Non-combustible Insulating Composite Panel and Sandwich Panel

The integration of steel plates, glass fibers, and CO₂ gas insulation in a multi-layer sandwich structure addresses the challenge of achieving high thermal insulation and non-combustibility, meeting building regulations and enhancing fire safety and constructability.

KR1020260161684APending Publication Date: 2026-11-10디앤아이이엔지주식회사
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020250057870
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-01
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Conventional insulation panels face challenges in achieving both high thermal insulation and non-combustibility, particularly in meeting building insulation regulations for roofing and walls, while also ensuring structural stability and fire safety, due to limitations in intermediate layer thickness and material adhesion.

Method used

A non-combustible insulation panel is developed by integrating steel plates and glass fibers with a non-combustible resin, incorporating a CO₂ gas insulation layer or board, and using a multi-layer sandwich structure with adjustable intermediate layer thickness to enhance thermal insulation and fire resistance, while ensuring structural integrity and constructability.

Benefits of technology

The panel achieves thermal resistance of 5.8 m²·K/W for roofing and 4.8 m²·K/W for walls, meets fire safety standards, prevents condensation, and reduces carbon emissions, while providing lightweight and cost-effective construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PAT00002_ABST
    Figure PAT00002_ABST
Patent Text Reader

Abstract

The present invention relates to a composite plate in which a steel plate (0.1–1.5 mm) and glass fiber are combined with a non-combustible resin, and to a non-combustible insulation panel having a multi-stage sandwich structure (air layer 10–80 mm). Insulation performance is maximized by including a CO₂ gas (thermal conductivity 0.016 W / m·K) pouch, a fill board, or a honeycomb material in the air layer. Heat transfer is minimized by applying a radiant heat reduction coating, achieving a thermal resistance of 5.8 m²·K / W (roofing material) and 4.8 m²·K / W (wall), thereby satisfying the NFPC 501 non-combustible standards. It provides the effects of preventing condensation and reducing carbon emissions.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to building materials and duct materials, and more specifically to a non-combustible insulation panel and a method for manufacturing the same, which provides excellent thermal insulation and non-combustible performance by forming a multi-stage sandwich structure using a composite plate in which steel plates and glass fibers are combined with a non-combustible resin. Additionally, by incorporating an inflatable insulation material using CO₂ gas (Application No. 10-2025-0055010), the thermal conductivity of the intermediate layer is lowered and thermal insulation performance is maximized. Background Technology

[0002] Building materials and duct insulation play a crucial role in increasing energy efficiency, maintaining indoor environmental quality, and ensuring fire safety. According to Korea’s Building Energy Conservation Design Standards, roofing materials must meet a thermal transmittance of 0.15–0.2 W / m²·K or less (thermal resistance 5.0–6.67 m²·K / W), and walls must meet a thermal transmittance of 0.25–0.3 W / m²·K or less (thermal resistance 3.33–4.0 m²·K / W), while indoor ducts require a minimum thermal resistance of 0.8 m²·K / W. To achieve this, an insulation thickness of 200–250 mm is recommended for roofing materials and at least 150 mm for walls.

[0003] Conventional insulation panel technologies have utilized fiberglass, polyurethane foam, and polyethylene foam; however, while they offer excellent thermal insulation performance, they suffer from insufficient fire resistance or poor constructability due to their thick thickness, and they cannot be used as interior or exterior materials. Polyurethane foam (thermal conductivity 0.020–0.030 W / m·K) poses a high fire risk due to the presence of flammable blowing agents (HFCs, coal), and the use of HFCs is restricted starting in 2024 in accordance with the Kigali Amendment (2016). A sandwich structure combining steel plates and an air layer provides thermal insulation performance and structural stability, but it has limitations in reducing radiant heat from air (thermal conductivity 0.026 W / m·K) and maximizing thermal resistance.

[0004] The potential of composite materials combining steel plates and fiberglass with non-combustible resins to provide both fire resistance and thermal insulation has been raised, but information on this is limited. In the case of ceramic-based non-combustible resins, it is difficult to stably bond steel plates and fiberglass due to insufficient adhesion, while organic non-combustible resins often exhibit inadequate fire resistance. Although low-emissivity coated fiberglass is commercially available as an insulating material that reduces radiant heat, it is rare to see it manufactured into composite panels by combining it with steel plates.

[0005] The thickness of the intermediate layer in insulation panels significantly impacts thermal insulation performance. Conventional sandwich structures limit the intermediate layer thickness to 5–20 mm, making them suitable for duct insulation; however, meeting building insulation regulations (200–250 mm for roofing and 150 mm for walls) requires an unrealistically large number of layers. Honeycomb structures maintain the intermediate layer stably due to their distinct diaphragms and can enhance structural strength and thermal insulation compared to corrugated structures (including egg carton shapes). However, even after fire-resistant treatment, paper honeycomb exhibits a weight loss of over 30% due to carbonization at high temperatures, making it difficult to meet Korean fire resistance test standards (KS F ISO 1182); conversely, using it in combination with steel plates for the insulation casing eliminates concerns regarding weight loss. Semi-fire-resistant paper honeycomb exhibits limited combustion and emits minimal smoke and toxic gases, making it highly promising for use as a building insulation material.

[0006] An inflatable insulation material using CO₂ gas (Application No. 10-2025-0055010) has a thermal conductivity of 0.016 W / m·K, which is superior to that of air (0.026 W / m·K), and provides fire safety by using non-combustible materials (aluminum, non-combustible resin) and CO₂ generating agents (sodium bicarbonate, NaHCO₃). The insulation board filled with CO₂ gas provides low thermal conductivity and structural rigidity, and can maximize insulation performance by replacing or reinforcing the intermediate layer of a multi-layer sandwich structure.

[0007] The present invention proposes a non-combustible insulation panel that integrates thermal insulation performance, non-combustibility, and interior / exterior material functions by integrating CO₂ insulation material into a steel plate and a glass fiber composite plate, and replacing the intermediate layer with a CO₂ gas insulation layer or a board filled with CO₂ gas. The problem to be solved

[0008] The present invention aims to provide thermal insulation and non-combustibility through a composite plate combining steel plates and glass fibers with a non-combustible resin, and to reduce the thermal conductivity of the intermediate layer and maximize thermal insulation performance by integrating an inflatable insulation material using CO₂ gas. In addition, by adjusting the thickness of the intermediate layer to 10 to 80 mm and introducing a non-combustible / semi-non-combustible treated honeycomb or insulation board filled with CO₂ gas, the invention aims to develop a non-combustible insulation panel that can be used as a building material and duct insulation material by meeting insulation regulations for roofing materials (thermal resistance 5.8 m²·K / W or more) and walls (4.8 m²·K / W or more) and enhancing condensation prevention performance. means of solving the problem

[0009] The non-combustible thermal insulation composite plate and panel according to the present invention have the following characteristics:

[0010] - Steel plate and fiberglass composite:

[0011] - Combines steel plates and glass fibers with non-combustible resin to provide thermal insulation and non-combustibility.

[0012] - The steel plate is a cold-rolled steel plate or galvanized steel plate with a thickness of 0.1 to 1.5 mm.

[0013] - The glass fiber is formed into a non-flammable resin-impregnated glass fiber mat or an uneven structure, and a low-emissivity coating (emissivity 0.05 or less) can be optionally applied.

[0014] - Multi-layer sandwich structure:

[0015] - Multiple steel plates and intermediate layers (including corrugated structure, honeycomb structure, CO₂ gas insulation layer, or insulation board filled with CO₂ gas) are arranged alternately.

[0016] - The thickness of the intermediate layer can be adjusted from 10 to 80 mm, and some intermediate layers include aluminum, glass fiber, non-combustible / semi-combustible treated paper honeycomb, or CO₂ insulation (Application No. 10-2025-0055010).

[0017] - Radiant heat reduction:

[0018] - Application of a low-emissivity coating to at least one surface in contact with the intermediate layer of the steel plate, or use of low-emissivity coated glass fibers.

[0019] - Low-emissivity coating is produced by plating, vaporizing, or laminating (e.g., combining 5–20 µm of aluminum foil with glass fiber) with materials having high reflectivity, such as silver, aluminum, or chrome.

[0020] - Thermal insulation performance:

[0021] - Roof material thermal resistance of 5.8 m²·K / W or higher, wall resistance of 4.8 m²·K / W or higher.

[0022] - Replace the intermediate layer with CO₂ gas (thermal conductivity 0.016 W / m·K), maximizing insulation performance.

[0023] - Prevents condensation in the temperature range of -15°C to +40°C.

[0024] - Non-combustible performance:

[0025] - Non-combustible resin-impregnated fiberglass, fiberglass honeycomb, and CO₂ insulation comply with NFPC 501 non-combustible material standards; paper honeycomb is treated as non-combustible or semi-non-combustible.

[0026] - Constructability:

[0027] - Designed with panel thicknesses of 20 to 250 mm, resulting in lightweight design and simplified construction. Effects of the invention

[0028] The present invention provides the following effects:

[0029] - Improved thermal insulation performance: Achieved thermal resistance of 5.8 m²·K / W (roofing) and 4.8 m²·K / W (walls) by adjusting the intermediate layer thickness to 10–80 mm and introducing a CO₂ gas insulation layer or insulation boards filled with CO₂ gas (thermal conductivity 0.016 W / m·K), meeting Korean building insulation regulations.

[0030] - Non-combustible and semi-non-combustible performance: Meets NFPC 501 non-combustible standards with non-combustible resin-impregnated glass fiber, glass fiber honeycomb, and CO₂ insulation; provides cost-effectiveness and semi-non-combustible performance with non-combustible / semi-non-combustible treated paper honeycomb.

[0031] - Condensation prevention: Maintains a surface temperature of 24.24°C at an internal duct temperature of 10°C under indoor conditions (25°C, relative humidity 60%, dew point 16.7°C), preventing condensation.

[0032] - Structural Stability: Improved stability and strength of the intermediate layer with honeycomb or CO₂ insulation boards, and simplified construction due to the clarity of the diaphragm compared to an uneven structure.

[0033] - Environmental Benefits: Annual reduction of approximately 10 tons of carbon emissions due to improved insulation performance, replacement of HFCs with CO₂ gas utilization, contribution to sustainability. Brief explanation of the drawing

[0035] Drawing 1: Cross-sectional view of a multi-layer sandwich structure non-combustible insulation panel. - A multi-stage structure composed of a steel plate (10) + an intermediate layer (20, including an uneven structure or honeycomb structure) + a steel plate (30) + an intermediate layer (40, including an uneven structure or honeycomb structure) + a steel plate (50). Drawing 2: 3D cross-sectional view of a multi-layer sandwich structure non-combustible insulation panel. - A structure with alternating steel plates and intermediate layers; honeycomb materials reinforce insulation and strength within the intermediate layers. Drawing 3: Cross-section of insulation board filled with CO₂ gas. - Pouch, including CO₂ gas filling space. Specific details for implementing the invention

[0036] 1. Prepare the steel plate

[0037] The steel plate is a cold-rolled steel plate or a galvanized steel plate with a thickness ranging from 0.1 to 1.5 mm, and in this embodiment, a steel plate with a thickness of 0.3 mm is used. The steel plate is cut and formed to fit the outer shape of the panel, and galvanizing or anti-corrosion coating may be applied to the surface to prevent corrosion. The size of the steel plate is adjusted according to the length and width of the panel, and is generally manufactured to a size of 1 m x 1 m.

[0038] 2. Fabrication of Non-Retardant Resin Impregnation Structure and Honeycomb

[0039] 2.1. Manufacture of Non-Retardant Resin

[0040] Non-combustible resin is composed of the following components to ensure heat resistance and non-flammability:

[0041] - Silicone resin: 50~70wt%, provides heat resistance and flexibility.

[0042] (Silicone resin can be replaced with acrylate)

[0043] - Expanded graphite (mesh 200, expansion ratio 100x): 15~25wt%, expands at high temperatures to form a thermal barrier layer.

[0044] - Alumina (Al₂O₃): 5~15wt%, enhanced heat resistance.

[0045] - Silica (SiO₂): 3~10wt%, enhanced heat resistance.

[0046] - Peroxide curing agent: 1~3 wt%, accelerates resin curing.

[0047] - Antioxidant (TiO₂): 0.5~2 wt%, thermal stability and oxidation prevention.

[0048] - Phosphorus-based flame retardant (TPP): 1~5 wt%, enhanced non-flammability.

[0049] - Aluminum hydroxide (Al(OH)₂): 5~10wt%, enhanced heat resistance, reduced smoke

[0050] Manufacturing process:

[0051] 1. 60 wt% silicone resin, 20 wt% expanded graphite, 10 wt% alumina, 5 wt% silica, 2 wt% peroxide curing agent, 1 wt% antioxidant, and 2 wt% phosphorus-based flame retardant are placed in a mixer and stirred at 80°C for 30 minutes to prepare a homogeneous mixture.

[0052] 2. Cool the mixture to 60°C to adjust the viscosity.

[0054] The non-combustible resin components, mixing ratios, and manufacturing methods presented above are examples and can be produced through various combinations.

[0055] 2.2. Preparation of Glass Fiber

[0056] Glass fiber is used in the form of a glass fiber mat with a thickness of 1 mm and a density of 450 g / m². S-GLASS glass fiber is used, providing excellent heat resistance and maintaining stable performance even at a heat resistance temperature of 1050°C. E-GLASS can be used instead of S-GLASS to reduce costs, and the lower heat resistance temperature of E-GLASS can be overcome through carbonization of the non-combustible resin. Optionally, a low-emissivity coating (emissivity of 0.05 or less) can be applied to one side of the glass fiber to enhance the radiant heat reduction effect.

[0057] 2.3. Non-retardant resin impregnation

[0058] The fiberglass mat is impregnated with a non-combustible resin. The impregnation process is as follows:

[0059] 1. Prepare the non-flammable resin in a roller coating machine, spray, or immersion tank.

[0060] 2. Immerse the fiberglass mat in a non-flammable resin, or coat it with a roller or spray it so that the non-flammable resin completely permeates into the fiber structure.

[0061] 3. The impregnated glass fibers are dried at 80°C for 30 minutes to cure the non-flammable resin, or loaded at room temperature for 12 hours to cure.

[0062] 4. S-GLASS glass fibers are impregnated with a non-combustible resin and combined with a steel plate, allowing them to be used while maintaining structural stability even at temperatures above 1050°C.

[0063] 2.4. Uneven Structure and Honeycomb Shape Forming

[0064] - Molding of uneven surface structure:

[0065] 1. Place the impregnated glass fiber mat in a molding mold (irregular structure mold, height 10~30mm, spacing 10mm).

[0066] 2. Place the mold into a press machine preheated to 120°C and pressurize it at a pressure of 50kPa for 5 minutes to form an uneven structure.

[0067] 3. Remove the molded glass fiber from the mold and cool it at room temperature for 1 hour to fix its shape.

[0068] 4. The uneven structure also includes an egg carton shape.

[0069] - Honeycomb molding:

[0070] 1. Prepare fiberglass or non-combustible / semi-combustible treated paper honeycomb material (cell size 5~10mm, thickness 10~30mm).

[0071] 2. Aluminum honeycomb is manufactured as a standard module, bonded with non-flammable resin, and inserted into the middle layer.

[0072] 3. The paper honeycomb is treated with a flame retardant (phosphorus-based or boron-based) to be non-combustible or semi-non-combustible, satisfying the KS F 2271 semi-non-combustible standard.

[0073] 4. The honeycomb material is cut and assembled to match the thickness of the middle layer.

[0074] 3. Fabrication of CO₂ insulation pouches and boards

[0075] CO₂ insulation is manufactured based on the expandable insulation technology disclosed in application number 10-2025-0055010.

[0076] 3.1. Fabrication of CO₂ Gas Insulation Layer Pouch

[0077] 1. A lid-type pouch structure is made of aluminum foil or a non-flammable resin-coated fiberglass mat, and the top is sealed with a pouch top seal (No. 70) or an aluminum-coated pouch bag is used as is.

[0078] 2. Insert a CO₂ generating agent (sodium bicarbonate, 10~20 wt%) and a water vapor absorbent into the pouch.

[0079] 3. Inhale air under low vacuum conditions (0.1~0.5 mbar) and seal with a self-healing material.

[0080] 4. Heat the pouch to 150°C for 10 minutes to generate CO₂ gas and steam.

[0081] 5. Cool to room temperature and absorb water vapor into the absorbent to form a CO₂ gas insulation layer.

[0082] 6. The finished pouch is inserted into the middle layer with a thickness of 10 to 30 mm.

[0083] 3.2. Fabrication of CO₂ Gas-Filled Insulation Boards

[0084] 1. A single layer or multiple layers (2 to 3 layers) of CO₂ gas insulation pouches are laminated, and the exterior is finished with a composite material of aluminum, glass fiber, and non-combustible resin.

[0085] 2. It is hardened into a board filled with CO₂ gas by compressing it with a press machine at 50 kPa pressure and 100°C for 5 minutes.

[0086] 3. Adjust the board thickness to 10~30mm and cut it for inserting an intermediate layer.

[0087] 4. Fabrication of steel plate and fiberglass composite panels

[0088] A composite panel is manufactured by combining steel plates and fiberglass with a non-combustible resin. The manufacturing process is as follows:

[0089] 1. Prepare a steel plate (thickness 0.3mm) and clean the surface to remove impurities.

[0090] 2. Apply a thin layer of non-flammable resin (thickness about 0.1 mm) to the steel plate to strengthen adhesion.

[0091] 3. Place a non-flammable resin-impregnated glass fiber corrugated structure (height 10~30mm) on a steel plate.

[0092] 4. Another steel plate is placed over the uneven structure, and a sandwich structure composite plate is formed by pressing with a press machine at 100°C for 3 minutes at a pressure of 30kPa.

[0093] 5. Cool the completed composite plate at room temperature for 2 hours to stabilize the structure.

[0094] 5. Fabrication of composite panels using low-emissivity coated glass fibers

[0095] An alternative process for manufacturing composite panels using low-emissivity coated glass fibers is as follows:

[0096] 1. Prepare a fiberglass mat with a low-emissivity coating (emissivity 0.05 or less) applied to one side.

[0097] 2. Apply a non-flammable resin to the fiberglass to enhance adhesion. When the fiberglass is exposed to the outside, the surface is provided with a surface suitable for color painting (excellent adhesion and durability).

[0098] 3. Prepare a steel plate (thickness 0.3mm) and clean the surface to remove impurities.

[0099] 4. Glass fiber coated with non-flammable resin is placed on a steel plate, and a composite plate is formed by applying pressure of 30 kPa at 100°C for 3 minutes using a press machine.

[0100] 5. Cool the completed composite plate at room temperature for 2 hours to stabilize the structure.

[0101] 6. Steel Plate Surface Treatment

[0102] 6.1. Low-emissivity coating

[0103] Radiant heat transfer is reduced by applying a low-emissivity coating to at least one surface in contact with the intermediate layer of the steel plate. The coating process is as follows:

[0104] 1. Clean the surface of the steel plate and prepare a low-emissivity coating solution (e.g., 30 wt% aluminum powder, 70 wt% binder).

[0105] 2. Apply the coating solution to the surface of the steel plate to a thickness of 0.1 mm using a spray coater.

[0106] 3. Dry the coated steel plate at 100°C for 30 minutes to form a coating layer.

[0107] In this embodiment, a low-emissivity coating is applied to the surfaces in contact with the intermediate layer among the three steel plates (e.g., the inner side of the first steel plate, one side of the second steel plate, and the outer side of the third steel plate). If low-emissivity coated glass fibers are used, the steel plate coating process can be omitted.

[0108] 7. Multi-layer sandwich structure assembly

[0109] The multi-layer sandwich structure is manufactured with alternating steel plates, fiberglass composite plates, and intermediate layers. The assembly process is as follows:

[0110] 1. Prepare a first steel plate (thickness 0.3 mm), and place an uneven structure (height 10~30 mm), a glass fiber honeycomb (thickness 10~30 mm), a CO₂ gas insulation layer pouch (thickness 10~30 mm), or an insulation board filled with CO₂ gas (thickness 10~30 mm) on it to form a first intermediate layer (thickness 10~80 mm).

[0111] 2. Apply a thin layer of non-combustible resin (thickness about 0.1 mm) over an uneven structure, honeycomb, or CO₂ insulation to enhance adhesion.

[0112] 3. A second steel plate (thickness 0.3 mm) is placed over the first intermediate layer, and a sandwich structure is formed by pressing with a press machine at 100°C for 3 minutes at a pressure of 30 kPa.

[0113] 4. To form a second intermediate layer (thickness 10~80mm) on the second steel plate, place an uneven structure (height 10~30mm), a honeycomb (thickness 10~30mm), a CO₂ gas insulation layer pouch (thickness 10~30mm), or a CO₂ insulation board (thickness 10~30mm) and bond them in the same way.

[0114] 5. Place a third steel plate (thickness 0.3 mm) over the second intermediate layer and press in the same way to complete the multi-layer sandwich structure.

[0115] 6. Cool the finished panel at room temperature for 2 hours to stabilize the structure.

[0116] 8. Panel finish

[0117] Condensation prevention performance is enhanced by additionally applying a vapor barrier (e.g., aluminum foil or a moisture-proof coating) to the surface of the finished panel. The vapor barrier is applied to a thickness of 0.1 mm to the outer steel plate or exposed fiberglass surface of the panel and completed by drying at 80°C for 1 hour. The exposed fiberglass surface provides excellent adhesion and durability during color painting.

[0118] Examples of the invention

[0119] Example 1: Fabrication of steel plate and glass fiber composite plate

[0120] 1. Prepare a steel plate (thickness 0.3 mm) and impregnate a glass fiber mat with a non-combustible resin (heat resistance 1050°C or higher) to form an uneven structure (height 20 mm).

[0121] 2. A non-combustible resin is applied to a steel plate, and a sandwich-type composite plate is produced by arranging an impregnated glass fiber corrugated structure.

[0122] 3. The composite plates are joined by applying pressure with a press machine, and the structure is stabilized by cooling at room temperature.

[0123] Example 2: Fabrication of a composite panel using low-emissivity coated glass fibers

[0124] 1. Prepare a fiberglass mat with a low-emissivity coating applied to one side.

[0125] 2. A composite plate is produced by applying a non-combustible resin to the fiberglass and bonding it to a steel plate. If the fiberglass is exposed to the outside, the surface is suitable for color painting.

[0126] 3. The composite plates are joined by applying pressure with a press machine, and the structure is stabilized by cooling at room temperature.

[0127] Example 3: Fabrication of a multi-layer sandwich structure non-combustible insulation panel

[0128] 1. Prepare a composite plate (steel plate + glass fiber corrugated structure) and apply a low-emissivity coating (emissivity 0.05) to the steel plate surface in contact with the intermediate layer.

[0129] 2. A glass fiber honeycomb (thickness 20 mm), a CO₂ gas insulation layer pouch, or an insulation board filled with CO₂ gas is inserted into some intermediate layers, and an intermediate layer (irregular structure, honeycomb, CO₂ insulation) is placed between the composite plates to form a multi-layer sandwich structure.

[0130] 3. Apply a moisture barrier to the panel surface to enhance condensation prevention performance.

[0131] Example 4: Fabrication of a multi-stage sandwich structure using CO₂ insulation

[0132] 1. A CO₂ gas insulation layer pouch (thickness 20 mm) is prepared according to Section 3.1 and inserted into the intermediate layer.

[0133] 2. Prepare an insulating board (thickness 20 mm) filled with CO₂ gas according to Section 3.2 and insert it into the intermediate layer.

[0134] 3. A multi-stage sandwich structure is formed by alternately arranging CO₂ gas insulation layer pouches and boards between composite plates (steel plate + glass fiber corrugated structure).

[0135] 4. Join by applying pressure of 100°C and 30kPa with a press machine, and cool at room temperature for 2 hours.

[0136] Example 5: Thermal insulation performance test

[0137] - Temperature conditions: Indoor 25°C, relative humidity 60%, duct internal temperature 10°C.

[0138] - Result: Surface temperature maintained above the dew point (16.7°C) at 24.24°C, no condensation occurred.

[0139] - Thermal Resistance: Meets building insulation standards with 5.8 m²·K / W for roofing and 4.8 m²·K / W for walls. Thermal resistance is improved when using insulation boards filled with CO₂ gas. Explanation of the symbols

[0141] 10: First iron plate 20: First air layer (including fiberglass egg cartons, honeycomb, CO₂ gas pouches, or CO₂ insulation boards) 21: Uneven structure (egg carton shape) 30: Second iron plate 40: Second air layer (including fiberglass egg cartons, honeycomb, CO₂ gas pouches, or CO₂ insulation boards) 50: Third iron plate 60: Non-retardant resin-impregnated glass fiber 70: Top finishing material (lid plate) 80: CO2 gas insulation 81: CO2 gas insulation outer shell main body 82: CO2 gas insulation outer shell cover 83: Pouch outer shell 84: Reflective coating layer 85: CO2 gas space

Claims

Claim 1 A non-combustible thermal insulation composite panel characterized by comprising: a steel plate; glass fibers; and a non-combustible resin that combines the steel plate and the glass fibers. Claim 2 A non-combustible thermal insulation composite plate according to claim 1, characterized in that the steel plate has a low-emissivity coating applied to at least one surface in contact with the intermediate layer to reduce radiant heat transfer. Claim 3 A non-combustible thermal insulation composite plate according to claim 1, characterized in that the glass fiber is formed as a non-combustible resin-impregnated glass fiber mat or an uneven structure. Claim 4 In paragraph 3, the non-combustible thermal insulation composite plate is characterized in that the height of the uneven structure is 10 to 80 mm. Claim 5 A non-combustible thermal insulation composite plate according to claim 1, characterized in that the steel plate is made of a cold-rolled steel plate or a galvanized steel plate with a thickness of 0.1 to 1.5 mm. Claim 6 A non-combustible insulation panel characterized by comprising: a plurality of non-combustible insulation composite plates according to claim 1; and a plurality of intermediate layers disposed between the plurality of non-combustible insulation composite plates and having a multi-stage sandwich structure including an intermediate layer. Claim 7 A non-combustible thermal insulation panel according to claim 6, characterized in that the plurality of intermediate layers are each formed with a thickness of 10 to 80 mm. Claim 8 A non-combustible insulation panel according to claim 6, characterized in that some of the plurality of intermediate layers comprise aluminum, glass fiber, honeycomb material made of non-combustible / semi-non-combustible treated paper, or an inflatable insulation pouch containing CO₂ gas. Claim 9 A non-combustible insulation panel according to claim 6, characterized in that a moisture barrier is additionally applied to the surface of the non-combustible insulation panel to prevent condensation. Claim 10 In claim 6, the non-combustible insulation panel is characterized by being used as a building material or duct insulation material. Claim 11 A non-combustible thermal insulation composite plate according to claim 1, characterized in that the glass fiber has a low-emissivity coating applied to one surface and is bonded to the steel plate by applying a non-combustible resin. Claim 12 A non-combustible insulation panel according to claim 6, characterized in that some of the plurality of intermediate layers comprise a board made of an expandable insulation material containing CO₂ gas. Claim 13 A non-combustible insulation panel according to claim 6, characterized in that some of the plurality of intermediate layers include a board made of insulating material filled with CO₂ gas.