 mm). In addition, the loads (N / 10 mm) of 10 test specimens were averaged.
[0223] [Area shrinkage rate due to heat treatment]
[0224] A separator was cut to a size of 180 mm in length in MD × 60 mm in length in TD and prepared as a test specimen. On this test specimen, marks were made at locations 20 mm and 170 mm from one end along the line bisecting the length in TD (referred to as Point A and Point B, respectively). Additionally, marks were made at locations 10 mm and 50 mm from one end along the line bisecting the length in MD (referred to as Point C and Point D, respectively). A clip was attached to this (the clip was attached between the end closest to Point A and Point A), and the specimen was suspended in an oven with the internal temperature adjusted to 120°C, 135°C, or 150°C, and heat treatment was performed for 1 hour without tension. The lengths between AB and CD were measured before and after the heat treatment, the area shrinkage rate was calculated using the following formula, and the area shrinkage rates of 10 test specimens were averaged.
[0225] Area shrinkage rate (%) = {1 - (Length of AB after heat treatment ÷ Length of AB before heat treatment) × (Length of CD after heat treatment ÷ Length of CD before heat treatment)} × 100
[0226] [Spot Heating]
[0227] A separator was cut to a size of MD 50 mm × TD 50 mm to serve as a test specimen. The test specimen was placed on a horizontal stand, and a soldering iron with a tip diameter of 2 mm was heated to a tip temperature of 260°C. The tip of the soldering iron was then made point contact with the surface of the separator for 60 seconds. The area (mm²) of the hole formed in the separator due to the point contact was measured, and the hole areas of 10 test specimens were averaged. The higher the heat resistance of the separator, the smaller the area of the hole formed in the separator.
[0228] [Gas Generation Amount]
[0229] A separator was cut to a size of 600 cm² and placed inside an aluminum laminate film pack. Electrolyte was injected into the pack to impregnate the separator, and the pack was sealed to obtain a test cell. As the electrolyte, a 1 mol / L mixed solution of LiPF6-ethylene carbonate and ethyl methyl carbonate (LiPF6-ethylene carbonate:ethyl methyl carbonate = 3:7 [mass ratio]) was used. The test cell was placed under an environment of 85°C for 20 days, and the volume of the test cell before and after heat treatment was measured. The amount of gas generated V (=V2-V1, unit: mL) was calculated by subtracting the volume of the test cell before heat treatment V1 from the volume of the test cell after heat treatment V2. In addition, the amount of gas generated V of 10 test cells was averaged.
[0230] [Evaluation Test of Pottery Appearance]
[0231] The separator was cut to a predetermined size (10 cm × 30 cm) and observed using an optical microscope via transmitted and reflected light to check for the presence of defects or foreign substances in the coating layer. Specifically, defects or foreign substances include defects caused by the peeling of aggregates, pinholes, filler aggregates, coating lines, and wrinkles.
[0232] Evaluation was conducted based on observation, where separators were deemed acceptable if no defects or foreign substances were found, and unacceptable if they were found. Specifically, for each separator, 60 randomly selected sections of a predetermined size were cut and evaluated, and the percentage of accepted separators was calculated. Based on the acceptance rate, they were classified according to the following criteria.
[0233] <Criteria>
[0234] A : The pass rate is 100%.
[0235] B: Pass rate of 95% or higher but less than 100%.
[0236] C: Pass rate of 90% or more but less than 95%.
[0237] D: Pass rate less than 90%.
[0238] Production of Separators
[0239] (Example 1)
[0240] A polyvinylidene fluoride-based resin (VDF-HFP copolymer, VDF:HFP (molar ratio) = 97.6:2.4, weight average molecular weight 1.13 million) was dissolved in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG = 80:20 [mass ratio]) so that the resin concentration was 4 mass%, and additionally, barium sulfate particles (BaSO4; average primary particle size 0.05 μm) were stirred and mixed to obtain a coating solution (P). Also, the ratio of barium sulfate particles to binder resin was set to 48 / 52 (volume ratio).
[0241] An appropriate amount of coating solution (P) was placed in a pair of Meyer bars, and a polyethylene microporous membrane (thickness 9 μm, porosity 36%, Gurley value 168 sec / 100 mL) was passed between the Meyer bars to coat both sides with an equal amount of coating solution (P). This was immersed in a coagulation solution (DMAc:TPG:water = 30:8:62 [mass ratio], liquid temperature 40°C) to solidify the coating layer, and then washed in a water bath at a water temperature of 40°C and dried. In this way, a separator with heat-resistant porous layers formed on both sides of a polyethylene microporous membrane was obtained.
[0242] (Examples 2-3)
[0243] A separator was prepared in the same manner as in Example 1, except that the volume ratio of barium sulfate particles was changed as described in Table 1.
[0244] (Example 4)
[0245] A separator was prepared in the same manner as in Example 1, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.10 μm).
[0246] (Example 5)
[0247] A separator was prepared in the same manner as in Example 1, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.25 μm).
[0248] (Comparative Examples 1, 4)
[0249] A separator was prepared in the same manner as in Example 1, except that the volume ratio of barium sulfate particles was changed as described in Table 1.
[0250] (Comparative Example 2)
[0251] A separator was prepared in the same manner as in Example 1, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.30 μm).
[0252] (Comparative Example 3)
[0253] A separator was prepared in the same manner as in Example 1, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.70 μm).
[0254] (Comparative Example 5)
[0255] A separator was prepared in the same manner as in Example 1, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.30 μm) and the volume ratio was changed as described in Table 1.
[0256] (Comparative Example 6)
[0257] A separator was prepared in the same manner as in Example 1, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.70 μm) and the volume ratio was changed as described in Table 1.
[0258] (Comparative Example 7)
[0259] A separator was prepared in the same manner as in Example 1, except that the barium sulfate particles were changed to magnesium hydroxide (average primary particle size 0.50 μm).
[0260] (Comparative Example 8)
[0261] A separator was prepared in the same manner as in Example 1, except that the barium sulfate particles were changed to magnesium hydroxide (average primary particle size 0.90 μm).
[0262] (Comparative Example 9)
[0263] A separator was prepared in the same manner as in Example 1, except that the barium sulfate particles were changed to alumina (average primary particle size 0.60 μm).
[0264] (Example 6)
[0265] Meta-type fully aromatic polyamide (represented as aramid in Table 2) was dissolved in a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG = 80:20 [mass ratio]) so that the resin concentration was 5 mass%, and additionally barium sulfate particles (average primary particle size 0.05 μm) were stirred and mixed to obtain a coating solution (A). In addition, the ratio of barium sulfate particles to binder resin was set to 42 / 58 (volume ratio).
[0266] An appropriate amount of coating solution (A) was placed in a Meyer bar, and the coating solution (A) was applied to one side of a polyethylene microporous membrane (thickness 9 μm, porosity 36%, Gurley value 168 s / 100 mL). This was immersed in a coagulation solution (DMAc:TPG:water = 30:8:62 [mass ratio], liquid temperature 40°C) to solidify the coating layer, and then washed in a water bath at a water temperature of 40°C and dried. In this way, a separator with a heat-resistant porous layer formed on one side of a polyethylene microporous membrane was obtained.
[0267] (Example 7)
[0268] A separator was manufactured in the same manner as in Example 6, except that the thickness of the heat-resistant porous layer, the mass per unit area, and the porosity were changed as described in Table 2.
[0269] (Example 8)
[0270] A separator was manufactured in the same manner as in Example 6, except that the coating solution was applied to both sides of the porous substrate.
[0271] (Examples 9–10)
[0272] A separator was manufactured in the same manner as in Example 6, except that the volume ratio of barium sulfate particles, the thickness of the heat-resistant porous layer, the mass per unit area, and the porosity were changed as described in Table 2.
[0273] (Example 11)
[0274] A separator was prepared in the same manner as in Example 6, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.10 μm).
[0275] (Example 12)
[0276] A separator was prepared in the same manner as in Example 6, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.25 μm).
[0277] (Comparative Examples 10, 13)
[0278] A separator was prepared in the same manner as in Example 6, except that the volume ratio of barium sulfate particles was changed as described in Table 2.
[0279] (Comparative Example 11)
[0280] A separator was prepared in the same manner as in Example 6, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.30 μm).
[0281] (Comparative Example 12)
[0282] A separator was prepared in the same manner as in Example 6, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.70 μm).
[0283] (Comparative Example 14)
[0284] A separator was prepared in the same manner as in Example 6, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.30 μm) and the volume ratio was changed as described in Table 2.
[0285] (Comparative Example 15)
[0286] A separator was prepared in the same manner as in Example 6, except that the barium sulfate particles were changed to other barium sulfate particles (average primary particle size 0.70 μm) and the volume ratio was changed as described in Table 2.
[0287] (Comparative Example 16)
[0288] A separator was prepared in the same manner as in Example 6, except that the barium sulfate particles were changed to magnesium hydroxide (average primary particle size 0.50 μm).
[0289] (Comparative Example 17)
[0290] A separator was prepared in the same manner as in Example 6, except that the barium sulfate particles were changed to magnesium hydroxide (average primary particle size 0.90 μm).
[0291] (Comparative Example 18)
[0292] A separator was prepared in the same manner as in Example 6, except that the barium sulfate particles were changed to alumina (average primary particle size 0.60 μm).
[0293] The composition, physical properties, and evaluation results of each separator in Examples 1 to 12 and Comparative Examples 1 to 18 are shown in Tables 1 and 2.
[0294] [Table 1]
[0295]
[0296] [Table 2]
[0297]
[0298] In an example comprising a binder resin and barium sulfate particles of a predetermined size and volume ratio, gas generation was suppressed, and the area shrinkage rate was low and heat resistance was excellent, resulting in good productivity.
[0299] In addition, in the above-described examples, the explanation focused on the case where a VDF-HFP copolymer (VDF:HFP (molar ratio) = 97.6:2.4, weight average molecular weight 1.13 million) was used as a polyvinylidene fluoride-based resin (PVDF-based resin) which is an example of a binder; however, the PVDF-based resin is not limited to the above-described VDF-HFP copolymer, and the same effect is produced when the PVDF-based resin is combined with specific barium sulfate particles. Furthermore, the explanation focused on the case where aramid was used as a heat-resistant resin which is an example of a binder; however, other heat-resistant resins other than aramid, such as amide-based resins or imide-based resins (polyamideimide, poly-N-vinylacetamide, polyacrylamide, copolymerized polyetherpolyamide, polyimide, polyetherimide, etc.), are also produced by combining with specific barium sulfate particles.
[0300] In addition, when comparing Comparative Examples 1 to 9 using polyvinylidene fluoride resin (PVDF resin) with Comparative Examples 10 to 18 using all-aromatic polyamide (aramid), the area shrinkage rate of Comparative Examples 10 to 18 is smaller at 135°C and 150°C. This is because the aramid has higher heat resistance than the PVDF resin.
[0301] When comparing Comparative Examples 1 to 6, which used barium sulfate particles, with Comparative Examples 7 to 9, which used magnesium hydroxide or alumina, the amount of shifted gas generated in Comparative Examples 1 to 6 is lower. Additionally, when comparing Comparative Examples 10 to 15, which used barium sulfate particles, with Comparative Examples 16 to 18, which used magnesium hydroxide or alumina, the amount of shifted gas generated in Comparative Examples 10 to 15 is lower. As such, the gas reduction effect caused by the use of barium sulfate particles was significantly demonstrated.
[0302] The disclosure of Japanese Patent Application No. 2019-052384, filed on March 20, 2019, is incorporated herein by reference in its entirety.
[0303] All documents, patent applications, and technical specifications described in this specification are introduced by reference within this specification to the same extent as where individual documents, patent applications, and technical specifications are specifically and individually described.
Claims
Claim 1 A separator for a non-aqueous secondary battery, comprising a porous substrate and a heat-resistant porous layer provided on one or both sides of the porous substrate, the heat-resistant porous layer comprising all-aromatic polyamide and barium sulfate particles, wherein the average primary particle size of the barium sulfate particles included in the heat-resistant porous layer is 0.05 μm or more and less than 0.30 μm, the volume ratio of the barium sulfate particles in the heat-resistant porous layer is 30 volume% or more and less than 50 volume%, and the content ratio of the barium sulfate particles and the all-aromatic polyamide included in the heat-resistant porous layer (barium sulfate particles / all-aromatic polyamide) is 32 / 68 to 49 / 51 in volume ratio. Claim 2 A separator for a non-aqueous secondary battery according to claim 1, wherein the area shrinkage rate when the separator for a non-aqueous secondary battery is heat-treated at 135°C for 1 hour is 30% or less. Claim 3 A separator for a non-aqueous secondary battery according to claim 1 or 2, wherein the area shrinkage rate when the separator for a non-aqueous secondary battery is heat-treated at 150°C for 1 hour is 45% or less. Claim 4 A separator for a non-aqueous secondary battery according to claim 1 or 2, wherein the porosity of the heat-resistant porous layer is 30% to 70%. Claim 5 A separator for a non-aqueous secondary battery according to claim 1 or 2, wherein the heat-resistant porous layer has a mass per unit area of 1.0 g / m² to 30.0 g / m² total for both sides. Claim 6 A separator for a non-aqueous secondary battery according to claim 1 or 2, wherein the heat-resistant porous layer is provided on one side of the porous substrate. Claim 7 A non-aqueous secondary battery comprising a positive electrode, a negative electrode, and a separator for a non-aqueous secondary battery described in claim 1 or 2 disposed between the positive electrode and the negative electrode, and obtaining an electromotive force by doping and taldoping of lithium.