Development of a Continuous Glycolide-L-Lactide Copolymer Production Process
The continuous reactor system for glycolide-lactide copolymer production addresses inefficiencies in batch processes by optimizing reaction conditions, achieving improved molecular weights and conversions while reducing costs and polydispersity.
Patent Information
- Application Number
- KR1020227042966
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-11
- Filing Date
- 2021-05-06
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2041-05-06
AI Technical Summary
Conventional batch processes for producing glycolide-lactide copolymers are inefficient, leading to high costs and suboptimal product quality, with issues in molecular weight and intrinsic viscosity.
A continuous process is developed, involving a multi-stage reactor system comprising a homogenizer, continuous stirred tank reactors (CSTRs), and a plug flow reactor (PFR) to control reaction conditions, ensuring efficient mixing and conversion rates, with catalyst and initiator mixing at lower temperatures to maintain higher molecular weights.
The continuous process reduces production costs and improves product quality by achieving targeted molecular weights and conversions, minimizing polydispersity, and ensuring high purity of the glycolide-lactide copolymers.
Smart Images

Figure 112022131464209-PCT00016_ABST
Abstract
Description
Technology Field
[0001] introduction
[0002] In a conventional method, copolymers such as glycolide-lactide copolymer (PGLA) are produced by a batch process, wherein a fixed ratio of monomer, catalyst, initiator, and optionally dye is loaded into a batch reactor and heated under a controlled oil-heater temperature profile. After maintaining the batch reactor at a target oil temperature (or temperature profile) for a target amount of time, the resulting batch reaction product can be extruded, pelletized, and dried. Subsequently, the batch reactor is cooled and, after undergoing a washing cycle, the raw materials for a new batch are added. Background Technology
[0003] Yu et al. reported on a polymerization model of L-lactide and noted that the initiation rate constant is >200 times higher than the propagation rate constant. [Yu, Y. et al.; Ind. Eng. Chem. Res. 2014, 53, 18, 7333-7342].
[0004] Studies by Kowalski et al. also showed that the reaction between first-note octoate and a hydroxyl-containing initiator induces the formation of an active site, which later serves as a source for a propagation reaction. [Kowalski, A., Duda, A., and Penczek, S.; Macromolecules 2000, 33, 3, 689-695].
[0005] Dechy-Cabaret et al. note that the homopolymerization reactivity ratio of glycolide to L-lactide is close to 10. [Odile Dechy-Cabaret, Blanca Martin-Vaca, and, and Didier Bourissou, Chemical Reviews 2004 104 (12), 6147-6176].
[0006] Additional background information can be found in the literature [Sedush, NG, Chvalun, SN; European Polymer Journal, 62, January 2015, 198]; literature [Yu, Y., Storti G., Morbidelli, M.; Macromolecules, 2009, 42, 8187-8197]; literature [Hiemenz, PC; Polymer Chemistry: The Basic Concepts; 1984; Equation 7.15].
[0007] The present invention relates to a continuous process capable of producing a copolymer, which reduces costs and improves product quality compared to a polymer produced in a batch process. Preferably, the copolymer has a glycolide to L-lactide molar% ratio of 95-5 to 85-15. More preferably, the copolymer has a glycolide to L-lactide molar% ratio of 95-5 to 10-90. The present document also discloses kinetic data obtained by a batch process, which is useful for designing a continuous polymerization process. Brief explanation of the drawing
[0008] Figure 1 illustrates a batch reactor temperature profile. Figure 2 is a graph showing the degree of reaction based on monomer conversion over time at different temperatures. Figure 3 illustrates the weight-average molecular weight of the polymer formed over time in a standard 90:10 glycolide:L-lactide copolymer batch process and at different temperatures. Figure 4 illustrates the intrinsic viscosity of the polymer formed over time in a standard 90:10 glycolide:L-lactide copolymer batch process and at different temperatures. Figure 5 illustrates the extent of the reaction over time for glycolide and L-lactide at 185°C. Figure 6 illustrates the extent of the reaction over time for glycolide and L-lactide at 195°C. Figure 7 illustrates the degree of reaction over time for glycolide and L-lactide at 210°C. Figure 8 illustrates the degree of reaction over time for glycolide and L-lactide at 220°C. Figure 9 illustrates an Arrhenius plot in which the slope and intercept provide the Arrhenius constant and activation energy. Figure 10 illustrates the overall process flow. Specific details for implementing the invention
[0009] Based on the inventors' experiments and the trends in monomer consumption found in the literature on ring-opening polymerization, the inventors hypothesize that polymerization is initiated by the interaction of a catalyst and an initiator. As a result of this rapid initiation step, an active monomer site is formed. In the chain growth type of the polymerization mechanism, a propagation step follows the initiation. In this step, the active site reacts with available monomers to induce ring-opening polymerization.
[0010] The propagation step considers the interactions of individual monomers, glycolide, and L-lactide and is slower than the initiation step. In this model, the following assumptions were applied:
[0011] a) The reactor provides a perfect mixture in which mass transfer is not rate-limited.
[0012] b) The reaction is irreversible.
[0013] c) All polymer chains were initiated by the reaction of the initiator molecule.
[0014] d) Propagation is significantly slower compared to the initiation phase.
[0015] e) The reactivity ratio does not change with temperature.
[0016] The reaction is exemplified by the following formula, where Gly is glycolide, Lac is L-lactide, In is an initiator, and Cat is a catalyst.
[0017]
[0018] Based on the rate-determining propagation step, the monomer consumption rate was quantified by formulating the following rate equation.
[0019]
[0020] In these equations, the rate constant (k) is a function of temperature and is obtained through data-model regression. During the experiment, the concentrations of glycolide and L-lactide, [Gly] and [Lac], are measured. However, the concentrations of the active sites at the ends of the polymer chains, [Gly·] and [Lac·], are not measured. Therefore, it was necessary to express these concentrations in terms of the measured values. During the propagation phase of polymerization, monomers are added one by one to the ends of the chains. At any given moment, the concentration of the active end group must be proportional to the consumption rate of that specific monomer. Therefore, the ratio of active monomer sites at any given time is expressed by the following equation.
[0021]
[0022] Theoretically, the total number of active sites is equal to the number of initiator molecules used in the system.
[0023]
[0024] Rearranging the above equation provides the following expression for the concentration of the active site:
[0025]
[0026] Substituting this into the main velocity equation provides the following velocity equation.
[0027]
[0028] The initial conditions for the copolymerization system consist of the ratio of monomer concentration to monomer consumption rate. The initial concentrations for the 90:10 glycolide:L-lactide system are provided below:
[0029] [Gly] 0 = 9.636 gmol / L
[0030] [Lac] 0 = 1.093 gmol / L
[0031] The initial conditions for the ratio of monomer consumption were determined by assuming that the following equation is true at the start of the reaction. Hiemens [Hiemenz, PC; Polymer Chemistry: The Basic Concepts; 1984] describes the use of this equation in copolymerization at a fixed monomer ratio. Substituting the initial concentrations into the initial condition equation also provides the value of this ratio.
[0032]
[0033] This aimed to fit the degree of reaction based on glycolide and L-lactide data to the reaction rate equation derived by the inventors above. To reduce the degrees of freedom in the inventors' data fitting, the monomer reactivity ratio, r G and r L It was used in the following.
[0034]
[0035] Figures 5 to 8 show a comparison of experimental data versus kinetic models regarding the extent of reactions based on glycolide and L-lactide over time at various temperatures.
[0036] Reactor Design and Process Flow
[0037] As demonstrated above, and in an aspect of the present invention, the reaction kinetics model for glycolide-lactide copolymers accurately formulates reaction rates up to 70 to 90% glycolide conversion and 25 to 45% L-lactide conversion. The utility of this model for designing new polymerization methods for glycolide-lactide copolymers can now be demonstrated as follows. Thus, it is now possible to design a continuous polymerization process for glycolide-lactide copolymers and (since the model can formulate reaction rates in terms of initiator, monomer concentration, and temperature) determine the size of the polymerization reactor (vessel), throughput, and predicted conversion values up to the accuracy or conversion limits of the model. For conversion rates higher than these levels, experimental trials at various mixing and shear rates need to be performed. However, this model significantly reduces the time and cost associated with designing new polymerization processes.
[0038] Homogenizing mixer:
[0039] The first significant constraint in the initial part of the process design is the apparent reduction in Mw (molecular weight) and IV (intrinsic viscosity) values observed during reaction kinetic experiments. (i.e., injecting the catalyst solution and initiator into the high-temperature monomer melt results in a low molecular weight.) Therefore, the design includes a homogenizer as a first unit operation for mixing the monomer, catalyst solution, and initiator at a low temperature (75 to 120°C, more preferably 85 to 95°C) below the reaction temperature. In this first step, copolymer conversion is very small or non-existent. A limited amount of reaction may occur in this vessel. This homogenization or mixing step can be achieved in a continuous process where the components are added continuously and the homogenized mixture is removed continuously. Alternatively, the homogenization step can be performed as a semi-batch process in two or more alternating reactors to fix the product composition.
[0040] Continuous Prepolymer Reactor:
[0041] The homogenizer feeds the prepolymer to a continuous reactor or a series of continuous reactors that polymerize the prepolymer by operating at a constant batch temperature of 140 to 230°C. Preferably, it operates at 150 to 215°C. In a preferred embodiment, the continuous reactor is a continuous stirred tank reactor (CSTR). The conversion rate in these reactor(s) will be limited to 80% for glycolide and 45% for lactide, so the reactor can operate under very efficient mixing conditions. Preferably, the final conversion rate will be 30% to 80% glycolide and 25% and 45% L-lactide. At these conversion rate values, the viscosity of the prepolymer allows for good mixing and transfer of the material to the next stage of the continuous process. The continuous reactor(s) are equipped with a sufficient combination of stirrers and baffles so that the feed does not have the possibility of easily channeling / shortcutting into the outlet stream. The reaction exothermic reaction needs to be controlled to compensate for the exothermic reaction, either by an internal cooling coil or by providing a sufficiently low jacket temperature. The average residence time requirement, τ, for this reactor was calculated using a reaction kinetics model.
[0042]
[0043] Here, [Gly] f is the feed glycolide concentration and [Gly] is the glycolide in the outlet stream.
[0044] For exemplary purposes, residence times and conversion rates were calculated for specific conditions including temperature and residence time. A CSTR operating at 215°C will require an average residence time of 40 minutes to reach 80% glycolide and 45% L-lactide conversion rates. By comparison, each of two CSTRs in series with an average residence time of 12 minutes can achieve the same conversion rates. In this reactor combination, the first CSTR will bring the glycolide conversion rate to 56%, and the second CSTR will further drive the reaction to an 80% glycolide conversion rate.
[0045] The biggest disadvantage of CSTRs is the increase in the polydispersity index (PDI) or heterogeneity index, which is a measure of the molecular mass distribution in a given polymer sample. PDI(M w / M n The molecular weight distribution (defined as the ratio of the weight-average molecular weight to the number-weight-average molecular weight of the polymer) is due to the mixing of the new feed with the already polymerized reactor contents. Using a series of CSTRs can mitigate the molecular weight distribution expansion effect (typically characterized by an increase in PDI) because it avoids backmixing by isolating the partially converted polymer. Based on the PDI requirements for the product, the number of CSTRs in series can be increased or decreased.
[0046] Plug Flow Reactor (PFR):
[0047] The product from the continuous reactor(s) (e.g., CSTR) is fed into a plug flow reactor (PFR) where the conversion rate and mixture viscosity are increased, and backmixing is limited by design. The PFR can be an extruder, a horizontal mixer, a horizontal kneader reactor, or any other suitable reactor having a long residence time. Preferably, the PFR is a horizontal kneader type reactor, where the product is conveyed, continuously mixed, and the conversion rate is increased as it moves along the length of the reactor. An important requirement for this reactor is a long residence time. Based on the final design, a residence time of 20 minutes to 4 hours is required to complete polymerization in a polymerization temperature range of 200 to 230°C. Preferably, the temperature range is 210 to 220°C. Mixing efficiency in this equipment is very important in determining the residence time requirement. Preferably, this type of PFR equipment includes a large free volume and vacuum capacity to remove volatile substances to facilitate the downstream drying process. To minimize the loss of monomer content, a vacuum must be applied downstream from the final part of the equipment or the reaction zone.
[0048] In one embodiment, the PFR reactor is operated at a temperature range of 210 to 220°C with a shorter residence time (20 to 45 minutes) with good devolatilization ability. Although peak polymer molecular weight can be achieved within this short residence time; the monomer conversion rate does not reach the target conversion rates of 99% glycolide and 78% L-lactide. In this process, conversion values can reach approximately the range of 90 to 94% for glycolide and 52 to 58% for L-lactide, and devolatilization can purify the product by removing excess glycolide and L-lactide. Devolatilization can also be performed separately by a subsequent devolatilization process. The process proposed in this embodiment prevents thermal decomposition, color change, and MW drop that may occur due to long residence times.
[0049] In another embodiment, the PFR reactor is operated by the process described in the above embodiment. A slightly excess amount of L-lactide is fed to the homogenizer reactor so that at the end of the process, the final polymer composition is 90% glycolide and 10% L-lactide. The homogenizer feed can similarly be fed to the CSTR reactor, and the CSTR can then be fed to the PFR in a manner similar to the process mentioned in the above embodiment. The amount of additional L-lactide for this purpose can be adjusted based on the CSTR-PFR configuration, processing conditions, and process flow. For example, the feed may have 85 mol% glycolide and 15% L-lactide. The final polymer glycolide:L-lactide ratio may be 90 to 10 mol after removing L-lactide from the final monomer-polymer mixture. The entire process flow is shown in FIG. 10.
[0050] Data-model comparison shows that the model can predict monomer conversion rates up to 70 to 90% glycolide conversion rates in terms of temperature, monomer, and initiator concentrations. The model's rate equation considers all components except the catalyst. The catalyst directly affects the activation energy, Ea term. As the catalyst increases, Ea decreases, leading to an increase in the reaction rate.
[0051] Adding a catalyst / initiator to a high-temperature monomer melt resulted in a lower MW, and consequently, it was recommended to mix the catalyst / initiator with the monomer at a low temperature. This can be accomplished by homogenizing equipment operating at a temperature lower than the reaction temperature (30 to 120°C). While not intended to be theoretical, the reason for the lower temperature may be that the initiator and catalyst have high reactivity or do not disperse well in the monomer over a short period of time.
[0052] Observations and data during the experiment suggest that a process using a PFR-type reactor following the CSTR series is most desirable. Due to viscosity and mixing efficiency limitations, it is suggested to use CSTR-type reactors up to 80% glycolide and 45% L-lactide conversion rates. CSTRs can cause an expansion of the molecular weight distribution. To mitigate this, an appropriate number of CSTRs in series can be used based on the PDI requirements of the final polymer. PFRs require a residence time of 30 minutes to 2 hours. Conventional twin-screw extruders will not achieve this in actual configurations. More specialized PFR-type equipment capable of handling high viscosity with very low backmixing and excellent stirring is key to successful production.
[0053] In summary, this document discloses three aspects of the present invention:
[0054] 1. Observation that higher molecular weight occurs at lower catalyst-initiator mixing temperatures.
[0055] 2. A model is developed to predict polymerization conversion rates of 70 to 90% glycolide and 25 to 45% L-lactide based on temperature.
[0056] 3. The model predicts a multi-stage continuous polymerization method comprising first a mixing step at a low temperature (75 to 120°C, preferably 85 to 95°C), followed by a reaction at a higher temperature (140 to 230°C, preferably 150 to 215°C) in a series of CSTR-type reactors (one or more) up to a glycolide conversion rate of 70 to 90%, a closing reaction in a PFR-type reactor at a glycolide conversion rate of >98%, and finally an optional devolatilization step. The recommended reactor residence times were estimated based on reaction kinetics.
[0057] Experimental results
[0058] Reaction kinetics studies are essential for determining reaction rates in terms of process parameters and ultimately designing a reactor capable of achieving the desired reaction conversion rate. In this regard, a series of experiments were conducted. For these kinetic studies, a 2.5-gallon conical 8CV reactor equipped with a double helical stirrer was used at 10 rpm. The conical reactor was packed with 6 kg of a glycolide:lactide monomer mixture in a 90:10 molar ratio. In all experimental runs, the monomer-to-catalyst molar ratio was 62,500, and the monomer-to-initiator (dodecanol) ratio was 800. Table 1 shows the actual amounts used in the experiments. The catalyst solution used in the experiments was prepared by mixing tin octoate with >90% purity dry toluene. The concentration of the catalyst was a 126 g Sn(Oc)2 / L solution.
[0059] [Table 1]
[0060]
[0061] After the continuous application of vacuum of less than 1 Torr and nitrogen (N2) gas purging, the monomer mixture in the sealed reactor was heated to the catalyst addition temperature (see Table 2). Subsequently, the initiator and catalyst were injected when the batch temperature in the reactor stabilized within ±1°C. The initiator and, a few minutes later, the catalyst solution were injected into the reactor using separate syringes. Since a sudden exothermic reaction is expected, these starting catalyst addition temperatures are intentionally set lower than the batch reaction temperature. The addition of the catalyst triggered a rapid exothermic reaction, which generated a large temperature jump within the reactor within minutes. Table 2 shows the catalyst addition temperatures and reaction temperatures used in the experiment.
[0062] [Table 2]
[0063]
[0064] During the exothermic reaction phase, the batch reactor temperature was controlled and maintained at the set steady-state reaction temperature within ±5°C by rapidly changing the reactor jacket temperature. The batch reactor temperature profiles for these experiments are shown in Fig. 1, where "t=0" is defined as the time at which the first conversion of the monomer into the polymer was detected in the process. For comparison, the standard 90:10 glycolide:L-lactide copolymer batch production temperature profile is also included in Fig. 1.
[0065] Samples were taken from the reactor at regular intervals to perform analyses of monomer conversion rate, molecular weight, intrinsic viscosity (IV), and polydispersity index (PDI). PDI is defined as the ratio of the weight-average molecular weight (Mw) to the number-average molecular weight (Mn). The conversion rate of monomers to polymers at <90% conversion rates was measured in real-time processing using an in-situ near-infrared (NIR) probe. Nuclear magnetic resonance (NMR) analysis of the samples provided monomer conversion rates greater than 90%. Gel permeation chromatography (GPC) was used for molecular weight and PDI analysis.
[0066] Results and Discussion
[0067] FIG. 2 shows the degree of reaction based on the monomer conversion rate over time at different temperatures. The inventors defined the degree of reaction, θ, as the ratio of the moles of a specific monomer consumed to the total moles at the start of the reaction. Thus, when θ=0, there is no reaction, and when θ=1, all of the specific monomer is converted into a polymer. This can be defined as follows in terms of experimentally measured values, where [M]0 is the initial monomer concentration (M may be glycolide or L-lactide) and [M] is the monomer concentration at any given time point.
[0068]
[0069] In Table 2, in addition to the isothermal experiments, a standard 90:10 glycolide:L-lactide copolymer batch process run was also included for comparison with the original process. In the standard batch test, the monomer, catalyst, and initiator were added at room temperature, and all components were heated over time until they reached 215°C. Subsequently, the temperature was maintained at 215°C.
[0070] As predicted by the Arrhenius equation, the conversion rate increases with increasing temperature. Figure 2 shows that the glycolide monomer reacts much faster than the L-lactide monomer. These findings suggest that the polymerization-starting end of the polymer chain is rich in glycolide, with a molar concentration of glycolide in the polymer >90%. As the chain grows longer, more L-lactide can be attached to the backbone. The opposite end of the polymer chain has <90% glycolide. Glycolide reaches a conversion rate of 98.6% after a reaction time of 4 hours at 210°C, but only 71.4% of the initial L-lactide is converted into the polymer backbone. Figures 3 and 4 respectively show the weight-average molecular weight and intrinsic viscosity of the formed polymer over time in a standard 90:10 glycolide:L-lactide copolymer batch process and at different temperatures.
[0071] Surprisingly, it is evident that the standard 90:10 glycolide:L-lactide copolymer batch process polymerization procedure produces copolymer products with higher MW and IV compared to reaction kinetic operations where the initiator and catalyst are added to the reactor at the reaction temperature. Furthermore, as the temperature at which the catalyst and initiator are added increases, the MW and IV of the final copolymer decrease. Isothermal batch experiments at 220°C resulted in an IV of 0.93, whereas experiments at 185°C yielded an IV of 1.24. Since having a polymer with a higher IV is desirable for good product performance, it is preferable to perform isothermal batch polymerization at a lower temperature (185°C instead of 220°C). Additionally, no monomer conversion was detected after the addition of the initiator in any isothermal experiment. Exothermic and monomer conversion can be detected only after the addition of the catalyst.
[0072] The inventors hypothesize that an initiation reaction occurs between the catalyst and the initiator, where active sites begin to form. The initiation reaction allows for a propagation step. Additionally, they hypothesize that high temperatures increase the number of initiation sites, leading to lower MW and IV. Therefore, it is important to maintain a lower temperature during initiation or during the mixing of the initiator and the catalyst. The effect on the continuous process is that the mixing of the catalyst, initiator, and monomer is performed at a relatively low temperature in the first stage (e.g., 75 to 120°C). o It is desirable that this occurs (at C). Subsequently, in a later step, the mixture is additionally (e.g., 210 to 220) for the remaining polymerization process. o Heat to C.
[0073] In FIGS. 3 and 4, the inventors presented two additional sets of data. In the first, as performed in a standard glycolide-L-lactide copolymer batch polymerization procedure, the catalyst and initiator were first mixed with the glycolide and L-lactide monomers at 140°C. After waiting 5 minutes at 140°C, the temperature was raised to 215°C, similar to the standard glycolide-L-lactide copolymer batch polymerization temperature profile. In this case, the MW and IV of the final polymer produced were lower than those in the standard glycolide-L-lactide copolymer batch run. However, the MW and IV values were higher than in any isothermal kinetic run, which supports the hypothesis that the low-temperature catalyst-initiator activation step is important for achieving high molecular weight. In the second, the initiator was already included in the initial mixture, and only the catalyst was added at 210°C to initiate the reaction. This also provided low MW and IV results. This supports one of the embodiments of the present invention, which is an unexpected finding that a higher molecular weight can be achieved in a continuous glycolide-lactide copolymerization process by having an initial catalyst-initiator activation step at a single temperature lower than the second polymerization temperature.
[0074] Surprisingly, experimental reaction degree data showed a good fit for a model using the initial portion of the reaction. This is particularly evident because the reaction mixture had very low viscosity, and the assumption of perfect mixing is easily valid. As shown herein, this demonstrates another embodiment of the invention, a model that predicts the conversion rate of glycolide in polymerization with L-lactide to about 70 to 90 percent.
[0075] The model overestimates the data at higher conversion rates. For example, at 185°C, the model can predict data up to a 70% glycolide conversion rate. Predictions were excellent up to an 80% glycolide conversion rate at 195°C and up to a 90% glycolide conversion rate at 210°C and 220°C. At these good prediction time intervals, only up to 25 to 45% L-lactide was converted. The inventors believe that the deviation in the model occurs for several reasons. First, when the aforementioned monomer conversion rates are exceeded, the viscosity of the monomer melt becomes too high to allow for a perfect mixing environment. Mass transfer rates and mixing rates are important for reaching higher conversion rates. In the inventors' experiments, they used a maximum allowable mixing rate of 10 rpm. Second, in this work, the inventors assumed irreversible reaction kinetics for simplification, which is a good assumption for glycolide. However, 2 to 6% L-lactide generally remains unreacted in experiments due to the thermodynamic equilibrium between the monomer and the polymer. Finally, the inventors did not include any decomposition type of reaction in the model. Any reaction other than a propagation reaction may cause deviations from the model.
[0076] The rate constants in Table 3 were obtained as a result of fitting a model to experimental data obtained from experiments at 185, 195, 210, and 220°C.
[0077] [Table 3]
[0078]
[0079] By substituting the rate constants at different temperatures into the Arrhenius equation below, the activation energy, E a and the Arrhenius constant, A, was calculated so that the reaction rate could be expressed in terms of temperature.
[0080]
[0081] In this equation, T is in Kelvin units, and R is the ideal gas constant, which is 8.314 J / mol·K.
[0082] Figure 9 shows an Arrhenius plot where the slope and intercept can provide the Arrhenius constant and activation energy. The calculated values are presented in Table 4. Note that the active L-lactide terminal requires about 5 kJ / mol higher energy to continue polymerization compared to the active glycolide terminal.
[0083] [Table 4]
[0084]
[0085] Example 1:
[0086] Continuous production of glycolide / L-lactide copolymer
[0087] 5.0 mL of a tin octoate solution (126 g / Sn(Oc)2 / L solution) in 10.87 kg of glycolide, 1.53 kg of L-lactide, 24.3 g of dodecanol, and toluene was charged into an oil-jacketed reactor equipped with a spiral stirrer. The reactor was exposed to multiple vacuum and N2 cycles to remove any moisture from the environment. The reactor jacket was set to a constant temperature of 100°C to melt and homogenize all components. The bottom drain valve of the reactor was opened to continuously transfer the molten material to a second reactor equipped with an oil jacket and a spiral stirrer. The temperature of the transfer line pipe was maintained between 91 and 110°C during the process. The second reactor was operated as a CSTR, and the jacket oil temperature was adjusted to maintain a batch temperature of approximately 180°C. The CSTR level was maintained at a level to provide an average residence time of 60 minutes. Under steady conditions, the reactor provided a poly(glycolide-co-L-lactide) (PLGA) copolymer product comprising 69 to 75% PLGA copolymer and the remainder being unreacted glycolide and L-lactide monomers. The glycolide and L-lactide conversion rates were 71 to 79% and 37 to 42%, respectively. The polymeric portion of the PLGA product consisted of 94.6 mol% glycolide and 5.4 mol% L-lactide with a weight average molecular weight of 51,100 g / mol and a PDI of 1.58.
[0088] Example 2:
[0089] Continuous production of glycolide / L-lactide copolymer
[0090] 9.0 mL of a tin octoate solution (126 g / Sn(Oc)2 / L solution) in 31.06 kg of glycolide, 4.37 kg of L-lactide, 69.4 g of dodecanol, and toluene was charged into an oil-jacketed reactor equipped with a spiral stirrer. The reactor was exposed to multiple vacuum and N2 cycles to remove any moisture from the environment. The reactor jacket was set to a constant temperature of 95°C to melt and homogenize all components.
[0091] The bottom drain valve of the reactor was opened to continuously transfer the molten material to a second reactor equipped with an oil jacket and a spiral stirrer. The liquid temperature in the transfer line was controlled to 78 to 84°C. A piston pump in the transfer line was used to provide a constant supply of 160 g / min into the second reactor. The second reactor was operated as a CSTR, and the jacket oil temperature was adjusted to maintain a batch temperature of 170°C. The reacted monomer mixture was withdrawn from the CSTR at approximately the same rate. During the process, approximately 7.2 kg of reactor contents were present in the CSTR. Under steady conditions, the reactor provided a product having 48 to 62% PLGA copolymer and the remainder being unreacted glycolide and L-lactide monomers. The glycolide and L-lactide conversion rates were 51 to 65% and 21 to 29%, respectively. The polymeric portion of the product consisted of 95.1 mol% glycolide and 4.9 mol% L-lactide monomer units with a weight average molecular weight of 75,800 g / mol and a PDI of 1.82.
[0092] Example 3:
[0093] Failure of continuous manufacturing of glycolide / L-lactide copolymer
[0094] 14.3 mL of a tin octoate solution (126 g / Sn(Oc)2 / L solution) containing 30.67 kg of glycolide, 4.32 kg of L-lactide, 68.5 g of dodecanol, and toluene was charged into an oil-jacketed reactor equipped with a spiral stirrer. The reactor was exposed to multiple vacuum and N2 cycles to remove any moisture from the environment. The reactor jacket was set to a constant temperature of 100°C to melt and homogenize all components. The bottom drain valve of the reactor was opened to continuously transfer the molten material to a second reactor equipped with an oil jacket and a spiral stirrer. The temperature of the transfer line pipe was maintained between 99 and 130°C during the process. The second reactor was operated as a CSTR, and the jacket oil temperature was set to 175°C. After a few minutes of monomer mixture flow through the transfer line, the line became clogged. Due to this clogging, the experiment had to be stopped.
[0095] Example 4:
[0096] Continuous polymerization
[0097] The glycolide / L-lactide copolymer / unreacted monomer mixture from Example 2 is fed into a plug flow type reactor with a melting temperature of 220°C. The residence time in the reactor is 60 minutes. The product is poured into a tray, cooled, ground, and dried. Model kinetics predict that the polymerization results in a conversion rate of 98% glycolide and 72% L-lactide, and the PLGA product consists of 95.9% copolymer, 1.2% glycolide, and 2.9% L-lactide, with a weight-average molecular weight of 86,000 g / mol and a PDI of 2.2.
[0098] Example 5
[0099] The continuous polymerization process of the glycolide / L-lactide copolymer is carried out as follows. 35.04 kg of glycolide, 4.96 kg of L-lactide, 94.4 mL of a first-tin octoate solution (126 g / Sn(Oc)2 / L solution) in toluene are loaded into a homogenizer reactor. The components are mixed at 110°C for 15 minutes. The homogenized mixture is then discharged at a rate of 5 kg / h into the first low-temperature CSTR (CSTR 1) at a constant batch temperature of 150°C and a content-volume of 1.24 L. Two identical homogenizers may be operated in parallel to alternately feed into CSTR 1 during the batch process.
[0100] Alternatively, if the raw material is fed continuously, the homogenizer can operate continuously similarly to the CSTR. The mixture has an average glycolide and 6% L-lactide conversion rate at the outlet of CSTR 1. The material flows from CSTR 1 into a second high-temperature CSTR (CSTR 2) with a volume of 1.63 L at the same rate of 5 kg / h. CSTR 2 has a constant, controlled batch temperature of 215°C. Model kinetics predicts that the material at the outlet of CSTR 2 has an average glycolide and 43% L-lactide conversion rate. The material from CSTR 2 is discharged into a PFR with a constant batch temperature of 220°C at a rate of 5 kg / h and a residence time of 50 minutes. Model kinetics predicts that the PFR provides monomer conversion rates of >94% for glycolide and >58% for L-lactide. The PFR is equipped with mixing equipment for high-viscosity liquids (>1 million cps), large free volume, rapid surface regeneration, and good vacuum capability. Model kinetics predict that the PFR devolatilization capacity removes 0.24 kg / h of unreacted glycolide and 0.23 kg / h of unreacted L-lactide during the process, and that the PFR provides 4.5 kg / h of polymer product, with the polymer product stream containing a PLGA copolymer with less than 0.4% residual glycolide and less than 4% residual L-lactide. In all these processes, the equipment is maintained at ambient pressure, except for the devolatilization segment of the PFR, by providing moisture and oxygen-free dry nitrogen or by venting excess pressure.
[0101] Example 6
[0102] 195 kg / h of glycolide and 27 kg / h of L-lactide are fed into a continuous homogenizer via separate continuous feed hoppers. Additionally, 0.09 L / h of a 0.02 L / h solution of tin octoate (126 g / Sn(Oc)2 / L solution) in 0.52 L / h of dodecanol and toluene is fed to this via a continuous liquid disperser. The components are mixed in the homogenizer at 105°C for an average residence time of 15 minutes. The components are mixed at 110°C for 15 minutes. The homogenized mixture is then discharged into the first CSTR (CSTR 1), having a content-volume of 9.1 gal, at a rate of 222 kg / h. CSTR 1 has a constant, controlled batch temperature of 215°C. Model kinetics predicts that the generated conversion rates at the outlet of CSTR 1 are, on average, 56% glycolide and 36% L-lactide conversions. Subsequently, the material flows from CSTR 1 into a second high-temperature CSTR (CSTR 2) with a constant volume of 9.4 gal at the same rate of 222 kg / h. Model kinetics predicts that the product at the outlet of CSTR 2 has, on average, 80% glycolide and 45% L-lactide conversions. Model kinetics predicts that the product from CSTR 2 is discharged into a PFR at a constant batch temperature of 215°C, a residence time of 1.5 hours, and a throughput of 222 kg / h, and that the PFR is achieved to provide a polymer outlet stream having conversions of >99% glycolide and >78% L-lactide. After the PFR, the material is fed into a horizontal extruder equipped with a devolatilization element and a vacuum port to remove residual monomers. Next, the material is pelletized and collected. Model kinetics predict that the polymer product stream has <0.4% residual glycolide and <4% residual L-lactide. The devolatilization portion of this process can also be carried out by the same PFR reactor mentioned above, which has vacuum, devolatilization capacity, and a large free volume, thereby eliminating an additional devolatilization step.In all of these processes, the equipment is maintained at ambient pressure, except for the devolatilization segment, by providing moisture and oxygen-free dry nitrogen or by discharging excess pressure.
[0103] Summary and Proposal
[0104] A series of isothermal batch reaction kinetics experiments were performed to understand the reaction rate. Reaction conversion, Mw, and IV data were collected using in-situ, real-time near-infrared measurements and off-line sampling techniques. A glycolide-lactide copolymerization kinetics model was developed. Subsequently, parameters for the continuous polymerization process were predicted using this model. The model was then validated by performing continuous polymerization tests using a homogenization reactor and a CSTR.
Claims
Claim 1 A reaction process for preparing a glycolide / L-lactide copolymer formulation, comprising: a) a step of continuously introducing 10 to 95 mol% of glycolide monomer, 5 to 90 mol% of L-lactide monomer, an initiator, and optionally a catalyst into at least one continuous reactor vessel under a dry nitrogen environment, wherein the monomers, initiator, and optional catalyst are mixed at a first low temperature in the range of 75 to 120°C or 85 to 95°C; b) a step of transferring the mixture to a second continuous reactor operating at a second high temperature of 140 to 230°C; and c) a step of exothermizing the blend of glycolide monomer, lactide monomer, initiator, and optional catalyst and maintaining it in a steady state to produce a PLGA copolymer reaction product. Claim 2 A reaction process according to claim 1, wherein the mixture is continuously transferred into a high-temperature continuous reactor through a transfer line, and the transfer line liquid temperature is in the range of 75 to 115°C or 85 to 95°C. Claim 3 A reaction process according to claim 1, wherein glycolide, l-lactide, an initiator, and an optional catalyst are heated to a temperature in the range of 75 to 120°C or in the range of 85 to 95°C in at least two parallel melting vessels and completely melted, and the homogenized contents of the vessels are transferred into the second continuous reactor to provide a continuous flow. Claim 4 A reaction process according to claim 1, wherein the second continuous reactor provides a material having a conversion rate of glycolide and L-lactide to a PLGA copolymer of >30 mol%, and the remainder being unreacted monomers. Claim 5 In claim 1, the reaction process is a continuous stirred tank reactor (CSTR) vessel that operates at a temperature of 140 to 230°C. Claim 6 A reaction process according to claim 1, wherein the copolymer reaction product is further reacted in a plug flow type reactor at a temperature range of 200 to 230°C or 210 to 220°C. Claim 7 A reaction process according to claim 5, wherein more than 98 mol% of the glycolide and more than 70 mol% of the L-lactide monomer react to form the copolymer reaction product, and the remainder is unreacted monomer. Claim 8 A reaction process according to claim 5, further comprising an additional conversion step at elevated temperature and a subsequent optional devolatilization step. Claim 9 In paragraph 8, the devolatilization is performed in a mixer-type plug flow reactor (PFR) or in a separate devolatilization extruder, or a thin film evaporator may be used in the reaction process. Claim 10 A reaction process according to claim 9, wherein more than 90 mol% of the glycolide and more than 52 mol% of the L-lactide monomer react to form the copolymer reaction product, and the remaining monomers are removed from the system through devolatilization. Claim 11 delete
Citation Information
Patent Citations
Preparation method of lactide-glycolide block copolymer
CN107602834A