Repairing method for structure

The repair method using a composition of cement, MMA resin, and magnesium hydroxide-titanate enhances durability against salt and acid corrosion, improving crack resistance and enabling winter repairs by heat application.

KR103043645B1Active Publication Date: 2026-11-11(주)에스알디엔지니어링
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020250130880
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-09-12
Publication Date
2026-11-11
Estimated Expiration
2045-09-12

AI Technical Summary

Technical Problem

Conventional repair materials for reinforced concrete structures lack long-term durability against salt damage and sulfuric acid corrosion, particularly in marine and wastewater-exposed environments, and do not ensure adequate physical properties like workability, crack resistance, and strength.

Method used

A repair method using a composition comprising cement, MMA resin, calcium sulfoaluminate, and magnesium hydroxide surface-modified by titanate, optionally with aluminum salts, calcium oxide, and tridecyl octanoate, applied in layers with a carbon fiber mesh for reinforcement and heat application.

Benefits of technology

The method enhances salt and sulfuric acid resistance, improves crack resistance, and allows repairs to be conducted even in winter by generating heat, ensuring the structure behaves as a unified unit with improved physical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025105150519-PAT00001_ABST
    Figure 112025105150519-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a structural repair method comprising the steps of: removing and cleaning a deteriorated area of ​​a structure to be repaired (S10); pouring a repair material composition comprising cement, MMA resin, and calcium sulfoaluminate onto the structure to be repaired (S20); and finishing the poured surface (S30), wherein the repair material composition further comprises magnesium hydroxide surface-modified by titanate.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a repair method using a repair material composition capable of improving various physical properties such as salt resistance and sulfuric acid resistance. Background Technology

[0003] Generally, reinforced concrete structures undergo deterioration due to various factors such as freeze-thaw cycles, salt damage, carbonation, chemicals, various bacteria and sulfur gases (S) generated from sewage. In cases of severe damage, the concrete may spall, the reinforcing steel within the concrete may be exposed or corroded internally, resulting in a decrease in durability and load-bearing capacity, which in turn leads to problems such as a reduction in the service life of the structure.

[0004] In order to repair or reinforce deteriorated areas of such reinforced concrete structures, a construction method involving plastering or spraying is applied to restore the area where the concrete was removed to its original state after removing the deteriorated and damaged concrete and performing repair or reinforcement on the rebar.

[0005] Regarding the mortar for the above-mentioned spray-on repair method, technologies such as Korean registered patent No. 10-0412339 (Title of invention: Composition of a structural repair material), Korean published patent No. 10-2005-0032358 (Title of invention: High-strength underwater non-separating cross-section repair cement composition), Korean published patent No. 10-2005-0032359 (Title of invention: Low-shrinkage grout mortar composition for cross-section injection), and Korean registered patent No. 10-0405022 (Title of invention: Mortar composition for concrete repair) have been proposed. As such, spray-on repair methods utilizing these technologies have the advantage of being able to repair simply and quickly.

[0006] However, the repair material compositions applied in these conventional concrete repair methods do not provide resistance to deterioration caused by various factors, and thus have the problem of being unable to ensure long-term durability against salt damage, sulfuric acid corrosion, etc., when applied to marine structures, structures exposed to wastewater, etc. Prior art literature

[0008] Republic of Korea Patent Registration No. 0412339 The problem to be solved

[0009] Accordingly, the present invention has been made to solve the aforementioned conventional problems, and its purpose is to provide a repair method using a repair material composition that has excellent resistance to various types of deterioration, including salt damage and sulfuric acid corrosion, while also ensuring physical properties such as workability, crack resistance, and strength. means of solving the problem

[0011] A structural repair method according to the present invention for achieving the above-mentioned purpose (hereinafter referred to as the "method of the present invention") comprises the steps of: removing and cleaning a deteriorated area of ​​a structure to be repaired (S10); pouring a repair material composition comprising cement, MMA resin, and calcium sulfoaluminate onto the structure to be repaired (S20); and finishing the poured surface (S30); wherein the repair material composition further comprises magnesium hydroxide surface-modified by titanate.

[0012] As an example, the above step S20 is characterized by including: a step of forming a primer layer by applying a primer to a repair target (S21); a step of forming a reinforcement layer by placing a mesh net on the primer layer (S22); and a step of forming a cross-sectional repair layer by pouring the repair material composition on top of the reinforcement layer (S23).

[0013] As one example, the above mesh is woven from carbon fiber and is characterized by being connected to an electric power supply means to apply electricity.

[0014] As an example, the above repair material composition is characterized by further including an aluminum salt.

[0015] As an example, the above repair material composition is characterized by further including calcium oxide.

[0016] As an example, the above-mentioned repair material composition is characterized by further including tridecyl octanoate.

[0017] delete

[0018] delete Effects of the invention

[0020] As explained above, the method of the present invention has the advantage of being able to improve various physical properties, such as salt resistance and sulfuric acid resistance, through the repair of the structure.

[0021] In addition, the method of the present invention has the advantage of enabling the deteriorated part of the structure and the cast part to behave as one unit by means of a reinforcing layer, and allowing heat to be applied to the reinforcing layer so that repairs can be performed even during the winter season. Brief explanation of the drawing

[0023] FIG. 1 is a block diagram illustrating the method of the present invention. FIG. 2 is a side cross-sectional view showing a structure cast by the method of the present invention. Figure 3 is a photograph showing a repair material composition used in the method of the present invention. Specific details for implementing the invention

[0024] A preferred embodiment according to the present invention will be described in detail below.

[0026] The method of the present invention is characterized by comprising the steps of: removing and cleaning the deteriorated area of ​​the structure to be repaired as shown in FIG. 1 (S10); pouring a repair material composition comprising cement, MMA resin, and calcium sulfoaluminate onto the structure to be repaired (S20); and finishing the poured surface (S30).

[0027] First, the method includes a step (S10) of removing and cleaning the deteriorated parts of the structure to be repaired. Here, since various known technologies can be applied for removing and cleaning the deteriorated parts, a detailed description thereof is omitted.

[0028] Next, there is a step (S20) of pouring a repair material composition comprising cement, MMA resin, and calcium sulfoaluminate onto the repair target.

[0029] The present step (S20) is characterized by including: a step of forming a primer layer by applying a primer to the repair target (S21); a step of forming a reinforcement layer by placing a mesh net on the primer layer (S22); and a step of forming a cross-sectional repair layer by pouring the repair material composition on top of the reinforcement layer (S23).

[0030] As shown in FIG. 2, through such construction, a structure is formed in which a primer layer (3), a reinforcing layer (4), and a cross-section repair layer (5) are sequentially stacked on the repair target (2) of the structure.

[0031] Since the primer constituting the above primer layer (3) can be made using various known technologies, a detailed description thereof is omitted.

[0032] A reinforcing layer (4) is formed on the upper part of the primer layer (3), and the reinforcing layer (4) is composed of a mesh so as to enable the primer layer (3) and the cross-section repair layer (5) to function as a single unit, thereby forming a cross-section repair layer (5) that is firmly attached to the repair target (2) of the structure.

[0033] In particular, in the present invention, the mesh net constituting the reinforcing layer (4) is formed by weaving carbon fibers (41), and additionally, although not shown in the drawings, an electric power supply means is connected to one side of the mesh net made of carbon fibers so that electricity is applied to the reinforcing layer (4) by the electric power supply means, thereby allowing heat generation to occur.

[0034] The reason for allowing heat generation by applying electricity to the reinforcing layer (4) in this way is to enable repair work to be carried out, especially during the winter season. That is, in addition to the solid repair function of the aforementioned cross-section repair layer (5), the reinforcing layer (4) allows for early hardening even during the winter season by applying heat to the primer layer (3) and the cross-section repair layer (5), thereby enabling the application of the repair method.

[0035] Since there are various known technologies for applying electricity by connecting an electric power supply means to a reinforcing layer (4) made of carbon fiber, a detailed description thereof is omitted.

[0036] In addition, the present invention provides a repair material composition capable of increasing resistance to various types of deterioration, which is described below.

[0037] The above repair material composition is characterized by comprising cement, MMA resin, and calcium sulfoaluminate.

[0038] Preferably, it is appropriate to include 5 to 30 parts by weight of MMA resin and 1 to 10 parts by weight of calcium sulfoaluminate per 100 parts by weight of cement.

[0039] The above MMA resin preferably includes PMMA, MMA, BAM (BUTYL ACRYLATE MONOMER), 2-HEA, Triethylene glycol diacrylate (TEGDA), and Methoxy silane.

[0040] 2-Hydroxyethyl-paran-toluidine (pte) is used as a curing accelerator, and 2,6-Di-tert-butyl-4-methylphenol (BHT) is used as a storage stabilizer.

[0041] PMMA is a solid polymer that forms a resin together with monomers MMA and BAM, and its tensile strength and elongation are determined according to their respective TG (glass transition temperature).

[0042] 2-HEA and Triethylene Glycol Diacrylate (TEGDA) serve as crosslinking agents; 2-HEA improves adhesion due to its -OH groups, while Triethylene Glycol Diacrylate (TEGDA) improves crosslinking density and provides flexibility. As a curing accelerator, 2-Hydroxyethyl-paran-toluidine (pte) promotes the reaction of the MMA resin at room temperature.

[0043] The above MMA resin is mixed with BPO to induce a continuous addition reaction to form a polymer. Then, methoxy silane is hydrolyzed by moisture adsorbed on the surface of the filler used in the present invention to produce highly reactive Si-oH groups, which are fixed on the surface in various forms such as physical adsorption, chemical adsorption, and hydrogen bonding.

[0044] As a result, it serves to strengthen the bonding strength between inorganic and organic materials of different phases. It is preferable that this MMA resin be formulated with 50 to 150 parts by weight of MMA, 50 to 100 parts by weight of BAM, 5 to 30 parts by weight of 2-HEA, 5 to 30 parts by weight of Triethyleneglycol diacrylate (TEGDA), and 0.5 to 1.5 parts by weight of methoxy silane, based on 100 parts by weight of PMMA.

[0045] The above calcium sulfur aluminate is intended to prevent cracking caused by the rapid reduction in the volume of cement during mortar curing.

[0046] If the content of the calcium sulfur aluminate is below the above mixing range, the amount used is too small to provide effective crack resistance; conversely, if used in excess of the above range, adhesion and bonding properties may decrease, or the density of the concrete after curing may be lowered, leading to a weakened strength; therefore, it is preferable to use it within the above range.

[0047] In addition, the present invention provides an example in which an aluminum salt is further included in addition to the above composition.

[0048] The purpose is to improve the salt resistance of the paste by including more aluminum salts. The type of aluminum salt is not limited, and aluminum sulfate, etc., may be used.

[0049] Al by the addition of these aluminum salts 3 + Ions have a high charge density, and within the retention material, Cl - It is designed to improve salt resistance by enabling electrostatic binding or adsorption with (chlorine ions).

[0050] Preferably, it is reasonable to mix 1 to 10 parts by weight of aluminum salt per 100 parts by weight of cement.

[0051] However, when aluminum salts are added, they can act as strong Lewis acids and react with initiators (e.g., BPO) or accelerators (e.g., amines) of MMA resins, thereby interfering with or delaying the polymerization reaction. In other words, problems such as reduced initial strength and delayed air curing may arise due to delayed curing.

[0052] In addition, as aluminum salts react with moisture to form an acidic environment, degradation due to corrosion of the paste may occur.

[0053] To solve these problems, the present invention provides an example in which calcium oxide is additionally included in addition to the aluminum salt.

[0054] Calcium hydroxide, which is preferentially hydrated by the addition of calcium oxide, is chloride ions (Cl - The purpose is to improve salt resistance by chemically adsorbing ) and, in particular, to ensure early strength that may be reduced by the addition of aluminum salts through the addition of calcium oxide.

[0055] Calcium oxide promotes the hydration reaction, allowing hydration products to form early, thereby ensuring early strength.

[0056] In addition, calcium oxide neutralizes acidic conditions that may be formed by aluminum salts, thereby enabling the control of degradation caused by corrosion of the paste.

[0057] Preferably, it is appropriate to mix 1 to 5 parts by weight of calcium oxide per 100 parts by weight of cement.

[0058] However, while the addition of calcium oxide ensures high strength, there is a problem in that crack resistance may be reduced due to a rapid exothermic reaction, and workability may be compromised.

[0059] Accordingly, the present invention provides an example in which tridecyl octanoate is further included. The addition of tridecyl octanoate delays the rapid hydration reaction caused by the addition of calcium oxide, thereby improving resistance to thermal cracking, and also alleviates viscosity to compensate for the decrease in workability.

[0060] It is appropriate to mix the above tridecyl octanoate in an amount of 0.01 to 0.1 parts by weight per 100 parts by weight of cement.

[0061] Meanwhile, the present invention provides an example in which magnesium hydroxide is additionally included in addition to the above compositions to improve sulfuric acid resistance.

[0062] Magnesium hydroxide is Mg 2 + and SO4 2- This is done to inhibit corrosion caused by sulfuric acid through the reaction or pH buffering action, thereby lowering the reactivity with sulfates.

[0063] Preferably, it is reasonable to mix 1 to 10 parts by weight of magnesium hydroxide with respect to 100 parts by weight of cement.

[0064] However, when only magnesium hydroxide is added, magnesium hydroxide is an inorganic fine particle with high polarity, resulting in weak compatibility and chemical bonding with MMA resin; consequently, there may be a problem where crack resistance is reduced due to interfacial separation.

[0065] In addition, the surface hydroxyl groups (-OH) of magnesium hydroxide can react with the initiator of the MMA resin, etc., and act as a factor that reduces early strength due to delayed curing.

[0066] To solve these problems, the present invention provides an example in which magnesium hydroxide surface-modified by titanate is added.

[0067] Surface modification by titanate reacts with the -OH groups on the surface of magnesium hydroxide to form a chemically immobilized organic layer, thereby improving adhesion at the interface, and curing delay can be controlled by suppressing side reactions with the initiator of the -OH groups.

[0068] Various known methods can be applied to surface-modify magnesium hydroxide into titanate. For example, 0.5 to 2 parts by weight of titanate coupling agent are prepared for every 100 parts by weight of magnesium hydroxide, and the titanate coupling agent is slowly mixed into the magnesium hydroxide powder by direct spraying or dropping, with a mixing speed of 500 to 1500 rpm and a mixing time of 10 to 30 minutes. Then, the mixture is dried at room temperature (about 18°C) for 12 to 24 hours to remove adsorbed moisture and reaction by-products, thereby obtaining the product.

[0070] The present invention will be explained below through experimental examples.

[0071] As shown below, each sample was prepared, and the experimental results are shown in Table 1.

[0072] [Example 1]

[0073] A sample was prepared by mixing 10 parts by weight of MMA resin and 5 parts by weight of calcium sulfoaluminate for every 100 parts by weight of cement.

[0074] [Example 2]

[0075] A sample was prepared by mixing 10 parts by weight of MMA resin, 5 parts by weight of calcium sulfur aluminate, and 5 parts by weight of aluminum salt for every 100 parts by weight of cement.

[0076] [Example 3]

[0077] A sample was prepared by mixing 10 parts by weight of MMA resin, 5 parts by weight of calcium sulfur aluminate, 5 parts by weight of aluminum salt, and 1 part by weight of calcium oxide for every 100 parts by weight of cement.

[0078] [Example 4]

[0079] A sample was prepared by mixing 10 parts by weight of MMA resin, 5 parts by weight of calcium sulfur aluminate, 5 parts by weight of aluminum salt, 1 part by weight of calcium oxide, and 0.05 parts by weight of tridecyl octanoate for every 100 parts by weight of cement.

[0080] [Example 5]

[0081] A sample was prepared by mixing 10 parts by weight of MMA resin, 5 parts by weight of calcium sulfur aluminate, and 5 parts by weight of magnesium hydroxide for every 100 parts by weight of cement.

[0082] [Example 6]

[0083] The mixture was formulated to include 10 parts by weight of MMA resin, 5 parts by weight of calcium sulfur aluminate, and 5 parts by weight of magnesium hydroxide surface-modified with titanate for every 100 parts by weight of cement. For the magnesium hydroxide surface-modified with titanate, 1 part by weight of titanate coupling agent was prepared for every 100 parts by weight of magnesium hydroxide, and the titanate coupling agent was mixed by spraying it directly onto the magnesium hydroxide powder, with a mixing speed of 1000 rpm and a mixing time of 30 minutes. After mixing, the mixture was dried at room temperature (approx. 18°C) for 12 hours to produce the product.

[0085] Test items unit Example 1 Example 1 Example 1 Example 1 Example 1 Example 1 Test standards Compressive strength (3 days) N / mm 2 21.1 17.2 24 22.3 16.3 21.9 KS F4042 Compressive strength (28 days) N / mm 2 41.2 40.1 44 42.5 39.7 43.2 Chloride ion penetration resistance Coulombs 824 541 519 523 718 711 Compressive strength after sulfate immersion (28 days) N / mm 2 21.5 20.1 23.5 22.1 36.7 38.8 Flow mm 150 155 125 150 155 160 Rate of change in length % -0.025 -0.029 -0.091 -0.031 -0.059 -0.031 Color change (after 90 days of curing) - Partial discoloration - - - -

[0087] As shown in Table 1 above, when comparing Example 1 and Example 2, it can be seen that Example 2 is advantageous in terms of salt resistance. However, in the case of Example 2, it can be seen that the initial strength decreases and discoloration of the paste occurs due to the addition of aluminum salt, whereas in the case of Example 3, it can be seen that the initial strength is improved by adding calcium oxide in addition to the aluminum salt, and discoloration does not occur by neutralizing the acidification of the paste.

[0088] However, in the case of Example 3, it can be seen that workability is significantly reduced compared to Example 2, and an unfavorable effect is also exhibited in terms of crack resistance. Accordingly, in the case of Example 4, it can be seen that by adding more tridecyl octanoate, the reduction in workability is controlled while maintaining early strength and anti-discoloration ability, and crack resistance is also improved.

[0089] Meanwhile, comparing Example 1 and Example 5, it can be seen that Example 5 is advantageous in terms of sulfuric acid resistance. This is attributed to the addition of magnesium hydroxide; on the other hand, in the case of Example 5, it can be seen that the initial strength is reduced compared to Example 1, and it is disadvantageous in terms of crack resistance. Accordingly, in the case of Example 6, by adding magnesium hydroxide surface-modified with titanate, it is possible to achieve an effect similar to Example 5 in terms of sulfuric acid resistance, while also improving the initial strength compared to Example 5 and exhibiting an advantageous effect in terms of crack resistance.

[0091] As described above, although the present invention has been explained by limited embodiments and drawings, the present invention is not limited to the above embodiments, and it is obvious that various modifications and variations from the description above may be possible by those skilled in the art to which the present invention belongs. Explanation of the symbols

[0093] 2 : Structure to be repaired 3 : Primer layer 4 : Reinforcement layer 5 : Section repair layer

Claims

Claim 1 A method for repairing a structure comprising: a step of removing and cleaning a deteriorated area of ​​a structure to be repaired (S10); a step of pouring a repair material composition comprising cement, MMA resin, and calcium sulfoaluminate onto the structure to be repaired (S20); and a step of finishing the poured surface (S30); wherein the repair material composition further comprises magnesium hydroxide surface-modified by titanate. Claim 2 A structural repair method according to claim 1, wherein the above step S20 comprises: a step of forming a primer layer by applying a primer to a repair target (S21); a step of forming a reinforcement layer by placing a mesh net on the primer layer (S22); and a step of forming a cross-sectional repair layer by pouring the repair material composition on top of the reinforcement layer (S23). Claim 3 A structural repair method according to claim 2, characterized in that the mesh is woven from carbon fiber and is connected to an electric power supply means to apply electricity. Claim 4 A structural repair method according to claim 1, characterized in that the repair material composition further includes an aluminum salt. Claim 5 A structural repair method according to claim 4, characterized in that the repair material composition further includes calcium oxide. Claim 6 A structural repair method according to claim 5, characterized in that the repair material composition further includes tridecyl octanoate. Claim 7 delete Claim 8 delete

Citation Information

Patent Citations

  • Dispersant compositions comprising hydrophobic and hydrophilic modified maleated natural oils, and applications thereof

    AU2024239017A1

  • Mortar composition for sectional restoration with light weight and rapid hardness, and method of sectional restoration using same

    KR101367166B1

  • Carbon fiber textile reinforcing member with anodic metal line, and repair and reinforcement method of concrete structure using the same

    KR1020190050553A

  • Flame retardant structure reinforcement that combines Basalt Fiber fiber and high strength fiber

    KR102230395B1

  • Crack inhibiting and rapid curing type mortar composition for repair and reinforcing concrete structure and constructing method using the same

    KR102370536B1