Photocurable red resin composition, display device, and method for manufacturing a laminate of an organic light-emitting element and an external light-reflecting anti-reflective film

A photocurable red resin composition with red and black materials forms a cured film on OLEDs to address the challenges of thickness, flexibility, and external light reflection, enhancing OLED display performance.

KR103044354B1Active Publication Date: 2026-11-06DNP FINE CHEMICALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020237022616
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-23
Filing Date
2021-12-01
Publication Date
2026-11-06
Estimated Expiration
2041-12-01

AI Technical Summary

Technical Problem

Existing organic light-emitting diode (OLED) display devices face challenges in achieving thinness, flexibility, and effective suppression of external light reflection due to the use of rigid circular polarizers, which reduce light utilization efficiency and flexibility.

Method used

A photocurable red resin composition containing a colorant, photopolymerizable compound, and photoinitiator, including red and black materials, is applied directly on the OLED to form a cured film that suppresses external light reflection, enhancing device thinness and flexibility.

Benefits of technology

The solution results in a thin and flexible OLED display device that effectively reduces external light reflection without the need for circular polarizers, maintaining high light utilization efficiency and visibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023073332658-PCT00018_ABST
    Figure 112023073332658-PCT00018_ABST
Patent Text Reader

Abstract

A photocurable red resin composition used for a cured film formed on an organic light-emitting diode, wherein the photocurable red resin composition contains a colorant, a photopolymerizable compound, and a photoinitiator, and the colorant comprises a red material and a black material.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a photocurable red resin composition, a display device containing a cured product of the photocurable red resin composition, and a method for manufacturing a laminate of an organic light-emitting element and an external light-reflecting anti-reflective film using the photocurable red resin composition. Background Technology

[0002] Recently, organic light-emitting diodes (OLEDs) are attracting attention as display elements for mobile devices and televisions because they are advantageous for thinning and flexibility compared to conventional liquid crystal displays, and in principle, have high light utilization efficiency.

[0003] These organic light-emitting diodes (OLEDs), particularly in mobile devices intended for outdoor use, are equipped with circular polarizers as anti-reflective films to prevent reduced visibility caused by the reflection of external light. However, since these circular polarizers block not only external light but also the light emitted by the OLEDs, the light utilization efficiency is significantly reduced. Furthermore, because circular polarizers have rigid properties, they reduce flexibility, making them disadvantageous for flexible displays. Consequently, there has been a demand for the development of display devices utilizing OLEDs that offer good outdoor visibility even without the use of circular polarizers.

[0004] In this regard, Patent Document 1 discloses a red photosensitive resin composition for pixel formation that suppresses reflection of external light by means of a color filter capable of replacing a polarizer and can realize high color reproduction while being capable of replacing a polarizer, wherein the composition comprises a coloring agent, an alkali-soluble resin, a photopolymerizable compound, a photopolymerization initiator, and a solvent, wherein the coloring agent comprises a red pigment and a black pigment, and wherein the red photosensitive resin composition is characterized in that, when forming a cured film having a thickness of 3 μm, the spectral transmittance at a wavelength of 430 to 590 nm is 20% or less and the spectral transmittance at a wavelength of 635 to 780 nm is 70% or more and less than 90%. Prior art literature

[0005] Patent Document 1: Japanese Patent Publication No. 2017-173828 The problem to be solved

[0006] The color filter replacing the polarizer in Patent Document 1 is formed on a glass substrate. Therefore, there were further problems in manufacturing a display device with improved thinness and flexibility.

[0007] The present invention, made in consideration of the above circumstances, aims to provide a photocurable red resin composition capable of suppressing external light reflection and manufacturing an organic light-emitting display device that is thin and has improved flexibility. Furthermore, the present invention aims to provide a display device capable of suppressing external light reflection, being thin and having improved flexibility, containing a cured product of the photocurable red resin composition, and a method for manufacturing a laminate of an organic light-emitting element and an external light reflection prevention film using the photocurable red resin composition. means of solving the problem

[0008] The photocurable red resin composition according to the present invention is a photocurable red resin composition used for a cured film formed on an organic light-emitting diode,

[0009] The above photocurable red resin composition contains a colorant, a photopolymerizable compound, and a photoinitiator, and

[0010] The above-mentioned color material includes red and black materials.

[0011] A display device according to the present invention has a cured film of a photocurable red resin composition according to the present invention on an organic light-emitting element.

[0012] A method for manufacturing a laminate of an organic light-emitting element and an external light reflection prevention film according to the present invention is,

[0013] A process of forming a coating film by applying a photocurable red resin composition according to the present invention onto an organic light-emitting diode,

[0014] A process of irradiating the above coating film with light,

[0015] A post-baking process for heating the film after the above light irradiation, and

[0016] By including a process for developing the film after the above light irradiation,

[0017] The method comprises forming a cured film of a photocurable red resin composition according to the present invention on an organic light-emitting diode. Effects of the invention

[0018] According to the present invention, a photocurable red resin composition can be provided to manufacture an organic light-emitting display device that is thin and has improved flexibility, capable of suppressing external light reflection. Furthermore, the present invention can provide a display device that is thin and has improved flexibility, capable of suppressing external light reflection, containing a cured product of the photocurable red resin composition, and a method for manufacturing a laminate of an organic light-emitting element and an external light reflection prevention film using the photocurable red resin composition. Brief explanation of the drawing

[0019] FIG. 1 is a schematic cross-sectional view illustrating an example of a display device equipped with an organic light-emitting element according to the present invention. Specific details for implementing the invention

[0020] Hereinafter, embodiments and examples of the present invention will be described with reference to the drawings. However, the present invention may be implemented in many different forms and is not to be interpreted as being limited to the contents described in the embodiments and examples exemplified below. Furthermore, in order to make the explanation clearer, the drawings may schematically depict the width, thickness, shape, etc. of each part in comparison with the actual form; however, this is merely an example and does not limit the interpretation of the present invention. In addition, in this specification and each drawing, elements that have been described above in previously shown drawings are given the same reference numerals, and detailed descriptions may be appropriately omitted. Also, for convenience of explanation, the words "up" or "down" may be used, but the up and down directions may be reversed.

[0021] In this specification, where any component, such as a member or region, is described as being "on (or under)" another component, such as another member or region, unless otherwise specifically limited, this includes not only the case where it is immediately above (or immediately below) the other component, but also the case where it is above (or below) the other component; that is, it includes the case where another component is included between the components above (or below) the other component.

[0022] In addition, in the present invention, light includes electromagnetic waves with wavelengths in the visible and non-visible regions, and furthermore, radiation, and radiation includes, for example, microwaves and electron beams. Specifically, it refers to electromagnetic waves and electron beams with a wavelength of 5 μm or less.

[0023] In the present invention, (meth)acryloyl refers to acryloyl and methacryloyl, respectively; (meth)acrylic refers to acrylic and methacrylic, respectively; and (meth)acrylate refers to acrylate and methacrylate, respectively.

[0024] Additionally, in this specification, "∼" indicating a numerical range is used to mean that the values ​​described before and after it are included as lower and upper limits.

[0025] Hereinafter, a photocurable red resin composition according to the present invention, a display device, and a method for manufacturing a laminate of an organic light-emitting element and an external light-reflecting anti-reflective film will be described in detail in sequence.

[0026] I. Photocurable red resin composition

[0027] The photocurable red resin composition according to the present invention is a photocurable red resin composition used for a cured film formed on an organic light-emitting diode,

[0028] The above photocurable red resin composition contains a colorant, a photopolymerizable compound, and a photoinitiator, and

[0029] The above-mentioned color material includes red and black materials.

[0030] Since the photocurable red resin composition according to the present invention comprises a red material and a black material as the colorant, the cured film of the photocurable red resin composition can effectively reduce the transmittance of the film and suppress external light reflection as a substitute for a polarizer.

[0031] In addition, the photocurable red resin composition according to the present invention is characterized by being used in a cured film formed on an organic light-emitting element. That is, the photocurable red resin composition according to the present invention is used in a cured film formed directly on a device substrate equipped with an organic light-emitting element. Since the photocurable red resin composition according to the present invention is a photocurable red resin composition used in a cured film formed adjacent to or through at least one layer on an organic light-emitting element, it is possible to manufacture a display device with improved thinning and flexibility compared to a display device in which an externally attached color filter formed on a substrate such as a glass substrate is attached to an organic light-emitting element.

[0032] The photocurable red resin composition according to the present invention contains at least a colorant, a photopolymerizable compound, and a photoinitiator, and may additionally contain other components to the extent that it does not impair the effects of the present invention.

[0033] Hereinafter, each component of the photocurable red resin composition according to the present invention will be described in detail in sequence.

[0034] Color

[0035] In the present invention, the colorant is not particularly limited and can be used by mixing two or more types of various organic pigments, inorganic pigments, dispersible dyes, dye-forming compounds, etc., as long as they are capable of producing a desired color when forming a colored layer of a color filter. It is characterized by including a red material and a black material.

[0036] Among red materials, organic pigments are preferably used because they have high color development and high heat resistance. Examples of organic pigments include compounds classified as pigments in the Color Index (CI; issued by The Society of Dyersand Colourists), specifically those assigned Color Index (CI) numbers as follows.

[0037] As for red materials, for example, CI pigment red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 40, 41, 42, 48:1, 48:2, 48:3, 48:4, 49:1, 49:2, 50:1, 52:1, 53:1, 57, 57:1, 57:2, 58:2, 58:4, 60:1, 63:1, 63:2, 64:1, 81:1, 83, 88, 90:1, 97, 101, 102, 104, 105, 106, 108, 112, 113, 114, 122, 123, 144, 146, 149, 150, 151, 166, 168, 170, 171, 172, 174, 175, 176, 177, 178, 179, 180, 185, 187, 188, 190, 193, 194, 202, 206, 207, 208, 209, 215, 216, 220, 224, 226, 242, 243, 245, 254, At least one selected from 255, 264, 265, 269, 272, 291, etc., and diketopyrrolopyrrole pigments represented by the following general formula (i).

[0038]

[0039] (of general formula (i), R 61 and R 62 Each is independently a 4-chlorophenyl group or a 4-bromophenyl group.)

[0040] As for the red material, at least one selected from Pigment Red 177, Pigment Red 254, and Pigment Red 291 is preferred in that the vertical rise of the transmission spectrum is steep and it is easy to improve the external light reflection suppression effect.

[0041] Pigment Red 177, Pigment Red 254, and Pigment Red 291 each have different vertical rising wavelengths of transmission spectra shifting slightly from the long wavelength side to the short wavelength side. Therefore, it is preferable to appropriately select and use one type alone or in combination of two or more types, taking into account the spectrum of the red light-emitting layer of the organic light-emitting device combined to perform external light reflection.

[0042] As for the black material, at least one selected from inorganic pigments such as carbon black or titanium black, organic pigments such as cyanine black, CI pigment black 1, 7, etc. is acceptable.

[0043] As for the black material, it is desirable to include carbon black, as it offers good storage stability and facilitates the improvement of the external light reflection suppression effect.

[0044] As for the carbon black, there are no particular limitations as long as it is a light-blocking pigment, and known carbon blacks may be used. Specifically, examples of carbon black for the above black pigment include channel black, furnace black, thermal black, lamp black, etc.

[0045] In addition to the coloring material, other coloring materials may be used to adjust the effect of suppressing external light reflection. Examples of other coloring materials include green, blue, purple, yellow, and orange colors.

[0046] Among these, it is preferable that the above-mentioned color material additionally includes at least one type of green material and blue material as other color materials, in that it is easy to adjust the shape of the transmission spectrum of the red material well and easy to improve the effect of suppressing external light reflection.

[0047] Examples of green materials include CI pigment greens 7, 36, 58, 59, 62, 63, etc.

[0048] Examples of blue pigments include CI pigment blue 5, 15:3, 15:4, 15:6, 60, etc.

[0049] In addition, examples of purple pigments include CI pigment violet 1, 19, 23, 29, 32, 36, 38, etc.

[0050] As a yellow material, for example, CI pigment yellow 1, 3, 12, 13, 14, 15, 16, 17, 20, 24, 31, 55, 60, 61, 65, 71, 73, 74, 81, 83, 93, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 116, 117, 119, 120, 126, 127, 128, 129, 138, 139, 150, 151, 152, 153, 154, 155, 156, 166, 168, Examples include derivative pigments of 175, 185, and CI pigment Yellow 150.

[0051] Examples of orange pigments include CI pigment orange 1, 5, 13, 14, 16, 17, 24, 34, 36, 38, 40, 43, 46, 49, 51, 61, 63, 64, 71, 73, etc.

[0052] The content ratio of the red material, black material, and other color materials that may be included as needed in the present invention is preferably adjusted so that when a cured film with a film thickness of 3.0 μm is formed by the photocurable red resin composition, the spectral transmittance at a wavelength of 430 nm to 580 nm is 15.0% or less, and the spectral transmittance at a wavelength of 610 nm to 630 nm is 50.0% or more and 90.0% or less.

[0053] When a cured film is formed with a film thickness of 3.0 μm, if the spectral transmittance at a wavelength of 430 nm to 580 nm is 15.0% or less, the decrease in red color purity is suppressed, and the decrease in color purity from the light-emitting device is also easily suppressed. When a cured film is formed with a film thickness of 3.0 μm, the spectral transmittance at a wavelength of 430 nm to 580 nm may be 10.0% or less, or 8.0% or less.

[0054] Meanwhile, when a cured film is formed with a film thickness of 3.0 μm, if the spectral transmittance at a wavelength of 610 nm to 630 nm is 50.0% or higher, it is easy to suppress brightness reduction or visibility defects of the display device. When a cured film is formed with a film thickness of 3.0 μm, the spectral transmittance at a wavelength of 610 nm to 630 nm may be 60.0% or higher, or 70.0% or higher.

[0055] In addition, when a cured film is formed with a thickness of 3.0 μm, if the spectral transmittance at a wavelength of 610 nm to 630 nm is 90.0% or less, it is easy to obtain an external light reflection suppression effect. When a cured film is formed with a thickness of 3.0 μm, the spectral transmittance at a wavelength of 610 nm to 630 nm may be 80.0% or less, or 70.0% or less.

[0056] In the colorant used in the present invention, the content of the red material may be typically 50 mass% or more and 99.9 mass% or less with respect to the total amount of colorant, preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, preferably 99.6 mass% or less, and more preferably 99.0 mass% or less.

[0057] In the colorant used in the present invention, the content of the black colorant may be typically 0.1 mass% or more and 20 mass% or less with respect to the total amount of colorant, preferably 0.4 mass% or more, more preferably 1.0 mass% or more, preferably 10 mass% or less, and more preferably 5 mass% or less.

[0058] In the colorant used in the present invention, the total content of red and black materials may be at least 50 mass% with respect to the total amount of colorant, preferably at least 70 mass%, more preferably at least 90 mass%, or at least 100 mass%, but if other colorants are included, it may be at least 99 mass% or at least 90 mass%.

[0059] In the colorant used in the present invention, the total content of other colorants may be 0 mass% with respect to the total amount of colorants, 1 mass% or more, or 10 mass% or more, while typically 50 mass% or less, and preferably 30 mass% or less.

[0060] When at least one type of green material and blue material is used as other coloring material, the total content may be typically 0.1 mass% or more and 30 mass% or less, preferably 1 mass% or more, more preferably 10 mass% or more, preferably 30 mass% or less, and more preferably 20 mass% or less.

[0061] The average primary particle size of the colorant used in the present invention is not particularly limited, provided that when formed into a cured film, it can suppress external light reflection and also transmit desired light from a light-emitting element to suppress a decrease in brightness of the display device. Although it varies depending on the type of colorant used, it is preferably within the range of 10 nm to 100 nm, and more preferably within the range of 15 nm to 60 nm. By having the average primary particle size of the colorant within the above range, a display device equipped with a cured film manufactured using the photocurable red resin composition according to the present invention can suppress external light reflection, have high contrast, and be of high quality.

[0062] In addition, the average dispersion particle size of the colorant in the photocurable red resin composition varies depending on the type of colorant used, but it is preferably within the range of 10 nm to 100 nm, and more preferably within the range of 15 nm to 60 nm.

[0063] The average dispersion particle size of the colorant in the photocurable red resin composition is the dispersion particle size of the colorant particles dispersed in a dispersion medium containing at least a solvent, and is measured by a laser light scattering particle size distribution meter. For measuring the particle size by the laser light scattering particle size distribution meter, the photocurable red resin composition is appropriately diluted (e.g., 1000 times, etc.) with the solvent used in the photocurable red resin composition to a concentration that can be measured by the laser light scattering particle size distribution meter, and the measurement can be performed at 23°C by the dynamic light scattering method using a laser light scattering particle size distribution meter (e.g., NanoTrack particle size distribution measuring device UPA-EX150 manufactured by Nikiso Co., Ltd.). The average distribution particle size here is the volume average particle size.

[0064] The colorant used in the present invention can be manufactured by known methods such as recrystallization or solvent salt milling. Additionally, commercially available colorants may be used after undergoing a micronization process.

[0065] In the photocurable red resin composition according to the present invention, the content of the colorant is not particularly limited. The content of the colorant is, for the sake of dispersibility and dispersion stability, preferably within the range of 3 mass% to 65 mass%, more preferably 4 mass% to 60 mass% with respect to the total solid content of the photocurable red resin composition. If it is above the lower limit, the cured film when the photocurable red resin composition is applied to a predetermined film thickness (typically 1.0 μm to 5.0 μm, for example 3.0 μm) is likely to have a sufficient color concentration and a good external light reflection suppression effect. Furthermore, if it is below the upper limit, it is easy to obtain a cured film with excellent storage stability and sufficient hardness or adhesion to the substrate. In particular, when forming a cured film with a high colorant concentration, the total content of the colorant is preferably within the range of 15 mass% to 65 mass%, more preferably 25 mass% to 60 mass% with respect to the total solid content of the photocurable red resin composition.

[0066] In addition, in the present invention, the solid content is all of the material other than the solvent described below, and also includes monomers dissolved in the solvent.

[0067] Photopolymerizable Compounds

[0068] Examples of photopolymerizable compounds used in a photocurable red resin composition include compounds having photopolymerizable groups in their molecules. As for the photopolymerizable groups, they only need to be capable of polymerization by a photoinitiator and are not particularly limited, but examples include ethylenically unsaturated double bonds, such as vinyl groups, allyl groups, acryloyl groups, or methacryloyl groups. Among these, acryloyl groups or methacryloyl groups are suitably used as photopolymerizable groups due to their UV curability.

[0069] As for the photopolymerizable compound, in terms of curability, it is preferable to contain a compound having two or more photopolymerizable groups in one molecule, and it is more preferable to contain a compound having three or more photopolymerizable groups in one molecule.

[0070] As a photopolymerizable compound, a compound having two or more ethylenically unsaturated double bonds is suitably used, and in particular, it is preferred to be a polyfunctional (meth)acrylate having two or more acryloyl or methacryloyl groups.

[0071] Such multi-functional (meth)acrylates may be appropriately selected from those previously known. Specific examples include those described in Japanese Patent Publication No. 2013-029832.

[0072] These multifunctional (meth)acrylates may be used as a single type or in combination of two or more types. In addition, when excellent photocurability (high sensitivity) is required for the photocurable red resin composition of the present invention, it is preferable that the poly(meth)acrylate has three or more polymerizable double bonds (tri-function), and poly(meth)acrylates of trivalent or higher polyhydric alcohols or their dicarboxylic acid modified products are preferred, specifically trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, succinic acid modified product of pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, succinic acid modified product of dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc. are preferred.

[0073] The content of the photopolymerizable compound used in the photocurable red resin composition is not particularly limited, but is preferably within the range of 5 mass% to 60 mass%, and more preferably 10 mass% to 40 mass%, with respect to the total solid content of the photocurable red resin composition. If the content of the photopolymerizable compound is above the lower limit, sufficient photocuring proceeds, making it easy to suppress leaching during development of the exposed area. Furthermore, if the content of the photopolymerizable compound is below the upper limit, sufficient alkali developability is easily achieved.

[0074] <Gwanggaesiseje>

[0075] As a photoinitiator used in the photocurable red resin composition of the present invention, one or more types of various photoinitiators known in the prior art may be used in combination.

[0076] Examples of photoinitiators include aromatic ketones, benzoin ethers, halomethyloxadiazole compounds, α-aminoketones, nonimidazoles, N,N-dimethylaminobenzophenones, halomethyl-S-triazine compounds, thioxantones, oxime esters, etc. Among these photoinitiators, conventionally known photoinitiators may be used, such as the photoinitiator described in International Publication No. 2018 / 062105.

[0077] In addition, as an oxime ester-based photoinitiator used in the present invention, among the oxime ester-based photoinitiators described in, for example, 1,2-octadione-1-[4-(phenylthio)phenyl]-,2-(o-benzoyloxime), ethanol, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-,1-(o-acetyloxime), Japanese Patent Publication No. 2000-80068, Japanese Patent Publication No. 2001-233842, Japanese Patent Publication No. 2010-527339, Japanese Patent Publication No. 2010-527338, Japanese Patent Publication No. 2013-041153, International Publication No. 2015 / 152153, Japanese Patent Publication No. 2010-256891, etc. You can choose appropriately.

[0078] When forming a cured film on a device substrate as in the present invention, since the heat resistance of the organic light-emitting device is low, it is considered desirable to perform low-temperature heating treatment, such as 130°C or lower and 100°C or lower, during the manufacturing process. In a conventional color filter manufacturing process, a cured film is cured by performing a heat treatment of about 230°C on a glass substrate, whereas it is difficult for the cured film to proceed with heat treatment at 130°C or lower. That is, there is a problem in that the cured film produced by low-temperature heating treatment tends to have insufficient substrate adhesion and solvent resistance.

[0079] Regarding these challenges, since the substrate adhesion and solvent resistance of the cured film are good even with low-temperature heat treatment, it is preferable that the photoinitiator includes at least one of the compounds represented by the following general formula (A) and the following general formula (B).

[0080]

[0081] (during food, R 1 and R 2 are each independently R 11 , OR 11 , COR 11 , SR 11, CONR 12 R 13 or represents CN,

[0082] R 11 , R 12 and R 13 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms, and

[0083] R 11 , R 12 and R 13 The hydrogen atom of the group represented as additionally R 21 , OR 21 , COR 21 , SR 21 , NR 22 R 23 , CONR 22 R 23 , -NR 22 -OR 23 , -NCOR 22 -OCOR 23 , NR 22 COR 21 , OCOR 21 , COOR 21 , SCOR 21 , OCSR 21 , COSR 21 , CSOR 21 , may be substituted with a hydroxyl group, a nitro group, CN, or a halogen atom, and

[0084] R 21 , R 22 and R 23 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms, and

[0085] R 21 , R 22 and R 23 The hydrogen atom of the group represented by may additionally be substituted with a hydroxyl group, a nitro group, CN, a halogen atom, or a carboxyl group, and

[0086] R 11 , R 12 , R 13 , R 21 , R 22 and R 23 The alkylene portion of the group represented by -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 It may include 1 to 5 groups of -, -SCO-, -COS-, -OCS-, or -CSO- under conditions where oxygen atoms are not adjacent, and

[0087] R 24 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms, and

[0088] R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The alkyl portion of the group represented by may have a branched side chain and may be a cyclic alkyl.

[0089] R 3 It represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms, and R 3 The alkyl portion of the group represented by may have a branched side chain, may be a cyclic alkyl, and also, R 3 and R 7 and R 3 and R 8 It is fine if each becomes one to form a ring, and

[0090] R 3 The hydrogen atom of the group represented as additionally R 21 , OR 21 , COR 21 , SR21 , NR 22 R 23 , CONR 22 R 23 , -NR 22 -OR 23 , -NCOR 22 -OCOR 23 , NR 22 COR 21 , OCOR 21 , COOR 21 , SCOR 21 , OCSR 21 , COSR 21 , CSOR 21 , may be substituted with a hydroxyl group, a nitro group, CN, or a halogen atom, and

[0091] R 4 , R 5 , R 6 and R 7 R each independently 11 , OR 11 , SR 11 , COR 14 , CONR 15 R 16 , NR 12 COR 11 , OCOR 11 , COOR 14 , SCOR 11 , OCSR 11 , COSR 14 , CSOR 11 , representing a hydroxyl group, CN, or a halogen atom, and R 4 and R 5 , R 5 and R 6 and R 6 and R 7 It is fine if each becomes one to form a ring, and

[0092] R 14 , R 15 and R 16 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, and R 14 , R 15 and R 16The alkyl portion of the group represented by may have a branched side chain and may be a cyclic alkyl,

[0093] R 8 is R 11 , OR 11 , SR 11 , COR 11 , CONR 12 R 13 , NR 12 COR 11 , OCOR 11 , COOR 11 , SCOR 11 , OCSR 11 , COSR 11 , CSOR 11 , representing a hydroxyl group, CN, or halogen atom,

[0094] k represents 0 or 1.

[0095]

[0096] (In Equation (B), X 1 , X 3 and X 6 R each independently 41 , OR 41 , COR 41 , SR 41 , CONR 42 R 43 Or represents CN, and X 2 represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms, and X 4 and X 5 are each independently R 41 , OR 41 , SR 41 , COR 41 , CONR 42 R 43 , NR 42 COR 41 , OCOR 41 , COOR 41 , SCOR 41 , OCSR 41 , COSR41 , CSOR 41 , CN, represents a halogen atom or a hydroxyl group.

[0097] R 41 , R 42 and R 43 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms, and

[0098] R 41 , R 42 and R 43 , and X 2 The hydrogen atom of the group represented by is additionally R 51 , OR 51 , COR 51 , SR 51 , NR 52 R 53 , CONR 52 R 53 , -NR 52 -OR 53 , -NCOR 52 -OCOR 53 , NR 52 COR 51 , OCOR 51 , COOR 51 , SCOR 51 , OCSR 51 , COSR 51 , CSOR 51 , may be substituted with a hydroxyl group, a nitro group, CN, or a halogen atom, and

[0099] R 51 , R 52 and R 53 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms, and

[0100] R 51 , R 52 and R 53The hydrogen atom of the group represented by may additionally be substituted with a hydroxyl group, a nitro group, CN, a halogen atom, or a carboxyl group, and

[0101] R 41 , R 42 , R 43 , X 2 , R 51 , R 52 and R 53 The alkylene portion of the group represented by -O-, -S-, -COO-, -OCO-, -NR 54 -, -NR 54 CO-, -NR 54 COO-, -OCONR 54 It may include 1 to 5 groups of -, -SCO-, -COS-, -OCS-, or -CSO- under conditions where oxygen atoms are not adjacent, and

[0102] R 54 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms, and

[0103] R 41 , R 42 , R 43 , R 51 , R 52 , R 53 and R 54 The alkyl portion of the group represented by may have a branched side chain and may be a cyclic alkyl.

[0104] a and b are each independently integers from 0 to 3.

[0105] (Compound represented by general formula (A))

[0106] In the oxime ester compound represented by the above general formula (A), geometric isomers due to the double bond of the oxime exist, but they are not distinguished. That is, in this specification, the compound represented by the above general formula (A), and the compound represented by the following general formula (A'), which is a preferred form of the said compound described below, and the exemplary compounds thereof represent a mixture of both or either one, and are not limited to structures having isomers.

[0107] R in the above general formula (A) 3 , R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 21 , R 22 , R 23 and R 24 Examples of alkyl groups having 1 to 20 carbon atoms represented by are methyl, ethyl, propyl, isopropyl, butyl, isobutyl, s-butyl, t-butyl, amyl, isoamyl, t-amyl, hexyl, heptyl, octyl, isooctyl, 2-ethylhexyl, t-octyl, nonyl, isononyl, decyl, isodecyl, undecyl, dodecyl, tetradecyl, hexadecyl, octadecyl, icosyl, cyclopentyl, cyclopentylmethyl, cyclopentylethyl, cyclohexyl, cyclohexylmethyl, cyclohexylethyl, etc.

[0108] R in the above general formula (A) 3 , R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Examples of aryl groups having 6 to 30 carbon atoms represented by phenyl, tolyl, xylyl, ethylphenyl, naphthyl, anthyl, phenanthrenyl, and phenyl, biphenyllyl, naphthyl, anthyl substituted with one or more of the above alkyl groups can be used.

[0109] R in the above general formula (A)3 , R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Examples of arylalkyl groups having 7 to 30 carbon atoms represented by benzyl, α-methylbenzyl, α,α-dimethylbenzyl, phenylethyl, etc.

[0110] R in the above general formula (A) 3 , R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Examples of complex groups having 2 to 20 carbon atoms represented by syl, such as pyridyl, pyrimidyl, furyl, thienyl, tetrahydrofuryl, dioxoranyl, benzoxazole-2-yl, tetrahydropyranyl, pyrrolidyl, imidazolidyl, pyrazolidyl, thiazolidyl, isothiazolidyl, oxazolidyl, isooxazolidyl, piperidyl, piperazyl, morpholinyl, and 5 to 7 complex groups.

[0111] R in the above general formula (A) 4 and R 5 , R 5 and R 6 and R 6 and R 7 , and R 3 and R 7 and R 3 and R 8 As for the rings that can be formed as one, 5 to 7-membered rings such as cyclopentane, cyclohexane, cyclopentene, benzene, piperidine, morpholine, lactone, and lactam rings are preferably cited.

[0112] In addition, R in the above general formula (A). 4 , R 5 , R 6 , R 7 and R 8A halogen atom represented by, and R in the above general formula (A). 3 , R 11 , R 12 , R 13 , R 21 , R 22 and R 23 Examples of halogen atoms that can be substituted include fluorine, chlorine, bromine, and iodine.

[0113] R in the above general formula (A) 11 , R 12 , R 13 , R 21 , R 22 and R 23 The alkylene portion of the group represented by -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 -, -SCO-, -COS-, -OCS-, or -CSO- may be included in 1 to 5 groups under the condition that oxygen atoms are not adjacent, and the divalent groups included may be of one or more than two types, and in the case of groups that can be included consecutively, two or more groups may be included consecutively.

[0114] In addition, R in the above general formula (A). 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The alkyl (alkylene) portion of the group represented by may have a branched side chain and may be a cyclic alkyl.

[0115] Among the compounds represented by the above general formula (A), R 3 An aromatic ring that is condensed, or a compound represented by the following general formula (A'), is desirable because it has high sensitivity and is easy to manufacture.

[0116]

[0117] (during food, R 1 , R 2 , R 4 , R 5 , R 6 , R 7 , R 8 and k are the same as the above general formula (A), and R 31 , R 32 , R 33 , R 34 and R 35 are each independently R 11 , OR 11 , SR 11 , COR 11 , CONR 15 R 16 , NR 12 COR 11 , OCOR 11 , COOR 14 , SCOR 11 , OCSR 11 , COSR 14 , CSOR 11 , representing a hydroxyl group, nitro group, CN, or halogen atom, and R 31 and R 32 , R 32 and R 33 , R 33 and R 34 and R 34 and R 35 Each may become one to form a ring.)

[0118] R 31 and R 32 , R 32 and R 33 , R 33 and R 34 and R 34 and R 35 As an example of a ring formed by becoming one, R 4 and R 5 , R 5 and R 6 and R 6 and R 7 , and R 3 and R 7 and R 3 and R8 As a ring that can be formed as one, a ring like the one exemplified above can be cited.

[0119] In the above general formulas (A) and (A'), R 1 As a carbon 1- to 12 alkyl group or carbon 7- to 15 arylalkyl group, R 11 It is preferable that this is an aryl group having 6 to 12 carbon atoms or an alkyl group having 1 to 8 carbon atoms because of its high solvent solubility, and R 2 As it is preferred to be a methyl group, an ethyl group, or a phenyl group due to high reactivity, and R 4 ~R 7 As a hydrogen atom or a cyano group, particularly a hydrogen atom, is preferred because it is easy to synthesize, and R 8 It is preferable that it be a hydrogen atom because synthesis is easy, and it is preferable that k is 1 because sensitivity is high, and in the above general formula (A'), R 31 ~R 35 At least one of which is a nitro group, CN, a halogen atom, or COR 11 and R 11 It is preferable that this is an aryl group having 6 to 12 carbon atoms or an alkyl group having 1 to 8 carbon atoms because of the high sensitivity, and R 31 ~R 35 It is more preferable that at least one of them is a nitro group, CN, or a halogen atom, and R 33 It is particularly desirable that this be a nitro group, CN, or halogen atom.

[0120] Preferred specific examples of the compound represented by the above general formula (A) include, for instance, the following compounds. Additionally, compounds No. 1 to No. 212 described in International Publication No. 2015 / 152153 may be cited.

[0121]

[0122] The compound represented by the above general formula (A) can be synthesized by appropriately selecting the solvent, reaction temperature, reaction time, purification method, etc., depending on the material used, for example by referring to International Publication No. 2015 / 152153. Alternatively, commercially available products may be appropriately obtained and used.

[0123] (Compound represented by general formula (B))

[0124] Although geometric isomers formed by the double bond of the oxime exist in the oxime ester compound represented by the above general formula (B), they are not distinguished. That is, in this specification, the compound represented by the above general formula (B) and the exemplary compounds thereof represent a mixture of both or either one, and are not limited to structures representing isomers.

[0125] X in the above general formula (B) 2 , R 41 , R 42 , R 43 , R 51 , R 52 , R 53 and R 54 Examples of alkyl groups having 1 to 20 carbon atoms represented by can be the same as the alkyl group having 1 to 20 carbon atoms in the general formula (A) above.

[0126] X in the above general formula (B) 2 , R 41 , R 42 , R 43 , R 51 , R 52 , R 53 and R 54 Examples of aryl groups having 6 to 30 carbon atoms represented by can be aryl groups having 6 to 30 carbon atoms in the above general formula (A).

[0127] X in the above general formula (B) 2 , R 41 , R 42 , R 43 , R 51 , R52 , R 53 and R 54 Examples of arylalkyl groups having 7 to 30 carbon atoms represented by can be arylalkyl groups having 7 to 30 carbon atoms in the above general formula (A).

[0128] X in the above general formula (B) 2 , R 41 , R 42 , R 43 , R 51 , R 52 , R 53 and R 54 Examples of complex radii with 2 to 20 carbon atoms represented by can be complex radii with 2 to 20 carbon atoms in the above general formula (A).

[0129] In addition, the halogen atom in the above general formula (B) can be the same as the halogen atom in the above general formula (A).

[0130] R in the above general formula (B). 41 , R 42 , R 43 , X 2 , R 51 , R 52 and R 53 The alkylene portion of the group represented by is -O-, -S-, -COO-, -OCO-, -NR 54 -, -NR 54 CO-, -NR 54 COO-, -OCONR 54 It may include 1 to 5 groups of -, -SCO-, -COS-, -OCS-, or -CSO- under conditions where oxygen atoms are not adjacent, and the divalent groups included may be of one or more than two types, and in the case of groups that can be included consecutively, two or more may be included consecutively.

[0131] X in the above general formula (B) 1More preferably, in terms of sensitivity, solubility, and compatibility, it is an alkyl group having 1 to 10 carbon atoms, such as a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, t-butyl group, n-amyl group, isoamyl group, t-amyl group, n-hexyl group, and 2-ethylhexyl group; a cyclic alkyl group having 5 to 10 carbon atoms, such as a cyclopentyl group and a cyclohexyl group; or an alkyl group having one ether bond in a methylene chain having 2 to 10 carbon atoms, such as a methoxymethyl group, ethoxymethyl group, ethoxyethyl group, 2-(1-methoxypropyl) group, and 2-(1-ethoxypropyl) group; and more preferably, an alkyl group having 1 to 10 carbon atoms, such as a methyl group, ethyl group, or 2-ethylhexyl group.

[0132] X in the above general formula (B) 2 , X 3 and X 6 Each is, in terms of sensitivity, solubility, and compatibility, particularly preferably an alkyl group having 1 to 6 carbon atoms such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-amyl group, an isoamyl group, a t-amyl group, and an n-hexyl group, a cyclic alkyl group having 5 to 6 carbon atoms such as a cyclopentyl group and a cyclohexyl group, or an alkyl group having 2 to 6 carbon atoms such as a methoxymethyl group, an ethoxymethyl group, an ethoxyethyl group, a 2-(1-methoxypropyl) group and a 2-(1-ethoxypropyl) group, and also having one ether bond in a methylene chain, and more preferably an alkyl group having 1 to 6 carbon atoms or an alkyl group having 2 to 6 carbon atoms and one ether bond in a methylene chain.

[0133] X 3 and X 6 Each is independently an alkyl group having 1 to 6 carbon atoms, which is more preferably in terms of sensitivity, solubility, and compatibility.

[0134] X 2 It is an alkyl group having one ether bond in a methylene chain having 2 to 6 carbon atoms, which is more preferably in terms of sensitivity, solubility, and compatibility.

[0135] X in the above general formula (B) 4 and X 5 Each is, in terms of sensitivity, solubility, and compatibility, particularly preferably hydrogen, or an alkyl group having 1 to 6 carbon atoms, such as a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, t-butyl group, n-amyl group, isoamyl group, t-amyl group, and n-hexyl group.

[0136] Preferred specific examples of the compound represented by the above general formula (B) include, for instance, the following compounds.

[0137]

[0138]

[0139] The compound represented by the above general formula (B) can be synthesized by appropriately selecting the solvent, reaction temperature, reaction time, purification method, etc., depending on the material used, for example by referring to Japanese Patent Publication No. 2010-256891. Alternatively, commercially available products may be appropriately obtained and used.

[0140] The total content of the photoinitiator used in the photocurable red resin composition of the present invention is not particularly limited as long as it does not impair the effects of the present invention, but is preferably within the range of 0.1 mass% to 15.0 mass% and more preferably 1.0 mass% to 10.0 mass% with respect to the total solid content of the photocurable red resin composition. If this content is above the lower limit, sufficient photocuring proceeds easily, and solvent resistance and substrate adhesion are easily improved; on the other hand, if it is below the upper limit, line width shift is suppressed, making it easy to form high-precision patterns.

[0141] The total content of at least one compound represented by the general formula (A) and the compound represented by the general formula (B) is preferably 30.0 mass% or more, more preferably 50.0 mass% or more, and even more preferably 70.0 mass% or more with respect to the total amount of photoinitiator, in that it is possible to form a cured film with good substrate adhesion and solvent resistance even in low-temperature heat treatment.

[0142] The photocurable red resin composition according to the present invention contains a colorant, a photopolymerizable compound, and a photoinitiator. By using a liquid photopolymerizable compound, a coating film can be formed without containing a solvent, and a patterned colored layer can be formed by using a means of applying in a patterned manner, such as an inkjet method.

[0143] The photocurable red resin composition according to the present invention may also be a photocurable red resin composition containing an alkali-soluble resin and a solvent, and having alkali-developable properties.

[0144] Alkali-soluble resin

[0145] The alkali-soluble resin used in the present invention may be appropriately selected from those having acidic groups, acting as a binder resin, and being soluble in the alkaline developer used when forming a pattern.

[0146] In the present invention, alkali-soluble resin may be defined based on having an acid value of 40 mgKOH / g or higher.

[0147] As for the alkali-soluble resin, conventionally known alkali-soluble resins can be appropriately selected and used, for example, an alkali-soluble resin described in International Publication No. 2016 / 104493 can be appropriately selected and used.

[0148] The preferred alkali-soluble resin in the present invention is a resin having an acidic group, typically a carboxyl group. Specifically, examples include (meth)acrylic resins such as (meth)acrylic copolymers having a carboxyl group and styrene-(meth)acrylic copolymers having a carboxyl group, and epoxy (meth)acrylate resins having a carboxyl group. (meth)acrylic resins such as (meth)acrylic copolymers having a carboxyl group and styrene-(meth)acrylic copolymers having a carboxyl group are suitably used. Among these, particularly preferred is one having a carboxyl group in a side chain and additionally having a photopolymerizable functional group, such as an ethylenically unsaturated group, in a side chain. This is because the film strength of the cured film formed by containing the photopolymerizable functional group is improved. In addition, these (meth)acrylic copolymers, (meth)acrylic resins such as styrene-(meth)acrylic copolymers, and epoxy (meth)acrylate resins may be used in a mixture of two or more types.

[0149] The alkali-soluble resin used in the photocurable red resin composition may be used as a single type or in combination of two or more types. There is no particular limit on the content of the alkali-soluble resin, but it is preferably within the range of 5 mass% to 60 mass%, more preferably 10 mass% to 40 mass%, with respect to the total solid content of the photocurable red resin composition. If the content of the alkali-soluble resin is above the above lower limit, sufficient alkali developability is obtained, and if the content of the alkali-soluble resin is below the above upper limit, film roughness or pattern loss can be suppressed during development.

[0150] Solvent

[0151] The solvent used in the present invention may be any organic solvent that does not react with each component of the photocurable red resin composition and can dissolve or disperse them, and is not particularly limited. The solvent may be used alone or in combination of two or more types.

[0152] Specific examples of solvents include alcohol-based solvents such as methyl alcohol, ethyl alcohol, N-propyl alcohol, i-propyl alcohol, methoxy alcohol, and ethoxy alcohol; carbitol-based solvents such as methoxyethoxyethanol and ethoxyethoxyethanol; ester-based solvents such as ethyl acetate, butyl acetate, methyl methoxypropionate, ethyl methoxypropionate, ethyl ethoxypropionate, ethyl lactate, methyl hydroxypropionate, ethyl hydroxypropionate, n-butyl acetate, isobutyl acetate, isobutyl butyrate, n-butyl butyrate, ethyl lactate, and cyclohexanol acetate; and ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and 2-heptanone. Glycol ether acetate-based solvents such as methoxyethyl acetate, propylene glycol monomethyl ether acetate, 3-methoxy-3-methyl-1-butyl acetate, 3-methoxybutyl acetate, ethoxyethyl acetate; carbitol acetate-based solvents such as methoxyethoxyethyl acetate, ethoxyethoxyethyl acetate, and butyl carbitol acetate (BCA); diacetates such as propylene glycol diacetate and 1,3-butylene glycol diacetate; glycol ether-based solvents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, and dipropylene glycol dimethyl ether; Examples include aprotic amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; lactone solvents such as γ-butyrolactone; cyclic ether solvents such as tetrahydrofuran; unsaturated hydrocarbon solvents such as benzene, toluene, xylene, and naphthalene; saturated hydrocarbon solvents such as N-heptane, N-hexane, and N-octane; and organic solvents such as aromatic hydrocarbons such as toluene and xylene. Among these solvents, glycol ether acetate solvents, carbitol acetate solvents, glycol ether solvents, and ester solvents are suitablely used in terms of solubility of other components.Among these, as a solvent used in the present invention, it is preferable to use one or more selected from the group consisting of propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, butyl carbitol acetate (BCA), 3-methoxy-3-methyl-1-butyl acetate, ethyl ethoxypropionate, ethyl lactate, and 3-methoxybutyl acetate in terms of the solubility of other components and suitability for application.

[0153] In the photocurable red resin composition according to the present invention, the solvent content may be appropriately set within a range that allows for the precise formation of a colored layer. The solvent content is typically preferably within the range of 55 mass% to 95 mass%, more preferably 65 mass% to 88 mass%, with respect to the total amount of the photocurable red resin composition containing the solvent. By having the solvent content within the above range, excellent coating properties can be achieved.

[0154] Dispersant

[0155] In the photocurable red resin composition of the present invention, when dispersing a colorant, a dispersant may be additionally included in terms of colorant dispersibility and colorant dispersion stability.

[0156] In the present invention, the dispersant may be appropriately selected from conventionally known dispersants. As the dispersant, surfactants such as cationic, anionic, nonionic, amphoteric, silicone-based, and fluorine-based surfactants may be used. Among surfactants, polymeric dispersants are preferred in that they can be dispersed uniformly and finely.

[0157] Examples of polymer dispersants include (meth)acrylate copolymer dispersants; polyurethanes; unsaturated polyamides; polysiloxanes; long-chain polyaminoamide phosphates; polyethyleneimine derivatives (amides or bases thereof obtained by reacting poly(lower alkyleneimine) with a polyester containing a free carboxyl group); polyallylamine derivatives (reaction products obtained by reacting polyallylamine with one or more compounds selected from three types of compounds: a polyester having a free carboxyl group, a polyamide, or a cocondensate of an ester and an amide (polyesteramide)).

[0158] In the present invention, it is preferable to use a (meth)acrylate copolymer-based dispersant as a dispersant because it facilitates good solvent resistance even during low-temperature heat treatment. Since the (meth)acrylate copolymer-based dispersant has good compatibility with the photopolymerizable compound and at least one photoinitiator of the compound represented by general formula (A) and the compound represented by general formula (B), the initiator is easily present uniformly in the colored layer, and as the colored layer is uniformly cured, unreacted components are reduced and the internal stress of the colored layer is reduced, so it is presumed that the change in the colored layer when immersed in a solvent is reduced.

[0159] In the present invention, the term (meth)acrylate copolymer dispersant refers to a dispersant that is a copolymer and comprises at least a constituent unit derived from (meth)acrylate.

[0160] It is preferable that the (meth)acrylate copolymer dispersant be a copolymer containing a constituent unit that functions as a colorant adsorption site and a constituent unit that functions as a solvent affinity site, and it is preferable that the constituent unit that functions as a solvent affinity site includes at least a constituent unit derived from (meth)acrylate.

[0161] The constituent units that function as color adsorption sites include constituent units derived from (meth)acrylates and constituent units derived from copolymerizable ethylenically unsaturated monomers. As color adsorption sites, constituent units derived from acidic group-containing ethylenically unsaturated monomers may also be constituent units derived from basic group-containing ethylenically unsaturated monomers.

[0162] As a constituent unit derived from an ethylenically unsaturated monomer containing a basic group, a constituent unit represented by the following general formula (I) is preferred in that it has excellent dispersibility.

[0163]

[0164] (of general formula (I), R 71 A hydrogen atom or a methyl group, A 1 is a divalent connector, R 72 and R 73 Each represents a hydrocarbon group that may independently contain a hydrogen atom or a heteroatom, and R 72 and R 73 These may combine to form a ring structure.

[0165] In general formula (I), A 1 ... is a divalent linker. Examples of divalent linkers include straight-chain, branched, or cyclic alkylene groups, straight-chain, branched, or cyclic alkylene groups having hydroxyl groups, arylene groups, -CONH- groups, -COO- groups, -NHCOO- groups, ether groups (-O- groups), thioether groups (-S- groups), and combinations thereof. Furthermore, in the present invention, the bonding direction of the divalent linker is optional. That is, when -CONH- is included in the divalent linker, -CO may be on the side of the carbon atom of the main chain and -NH may be on the side of the nitrogen atom of the side chain, or conversely, -NH may be on the side of the carbon atom of the main chain and -CO may be on the side of the nitrogen atom of the side chain.

[0166] In particular, regarding dispersion, A in general formula (I) 1It is preferable that the linker be a divalent linker including a -CONH- group or a -COO- group, and more preferable that the linker be a divalent linker including a -CONH- group or a -COO- group and an alkylene group having 1 to 10 carbon atoms.

[0167] R 72 and R 73 In the case of hydrocarbon groups that may include heteroatoms, examples of hydrocarbon groups include alkyl groups, aralkyl groups, aryl groups, etc.

[0168] Examples of alkyl groups include methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2-ethylhexyl, cyclopentyl, and cyclohexyl groups, and the number of carbon atoms in the alkyl group is preferably 1 to 18, and among these, it is more preferable that it be a methyl or ethyl group.

[0169] Examples of aralkyl groups include benzyl groups, phenethyl groups, naphthylmethyl groups, biphenylmethyl groups, etc. The number of carbon atoms in the aralkyl group is preferably 7 to 20, and more preferably 7 to 14.

[0170] In addition, examples of aryl groups include phenyl groups, biphenyl groups, naphthyl groups, tolyl groups, xylyl groups, etc. The number of carbon atoms in the aryl group is preferably 6 to 24, and more preferably 6 to 12. In addition, the number of carbon atoms of the substituents is not included in the above-mentioned preferred number of carbon atoms.

[0171] A hydrocarbon group containing heteroatoms has a structure in which a carbon atom in the hydrocarbon group is substituted with a heteroatom, or a hydrogen atom in the hydrocarbon group is substituted with a substituent containing a heteroatom. Examples of heteroatoms that may be included in the hydrocarbon group include oxygen atoms, nitrogen atoms, sulfur atoms, silicon atoms, etc.

[0172] In addition, hydrogen atoms in the hydrocarbon group may be substituted with halogen atoms such as fluorine atoms, chlorine atoms, or bromine atoms.

[0173] R72 and R 73 The fact that they combine with each other to form a ring structure is, R 72 and R 73 It refers to the formation of a ring structure through this nitrogen atom. R 72 and R 73 The ring structure formed may include heteroatoms. The ring structure is not particularly limited, but examples include pyrrolidine rings, piperidine rings, and morpholine rings.

[0174] In the present invention, among them, R 72 and R 73 Each of these is independently a hydrogen atom, a C1- to C5 alkyl group, a phenyl group, or R 72 and R 73 It is desirable that these combine to form a pyrrolidine ring, a piperidine ring, and a morpholine ring.

[0175] As monomers that derive the constituent unit represented by the above general formula (I), examples include alkyl group-substituted amino group-containing (meth)acrylates such as dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and diethylaminopropyl (meth)acrylate, and alkyl group-substituted amino group-containing (meth)acrylamides such as dimethylaminoethyl (meth)acrylamide and dimethylaminopropyl (meth)acrylamide. Among these, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylaminopropyl (meth)acrylamide can be preferably used in that dispersibility and dispersion stability are improved.

[0176] In the polymer, the constituent unit represented by the general formula (I) may consist of one type or may include two or more types of constituent units.

[0177] In addition, as a constituent unit functioning as a color adsorption site, at least one of the nitrogen portions of the constituent unit represented by the general formula (I) and at least one type selected from the group consisting of organic acid compounds and halogenated hydrocarbons may form a salt (hereinafter, such a copolymer may be referred to as a salt-type copolymer).

[0178] Among the above organic acid compounds, compounds represented by the following general formula (1) and compounds represented by the following general formula (3) are preferred, and among the above halogenated hydrocarbons, compounds represented by the following general formula (2) are preferred. That is, among at least one selected from the group consisting of the above organic acid compounds and halogenated hydrocarbons, one or more compounds selected from the group consisting of the following general formulas (1) to (3) can be preferably used.

[0179]

[0180] (In general formula (1), R a ...a straight-chain, branched-chain, or cyclic alkyl group having 1 to 20 carbon atoms, a vinyl group, a phenyl group or benzyl group that may have a substituent, or -OR e Represents, and R e represents a straight-chain, branched-chain, or cyclic alkyl group having 1 to 20 carbon atoms, a vinyl group, a phenyl group or benzyl group which may have a substituent, or a (meth)acryloyl group through an alkylene group having 1 to 4 carbon atoms. In general formula (2), R b , R b' and R b" Each independently a hydrogen atom, an acidic group or its ester group, a straight-chain, branched-chain, or cyclic alkyl group having 1 to 20 carbon atoms, which may have substituents, a vinyl group, which may have substituents, a phenyl or benzyl group, which may have substituents, or -OR f Represents, and R frepresents a straight-chain, branched-chain, or cyclic alkyl group having 1 to 20 carbon atoms, which may have substituents; a vinyl group having substituents; a phenyl or benzyl group having substituents; or a (meth)acryloyl group through an alkylene group having 1 to 4 carbon atoms, which may have substituents; and X represents a chlorine atom, a bromine atom, or an iodine atom. In general formula (3), R c and R d Each independently comprises a hydrogen atom, a hydroxyl group, a straight-chain, branched-chain, or cyclic alkyl group having 1 to 20 carbon atoms, a vinyl group, a phenyl group or benzyl group that may have a substituent, or -OR e Represents, and R e represents a straight-chain, branched-chain, or cyclic alkyl group having 1 to 20 carbon atoms, a vinyl group, a phenyl or benzyl group that may have a substituent, or a (meth)acryloyl group through an alkylene group having 1 to 4 carbon atoms. provided that R c and R d At least one of them contains a carbon atom.)

[0181] Regarding each of the symbols in the above general formulas (1) to (3), they may be the same as those described in International Publication No. 2016 / 104493.

[0182] It is preferable that the above organic acid compound is an acidic organic phosphorus compound such as phenylphosphonic acid or phenylphosphinic acid, as this provides excellent dispersibility and dispersion stability of the colorant. Specific examples of organic acid compounds used in such dispersants include organic acid compounds described in Japanese Patent Publication No. 2012-236882, etc.

[0183] In addition, the above-mentioned halogenated hydrocarbon is preferably at least one of allyl halides and aryl halides, such as allyl bromide and benzyl chloride, in that the dispersibility and dispersion stability of the colorant are excellent.

[0184] In the salt-type copolymer, since the content of at least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons forms a salt with the terminal nitrogen portion of the constituent unit represented by general formula (I), it is preferable to have a total of at least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons with respect to the terminal nitrogen portion of the constituent unit represented by general formula (I) of 0.01 mole or more, more preferable to have 0.05 mole or more, even more preferable to have 0.1 mole or more, and particularly preferable to have 0.2 mole or more. If it is above the lower limit, it is easy to obtain the effect of improving the dispersibility of the colorant due to salt formation. Likewise, it is preferable to have 1 mole or less, more preferable to have 0.8 mole or less, even more preferable to have 0.7 mole or less, and particularly preferable to have 0.6 mole or less. If it is below the upper limit, it can be made that the developing adhesion and solvent redissolvability are excellent.

[0185] In addition, at least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons may be used alone or in combination of two or more. When two or more are combined, it is preferable that the total content be within the above range.

[0186] As a method for preparing a salt-type copolymer, examples include adding at least one selected from the group consisting of the organic acid compound and the halogenated hydrocarbon to a solvent in which the copolymer before salt formation is dissolved or dispersed, stirring, and heating if necessary.

[0187] In addition, the fact that the terminal nitrogen portion of the constituent unit represented by the general formula (I) of the copolymer and at least one type selected from the group consisting of the organic acid compound and the halogenated hydrocarbon forms a salt, and the ratio thereof, can be confirmed by known methods such as NMR.

[0188] In terms of dispersibility and dispersion stability, the copolymer having a constituent unit represented by the above general formula (I) is more preferably at least one of a graft copolymer having a constituent unit represented by the above general formula (I) and a constituent unit of (meth)acrylate in the graft polymer chain, and a block copolymer having an A block containing a constituent unit represented by the above general formula (I) and a B block containing a constituent unit of (meth)acrylate.

[0189] Hereinafter, the graft copolymer and the block copolymer will be described sequentially.

[0190] As a graft copolymer having a constituent unit represented by the above general formula (I) and having a constituent unit derived from (meth)acrylate in the graft polymer chain, examples include a graft copolymer having a constituent unit represented by the above general formula (I) and a constituent unit represented by the following general formula (II), and at least one salt-type graft copolymer in which at least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons forms a salt with at least a portion of the nitrogen portion of the constituent unit represented by the above general formula (I) of the graft copolymer.

[0191]

[0192] (of general formula (II), R 71' is a hydrogen atom or a methyl group, A 2 represents a direct bond or a divalent linker, Polymer represents a polymer chain, and the constituent units of the polymer chain include constituent units derived from (meth)acrylate.

[0193] In the above general formula (II), A 2 is a direct coupling or a bivalent connector. A 2As for the divalent linker in [the case], there are no particular restrictions as long as it is capable of connecting a carbon atom derived from an ethylenically unsaturated double bond to a polymer chain. A 2 As a two-way connector in the case, for example, the above A 1 Examples include the two-way connector in this case.

[0194] In particular, regarding dispersion, A in general formula (II) 2 It is preferable that the linker is a divalent linker comprising a -CONH- group or a -COO- group, and more preferable that the linker is a divalent linker comprising a -CONH- group or a -COO- group and an alkylene group having 1 to 10 carbon atoms.

[0195] In the above general formula (II), the polymer represents a polymer chain, and the constituent unit of this polymer chain includes a constituent unit derived from (meth)acrylate. By having a constituent unit represented by the above general formula (II) having a specific polymer chain, the graft copolymer has good solvent affinity, good dispersibility and dispersion stability of the colorant, and also good compatibility with the photoinitiator described above.

[0196] As constituent units of the above polymer chain, constituent units represented by the following general formula (III) may be used.

[0197]

[0198] (of general formula (III), R 74" is a hydrogen atom or a methyl group, A 4 is a divalent connector, R 80 It is a hydrocarbon group that may contain hydrogen atoms or heteroatoms.

[0199] A 4 As a two-way connector of, for example, the above A 1 Examples include divalent linkers in [the case]. In the present invention, as a constituent unit derived from (meth)acrylate, A of general formula (III)4 At least one constituent unit represented by general formula (III), which is a divalent linker containing a -COO- group, is included. In terms of solubility in organic solvents used for color filter applications, A in general formula (III) 4 It may include a divalent connector containing a -CONH- group.

[0200] R 80 In the above, the hydrocarbon group that may include heteroatoms can be, for example, an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkyl-substituted aryl group, or combinations thereof. R 80 Examples of hydrocarbon groups that may include heteroatoms include, for instance, alkyl groups having 1 to 18 carbon atoms, alkenyl groups having 2 to 18 carbon atoms, aryl groups, aralkyl groups, or combinations thereof such as alkyl-substituted aryl groups.

[0201] The above alkyl group having 1 to 18 carbon atoms may be straight-chain, branched, or cyclic, and examples include methyl, ethyl, n-propyl, isopropyl, n-butyl, n-nonyl, n-lauryl, n-stearyl, cyclopentyl, cyclohexyl, bornyl, isobornyl, dicyclofentanyl, adamantyl, lower alkyl-substituted adamantyl groups, etc. The number of carbon atoms in the alkyl group is preferably 1 to 12, and more preferably 1 to 6.

[0202] The above alkenyl group having 2 to 18 carbon atoms may be linear, branched, or cyclic. Examples of such alkenyl groups include vinyl groups, allyl groups, propenyl groups, etc. Although there is no limitation on the position of the double bond of the alkenyl group, it is preferable for the double bond to be located at the end of the alkenyl group in terms of the reactivity of the obtained polymer. The number of carbon atoms in the alkenyl group is preferably 2 to 12, and more preferably 2 to 8.

[0203] Examples of aryl groups include phenyl groups, biphenyl groups, naphthyl groups, tolyl groups, xylyl groups, etc. The number of carbon atoms in the aryl group is preferably 6 to 24, and more preferably 6 to 12.

[0204] In addition, examples of aralkyl groups include benzyl groups, phenethyl groups, naphthylmethyl groups, biphenylmethyl groups, etc., and may additionally have substituents. The number of carbon atoms in the aralkyl group is preferably 7 to 20, and more preferably 7 to 14.

[0205] In addition, a straight-chain or branched alkyl group having 1 to 30 carbon atoms may be bonded as a substituent to the aromatic ring, such as the aryl group or aralkyl group.

[0206] R 80 As for the hydrocarbon group in the above, in particular, in terms of dispersion stability, it is preferable to have one or more selected from the group consisting of an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 12 carbon atoms that may be substituted with an alkyl group, and an aralkyl group having 7 to 14 carbon atoms that may be substituted with an alkyl group, and it is preferable to have one or more selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an n-nonyl group, an n-lauryl group, an n-stearyl group, a phenyl group that may be substituted with an alkyl group, and a benzyl group.

[0207] Examples of heteroatoms that may be included in a hydrocarbon group include oxygen atoms, nitrogen atoms, sulfur atoms, silicon atoms, etc. Examples of hydrocarbon groups that may include heteroatoms include structures in which linking groups such as -CO-, -COO-, -OCO-, -O-, -S-, -CO-S-, -S-CO-, -O-CO-O-, -CO-NH-, -NH-CO-, -OCO-NH-, -NH-COO-, -NH-CO-NH-, -NH-O-, -O-NH- are included in the carbon chain of the hydrocarbon group.

[0208] In addition, the hydrocarbon group may have substituents within a range that does not interfere with the dispersion performance of the graft copolymer, and examples of substituents include halogen atoms, hydroxyl groups, carboxyl groups, alkoxy groups, nitro groups, cyano groups, epoxy groups, isocyanate groups, thiol groups, etc.

[0209] Also, R 80 As for the hydrocarbon group that may include a heteroatom, it may be a structure in which a polymerizable group, such as an alkenyl group, is added to the terminal end through a linker containing a heteroatom in the hydrocarbon group. For example, the constituent unit represented by general formula (III) may be a structure such as one in which glycidyl (meth)acrylate is reacted with a constituent unit derived from (meth)acrylic acid. That is, -A in general formula (III) 4 -R 80 The structure may be represented as -COO-CH2CH(OH)CH2-OCO-CR=CH2 (where R is a hydrogen atom or a methyl group). Additionally, the constituent unit represented by general formula (III) may be a structure obtained by reacting a 2-isocyanatoalkyl (meth)acrylate with a constituent unit derived from a hydroxyalkyl (meth)acrylate. That is, R in general formula (III). 80 This structure may also be represented as -R'-OCONH-R"-OCO-CR=CH2 (where R' and R" are each independently an alkylene group, R is a hydrogen atom or a methyl group).

[0210] As monomers deriving the constituent unit represented by general formula (III), for example, methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, dicyclofentanyl (meth)acrylate, adamanthyl (meth)acrylate, (meth)acrylic acid, 2-methacryloyloxyethylsuccinate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, It is preferable to have constituent units derived from 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, phenoxyethyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate, phenoxyethylene glycol (meth)acrylate, etc. However, it is not limited to these.

[0211] In the present invention, the above R 80 Among these, it is preferable to use one that has excellent solubility with the organic solvent described below, and it should be appropriately selected to match the organic solvent used in the colorant dispersion. Specifically, for example, when the above organic solvent is an organic solvent such as an ether alcohol acetate system, ether system, ester system, or alcohol system that is generally used as an organic solvent for the colorant dispersion, methyl group, ethyl group, isobutyl group, n-butyl group, 2-ethylhexyl group, benzyl group, cyclohexyl group, dicyclofentanyl group, hydroxyethyl group, phenoxyethyl group, adamantyl group, methoxypolyethylene glycol group, methoxypolypropylene glycol group, polyethylene glycol group, etc. are preferred.

[0212] The above graft copolymer is preferably configured such that, in the polymer chain constituent unit of the constituent unit represented by the above general formula (II), at least one constituent unit selected from the group consisting of the constituent unit represented by the following general formula (IV) and the constituent unit represented by the following general formula (IV'), the solvent resistance of the cured product of the photocurable red resin composition is further improved, and the development time of the photocurable red resin composition is shortened.

[0213] The constituent unit represented by the following general formula (IV) and the constituent unit represented by the following general formula (IV') are constituent units included in the constituent unit represented by the above general formula (III).

[0214]

[0215] (of general formula (IV), R 74 is a hydrogen atom or a methyl group, A 3 is a divalent connector, R 75 is an ethylene group or a propylene group, R 76 is a hydrogen atom or a hydrocarbon group, and m represents a number between 3 and 80.

[0216] Among the general formula (IV'), R 74' is a hydrogen atom or a methyl group, A 3' is a divalent connector, R 77 is an alkylene group having 1 to 10 carbon atoms, R 78 is an alkylene group having 3 to 7 carbon atoms, R 79 is a hydrogen atom or a hydrocarbon group, and n represents a number between 1 and 40.

[0217] A 3 As a two-way connector of, for example, the above A 1 Examples include the divalent linker in [the case]. Among these, in terms of solubility in organic solvents used for color filter applications, A in general formula (IV) 3It is preferable that the linker is a divalent linker including a -CONH- group or a -COO- group, more preferable that it is a -CONH- group or a -COO- group, and even more preferable that it is a -COO- group.

[0218] The above m represents the number of repeating units of an ethylene oxide chain or a propylene oxide chain, and represents a number of 3 or more, but among them, it is preferable that it be 19 or more and more preferable that it be 21 or more in terms of suppressing water stains and solvent resistance.

[0219] When the above m is 19 or greater, the graft copolymer contains a main chain portion having a constituent unit represented by general formula (I) and a constituent unit represented by general formula (II), and the constituent unit represented by general formula (II) includes a constituent unit represented by general formula (IV) which includes a polyethylene oxide chain or a polypropylene oxide chain having a specific number of repetitions in the polymer chain. In the specific graft copolymer used in the present invention, the constituent unit of the polymer chain grafted in this way includes a constituent unit having a polyethylene oxide chain or a polypropylene oxide chain having a specific number of repetitions, and the grafted polymer chain itself has a branched structure. It is presumed that the penetration of solvent into the coating film or the reaching of the colorant can be further suppressed because the multiple grafted polymer chains expand three-dimensionally within the film and the specific surface area increases.

[0220] Meanwhile, the upper limit of m is 80 or less, but it is preferable that it be 50 or less in terms of solubility in organic solvents used for color filters.

[0221] R 76 The hydrocarbon group in is the above R 80 It may be the same as the hydrocarbon group in.

[0222] R 76As for the hydrocarbon group in the above, in terms of dispersion stability and compatibility, it is preferable to have one or more selected from the group consisting of an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 12 carbon atoms that may be substituted with an alkyl group, and an aralkyl group having 7 to 14 carbon atoms that may be substituted with an alkyl group, and it is preferable to have one or more selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an n-nonyl group, an n-lauryl group, an n-stearyl group, a phenyl group that may be substituted with an alkyl group, and a benzyl group.

[0223] In addition, among the above general formula (IV'), A 3' As a two-way connector of, for example, the above A 1 Examples include divalent linkers in this case. In particular, regarding solubility in organic solvents used for color filter applications, A in general formula (IV') 3' It is preferable that it be a divalent linker including a -CONH- group or a -COO- group, more preferable that it be a -CONH- group or a -COO- group, and even more preferable that it be a -COO- group.

[0224] In the above general formula (IV'), R 77 The group is an alkylene group having 1 to 10 carbon atoms, but among them, an alkylene group having 2 to 8 carbon atoms is preferred in terms of solvent redissolvability.

[0225] R 78 It is an alkylene group having 3 to 7 carbon atoms, but among them, it is preferable to have an alkylene group having 3 to 5 carbon atoms, and additionally an alkylene group having 5 carbon atoms, in terms of adhesion to the substrate.

[0226] R 79 is a hydrogen atom or a hydrocarbon group, and the above R 79 The hydrocarbon group in is the above R 76 It may be the same as the hydrocarbon group in.

[0227] In the above general formula (IV'), n represents the number of repeating units of the ester chain and represents a number of 1 or more, but among them, it is preferable that it be 2 or more and more preferable that it be 3 or more in order to simultaneously satisfy shortening of the development time and excellent solvent resistance.

[0228] Meanwhile, the upper limit of n is 40 or less, but it is preferable that it be 20 or less in terms of solubility in organic solvents used for color filters.

[0229] In the above polymer chain, at least one constituent unit selected from the group consisting of the constituent unit represented by the above general formula (IV) and the constituent unit represented by the following general formula (IV') may be one type alone, or two or more types may be mixed.

[0230] In the above polymer chain, it is preferable to include a constituent unit represented by the general formula (IV) so that the action of the solvent affinity part by the oxygen atom becomes more pronounced, and the development time of the photocurable red resin composition is shortened and the solvent resistance is improved.

[0231] In particular, in that the solvent resistance is improved, the water stain suppression effect is improved, and the development residue suppression effect is also improved, it is more preferable to include a combination of at least one selected from the group of constituent units represented by the general formula (IV) having a m of 19 or more and 80 or less, and at least one selected from the group of constituent units represented by the general formula (IV) having a m of 3 or more and 10 or less, in the polymer chain constituent unit represented by the general formula (II) above, in that m is improved, and m is improved. It is even more preferable to include a combination of at least one selected from the group of constituent units represented by the general formula (IV) having a m of 19 or more and 50 or less, and at least one selected from the group of constituent units represented by the general formula (IV) having a m of 3 or more and 8 or less.

[0232] When the polymer chain constituent unit among the constituent units represented by the general formula (II) contains at least one selected from the group consisting of constituent units represented by the general formula (IV) having a m of 19 or more and 80 or less, the total ratio of the constituent units represented by the general formula (IV) having a m of 19 or more and 80 or less is preferably 1 mass% or more, more preferably 2 mass% or more, and even more preferably 4 mass% or more in terms of water stain suppression effect when the total constituent unit of the polymer chain is 100 mass%. Meanwhile, in terms of solvent redissolvability and water stain suppression effect, it is preferably 75 mass% or less, more preferably 65 mass% or less, and even more preferably 50 mass% or less.

[0233] When the polymer chain constituent unit among the constituent units represented by the general formula (II) contains a combination of at least one selected from the group consisting of constituent units represented by the general formula (IV) having a m of 19 or more and 80 or less, and at least one selected from the group consisting of constituent units represented by the general formula (IV) having a m of 3 or more and 10 or less, the total ratio of the constituent units represented by the general formula (IV) having a m of 3 or more and 10 or less is preferably 20 mass% or more when the total constituent units of the polymer chain are 100 mass%. Meanwhile, in terms of solvent redissolvability, the total ratio of the constituent units represented by the general formula (IV) having a m of 3 or more and 10 or less in the polymer chain is preferably 80 mass% or less, and more preferably 60 mass% or less when the total constituent units of the polymer chain are 100 mass%.

[0234] In addition, regarding the polymer chain, the mixing ratio of the constituent unit represented by the general formula (IV) having m of 19 or more and 80 or less, and the constituent unit represented by the general formula (IV) having m of 3 or more and 10 or less, is such that when the total of the constituent unit represented by the general formula (IV) having m of 19 or more and 80 or less is 100 parts by mass, it is preferable that the total of the constituent unit represented by the general formula (IV) having m of 19 or more and 80 or less is 3 parts by mass or more, more preferable that it is 6 parts by mass or more, more preferable that it is 80 parts by mass or less, and more preferable that it is 60 parts by mass or less.

[0235] In terms of simultaneously satisfying dispersion stability, high contrast, shortened development time, and excellent solvent resistance, when the total constituent unit of the polymer chain is 100 mass%, the total ratio of at least one constituent unit selected from the group consisting of the constituent unit represented by general formula (IV) and the constituent unit represented by general formula (IV') is preferably 1 mass% or more, more preferably 2 mass% or more, and even more preferably 4 mass% or more. In terms of solvent resolubility, when the total constituent unit of the polymer chain is 100 mass%, the total ratio of at least one constituent unit selected from the group consisting of the constituent unit represented by general formula (IV) and the constituent unit represented by general formula (IV') is preferably 80 mass% or less, more preferably 70 mass% or less, and even more preferably 60 mass% or less.

[0236] In the above polymer chain, the constituent unit represented by the general formula (III), which includes the constituent unit represented by the general formula (IV) and the constituent unit represented by the general formula (IV'), may be of one type alone, or may be of two or more types mixed together.

[0237] In terms of the dispersibility and dispersion stability of the colorant, the total ratio of the constituent units represented by the general formula (III) is preferably 70 mass% or more, and more preferably 90 mass% or more, when the total constituent units of the polymer chain are 100 mass%. Meanwhile, in terms of simultaneously satisfying dispersion stability and excellent solvent resistance, the total ratio of the constituent units represented by the general formula (III) in the polymer chain may be 100 mass% when the total constituent units of the polymer chain are 100 mass%.

[0238] Among these, the total proportion of constituent units derived from (meth)acrylate is preferably 60 mass% or more and more preferably 80 mass% or more when the total constituent units of the polymer chain are set to 100 mass% in terms of dispersion stability, solvent resistance, and compatibility with the initiator. Meanwhile, in terms of simultaneously satisfying dispersion stability and excellent solvent resistance, the total proportion of constituent units derived from (meth)acrylate in the polymer chain may be 100 mass% when the total constituent units of the polymer chain are set to 100 mass%.

[0239] The constituent units of the polymer chains among the constituent units represented by the general formula (II) of the above graft copolymer may include other constituent units in addition to the constituent units represented by the general formula (III).

[0240] Other constituent units may include constituent units derived from monomers having unsaturated double bonds that are copolymerizable with monomers that derive the constituent unit represented by the general formula (III) above.

[0241] Monomers that derive other constituent units include, for example, styrenes such as styrene and α-methylstyrene, vinyl ethers such as phenylvinyl ether.

[0242] In the polymer chain among the constituent units represented by the general formula (II) of the above graft copolymer, the total ratio of other constituent units is preferably 30 mass% or less when the total constituent units of the polymer chain are 100 mass%, and more preferably 10 mass% or less, in terms of the effect of the present invention.

[0243] The mass average molecular weight (Mw) of the polymer chain in the polymer is preferably 2000 or more, more preferably 3000 or more, more preferably 4000 or more, more preferably 15000 or less, and more preferably 12000 or less, in terms of the dispersibility and dispersion stability of the colorant.

[0244] By being within the above range, sufficient steric repulsion effect as a dispersant can be maintained, and as the specific surface area of ​​the solvent affinity portion of the dispersant increases, it becomes easier to suppress the penetration of the solvent into the coating film or its arrival at the colorant.

[0245] In addition, the polymer chain in the polymer preferably has a solubility of 20 (g / 100 g solvent) or more at 23°C with respect to the organic solvent used in combination, as a standard.

[0246] The solubility of the above polymer chain can be based on the fact that the raw material into which the polymer chain is introduced when preparing the graft copolymer has the above solubility. For example, when using a polymerizable oligomer (macromonomer) containing a polymer chain and a group having an ethylenically unsaturated double bond at its end to introduce a polymer chain into the graft copolymer, the polymerizable oligomer must have the above solubility. In addition, when introducing a polymer chain using a polymer chain containing a reactive group capable of reacting with a reactive group included in the copolymer after the copolymer has been formed by a monomer containing a group having an ethylenically unsaturated double bond, the polymer chain containing the reactive group must have the above solubility.

[0247] In the above graft copolymer, the constituent unit represented by the general formula (I) is preferably included in a ratio of 3 mass% to 60 mass%, more preferably 6 mass% to 45 mass%, and even more preferably 9 mass% to 30 mass%. If the constituent unit represented by the general formula (I) in the graft copolymer is within the above range, the ratio of the affinity portion with the colorant in the graft copolymer becomes appropriate, and since the decrease in solubility for organic solvents can be suppressed, the adsorption of the colorant becomes good, and it is easy to obtain excellent dispersibility and dispersion stability.

[0248] Meanwhile, in the graft copolymer, the constituent unit represented by the general formula (II) is preferably included in a ratio of 40 mass% to 97 mass%, more preferably 55 mass% to 94 mass%, and even more preferably 70 mass% to 91 mass%. When the constituent unit represented by the general formula (II) in the graft copolymer is within the above range, the ratio of the solvent affinity portion in the graft copolymer becomes appropriate, so that a sufficient steric repulsion effect as a dispersant can be maintained, and furthermore, as the specific surface area of ​​the solvent affinity portion of the dispersant increases, it is easy to suppress the penetration of the solvent into the coating film or the reaching of the colorant.

[0249] The graft copolymer used in the present invention may have additional constituent units in addition to the constituent unit represented by the general formula (I) and the constituent unit represented by the general formula (II), to the extent that the effects of the present invention are not impaired. As other constituent units, other constituent units may be introduced by appropriately selecting and copolymerizing an ethylene unsaturated double bond-containing monomer capable of copolymerizing with the ethylene unsaturated double bond-containing monomer that induces the constituent unit represented by the general formula (I).

[0250] Other constituent units copolymerized with the constituent unit represented by the above general formula (I) include, for example, the constituent unit represented by the above general formula (III).

[0251] In addition, the content ratio of the above constituent units is calculated from the amount of monomer injected to induce the constituent unit represented by the above general formula (I), the constituent unit represented by the above general formula (II), and the constituent unit represented by the above general formula (III), etc., when synthesizing the graft copolymer during manufacturing.

[0252] In addition, regarding dispersibility and dispersion stability, the mass average molecular weight (Mw) of the graft copolymer is preferably 4,000 or higher, more preferably 6,000 or higher, and even more preferably 8,000 or higher. Meanwhile, regarding solvent redissolvability, it is preferably 50,000 or lower, and more preferably 30,000 or lower.

[0253] In addition, in the present invention, the mass average molecular weight (Mw) is a value measured by GPC (gel permeation chromatography). The measurement was performed using an HLC-8120 GPC manufactured by Dosho, with N-methylpyrrolidone with 0.01 mol / liter of lithium bromide added as the elution solvent, and polystyrene standards for the calibration curve were set to Mw 377400, 210500, 96000, 50400, 20650, 10850, 5460, 2930, 1300, 580 (all, Easi PS-2 series manufactured by Polymer Laboratories) and Mw 1090000 (manufactured by Dosho), and the measurement column was TSK-GEL ALPHA-M × 2 (manufactured by Dosho).

[0254] (Method for manufacturing graft copolymer)

[0255] In the present invention, the method for manufacturing the graft copolymer is not particularly limited, provided that it is a method capable of manufacturing a graft copolymer having a constituent unit represented by general formula (I) and a constituent unit represented by general formula (II). When manufacturing a graft copolymer having a constituent unit represented by general formula (I) and a constituent unit represented by general formula (II), for example, a method may be used to manufacture the graft copolymer by copolymerizing a monomer represented by the following general formula (Ia) and a polymerizable oligomer (macromonomer) comprising a polymer chain and a group having an ethylenically unsaturated double bond at its end, as copolymerizing components.

[0256] If necessary, additional monomers may also be used, and a graft copolymer may be prepared using known polymerization means.

[0257]

[0258] (of general formula (Ia), R 71 , A 1 , R 72 and R 73 is the same as general formula (I).

[0259] In addition, when preparing a graft copolymer having a constituent unit represented by the general formula (I) and a constituent unit represented by the general formula (II), a copolymer may be formed by addition polymerization of a monomer represented by the general formula (Ia) and a monomer containing a group having an ethylenically unsaturated double bond, and then a polymer chain may be introduced using a polymer chain containing a reactive group capable of reacting with a reactive group included in the copolymer. Specifically, for example, a copolymer having substituents such as an alkoxy group, a hydroxyl group, a carboxyl group, an amino group, an epoxy group, an isocyanate group, or a hydrogen bond-forming group may be synthesized, and then a polymer chain containing a functional group that reacts with said substituent may be reacted to introduce the polymer chain.

[0260] For example, a polymer chain can be introduced by reacting a polymer chain having a carboxyl group at the end with a copolymer having a glycidyl group in the side chain, or by reacting a polymer chain having a hydroxyl group at the end with a copolymer having an isocyanate group in the side chain.

[0261] In addition, in the above polymerization, additives generally used in polymerization, such as polymerization initiators, dispersion stabilizers, chain transfer agents, etc., may be used.

[0262] Next, a block copolymer having a block A comprising a constituent unit represented by the above general formula (I) and a block B comprising a constituent unit of (meth)acrylate origin is described.

[0263] In the present invention, the arrangement of each block of the block copolymer is not particularly limited and may be, for example, an AB block copolymer, an ABA block copolymer, a BAB block copolymer, etc. Among these, an AB block copolymer or an ABA block copolymer is preferred in that it has excellent dispersibility.

[0264] Block A is a block that functions as a color adsorption site and includes at least a constituent unit represented by the general formula (I). It may also be a salt-type block copolymer in which at least one type selected from the group consisting of organic acid compounds and halogenated hydrocarbons forms a salt with at least a portion of the nitrogen portion of the constituent unit represented by the general formula (I) of the block copolymer.

[0265] Block A may have a constituent unit other than the constituent unit represented by general formula (I) to the extent that it achieves the purpose of the present invention, and may contain any constituent unit copolymerizable with the constituent unit represented by general formula (I). Specifically, examples include, for instance, the constituent unit represented by the above general formula (III).

[0266] In the block copolymer prior to salt formation, the content ratio of the constituent unit represented by general formula (I) in block A is preferably 50 mass% to 100 mass% with respect to the total mass of all constituent units of block A, more preferably 80 mass% to 100 mass%, and most preferably 100 mass%. This is because the higher the ratio of the constituent unit represented by general formula (I), the better the adsorption capacity to the colorant and the better the dispersibility and dispersion stability of the block copolymer. In addition, the content ratio of the constituent unit is calculated from the injection mass when synthesizing block A having the constituent unit represented by general formula (I).

[0267] Among the block copolymers prior to salt formation, the total content ratio of the total constituent units of block A, which includes constituent units represented by general formula (I), is preferably 5% to 60% with respect to the total mass of the total constituent units of the block copolymer, and more preferably 10% to 50% with respect to the total mass of the block copolymer, in that the dispersibility and dispersion stability are good.

[0268] In addition, among the block copolymer prior to salt formation, the content ratio of the constituent unit represented by general formula (I) is preferably 5% to 60% by mass relative to the total mass of all constituent units of the block copolymer, and more preferably 10% to 50% by mass, in order to ensure good dispersibility and dispersion stability. Furthermore, the content ratio of each constituent unit in the block copolymer is calculated from the injection mass when synthesizing the block copolymer prior to salt formation.

[0269] In addition, the constituent unit represented by general formula (I) may have affinity with the color material, and may consist of one type or may include two or more types of constituent units.

[0270] Block B is a block that functions as a solvent-affinity site and contains at least a constituent unit of (meth)acrylate origin.

[0271] The constituent units derived from (meth)acrylate may be as described above.

[0272] As for the B block, it is preferable to use a monomer having an unsaturated double bond that is copolymerizable with a monomer that derives a constituent unit represented by general formula (I), appropriately selected according to the solvent to have solvent affinity. As a standard, it is preferable to introduce the B block such that the solubility of the copolymer at 23°C with respect to the solvent used in combination is 20 (g / 100 g solvent) or higher. The constituent unit constituting the B block may consist of one type or may include two or more types of constituent units.

[0273] As constituent units included in block B, examples include constituent units represented by the above general formula (III).

[0274] In the block copolymer used as a dispersant of the present invention, the ratio (m / n) of the number of units m of the constituent unit represented by the general formula (I) and the number of units n of another constituent unit constituting the solvent-affinity block part is preferably within the range of 0.01 or more and 1 or less, and is more preferably within the range of 0.05 or more and 0.7 or less in terms of the dispersibility and dispersion stability of the colorant.

[0275] Among the block copolymers used as dispersants of the present invention, it is preferable that the block copolymer contains an A block comprising a constituent unit represented by the general formula (I), a B block comprising a constituent unit derived from a carboxyl group-containing monomer and a constituent unit derived from (meth)acrylate, and at least one salt-type block copolymer in which at least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons forms a salt with at least a portion of the nitrogen portion of the constituent unit represented by the general formula (I) of the block copolymer, and the acid value of at least one of the block copolymer and the salt-type block copolymer is 1 mgKOH / g to 18 mgKOH / g and the glass transition temperature is 30°C or higher, in that the substrate adhesion and solvent resistance of the cured film are good even in low-temperature heat treatment and the occurrence of developing residue is suppressed. In addition, the specific dispersant is preferred in that its solvent resistance is further improved when combined with a photoinitiator comprising at least one of the compound represented by the general formula (A) and the compound represented by the general formula (B).

[0276] In this case, Block B includes a constituent unit derived from (meth)acrylate as an essential component, but may be the same as Block B of International Publication No. 2016 / 104493.

[0277] As the above carboxyl group-containing monomer, a monomer containing an unsaturated double bond and a carboxyl group that is copolymerizable with a constituent unit represented by general formula (I) may be used. Examples of such monomers include (meth)acrylic acid, vinyl benzoic acid, maleic acid, maleic acid monoalkyl ester, fumaric acid, itaconic acid, crotonic acid, cinnamic acid, acrylic acid dimer, etc. Additionally, the addition reaction product of a monomer having a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, with a cyclic anhydride such as maleic anhydride, phthalic anhydride, or cyclohexanedicarboxylic acid anhydride, and ω-carboxy-polycaprolactone mono(meth)acrylate may also be used. Furthermore, as a precursor of the carboxyl group, an acid anhydride-containing monomer such as maleic anhydride, itaconic anhydride, or citraconic anhydride may be used. Among them, (meth)acrylic acid is particularly desirable in terms of copolymerization, cost, solubility, and glass transition temperature.

[0278] The content ratio of constituent units derived from carboxyl group-containing monomers in the block copolymer prior to salt formation can be appropriately set so that the acid value of the block copolymer is within the range of the specific acid value mentioned above, and is not particularly limited, but it is preferable that it be 0.05 mass% to 4.5 mass% with respect to the total mass of all constituent units of the block copolymer, and more preferable that it be 0.07 mass% to 3.7 mass%.

[0279] The effect of suppressing development residue is exhibited when the content ratio of constituent units derived from carboxyl group-containing monomers is greater than or equal to the above lower limit, and when it is less than or equal to the above upper limit, it is possible to prevent deterioration of development adhesion or deterioration of solvent re-solubility.

[0280] In addition, the constituent unit derived from the carboxyl group-containing monomer may have the above-mentioned specific acid value, and may include one type or include two or more types of constituent units.

[0281] In addition, it is desirable for the B block of the block copolymer to include constituent units derived from hydroxyl group-containing monomers, as this improves development adhesion. When constituent units derived from hydroxyl group-containing monomers are included in the B block, the development speed is also further improved. Furthermore, the hydroxyl group referred to here means an alcoholic hydroxyl group bonded to an aliphatic hydrocarbon.

[0282] For the constituent unit derived from the hydroxyl group-containing monomer, a monomer containing an unsaturated double bond and a hydroxyl group that is copolymerizable with the monomer that derives the constituent unit represented by general formula (I) may be used. Examples of such monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerin mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, ε-caprolactone 1 molar adduct of 2-hydroxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, etc.

[0283] In terms of improving adhesion, it is preferable to use one or more selected from the group consisting of 2-hydroxyethyl methacrylate and 2-hydroxy-3-phenoxypropyl (meth)acrylate.

[0284] In the block copolymer prior to salt formation, the content ratio of constituent units derived from hydroxyl group-containing monomers is preferably 1 mass% or more with respect to the total mass of all constituent units of the block copolymer, more preferably 2 mass% or more, even more preferably 3 mass% or more, and particularly preferably 4 mass% or more. If the content ratio is above the lower limit, the adhesion to the developing substrate can be considered desirable. Likewise, it is preferably 70 mass% or less, more preferably 60 mass% or less, even more preferably 50 mass% or less, and particularly preferably 40 mass% or less. If the content ratio is below the upper limit, it can be considered desirable in that it allows for an increased introduction ratio of other useful monomers. Furthermore, the content ratio of the constituent units is calculated from the input mass when synthesizing the block copolymer prior to salt formation.

[0285] The acid value of at least one of the above block copolymer and salt-type block copolymer is preferably 1 mgKOH / g or higher as a lower limit, and more preferably 2 mgKOH / g or higher, in terms of the effect of suppressing developing residue. In addition, the acid value of at least one of the above block copolymer and salt-type block copolymer is preferably 18 mgKOH / g or lower as an upper limit, more preferably 16 mgKOH / g or lower, and even more preferably 14 mgKOH / g or lower, in terms of preventing deterioration of developing adhesion or deterioration of solvent re-solubility.

[0286] The acid value of at least one of the above block copolymers and salt-type block copolymers can be obtained by the method described in International Publication No. 2016 / 104493.

[0287] The glass transition temperature of at least one of the above block copolymers and salt-type block copolymers is preferably 30°C or higher in terms of developing adhesion, and among them, 32°C or higher is preferable, and 35°C or higher is more preferable. Meanwhile, from the perspective of operability during use, such as ease of precise weighing, it is preferable that it be 200°C or lower.

[0288] At least one glass transition temperature of the above block copolymer and salt-type block copolymer is determined by measuring by differential scanning calorimetry (DSC) in accordance with JIS K7121. If two or more peaks representing the glass transition temperature are observed, the peak with the largest peak area, that is, the area of ​​the portion protruding from the baseline of the obtained chart, is taken as the representative value of the glass transition temperature.

[0289] The mass average molecular weight (Mw) of the above block copolymer is not particularly limited, but is preferably 1000 to 20000, more preferably 2000 to 15000, and even more preferably 3000 to 12000 in order to provide good colorant dispersibility and dispersion stability.

[0290] Here, the mass average molecular weight (Mw) can be measured in the same way as described above.

[0291] In addition, regarding dispersion stability, solvent resistance, and compatibility with photoinitiators, the total proportion of constituent units derived from (meth)acrylate is preferably 60 mass% or more, more preferably 80 mass% or more, and even more preferably 90 mass% or more when the total constituent units in block B of the block copolymer are set to 100 mass%. Meanwhile, regarding the simultaneous satisfaction of dispersion stability and excellent solvent resistance, the total proportion of constituent units derived from (meth)acrylate may be 100 mass% when the total constituent units in block B are set to 100 mass%. In the case where block B contains constituent units derived from the carboxyl group-containing monomer, the total proportion of constituent units derived from (meth)acrylate may be 100 mass% when the total constituent units different from the constituent units derived from the carboxyl group-containing monomer in block B are set to 100 mass%.

[0292] In the block copolymer prior to salt formation, the total content ratio of the entire constituent unit of block B is preferably 5% to 60% with respect to the total mass of the entire constituent unit of the block copolymer, and more preferably 10% to 50% with respect to the total mass of the entire constituent unit of the block copolymer, in that the dispersibility and dispersion stability are good.

[0293] In addition, among the block copolymer prior to salt formation, the content ratio of the constituent unit represented by the general formula (III) is preferably 40% to 95% with respect to the total mass of the entire constituent unit of the block copolymer, and more preferably 50% to 90% with respect to the total mass of the entire constituent unit of the block copolymer, in order to improve the dispersibility of the colorant. In addition, the content ratio of the constituent unit is calculated from the injection mass when synthesizing the block copolymer prior to salt formation.

[0294] A (meth)acrylate-based copolymer comprising a constituent unit represented by the above general formula (I) is preferred in that the copolymer has an amine value of 40 mgKOH / g to 120 mgKOH / g, has good dispersibility, does not precipitate foreign substances when forming a coating film, and improves brightness and contrast.

[0295] Since the amine value is within the above range, the stability of viscosity over time and heat resistance are excellent, and the alkali development properties and solvent redissolvability are also excellent. In the present invention, the amine value of the (meth)acrylate copolymer containing the constituent unit represented by the general formula (I) is preferably 80 mgKOH / g or higher, and more preferably 90 mgKOH / g or higher. Meanwhile, regarding solvent redissolvability, the amine value of the (meth)acrylate copolymer containing the constituent unit represented by the general formula (I) is preferably 110 mgKOH / g or lower, and more preferably 105 mgKOH / g or lower.

[0296] The amine value refers to the number of milligrams of potassium hydroxide equivalent to perchloric acid required to neutralize the amine component contained in 1 g of a sample, and can be measured by the method defined in JIS-K7237. When measured by the above method, even if the amino group forms a salt with the organic acid compound in the dispersant, the organic acid compound usually dissociates, so the amine value of the block copolymer itself used as a dispersant can be measured.

[0297] The content ratio (mol%) of each constituent unit in the copolymer of the dispersant can be determined from the amount of raw material injected during manufacturing, and can also be measured using an analytical device such as NMR. In addition, the structure of the dispersant can be measured using NMR, various mass spectrometers, etc. Furthermore, if necessary, the dispersant can be decomposed by thermal decomposition, and the obtained decomposition product can be determined using high-speed liquid chromatography, gas chromatograph mass spectrometer, NMR, elemental analysis, XPS / ESCA, and TOF-SIMS.

[0298] In the photocurable red resin composition according to the present invention, the content of the dispersant is selected to ensure excellent dispersibility and dispersion stability of the colorant, and is not particularly limited, but is preferably within the range of 2 mass% to 30 mass% and more preferably 3 mass% to 25 mass% with respect to the total solid content of the photocurable red resin composition. If the content is above the lower limit, the dispersibility and dispersion stability of the colorant are excellent, and the storage stability of the photocurable red resin composition is better. Furthermore, if the content is below the upper limit, the developability is good. In particular, when forming a cured film with a high colorant concentration, the content of the dispersant is preferably within the range of 2 mass% to 25 mass% and more preferably 3 mass% to 20 mass% with respect to the total solid content of the photocurable red resin composition.

[0299] Thiol compounds

[0300] The photocurable red resin composition of the present invention preferably additionally contains a thiol compound in order to improve solvent resistance and substrate adhesion after low-temperature heat treatment.

[0301] Examples of thiol compounds include monofunctional thiol compounds with one thiol group and polyfunctional thiol compounds with two or more thiol groups. In terms of suppressing linewidth shift and improving substrate adhesion, it is more preferable to use monofunctional thiol compounds with one thiol group.

[0302] Examples of monofunctional thiol compounds include 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, 2-mercaptobenzimidazole, 2-mercapto-5-methoxybenzothiazole, 2-mercapto-5-methoxybenzimidazole, 3-mercaptopropionic acid, methyl 3-mercaptopropionic acid, ethyl 3-mercaptopropionic acid, octyl 3-mercaptopropionic acid, etc.

[0303] Examples of polyfunctional thiol compounds include, for instance, 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris-(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), pentaerythritol tetrakis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), and tetraethyleneglycolbis(3-mercaptopropionate).

[0304] As for the thiol compound, it may be used alone or in combination of two or more types, and among them, 2-mercaptobenzoxazole or 2-mercaptobenzothiazole is preferred in that it improves solvent resistance and substrate adhesion after low-temperature heat treatment.

[0305] The content of the thiol compound is typically within the range of 0.5 mass% to 10 mass%, preferably 1 mass% to 5 mass%, with respect to the total solid content of the photocurable red resin composition. If the content is above the lower limit, the solvent resistance and substrate adhesion after low-temperature heat treatment tend to be excellent. On the other hand, if the content is below the upper limit, the photocurable red resin composition of the present invention tends to have good developability and suppress linewidth shift.

[0306] Other ingredients

[0307] The photocurable red resin composition of the present invention may additionally include various additives as needed. Examples of additives include antioxidants, polymerization inhibitors, chain transfer agents, leveling agents, plasticizers, surfactants, defoaming agents, silane coupling agents, UV absorbers, adhesion promoters, etc.

[0308] Specific examples of surfactants and plasticizers include those described in Japanese Patent Publication No. 2013-029832.

[0309] It is preferable for the photocurable red resin composition of the present invention to additionally include an antioxidant, in order to suppress the amount of linewidth shift of the cured film. By including an antioxidant in combination with, for example, a compound represented by the general formula (A) above, the photocurable red resin composition of the present invention can control excessive radical chain reactions without impairing curability when forming a cured film. Consequently, when forming fine line patterns, linearity is further improved, or the ability to form fine line patterns according to the design of the mask linewidth is enhanced. Furthermore, since heat resistance can be improved and the decrease in brightness after exposure and post-baking can be suppressed, brightness can be improved.

[0310] The antioxidant used in the present invention is not particularly limited and may be appropriately selected from those known in the prior art. Specific examples of the antioxidant include hindered phenol-based antioxidants, amine-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, hydrazine-based antioxidants, etc. It is preferable to use a hindered phenol-based antioxidant in terms of heat resistance and the ability to form fine line patterns according to the design of the mask line width. A latent antioxidant such as that described in International Publication No. 2014 / 021023 may also be used.

[0311] Hindered phenol-based antioxidants include, for example, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name: IRGANOX 1010, manufactured by BASF), 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate (trade name: Irganox 3114, manufactured by BASF), 2,4,6-tris(4-hydroxy-3,5-di-tert-butylbenzyl)meshtylene (trade name: Irganox 1330, manufactured by BASF), 2,2'-methylenebis(6-tert-butyl-4-methylphenol) (trade name: Sumirizer MDP-S, manufactured by Sumitomo Chemical), Examples include 6,6'-thiobis(2-tert-butyl-4-methylphenol) (trade name: Irganox 1081, manufactured by BASF) and 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid diethyl (trade name: Irgamod 195, manufactured by BASF). Among these, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name: IRGANOX 1010, manufactured by BASF) is preferred in terms of heat resistance and light resistance.

[0312] The content of the antioxidant is typically within the range of 0.1 mass% to 10.0 mass%, preferably 0.5 mass% to 5.0 mass%, relative to the total solid content of the photocurable red resin composition. If the value is above the lower limit, the ability to form fine line patterns according to the design of the mask line width is improved, and heat resistance is excellent. On the other hand, if the value is below the upper limit, it is easy to make the photocurable red resin composition of the present invention a high-sensitivity photocurable red resin composition.

[0313] In addition, examples of silane coupling agents include KBM-502, KBM-503, KBE-502, KBE-503, KBM-5103, KBM-903, KBE-903, KBM573, KBM-403, KBE-402, KBE-403, KBM-303, KBM-802, KBM-803, KBE-9007, and X-12-967C (manufactured by Shin-Etsu Silicon Co., Ltd.). Among these, KBM-502, KBM-503, KBE-502, KBE-503, and KBM-5103 having methacrylic and acrylic groups are preferred in terms of adhesion to the SiN substrate.

[0314] The content of the silane coupling agent is typically within the range of 0.05 mass% to 10.0 mass%, preferably 0.1 mass% to 5.0 mass%, based on the total solid content of the photocurable red resin composition. If the content is above the lower limit and below the upper limit, the effect of improving substrate adhesion is likely to be good.

[0315] Method for manufacturing a photocurable red resin composition

[0316] The method for preparing the photocurable red resin composition of the present invention can be prepared by mixing a colorant, a photopolymerizable compound, a photoinitiator, and various additive components used as desired, using known mixing means.

[0317] When the photocurable red resin composition of the present invention contains a colorant, a dispersant, an alkali-soluble resin, a photopolymerizable compound, a photoinitiator, a solvent, and various additive components used as desired, the method of preparing said resin composition is, for example, (1) first, a colorant dispersion solution is prepared by adding a colorant and a dispersant to a solvent, and then mixing an alkali-soluble resin, a photopolymerizable compound, a photoinitiator, and various additive components used as desired into said dispersion solution; (2) a method of simultaneously adding and mixing a colorant, a dispersant, an alkali-soluble resin, a photopolymerizable compound, a photoinitiator, and various additive components used as desired into a solvent; (3) a method of adding and mixing a dispersant, an alkali-soluble resin, a photopolymerizable compound, a photoinitiator, and various additive components used as desired into a solvent, and then adding and dispersing a colorant. (4) A method of preparing a colorant dispersion by adding a colorant, a dispersant, and an alkali-soluble resin to a solvent, and then adding an alkali-soluble resin, a solvent, a photopolymerizable compound, a photoinitiator, and various additive components as desired to the dispersion and mixing them.

[0318] Among these methods, the above methods (1) and (4) are preferred in that they effectively prevent the aggregation of the color material and allow it to be uniformly dispersed.

[0319] A method for preparing a colorant dispersion can be appropriately selected from conventionally known dispersion methods. For example, (1) a method of preparing a dispersant solution by mixing and stirring a dispersant in a solvent beforehand, and then mixing an organic acid compound as needed to form a salt of the amino group of the dispersant and the organic acid compound. This is then mixed with a colorant and, if necessary, other components, and dispersed using a known stirrer or disperser; (2) a method of preparing a dispersant solution by mixing and stirring a dispersant in a solvent, then mixing a colorant and, if necessary, an organic acid compound and, if necessary, additionally, other components, and dispersed using a known stirrer or disperser; (3) a method of preparing a dispersant solution by mixing and stirring a dispersant in a solvent, then mixing a colorant and, if necessary, other components, and, after forming a dispersion using a known stirrer or disperser, adding an organic acid compound as needed.

[0320] Examples of dispersers for performing dispersion treatment include roll mills such as 2-roll or 3-roll mills, ball mills such as ball mills and vibrating ball mills, paint conditioners, continuous disc-type bead mills, and continuous annular-type bead mills. As for the preferred dispersion conditions of the bead mill, the bead diameter used is preferably 0.03 mm to 2.00 mm, and more preferably 0.10 mm to 1.0 mm.

[0321] <Uses>

[0322] The photocurable red resin composition according to the present invention is suitable for forming a colored cured film that replaces a circular polarizer, as the cured film has an external light reflection suppression effect. When the cured film of the photocurable red resin composition according to the present invention is used as a replacement for a circular polarizer, the display device can be made without a polarizer; therefore, the photocurable red resin composition according to the present invention is suitable for use in a display device that does not include a polarizer.

[0323] In addition, since the photocurable red resin composition according to the present invention is a photocurable red resin composition used for a cured film formed on an organic light-emitting element, it is suitable for use in display devices that do not include an externally attached color filter substrate, and for use in thin-film organic light-emitting display devices with improved flexibility.

[0324] In addition, the photocurable red resin composition according to the present invention can form a cured film with good solvent resistance and excellent substrate adhesion even during low-temperature heat treatment by appropriately selecting the components as described above, so it can be suitably used for forming a cured film on a substrate having a device with low heat resistance at 130°C or lower, or at 100°C or lower, or 90°C or lower, through low-temperature heat treatment.

[0325] II. Display Devices

[0326] A display device according to the present invention is characterized by having a cured film of a photocurable red resin composition according to the present invention on an organic light-emitting element.

[0327] In the display device according to the present invention, since the cured film of the photocurable red resin composition used for the cured film formed on the organic light-emitting element according to the present invention is formed on the organic light-emitting element, an externally attached circular polarizer or an externally attached color filter substrate is unnecessary, and it is acceptable not to have them.

[0328] The display device according to the present invention utilizes a photocurable red resin composition used for a cured film formed on an organic light-emitting element according to the present invention to form a cured film on the organic light-emitting element. Since the cured film is formed on the organic light-emitting element, it does not have a substrate used for an externally attached color filter substrate between the organic light-emitting element and the cured film, thereby improving thinness and flexibility.

[0329] An organic light-emitting display device including an organic light-emitting element according to the present invention will be described with reference to the drawings. FIG. 1 is a schematic cross-sectional view illustrating an example of a display device having an organic light-emitting element according to the present invention. As illustrated in FIG. 1, the display device (100) according to the present invention comprises a device substrate (30) having an organic light-emitting element, an external light reflection prevention film (20) including a colored cured film (9R, 9G, 9B) on the device substrate (30), and a sealing film (11) thereon.

[0330] The device substrate (30) having the above-mentioned organic light-emitting element has a thin-film transistor (TFT) (2), which is a driving element, arranged on the substrate (1) so as to correspond to each subpixel, and a sealing film (3) is provided thereon. Additionally, on the sealing film (3), an electrode (4) (anode) corresponding to each subpixel and a partition (5) partitioning each subpixel are provided, and within the partition, an organic light-emitting element (6R, 6G, 6B) constituting three colors R, G, and B subpixels is arranged, and an electrode (7) (cathode) is also provided on the organic light-emitting element (6R, 6G, 6B). The device substrate (30) having the above-mentioned organic light-emitting element also has a sealing layer (8) covering the organic light-emitting element thereon.

[0331] On the sealing layer (8) on the organic EL elements (6R, 6G, 6B) in the element substrate (30), an external light reflection prevention film (20) comprising a light-blocking portion (10) and three colored cured films (9R, 9G, 9B) corresponding to each organic EL element formed using a photocurable colored resin composition is provided, and a sealing film (11) is provided thereon.

[0332] The display device (100) according to the present invention may additionally have a touch sensor layer including an insulating film and a transparent electrode layer on a sealing film (11), although not illustrated, and may also appropriately have a known configuration such as a hard coat layer on the touch sensor layer.

[0333] As described above, since the layers of the colored cured film (9R, 9G, 9B) and the light-blocking portion (10) formed on the device substrate (30) equipped with the organic light-emitting element are used as an external light reflection prevention film (20), the external light reflection prevention film used in the present invention can improve thinness and flexibility without including a separate substrate such as an externally attached circular polarizer or an externally attached color filter substrate.

[0334] In the display device according to the present invention, it is preferable to adjust the color of the (6R, 6G, 6B) subpixel of the organic light-emitting element and the color of the colored cured film (9R, 9G, 9B) directly above it through at least one layer, such as a sealing layer (8), so that they are of the same color. By the colored cured film formed on the organic light-emitting element, external light is shielded except for the color originally emitted by the organic light-emitting element, and the light emitted by the organic light-emitting element is not cut off, so external light reflection can be suppressed without reducing light utilization efficiency.

[0335] The cured film of the photocurable red resin composition according to the present invention may be the red cured film (9R) among the three colored cured films (9R, 9G, 9B).

[0336] A substrate (1), a thin-film transistor (TFT) (2) which is a driving element, a sealing film (3), an electrode (4) (anode), a partition (5) which separates each subpixel, an organic light-emitting element (6R, 6G, 6B) constituting the subpixel, an electrode (7) (cathode), etc. used in the display device according to the present invention may be appropriately selected from known configurations.

[0337] In addition to the light-emitting layer, the organic light-emitting device may also have known configurations such as a hole injection layer, a hole transport layer, and an electron injection layer.

[0338] As a sealing layer (8) on an organic EL element used in a display device according to the present invention, an inorganic film or an organic film and a multilayer film formed by stacking the same may be used. It is preferable to use a multilayer film in that it has a high effect of suppressing the intrusion of moisture or oxygen.

[0339] Specifically, examples include multilayer films formed by stacking inorganic films such as metal films, metal oxide films, SiOx, and SiNx with organic films.

[0340] The colored cured film used in the display device according to the present invention is, at least one, a cured film of the photocurable red resin composition according to the present invention.

[0341] The colored cured film is typically formed at the opening of the light-blocking portion described later on the sealing layer (8) on the organic light-emitting element, and is typically composed of a coloring pattern of three or more colors. These may be coloring patterns such as (6R, 6G, 6B) of the subpixel of the organic light-emitting element.

[0342] The arrangement of the colored curing film (9R, 9G, 9B) can be a general arrangement such as a stripe type, mosaic type, triangle type, or 4-pixel arrangement type. In addition, the width and area of ​​the colored layer can be appropriately set to suit the (6R, 6G, 6B) of the subpixel of the organic light-emitting device.

[0343] The thickness of the above-mentioned colored cured film is appropriately controlled by adjusting the coating method, the solid content concentration or viscosity of the photocurable red resin composition, etc., but is typically in the range of 1 μm to 5 μm.

[0344] The light-blocking part (10) used in the display device according to the present invention is formed in a pattern shape on a sealing layer (8) on an organic light-emitting element, and can be made in the same way as a light-blocking part used in a general color filter.

[0345] The pattern shape of the light-shielding portion may be appropriately selected to match the shape of the colored cured film, such as a stripe shape or a matrix shape. The light-shielding portion may be a metal thin film, such as chrome, produced by a sputtering method or a vacuum deposition method. Alternatively, the light-shielding portion may be a resin layer containing light-shielding particles, such as carbon fine particles, metal oxides, inorganic pigments, or organic pigments, within a resin binder. In the case of a resin layer containing light-shielding particles, methods such as patterning by developing using a photosensitive resist, patterning using an inkjet ink containing light-shielding particles, or thermal transfer of a photosensitive resist are available.

[0346] As for the film thickness of the light-blocking part, in the case of a metal thin film, it is set to about 0.2 μm to 0.4 μm, and in the case of a black pigment dispersed or dissolved in a binder resin, it is set to about 0.5 μm to 2 μm.

[0347] For the sealing film (11) formed on the colored curing film (9R, 9G, 9B) and the light-blocking part (10), known materials can be appropriately selected and used.

[0348] In addition, the display device according to the present invention is not limited to the configuration shown in FIG. 1, and may additionally have a configuration of a display device equipped with a known organic light-emitting element.

[0349] III. Method for manufacturing a laminate of an organic light-emitting diode and an external light-reflecting anti-reflective film

[0350] A method for manufacturing a laminate of an organic light-emitting element and an external light reflection prevention film according to the present invention is,

[0351] A process of forming a coating film by applying a photocurable red resin composition according to the present invention onto an organic light-emitting diode,

[0352] A process of irradiating the above coating film with light,

[0353] A post-baking process for heating the film after the above light irradiation, and

[0354] By including a process for developing the film after the above light irradiation,

[0355] The method comprises forming a cured film of a photocurable red resin composition according to the present invention on an organic light-emitting diode.

[0356] Each process is explained below.

[0357] In the process of applying the photocurable red resin composition according to the present invention onto an organic light-emitting element, the organic light-emitting element may not be applied adjacent to the organic light-emitting element, and may be applied through at least one layer. As shown in FIG. 1, in a device substrate (30) equipped with an organic light-emitting element, an electrode (7) or a sealing layer (8) for suppressing the intrusion of moisture or oxygen is typically additionally formed on the (6R, 6G, 6B) of the subpixels of the organic light-emitting element, so the composition may be applied onto the organic light-emitting element through these electrodes and sealing layer.

[0358] For example, a light-blocking portion (10) may be formed in advance on the sealing layer (8) by a known method as exemplified above, and a colored cured film (9R, 9G, 9B) may be applied to form a color-blocking film at an opening of the light-blocking portion (10).

[0359] For example, the photocurable red resin composition of the present invention described above is applied onto the organic light-emitting diode using a coating means such as a spray coating method, a dip coating method, a bar coating method, a roll coating method, a spin coating method, a die coating method, or an inkjet method. Among these, the spin coating method and the die coating method may be preferably used as coating means.

[0360] Next, the wet film is dried using a hot plate or an oven to form a film.

[0361] The obtained coating film is exposed to light through a mask of a predetermined pattern to photopolymerize a photopolymerizable compound and, if necessary, an alkali-soluble resin. Alternatively, a patterned coating film is exposed to light to photopolymerize a photopolymerizable compound. Light sources used for exposure include, for example, ultraviolet rays from low-pressure mercury lamps, high-pressure mercury lamps, and metal halide lamps, as well as electron beams. The amount of exposure is appropriately adjusted according to the light source used and the thickness of the coating film.

[0362] Next, in order to promote the polymerization reaction after exposure, a post-baking process may be performed to heat the film after the light irradiation. The heating conditions may be appropriately selected according to the mixing ratio of each component in the photocurable red resin composition used or the thickness of the film.

[0363] The post-baking process may be performed on the film after the light irradiation described above before the development process described later, after the development process, or before and after the development process.

[0364] In the present invention, since a color-cured film is directly formed on a device substrate equipped with an organic light-emitting element, it is preferable that the heating temperature in the post-baking process be 130°C or lower. The heating temperature is more preferably 100°C or lower, and even more preferably 90°C or lower. Additionally, the heating temperature may be 30°C or higher, 35°C or higher, or 40°C or higher.

[0365] Next, the film after the light irradiation is developed as needed. The film after the light irradiation to be developed may be the film after post-baking.

[0366] In the development process, a developing solution is used to treat the surface, and unexposed areas are dissolved and removed, thereby forming a coating film with a desired pattern. Typically, a solution in which an alkali is dissolved in water or a water-soluble solvent is used as the developing solution. An appropriate amount of surfactants may be added to this alkaline solution. Furthermore, a general development method may be employed.

[0367] After the development process, the developer is typically washed and the cured film of the photocurable red resin composition is dried to form a colored cured film. Additionally, a heat treatment may be performed after the development process to sufficiently cure the coating film.

[0368] In the present invention, since a colored cured film is directly formed on a device substrate equipped with an organic light-emitting element, the heating temperature in this post-baking process is preferably 130°C or lower, more preferably 100°C or lower, and even more preferably 90°C or lower. Additionally, the heating temperature may be 30°C or higher, 35°C or higher, or 40°C or higher.

[0369] In addition, to further cure the film after development or post-baking, additional light irradiation (exposure) may be performed.

[0370] Examples

[0371] The present invention will be described in detail below by presenting examples. The present invention is not limited by these descriptions.

[0372] The mass average molecular weight (Mw) of the copolymer prior to salt formation was obtained as a standard polystyrene equivalent value by GPC (gel permeation chromatography) according to the measurement method described in the specification of the present invention above.

[0373] (Synthesization Example 1: Synthesis of Block Copolymer 1)

[0374] 250 parts by mass of THF and 0.6 parts by mass of lithium chloride were added to a 500 mL round-bottom, four-necked flask equipped with a condenser, an addition funnel, a nitrogen inlet, a mechanical stirrer, and a digital thermometer, and sufficient nitrogen purging was performed. After cooling the reaction flask to -60°C, 4.9 parts by mass of butyllithium (15% by mass hexane solution), 1.1 parts by mass of diisopropylamine, and 1.0 parts by mass of methyl isobutyrate were injected using a syringe. 2.2 parts by mass of 1-ethoxyethyl methacrylate (EEMA), 29.1 parts by mass of 2-(trimethylsilyloxy)ethyl methacrylate (TMSMA), 12.8 parts by mass of 2-ethylhexyl methacrylate (EHMA), 13.7 parts by mass of n-butyl methacrylate (BMA), 9.5 parts by mass of benzyl methacrylate (BzMA), and 17.5 parts by mass of methyl methacrylate (MMA) were added dropwise over 60 minutes using an adding funnel. After 30 minutes, 26.7 parts by mass of dimethylaminoethyl methacrylate (DMMA), the monomer for Block A, were added dropwise over 20 minutes. After reacting for 30 minutes, 1.5 parts by mass of methanol were added to stop the reaction. The obtained precursor block copolymer THF solution was reprecipitated in hexane, purified by filtration and vacuum drying, and diluted with PGMEA to obtain a solution with a solid content of 30 mass%. 32.5 mass parts of water were added, the temperature was raised to 100°C, and the reaction was carried out for 7 hours. The constituent units derived from EEMA were deprotected to become constituent units derived from methacrylic acid (MAA), and the constituent units derived from TMSMA were deprotected to become constituent units derived from 2-hydroxyethyl methacrylate (HEMA). The obtained block copolymer PGMEA solution was reprecipitated in hexane, purified by filtration and vacuum drying, to obtain block copolymer 1 (amine value 95 mgKOH / g, acid value 8 mgKOH / g, Tg 38°C) containing constituent units represented by the above general formula (I). The weight average molecular weight (Mw) was 7730.

[0375] (Synthesization Example 2: Synthesis of Graft Copolymer 2)

[0376] (1) Preparation of macromonomer A

[0377] 70.0 parts by mass of propylene glycol methyl ether acetate (PGMEA) was injected into a reactor equipped with a cooling tube, an adding funnel, a nitrogen inlet, a mechanical stirrer, and a digital thermometer, and heated to 90°C while stirring under a nitrogen stream. A monomer having a PEG chain that derives the constituent unit represented by general formula (III) (manufactured by Evonik, trade name: VISIOMER MPEG 1005 MA W, R in general formula (IV) 74 is CH3, A 3 COO, R 75 is the ethylene group, R 76 A mixed solution of 6.0 parts by mass of CH3 (m=22), 69.0 parts by mass of triethylene glycol monoethyl ether methacrylate (manufactured by Tokyo Kasei High School, m=3), 25.0 parts by mass of methyl methacrylate (MMA), 4.0 parts by mass of mercaptoethanol, 30 parts by mass of PGMEA, and 1.0 parts by mass of α,α'-azobisisobutyronitrile (AIBN) was added dropwise over 1.5 hours and reacted for 3 hours. Subsequently, the nitrogen stream was stopped, the reaction solution was cooled to 80°C, and 8.74 parts by mass of Karens MOI (manufactured by Showa Denko Co., Ltd.), 0.125 g of dioctyl tin dilaurate, 0.125 parts by mass of p-methoxyphenol, and 30 parts by mass of PGMEA were added and stirred for 3 hours to obtain a 50% solution of macromonomer A. The obtained macromonomer B was identified by GPC (gel permeation chromatography) under conditions of N-methylpyrrolidone, 0.01 mol / L lithium bromide addition / polystyrene standard, and had a weight average molecular weight (Mw) of 5800 and a molecular weight distribution (Mw / Mn) of 1.6.

[0378] (2) Synthesis of graft copolymer 2

[0379] 63.1 parts by mass of PGMEA were injected into a reactor equipped with a cooling tube, an additive funnel, a nitrogen inlet, a mechanical stirrer, and a digital thermometer, and the mixture was heated to 85°C while stirring under a nitrogen stream. A mixed solution of 141 parts by mass of the above macromonomer A solution (effective solid content 70.5 parts by mass), 29.5 parts by mass of methacrylic acid 2-(dimethylamino)ethyl (DMMA), 1.24 parts by mass of n-dodecyl mercaptan, 49.4 parts by mass of PGMEA, and 1.0 parts by mass of AIBN was added dropwise over 1.5 hours, and after heating and stirring for 3 hours, a mixed solution of 0.10 parts by mass of AIBN and 6.0 parts by mass of PGMEA was added dropwise over 10 minutes, and the mixture was aged at the same temperature for 1 hour to obtain a 35.0% by mass solution of graft copolymer 2. The obtained graft copolymer 2 had a weight-average molecular weight (Mw) of 10,000 as a result of GPC measurement. At this time, the amine value was 105 mgKOH / g.

[0380] (Synthetic Example 3: Synthesis of an oxime ester-based photoinitiator represented by Formula (A-2))

[0381] An oxime ester-based photoinitiator represented by the above formula (A-2) was synthesized in the same manner as the preparation of compound No. 73 of paragraphs 0114 to 0117 of International Publication No. 2015 / 152153.

[0382] (Synthetic Example 4: Synthesis of an oxime ester-based photoinitiator represented by Formula (B-1))

[0383] An oxime ester-based photoinitiator represented by the formula (B-1) was synthesized in the same manner as the preparation of the photopolymerization initiator W (photopolymerization initiator represented by formula (3)) of paragraph 0080 of Japanese Patent Publication No. 2010-256891.

[0384] (Preparation Example 1: Preparation of alkali-soluble resin A)

[0385] 300 parts by mass of PGMEA were injected into a polymerization vessel, and after raising the temperature to 100°C under a nitrogen atmosphere, 90 parts by mass of 2-phenoxyethyl methacrylate (PhEMA), 54 parts by mass of MMA, 36 parts by mass of methacrylic acid (MAA), 6 parts by mass of perbutyl O (manufactured by Nichiyu Kabushiki Kaisha), and 2 parts by mass of a chain transfer agent (n-dodecyl mercaptan) were continuously added dropwise over a period of 1.5 hours. Afterward, the reaction was continued by maintaining the temperature at 100°C, and 0.1 parts by mass of p-methoxyphenol was added as a polymerization inhibitor 2 hours after the end of the dropwise addition of the main chain forming mixture to stop the polymerization.

[0386] Next, while blowing air, 20 parts by mass of glycidyl methacrylate (GMA) as an epoxy group-containing compound was added, and after raising the temperature to 110°C, 0.8 parts by mass of triethylamine was added and an addition reaction was carried out at 110°C for 15 hours to obtain an alkali-soluble resin A solution (weight average molecular weight (Mw) 8500, acid value 75 mgKOH / g, solid content 40% by mass).

[0387] In addition, the weight-average molecular weight was measured using a Shodex GPC System-21H with polystyrene as the standard material and THF as the eluent. In addition, the acid value was measured based on JIS K 0070.

[0388] (Example 1: Preparation of Photocurable Red Resin Composition R-1)

[0389] (1) Preparation of color dispersion R(1)

[0390] 64.9 parts by mass of PGMEA, 13.5 parts by mass of the alkali-soluble resin A solution of Preparation Example 1 (solid content 40 mass%), and 9.2 parts by mass of the PGMEA solution of block copolymer 1 of Synthesis Example 1 (solid content 35 mass%) were added to a 225 mL mayonnaise jar and stirred. 0.39 parts by mass of phenylphosphonic acid (product name: PPA, manufactured by Nissan Kagaku Co., Ltd.) were added thereto and stirred at room temperature for 30 minutes.

[0391] Thereby, 12.0 parts by mass of CI pigment red 254 (R254) and 100 parts by mass of 2.0 mm particle size zirconia beads were added as red pigments, and the mixture was shaken for 1 hour in a paint shaker (manufactured by Asada Tech Co., Ltd.) as a preliminary disintegration, then changed to 200 parts of 0.1 mm particle size zirconia beads, and dispersed in a paint shaker for 4 hours as a full disintegration to obtain colorant dispersion R (1). In addition, block copolymer 1 was salted by phenylphosphonic acid to become salt-type block copolymer 1.

[0392] (2) Preparation of color dispersion BK (1)

[0393] In the preparation of color dispersion R (1), color dispersion BK (1) was obtained in the same manner as the preparation of color dispersion R (1), except that CI pigment red 254 (R254) was changed to carbon black (BK) (Mitsubishi Chemical, MA77).

[0394] (3) Preparation of photocurable red resin composition R-1

[0395] 44.16 parts by mass of the colorant dispersion R (1) obtained in Preparation Example 1, 0.18 parts by mass of the colorant dispersion BK (1), 2.61 parts by mass of the alkali-soluble resin A solution obtained in Preparation Example 1, 4.18 parts by mass of a multi-functional monomer (product name: Aronics M-305, manufactured by Doagosei Co., Ltd.), 0.46 parts by mass of an oxime ester-based photoinitiator represented by the above formula (A-2), 0.03 parts by mass of a fluorine-based surfactant (product name: Megapark R-08MH, manufactured by DIC Co., Ltd.), and 48.38 parts by mass of PGMEA were added to obtain a photocurable red resin composition R-1.

[0396] (Examples 2 to 12: Preparation of photocurable red resin compositions R-2 to R-12)

[0397] In Example 1, photocurable red resin compositions R-2 to R-12 were obtained in the same manner as photocurable red resin composition R-1, except that the type and / or mass ratio of the red material and the black material and / or the type of photoinitiator were changed as shown in Table 1.

[0398] In addition, the color dispersion of CI pigment red 177 (R177), CI pigment red 291 (R291), or CI pigment green 58 (G58) was obtained as color dispersion R (2), R (3), or G by making the same process as making color dispersion R (1), except that CI pigment red 254 (R254) was changed to CI pigment red 177 (R177), CI pigment red 291 (R291), or CI pigment green 58 (PG58) in the preparation of color dispersion R (1).

[0399] (Example 13: Preparation of Photocurable Red Resin Composition R-13)

[0400] In Example 1, a photocurable red resin composition R-13 was prepared in the same manner as in Example 1, except that colorant dispersion R (1) was used instead of colorant dispersion R (2), and the oxime ester-based photoinitiator represented by formula (A-2) was changed to 1-[4-(phenylthio)phenyl]octane-1,2-dione=2-(O-benzoyloxime) (product name: Yirgacure OXE01, manufactured by BASF).

[0401] (Example 14: Preparation of Photocurable Red Resin Composition R-14)

[0402] 40.07 parts by mass of colorant dispersion R (1), 0.88 parts by mass of colorant dispersion BK (1), 0.71 parts by mass of colorant dispersion G, 2.61 parts by mass of alkali-soluble resin A solution obtained in Preparation Example 1, 4.18 parts by mass of a multi-functional monomer (product name: Aronix M-305, manufactured by Doagosei Co., Ltd.), 0.39 parts by mass of an oxime ester-based photoinitiator represented by formula (A-2), 0.07 parts by mass of an oxime ester-based photoinitiator represented by formula (B-1), 0.03 parts by mass of a fluorine-based surfactant (product name: Megapark R-08MH, manufactured by DIC Co., Ltd.), and 48.24 parts by mass of PGMEA were added to obtain a photocurable red resin composition R-14.

[0403] (Examples 15–20: Preparation of photocurable red resin compositions R-15–R-20)

[0404] Photocurable red resin compositions R-15 to R-20 were prepared in the same manner as in Examples 1, 3, 5, 7, 9, or 11, except that 0.22 parts by mass of a monofunctional thiol compound (2-mercaptobenzoxazole, 2-MBO) was added to each of the photocurable red resin compositions of Examples 1, 3, 5, 7, 9, or 11.

[0405] (Example 21: Preparation of Photocurable Red Resin Composition R-21)

[0406] (1) Preparation of color dispersion R(4)

[0407] In the preparation of colorant dispersion R (1), the PGMEA solution (solid content 35 mass%) of block copolymer 1 of Synthesis Example 1 was changed to the PGMEA solution (solid content 35 mass%) of graft copolymer 2 of Synthesis Example 2, and the colorant dispersion R (4) was obtained in the same manner as the preparation of colorant dispersion R (1). In addition, graft copolymer 2 was salted by phenylphosphonic acid and became salt-type graft copolymer 2.

[0408] (2) Preparation of color dispersion BK (2)

[0409] In the preparation of color dispersion R (4), color dispersion BK (2) was obtained in the same manner as the preparation of color dispersion R (4), except that CI pigment red 254 (R254) was changed to carbon black (BK) (Mitsubishi Chemical, MA77).

[0410] (3) Preparation of photocurable red resin composition R-21

[0411] In Example 1, a photocurable red resin composition R-21 was prepared in the same manner as in Example 1, except that color dispersion R (4) was used instead of color dispersion R (1), and color dispersion BK (2) was used instead of color dispersion BK (1).

[0412] (Examples 22–26: Preparation of photocurable red resin compositions R-22–R-26)

[0413] In Example 21, photocurable red resin compositions R-22 to R-26 were obtained in the same manner as photocurable red resin composition R-21, except that the type and / or mass ratio of the red material and the black material were changed as shown in Table 1.

[0414] In addition, the color dispersion of CI pigment red 177 (R177) or CI pigment red 291 (R291) was obtained as color dispersion R (5) or R (6) by making the same method as making color dispersion R (4), except that CI pigment red 254 (R254) was changed to CI pigment red 177 (R177) or CI pigment red 291 (R291) in the preparation of color dispersion R (4).

[0415] (Comparative Examples 1 to 6: Preparation of comparative photocurable red resin compositions CR-1 to CR-6)

[0416] In Example 1, comparative photocurable red resin compositions CR-1 to CR-6 were obtained in the same manner as photocurable red resin composition R-1, except that only a red material was used without using a black material as shown in Table 1, the type of red material and / or the type of initiator was changed, the ratio of the multifunctional monomer (product name: Aronics M-305, manufactured by Doagosei Co., Ltd.) to the alkali-soluble resin A solution and the initiator was not changed, and the amount of components other than the pigment was changed to the pigment concentration shown in Table 2.

[0417] [Evaluation Method]

[0418] <Transmittance>

[0419] The photocurable red resin composition obtained in each example and each comparative example was applied to a glass substrate (manufactured by NH Technoglass Co., Ltd., “NA35”) having a SiNx film formed thereon using a spin coater so that the cured film had a thickness of 3.0 μm, and then dried at 80°C for 3 minutes using a hot plate to form a film on the substrate. The film was then exposed to ultraviolet light of 50 mJ / cm² using an ultra-high pressure mercury lamp to form a post-exposure film on the SiNx film. After that, a cured film was formed by post-baking in a clean oven at 90°C for 30 minutes.

[0420] Using the OSP-SP200 microspectrometer, the transmission spectrum from 380 nm to 780 nm was measured, and the maximum transmittance from 430 nm to 580 nm, and the maximum and minimum transmittance from 610 nm to 630 nm were measured.

[0421] In addition, the photocurable red resin composition obtained in each example and each comparative example was applied using a spin coater to the SiNx film of a glass substrate (manufactured by NH Technoglass Co., Ltd., “NA35”) and a PET film (thickness 70 μm) having a SiNx film formed on it, respectively, so that the cured film had a thickness of 3.0 μm, and then dried at 80°C for 3 minutes using a hot plate to form a film on the substrate. On this film, a film was formed after exposure by exposing it to ultraviolet light of 50 mJ / cm² using an ultra-high pressure mercury lamp through a photomask (chrome mask) having a pattern with an aperture size of 2 μm to 100 μm to form independent fine lines. Next, spin developing was performed using a 0.05 wt% aqueous potassium hydroxide solution as the developer, and the film was developed by rinsing with pure water after 60 seconds of contact with the developer to obtain a film with an independent fine line pattern. Subsequently, a cured film with an independent fine line pattern was formed by post-baking in a clean oven at 90°C for 30 minutes. Adhesion and solvent resistance evaluations were performed on the obtained cured film.

[0422] Closeness Assessment

[0423] The obtained cured film was observed with an optical microscope to determine how many μm of pattern the mask aperture remained and the line width of the thinnest pattern.

[0424] (Evaluation criteria for closeness assessment)

[0425] AA: Pattern remains up to the mask opening of 4 µm or less (line width of the finest pattern is 4 µm or less)

[0426] A: The line width of the finest pattern is 5 µm to 10 µm or less

[0427] B: The line width of the finest pattern is 11 µm to 20 µm or less

[0428] C: The finest pattern line width is 21 µm to 30 µm or less

[0429] D: The line width of the finest pattern is 31 μm or more

[0430] If the evaluation result is B, the substrate adhesion is good, and if the evaluation result is A, or furthermore AA, the substrate adhesion is excellent.

[0431] <Content Compliance (Internal PGME) Assessment>

[0432] After measuring the film thickness of the obtained cured film, it was immersed in propylene glycol monomethyl ether (PGME) for 10 minutes, air-dried, and the film thickness was measured again. Additionally, a tactile step film thickness gauge “P-15 Tencor” (manufactured by Instruments) was used to measure the film thickness. The residual film rate was calculated as film thickness after solvent immersion / film thickness before solvent immersion × 100.

[0433] (Evaluation criteria for content quality)

[0434] AA: Residue rate after solvent immersion is 98.5% or higher

[0435] A: Residue rate after solvent immersion is 96% or higher and less than 98.5%

[0436] B: Residue rate after solvent immersion is 94% or more and less than 96%

[0437] C: Residue rate after solvent immersion is 92% or more and less than 94%

[0438] D: Residue rate after solvent immersion is less than 92%

[0439] If the evaluation result is B, the content resistance is good, and if the evaluation result is A, or even AA, the content resistance is excellent.

[0440]

[0441]

[0442] In Tables 1 and 2, the abbreviations are as follows.

[0443] ·R254 (CI Pigment Red 254)

[0444] ·R177 (CI Pigment Red 177)

[0445] ·R291 (CI Pigment Red 291)

[0446] · BK (Carbon Black, MA77 manufactured by Mitsubishi Chemical)

[0447] ·G58 (CI Pigment Green 58)

[0448] · A-2: Compound represented by the above chemical formula (A-2)

[0449] · B-1: Compound represented by the above chemical formula (B-1)

[0450] ·OXE01: 1-[4-(phenylthio)phenyl]octane-1,2-dione=2-(O-benzoyloxime)(Trade name: Yirgacure OXE01, manufactured by BASF)

[0451] ·2-MBO(2-mercaptobenzoxazole)

[0452] [Summary of Results]

[0453] In order to improve anti-reflection performance, it is necessary to lower the transmittance of the film, but in the comparative photocurable red resin compositions of Comparative Examples 1 to 6 containing only red material, in order to make the maximum transmittance of 610 nm to 630 nm at a film thickness of 3.0 μm 90% or less, it is necessary to increase the pigment concentration, so even if the same binder component as in the example is used, it was difficult to achieve solvent resistance or substrate adhesion.

[0454] In this regard, in Examples 1 to 26, which are photocurable red resin compositions according to the present invention, a cured film was formed by performing post-baking at a low temperature (90°C) preferred when forming on an organic light-emitting device. When the cured film was formed with a film thickness of 3.0 μm, it was clearly shown that the spectral transmittance at a wavelength of 430 nm to 580 nm was 15.0% or less, and the spectral transmittance at a wavelength of 610 nm to 630 nm was 50.0% or more and 90.0% or less, resulting in a good external light reflection suppression effect. Furthermore, it was revealed that a cured film with good solvent resistance and excellent substrate adhesion can be formed even with low-temperature heat treatment. Accordingly, it was revealed that the photocurable red resin composition according to the present invention is suitable for use in a cured film formed on an organic light-emitting device, and furthermore, the cured film is a thin film capable of suppressing external light reflection, and an organic light-emitting display device with improved flexibility can be manufactured. Explanation of the symbols

[0455] 1: Substrate, 2: Thin-film transistor (TFT), 3: Sealing film, 4: Electrode, 5: Barrier, 6R, 6G, 6B: Organic light-emitting diode, 7: Electrode, 8: Sealing layer, 9R, 9G, 9B: Color-cured film, 10: Light-shielding portion, 11: Sealing film, 20: Anti-external light reflection film, 30: Device substrate equipped with an organic light-emitting diode, 100: Display device

Claims

Claim 1 A photocurable red resin composition used for a cured film formed on an organic light-emitting diode, wherein the photocurable red resin composition contains a colorant, a photopolymerizable compound, and a photoinitiator, wherein the colorant includes a red material and a black material, and the photoinitiator includes at least one compound selected from the compounds represented by the following general formula (A). (during food, R 1 and R 2 are each independently R 11 , OR 11 , COR 11 , SR 11 , CONR 12 R 13 or represents CN, and R 11 , R 12 and R 13 Each independently represents a hydrogen atom, a C1–20 alkyl group, a C6–30 aryl group, a C7–30 arylalkyl group, or a C2–20 heterocyclic group, and R 11 , R 12 and R 13 The hydrogen atom of the group represented as additionally R 21 , OR 21 , COR 21 , SR 21 , NR 22 R 23 , CONR 22 R 23 , -NR 22 -OR 23 , -NCOR 22 -OCOR 23 , NR 22 COR 21 , OCOR 21 , COOR 21 , SCOR 21 , OCSR 21 , COSR 21 , CSOR 21 , may be substituted with a hydroxyl group, a nitro group, CN, or a halogen atom, and R 21 , R 22 and R 23 Each independently represents a hydrogen atom, a C1–20 alkyl group, a C6–30 aryl group, a C7–30 arylalkyl group, or a C2–20 heterocyclic group, and R 21 , R 22 and R 23 The hydrogen atom of the group represented by may additionally be substituted with a hydroxyl group, a nitro group, CN, a halogen atom, or a carboxyl group, and R 11 , R 12 , R 13 , R 21 , R 22 and R 23 The alkylene portion of the group represented by -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 It may contain 1 to 5 groups of -, -SCO-, -COS-, -OCS-, or -CSO- under conditions where oxygen atoms are not adjacent, and R 24 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms, and R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The alkyl portion of the group represented by may have a branched side chain, may be a cyclic alkyl, and R 3 It represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms, and R 3 The alkyl portion of the group represented by may have a branched side chain, may be a cyclic alkyl, and also, R 3 and R 7 and R 3 and R 8 Each may become one to form a ring, and R 3 The hydrogen atom of the group represented as additionally R 21 , OR 21 , COR 21 , SR 21 , NR 22 R 23 , CONR 22 R 23 , -NR 22 -OR 23 , -NCOR 22 -OCOR 23 , NR 22 COR 21 , OCOR 21 , COOR 21 , SCOR 21 , OCSR 21 , COSR 21 , CSOR 21 , may be substituted with a hydroxyl group, a nitro group, CN, or a halogen atom, and R 4 , R 5 , R 6 and R 7 R each independently 11 , OR 11 , SR 11 , COR 14 , CONR 15 R 16 , NR 12 COR 11 , OCOR 11 , COOR 14 , SCOR 11 , OCSR 11 , COSR 14 , CSOR 11 , representing a hydroxyl group, CN, or a halogen atom, and R 4 and R 5 , R 5 and R 6 and R 6 and R 7 Each may become one to form a ring, and R 14 , R 15 and R 16 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, and R 14 , R 15 and R 16 The alkyl portion of the group represented by may have a branched side chain, may be a cyclic alkyl, and R 8 is R 11 , OR 11 , SR 11 , COR 11 , CONR 12 R 13 , NR 12 COR 11 , OCOR 11 , COOR 11 , SCOR 11 , OCSR 11 , COSR 11 , CSOR 11 , represents a hydroxyl group, CN, or halogen atom, and k represents 0 or 1.) Claim 2 A photocurable red resin composition according to claim 1, wherein when a cured film is formed with a film thickness of 3.0 μm, the spectral transmittance at a wavelength of 430 nm to 580 nm is 15.0% or less, and the spectral transmittance at a wavelength of 610 nm to 630 nm is 50.0% or more and 90.0% or less. Claim 3 A photocurable red resin composition according to claim 1 or 2, which does not include a thermosetting resin represented by the following chemical formula 1. Chemical Formula 1 (in the above Chemical Formula 1, n is an integer from 0 to 10.) Claim 4 A photocurable red resin composition according to claim 1 or 2, wherein the colorant further comprises at least one of a green material and a blue material. Claim 5 A photocurable red resin composition according to claim 1 or 2, wherein the black material comprises carbon black. Claim 6 A photocurable red resin composition according to claim 1 or 2, wherein the red material comprises at least one selected from Pigment Red 177, Pigment Red 254, and Pigment Red 291. Claim 7 A photocurable red resin composition according to claim 1 or 2, further comprising a thiol compound. Claim 8 A display device having a cured film of a photocurable red resin composition described in claim 1 or 2 on an organic light-emitting diode. Claim 9 A method for manufacturing a laminate of an organic light-emitting device and an external light-reflecting anti-reflective film, comprising: a process of forming a film by applying a photocurable red resin composition described in claim 1 or 2 onto an organic light-emitting device; a process of irradiating the film with light; a post-baking process of heating the film after the light irradiation; and a process of developing the film after the light irradiation, thereby forming a cured film of the photocurable red resin composition described in claim 1 or 2 onto an organic light-emitting device. Claim 10 A method for manufacturing a laminate of an organic light-emitting element and an external light-reflecting anti-reflective film according to claim 9, wherein the heating temperature in the post-baking process is 130°C or lower. Claim 11 A photocurable red resin composition according to claim 1 or 2, wherein the content of the red material is 70 mass% or more and 99.9 mass% or less with respect to the total amount of the colorant, and the content of the black material is 0.1 mass% or more and 5 mass% or less with respect to the total amount of the colorant. Claim 12 In claim 1 or 2, additionally as a dispersant, the invention comprises at least one salt-type graft copolymer having a constituent unit represented by the following general formula (I) and a constituent unit represented by the following general formula (II), and at least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons forming a salt with at least a portion of the nitrogen site of the constituent unit represented by the following general formula (I) of the graft copolymer, or a block copolymer comprising an A block containing a constituent unit represented by the following general formula (I) and a B block containing a constituent unit derived from a carboxyl group-containing monomer and a constituent unit derived from a (meth)acrylate, and at least one salt-type block copolymer having at least a portion of the nitrogen site of the constituent unit represented by the following general formula (I) of the block copolymer and at least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons forming a salt, wherein the acid value of at least one of the block copolymer and the salt-type block copolymer is 1 A photocurable red resin composition having mgKOH / g to 18 mgKOH / g and a glass transition temperature of 30°C or higher. (of general formula (I), R 71 A hydrogen atom or a methyl group, A 1 is a divalent connector, R 72 and R 73 Each represents a hydrocarbon group that may independently contain a hydrogen atom or a heteroatom, and R 72 and R 73 These may combine to form a ring structure. (of general formula (II), R 71' is a hydrogen atom or a methyl group, A 2 is a direct linkage or a divalent linker, Polymer represents a polymer chain, and the constituent unit of the polymer chain includes a constituent unit derived from (meth)acrylate, and includes at least one constituent unit selected from the group consisting of a constituent unit represented by the following general formula (IV) and a constituent unit represented by the following general formula (IV'). (of general formula (IV), R 74 is a hydrogen atom or a methyl group, A 3 is a divalent connector, R 75 is an ethylene group or a propylene group, R 76 is a hydrogen atom or hydrocarbon group, and m represents a number between 3 and 80. In general formula (IV'), R 74' is a hydrogen atom or a methyl group, A 3' is a divalent connector, R 77 is an alkylene group having 1 to 10 carbon atoms, R 78 is an alkylene group having 3 to 7 carbon atoms, R 79 is a hydrogen atom or a hydrocarbon group, and n represents a number between 1 and 40. Claim 13 A photocurable red resin composition according to claim 1 or 2, further comprising, as a dispersant, a graft copolymer having a constituent unit represented by the following general formula (I) and a constituent unit represented by the following general formula (II), and at least one salt-type graft copolymer in which at least one selected from the group consisting of organic acid compounds and halogenated hydrocarbons forms a salt with at least a portion of the nitrogen sites of the constituent unit represented by the general formula (I) of the graft copolymer. (of general formula (I), R 71 A hydrogen atom or a methyl group, A 1 is a divalent connector, R 72 and R 73 Each represents a hydrocarbon group that may independently contain a hydrogen atom or a heteroatom, and R 72 and R 73 These may combine to form a ring structure. (of general formula (II), R 71' is a hydrogen atom or a methyl group, A 2 is a direct linkage or a divalent linker, Polymer represents a polymer chain, and the constituent unit of the polymer chain includes a constituent unit derived from (meth)acrylate, and includes at least one constituent unit selected from the group consisting of a constituent unit represented by the following general formula (IV) and a constituent unit represented by the following general formula (IV'). (of general formula (IV), R 74 is a hydrogen atom or a methyl group, A 3 is a divalent connector, R 75 is an ethylene group or a propylene group, R 76 is a hydrogen atom or hydrocarbon group, and m represents a number between 3 and 80. In general formula (IV'), R 74' is a hydrogen atom or a methyl group, A 3' is a divalent connector, R 77 is an alkylene group having 1 to 10 carbon atoms, R 78 is an alkylene group having 3 to 7 carbon atoms, R 79 is a hydrogen atom or a hydrocarbon group, and n represents a number between 1 and 40.

Citation Information

Patent Citations

  • Photosensitive coloring composition, coloring spacer, and image display device

    JP2019133167A

  • Colored photo sensitive resin composition, a color filter comprising the same, and a display devide comprising the color filter

    KR1020190096080A