Manufacturing method of multilayer glass substrate for semiconductors and Multilayer glass substrate for semiconductors

The method addresses adhesion and bonding issues in multilayer glass substrates by using a trench-based structure with brazing and sintering, achieving efficient, cost-effective, and reliable semiconductor packaging.

KR103043841B1Active Publication Date: 2026-11-06AMOSENSE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020240106490
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2026-11-06
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Existing methods for manufacturing multilayer glass substrates for semiconductors face challenges such as poor adhesion of electrodes, complex processes, high costs, and interlayer bonding issues due to differences in thermal expansion coefficients, which affect the reliability and efficiency of semiconductor packaging.

Method used

A method involving the use of a glass core with trenches, a brazing adhesive layer, and a conductive paste to form a preliminary electrode, followed by a single sintering step to create robust interlayer bonding and solidified electrodes, using materials like Al-Si or Mg-Zn alloys and glass frit pastes to achieve strong bonding and reduce process complexity.

Benefits of technology

This method significantly reduces process time and costs while enhancing electrode adhesion and interlayer bonding reliability, forming high-density electrodes with improved thermal expansion matching, resulting in a highly reliable multilayer glass substrate for semiconductors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024086750905-PAT00001_ABST
    Figure 112024086750905-PAT00001_ABST
Patent Text Reader

Abstract

A method for manufacturing a multilayer glass substrate for semiconductors and a multilayer glass substrate for semiconductors are disclosed. The disclosed method for manufacturing a multilayer glass substrate for semiconductors is characterized by comprising: a preparation step of preparing a glass core having a trench formed in the thickness direction; a brazing adhesive layer forming step of forming a brazing adhesive layer on a surface partitioning the trench; a preliminary electrode forming step of forming a preliminary electrode in the trench where the brazing adhesive layer is formed using a conductive paste; a glass bonding layer forming step of forming a glass bonding layer by printing a glass bonding material on the surface of the glass core where the preliminary electrode is exposed, excluding a portion of the area; a substrate stacking step of placing another glass core on the glass bonding layer; and a sintering step of performing heat treatment at a specific temperature to perform brazing bonding between the surface partitioning the trench and the preliminary electrode, main curing of the preliminary electrode, and sealing bonding between two stacked glass cores.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a glass substrate, and in particular to a method for manufacturing a multilayer glass substrate for semiconductors in which two or more glass substrates are laminated and bonded, and to a multilayer glass substrate for semiconductors. Background Technology

[0002] In the manufacturing of electronic components, the process of implementing circuits on a semiconductor wafer is called the Front-End (FE) process. The process of assembling the wafer into a state suitable for use in actual products is called the Back-End (BE) process. This Back-End (BE) process includes the Multi-Chip Package (MQP) process, which involves assembling multiple semiconductors produced in wafer form into a bundle advantageous for device integration.

[0003] Semiconductor technology is evolving into various forms, such as micro- and nano-scale linewidths, more than ten million cells, high-speed operation, and high heat dissipation; however, the technology to perfectly package these technologies has not been adequately supported. Consequently, the electrical performance of semiconductors is sometimes determined by packaging technology and the resulting electrical connections rather than by the performance of the semiconductor technology itself.

[0004] Ceramic or resin is generally used as the material for packaging substrates. However, ceramic substrates are difficult to mount high-performance, high-frequency semiconductor devices due to their high resistance or dielectric constant. While resin substrates offer the advantage of being relatively easy to mount high-performance, high-frequency semiconductor devices, they have limitations in reducing wiring pitch and, in particular, are restricted for high-performance semiconductor packaging undergoing continuous miniaturization due to their uneven surfaces.

[0005] Although a method using smooth-surfaced silicon as an alternative packaging substrate has been developed, this approach has the disadvantages of high costs and difficulty in large-area manufacturing. In particular, silicon packaging substrates have the disadvantage of a high Coefficient of Thermal Expansion (CTE), making them unsuitable for use in die packaging where micro-sized bumps are formed at high density, such as in High Bandwidth Memory (HBM).

[0006] Glass substrates are a technology that has recently been gaining attention as a potential replacement for silicon substrates. Glass substrates are more cost-effective than silicon substrates and offer the advantage of enabling the production of a large number of chips due to the ability to design and manufacture them over larger areas. Furthermore, the inherent properties of glass result in a very smooth and flat surface that allows for detailed circuit design, making it advantageous for implementing high-performance, high-density circuits.

[0007] However, when forming electrodes (or electrical wiring) on ​​a glass substrate using a conductive paste that functions as an electrical connection medium, issues regarding adhesion reliability and yield are continuously being raised. This is because the adhesion to the conductive paste is poor due to the smooth surface characteristics of the glass substrate, causing the electrical wiring solidified after sintering to easily peel off from the glass substrate.

[0008] Moreover, when manufacturing in the form of a multilayer glass substrate that is advantageous for packaging, the process is complex and the process cost increases proportionally to the complexity of the process, as the printing and sintering must be repeated multiple times, such as printing a conductive paste onto the glass substrate and sintering it to form electrical wiring on the glass substrate, printing a bonding agent onto the organic substrate with the electrical wiring formed thereon and sintering it once again to bond the glass substrate.

[0009] In particular, glass substrates have the disadvantage that interlayer bonding is difficult when manufactured in the form of multilayer glass substrates using stacked layers due to their material properties. Furthermore, when general bonding materials are used for interlayer bonding of glass substrates, bonding reliability issues arise, such as interlayer separation occurring due to the difference in the coefficient of thermal expansion between the bonding material and the glass.

[0010] The matters described in the background technology above are intended to aid in understanding the background of the invention and may include matters that are not disclosed prior art. Prior art literature

[0011] Korean Registered Patent No. 10-1261468 (Publication Date: May 10, 2013) Korean Registered Patent No. 10-0523940 (Publication Date: October 26, 2005) The problem to be solved

[0012] The technical problem that the present invention aims to solve is to provide a method for manufacturing a multilayer glass substrate for semiconductors and a multilayer glass substrate for semiconductors that can improve the adhesion of electrodes (or electrical wiring) to a glass substrate and thereby improve the electrode peel-off problem.

[0013] Another technical problem that the present invention aims to solve is to provide a method for manufacturing a multilayer glass substrate for semiconductors and a multilayer glass substrate for semiconductors that can shorten the process and reduce process costs by simultaneously realizing the formation of a solidified electrode through a single sintering step at the end of the process, a robust bonding between the solidified electrode and the glass substrate, and a robust interlayer bonding between stacked glass substrates.

[0014] Another technical problem that the present invention aims to solve is to provide a method for manufacturing a multilayer glass substrate for semiconductors and a multilayer glass substrate for semiconductors that can increase interlayer bonding strength between glass substrates when manufacturing the glass substrates into a multilayer glass substrate form advantageous for packaging. means of solving the problem

[0015] According to one aspect of the present invention as a means of solving the problem, a method for manufacturing a multilayer glass substrate for semiconductors is provided, comprising: a preparation step of preparing a glass core having a trench formed in the thickness direction; a brazing adhesive layer forming step of forming a brazing adhesive layer on a surface partitioning the trench; a preliminary electrode forming step of forming a preliminary electrode in the trench where the brazing adhesive layer is formed using a conductive paste; a glass bonding layer forming step of forming a glass bonding layer by printing a glass bonding material on the surface of the glass core excluding a portion of the area; a substrate stacking step of placing another glass core on the glass bonding layer; and a sintering step of brazing bonding between the surface partitioning the trench and the preliminary electrode by heat treatment at a specific temperature, main curing of the preliminary electrode, and sealing bonding between two stacked glass cores.

[0016] In the preparation step of the method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the glass core may be oxide-strengthened glass having a thickness of 20 to 30 μm and having high strength, corrosion resistance, transparency, and hardness at room temperature.

[0017] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the glass core may be borosilicate glass or aluminum silicate glass.

[0018] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the step of forming a brazing adhesive layer may include the step of forming a cover layer having pattern holes formed in a shape corresponding to the trench on the glass core, the step of depositing brazing metal particles onto the surface of the trench exposed through the pattern holes by spraying them at high pressure toward the cover layer in a vacuum atmosphere, and the step of removing the cover layer.

[0019] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the step of forming the cover layer may include the step of forming a photosensitive layer on the glass core, the step of placing a mask that covers the remaining portion excluding the trench on the photosensitive layer and then exposing it, and the step of developing the exposed portion to form a cover layer having a pattern hole corresponding to the trench.

[0020] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the step of forming a preliminary electrode may include the step of filling a trench in which a brazing adhesive layer is formed with a conductive paste, and the step of drying the conductive paste to form a pre-cured preliminary electrode.

[0021] In the step of filling the conductive paste in a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, a screen mask having an open pattern corresponding to the trench is placed on the upper surface of a glass core, and after applying the conductive paste onto the screen mask, the conductive paste can be filled into the trench by passing the conductive paste through the open pattern portion of the screen mask using a squeegee that moves from one side to the other.

[0022] In the step of forming the pre-cured pre-electrode in a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the conductive paste can be pre-cured by drying at a temperature of 80°C or higher and 120°C or lower.

[0023] As a preferred embodiment, the material of the brazing adhesive layer may be an Al-Si alloy having a silicon (Si) content of 12.5 to 12.6 weight% and the remainder being aluminum (Al), and the conductive paste may be an Ag paste with silver (Ag) as the main base. In addition, the glass bonding material may be a glass frit paste containing a glass frit having a melting point higher than the melting point of the Al-Si alloy and lower than the softening point of the glass core.

[0024] In this case, during the sintering step, it is preferable to sinter at a temperature between the melting point of the glass frit and the softening point of the glass core so that the brazing bonding of the pre-electrode, the main curing of the pre-electrode, and the sealing bonding between the two stacked glass cores are achieved at once.

[0025] In a preferred embodiment, the sintering temperature in the sintering step may be between 600℃ and 630℃.

[0026] As another preferred embodiment, the material of the brazing adhesive layer may be a Mg-Zn alloy having a zinc (Zn) content of 5 to 6 weight% and the remainder being magnesium (Mg), and the conductive paste may be an Ag paste with silver (Ag) as the main base. The glass bonding material may be a high-temperature epoxy adhesive or a high-temperature silicone adhesive that maintains adhesive performance at a temperature higher than the melting point of the Mg-Zn alloy.

[0027] In this case, during the sintering step, it is preferable to sinter at a temperature higher than the melting point of the Mg-Zn alloy so that the brazing bonding of the pre-electrode, the main hardening of the pre-electrode, and the sealing bonding between the two stacked glass cores are achieved at once.

[0028] In another preferred embodiment, the sintering temperature in the sintering step may be between 350℃ and 370℃.

[0029] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, the conductive paste may have a composition comprising 70 to 90 weight% silver (Ag) powder, 5 to 10 weight% binder, 4 to 15 weight% organic solvent, and 1 to 5 weight% additive. In this case, the organic solvent may be selected from the group consisting of butyl acetate, terpineol, turpentine oil, butyl carbitol, isopropyl alcohol, or a combination thereof, and the binder may be an acrylic binder or a nitrocellulose binder. The additive may be selected from the group consisting of glycerin, polyethylene glycol (PEG), glass powder, or a combination thereof.

[0030] In a method for manufacturing a multilayer glass substrate for semiconductors according to one aspect of the present invention, in the step of forming the glass bonding layer, the glass bonding layer can be formed by printing the glass bonding material with a uniform thickness on the surface of the glass core, excluding some areas, using screen printing, and then pre-sintering.

[0031] According to another aspect of the present invention as a means of solving the problem, a multilayer glass substrate for a semiconductor is provided, comprising two or more glass cores arranged in a stacked configuration, a trench formed in the thickness direction in the glass cores, a brazing adhesive layer formed on a surface partitioning the trench, an electrode bonded to the brazing adhesive layer within the trench, and a glass bonding layer mediating a sealing bond between the glass cores between the two glass cores.

[0032] In a multilayer glass substrate for semiconductors according to another aspect of the present invention, the glass core may be borosilicate glass or aluminum silicate glass having a thickness of 20 to 30 μm.

[0033] In a multilayer glass substrate for semiconductors according to another aspect of the present invention, the brazing adhesive layer may be formed by vacuum deposition in which metal particles for brazing are sprayed at high pressure in a vacuum atmosphere. The electrode may be formed by filling a conductive paste containing conductive particles into the trench in which the brazing adhesive layer is formed, and then sintering.

[0034] As a preferred embodiment, in a multilayer glass substrate for semiconductors according to another aspect of the present invention, the material of the brazing adhesive layer may be an Al-Si alloy having a silicon (Si) content of 12.5 to 12.6 weight% and the remainder being aluminum (Al), and the conductive paste may be an Ag paste with silver (Ag) as the main base. The glass bonding layer may be formed by pre-sintering after printing a glass frit paste containing glass frit, which has a melting point higher than the melting point of the Al-Si alloy and a softening point lower than that of the glass core, onto the surface of a glass core with exposed electrodes, excluding a portion of the area.

[0035] As another preferred embodiment, in a multilayer glass substrate for semiconductors according to another aspect of the present invention, the material of the brazing adhesive layer may be a Mg-Zn alloy having a zinc (Zn) content of 5 to 6 weight% and the remainder being magnesium (Mg). In this case, the glass bonding layer may be formed by printing a high-temperature epoxy adhesive or a high-temperature silicone adhesive, which maintains adhesive performance at a temperature higher than the melting point of the Mg-Zn alloy, onto the surface of a glass core with exposed electrodes, excluding a portion of the area, and then drying it.

[0036] In a multilayer glass substrate for semiconductors according to another aspect of the present invention, the conductive paste may have a composition comprising 70 to 90 weight% silver (Ag) powder, 5 to 10 weight% binder, 4 to 15 weight% organic solvent, and 1 to 5 weight% additive. In this case, the organic solvent may be selected from the group consisting of butyl acetate, terpineol, turpentine oil, butyl carbitol, isopropyl alcohol, or a combination thereof, and the binder may be an acrylic binder or a nitrocellulose binder. The additive may be selected from the group consisting of glycerin, polyethylene glycol (PEG), glass powder, or a combination thereof.

[0037] In a multilayer glass substrate for semiconductors according to another aspect of the present invention, the electrode may preferably be composed of a signal electrode for transmitting a signal or information, a power electrode for supplying power isolated from the signal electrode, and a conductive electrode formed for each glass core for electrical connection between mutually matching electrodes of two adjacent glass cores.

[0038] As a preferred example, the signal electrode and power electrode can be formed on each glass core.

[0039] As another preferred example, a signal electrode is formed on one glass core and a power electrode is formed on another glass core, and the glass core with the signal electrode formed and the glass core with the power electrode formed can be alternately stacked. Effects of the invention

[0040] According to the present invention, since the method simultaneously achieves the formation of a solidified electrode, brazing bonding between the solidified electrode and a glass substrate (glass core), and robust interlayer bonding between glass substrates through a single sintering step performed at the final stage of the process, the process can be significantly shortened and process costs reduced in the process of manufacturing a semiconductor glass substrate in the form of a multilayer glass substrate advantageous for packaging.

[0041] In addition, since the method involves forming a brazing adhesive layer in the trench by deposition, filling it with conductive paste, and then forming a solidified electrode through a final firing process, a high-density electrode can be formed in which the conductive particles are strongly fused together, and the adhesion of the electrode can be greatly increased as the metal particles of the brazing adhesive layer and the conductive particles forming the electrode react with each other to form a strong bond due to the heat applied during the firing process.

[0042] In addition, by forming the electrode with a trench electrode structure in which at least three sides are in contact with the glass substrate, the adhesion of the electrode is further increased, thereby effectively improving the electrode peel-off that occurs in conventional glass substrates, and accordingly, a highly reliable multilayer glass substrate for semiconductors with uniform and strong electrode bonding properties can be provided. Furthermore, when silver is used as the electrode material, there is an advantage that firing can be performed in an atmospheric environment.

[0043] In addition, in the case of an embodiment in which bonding between glass substrates is implemented using a glass material with a melting point lower than that of the glass core, the coefficient of thermal expansion (CTE) of the glass core and the glass bonding layer can be matched, thereby resolving the problem of interlayer separation between glass substrates after bonding due to the difference in the coefficient of thermal expansion, and as a result, a highly reliable multilayer glass substrate with improved bonding reliability between the glass core (glass substrate) can be provided. Brief explanation of the drawing

[0044] FIG. 1 is a flowchart illustrating a method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment of the present invention. FIG. 2 is a schematic process diagram illustrating the manufacturing process of a multilayer glass substrate for semiconductors according to an embodiment of the present invention. FIG. 3 is a schematic process diagram illustrating the process of forming a bonded metal layer in a trench in a method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment of the present invention. FIG. 4 is a schematic diagram illustrating the conductive paste filling step in a method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment of the present invention. FIG. 5 is a cross-sectional view of a multilayer glass substrate for semiconductors manufactured by a method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment of the present invention. FIG. 6 is an enlarged view of the main part of a multilayer glass substrate for semiconductors shown in FIG. 4, and is an enlarged view of the main part of the present invention showing part 'A' of FIG. 5. FIG. 7 is a drawing showing another preferred embodiment of a multilayer glass substrate for semiconductors. Specific details for implementing the invention

[0045] Hereinafter, preferred embodiments of the present invention will be described in detail.

[0046] In describing the embodiments of the present invention, identical or similar components are assigned the same reference numerals, and redundant descriptions thereof are omitted. Furthermore, detailed descriptions of related prior art are omitted if it is determined that such detailed descriptions could obscure the essence of the embodiments disclosed in this specification.

[0047] In addition, the attached drawings are intended only to facilitate understanding of the embodiments disclosed in this specification, and the technical concept disclosed in this specification is not limited by the attached drawings, and it should be noted that they include all modifications, equivalents, and substitutions that fall within the concept and technical scope of the present invention.

[0048] Furthermore, when it is mentioned that a component is "connected" or "joined" to another component, it should be understood that while it may be directly connected or joined to that other component, there may also be other components in between.

[0049] On the other hand, when it is stated that one component is "directly connected" or "directly coupled" to another component, it should be understood that there are no other components in between.

[0050] Furthermore, terms such as "comprising," "having," and "having" used in describing embodiments of the present invention are intended to specify the existence of features, numbers, steps, actions, components, parts, or combinations thereof of the invention, and should be understood as not excluding in advance the existence or addition of one or more other features, numbers, steps, actions, components, parts, or combinations thereof.

[0051] The drawings are intended solely to facilitate an understanding of the concept of the present invention and should not be interpreted as limiting the scope of the invention. Furthermore, it is noted that relative thicknesses, lengths, or sizes in the drawings may be exaggerated for convenience and clarity of explanation.

[0052] FIG. 1 is a flowchart for explaining a method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment of the present invention, and FIG. 2 is a schematic process diagram schematically illustrating the manufacturing process of a multilayer glass substrate for semiconductors according to an embodiment of the present invention.

[0053] FIG. 1 is a flowchart for explaining a method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment of the present invention, and FIG. 2 is a schematic process diagram schematically illustrating the manufacturing process of a multilayer glass substrate for semiconductors according to an embodiment of the present invention.

[0054] Referring to FIGS. 1 and 2, a method for manufacturing a multilayer glass substrate for semiconductor according to an embodiment includes a preparation step (S100) of preparing a glass core (10) in which a trench (20) is formed in the thickness direction, a brazing adhesive layer forming step (S200) of forming a brazing adhesive layer (25) on a surface that partitions the trench (20), and a preliminary electrode forming step (S300) of forming a preliminary electrode (32) by filling a conductive paste into the trench (20) in which the brazing adhesive layer (25) is formed and drying it.

[0055] A method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment also includes a glass bonding layer forming step (S400) of forming a glass bonding layer (40) by printing a glass bonding material on the surface of a glass core (10), a substrate stacking step (S500) of placing another glass core (10b) on the glass bonding layer (40), and a brazing bonding step (S600) for forming a solidified electrode by main curing of the preliminary electrode (32) and sealing bonding between two stacked glass cores (10a, 10b).

[0056] In the method for manufacturing a semiconductor glass substrate according to the embodiment, the glass core that serves as the main substrate, i.e., the glass core (10) prepared in the preparation step (S100), may be oxide-strengthened glass. In the method for manufacturing a semiconductor glass substrate according to the embodiment, the glass core (10) that serves as the main substrate may be a strengthened glass having a thickness of 20 to 30 μm, high strength and corrosion resistance at room temperature, and a main component of oxide.

[0057] As a preferred example, the glass core (10), which serves as the main substrate in the semiconductor glass substrate manufacturing method according to the embodiment, may be a borosilicate glass that is a glass based on boric acid instead of silicic acid, contains at least 5% boric acid, has chemical acid resistance and weather resistance with a low coefficient of expansion, and has excellent thermal shock resistance.

[0058] As another preferred example, the glass core (10), which serves as the main substrate in the semiconductor glass substrate manufacturing method according to the embodiment, may be aluminum silicate glass composed of alumina and boron oxide, which has characteristics similar to borosilicate glass, while having superior heat resistance and high chemical resistance compared to borosilicate glass.

[0059] In the preparation step (S100), a glass core (10) having a trench (20) formed in the thickness direction is prepared. The trench (20) can be formed in the thickness direction on the glass core (10) through etching. For example, it can be formed by forming a predetermined pattern with a photosensitive material on the glass core (10) through a known photolithography process of drawing a semiconductor circuit on a wafer, and performing an etching process using the photosensitive material with the formed pattern as a mask.

[0060] For reference, the term ‘trench (20)’ used in describing the present invention refers to a fine hole (Via, 20b) or groove (20a) formed in the thickness direction in the glass core (10) through an etching process.

[0061] Dry etching using plasma or a laser, or wet etching using an etching solution, may be applied for etching to form the trench (20). In the case of wet etching, HF or NaOH may be used as the etching solution. HF has the advantage of enabling room temperature etching and fast etching speed, while NaOH has the advantage of enabling precise etching, although the etching conditions are stricter compared to HF.

[0062] According to the embodiment, a LIDE (Laser induced Deep Etching) method may be applied in which the trench (20) is completed by pre-processing with a laser and then post-processing through chemical etching. The LIDE method is a technique that induces a selective chemical phase change of glass through a laser and then forms a trench by selectively etching only the parts deformed by the laser through a chemical etching process.

[0063] Among the trenches (20, fine holes and grooves) formed in the glass core (10) through etching, the groove (20a) can be formed with a specific depth and width. Considering that the thickness of the glass core (10) is 20 to 30 μm, the depth (d) of the groove (20a) among the trenches (fine holes and grooves) formed in the glass core (10) during the etching step (S200) is preferably 0.8 to 1.2 μm, and the width (width of the groove, w) is preferably 1.8 to 2.2 μm.

[0064] The brazing adhesive layer formation step (S200) is a step of forming a brazing adhesive layer (25) with a uniform thickness on the wall surface or the wall surface and bottom surface of the trench (20) formed in the glass core (10). In the brazing adhesive layer formation step (S200), the brazing adhesive layer (25) can be formed by depositing metal particles capable of forming a strong bond with glass on the wall surface or the wall surface and bottom surface that partition the trench (20) with a uniform thickness.

[0065] In the brazing adhesive layer formation step (S200), the brazing adhesive layer (25) may be composed of a metal that can be well attached to glass and has good matching properties with the main substrate (conductive particle) of the preliminary electrode (32) described later. For example, if the main substrate constituting the preliminary electrode (32) is silver (Ag), the material of the brazing adhesive layer (25) may be an Al-Si alloy with aluminum (Al) and silicon (Si) as main components, or a Mg-Zn alloy with magnesium (Mg) and zinc (Zn) as main components.

[0066] When using an Al-Si alloy as the material for the brazing adhesive layer (25), an Al-Si alloy having a silicon (Si) content of 12.5 to 12.6 weight% and the remainder being aluminum (Al) may be used. And when using an Mg-Zn alloy as the material for the brazing adhesive layer (25), it is preferable to use a Mg-Zn alloy having a zinc (Zn) content of 5 to 6 weight% and the remainder being magnesium (Mg).

[0067] Al-Si alloys are characterized by their lightness and high ductility and malleability. Additionally, Al-Si alloys possess low melting points and shrinkage rates, strong corrosion resistance, and good fluidity in the molten state. Consequently, they easily melt at relatively low temperatures, allowing them to form a fusion brazing interface that mediates a strong bond between glass and metal. Therefore, they are suitable as brazing materials for glass substrates.

[0068] Mg-Zn alloys offer high strength while remaining lightweight due to their low specific gravity. Mg-Zn alloys also have excellent corrosion resistance and, like Al-Si alloys, have the advantage of good fluidity in the molten state. In particular, with a melting point of approximately 340°C, they can reach a molten state at a lower temperature than Al-Si alloys, forming a fusion brazing interface that mediates a strong bond between glass and metal.

[0069] In the brazing adhesive layer formation step (S200), the brazing adhesive layer (25) can be formed with a uniform thickness (t1) on the surface partitioning the trench (20) by sputtering, in which particles of the aforementioned alloy (Al-Si alloy or Mg-Zn alloy) are deposited by spraying them under high pressure in a vacuum atmosphere. As a preferred example, the brazing adhesive layer (25) formed in the trench (20) can be formed as a single layer structure with a thickness of 50 nm.

[0070] Let us examine the process of forming a brazing adhesive layer in the trench during the brazing adhesive layer formation step in more detail with reference to Fig. 3.

[0071] FIG. 3 is a schematic diagram of a process illustrating the process of forming a brazing adhesive layer in a trench in a method for manufacturing a multilayer glass substrate for semiconductors according to an embodiment of the present invention.

[0072] Referring to FIG. 3, the brazing adhesive layer forming step (S200) may include the step (S202) of forming a cover layer (70) having a pattern hole (72) formed in a shape corresponding to the trench (20) on a glass core (10), the step (S204) of depositing brazing metal particles onto the surface of the trench (20) exposed through the pattern hole (72) by spraying them at high pressure toward the cover layer (70) in a vacuum atmosphere, and the step (S206) of removing the cover layer (70).

[0073] The cover layer formation step (S202) includes a step (S202-1) of forming a photosensitive layer (50) with a uniform thickness by applying a photosensitive agent to the glass core (10). Additionally, it includes a step (S202-2) of placing a mask (60) that covers the remaining parts excluding the trench (20) on the photosensitive layer (50) and then exposing it, and a step (S202-3) of finally forming a cover layer (70) having a pattern hole (72) by developing the exposed parts.

[0074] In the cover layer removal step (S206), for example, a process can be performed to remove the cover layer (70) and unnecessary deposits on the cover layer (70) all at once through dry ashing using plasma. In some cases, the cover layer (70) and unnecessary deposits may be removed through a Chemical Mechanical Polishing (CMP) process that flattens the surface of the glass core (10) while removing the cover layer (70) and unnecessary deposits.

[0075] The preliminary electrode formation step (S300) is a step of forming a preliminary electrode (32) by filling a trench (20) in which a brazing adhesive layer (25) is formed with a uniform thickness with a conductive paste. The preliminary electrode formation step (S400) includes a step (S302) of filling a trench (20) in which a brazing adhesive layer (25) is formed with a conductive paste, and a step (S304) of forming a pre-cured preliminary electrode (32) by drying the conductive paste at a temperature of 80°C or higher and 120°C or lower.

[0076] In the paste filling step (S302), as shown in FIG. 4, a screen mask (M) having an open pattern (P) corresponding to the trench (20) is placed on the upper surface of the glass core (10), and a conductive paste is applied over the screen mask (M). Then, the conductive paste can be filled through a type of screen printing method in which the conductive paste is passed through the open pattern (P) using a squeegee (S) that moves from one side to the other (see arrow direction).

[0077] In the example, the conductive particles, which are the main substrate constituting the conductive paste, may be silver (Ag). Silver (Ag) has an electrical conductivity of approximately 63.01 x 10⁻⁶. 6It has the highest S / m (Siemens / meter) among all metals. In particular, using silver (Ag) as the main substrate for conductive paste allows for burning in an atmospheric environment, which can reduce process size and process costs. This is due to the property of silver being less sensitive to oxidation compared to other metals.

[0078] In the example, the conductive paste may include silver powder, a binder that helps bond the silver powders together and adhere to a substrate, an organic solvent for uniform dispersion of the silver powder, and additives for controlling the sintering temperature, paste viscosity, and preventing oxidation. In the example, the preferred composition of the conductive paste may be 70 to 90 wt% silver powder, 5 to 10 wt% binder, 4 to 15 wt% organic solvent, and 1 to 5 wt% additive.

[0079] In the example, the organic solvent may be selected from the group consisting of butyl acetate, terpineol, turpentine oil, butyl carbitol, isopropyl alcohol, or a combination thereof, and the binder may be an acrylic binder or a nitrocellulose binder. The additive may be selected from the group consisting of glycerin, polyethylene glycol (PEG), glass powder, or a combination thereof.

[0080] The glass bonding layer formation step (S400) is a step of forming a glass bonding layer (40) by printing a glass bonding material on the surface of a glass core (10). In the glass bonding layer formation step (S400), the glass bonding layer (40) can be formed by printing a glass bonding material on the surface of a glass core (10) with a uniform thickness and then performing pre-sintering. Here, pre-sintering can be performed under temperature and pressure conditions that can prevent deterioration of the glass core while applying sufficient heat to the glass bonding material.

[0081] In the glass bonding layer formation step (S400), screen printing may be used to form a glass bonding layer (40) on the surface of the glass core (10) where the preliminary electrode (10) is exposed. In this case, it is preferable to print the glass bonding material only on the area excluding the portion where the preliminary electrode is exposed, so that the preliminary electrode (32b) formed in the fine hole (Via, 20b) portion of the trench is exposed to the outside and forms an electrical connection with the preliminary electrode (32b) of another glass core (10).

[0082] The glass bonding material forming the glass bonding layer (40) may vary depending on the material of the aforementioned brazing adhesive layer (25). As a preferred example, if the brazing material is the aforementioned Al-Si alloy, glass frit paste may be used as the glass bonding material. As another preferred example, if the brazing material is an Mg-Zn alloy, a high-temperature epoxy adhesive or a high-temperature silicone adhesive that maintains adhesive performance even at a temperature higher than the melting point of the Mg-Zn alloy may be used as the glass bonding material.

[0083] In an embodiment in which glass frit paste is used as a glass bonding material, the glass frit paste may be composed of glass frit as the main base material, which has a melting point higher than that of an Al-Si alloy applied as a brazing material and is approximately 100°C lower than that of a glass core, and may include an organic solvent and a binder.

[0084] In this case, the glass frit may be, for example, a mixture of silica sand, aluminum oxide (Al2O3), and calcium carbonate (CaCO3) in specific proportions, melted at a high temperature, rapidly cooled, and then ground into a fine powder. The organic solvent may consist of, for example, butyl acetate or terpineol, or a combination thereof, and an acrylic binder or a nitrocellulose binder may be used as the binder.

[0085] In the substrate stacking step (S500), a process is performed to place another glass core (10b) on the glass bonding layer (40) of the glass core (10a). More specifically, in the substrate stacking step (S500), two glass cores (10a, 10b) are arranged in a stacked structure so as to face each other with the glass bonding layer (40) in between. In the substrate stacking step (S500), accurate and precise stacking can be achieved by using a dedicated stacking device including a sensor, an alignment unit, and a jig.

[0086] The sintering step (S600) is a step that implements brazing bonding between the surface partitioning the trench (20) and the pre-electrode (32), solidified electrode formation following the main curing of the pre-electrode (32), and sealing bonding between two stacked glass cores (10a, 10b) through a single sintering step. In the sintering step (S600), the sintering temperature may vary depending on the brazing material mediating the physical bonding between the surface partitioning the trench (20) and the pre-electrode (32), the main substrate of the conductive paste to form the electrode, and the glass bonding material forming the glass bonding layer (40).

[0087] In one embodiment, when a glass frit paste is used as a glass bonding material, wherein the brazing material is an Al-Si alloy with a silicon (Si) content of 12.5 to 12.6%, the main substrate of the conductive paste is silver (Ag), and the glass frit paste is used, wherein the glass frit paste has a melting point higher than the melting point of the Al-Si alloy and is about 100°C lower than the softening point of the glass core, sintering can be performed at a temperature between the melting point of the glass frit and the softening point of the glass core.

[0088] Preferably, considering that the melting point of an Al-Si alloy with a Si content of 12.5% ​​is 577°C and the softening point of borosilicate strengthened glass is about 820°C, in the case of one embodiment, when sintering is performed at a temperature between 600°C and 630°C, a strong brazing bond of the pre-electrode by melting the brazing adhesive layer, solidification (main curing) of the pre-electrode by heating, and a sealing bond between two stacked glass cores can be achieved at once.

[0089] As another embodiment, when the brazing material is an Mg-Zn alloy with a zinc (Zn) content of 5 to 6 weight%, the main substrate of the conductive paste is silver (Ag), and a high-temperature epoxy adhesive or high-temperature silicone adhesive that maintains adhesive performance at a temperature higher than the melting point of the Mg-Zn alloy is used as the glass bonding material, the sintering temperature in the sintering step (S600) may be at least higher than the melting point of the Mg-Zn alloy.

[0090] Preferably, considering that the melting point of an Mg-Zn alloy with a Zn content of 6% is about 340°C, in the case of another embodiment, a strong brazing bond of the pre-electrode by melting the brazing adhesive layer, solidification (main curing) of the pre-electrode by heating, and sealing bond between two stacked glass cores can be achieved at once by sintering alone in a temperature range of 350°C to 370°C, which is relatively lower than in one embodiment.

[0091] As mentioned, silver (Ag) is less susceptible to oxidation compared to other conductive metals. Therefore, sintering is possible in an atmospheric environment. However, at high temperatures above 700°C, the surface of silver may oxidize, and at temperatures below 350°C, the fusion between silver particles may be poor and organic solvents or binders may remain. Therefore, when using silver (Ag) paste as a conductive paste to form an electrode, a sintering temperature of 350°C or higher and less than 700°C is suitable.

[0092] A drying process (not shown) may be added to the sintering step (S600). If a drying process is performed additionally after the sintering process, the organic solvent remaining in the conductive paste can be removed more effectively. In the drying process, it is preferable to perform the drying at a temperature and time that allows the organic solvent to be removed by vaporization while also allowing the electrode temperature to be gradually cooled.

[0093] According to the manufacturing method of the above embodiment of the present invention, since the method simultaneously achieves the formation of a solidified electrode, brazing bonding between the solidified electrode and the glass substrate (glass core), and robust interlayer bonding between glass substrates through a single sintering step performed at the final stage of the process, the process can be significantly shortened and process costs can be reduced accordingly when manufacturing a semiconductor glass substrate into a multilayer glass substrate form advantageous for packaging.

[0094] In addition, since the method involves forming a brazing adhesive layer in the trench by deposition, filling it with conductive paste, and then forming a solidified electrode through a final firing process, a high-density electrode can be formed in which the conductive particles are strongly fused together, and the adhesion of the electrode can be greatly increased as the metal particles of the brazing adhesive layer and the conductive particles forming the electrode react with each other to form a strong bond due to the heat applied during the firing process.

[0095] In addition, by forming the electrode with a trench electrode structure in which at least three sides are in contact with the glass substrate, the adhesion of the electrode is further increased, thereby effectively improving the electrode peel-off that occurs in conventional glass substrates, and accordingly, a highly reliable multilayer glass substrate for semiconductors with uniform and strong electrode bonding properties can be provided. Furthermore, when silver is used as the electrode material, there is an advantage that firing can be performed in an atmospheric environment.

[0096] In addition, in the case of an embodiment in which bonding between glass substrates is implemented using a glass material with a melting point lower than that of the glass core, the coefficient of thermal expansion (CTE) of the glass core and the glass bonding layer can be matched, thereby resolving the problem of interlayer separation between glass substrates after bonding due to the difference in the coefficient of thermal expansion, and as a result, a highly reliable multilayer glass substrate with improved bonding reliability between the glass core (glass substrate) can be provided.

[0097] FIG. 5 is a cross-sectional view of a multilayer glass substrate for semiconductors manufactured by the method for manufacturing a multilayer glass substrate for semiconductors described above, and FIG. 6 is an enlarged view of the main part of the present invention showing the enlarged view of part 'A' of FIG. 5.

[0098] Referring to FIGS. 5 and 6, a multilayer glass substrate (1) for semiconductors comprises two or more glass cores (10a, 10b) that are stacked and each have a trench (20), and a glass bonding layer (40) that mediates a sealing bond between the glass cores (10a, 10b) between two adjacent glass cores (10a, 10b). In the trench (20) of each glass core (10a, 10b), a brazing adhesive layer (25) may be formed with a specific thickness on the surface partitioning the trench, and an electrode (30) may be bonded to the brazing adhesive layer (25) within the trench (20).

[0099] The trench (20) may be a groove (20a) or a fine hole (20b) formed in the thickness direction of the glass core (10), and the glass bonding layer (40) mediating a sealing bond between the glass cores between two adjacent glass cores (10a, 10b) may be formed on one of the upper and lower surfaces of the glass core (10) or on both the upper and lower surfaces of the glass core (10).

[0100] The glass core (10) may be a tempered glass having a thickness of 20 to 30 μm, a first surface (12, upper surface in the drawing) that is smooth, and a second surface (14, lower surface in the drawing) parallel to the first surface, and the trench (20) may be formed by forming a predetermined pattern with a photosensitive material on the glass core (10) through a photolithography process, and performing an etching process using the photosensitive material with the formed pattern as a mask.

[0101] For reference, the drawing (Fig. 5) illustrates an example configuration in which a groove-shaped trench (20a) is formed on the first surface (12) side of the glass core (10), but is not limited thereto. Depending on the embodiment, a groove-shaped trench (20a) may be formed on the second surface (14) side of the glass core (10), or a groove-shaped trench (20a) may be formed on both the first surface (12) side and the second surface (14) side.

[0102] The glass core (10) may be tempered glass with a thickness of 20 to 30 μm. In the embodiment, the glass core (10) may be tempered glass having high strength, corrosion resistance, transparency, and hardness at room temperature, with the main component being an oxide. As a preferred example, the glass core (10) may be borosilicate glass. Depending on the embodiment, it may be aluminum silicate glass.

[0103] Borosilicate reinforced glass is a glass based on boric acid instead of silica, containing at least 5% boric acid. It has a low coefficient of expansion, possesses chemical acid resistance and weather resistance, and has excellent thermal shock resistance, making it suitable as a semiconductor glass substrate. Aluminum silicate reinforced glass is composed of alumina and boron oxide and has similar properties to borosilicate glass, but possesses superior heat resistance and high chemical resistance compared to borosilicate glass, making it suitable as a semiconductor glass substrate.

[0104] Among the trenches (fine holes and grooves) formed in the glass core (10), the groove (20a) can be formed with a specific depth and width. Considering that the thickness of the glass core (10) is 20 to 30 μm, the groove (20a) among the trenches (fine holes and grooves) formed in the glass core (10) can be formed with a depth (d) of 0.8 to 1.2 μm and a width (width of the groove, w) of 1.8 to 2.2 μm.

[0105] The brazing adhesive layer (25) mediates a strong bond between the electrode (30) and the glass core (10). The brazing adhesive layer (25) can be formed with a uniform thickness on all sides partitioning the trench (20). For example, if the trench (20) is formed in the shape of a groove with a square cross-section (see shape 20a in FIG. 5), the brazing adhesive layer (25) can be formed with a uniform thickness on all sides partitioning the trench (20), namely the vertical walls facing each other and the flat bottom surface connecting the bottoms of these walls.

[0106] The brazing adhesive layer (25) can be formed by depositing metal particles of a uniform thickness that can form a strong bond with glass on the surface partitioning the trench (20). The brazing adhesive layer (25) can be composed of a metal that can adhere well to glass and has good matching properties with the particles (conductive particles) of the electrode.

[0107] The brazing adhesive layer (25) can be formed with a uniform thickness (t1) on the surface partitioning the trench (20) through a sputtering process in which metal particles for brazing are deposited by spraying them onto the surface of the glass core under high pressure in a vacuum atmosphere. As a preferred example, the brazing adhesive layer (25) formed in the trench (20) can be formed as a single layer structure with a thickness of 50 nm.

[0108] The brazing adhesive layer (25) can be formed, for example, by forming a cover layer (see Figure 3 above) having pattern holes formed in a shape corresponding to the trench (20) on a glass core (10), and then forming the brazing adhesive layer (25) by spraying metal particles at high pressure toward the cover layer to deposit the brazing adhesive layer (25) inside the trench (20) exposed through the pattern holes, and then removing the cover layer on the glass core along with unnecessary deposits by dry ashing or the like through a series of processes.

[0109] The electrode (30) can be formed from a conductive paste filled into the trench (20). The electrode (30) can be formed by filling the trench (20) with the conductive paste and sintering it at a specific temperature. The electrode (30) can be bonded to the brazing adhesive layer (25) within the trench (20) in a rigid bond, except for a surface (exposed to the outside) that is aligned coplanar with the surface of the glass core.

[0110] The conductive paste constituting the electrode (30) contains conductive particles. The conductive particles may be silver (Ag). Silver (Ag) has an electrical conductivity of approximately 63.01 x 10⁻¹⁰. 6 It has the highest S / m (Siemens / meter) among all metals, and in particular, if silver (Ag) is used as the main substrate of the conductive paste, burning treatment in an atmospheric environment is possible, which can reduce process size and process costs.

[0111] The conductive paste may be an Ag paste comprising silver powder as a main substrate, a binder that helps bond the silver powders together and adhere to the substrate, an organic solvent for uniform dispersion of the silver powder, and additives for controlling the sintering temperature, paste viscosity, and preventing oxidation. The preferred composition of the Ag paste may be 70 to 90 wt% silver powder, 5 to 10 wt% binder, 4 to 15 wt% organic solvent, and 1 to 5 wt% additives.

[0112] In this case, the organic solvent may be selected from the group consisting of butyl acetate, terpineol, turpentine oil, butyl carbitol, isopropyl alcohol, or a combination thereof. The binder may be an acrylic binder or a nitrocellulose binder, and the additive may be selected from the group consisting of glycerin, polyethylene glycol (PEG), glass powder, or a combination thereof.

[0113] As a preferred example, the material of the brazing bonding layer (25) may be an Al-Si alloy having a silicon (Si) content of 12.5 to 12.6 weight% and the remainder being aluminum (Al). The glass bonding layer (40) may be formed by pre-sintering after printing a glass frit paste containing a glass frit, which has a melting point higher than the melting point of the Al-Si alloy and is about 100°C lower than the softening point of the glass core, onto the surface of the glass core (10) with the electrode exposed.

[0114] In this case (where the brazing material is an Al-Si alloy with a silicon (Si) content of 12.5 to 12.6 wt%, the electrode material is silver (Ag), and the glass bonding layer is formed of a glass frit with a temperature approximately 100°C lower than the softening point of the glass core), a multilayer glass substrate according to the embodiment can be formed through a single sintering process performed between the melting point of the glass frit and the softening point of the glass core, preferably between the melting point of the glass frit and a temperature that can prevent surface oxidation of silver.

[0115] Here, the glass frit may be, for example, a mixture of silica sand, aluminum oxide (Al2O3), and calcium carbonate (CaCO3) in specific proportions, melted at a high temperature, rapidly cooled, and then ground into a fine powder. The organic solvent may consist of, for example, butyl acetate or terpineol, or a combination thereof, and an acrylic binder or a nitrocellulose binder may be used as the binder.

[0116] As another preferred example, the material of the brazing adhesive layer (25) may be a Mg-Zn alloy having a zinc (Zn) content of 5 to 6 weight percent and the remainder being magnesium (Mg). And the glass bonding layer (40) may be formed by printing a high-temperature epoxy adhesive or a high-temperature silicone adhesive, which maintains adhesive performance at a temperature higher than the melting point of the Mg-Zn alloy, onto the surface of a glass core with exposed electrodes and then drying it.

[0117] In this case (where the brazing material is an Mg-Zn alloy with a zinc (Zn) content of 5 to 6 weight%, the electrode material is silver (Ag), and the glass bonding layer is formed with a high-temperature epoxy adhesive or a high-temperature silicone adhesive that maintains adhesive performance at a temperature higher than the melting point of the Mg-Zn alloy), a multilayer glass substrate according to the embodiment can be formed through a single sintering process performed at a temperature that is at least higher than the melting point of the Mg-Zn alloy and prevents surface oxidation of silver.

[0118] Meanwhile, screen printing may be used to form a glass bonding layer (40) that mediates a strong bond between two glass cores (10a, 10b). In this case, the glass bonding layer (40) may be formed with a predetermined thickness only in the area excluding the part where the electrode is exposed, so that an electrode (30b, conductive electrode) formed in the fine hole (Via, 20b) portion of the trench of the glass core (10a) is exposed to the outside and forms an electrical connection with the corresponding electrode (30b) of the other glass core (10b).

[0119] FIG. 7 is a drawing showing another preferred embodiment of a multilayer glass substrate for semiconductors.

[0120] Referring to FIG. 7, the electrode (30) formed on the multilayer glass substrate (1) for semiconductors can be divided into a signal electrode (30a), a power electrode (30c), and a current-carrying electrode (30b) that are isolated from each other.

[0121] Signals or information can be transmitted between glass cores (10a, 10b) through the signal electrode (30a), and power can be supplied through the power electrode (30c). Additionally, a conductive electrode (30b) can be formed on each glass core (10a, 10b) for electrical connection between mutually matching electrodes of two adjacent glass cores.

[0122] The signal electrode (30a) and the power electrode (30c) can be formed with different widths and depths. For example, as shown in the example of FIG. 7, the power electrode (30c) can be formed to be wider and deeper than the signal electrode (30a).

[0123] As shown in FIG. 7(a), the signal electrode (30a) and the power electrode (30c) can be formed on each glass core (10a, 10b). That is, each glass core (10a, 10b) can be equipped with both the signal electrode (30a) and the power electrode (30c). A configuration in which each glass core (10a, 10b) is equipped with both the signal electrode (30a) and the power electrode (30c) is advantageous for the compactness and high integration of the multilayer glass substrate.

[0124] Alternatively, as illustrated in FIG. 7(b), the signal electrode (30a) and the power electrode (30b) may be formed on different glass cores. That is, the signal electrode (30a) may be formed on one glass core (10a), and the power electrode (30c) may be formed on the other glass core (10b). In this case, the glass core (10a) on which the signal electrode (30a) is formed and the glass core (10b) on which the power electrode (30c) is formed may be alternately stacked.

[0125] Although the configuration of Fig. 7(b) has disadvantages in terms of compactness or integration compared to the configuration of Fig. 7(a) above, the problem of electrical interference between the signal electrode (30a) and the power electrode (30c) being distorted by the signal or information transmitted through the signal electrode (30a) by the high voltage power source when a high voltage power source is applied can be reliably prevented due to more reliable isolation between the signal electrode (30a) and the power electrode (30c).

[0126] In a multilayer glass substrate for semiconductors with the above configuration, electrodes are formed in the form of trench electrodes in which at least three sides are bonded to the glass substrate (glass core), thereby significantly increasing the adhesion of the electrodes to the glass substrate. Consequently, problems of the conventional technology, such as electrode peel-off, can be clearly improved. As a result, a highly reliable product with robust and uniform electrode adhesion quality can be provided.

[0127] The above description is merely an illustrative explanation of the technical concept of the present invention, and those skilled in the art to which the present invention pertains will be able to make various modifications and variations within the scope of the essential characteristics of the present invention.

[0128] Accordingly, the embodiments disclosed in this invention are intended to illustrate, not limit, the technical concept of the invention, and the scope of the technical concept of the invention is not limited by these embodiments. The scope of protection of this invention shall be interpreted by the claims below, and all technical concepts within an equivalent scope shall be interpreted as being included within the scope of rights of this invention. Explanation of the symbols

[0129] 1: Multilayer glass substrate for semiconductors 10: Glass core 20: Trench (groove or fine hole formed in the glass core) 25: Brazing adhesive layer 30: Electrode 30a: Signal electrode 30b: Conductive electrode 30c: Power electrode 32: Preliminary electrode 40: Glass bonding layer 50: Photosensitive layer 60: Mask 70: Cover layer 72: Pattern hole

Claims

Claim 1 A preparation step for preparing a glass core having a trench formed in the thickness direction; a brazing adhesive layer formation step for forming a brazing adhesive layer on a surface partitioning the trench; a preliminary electrode formation step for forming a preliminary electrode in the trench where the brazing adhesive layer is formed using a conductive paste; a glass bonding layer formation step for forming a glass bonding layer by printing a glass bonding material on the surface of the glass core; and a substrate stacking step for placing another glass core on the glass bonding layer. A method for manufacturing a multilayer glass substrate for semiconductors, comprising: a brazing bonding step between a surface partitioning a trench and a pre-electrode by heat treatment at a specific temperature, a main curing step of the pre-electrode, and a sealing bonding step between two stacked glass cores; wherein the material of the brazing adhesive layer is an Al-Si alloy having a silicon (Si) content of 12.5 to 12.6 wt% and the remainder being aluminum (Al); the conductive paste is an Ag paste with silver (Ag) as the main base; and the glass bonding material is a glass frit paste containing glass frit having a melting point higher than the melting point of the Al-Si alloy and lower than the softening point of the glass core. Claim 2 A preparation step for preparing a glass core having a trench formed in the thickness direction; a brazing adhesive layer formation step for forming a brazing adhesive layer on a surface partitioning the trench; a preliminary electrode formation step for forming a preliminary electrode in the trench where the brazing adhesive layer is formed using a conductive paste; a glass bonding layer formation step for forming a glass bonding layer by printing a glass bonding material on the surface of the glass core; and a substrate stacking step for placing another glass core on the glass bonding layer. A method for manufacturing a multilayer glass substrate for semiconductors, comprising: a brazing bonding step between a surface partitioning a trench and a pre-electrode by heat treatment at a specific temperature, a main curing step of the pre-electrode, and a sealing bonding step between two stacked glass cores; wherein the material of the brazing adhesive layer is a Mg-Zn alloy having a zinc (Zn) content of 5 to 6 weight% and the remainder being magnesium (Mg); the conductive paste is an Ag paste with silver (Ag) as the main base; and the glass bonding material is a high-temperature epoxy adhesive or a high-temperature silicone adhesive that maintains adhesive performance at a temperature higher than the melting point of the Mg-Zn alloy. Claim 3 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 1 or 2, wherein, in the preparation step, the glass core is formed with a thickness of 20 to 30 μm. Claim 4 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 3, wherein the glass core is borosilicate glass or aluminum silicate glass. Claim 5 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 1 or 2, wherein the step of forming a brazing adhesive layer comprises: forming a cover layer having pattern holes formed in a shape corresponding to the trench on the glass core; spraying metal particles for brazing at high pressure toward the cover layer in a vacuum atmosphere to deposit them on the surface of the trench exposed through the pattern holes; and removing the cover layer. Claim 6 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 5, wherein the step of forming the cover layer comprises: forming a photosensitive layer on the glass core; placing a mask covering the remaining portion excluding the trench on the photosensitive layer and then exposing it; and developing the exposed portion to form a cover layer having pattern holes corresponding to the trench. Claim 7 A method for manufacturing a multilayer glass substrate for semiconductors, wherein, in claim 1 or 2, the preliminary electrode forming step comprises: filling a trench in which a brazing adhesive layer is formed with a conductive paste; and drying the conductive paste to form a pre-cured preliminary electrode. Claim 8 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 7, wherein in the step of filling the conductive paste, a screen mask having an open pattern corresponding to the trench is placed on the upper surface of a glass core, and after applying a conductive paste over the screen mask, the conductive paste is passed through the open pattern portion of the screen mask using a squeegee that moves from one side to the other to fill the trench. Claim 9 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 7, wherein in the step of forming the pre-cured pre-electrode, the conductive paste is pre-cured by drying treatment at 80°C or higher and 120°C or lower. Claim 10 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 1, wherein in the sintering step, sintering is performed at a temperature between the melting point of the glass frit and the softening point of the glass core, so that brazing bonding of the pre-electrode, main curing of the pre-electrode, and sealing bonding between two stacked glass cores are achieved at once. Claim 11 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 10, wherein the sintering temperature in the sintering step is between 600℃ and 630℃. Claim 12 delete Claim 13 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 2, wherein in the sintering step, sintering is performed at a temperature higher than the melting point of the Mg-Zn alloy, so that brazing of the pre-electrode, main curing of the pre-electrode, and sealing of the two stacked glass cores are achieved at once. Claim 14 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 13, wherein the sintering temperature in the sintering step is between 350℃ and 370℃. Claim 15 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 1 or 2, wherein the conductive paste comprises 70 to 90 weight% silver (Ag) powder, 5 to 10 weight% binder, 4 to 15 weight% organic solvent, and 1 to 5 weight% additive, wherein the organic solvent is selected from the group consisting of butyl acetate, terpineol, turpentine oil, butyl carbitol, isopropyl alcohol, or a combination thereof, the binder is an acrylic binder or a nitrocellulose binder, and the additive is selected from the group consisting of glycerin, polyethylene glycol (PEG), glass powder, or a combination thereof. Claim 16 A method for manufacturing a multilayer glass substrate for semiconductors according to claim 1 or 2, wherein in the step of forming the glass bonding layer, the glass bonding material is printed to a uniform thickness on the surface of the glass core using screen printing, and then pre-sintered to form a glass bonding layer. Claim 17 Two or more glass cores stacked in an array; a trench formed in the thickness direction in the glass cores; a brazing adhesive layer formed on a surface partitioning the trench; and an electrode bonded to the brazing adhesive layer within the trench. A multilayer glass substrate for semiconductors comprising: a glass bonding layer mediating a sealing bond between two glass cores; wherein the electrode is formed by filling a trench in which a brazing adhesive layer is formed with a conductive paste containing conductive particles and then sintering, the material of the brazing adhesive layer is an Al-Si alloy having a silicon (Si) content of 12.5 to 12.6 weight% and the remainder being aluminum (Al), the conductive paste is an Ag paste with silver (Ag) as the main base, and the glass bonding layer is formed by pre-sintering after printing a glass frit paste containing glass frit, which has a melting point higher than the melting point of the Al-Si alloy and a softening point lower than that of the glass core, onto the surface of a glass core with the electrode exposed. Claim 18 A multilayer glass substrate for semiconductors comprising: two or more glass cores stacked in an array; a trench formed in the thickness direction in the glass cores; a brazing adhesive layer formed on a surface partitioning the trench; an electrode bonded to the brazing adhesive layer within the trench; and a glass bonding layer mediating a sealing bond between the two glass cores; wherein the electrode is formed by filling a conductive paste containing conductive particles into the trench where the brazing adhesive layer is formed and then sintering, the material of the brazing adhesive layer is a Mg-Zn alloy having a zinc (Zn) content of 5 to 6 weight% and the remainder being magnesium (Mg), the conductive paste is an Ag paste with silver (Ag) as the main base, and the glass bonding layer is formed by printing a high-temperature epoxy adhesive or a high-temperature silicone adhesive that maintains adhesive performance at a temperature higher than the melting point of the Mg-Zn alloy onto the surface of the glass core where the electrode is exposed, and then drying. Claim 19 A multilayer glass substrate for semiconductors according to claim 17 or 18, wherein the glass core is borosilicate glass or aluminum silicate glass having a thickness of 20 to 30 μm. Claim 20 A multilayer glass substrate for semiconductors according to claim 17 or 18, wherein the brazing adhesive layer is formed through vacuum deposition in which metal particles for brazing are sprayed at high pressure in a vacuum atmosphere. Claim 21 delete Claim 22 A multilayer glass substrate for semiconductors according to claim 17 or 18, wherein the conductive paste comprises 70 to 90 weight% silver (Ag) powder, 5 to 10 weight% binder, 4 to 15 weight% organic solvent, and 1 to 5 weight% additive, wherein the organic solvent is selected from the group consisting of butyl acetate, terpineol, turpentine oil, butyl carbitol, isopropyl alcohol, or a combination thereof, the binder is an acrylic binder or a nitrocellulose binder, and the additive is selected from the group consisting of glycerin, polyethylene glycol (PEG), glass powder, or a combination thereof. Claim 23 A multilayer glass substrate for semiconductors according to claim 17 or 18, wherein the electrode comprises: a signal electrode for transmitting a signal or information; a power electrode for power supply isolated from the signal electrode; and a conductive electrode formed for each glass core for electrical connection between mutually matching electrodes of two adjacent glass cores. Claim 24 A multilayer glass substrate for semiconductors according to claim 23, wherein the signal electrode and power electrode are formed in each glass core. Claim 25 A multilayer glass substrate for semiconductors according to claim 23, wherein a signal electrode is formed on one glass core and a power electrode is formed on another glass core, and the glass core having the signal electrode formed thereon and the glass core having the power electrode formed thereon are alternately stacked.

Citation Information

Patent Citations

  • Ceramic circuit board, method for manufacture thereof and electric device for the same

    KR1020090071010A

  • Printed circuit board and manufacturing method thereof

    KR1020090130942A

  • Passive device packaging structure embedded in glass medium and method for manufacturing the same

    KR1020220021864A

  • Method of metallizing glass articles

    KR1020220125250A