Extruded composite parts, method for manufacturing the same and mold apparatus for manufacturing the extruded composite parts
By inserting a reinforcing member like steel wire into the extrusion process, the method addresses the limitations of conventional aluminum extrusions, achieving improved mechanical properties and simplifying manufacturing, suitable for automotive applications.
Patent Information
- Application Number
- KR1020250058057
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-02
- Publication Date
- 2026-11-10
AI Technical Summary
Conventional methods for enhancing aluminum extrusions face challenges such as poor extrudability, complex manufacturing processes, and high material costs due to the addition of alloying elements like Sc, leading to variations in mechanical characteristics and difficulties in mass production.
A method involving the insertion of a reinforcing member, such as steel wire, into the extrusion die during the extrusion process to create a composite part, optimizing parameters like extrusion speed, ratio, and weld zone length to improve tensile strength and toughness.
The resulting extruded composite parts exhibit enhanced tensile strength, bending strength, and impact resistance, enabling the production of lightweight yet durable automotive components without compromising productivity.
Smart Images

Figure PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a part produced by an extrusion process, a method for manufacturing the same, and a mold for an extrusion process. Background Technology
[0002] For example, the automotive industry is under continuous pressure to produce vehicles with excellent fuel efficiency and safety. Consequently, active developments are underway, such as applying lightweight materials to designs that enhance rigidity or using less high-strength materials. Furthermore, research on crash components is actively being conducted to respond to increasingly stringent crash regulations worldwide.
[0003] Although aluminum is used in various industrial fields due to its lightness and excellent processability, its inherent alloy characteristics result in relatively lower strength and durability compared to iron-based materials, exposing limitations when applied to structures subjected to heavy loads. To overcome these inherent limitations and align with the aforementioned trends, research has traditionally focused on developing materials and heat treatments that enhance strength and ductility to ensure shock absorption capabilities in aluminum extrusions. Examples include the development of 6000- and 7000-series high-strength alloys and technologies for manufacturing high-toughness extrusions by controlling grain growth through heat treatment optimization.
[0004] In conventional technology, high-strength materials produced by adding alloying elements suffer from poor extrudability, which necessitates lowering extrusion speeds and consequently reduces productivity. Furthermore, the traditional methods described earlier for enhancing aluminum properties have limitations in fundamentally improving mechanical characteristics. To overcome this, additional processes, such as incorporating design modifications or applying composite materials, inevitably occur, resulting in disadvantages such as complex manufacturing processes and increased material costs.
[0005] In addition, adding rare earth elements such as Sc is disadvantageous in terms of cost, and the grain refinement method through heat treatment control results in variations in different parts of the extruded material, requiring a high level of quality control to overcome this, which is disadvantageous in terms of mass production. Therefore, there is a need for a simpler and more effective method of strength improvement.
[0006] The matters described in the background technology above are intended to aid in understanding the background of the invention and may include matters that are not prior art already known to those skilled in the art to which this technology belongs. Prior art literature
[0007] Korean Patent Publication No. 10-2023-0142779 The problem to be solved
[0008] The present invention has been devised to solve the aforementioned problems, and the purpose of the present invention is to provide an extruded composite part having high strength and high toughness compared to aluminum material by applying an extruded composite material in which a reinforcing member is inserted into the extruded material. means of solving the problem
[0009] A method for manufacturing an extruded composite part according to one aspect of the present invention comprises the steps of inserting a reinforcing member into the internal space of an extrusion die and pressurizing an extrusion material supplied into the internal space of the extrusion die to extrude from the die hole of the extrusion die.
[0010] Here, the extrusion step is characterized in that the billet formed from the extrusion material is branched and then combined and extruded from the die hole.
[0011] Specifically, by the extrusion step, the reinforcing member is inserted onto the weld line where the branched billets are joined.
[0012] Alternatively, by the extrusion step, the reinforcing member is characterized by being aligned and inserted into the center of the extruded material.
[0013] In addition, the extruded material is made of aluminum, and the reinforcing member may be steel wire.
[0014] Meanwhile, the extrusion speed of the above extrusion step may be 1 to 3 mm / s.
[0015] In addition, the extrusion ratio (A0 / Af), which is the ratio of the billet cross-sectional area (A0) to the extrusion cross-sectional area (Af) in the above extrusion step, may be 45 or more and 100 or less.
[0016] In addition, the length of the weld zone where the branched billets are joined in the extrusion step may be 20 mm to 40 mm.
[0017] In addition, the surface roughness (Ra) of the above reinforcing member may be 0.3 to 0.5 μm.
[0018] Next, an extruded composite part according to one aspect of the present invention is characterized by an extruded composite comprising an extruded material and a reinforcing member inserted inside the extruded material, which is extruded.
[0019] Here, the reinforcing member is characterized by being aligned and inserted into the center of the extruded material.
[0020] In addition, the extruded material is made of aluminum, and the reinforcing member may be steel wire.
[0021] Next, a mold device for manufacturing an extruded composite part according to one aspect of the present invention comprises an extrusion die having an internal space and a die hole formed therein, a ram that pressurizes an extrusion material supplied to the internal space of the extrusion die to extrude the extrusion material from the die hole of the extrusion die, and a reinforcing member supply unit disposed in the internal space of the extrusion die and supplying a reinforcing member to the internal space of the extrusion die.
[0022] In addition, the reinforcing member supply unit may be spaced apart from the inner surface of the extrusion die.
[0023] In addition, the reinforcing member supply unit may be positioned in the center of the extrusion die. Effects of the invention
[0024] The extruded composite part according to the present invention has improved tensile strength, bending strength, and impact resistance compared to conventional aluminum parts.
[0025] For example, it is possible to manufacture extruded parts with a tensile strength of 400 MPa using a high-strength wire insert by using a commercial extruded 6xxx-series material with a strength of 250 to 300 MPa.
[0026] In addition, by using stainless steel wire with a small difference in thermal expansion coefficient from aluminum, the formation of intermetallic compounds at the interface of the extruded composite can be suppressed and bonding strength can be secured.
[0027] Furthermore, by forming guide holes in the extrusion die and utilizing the flow force of the billet to feed the wire, the extrusion of heterogeneous composite materials is possible without a separate feeding mechanism. Instead of configuring a separate device, existing industrial extrusion equipment can be utilized, simplifying equipment configuration and reducing maintenance costs. Brief explanation of the drawing
[0028] Figure 1 schematically illustrates the mold and extrusion process of the present invention. Figure 2 is an enlarged view of the die hole portion of Figure 1 and shows a part of the extruded composite part. Figure 3 shows the flow and wire feed during extrusion. FIG. 4 sequentially illustrates the method for manufacturing an extruded composite part of the present invention. Figure 5 shows the results of strength and elongation of a comparative example part, and Figure 6 shows the results of strength and elongation of a part according to the present invention. FIG. 7 is the actual shape of an extruded composite part according to the present invention, and FIG. 8 is a cross-section of the extruded composite. Figures 9 and 10 show the interface state according to the wire specifications. Figure 11 shows the grain growth state according to RAM speed. FIGS. 12 and FIGS. 13 are examples of applications of the extruded composite parts of the present invention. FIGS. 14 and FIGS. 15 are examples of extruded composite parts manufactured according to the present invention. Specific details for implementing the invention
[0029] In order to fully understand the present invention, the operational advantages of the present invention, and the objectives achieved by the implementation of the present invention, reference must be made to the accompanying drawings illustrating preferred embodiments of the present invention and the contents described therein.
[0030] In describing preferred embodiments of the present invention, known technologies or repetitive descriptions that may unnecessarily obscure the essence of the invention will be shortened or omitted.
[0031] FIG. 1 schematically illustrates the mold and extrusion process of the present invention, and FIG. 2 shows an enlarged view of the die hole portion of FIG. 1 and a part of an extruded composite part.
[0032] And, FIG. 4 sequentially illustrates the method for manufacturing an extruded composite part of the present invention.
[0033] Hereinafter, with reference to FIGS. 1, 2 and 4, an extruded composite part according to one embodiment of the present invention, a method for manufacturing the same, and a mold for manufacturing an extruded composite part will be described.
[0034] The present invention relates to a technology for an automotive part in which a high-strength / high-toughness unidirectional extruded composite material is applied, in which a reinforcing member is inserted inside an aluminum extruded material.
[0035] That is, it is a technology for manufacturing extruded composite parts by extruding an extruded composite material in which a reinforcing member (21) is inserted inside an aluminum extruded material (22).
[0036] The concept of the invention can be simply explained as inserting stainless steel, which has an elastic modulus three times that of aluminum, into the interior of an aluminum extruded material in an existing extrusion process capable of producing complex shapes with high dimensional accuracy. Through this, the high-rigidity material internally shares the external force applied to the material, thereby securing high-rigidity characteristics compared to conventional aluminum extruded materials. In addition, since stainless steel wire has excellent tensile properties, the unidirectional composite material of this technology can secure good tensile properties even when using low-strength aluminum material, and has the advantage of maintaining productivity without compromising extrudability.
[0037] A billet-shaped extrusion material (22) is supplied by pressure from a ram into the internal space of an extrusion die (30), and the supplied extrusion material (22) is extruded from the die hole, thereby manufacturing an extrusion composite part (10) processed into the cross-sectional shape of the extrusion die (30).
[0038] The extrusion die (30) includes a reinforcing member supply unit (31) disposed in an internal space, and a reinforcing member (21) is supplied through a reinforcing member guide hole formed in the reinforcing member supply unit (31) and inserted into the extrusion material (22).
[0039] As referenced in FIG. 3, a wire can be inserted by a metal flow that is combined with and advances with a billet without a separate feeder. The reinforcing member (21) can be inserted on the weld line where the branched billet flow is combined, and can be inserted aligned with the center of the extruded material (22) during the flow process.
[0040] To this end, it is preferable that the reinforcing member supply unit (31) be spaced apart from the inner surface of the extrusion die (30) and positioned in the center of the internal space of the extrusion die (30).
[0041] Referring to Fig. 4, the method for manufacturing an extruded composite is summarized as follows: first, the billet and the mold are preheated, and a reinforcing member (wire) is inserted and supplied through the reinforcing member guide hole of the reinforcing member supply section.
[0042] Then, the billet is pressurized to extrude the material, and an extruded composite part is manufactured through processes such as cutting / straightening, heat treatment, and surface treatment.
[0043] The supply of reinforcing material can be carried out at a time corresponding to the start of extrusion.
[0044] Here, by optimizing the extrusion speed, extrusion ratio, internal weld zone length, and surface condition of the insert wire to ensure the quality and mechanical performance of the extruded composite, it can be applied to the manufacture of automotive structural parts that simultaneously secure precise durability and lightweight properties.
[0045] The process factors affecting extrusion properties are as follows, and detailed boundary process conditions are required to ensure wire feeding and interface quality.
[0046] 1. Alloy composition: Extrusion is easier when the types and amounts of fine alloying elements are fewer. In this invention, A6082-T6 material, which is mainly used for high-strength impact parts, was applied, but alloys such as A6060, A6005, and A6063, which are used for general automobile body parts, can also be applied.
[0047] 2. Billet temperature: Although extrusion is easier at higher temperatures, the process was fixed at 450°C to prevent defects caused by liquefaction (600~650°C) in cases of excessively high temperatures.
[0048] 3. Extrusion Speed: While a faster extrusion speed improves productivity, it increases the risk of internal defects (cracks, pores) and may result in uneven deformation distribution. An extrusion speed of 1 to 3 mm / s is desirable.
[0049] 4. Extrusion ratio: Refers to the ratio (A0 / Af) of the billet cross-sectional area (A0) to the extrusion cross-sectional area (Af). As the extrusion ratio increases, strength increases, but internal cracks may occur. It is desirable to have a ratio of 45 or higher and 100 or lower.
[0050] 5. Mold Design: If the weld zone length is short, it is difficult to automatically pull the wire and interfacial bonding is poor, so it is important to secure the length of the weld zone. It is desirable to have a length of 20 mm to 40 mm. The weld zone refers to the length of the mold area where divided metals meet and bond inside the extrusion mold.
[0051] 6. Wire surface condition: Two wire specifications, Bright and Dull, with controlled surface conditions were applied so that the flowing aluminum could effectively pull the wire, and the Bright specification is more preferable.
[0052] It is preferable that the surface roughness (Ra) of the bright wire be 0.3 to 0.5 μm and the surface roughness (Ra) of the dull wire be 1.0 to 1.6 μm.
[0053] Table 1 shows the results of a test plan designed using the 'response surface method-central composite design' for the four factors (extrusion speed, extrusion ratio, weld zone length inside the mold, and wire surface specifications) presented in the present invention. The extrusion material used in the example is a 7-inch A6082 alloy billet, and the material specified as the reinforcing member is a SUS304 wire with a tensile strength of 1800 MPa, a fracture elongation of 2.5%, and a diameter of Φ1.
[0054] division Extrusion variables Physical properties Extrusion ratio Weld zone(mm) RAM speed (mm / s) Billet preheating temperature (°C) Wire types Tensile strength × Fracture deformation (MPa%) Remarks (Comparison Subject_Effect and Cause) Comparative Example 1 45 20 3.0 450 - 3862 standard Comparative Example 2 80 20 3.0 450 - 4362 Comparative Example 1_Improvement of Physical Properties_Increase in Extrusion Ratio Comparative Example 3 100 20 3.0 450 - 6110 Comparative Example 2_Improvement of Physical Properties_Increase in Extrusion Ratio Comparative Example 4 115 20 3.0 450 - 4634 Comparative Example 3_Degradation of physical properties, internal defects_Increase in extrusion ratio Comparative Example 5 80 10 3.0 450 1800MPa / 2.5% / Bright - Comparative Example 2_Wire feeding impossible_Internal defect_Weld zone reduction Example 1 80 20 3.0 450 1800MPa / 2.5% / Bright 6140 Comparative Examples 2 & 5_Improvement of Physical Properties Example 2 80 40 3.0 450 1800MPa / 2.5% / Bright 6411 Example 1_Improvement of physical properties (improvement of interfacial bonding)_Increase in weld zone Example 3 80 40 1.0 450 1800MPa / 2.5% / Bright 6489 Example 2_Equivalent Physical Properties_Lower Limit of RAM Speed Comparative Example 6 80 40 0.5 450 1800MPa / 2.5% / Bright 5291 Examples 2 & 3_Physical Property Saturation and Reduction (Grain Growth)_RAM Speed Reduction Comparative Example 7 80 40 5.0 450 1800MPa / 2.5% / Bright 4171 Example 2_Degradation of physical properties) Defects / Wire breakage_Excessive RAM speed Comparative Example 8 80 40 1.0 450 1800MPa / 2.5% / Dull 4100 Example 3_Degradation of physical properties_Interface non-bonding_Dull wire Example 4 45 20 3.0 450 1800MPa / 2.5% / Bright 5050 Comparative Example 1_Improvement of physical properties Example 5 45 40 1.0 450 1800MPa / 2.5% / Bright 5015 Example 4_Similar physical properties Comparative Example 9 45 40 1.0 450 1800MPa / 2.5% / Dull 3862 Example 4_Degradation of physical properties_Interfacial non-bonding_Dull wire Example 6 100 20 3.0 450 1800MPa / 2.5% / Bright 7220 Comparative Example 3_Improvement of physical properties Example 7 100 40 1.0 450 1800MPa / 2.5% / Bright 7550 Example 6_Physical properties equivalent Comparative Example 10 100 40 1.0 450 1800MPa / 2.5% / Dull 3978 Example 7_Degradation of physical properties_Interfacial non-bonding_Dull wire
[0055] (Comparative Examples 1-5) Conventional extruded materials without high-strength insert wires have a 'tensile strength × elongation at break' of 3800 to 6100 MPa%. As the extrusion ratio increases up to 100, the physical properties improve, but if it exceeds this, not only do the physical properties become non-uniform, but productivity also decreases and the equipment may be burdened.
[0056] When extruded under the conditions of the embodiment of the present invention, the 'tensile strength × elongation at break' is 3800~7550 MPa%. This indicates that the impact performance of the extruded material to which the present invention is applied is improved, and it was confirmed that the physical properties increase by approximately 20%. However, even if a high-strength wire is present as an insert, if the extrusion conditions and the wire surface condition are not optimized, there is a possibility that the physical properties or the extrusion process may be disadvantageous.
[0057] First, looking at the conditions of the examples, which are similar to those confirmed in the comparative example, if the speed is less than 1 mm / s, the critical deformation amount is small, so the grain size increases and the material properties deteriorate, and if it exceeds 3.0 mm / s, excessive processing heat is generated, causing a problem of quality deterioration. Also, if the weld zone length in the mold is short, less than 20 mm, the extruded material is insufficient to pull the wire and cannot be supplied, and a problem of poor interface quality occurs.
[0058] Furthermore, it can be observed that when the wire has a high surface roughness (Dull specification), the interface between the wire and the extruded base material is not bonded, resulting in a decrease in strength. This trend is contrary to the generally known facts regarding the bonding of various dissimilar materials. In typical dissimilar material bonding (insert casting, CFRP-metal bonding, etc.), the bonding surface is enlarged through various patterns on the solid metal material to induce the formation of a mechanical interlocking structure. However, in the present invention, interfacial bonding is good when the surface roughness of the bonding surface is smooth, while a separation of the interface can be observed when the roughness is poor. This is presumed to be due to the pressure environment where the solid flow of the extruded metal is insufficient to fill the narrow patterning space provided on the small contact surface of the Φ1.0 wire.
[0059] The actual test results of the comparative and exemplary examples presented in Table 1 are shown in Figures 5 and 6. As shown in Figure 5, in extruded materials without a wire inserted, physical properties can be improved by adjusting the extrusion ratio. When a wire is inserted, the maximum tensile strength increases as shown in Figure 6. In particular, when a wire of the Bright specification with excellent surface roughness was applied, it was possible to produce products with good interfacial bonding and excellent strength and elongation (Examples 3 and 7), whereas in the case of a wire with the Dull surface treatment specification, the wire fractured first after reaching the maximum tensile strength, followed by secondary fracture of the aluminum base material (Comparative Example 8).
[0060] FIG. 7 is the actual shape of an extruded composite part according to the present invention, and FIG. 8 is a cross-section of the extruded composite.
[0061] Figures 9 and 10 show the interface state according to the wire specifications. As can be seen in Figures 9 and 10, this is due to the interfacial bonding force between the wire and the aluminum matrix. The Bright specification showed good interfacial bonding, whereas when the Dull specification wire was applied, interfacial non-bonding occurred. Through this, it was possible to understand the effect of the difference in load distribution of the internal high-strength member according to the interfacial bonding force on the mechanical properties of the composite.
[0062] In addition, the ram speed on the left side of FIG. 11 is 3.0 mm / sec and on the right side is 0.5 mm / sec. When the extrusion ram speed is too low at 0.5 mm / sec, the crystal grains grow and the material properties decrease; when it is too high at 5.0 mm / sec, as shown in FIG. 12, the wire cannot be fed into the composite material at an appropriate speed and breaks during feeding. (Comparative Examples 6, 7)
[0063] In addition, when the weld zone length is insufficient at 10 mm, as shown in FIG. 13, the contact length between the aluminum and the wire is insufficient, resulting in a problem where proper feeding is not achieved and internal defects are caused (Comparative Example 5).
[0064] As described above, the extruded composite part according to the present invention has improved tensile strength, bending strength, and impact resistance compared to conventional aluminum parts.
[0065] Therefore, when applied to a bumper beam / side sill component (11) for a vehicle body as shown in Fig. 14, the absorption capacity for absorbing impact energy is high, thereby reducing the collision energy transmitted to passengers inside the cabin.
[0066] Meanwhile, when a vehicle is driven at high speed, the vehicle body undergoes deformation due to the force applied to the suspension. Since the extruded composite material of the present invention has a higher tensile strength compared to conventional aluminum materials, it is possible to manufacture a strut bar (12) that controls torsional deformation and evenly distributes the load received by the suspension.
[0067] Although the present invention has been described above with reference to the illustrated drawings, it is obvious to those skilled in the art that it is not limited to the described embodiments and can be modified and varied in various ways without departing from the spirit and scope of the invention. Accordingly, such modifications or variations should be deemed to fall within the scope of the claims of the present invention, and the scope of rights of the present invention should be interpreted based on the appended claims. Explanation of the symbols
[0068] 10 : Extruded composite parts 21 : Reinforcement member 22 : Extruded material 30: Extrusion die 31 : Reinforcement member supply section
Claims
Claim 1 A method for manufacturing an extruded composite part, comprising the steps of: inserting a reinforcing member into the internal space of an extrusion die; and pressurizing the extrusion material supplied into the internal space of the extrusion die to extrude it from the die hole of the extrusion die. Claim 2 A method for manufacturing an extruded composite part according to claim 1, wherein the extrusion step is characterized in that a billet formed from the extruded material is branched and then combined and extruded from the die hole. Claim 3 A method for manufacturing an extruded composite part according to claim 2, characterized in that, by the extrusion step, the reinforcing member is inserted onto a weld line where the branched billets are joined. Claim 4 A method for manufacturing an extruded composite part according to claim 2, characterized in that, by the extrusion step, the reinforcing member is aligned and inserted into the center of the extruded material. Claim 5 A method for manufacturing an extruded composite part according to claim 1, characterized in that the extruded material is an aluminum material and the reinforcing member is a steel wire. Claim 6 A method for manufacturing an extruded composite part according to claim 1, characterized in that the extrusion speed of the extrusion step is 1 to 3 mm / s. Claim 7 A method for manufacturing an extruded composite part according to claim 1, wherein the extrusion ratio, which is the ratio (A0 / Af) of the billet cross-sectional area (A0) to the extrusion cross-sectional area (Af) in the extrusion step, is 45 or more and 100 or less. Claim 8 A method for manufacturing an extruded composite part, wherein, in claim 1, the length of the weld zone where the branched billets are joined during the extrusion step is 20 mm to 40 mm. Claim 9 A method for manufacturing an extruded composite part, characterized in that, in claim 1, the surface roughness (Ra) of the reinforcing member is 0.3 to 0.5 μm. Claim 10 An extruded composite part comprising an extruded material; and a reinforcing member inserted inside the extruded material, wherein the extruded composite is extruded. Claim 11 An extruded composite part according to claim 10, characterized in that the reinforcing member is aligned and inserted into the center of the extruded material. Claim 12 An extruded composite part according to claim 10, characterized in that the extruded material is aluminum and the reinforcing member is steel wire. Claim 13 A mold device for manufacturing extruded composite parts, comprising: an extrusion die having an internal space and a die hole formed therein; a ram that pressurizes an extrusion material supplied to the internal space of the extrusion die to extrude the extrusion material from the die hole of the extrusion die; and a reinforcing member supply unit disposed in the internal space of the extrusion die and supplying a reinforcing member to the internal space of the extrusion die. Claim 14 A mold device for manufacturing extruded composite parts, wherein, in claim 13, the reinforcing member supply unit is spaced apart from the inner surface of the extrusion die. Claim 15 A mold device for manufacturing extruded composite parts, wherein, in claim 14, the reinforcing member supply unit is disposed in the central part of the extrusion die.