Sulfide-based solid electrolyte, solid electrolyte layer, and lithium-ion secondary battery
By incorporating sulfur in the S8 state within the crystal structure, the sulfide-based solid electrolyte achieves improved adhesion and conductivity, addressing brittleness and binder-related issues, leading to better battery performance.
Patent Information
- Application Number
- KR1020237015315
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-11
- Filing Date
- 2021-11-05
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2041-11-05
AI Technical Summary
Sulfide-based solid electrolytes with an agyrodite-type crystal structure face challenges in achieving good adhesion and maintaining lithium ion conductivity due to brittleness and the need for binders, which reduce the electrolyte proportion and conductivity.
Incorporating sulfur in the S8 state within the crystal structure of the sulfide-based solid electrolyte enhances adhesion and flexibility, resulting in improved lithium ion conductivity without the need for excessive binders.
The modified electrolyte exhibits excellent adhesion and lithium ion conductivity, facilitating easier compaction into compact forms with enhanced battery characteristics.
Smart Images

Figure 112023049867812-PCT00001
Abstract
Description
Technology Field
[0001] The present invention relates to a sulfide-based solid electrolyte, a solid electrolyte layer, and a lithium-ion secondary battery. Background Technology
[0002] Lithium-ion secondary batteries are widely used in portable electronic devices such as mobile phones and notebook personal computers.
[0003] Conventionally, liquid electrolytes have been used in lithium-ion secondary batteries, but there were concerns about leakage or ignition, and it was necessary to enlarge the case for safety design. In addition, improvements were desired regarding the short battery life and narrow operating temperature range.
[0004] In contrast, all-solid-state lithium-ion secondary batteries that use a solid electrolyte as the electrolyte are attracting attention due to the potential for improved safety, high-speed charging and discharging, and miniaturization of the case.
[0005] Solid electrolytes are broadly classified into sulfide-based and oxide-based solid electrolytes, but sulfide ions exhibit a higher polarization rate and higher ionic conductivity compared to oxide ions. As a sulfide-based solid electrolyte, Li 10 GeP2S 12 LGPS-type crystals such as Li6PS5Cl, argyrodite-type crystals such as Li7P3S 11 LPS crystallized glass, such as crystallized glass, is known.
[0006] Patent Document 1 can be cited as an example in which an azirodite-type sulfide-based solid electrolyte is disclosed. The sulfide-based solid electrolyte disclosed in Patent Document 1 has a cubic crystal structure belonging to the space group F-43m, and composition formula: Li 7-x PS 6-x Ha xIt contains a compound represented by (Ha is Cl or Br) (x=0.2 to 1.8), and also has a lightness L value of the L*a*b* color system of 60.0 or higher. This is intended to increase charge-discharge efficiency or cycle characteristics by increasing lithium ion conductivity and lowering electron conductivity. Prior art literature
[0007] International Publication No. 2015 / 012042 The problem to be solved
[0008] When using sulfide-based solid electrolytes in lithium-ion secondary batteries, powdered sulfide-based solid electrolytes are sometimes processed into compacted forms such as pellets or layers (sheets). However, sulfide-based solid electrolytes having an agyrodite-type crystal structure are harder and have poor adhesion between powders compared to, for example, crystallized LPS glass.
[0009] In the case of such a azirodite-type sulfide-based solid electrolytes, it is necessary to apply relatively high pressure to sufficiently adhere the powder and improve the lithium ion conductivity of the compact. Furthermore, although it is possible to process it into a compact by applying relatively high pressure, the resulting compact tends to become brittle; therefore, to maintain the strength of the compact, it is necessary to add binders or the like to supplement the adhesion. If the amount of binders or the like increases, the proportion of the sulfide-based solid electrolyte in the compact becomes relatively small, and there is concern that the lithium ion conductivity of the compact will decrease.
[0010] Therefore, the present invention aims to provide a sulfide-based solid electrolyte in which the compacted body exhibits good lithium ion conductivity due to excellent adhesion. means of solving the problem
[0011] As a result of repeated careful examination, the inventors discovered that in a sulfide-based solid electrolyte comprising an azirodite-type crystal structure, by incorporating sulfur in the crystal structure in the S8 state, the sulfide-based solid electrolyte becomes relatively flexible, thereby obtaining a sulfide-based solid electrolyte with excellent adhesion when formed into a compact, and thus completed the present invention.
[0012] That is, the present invention relates to the following [1] to [7].
[0013] [1] It is a sulfide-based solid electrolyte used in lithium-ion secondary batteries, and
[0014] It includes an azirodite-type crystal structure containing Li, P, S and Ha, and
[0015] The above Ha is at least one selected from the group consisting of F, Cl, Br, and I, and
[0016] In the Raman spectrum obtained by Raman spectroscopy measurement, 140 to 170 cm⁻¹ -1 , 205 to 235 cm -1 and 460 to 490 cm -1 Having a peak at least 1 selected from the group consisting of,
[0017] A sulfide-based solid electrolyte that does not have an endothermic peak within the range of 70 to 160°C in a DSC curve obtained by differential scanning calorimetry (DSC).
[0018] [2] The composition of the above crystal structure is Li a PS b Ha c (5≤a≤7, 4≤b≤6 also 0 <c≤2)로 표시되는, 상기 [1]에 기재된 황화물계 고체 전해질.
[0019] [3] In the above Raman spectrum, 420 to 440 cm -1 Peak intensity of (I A ) and 460 to 490cm -1 Peak intensity of (IB Ratio of ) B / I A A sulfide-based solid electrolyte described in [1] or [2] above, having a value of 0.005 or higher.
[0020] [4] When in powder form with an average particle size of 2 to 10 μm,
[0021] The lithium ion conductivity σ (30kN) at 25℃ when the above powder is compacted into a compact at a pressure of 30kN, and
[0022] A sulfide-based solid electrolyte described in any one of [1] to [3], wherein the ratio of lithium ion conductivity σ(10kN) to σ(10kN) at 25°C when the above powder is compacted at a pressure of 10kN is 1.34 or less.
[0023] [5] A sulfide-based solid electrolyte described in any one of [1] to [4], having an elastic modulus of 5 to 40 GPa.
[0024] [6] A solid electrolyte layer comprising a sulfide-based solid electrolyte described in any one of [1] to [5] above.
[0025] [7] A lithium-ion secondary battery comprising a sulfide-based solid electrolyte as described in any one of [1] to [5] above. Effects of the invention
[0026] According to the sulfide-based solid electrolyte of the present invention, since the adhesion is excellent when forming a compact from a powder state, it becomes easy to obtain a compact exhibiting good lithium ion conductivity. By using the sulfide-based solid electrolyte of the present invention as a solid electrolyte for a lithium-ion secondary battery, an improvement in the battery characteristics of the lithium-ion secondary battery can be expected. Specific details for implementing the invention
[0027] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and may be implemented with arbitrary modifications within the scope of not departing from the gist of the present invention. In addition, the term "to" indicating a numerical range is used to mean that the values described before and after it are included as lower and upper limits. In this specification, sulfide-based solid electrolytes may be simply referred to as "solid electrolytes." In this specification, weight-based ratios (percentages, etc.) are the same as mass-based ratios (percentages, etc.).
[0028] Sulfide-based solid electrolytes
[0029] A sulfide-based solid electrolyte according to an embodiment of the present invention (hereinafter referred to as "the present solid electrolyte") is used in a lithium-ion secondary battery. The present solid electrolyte comprises an azyrodite-type crystal structure (hereinafter also referred to as "azyrodite-type crystal") comprising Li, P, S, and Ha. Here, Ha is at least one selected from the group consisting of F, Cl, Br, and I. Furthermore, the present solid electrolyte has a combined S8 peak in the Raman spectrum obtained by Raman spectroscopy and does not have an endothermic peak attributed to the phase transition or melting of sulfur in the DSC curve obtained by differential scanning calorimetry (DSC). That is, the present solid electrolyte has, in the Raman spectrum, a peak between 140 and 170 cm⁻¹. -1 , 205 to 235 cm -1 and 460 to 490 cm -1 It has a peak at least one selected from the group consisting of, and in the DSC curve, does not have an endothermic peak within the range of 70 to 160°C.
[0030] The present solid electrolyte comprises an azyrodite-type crystal structure containing Li, P, S, and Ha. The halogen element represented by Ha is at least one selected from the group consisting of F, Cl, Br, and I. The azyrodite-type crystal may consist of only one type with the same composition, or may include two or more types with different compositions.
[0031] The halogen element is at least one selected from the group consisting of F, Cl, Br, and I, but since the crystal is prone to becoming an azirodite type, it is preferable to include at least one of Cl and Br, more preferable to include Cl, and even more preferable to include Cl alone or a mixture of Cl and Br.
[0032] The crystal structure can be interpreted from the powder X-ray diffraction (XRD) pattern. In the XRD pattern, the crystal can be described as a azirodite type by having peaks at positions 2θ = 15.7±0.5° and 30.2±0.5°. In addition to the above, it is preferable for the XRD pattern to additionally have a peak at the position 2θ = 18.0±0.5°, and it is even more preferable for it to have a peak at the position 2θ = 25.7±0.5°.
[0033] The preferred crystal structure is cubic (e.g., F-43m), but rhombohedral, tetragonal, or rectangular structures with reduced symmetry, as well as monoclinic structures with reduced symmetry, may also exist.
[0034] In the present solid electrolyte, the azirodite-type crystal structure contains S8 molecules within the crystal structure. Furthermore, "containing S8 molecules within the crystal structure" includes not only cases where S8 molecules are contained within the crystal structure, but also cases where S8 molecules exist outside the azirodite-type crystal structure but are uniformly dispersed at the grain boundaries between crystals. That is, in the present solid electrolyte, S8 molecules are considered to exist in a state where they are uniformly dispersed within the crystal structure and at least one of the grain boundaries between crystals.
[0035] S8 crystalline sulfur has a relatively low elastic modulus. In other words, the S8 molecular structure can be considered flexible. Consequently, as S8 molecules exist uniformly within an agyrodite-type crystal structure, the crystal becomes relatively flexible, meaning the elastic modulus is reduced. This allows for improved adhesion of the solid electrolyte.
[0036] In contrast, when a heterogeneous state exists in which azyrodite-type crystals and S8 molecules are separated—in other words, when regions composed of aggregated S8 molecules exist in the solid electrolyte—it is believed that these aggregates of S8 molecules act as a resistive layer, hindering the lithium ion conduction of the crystal. Furthermore, regions where S8 molecules are aggregated tend to have a locally lower elastic modulus, and since deformation tends to concentrate in these areas, it is thought that the presence of such regions makes it difficult to apply uniform pressure to the solid electrolyte. That is, by uniformly incorporating S8 molecules into the crystal structure, this solid electrolyte becomes a relatively flexible and uniform crystal, and also exhibits excellent lithium ion conductivity.
[0037] The present solid electrolyte has a binding peak of S8 in the Raman spectrum obtained by Raman spectroscopy. On the other hand, the present solid electrolyte does not have an endothermic peak attributed to the phase transition or melting of sulfur in the DSC curve obtained by differential scanning calorimetry (DSC). Having a binding peak of S8 in the Raman spectrum implies that the solid electrolyte contains S8 molecules. In contrast, not having an endothermic peak of sulfur in the DSC curve implies that there is no sulfur in the solid electrolyte existing as a group of S8 molecules separated from the azirodite-type crystal structure. In a solid electrolyte having a region where S8 is separated from the azirodite-type crystal structure and exists as a group of S8 molecules, the DSC curve has an endothermic peak of sulfur. Therefore, since the Raman spectrum has a binding peak of S8 and the DSC curve does not have an endothermic peak attributed to the phase transition or melting of sulfur, it can be determined that the solid electrolyte contains S8 molecules in its crystal structure.
[0038] Furthermore, in materials that uniformly contain S8 molecules within their crystal structure, such as the present solid electrolyte, there is a difference in the particle size distribution after grinding compared to heterogeneous solid electrolytes in which azirodite-type crystals and S8 exist separately. That is, the present solid electrolyte tends to exhibit smaller variation in particle size after grinding and a sharp shape in the particle size distribution, whereas heterogeneous solid electrolytes tend to exhibit larger variation in particle size after grinding and a broad shape in the particle size distribution. The particle size distribution can be verified by measuring it using a laser diffraction particle size analyzer.
[0039] The S8 coupling peak in the Raman spectrum refers specifically to the Raman shift 140 to 170 cm⁻¹ originating from the SS bond of the S8 molecule. -1 , 205 to 235 cm -1 and 460 to 490 cm -1It refers to the peak in [location]. That is, in the Raman spectrum, this solid electrolyte [is] at 140 to 170 cm⁻¹. -1 , 205 to 235 cm -1 and 460 to 490 cm -1 It has a peak at least 1 selected from the group consisting of
[0040] In addition, the Raman spectrum obtained by Raman spectroscopy measurement refers to the one obtained under general conditions, such as an excitation light wavelength of 532 nm and a power of 1 to 3 mW, although it is not particularly changed by the measurement conditions.
[0041] The endothermic peak originating from the phase transition of sulfur in the DSC curve specifically refers to the endothermic peak around 90 to 115°C resulting from the state change from the α-form to the β-form. The endothermic peak originating from the melting of sulfur specifically refers to the endothermic peak around 115 to 140°C resulting from the state change of sulfur from solid to liquid. Here, "nearby" refers to a range, for example, within ±20°C. Therefore, by not having an endothermic peak within the range of 70 to 160°C in the DSC curve, it can be confirmed that the present solid electrolyte does not possess an endothermic peak attributed to phase transition or melting. In cases where S8 is contained in the crystal structure, as in the present solid electrolyte, it is believed that an azyrodite-type crystal is positioned right next to the S8 molecule. Consequently, since the S8 molecule does not undergo thermodynamic state changes such as phase transition or melting, it is believed that such an endothermic peak is not observed.
[0042] In this specification, a DSC curve obtained by differential scanning calorimetry (DSC) refers to one obtained under conditions of a heating rate of 5°C / min and a measurement temperature range of 25°C to 300°C.
[0043] The composition of the azirodite-type crystal structure is Li a PS b Hac (5≤a≤7, 4≤b≤6 also 0 <c≤2)로 표시된다.
[0044] Here, from the perspective of lithium ion conductivity, c, representing the content ratio of Ha, is preferably 0.5 or higher, more preferably 1 or higher, and even more preferably 1.5 or higher. Additionally, from the perspective of inhibiting corrosion of the metal current collector, c is preferably 1.9 or lower, more preferably 1.8 or lower, and even more preferably 1.7 or lower.
[0045] In addition, the above Li a PS b Ha c It is a composition that also includes S of S8 in the crystal structure.
[0046] Here, since typical azyrodite-type crystals tend to be deficient in sulfur, a:b:c in a typical azyrodite-type solid electrolyte is,
[0047] (6-x):(5-xy):(1+x)(y is 0≤y≤1)
[0048] There is a tendency for this to happen.
[0049] Meanwhile, in that the present solid electrolyte involves the addition of S8 to a general azyrodite-type crystal, the amount of S8 is z (z is 0 <z≤2)로 하면, 본 고체 전해질에 있어서의 a:b:c는,
[0050] (6-x):(5-x-y+z):(1+x)
[0051] It can be.
[0052] The composition can be analyzed by appropriately combining ICP emission spectroscopy, atomic absorption spectroscopy, ion chromatography, etc.
[0053] In addition, regarding the content of S8 in the present solid electrolyte, 420 to 440 cm of the Raman spectrum -1 PS4 visible in the location 3- Peak intensity of origin (I A ) and 460 to 490cm-1 Peak intensity of S8 origin visible at position (I B Ratio of ) B / I A It can be evaluated as follows. In the Raman spectrum, 420 to 440 cm -1 Peak intensity of (I A ) and 460 to 490cm -1 Peak intensity of (I B Ratio of ) B / I A In terms of improving adhesion, 0.005 or higher is preferable, 0.007 or higher is more preferable, and 0.01 or higher is even more preferable. Also, I B / I A In terms of suppressing the decrease in lithium ion conductivity, 0.5 or less is preferable, and 0.3 or less is more preferable.
[0054] The crystallite size of the azirodite-type crystal is preferably small from the perspective of obtaining good lithium ion conductivity when the solid electrolyte is finely ground and formed into a battery, and specifically, it is preferably 1000 nm or less, more preferably 500 nm or less, and even more preferably 250 nm or less. The lower limit of the crystallite size is not particularly limited, but is generally 5 nm or more.
[0055] The crystallite size after heat treatment increases compared to before heat treatment, but it is desirable that the crystallite size remains within the above range even after heat treatment.
[0056] The crystallite size can be calculated by using Scherrer's formula to determine the half-width of the peaks in the XRD pattern.
[0057] As one of the criteria for evaluating the adhesion of the solid electrolyte, the ratio σ(30kN) / σ(10kN) can be used, which is the lithium ion conductivity σ(30kN) when the powder is compacted at a pressure of 30kN and the lithium ion conductivity σ(10kN) when the powder is compacted at a pressure of 10kN, when the powder is in a powder state with an average particle size of 2 to 10㎛. Here, the average particle size refers to the D50 average particle size (median diameter: the particle size at which the cumulative frequency on a volume basis reaches 50%). The average particle size is obtained, for example, by a particle size distribution measuring device. Furthermore, in this specification, the lithium ion conductivity σ is used as a value at 25℃ unless otherwise specified.
[0058] In addition, depending on the application, the solid electrolyte of this powder having an average particle size of 2 to 10 μm may be further ground into a powder form with an average particle size of less than 2 μm. In that case, the value of the ratio σ' (30 kN) / σ' (10 kN), which is the lithium ion conductivity σ' (30 kN) when the powder with an average particle size of less than 2 μm is compacted at a pressure of 30 kN and the lithium ion conductivity σ' (10 kN) when the powder with an average particle size of less than 2 μm is compacted at a pressure of 10 kN, becomes greater than the ratio σ (30 kN) / σ (10 kN) when the powder has an average particle size of 2 to 10 μm.
[0059] When a solid electrolyte in powder form is processed into a compact for use, the lithium ion conductivity of the compact improves as the powder particles become more closely bonded to each other. This is believed to be because the grain boundary resistance at the interface between powder particles decreases as the contact interface between particles increases.
[0060] When the same powder is compacted into a compact at higher pressure, adhesion improves, and consequently, lithium-ion conductivity increases. However, when the pressure exceeds a certain level, the lithium-ion conductivity reaches an upper limit (maximum conductivity) where it can no longer increase. The lower the pressure required to achieve maximum conductivity in the compact, the better the adhesion of the powder can be evaluated, as this allows the powder to be sufficiently compacted at lower pressure.
[0061] Powders requiring high pressure to achieve maximum conductivity can be processed into compacts by applying high pressure, but the resulting compacts are prone to brittleness. In such cases, it is necessary to add binders or similar materials to improve adhesion in order to maintain the strength of the compact. However, if the amount of binders or similar materials increases, the proportion of sulfide-based solid electrolytes within the compact becomes relatively small, raising concerns about a decrease in the lithium-ion conductivity of the compact. Therefore, if the adhesion of the powder is good, not only is it easier to achieve maximum conductivity at lower pressures, but the amount of binders or similar materials can also be suppressed to increase the proportion of sulfide-based solid electrolytes within the compact, thereby consequently improving the lithium-ion conductivity of the compact.
[0062] That is, σ(30kN) / σ(10kN) is typically 1 or greater, but as the value of σ(30kN) / σ(10kN) is smaller and closer to 1, it can be evaluated that the pressure required to achieve maximum conductivity of the compacted body is smaller. σ(30kN) / σ(10kN) is preferably 1.34 or less, more preferably 1.32 or less, and even more preferably 1.3 or less.
[0063] In addition, the lithium ion conductivity σ (30kN) of the solid electrolyte is preferably 0.1 mS / cm or higher, more preferably 0.5 mS / cm or higher, and even more preferably 1 mS / cm or higher from the perspective of obtaining good battery characteristics when used in a lithium-ion secondary battery. Although a larger value of σ (30kN) is desirable, typically the upper limit is about 100 mS / cm.
[0064] The elastic modulus of the solid electrolyte is preferably 50 GPa or less, more preferably 40 GPa or less, and even more preferably 30 GPa or less from the perspective of improving adhesion. The elastic modulus is preferably 1 GPa or more, more preferably 2 GPa or more, and even more preferably 5 GPa or more from the perspective of maintaining shape after molding. The elastic modulus can be measured, for example, using a nanoindenter.
[0065] In the present solid electrolyte, the proportion of an azirodite-type crystal structure is preferably 50 mass% or more, more preferably 65 mass% or more, and even more preferably 80 mass% or more, from the perspective of realizing high lithium-ion conductivity and obtaining the effects of the present invention more effectively. In addition, the upper limit is not particularly limited and may be 100 mass%, but generally it is 99 mass% or less. The proportion of an azirodite-type crystal structure can be calculated by including an internal standard material, measuring by XRD or neutron scattering, and comparing the peak intensity with that of the internal standard material.
[0066] In addition to azirodite-type crystals, other materials that may be included in the solid electrolyte include, for example, Li3PS4, Li4P2S6, Li2S, LiHa (where Ha is at least one halogen element selected from F, Cl, Br, and I). In addition, other lithium-ion conductive solid electrolytes may be included. Examples of other lithium-ion conductive solid electrolytes include glass or crystallized glass containing Li, P, and S.
[0067] However, if the present solid electrolyte further includes a substance having a binding peak of S8 in the Raman spectrum or an endothermic peak of sulfur in the DSC curve in addition to an azirodite-type crystal containing S8 in its crystal structure, the present solid electrolyte needs to be specified with such substance removed. Furthermore, the above case is, for example, when the present solid electrolyte additionally contains elemental sulfur (S8) in addition to an azirodite-type crystal. Also, in a solid electrolyte in which the azirodite-type crystal and S8 exist separately, the elemental sulfur (S8) present can be removed by, for example, heat treatment at 300°C for 1 hour.
[0068] Method for manufacturing sulfide-based solid electrolytes
[0069] As for the method for manufacturing the solid electrolyte, the method is not particularly limited as long as it is a method for obtaining a solid electrolyte having the above-described characteristics, but, for example, a method comprising a process of heating and melting raw materials containing Li, P, S and Ha (heating and melting process), and performing the heating and melting under a gas atmosphere containing sulfur elements.
[0070] In addition, the method for manufacturing the solid electrolyte may include other processes in a timely manner, such as a process for cooling the molten liquid obtained by additional heating and melting (cooling process), a process for reheating the solid obtained by the cooling process (reheating process), a grinding process, a drying process, etc. Each process is described below.
[0071] (Raw materials)
[0072] The raw material containing Li, P, S, and Ha can be a material that obtains a azirodite-type crystal containing Li, P, S, and Ha, and can use a conventionally known material.
[0073] For example, a mixture of a compound containing Li (lithium), a compound containing P (phosphorus), a compound containing S (sulfur), and a compound containing Ha (halogen) can be cited.
[0074] Examples of compounds containing Li include lithium compounds such as lithium sulfide (Li2S) and lithium oxide (Li2O), or lithium metal itself.
[0075] Examples of compounds containing P include phosphorus sulfides such as triphosphorus trisulfide (P2S3) and pentaphosphorus pentasulfide (P2S5), or phosphorus compounds such as phosphorus sulfides.
[0076] Examples of compounds containing S include the above lithium sulfide (Li2S), the above phosphorus sulfide (P2S3, P2S5), or hydrogen sulfide (H2S), and sulfur compounds can also be used.
[0077] Among compounds containing Ha, compounds containing Cl (chlorine) include, for example, lithium chloride (LiCl).
[0078] Among compounds containing Ha, compounds containing Br (bromine) include, for example, lithium bromide (LiBr).
[0079] Among these, as raw materials, a combination comprising at least one of lithium sulfide, phosphorus sulfide, lithium chloride, and lithium bromide is preferred.
[0080] These raw materials are highly unstable in the atmosphere, decompose upon reaction with water, and pose a risk of generating hydrogen sulfide gas or oxidation. Therefore, it is desirable to mix them in an inert atmosphere.
[0081] The raw materials may include additional substances (compounds, etc.) in addition to the above substances as additives, etc.
[0082] For example, in terms of improving the glass formation state of the obtained sulfide-based solid electrolyte, the raw material may include sulfides such as SiS2, B2S3, GeS2, Al2S3, Ga2S3, SnS2, SnS, and ZnS2. In addition, in terms of imparting moisture resistance, the raw material may include oxides such as SiO2, B2O3, GeO2, Al2O3, Ga2O3, SnO2, SnO, and ZnO. These compounds may be used individually or in combination of two or more types.
[0083] The amount of these compounds added is preferably 0.1% by weight or more relative to the total amount of raw materials, and more preferably 0.5% by weight or more. In addition, the amount added is preferably 50% by weight or less, and more preferably 40% by weight or less.
[0084] Mixing of raw materials can be performed, for example, by mixing using a mortar and pestle, mixing using media such as a planetary ball mill, or media-free mixing such as a fin mill, powder stirrer, or airflow mixing. The raw materials may be amorphized by mixing prior to heating. Additionally, heat treatment may be performed on the raw materials prior to heating and melting for purposes such as obtaining intermediates.
[0085] (Heating and melting process)
[0086] In the heating and melting process, the above-described raw material is heated and melted under a gas atmosphere containing sulfur elements.
[0087] Heating and melting are performed under a gas atmosphere containing sulfur. Examples of gases containing sulfur include sulfur gas, hydrogen sulfide gas, carbon disulfide gas, etc. From the perspective of efficiently introducing S8 into the crystal structure, it is desirable to include sulfur gas.
[0088] The gas containing the element sulfur may consist solely of gaseous compounds containing the element sulfur, such as sulfur gas, hydrogen sulfide gas, and carbon disulfide gas; however, from the perspective of cost reduction and use as a carrier gas for transporting the sulfur component, it is also desirable to include inert gases such as N2 gas, argon gas, and helium gas. Furthermore, the gas containing the element sulfur may contain impurities originating from sulfur sources, etc., provided that the present solid electrolyte is obtained within the specified range.
[0089] Sulfur gas (S) in a gas containing the element sulfur x The content of (x=2 to 8)) is preferably 0.01 vol% or more, more preferably 0.1 vol% or more, and even more preferably 0.2 vol% or more, from the perspective of ensuring a sufficient amount of sulfur element and carrying out the sulfur introduction reaction. In addition, the sulfur gas content is 100 vol% or less, and from the perspective of cost reduction or using an inert gas as a carrier gas, it is preferably 99 vol% or less, and more preferably 98 vol% or less. Sulfur gas (S x The content of (x=2 to 8)) can be measured by mass spectrometry gas chromatography.
[0090] Gases containing the elemental sulfur are obtained by heating a sulfur source. Therefore, the sulfur source is not particularly limited as long as it is elemental sulfur or a sulfur compound from which a gas containing the elemental sulfur is obtained by heating, but examples include elemental sulfur, organic sulfur compounds such as hydrogen sulfide and carbon disulfide, and iron sulfide (FeS, Fe2S3, FeS2, Fe 1-X (S, etc.), bismuth sulfide (Bi2S3), copper sulfide (CuS, Cu2S, Cu 1-x Examples include polysulfides such as S, lithium polysulfide, sodium polysulfide, polysulfides, and rubber that has undergone sulfur vulcanization treatment.
[0091] These sulfur sources are heated in a separately provided sulfur source heating section to generate a gas containing sulfur elements, and an inert gas such as N2, argon, or helium is conveyed to a heating and melting furnace as a carrier gas to obtain a gas atmosphere containing sulfur elements. By separating the sulfur source heating section from the section where the heating and melting process is performed, oxygen or moisture can be removed by reacting with the sulfur gas even if they are present in the incoming gas, thereby obtaining a high-quality, high-purity sulfide-based solid electrolyte with few impurities.
[0092] The temperature at which the sulfur source is heated can be appropriately selected depending on the type of sulfur source used, but for example, when using pure sulfur as the sulfur source, it is preferable to have a temperature of 250°C or higher and 750°C or lower.
[0093] Alternatively, among the above sulfur sources, a solid sulfur source such as elemental sulfur, H2S, Bi2S3, iron sulfide, copper sulfide, and CS2 may be conveyed in a fine state, such as powder, to a heated melting furnace by a carrier gas to obtain a gas atmosphere containing sulfur elements.
[0094] Alternatively, it is also desirable to obtain a gas atmosphere containing sulfur elements by adjusting the mixing ratio of the aforementioned compounds or elements so that sulfur is in excess in the raw materials, and by evaporating a portion of the sulfur component in the raw materials during heating and melting.
[0095] For example, the heating and melting process can be performed as follows. In a configuration divided into a sulfur source heating section and a section for performing the heating and melting process, a sulfur source is heated in the sulfur source heating section to generate a gas containing sulfur elements. The gas containing sulfur elements in an amount corresponding to the required sulfur partial pressure is sent to the section for performing the heating and melting process to obtain a gas atmosphere containing sulfur elements. The raw material described above is heated and melted under this atmosphere. At this time, the sulfur partial pressure in the gas atmosphere containing sulfur elements is 10 -3 Up to 100 atm is preferred.
[0096] By heating and melting the raw material under a gas atmosphere containing sulfur elements, sulfur is introduced into the molten raw material. By doing so, sulfur components that are prone to volatilization from the raw material can be replenished, and a sufficient amount of sulfur can be introduced into the solid electrolyte.
[0097] At this time, the molten raw material has a lowered viscosity due to the fluidization of the solid and is in a highly homogenized state. Therefore, the molten raw material has high solubility and diffusivity for gases containing sulfur elements. It is believed that by introducing sulfur in this liquid state, not only is the sulfur component constituting the crystal simply replenished, but S8 is also introduced into the crystal structure, thereby obtaining the present solid electrolyte. Furthermore, by introducing sulfur in the liquid state, the homogeneity of the composition of the solid electrolyte obtained is easily improved, and S8 is uniformly dispersed and contained within the crystal structure. Additionally, as described above, the inclusion of S8 within the crystal structure includes not only the case where S8 enters and is contained within the crystal structure, but also the case where S8 exists outside the azirodite-type crystal structure but is contained in a state of being uniformly dispersed at the grain boundaries between crystals.
[0098] In addition, it is preferable to perform heating and melting while stirring the molten liquid or a gas containing sulfur elements, as this makes it easier to obtain the effects of sulfur introduction and improved homogeneity.
[0099] The heating and melting temperature is preferably 600°C or higher, more preferably 630°C or higher, and even more preferably 650°C or higher, as this increases the fluidity of the molten liquid and promotes the reaction of sulfur introduction. In addition, the heating and melting temperature is preferably 900°C or lower, more preferably 850°C or lower, and even more preferably 800°C or lower from the perspective of suppressing deterioration or decomposition of components in the molten liquid due to heating.
[0100] The heating and melting time is preferably 0.1 hours or more, more preferably 0.5 hours or more, more preferably 0.7 hours or more, and more preferably 1 hour or more, as it allows the reaction of sulfur introduction to proceed. In addition, the heating and melting time is preferably 10 hours or less, more preferably 9.5 hours or less, and more preferably 9 hours or less, from the perspective of inhibiting deterioration or decomposition of components in the molten liquid due to heating.
[0101] In addition, the pressure during heating and melting is not particularly limited, but, for example, atmospheric pressure to low pressure is preferred, and atmospheric pressure is more preferred. Also, the sulfur partial pressure is 10 -3 It is preferable to set it to 100 atm. By using such a partial pressure of sulfur, sulfur can be introduced efficiently and at low cost without complicating the equipment, making it easy to obtain the desired sulfide-based solid electrolyte.
[0102] In order to prevent adverse reactions with steam or oxygen during heating and melting, the dew point is preferably -20°C or lower, and while the lower limit is not specifically restricted, it is generally around -80°C. In addition, the oxygen concentration is preferably 1000 ppm (by volume) or lower.
[0103] The specific method for heating and melting is not particularly limited, but for example, a method of placing the raw material in a heat-resistant container and heating it in a furnace may be used. As for the heat-resistant container, examples include a heat-resistant container made of carbon, a heat-resistant container containing oxides such as quartz, quartz glass, borosilicate glass, aluminosilicate glass, alumina, zirconia, and mullite, a heat-resistant container containing nitrides such as silicon nitride and boron nitride, and a heat-resistant container containing carbides such as silicon carbide. In addition, these heat-resistant containers may be formed as a bulk of the above materials, or they may be containers in which layers of carbon, oxides, nitrides, carbides, etc. are formed. In addition, heating may be performed while in a vacuum-sealed state.
[0104] (Cooling process)
[0105] The method for manufacturing the solid electrolyte preferably further includes a process of cooling a molten liquid obtained by heating and melting to obtain a solid. Cooling can be performed by a known method, and the method is not particularly limited.
[0106] With respect to maintaining the composition obtained by the heating and melting process, the cooling rate is preferably 0.01℃ / sec or higher, more preferably 0.05℃ / sec or higher, and even more preferably 0.1℃ / sec or higher. In addition, although no upper limit value for the cooling rate is specifically set, the cooling rate of the twin roller, which is generally said to have the highest cooling rate, is 1,000,000℃ / sec or lower.
[0107] Here, if the obtained solid is to be an amorphous sulfide-based solid electrolyte, it is preferable to obtain the solid by rapidly cooling the molten liquid obtained by heating and melting. Specifically, when rapidly cooling, the cooling rate is preferably 500°C / sec or higher, and more preferably 700°C / sec or higher. In addition, although the upper limit of the cooling rate is not specifically determined, the cooling rate of the twin roller, which is generally said to have the highest cooling rate, is 1,000,000°C / sec or lower.
[0108] In addition, during the cooling process, slow cooling may be performed to crystallize at least a portion of the solid, thereby obtaining a sulfide-based solid electrolyte having a desired crystal structure or a sulfide-based solid electrolyte composed of a crystalline phase and an amorphous phase. When slow cooling, the cooling rate is preferably 0.01°C / sec or higher, and more preferably 0.05°C / sec or higher. In addition, the cooling rate is preferably 500°C / sec or lower, and more preferably 450°C / sec or lower. Furthermore, the cooling rate may be appropriately adjusted according to the crystallization conditions.
[0109] (Reheating process)
[0110] Amorphous sulfide-based solid electrolytes or sulfide-based solid electrolytes containing an amorphous phase can promote high-temperature crystallization by heat treatment (post-annealing). In the method for manufacturing the solid electrolyte, if the solid obtained from the cooling process is an amorphous sulfide-based solid electrolyte, a sulfide-based solid electrolyte containing a crystalline phase is obtained by reheating the solid. Alternatively, if the solid obtained from the cooling process is, for example, a sulfide-based solid electrolyte containing an amorphous phase and a crystalline phase, the method may further include reheating the solid as necessary.
[0111] Depending on the intended use of the sulfide-based solid electrolyte obtained, the method for manufacturing the solid electrolyte may include a process of grinding the sulfide-based solid electrolyte obtained in the above process and a drying process. The specific methods are not limited and may be carried out using known methods.
[0112] (Solid electrolyte layer, lithium-ion secondary battery)
[0113] Since this solid electrolyte has excellent adhesion when formed from a powder into a compact, good lithium ion conductivity is obtained when processed into a compact such as a pellet or a layer (sheet).
[0114] Therefore, the present solid electrolyte can be suitably used in a solid electrolyte layer used in a lithium-ion secondary battery. The solid electrolyte layer may include other components, such as a binder, as needed. The binder or other components may be conventionally known materials.
[0115] With respect to the entire solid electrolyte layer, the content of the solid electrolyte is preferably 80 mass% or more, and more preferably 90 mass% or more. Since the solid electrolyte has excellent adhesion, the content of components added to supplement adhesion, such as binders, can be relatively small, and it is easy to improve the lithium ion conductivity of the solid electrolyte layer.
[0116] A method for forming a solid electrolyte layer is used according to conventionally known methods. For example, a solid electrolyte layer can be formed by dry press molding of solid electrolyte powder, etc., on a surface such as a positive electrode or a negative electrode. Alternatively, components constituting the solid electrolyte layer may be dispersed or dissolved in a solvent to form a slurry, coated into a layer (sheet), dried, and optionally press. Furthermore, a solid electrolyte layer may be formed on another substrate and transferred onto a surface such as a positive electrode or a negative electrode.
[0117] Regardless of the method used to form the solid electrolyte layer, in a solid electrolyte layer using this solid electrolyte, the adhesion between the particles of the solid electrolyte powder within the layer, or between the particles of the solid electrolyte powder and other components, is improved, making it easy to improve lithium ion conductivity.
[0118] The present solid electrolyte may be mixed with a positive electrode active material or a negative electrode active material and used as a positive electrode layer or a negative electrode layer. The positive electrode active material or negative electrode active material, current collector, binder, conductivity aid, etc., used in the positive electrode layer or negative electrode layer may be conventionally known materials. Even in the positive electrode layer or negative electrode layer, by using the present solid electrolyte, the adhesion between the particles of the solid electrolyte powder within the layer, or between the particles of the solid electrolyte powder and other components, is improved, making it easy to improve lithium ion conductivity.
[0119] The composition of the lithium-ion secondary battery containing the present solid electrolyte is not particularly limited, but for example, an all-solid-state lithium-ion secondary battery may be provided, comprising a solid electrolyte layer, a positive electrode layer, and a negative electrode layer, wherein at least one of these layers contains the present solid electrolyte. According to the lithium-ion secondary battery containing the present solid electrolyte, the adhesion between particles of the solid electrolyte powder or between particles of the solid electrolyte powder and other components within the lithium-ion secondary battery is improved, making it easier to improve lithium-ion conductivity, and thus an improvement in battery characteristics is expected.
[0120] The casing material of the lithium-ion secondary battery may also be a conventionally known material. The shape of the lithium-ion secondary battery may also be a conventionally known material, but examples include coin type, sheet type (film type), foldable type, cylindrical type with a wound bottom, button type, etc., and can be appropriately selected depending on the application.
[0121] Examples
[0122] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. Examples 1 to 5 are examples, and Examples 6 to 9 are comparative examples.
[0123] [evaluation]
[0124] (Powder X-ray diffraction)
[0125] XRD measurements were performed under the following conditions to obtain XRD spectra and analyze the crystal structure.
[0126] Device: Kabushiki Kaisha Rigaku, SmartLab
[0127] Source: CuKα line (λ=1.5418Å), Scan angle: 10 to 100°, Scan speed: 5° / min, Step count: 0.01° / step.
[0128] Since the sulfide-based solid electrolyte serving as the measurement sample deteriorates when exposed to the atmosphere, the sample was prepared under an atmosphere of non-exposure to the atmosphere and provided for measurement.
[0129] Sample preparation: Sulfide-based solid electrolyte powder with an average particle size of 5 to 10 μm was prepared by passing sulfide-based solid electrolyte powder, ground with a mortar and pestle, through a sieve with a mesh size of 100 μm. In addition, the particle size distribution was measured using a Microtrac laser diffraction particle size distribution analyzer MT3300EXII, and the average particle size was measured from the obtained volume-based particle size distribution chart.
[0130] (Composition Analysis)
[0131] The solid electrolyte powder weighed inside the glove box was dissolved in an alkaline aqueous solution, and the composition was analyzed by ICP emission spectroscopy for elements P and S, analysis by atomic absorption spectroscopy for element Li, and analysis by ion chromatography for elements Cl and Br.
[0132] (Raman spectroscopy measurement)
[0133] Raman spectroscopic measurements were performed under the following conditions to obtain Raman spectra and confirm the presence or absence of the S8 coupling peak. The measurements were conducted in an atmospheric non-exposure environment.
[0134] In Table 1, Raman shift 140 to 170 cm -1 , 205 to 235 cm -1 and 460 to 490 cm -1 If a peak was identified in at least one of them, it was indicated as "present" for the S8 coupling peak. On the other hand, if these peaks were not identified, it was indicated as "absent" for the S8 coupling peak. Furthermore, for the example where the S8 coupling peak is "present," from the obtained Raman spectrum, 420 to 440 cm⁻¹ -1 PS4 3- Peak intensity of origin (I A ) and 460 to 490cm -1 Peak intensity derived from S8 (I B Ratio of ) B / I A It produced.
[0135] Device Name: Kabushiki Kaisha Horiba Seisakusho, LabRAM HR Evolution
[0136] Excitation light wavelength: 532 nm, power during sample irradiation: 1 to 3 mW, objective lens: ×10, confocal pinhole: 200 µm, grating: 1200 gr / mm, number of integration cycles: 2 sec × 10 times, average of 10 measurement points.
[0137] (DSC measurement)
[0138] Under the following conditions, DSC measurements were performed using a differential scanning calorimeter to obtain a DSC curve, and the presence or absence of an endothermic peak of sulfur in the range of 70 to 160°C was confirmed.
[0139] In Table 1, if the sulfur endothermic peak was confirmed, it was marked "present," and if it was not confirmed, it was marked "absent." Measurements were taken in an environment without atmospheric exposure.
[0140] Device name: BRUKER AXS, DSC3300, Sample amount: 20 mg, Heating rate: 5 ℃ / min, Measurement temperature range: 25 ℃ to 300 ℃.
[0141] (Lithium ion conductivity measurement)
[0142] Using 100 mg of powder of a sulfide-based solid electrolyte, a compact (pellet 1) with a diameter of 1 cm was prepared at a pressure of 10 kN. In addition, a compact (pellet 2) with a diameter of 1 cm was prepared in the same way at a pressure of 30 kN.
[0143] For each pellet, the lithium ion conductivity was measured at 25°C by the AC impedance method (Potentistat / Galvanostat VSP manufactured by Bio-Logic Sciences Instruments, measurement frequency: 1 MHz to 100 Hz). The ratio σ(30 kN) / σ(10 kN), which is the lithium ion conductivity σ(10 kN) of Pellet 2 to the lithium ion conductivity σ(10 kN) of Pellet 1, is shown in Table 1.
[0144] In addition, σ (30 kN) is shown in Table 1 as the lithium ion conductivity of each sulfide-based solid electrolyte.
[0145] [Example 1]
[0146] Li6PS so that a gas atmosphere containing sulfur elements is obtained upon heating and melting. 5.3With Cl (excess sulfur) as the target composition, lithium sulfide powder (Sigma, purity 99.98%), phosphorus pentasulfide powder (Sigma, purity 99%), sulfur (Sigma, purity 99.99%), and lithium chloride powder (Sigma, purity 99.99%) were weighed under a dry nitrogen atmosphere, and mixed at 400 rpm for 4 hours using a planetary ball mill in the same atmosphere.
[0147] (Heating and melting process)
[0148] The obtained raw material mixture was placed in a heat-resistant container and heated and melted at 750°C for 1 hour under an atmosphere with a dew point of -60°C.
[0149] (Cooling process)
[0150] Subsequently, by cooling at a cooling rate of 1 to 1000℃ / sec, a solid was obtained as a sulfide-based solid electrolyte containing an amorphous phase and an azirodite-type crystalline phase. Li 6.01 PS 5.25 Cl 0.99 A product of the composition was obtained, and it was ground in an agate mortar and pestle, and the average particle size of the obtained powder was 5 μm.
[0151] [Example 2]
[0152] With Li6PS5Cl as the target composition, lithium sulfide powder (Sigma, purity 99.98%), phosphorus pentasulfide powder (Sigma, purity 99%), and lithium chloride powder (Sigma, purity 99.99%) were weighed under a dry nitrogen atmosphere and heated at 300°C for 1 hour in the same atmosphere.
[0153] (Heating and melting process)
[0154] The obtained compound was placed in a heat-resistant container and heated and melted at 730°C for 30 minutes under an atmosphere with a dew point of -60°C. At this time, sulfur gas obtained by heating elemental sulfur at a temperature of 350°C was supplied with N2 as a carrier gas so that the partial pressure of the sulfur gas was 0.1 atm, thereby obtaining a gas atmosphere containing sulfur elements, and sulfur was introduced into the molten liquid by performing heating and melting under this gas atmosphere. The content of sulfur gas in the gas atmosphere containing sulfur elements was 0.1 vol%.
[0155] (Cooling process)
[0156] Subsequently, by cooling at a cooling rate of 1 to 1000℃ / sec, a solid was obtained as a sulfide-based solid electrolyte containing an amorphous phase and an azirodite-type crystalline phase. Composition Li 6.05 PS 6.04 Cl 1.11 A sulfide-based solid electrolyte was obtained, and it was ground in an agate mortar and pestle, and the average particle size of the obtained powder was 5 μm.
[0157] [Example 3]
[0158] Except for changing the mixing ratio of the raw materials, the sulfide-based solid electrolyte Li is prepared in the same manner as in Example 1. 5.45 PS 4.72 Cl 1.70 ...was obtained. The mixing ratio of the raw materials was set to be in excess of sulfur so that a gas atmosphere containing sulfur elements was obtained during heating and melting. As in Example 1, the average particle size of the powder obtained after grinding was 4 μm.
[0159] [Example 4]
[0160] Except for changing the mixing ratio of the raw materials, the sulfide-based solid electrolyte Li is prepared in the same manner as in Example 2. 5.47 PS 4.79 Cl 1.72 ...was obtained. As with Example 2, after grinding, the average particle size of the obtained powder was 4㎛.
[0161] [Example 5]
[0162] Except for changing the mixing ratio of the raw materials, the sulfide-based solid electrolyte Li is prepared in the same manner as in Example 2. 5.52 PS 4.89 Cl 1.01 Br 0.63 ...was obtained. As with Example 2, after grinding, the average particle size of the obtained powder was 5㎛.
[0163] [Example 6]
[0164] The raw materials were prepared in the same manner as in Example 1, except for changing the mixing ratio of the raw materials. They were placed in a carbon container and, while sealed, heated and calcined at a temperature of 550°C for 5 hours to induce a solid-state reaction. Sulfide solid electrolyte Li 5.94 PS 4.94 Cl 1.05 ...was obtained. The heating and cooling rates were set to 5°C / min. The obtained sulfide-based solid electrolyte was subjected to grinding treatment using an agate mortar and pestle. The average particle size of the obtained powder was 6 μm.
[0165] [Example 7]
[0166] Except for changing the mixing ratio of the raw materials, the sulfide-based solid electrolyte Li is prepared in the same manner as in Example 6. 5.40 PS 4.37 Cl 1.63 ...was obtained. As with Example 6, after grinding, the average particle size of the obtained powder was 6㎛.
[0167] [Example 8]
[0168] Except for the addition of sulfur powder before heating and calcination, the sulfide-based solid electrolyte Li6PS5Cl+S was prepared in the same manner as in Example 6. 0.5 I obtained.
[0169] As with Example 6, the average particle size of the powder obtained after grinding was 5 μm.
[0170] [Example 9]
[0171] Raw materials were prepared in the same manner as in Example 1. The raw materials were vacuum-sealed in a carbon-coated quartz tube and heated at 550°C for 5 hours to induce a solid-state reaction. Additionally, the mixture was extracted, pelletized, vacuum-sealed again in a carbon-coated quartz tube, and heat-treated at 650°C for 30 minutes to produce a sulfide-based solid electrolyte Li. 6.11 PS 4.83 Cl 1.07 The obtained sulfide-based solid electrolyte was subjected to grinding treatment using an agate mortar. After grinding, the average particle size of the obtained powder was 5 μm.
[0172] As a result of XRD measurements, the sulfide-based solid electrolytes obtained in Examples 1 to 9 all had an azirodite-type crystal structure. The composition of the crystal structure of each example obtained by compositional analysis is shown in Table 1. In addition, the results of Raman spectroscopy, DSC measurements, and lithium ion conductivity measurements for each sulfide-based solid electrolyte are shown in Table 1.
[0173]
[0174] In the sulfide-based solid electrolytes of Examples 1 to 5, S8 bonding peaks were confirmed in the Raman spectrum, while endothermic peaks attributable to the phase transition or melting of sulfur were not confirmed in the DSC curve; thus, it is believed that the structure consists of S8 molecules uniformly dispersed within an azyrodite-type crystal structure. On the other hand, in the sulfide-based solid electrolytes of Comparative Examples 6, 7, and 9, S8 bonding peaks were not confirmed in the Raman spectrum, so it is believed that they do not contain sulfur in the S8 state. Furthermore, in the sulfide-based solid electrolyte of Example 8, although S8 bonding peaks were confirmed in the Raman spectrum, endothermic peaks of sulfur were also confirmed in the DSC curve. Therefore, it is believed that although the sulfide-based solid electrolyte of Example 8 contains S8 molecules, the S8 molecules are not dispersed within the crystal structure but exist as a group of S8 molecules separated from the crystal structure.
[0175] In Examples 1 to 5, the σ (30kN) / σ (10kN) ratio was smaller compared to Comparative Examples 6 to 9, and the adhesion was good when forming a compact from a powder state. Furthermore, when comparing the Examples and Comparative Examples, which have the same type of Ha (Cl) and a similar content ratio—specifically Examples 1 and 2 versus Examples 6, 8, and 9, or Examples 3 and 4 versus Example 7—the lithium ion conductivity of the compact in the Examples was found to be superior. If this solid electrolyte is processed into a compact in the form of pellets or layers (sheets) and used in lithium-ion secondary batteries, an improvement in the battery characteristics of the lithium-ion secondary battery can be expected.
[0176] Although the present invention has been described in detail with reference to specific embodiments, it is clear to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the invention. This application is based on Japanese patent application filed on November 11, 2020 (Japanese Patent Application No. 2020-188040), the contents of which are incorporated herein by reference.
Claims
Claim 1 A sulfide-based solid electrolyte used in a lithium-ion secondary battery, comprising an azyrodite-type crystal structure containing Li, P, S, and Ha, wherein Ha is at least one selected from the group consisting of F, Cl, Br, and I, and in a Raman spectrum obtained by Raman spectroscopy measurement, 140 to 170 cm⁻¹ -1 , 205 to 235 cm -1 and 460 to 490 cm -1 A sulfide-based solid electrolyte having at least one peak selected from the group consisting of, and not having an endothermic peak within the range of 70 to 160°C in a DSC curve obtained by differential scanning calorimetry (DSC). Claim 2 In claim 1, the composition of the crystal structure is Li a PS b Ha c (5≤a≤7, 4≤b≤6 also 0 <c≤2)로 표시되는, 황화물계 고체 전해질. Claim 3 In claim 1 or 2, in the Raman spectrum, 420 to 440 cm -1 Peak intensity of (I A ) and 460 to 490cm -1 Peak intensity of (I B Ratio of ) B / I A Sulfide-based solid electrolyte with a g of 0.005 or higher. Claim 4 A sulfide-based solid electrolyte according to claim 1 or 2, wherein, when the powder is in a powder state with an average particle size of 2 to 10 μm, the ratio σ (30 kN) of the lithium ion conductivity at 25°C when the powder is compacted at a pressure of 30 kN and the ratio σ (10 kN) of the lithium ion conductivity at 25°C when the powder is compacted at a pressure of 10 kN is 1.34 or less. Claim 5 A sulfide-based solid electrolyte according to claim 1 or 2, having an elastic modulus of 5 to 40 GPa. Claim 6 A solid electrolyte layer comprising a sulfide-based solid electrolyte as described in claim 1 or 2. Claim 7 A lithium-ion secondary battery comprising a sulfide-based solid electrolyte as described in claim 1 or 2.
Citation Information
Patent Citations
Method for producing sulfide solid electrolyte material
KR101739218B1
Solid electrolyte
KR1020140096273A
A sulfide-based solid electrolyte for all-solid battery having a crystal structure of argyrodite derived from single substance and preparing method thereof
KR1020190074484A
All solid state secondary battery
KR1020190100078A
Production method for LGPS-based solid electrolyte
KR1020190127851A