Liquid resin composition and repair method for asphalt pavement using the same

The liquid resin composition and application method address the challenges of costly and unsafe asphalt repairs by enhancing durability and slip resistance, ensuring easy application and effective pavement repair.

KR103044163B1Active Publication Date: 2026-11-06INSUNG A&T
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020250188512
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-12-02
Publication Date
2026-11-06
Estimated Expiration
2045-12-02

AI Technical Summary

Technical Problem

Existing asphalt pavement repair methods are costly, difficult to construct, and fail to meet slip resistance standards, leading to safety issues and durability concerns.

Method used

A liquid resin composition comprising phenolic resin, petroleum resin, SBS, SBR, or EVA, straight asphalt, lubricating base oil, surfactants, and water, applied using a work vehicle with a squeeze member and silica sand spraying device to penetrate and compress the resin onto the pavement surface.

Benefits of technology

The method provides easy application, enhances durability, improves slip resistance, prevents aggregate detachment, and offers anti-freezing effects, resulting in improved asphalt pavement performance and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025135962715-PAT00019_ABST
    Figure 112025135962715-PAT00019_ABST
Patent Text Reader

Abstract

The present invention provides a liquid resin composition for asphalt pavement repair characterized by comprising: 15-25% of a phenolic resin or petroleum resin as an anti-adhesion agent; 5-15% of any one of SBS, SBR, or EVA as a liquid polymer additive; 20-30% of straight asphalt as a binder; 0.2-0.5% of any one of a lubricating base oil, paraffin oil, or surfactant as a penetration improver; 0.4-1.5% of an amine-based surfactant that emulsifies asphalt and water; 0.5-1% of hydrochloric acid as a neutralizing agent that neutralizes the surfactant; 0.01-0.1% of cellulose powder as a storage stabilizer that improves storage performance; and 30-40% of water, thereby making construction easy and providing excellent durability after repair.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to the field of construction technology, and more specifically, to a liquid resin composition and an asphalt pavement repair method using the same. Background Technology

[0002] Various types of damage occur in asphalt road pavements, such as cracks and surface damage caused by damage to the asphalt film.

[0003] Conventionally, to repair this, cutting and overlaying methods, surface treatment methods (fog seal, sand seal), and slurry seal methods have been used.

[0004] The cutting and overlaying method has the disadvantage of being difficult to construct and expensive.

[0005] Surface treatment methods such as fog seals and sand seals do not currently meet domestic slip resistance performance standards, which may lead to traffic safety issues.

[0006] The slurry seal method is more expensive than fog seals or sand seals, and has the problem that it can be easily damaged if there is heavy traffic.

[0007] Therefore, there is an urgent need for research on asphalt pavement repair methods that are easy to construct and provide excellent durability after repair. Prior art literature

[0008] (Patent Document 0001) KR 10-2025-0155787 A(Patent Document 0002) KR 10-2025-0083465 A(Patent Document 0003) JP 7617307 B2(Patent Document 0004) JP 7386955 B1(Patent Document 0005) JP 2023-158941 A(Patent Document 0006) JP 7350599 B2 The problem to be solved

[0009] The present invention was developed to solve the aforementioned problems and aims to provide a liquid resin composition that is easy to apply and has excellent durability after repair, as well as an asphalt pavement repair method using the same.

[0010] In addition, the purpose is to improve the service performance of asphalt pavements by repairing cracks on the asphalt surface, preventing aggregate detachment due to wear of the asphalt coating on the surface of the asphalt pavement, enhancing slip resistance performance through surface treatment and aggregate spreading, providing anti-freezing effects based on the characteristics of the surface treatment method, and improving the appearance of the new pavement. means of solving the problem

[0011] To solve the above problem, the present invention provides a liquid resin composition for asphalt pavement repair characterized by comprising: 15-25% of a phenolic resin or petroleum resin as an anti-adhesion agent; 5-15% of any one of SBS, SBR, or EVA as a liquid polymer additive; 20-30% of straight asphalt as a binder; 0.2-0.5% of any one of a lubricating base oil, paraffin oil, or surfactant as a penetration improver; 0.4-1.5% of an amine-based surfactant that emulsifies asphalt and water; 0.5-1% of hydrochloric acid as a neutralizing agent that neutralizes the surfactant; 0.01-0.1% of cellulose powder as a storage stabilizer that improves storage performance; and 30-40% of water.

[0012] It is preferable that the above anti-adhesion agent has a softening point of 90 to 120°C.

[0013] The above liquid polymer additive preferably has a pH of 4 to 7.

[0014] The above penetration enhancer has a kjnematic viscosity (40℃) of 1 to 100 mm 2 It is desirable to be / s.

[0015] The present invention provides a method for manufacturing a liquid resin composition for asphalt pavement repair, comprising: a step of manufacturing a modified asphalt composition by heating the straight asphalt to 150 to 170°C, adding the anti-adhesion agent, and mixing for 12 to 14 hours to manufacture a modified asphalt composition; a step of manufacturing an emulsified water composition by sequentially adding and mixing water, a neutralizing agent, an amine-based surfactant, a storage stabilizer, and a liquid polymer additive to manufacture an emulsified water composition; and a step of manufacturing a liquid resin composition by mixing the modified asphalt composition, the emulsified water composition, and a penetration power improving agent to manufacture the liquid resin composition for asphalt pavement repair.

[0016] The present invention provides an asphalt pavement repair method using the above-described liquid resin composition for asphalt pavement repair, comprising: a work vehicle preparation step of preparing a work vehicle (10) equipped with a storage unit and an application unit (110) of the above-described liquid resin composition; a squeeze member preparation step of preparing a squeeze member (100) that contacts and compresses the road pavement surface so that the above-described liquid resin composition applied to the road pavement surface penetrates downward, and attaching the squeeze member (100) to the rear of the work vehicle (10); and a liquid resin composition application step of applying the above-described liquid resin composition while driving the work vehicle (10) over the road pavement surface requiring repair, and simultaneously compressing the road pavement surface by the squeeze member (100).

[0017] The squeeze member (100) comprises: a coating portion (110) formed with an upper opening and a lower opening, and a closed structure formed by a wall portion; a connecting portion (120) extended toward the rear of the coating portion (110); and a compression portion (130) formed to be coupled to the rear end of the connecting portion (120) so as to be spaced apart from the rear of the coating portion (110) and to compress the road pavement surface. It is preferable that when the liquid resin composition is introduced into the upper opening of the coating portion (110), the liquid resin composition is applied to the road pavement surface through the lower opening of the coating portion (110), and the compression portion (130) compresses the applied liquid resin composition.

[0018] The wall portion of the coating portion (110) comprises a straight wall portion (111) formed in a straight structure at the front; and a curved wall portion (112) formed in a curved structure at the rear of the straight wall portion (111); and the compression portion (130) is preferably formed in a curved wall structure corresponding to the curved wall portion (112).

[0019] The squeeze member (100) preferably comprises a steel frame (101) forming the upper portion of the coating portion (110), connecting portion (120), and compression portion (130); and an EVA foam (102) coupled to the lower portion of the steel frame (101).

[0020] After the above liquid resin composition application step, it is preferable to further include a silica sand spraying step in which silica sand is sprayed by a silica sand spraying device (200) on the road pavement surface on which the above liquid resin composition has been applied and compressed.

[0021] The above silica sand spreading device (200) comprises: a main body (210) having a frame structure; a wheel (220) installed at the bottom of the main body (210); a silica sand storage unit (230) installed on the main body (210); a silica sand supply unit (231) formed at the bottom of the silica sand storage unit (230); a rotating shaft (240) installed at the bottom of the silica sand storage unit (230); and a rotating plate (250) installed at the bottom of the rotating shaft (240). It is preferable that the silica sand supplied through the silica sand supply unit (231) is scattered in all directions after contacting the upper surface of the rotating plate (250).

[0022] It is preferable that a plurality of protrusions (251) are formed on the upper surface of the above-mentioned rotating plate (250) at spaced intervals from the center toward the edge. Effects of the invention

[0023] The present invention provides a liquid resin composition that is easy to apply and has excellent durability after repair, and an asphalt pavement repair method using the same.

[0024] In addition, the service performance of the asphalt pavement can be improved by repairing cracks on the asphalt surface, preventing aggregate detachment due to wear of the asphalt coating on the surface, enhancing slip resistance performance through surface treatment and aggregate spreading, providing anti-freezing effects based on the characteristics of the surface treatment method, and improving the appearance of the new pavement. Brief explanation of the drawing

[0025] FIG. 1 and below illustrate embodiments of the present invention, Figure 1 is a photograph of a measuring container. Figure 2 is a photograph of a measuring container filled with standard sand. Figure 3 is a photograph showing the case where penetration of the liquid resin composition occurs well. Figure 4 is a photograph of the case where penetration does not occur and it hardens on the surface. FIG. 5 is a flowchart of a method for manufacturing a liquid resin composition. FIG. 6 is a perspective view of a squeeze member. FIG. 7 is a cross-sectional view of a squeeze member. FIG. 8 is a diagram showing the usage state of the squeeze member. Figure 9 is a photograph of a silica sand spreading device. FIG. 10 is a perspective view of a rotating plate. Specific details for implementing the invention

[0026] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings.

[0027] As illustrated in FIG. 1 and below, the present invention relates to a liquid resin composition for repairing asphalt pavement.

[0028] This comprises 15-25% of phenolic resin or petroleum resin as an anti-adhesion agent; 5-15% of any one of SBS, SBR, or EVA as a liquid polymer additive; 20-30% of straight asphalt as a binder; 0.2-0.5% of any one of lubricating base oil, paraffin oil, or surfactant as a penetration improver; 0.4-1.5% of an amine-based surfactant that emulsifies asphalt and water; 0.5-1% of hydrochloric acid as a neutralizing agent that neutralizes the surfactant; 0.01-0.1% of cellulose powder as a storage stabilizer that improves storage performance; and 30-40% of water.

[0029] Anti-adhesion agents (phenol resin, petroleum resin) have a softening point of 90 to 120°C and play a role in preventing damage after application and improving adhesion performance.

[0030] Liquid polymer additives (SBS, SBR, EVA) have a pH of 4 to 7 and improve adhesion performance, thereby enhancing packaging performance.

[0031] Penetration improvers (lubricating base oil, paraffin oil, surfactants) have a kinematic viscosity (40℃) of 1–100 mm 2 It is / s and plays a role in improving penetration ability.

[0032] FIGS. 1 to 4 are photographs relating to the testing process of the penetration power of a liquid resin composition according to the present invention, and specific examples relating to the method for evaluating penetration power will be described later.

[0034] The method for manufacturing a liquid resin composition for asphalt pavement repair according to the present invention is carried out by the following process (Fig. 5).

[0035] After heating straight asphalt to 150~170℃, an anti-adhesion agent is added and mixed for 12~14 hours to produce a modified asphalt composition.

[0036] Water, a neutralizing agent, an amine-based surfactant, a storage stabilizer, and a liquid polymer additive are added sequentially and mixed for at least 30 minutes to prepare an emulsified water composition.

[0037] A liquid resin composition for asphalt pavement repair is prepared by mixing a modified asphalt composition, an emulsified water composition, and a penetration improver.

[0038] At this time, it is preferable that the rotational speed of the mixer be 3,000 rpm or higher.

[0040] Hereinafter, an asphalt pavement repair method using a liquid resin composition for asphalt pavement repair according to the present invention will be described. (Figs. 6 to 10)

[0041] A work vehicle (10) is prepared having a storage section and an application section (110) for a liquid resin composition.

[0042] A squeeze member (100) that contacts and compresses the road surface is prepared and attached to the rear of the work vehicle (10) so that the liquid resin composition applied to the road surface penetrates downward.

[0043] While driving a work vehicle (10) over a road surface requiring repair, a liquid resin composition is applied, and the road surface is compressed by a squeeze member (100).

[0044] On the road surface where the liquid resin composition has been applied and compressed, silica sand is sprayed by a silica sand spraying device (200).

[0045] The squeeze member (100) comprises: an application portion (110) formed with an upper opening and a lower opening, and a closed structure formed by a wall portion; a connecting portion (120) extended toward the rear of the application portion (110); and a compression portion (130) formed to be coupled to the rear end of the connecting portion (120) so as to be spaced apart from the rear of the application portion (110) and to compress the road pavement surface.

[0046] When a work vehicle (10) is operated and a liquid resin composition is introduced through the upper opening of the coating part (110), the liquid resin composition is applied to the road surface through the lower opening of the coating part (110), and the applied liquid resin composition is compressed by the compression part (130).

[0047] The wall portion of the coating portion (110) is configured to include a straight wall portion (111) formed in a straight structure at the front; and a curved wall portion (112) formed in a curved structure at the rear of the straight wall portion (111).

[0048] The compression section (130) is formed as a curved wall structure corresponding to the curved wall section (112).

[0049] This structure prevents the applied liquid resin composition from escaping to the outside of the repair area, thereby enabling tight repair without wasting material.

[0050] The squeeze member (100) may be configured to include a steel frame (101) forming the upper portion of the coating portion (110), the connecting portion (120), and the compression portion (130); and an EVA foam (102) attached to the lower portion of the steel frame (101).

[0051] It is preferable to use high-density EVA foam (102) with a hardness of 15 to 50.

[0052] The steel frame (101) serves to compress the EVA foam (102) by its weight, and the EVA foam (102) ensures that the applied liquid resin composition is evenly compressed onto the road surface.

[0053] A silica sand spreading device (200) comprises: a main body (210) having a frame structure; a wheel (220) installed at the bottom of the main body (210); a silica sand storage unit (230) installed on the main body (210); a silica sand supply unit (231) formed at the bottom of the silica sand storage unit (230); a rotating shaft (240) installed at the bottom of the silica sand storage unit (230); and a rotating plate (250) installed at the bottom of the rotating shaft (240). (Fig. 9)

[0054] When silica sand is supplied through the silica sand supply unit (231), it comes into contact with the upper surface of the rotating plate (250) and is then scattered in all directions.

[0055] In order to ensure that silica sand is evenly dispersed in all directions, a plurality of protrusions (251) are formed on the upper surface of the rotating plate (250) in a radially symmetric structure, spaced apart from each other from the center toward the edge. (Fig. 10)

[0057] Hereinafter, an example for demonstrating the physical properties of the liquid resin composition according to the present invention will be described.

[0059] Anti-adhesion agents (phenol resin, petroleum resin) were applied to prevent damage caused by vehicles when traffic is reopened following repair work using this method, thereby ensuring that the construction condition is maintained on the asphalt pavement surface for a long time.

[0060]

[0061] Table 1 shows the formulations of comparative examples and embodiments of the present invention to evaluate the difference in performance depending on whether an anti-adhesion agent is incorporated.

[0062] An embodiment of the present invention incorporates 10 to 35 weight percent of phenolic resin as an anti-adhesion agent, and a comparative example incorporates silica powder and calcium carbonate instead of an anti-adhesion agent.

[0063]

[0064] Table 2 shows the results of testing the difference in physical properties according to whether an anti-adhesion agent is mixed, according to the tack coat tire adhesion loss rate test method of Annex IV-8 of the Ministry of Land, Infrastructure and Transport's "Asphalt Concrete Construction Guidelines."

[0065] As a result of the test, the comparative example did not satisfy the adhesion rate evaluation criteria (tire adhesion loss rate within 10%), whereas the example was found to satisfy the adhesion rate evaluation criteria when 15 weight% or more of the anti-adhesion agent was mixed.

[0066] In addition, since there is no significant difference in performance between Example 3, which incorporated 25 weight% of an anti-adhesion agent, and Example 4, which incorporated 35 weight% of an anti-adhesion agent, it is determined that the incorporation rate of the anti-adhesion agent is appropriate at 15 to 25 weight%.

[0068] Liquid granular additives (SBS, SBR, EVA), after being mixed with a binder, penetrate and coat cracks and surfaces, thereby improving adhesion performance and enhancing the serviceability of damaged asphalt pavements.

[0069]

[0070] Table 3 shows the formulations of comparative examples and embodiments of the present invention to evaluate the difference in performance depending on whether a liquid polymer additive is incorporated.

[0071] An example of the present invention is one in which 5 to 20 weight percent of SBS is incorporated as a liquid polymer additive, and a comparative example is one in which no liquid polymer additive is incorporated.

[0072]

[0073] Table 4 shows the results of testing the difference in physical properties according to whether liquid polymer additives are incorporated, according to the asphalt performance grade test method KS F 2393 (Dynamic Shear Rheological Characteristics Test of Asphalt).

[0074] As a result of the dynamic shear test, in the case of the comparative example, G* / sin The value was found to be 0.89, which does not meet the test standard (1.0 or less at 76℃).

[0075] In contrast, for Examples 1 to 4, G* / sin As all values ​​were found to satisfy the test standards, it was confirmed that high-temperature performance was improved.

[0076] In addition, since there is no significant difference in performance between Example 3, which incorporated 15% by weight of a liquid polymer additive, and Example 4, which incorporated 20% by weight of a liquid polymer additive, it is determined that the incorporation rate of the anti-adhesion agent is appropriate at 5 to 15% by weight.

[0078] Penetration improvers (lubricating base oils, paraffin oils, surfactants) enhance penetration power and play a role in improving penetration performance in asphalt pavement cracks.

[0079]

[0080] Table 5 shows the formulations of comparative examples and embodiments of the present invention to evaluate the difference in performance depending on whether a penetration power improver is incorporated.

[0081] An embodiment of the present invention is one in which 0.2 to 0.5 weight percent of lubricating base oil is incorporated as a penetration power improving agent, and a comparative example is one in which 0 to 0.1 weight percent of a penetration power improving agent is incorporated.

[0082]

[0083] Table 6 shows the results of testing the difference in physical properties depending on whether a penetration improver is incorporated.

[0084] Since there are no test standards for penetration testing methods in Korea yet, a test method based on the European emulsified asphalt penetration testing method (EN 12849) was applied.

[0085] As a method for evaluating penetration power, as shown in FIGS. 1 to 4, 650g of standard sand was filled into a container with a diameter of about 80mm, 50g of emulsified asphalt was poured within 5 seconds, and the time of penetration was measured.

[0086] Figure 1 is a photograph of a measuring container, and Figure 2 is a photograph of the measuring container filled with standard sand.

[0087] Figure 3 is a photograph showing the case where penetration of the liquid resin composition occurs well, and Figure 4 is a photograph showing the case where penetration does not occur and it hardens on the surface.

[0088] In the case of the comparative example, no penetration occurred, and hardening on the surface was observed after approximately 24 hours. (Fig. 4)

[0089] In the case of the example, it was confirmed that smooth penetration occurred within 30 minutes (Fig. 3).

[0090] Since the target penetration time in the repair method according to the present invention is within 30 minutes, the appropriate mixing rate of the penetration power improving agent was determined to be 0.2 to 0.5 weight%.

[0092] It was confirmed that there is a difference in penetration performance depending on at which stage the penetration improver (lubricating base oil, paraffin oil, surfactant) is incorporated.

[0093]

[0094] Table 7 shows the mixing method of the comparative example and the embodiment of the present invention to evaluate the difference in performance according to the incorporation stage of the penetration power improver.

[0095] Comparative Examples 1 and 2 are cases where a penetration improver was mixed during the mixing process of a modified asphalt composition (a mixture of straight asphalt and an anti-adhesion agent).

[0096] The example is a case in which a penetration improving agent is mixed when mixing a modified asphalt composition (a mixture of straight asphalt and an anti-adhesion agent) and an emulsified water composition (a mixture of water, a neutralizing agent, an amine-based surfactant, a storage stabilizer, and a liquid polymer additive), as in the method for manufacturing a liquid resin composition for asphalt pavement repair according to the present invention described above.

[0097]

[0098] Table 8 shows the test results regarding the penetration power improvement performance of Comparative Examples 1 and 2 and the Example, and the test method is the same as that of Example 3.

[0099] The comparative example is a case where asphalt and a penetration improver are mixed over a long period of time, and the example is a case where asphalt and a penetration improver are mixed over a short period of time; it can be confirmed that in the former case, the penetration improvement effect is reduced.

[0100] Accordingly, as described in the example of the method for manufacturing a liquid resin composition for asphalt pavement repair according to the present invention, it was confirmed that it is preferable to mix a penetration improving agent in the mixing step of the modified asphalt composition (a mixture of straight asphalt and an anti-adhesion agent) and the emulsified water composition (a mixture of water, a neutralizing agent, an amine-based surfactant, a storage stabilizer, and a liquid polymer additive).

[0102] Friction resistance performance is an evaluation criterion used to verify vehicle slip prevention upon road opening after construction is completed, and it is a critical evaluation factor directly related to safety.

[0103]

[0104] Table 9 shows the results of a friction resistance test conducted on the comparative example and Examples 1 and 2 of the present invention.

[0105] Comparative examples relate to road pavement surfaces to which the fog seal method is applied, Example 1 relates to a road pavement surface to which a liquid resin composition according to the present invention is applied and finished by a squeeze member (100), and Example 2 relates to a road pavement surface to which silica sand is additionally sprayed on Example 1.

[0106] The comparative example (Fog Seal) relates to a surface treatment method involving the simple application of emulsified asphalt, which has low frictional resistance and a high likelihood of exposure to the risk of slip accidents.

[0107] However, in the case of the embodiments of the present invention, it can be confirmed that the risk of slip accidents can be reduced due to the excellent frictional resistance.

[0109] The present invention relates to a surface treatment method for repairing a surface by penetrating a liquid resin repair agent into the surface of an asphalt pavement and then scraping it off using a squeeze method, wherein a liquid resin repair agent with improved adhesion, penetration power, and damage prevention performance is applied.

[0110] Since the squeeze method is used for construction, sufficient penetration into cracks in the pavement improves the serviceability of the pavement and minimizes the surface laying thickness, thereby improving friction resistance performance.

[0111] The application of the liquid resin repair agent and the squeegee installation are performed simultaneously, offering the advantages of simple installation and low cost.

[0112] Because water-soluble materials are applied, it is more convenient and stable to use compared to cutback-type (solvent) materials currently used in surface treatment methods, and it is eco-friendly as it does not generate residual oil.

[0113] If necessary, silica sand can be sprayed to improve friction resistance performance, which can help ensure driving stability.

[0115] The foregoing merely describes some preferred embodiments that can be implemented by the present invention. As is well known, the scope of the present invention should not be interpreted as being limited to the above embodiments, and all technical concepts that share the fundamental principles with the technical concept of the present invention described above shall be considered to be included within the scope of the present invention. Explanation of the symbols

[0116] 10 : Work vehicle 100 : Squeeze missing 101: Steel frame 102: EVA foam 110 : Coating section 111 : Straight wall section 112 : Curved wall section 120 : Connecting section 130 : Compression section 200 : Silica sand spreading device 210: Main body 220: Wheels 230: Silica sand storage unit 231: Silica sand supply unit 240 : Rotation axis 250 : Turntable 251 : Protrusion

Claims

Claim 1 A modified asphalt composition preparation step comprising: 15-25% of phenolic resin or petroleum resin as an anti-adhesion agent; 5-15% of any one of SBS, SBR, or EVA as a liquid polymer additive; 20-30% of straight asphalt as a binder; 0.2-0.5% of any one of lubricating base oil, paraffin oil, or surfactant as a penetration improver; 0.4-1.5% of an amine-based surfactant that emulsifies asphalt and water; 0.5-1% of hydrochloric acid as a neutralizing agent that neutralizes the surfactant; 0.01-0.1% of cellulose powder as a storage stabilizer that improves storage performance; and 30-40% of water; wherein the straight asphalt is heated to 150-170°C, the anti-adhesion agent is added, and the mixture is mixed for 12-14 hours to prepare a modified asphalt composition; wherein the water, neutralizing agent, amine-based surfactant, storage stabilizer, and liquid polymer additive A liquid resin composition for asphalt pavement repair, characterized by being produced by a manufacturing method comprising: a step of preparing an emulsified water composition by sequentially adding and mixing to prepare an emulsified water composition; and a step of preparing a liquid resin composition by mixing the modified asphalt composition, the emulsified water composition, and a penetration power improver to prepare the liquid resin composition for asphalt pavement repair. Claim 2 A liquid resin composition for asphalt pavement repair according to claim 1, characterized in that the anti-adhesion agent has a softening point of 90 to 120°C. Claim 3 A liquid resin composition for asphalt pavement repair according to claim 1, wherein the liquid polymer additive has a pH of 4 to 7. Claim 4 In claim 1, the penetration power improver has a kjnematic viscosity (40℃) of 1 to 100 mm 2 Liquid resin composition for asphalt pavement repair characterized by being / s. Claim 5 delete Claim 6 An asphalt pavement repair method using a liquid resin composition for asphalt pavement repair comprising: 15-25% of a phenolic resin or petroleum resin as an anti-adhesion agent; 5-15% of any one of SBS, SBR, or EVA as a liquid polymer additive; 20-30% of straight asphalt as a binder; 0.2-0.5% of any one of lubricating base oil, paraffin oil, or surfactant as a penetration improver; 0.4-1.5% of an amine-based surfactant that emulsifies asphalt and water; 0.5-1% of hydrochloric acid as a neutralizing agent that neutralizes the surfactant; 0.01-0.1% of cellulose powder as a storage stabilizer that improves storage performance; and 30-40% of water; wherein the method comprises: a work vehicle preparation step of preparing a work vehicle (10) equipped with a storage section and an application section (110) of the liquid resin composition; and a method of pressing in contact with the road pavement surface so that the liquid resin composition applied to the road pavement surface penetrates downward. An asphalt pavement repair method characterized by comprising: a squeeze member preparation step of preparing a squeeze member (100) and attaching it to the rear of the work vehicle (10); and a liquid resin composition application step of applying the liquid resin composition while driving the work vehicle (10) over the road pavement surface requiring repair, and simultaneously compressing the road pavement surface by the squeeze member (100). Claim 7 In claim 6, the squeeze member (100) comprises: an application portion (110) formed with an upper opening and a lower opening and a closed structure formed by a wall portion; a connecting portion (120) extended toward the rear of the application portion (110); and a compression portion (130) formed to be coupled to the rear end of the connecting portion (120) so as to be spaced apart from the rear of the application portion (110) and to compress the road pavement surface; and when the liquid resin composition is poured into the upper opening of the application portion (110), the liquid resin composition is applied to the road pavement surface through the lower opening of the application portion (110), and the compression portion (130) compresses the applied liquid resin composition. Claim 8 In claim 7, the wall portion of the coating portion (110) comprises a straight wall portion (111) formed in a straight structure at the front; and a curved wall portion (112) formed in a curved structure at the rear of the straight wall portion (111); and the compression portion (130) is formed in a curved wall structure corresponding to the curved wall portion (112), characterized in that it is an asphalt pavement repair method. Claim 9 In claim 7, the asphalt pavement repair method is characterized in that the squeeze member (100) comprises: a steel frame (101) forming the upper part of the coating part (110), the connecting part (120), and the compression part (130); and an EVA foam (102) coupled to the lower part of the steel frame (101). Claim 10 The asphalt pavement repair method according to claim 6 further comprises a silica sand spraying step in which silica sand is sprayed by a silica sand spraying device (200) on the road pavement surface on which the liquid resin composition has been applied and compressed, after the liquid resin composition application step. Claim 11 In claim 10, the silica sand spreading device (200) comprises: a main body (210) having a frame structure; a wheel (220) installed at the bottom of the main body (210); a silica sand storage unit (230) installed on the main body (210); a silica sand supply unit (231) formed at the bottom of the silica sand storage unit (230); a rotating shaft (240) installed at the bottom of the silica sand storage unit (230); and a rotating plate (250) installed at the bottom of the rotating shaft (240); and the silica sand supplied through the silica sand supply unit (231) is scattered in all directions after contacting the upper surface of the rotating plate (250), characterized in that the asphalt pavement repair method is characterized in that the silica sand supplied through the silica sand supply unit (231) is scattered in all directions. Claim 12 In claim 11, the asphalt pavement repair method is characterized by having a plurality of protrusions (251) formed spaced apart from each other on the upper surface of the rotating plate (250) from the center toward the edge.

Citation Information

Patent Citations

  • Asphalt pavement construction method using emulsified asphalt composition for rapid setting type

    KR1020230149360A

  • method for repairing concrete and asphalt road using composition FOR REPAIRING ROAD and composition for Acrylic Film Sealer