Alpha-olefin copolymer with improved molecular design for photovoltaic encapsulant

A novel ethylene/alpha-olefin copolymer with specific properties and production process addresses the inefficiencies of conventional encapsulation materials, enabling high extrusion rates and effective crosslinking for improved photovoltaic encapsulation.

KR103044762B1Active Publication Date: 2026-11-06DOW GLOBAL TECHNOLOGIES LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020227025582
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-26
Filing Date
2020-12-17
Publication Date
2026-11-06
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Existing photovoltaic encapsulation materials face challenges in achieving high extrusion rates and efficient crosslinking while balancing optical opacity and mechanical stability, with conventional compositions being economically inefficient and requiring low extrusion speeds.

Method used

A novel ethylene/alpha-olefin copolymer composition with specific characteristics, including total unsaturation ≥ 0.30, molecular weight distribution ≤ 3.0, and a TGIC width parameter B 1/4 ≤ 8.0, produced using a solution polymerization process at elevated reactor temperatures with a biphenylphenol metal complex, enabling high extrusion rates and effective crosslinking.

Benefits of technology

The composition allows for high extrusion rates and improved curing performance, enhancing adhesion to glass and mechanical stability, while maintaining optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022076676516-PCT00024_ABST
    Figure 112022076676516-PCT00024_ABST
Patent Text Reader

Abstract

Composition comprising an ethylene / alpha-olefin copolymer having the following characteristics: a) total unsaturation / 1000C ≥ 0.30; b) molecular weight distribution (MWD) ≤ 3.0; c) TGIC broadness parameter B1 / 4 ≤ 8.0. Solution polymerization process for preparing an ethylene / alpha-olefin / copolymer; said process comprises the step of polymerizing a reaction mixture comprising ethylene, an alpha-olefin, a solvent, and a metal complex described herein in a single reactor at a reactor temperature of 150°C or higher. Method for determining the TGIC broadness parameter B1 / x of a polymer composition comprising one or more olefin-based polymers.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] Cross-reference of related applications

[0002] This application claims priority to international application PCT / CN2019 / 128574 filed on December 26, 2019, the entire contents of which are incorporated herein by reference. Background Technology

[0003] Polymers designed for photovoltaic encapsulation materials must satisfy numerous requirements. To prevent movement of electrical components and wiring during qualification testing and use, polymeric materials must not flow significantly at temperatures up to 85°C. One method to achieve this is to incorporate semicrystalline polymers with melting points above this temperature. However, other encapsulation material requirements, such as high optical opacity and low modulus, are optimized for low-crystallinity polymers. To balance these requirements, low-crystallinity polymers, such as ethylene-vinyl acetate copolymer (EVA) or polyolefin elastomer (POE), are typically used in conjunction with peroxide-based reactive curing packages. While low-crystallinity polymers provide high opacity and low modulus, the curing packages promote a cross-linking reaction that causes the polymer to form a network, thereby providing mechanical stability at high temperatures. This cross-linking reaction typically occurs during module lamination, which is carried out at 150°C.

[0004] Since the film compression process must be carried out at low temperatures to prevent the decomposition of peroxides and the initiation of crosslinking reactions within the extruder, the inclusion of such peroxide-cured packages creates additional design conflicts. Heat generation during extrusion is related to the extrusion speed and polymer viscosity; high viscosity and high compression speeds generate more heat. Therefore, for extruding peroxide-cured compositions, low-viscosity resins extruded at low speeds are preferred. However, low extrusion speeds are economically disadvantageous, and low viscosity is typically achieved through the use of low molecular weight resins. Typically, low molecular weight resins cannot be effectively crosslinked and require higher loading amounts of peroxide-cured packages or longer times in the module stacking process to reach the required level of crosslinking. Both of these solutions are expensive and inefficient.

[0005] There is a need for novel polymers that can be extruded at high speeds and highly crosslinked compared to conventional polymers used for photovoltaic encapsulants. European Patent EP 2958151B1 discloses a resin composition for solar cell encapsulants, which is disclosed to have excellent crosslinking, excellent heat resistance, and excellent transparency. The resin composition contains an ethylene / alpha-olefin copolymer and satisfies the following relationship: N x V ≥ 10, where N is the number of branches derived from the comonomer and V is the total number of vinyl and vinylidene in the copolymer (see, for example, paragraphs

[0030] and

[0031] ). Here, V is 0.17 or greater. Also, refer to Japanese Patent Application Publication JP 2012 / 009688A (machine translation), which has a total unsaturated amount of 0.22 (vinyl, vinylidene, cis and trans vinylene, trisubstituted vinylene); A solar sealing composition is disclosed comprising an ethylene / alpha-olefin copolymer having a density of 0.860 to 0.920 g / cc and an Mz / Mn of 8.0 or less. Other polymer compositions for solar encapsulants are disclosed in the following references: European Patent EP 2637217B1 (a composition comprising an ethylene / alpha-olefin copolymer having, in part, an MFR of 2 to less than 10, a density of 0.865 to 0.884 g / cc, and a Shore A strength of 60 to 85; wherein the MWD may be 1.2 to 3.5) and U.S. Patent No. 8581094 (a composition comprising a polyolefin copolymer having, in part, a density of about 0.90 g / cc or less, a melting point of about 95°C or less, and a 2% secant modulus of about 150 megapascals or less). However, these references do not disclose novel resin designs for achieving high extrusion rates and high crosslinking. There is still a need for such compositions that promote high extrusion rates and high crosslinking. This need has been met by the present invention.

[0006] Composition comprising an ethylene / alpha-olefin copolymer having the following characteristics:

[0007] a) Total unsaturation / 1000C ≥ 0.30;

[0008] b) Molecular weight distribution (MWD) ≤ 3.0;

[0009] c) TGIC broadness parameter B 1 / 4 ≤ 8.0.

[0010] A solution polymerization process for producing an ethylene / alpha-olefin / hybrid polymer, comprising the step of polymerizing a reaction mixture comprising ethylene, an alpha-olefin, a solvent, and a metal complex selected from a) below at a reactor temperature of 150°C or higher in a single reactor:

[0011] a) A biphenylphenol metal complex selected from the following structural formula 1:

[0012]

[0013] Structural Formula 1 , in the above formula,

[0014] M is Zr or Hf, and the metal is in a formal oxidation state of +2, +3, or +4;

[0015] n is 0, 1, or 2, and;

[0016] When n is 1, X is a monodentate or bidentate ligand;

[0017] When n is 2, each X is an independently selected monodentate ligand;

[0018] The above metal complex is entirely neutral;

[0019] Each -Z 1 - and -Z 2 - is independently -O-, -S-, -N(R N )-, or -P(R P Selected from )-;

[0020] R1 and R 8 is independently -H, (C1-C 40 )hydrocarbyl, (C1-C 40 )heterohydrocarbyl, -Si(R C )3, -Ge(R C )3, -P(R P )2, -N(R N )2, -OR C , -SR C , -NO2, -CN, -CF3, R C S(O)-, R C S(O)2-, (R C )2C=N-, R C C(O)O-, R C OC(O)-, R C C(O)N(R)-, (R C )2NC(O)-, selected from the group consisting of a halogen, a radical having chemical formula (I), a radical having chemical formula (II), and a radical having chemical formula (III):

[0021]

[0022] In the above equation, each R 31-35 , R 41-48 , and R 51-59 is independently (C1-C 40 )hydrocarbyl, (C1-C 40 )heterohydrocarbyl, -Si(R C )3, -Ge(R C )3, -P(R P )2, -N(R N )2, -N=CHR C , -OR C , -SR C , -NO2, -CN, -CF3, R C S(O)-, R C S(O)2-, (R C )2C=N-, R C C(O)O-, R C OC(O)-, R C C(O)N(R N )-, (R CSelected from )2NC(O)-, halogen, or -H;

[0023] Each R 2-7 , R 9-16 is independently (C1-C 40 )hydrocarbyl, (C1-C 40 )heterohydrocarbyl, -Si(R C )3, -Ge(R C )3, -P(R P )2, -N(R N )2, -N=CHR C , -OR C , -SR C , -NO2, -CN, -CF3, R C S(O)-, R C S(O)2-, (R C )2C=N-, R C C(O)O-, R C OC(O)-, R C C(O)N(R N )-, (R C Selected from )2NC(O)-, halogen, or -H;

[0024] L is (C1-C 40 )hydrocarbylene or (C1-C 40 )heterohydrocarbylene, where (C1-C 40 ) Hydrocarbylene has a portion containing a linker framework of 1-carbon to 10-carbon atoms, connecting two Z groups (to which L is bonded) in Structural Formula 1; (C1-C 40 )Heterohydrocarbylene has a portion containing a 1- to 10-atom linker framework, connecting two Z groups in Structural Formula 1, and (C1-C 40 )1 to 10 atoms of the 1-atom to 10-atom linker framework of heterohydrocarbylene are each independently carbon atoms or heteroatom groups, and each heteroatom group is independently O, S, S(O), S(O)2, Si(R C )2, Ge(R C )2, P(R C ), or N(RC ) and; each R in structural formula 1 C , R P , and R N is independently (C1-C 30 )hydrocarbyl, (C1-C 30 )heterohydrocarbyl, or -H.

[0025] TGIC width parameter B of a polymer composition comprising one or more olefinic polymers 1 / x A determination method comprising the following steps as a method of determining:

[0026] a) a step of dissolving the above polymer composition in an organic solvent to form a polymer solution;

[0027] b) a step of injecting at least a portion of the polymer solution onto a column comprising a support material including graphite;

[0028] c) a step of cooling the support material at a rate of 0.1℃ / min or higher;

[0029] d) a step of increasing the temperature of the support material to elute the polymer(s) of the polymer composition;

[0030] e) Step to generate a "dwi / dT versus temperature" profile;

[0031] f) For the maximum height of the above profile (dwi / dTi versus temperature), a step of calculating the width of the profile at 1 / x of the maximum height, wherein x > 1;

[0032] g) A step of determining the temperature (Tp) at the maximum height of the above profile;

[0033] h) HDPE peak height from eicosan / iPP / HDPE reference 1 / x Peak width of HDPE (at an elution temperature of 150.0℃) Peak width @ 1 / x A step for calculating ), wherein the reference material is analyzed by TGIC according to steps a) to g);

[0034] i) Based on the following equation B 1 / x Step to calculate:

[0035] Brief explanation of the drawing

[0036] Figure 1 illustrates the elution temperature extrapolation for TGIC temperature correction. The solid line represents experimental data, and the dotted line represents the extrapolation of the elution temperature for two isothermal steps. Figure 2 is a TGIC chromatogram of an eicosan / iPP / HDPE mixture. Figure 3 illustrates the correlation between the elution peak temperature (Tp) and weight% octene of an ethylene-octene copolymer. Figure 4 is the TGIC profile of the POE (POE A) of the present invention. Figure 5 is the TGIC profile of the comparison POE(POE C). Specific details for implementing the invention

[0037] It was found that the ethylene / alpha-olefin / copolymer design provides improved curing performance and excellent extrudability. It was also found that a narrow comonomer distribution and a higher vinyl fraction among the total unsaturated copolymers provide improved adhesion to glass.

[0038] As discussed, a composition comprising an ethylene / alpha-olefin copolymer having the following characteristics is provided:

[0039] a) Total unsaturation / 1000C ≥ 0.30;

[0040] b) Molecular weight distribution (MWD) ≤ 3.0;

[0041] c) TGIC width parameter B 1 / 4 ≤ 8.0.

[0042] The above composition may include a combination of two or more embodiments described herein. The ethylene / alpha-olefin copolymer may include a combination of two or more embodiments described herein.

[0043] The above TGIC width parameter B 1 / 4 is an indication of the breath of the comonomer distribution of the ethylene / alpha-olefin copolymer. B 1 / 4 A smaller value indicates that the comonomer distribution is narrower. In each of the embodiments described herein or a combination of two or more embodiments, the TGIC width parameter B 1 / 4 is 7.5 or less, or 7.0 or less, or 6.5 or less, or 6.0 or less, or 5.5 or less, or 5.0 or less, or 4.8 or less, or 4.6 or less, or 4.4 or less, or 4.2 or less, or 4.0 or less, or 3.8 or less. In each of the embodiments described herein or a combination of two or more embodiments, the TGIC width parameter B 1 / 4 is 1.5 or higher, or 2.0 or higher, or 2.2 or higher, or 2.4 or higher, or 2.6 or higher, or 2.8 or higher, or 3.0 or higher, or 3.2 or higher.

[0044] In each of the embodiments described herein or a combination of two or more embodiments, the ethylene / alpha-olefin copolymer has a density of 0.860 g / cc or more, or 0.861 g / cc or more, or 0.862 g / cc or more, or 0.863 g / cc or more, or 0.864 g / cc or more, or 0.865 g / cc or more, or 0.866 g / cc or more, or 0.867 g / cc or more, or 0.868 g / cc or more, or 0.869 g / cc or more, or 0.870 g / cc (1 cc = 1 cm³). In each of the embodiments described herein or a combination of two or more embodiments, the ethylene / alpha-olefin copolymer has a density of 0.900 g / cc or less, or 0.890 g / cc or less, or 0.888 g / cc or less, or 0.886 g / cc or less, or 0.885 g / cc or less, or 0.884 g / cc or less, or 0.883 g / cc or less, or 0.882 g / cc or less, or 0.880 g / cc or less, or 0.878 g / cc or less.

[0045] In each embodiment or combination of two or more embodiments described herein, the ethylene / alpha-olefin copolymer has a total unsaturated / 1000C of 0.32 or more, or 0.35 or more, or 0.40 or more, or 0.45 or more, or 0.50 or more, or 0.52 or more, or 0.54 or more, or 0.56 or more. In each embodiment or combination of two or more embodiments described herein, the ethylene / alpha-olefin copolymer has a total unsaturated / 1000C of 1.00 or less, or 0.95 or less, or 0.90 or less, or 0.85 or less, or 0.80 or less, or 0.78 or less, or 0.76 or less, or 0.74 or less, or 0.72 or less, or 0.70 or less.

[0046] In each embodiment or combination of two or more embodiments described herein, the ethylene / alpha-olefin copolymer has a molecular weight distribution (MWD = Mw / Mn) of 1.6 or more, or 1.7 or more, or 1.8 or more, or 1.9 or more, or 2.0 or more. In each embodiment or combination of two or more embodiments described herein, the ethylene / alpha-olefin copolymer has a molecular weight distribution MWD of 2.9 or less, or 2.8 or less, or 2.7 or less, or 2.6 or less, or 2.5 or less, or 2.4 or less, or 2.3 or less, or 2.2 or less.

[0047] In each of the embodiments described herein or a combination of two or more embodiments, the copolymer [(vinyl / 1000C)*(Mn)] results in 5.0 x 10 3 (g / mol) or more, or 6.0 x 10⁻⁶ 3 (g / mol) or more, or 7.0 x 10⁻⁶ 3 (g / mol) or more, or 7.5 x 10⁻⁶ 3 (g / mol) or more, or 8.0 x 10⁻⁶ 3 (g / mol) or more, or 8.5 x 10⁻⁶ 3 (g / mol) or more, or 9.0 x 10⁻⁶ 3 (g / mol) or more, or 9.5 x 10⁻⁶ 3 (g / mol) or more, or 10 x 10⁻⁶ 3 It further includes (g / mol) or more. In each of the embodiments described herein or a combination of two or more embodiments, the copolymer has a result of [(vinyl / 1000C)*(Mn)] of 30 x 10 3 (g / mol) or less, or 20 x 10⁻⁶ 3 (g / mol) or less,), or 18 x 10 3 (g / mol) or less, or 16 x 10⁻⁶ 3 (g / mol) or less, or 14 x 10⁻⁶ 3 (g / mol) or less, or 12 x 10⁻⁶ 3It additionally includes those with a value of (g / mol) or less.

[0048] In each embodiment or combination of two or more embodiments described herein, the copolymer further comprises a ratio of [(vinyl / 1000C) / (vinylidene / 1000C)] of 2.0 or more, or 2.2 or more, or 2.4 or more, or 2.6 or more, or 2.8 or more, or 3.0 or more, or 3.1 or more, or 3.2 or more, or 3.3 or more, or 3.4 or more. In each embodiment or combination of two or more embodiments described herein, the copolymer further comprises a ratio of [(vinyl / 1000C) / (vinylidene / 1000C)] of 6.0 or less, or 5.5 or less, or 5.0 or less, or 4.8 or less, or 4.6 or less, or 4.4 or less, or 4.2 or less, or 4.0 or less, or 3.8 or less.

[0049] In each of the embodiments described herein or a combination of two or more embodiments, the ethylene / alpha-olefin copolymer further comprises 50% or more, or 52% or more, or 54% or more, or 56% or more, or 58% or more, or 60% or more, or 62% or more %vinyl. %vinyl = [(vinyl / 1000C) / (total unsaturated / 1000C)] x 100.

[0050] In each embodiment or combination of two or more embodiments described herein, the composition further comprises a peroxide and a silane coupling agent. In each embodiment or combination of two or more embodiments described herein, the composition further comprises a crosslinking coagent.

[0051] An article comprising at least one component formed from any one embodiment or a combination of two or more embodiments described herein is also provided. In each one embodiment or a combination of two or more embodiments described herein, the article is a film. In each one embodiment or a combination of two or more embodiments described herein, the article is a solar cell module.

[0052] The ethylene / alpha-olefin copolymer comprises ethylene and alpha-olefin in the polymerization form. The alpha-olefin may be an aliphatic or aromatic compound. The alpha-olefin is preferably C3-C 20 Aliphatic compounds, preferably C3-C 16 Aliphatic compounds, and more preferably C3-C 10 It is an aliphatic compound. A desirable C3-C 10 Aliphatic alpha-olefins include propylene, 1-butene, 1-hexene, 1-octene, and 1-decene, and more preferably include 1-octene.

[0053] The peroxide (containing at least one "-OO-" group) is preferably, for example, t-butylperoxy-2-ethylhexyl carbonate; di-t-butyl peroxide; t-butyl peroxide; t-butyl-cumyl peroxide; dicumyl peroxide; 2,5-dimethyl-2,5-di-(t-butylperoxy)hexane; di-(t-butyl-peroxy-isopropyl)benzene; t-butyl peroxybenzoate; 1,1-di-(t-butylperoxy)-3,3,5-trimethyl-cyclohexane; 2,5-dimethyl-2,5-di(t-amylperoxy)-hexane; 2,5-dimethyl-2,5-di(t-butyl-peroxy)hexine-3,2,5-dimethyl-2,5-di(t-amylperoxy)hexine-3; Organic peroxides such as di-t-amyl peroxide; 1,3-dimethyl-3-(t-butyl-peroxy)butanol; 1,3-dimethyl-3-(t-amylperoxy)butanol; and mixtures of two or more of these initiators. For example, see TRIGONOX peroxide from AkzoNobel and LUPEROX peroxide from ARKEMA.

[0054] Silane coupling agents include, but are not limited to, vinyltrimethoxysilane and 3-(trimethoxysilyl)propyl methacrylate. Crosslinking agents include, but are not limited to, trialyl cyanurate, trialyl phosphate, trialyl isocyanurate, and 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane. The composition of the present invention may also include one or more additives, such as UV stabilizers, antioxidants, and combinations thereof.

[0055] In each embodiment or combination of two or more embodiments described herein, the composition of the present invention further comprises a thermoplastic polymer different from the ethylene / alpha-olefin copolymer of the present invention in one or more characteristics, such as monomer(s) type and / or amount, Mn, Mw, Mz, MWD, V0.1, V100, RR(V0.1 / V100), or any combination thereof. The polymer comprises, but is not limited to, ethylene-based polymers, propylene-based polymers, and olefin multiblock copolymers. Suitable ethylene-based polymers include, but are not limited to, linear low-density polyethylene (LLDPE), very low-density polyethylene (VLDPE), ultra-low-density polyethylene (ULDPE), homogeneously branched linear ethylene-based polymers, and homogeneously branched substantially linear ethylene-based polymers (i.e., homogeneously branched long-chain branched ethylene polymers). Examples of propylene-based polymers include polypropylene homopolymers and propylene / ethylene copolymers.

[0056] A solution polymerization process for producing an ethylene / alpha-olefin / hybrid polymer is also provided; the process comprises the step of polymerizing a reaction mixture comprising ethylene, an alpha-olefin, a solvent, and a metal complex selected from structural formula 1 described in the contents (SOI) of the invention at a reactor temperature of 150°C or higher in a single reactor.

[0057] The process of the present invention may include a combination of two or more embodiments described herein. The biphenylphenol metal complex may include a combination of two or more embodiments described herein. As used herein, R1 = R 1 , R2 = R 2 , R3 = R 3 etc. Also, notation R a(1) -R a(n) is R a(1) , R a(2) , R a(3) , … , R a(n) It refers to, and "a(1) to a(n)" represent consecutive numbers. For example, R 31 -R 35 is R 31 , R 32 , R 33 , R 34 , R 35 Referring to; R 51 -R 59 is R 51 , R 52 , R 53 , R 54 , R 55 , R 56 , R 57 , R 58 , R 59 It refers to. In each of the chemical formulas (I) to (III), the wavy line represents each chemical formula (R 1 or R 8 It represents the attachment (bonding) between the group) and the rest of the biphenylphenol metal complex.

[0058] In each of the embodiments described herein or a combination of two or more embodiments, in the case of Structural Formula 1, L is -(CH2) n -, where, n = 2 to 4; -CH2C(R a R b )CH2-, here, R a and R b are independently (C1-C 40 )hydrocarbyl, (C1-C 40)heterohydrocarbyl, or -H; or -CH2Ge(R D )2CH2- or -CH2Si(R D )2CH2-, where, each R D is independently -H, (C1-C 40 )hydrocarbyl, (C1-C 40 )heterohydrocarbyl, -Si(R C )3, -Ge(R C )3, -P(R P )2, -N(R N )2, -OR C , -SR C , -NO2, -CN, -CF3, R C S(O)-, R C S(O)2-, (R C )2C=N-, R C C(O)O-, R C OC(O)-, R C C(O)N(R N )-, and (R N Selected from the group consisting of )2NC(O)-; and each R in structural formula 1 C , R P , and R N is independently (C1-C 30 )hydrocarbyl, (C1-C 30 )heterohydrocarbyl, or -H.

[0059] In each of the embodiments described herein or a combination of two or more embodiments, in the case of Structural Formula 1, L is -CH2C(R a R b )CH2-, here, R a and R b are independently (C1-C 40 )hydrocarbyl, (C1-C 40 )heterohydrocarbyl, or -H; or -CH2Ge(R D )2CH2- or -CH2Si(R D )2CH2-, where each R D is independently -H, (C1-C 40 )hydrocarbyl and (C1-C40 )Selected from the group consisting of heterohydrocarbyls; is.

[0060] In each of the embodiments described herein or a combination of two or more embodiments, in the case of Structural Formula 1, -Z 1 - and -Z 2 - is -O- respectively.

[0061] In each of the embodiments described herein or a combination of two or more embodiments, in the case of Structural Formula 1, R 1 and R 8 The radical is identical and is selected from the group consisting of a radical having chemical formula (I), a radical having chemical formula (II), and a radical having chemical formula (III), and is additionally selected from a radical having chemical formula (II).

[0062] In each of the embodiments described herein or a combination of two or more embodiments, in the case of Structural Formula 1, n = 2, and each X is the same and is an unsubstituted alkyl.

[0063] In each of the embodiments described herein or a combination of two or more embodiments, the reaction mixture further comprises a co-catalyst-1 comprising borate and a co-catalyst-2 comprising alumonic acid.

[0064] In each of the embodiments described herein or a combination of two or more embodiments, the process is performed at a reactor temperature of 155°C or higher, or 160°C or higher, or 165°C or higher, or 170°C or higher, or 175°C or higher, or 180°C or higher, or 185°C or higher, or 186°C or higher, or 187°C, or 188°C or higher, or 189°C or higher, or 190°C or higher, with 2.5 x 10 6 More than, or 2.6 x 10 6 More than, or 2.8 x 10 6 More than, or 3.0 x 10 6 More than, or 3.2 x 10 6 More than, or 3.4 x 10 6 More than, or 3.6 x 106 More than, or 3.7 x 10 6 More than, or 3.8 x 10 6 More than, or 3.9 x 10 6 More than, or 4.0 x 10 6 More than, or 4.1 x 10 6 More than, or 4.2 x 10 6 It has a total catalytic efficiency of [(grams of copolymer) / (grams of total catalytic metal)].

[0065] In each of the embodiments described herein or a combination of two or more embodiments, the process is performed at an ethylene / alpha-olefin / hybrid polymer density of 0.860 to 0.900 g / cc, or 0.865 to 0.890 g / cc, or 0.868 to 0.880 g / cc (1 cc = 1 cm³) of 2.5 x 10 6 More than, or 2.6 x 10 6 More than, or 2.8 x 10 6 More than, or 3.0 x 10 6 More than, or 3.2 x 10 6 More than, or 3.4 x 10 6 More than, or 3.6 x 10 6 More than, or 3.7 x 10 6 More than, or 3.8 x 10 6 More than, or 3.9 x 10 6 More than, or 4.0 x 10 6 More than, or 4.1 x 10 6 More than, or 4.2 x 10 6 It has a total catalytic efficiency of [(grams of copolymer) / (grams of total catalytic metal)].

[0066] In each embodiment or combination of two or more embodiments described herein, the process is carried out at a reactor temperature of 155°C or higher, or 160°C or higher, or 165°C or higher, or 170°C or higher, or 175°C or higher, or 180°C or higher, or 185°C or higher, or 186°C or higher, or 187°C, or 188°C or higher, or 189°C or higher, or 190°C or higher. In each embodiment or combination of two or more embodiments described herein, the process is carried out at a reactor temperature of 250°C or lower, or 240°C or lower, or 230°C or lower, or 220°C or lower, or 210°C or lower, or 200°C or lower.

[0067] The term "substituent" refers to a substituent (R) of a hydrogen atom (-H) bonded to a carbon atom or heteroatom of the corresponding unsubstituted compound. S Refers to the substitution with ). Notation "R S " refers to a heteroatom or at least a chemical group containing a heteroatom. The term "substitution" refers to at least one hydrogen atom (-H) bonded to a carbon atom or heteroatom of the corresponding unsubstituted compound being a substituent (R s It means that it has been replaced by ).

[0068] The term "heteroatom" refers to an atom other than hydrogen or carbon. The term "heteroatom group" refers to a chemical group containing a heteroatom or one or more heteroatoms. Examples of heteroatom groups are O, S, S(O), and S(O). 2, Si(R C ) 3, P(R P )2, N(R N )2, -N=C(R C )2, -Ge(R C )2-, or -Si(R C Includes, but is not limited to, )2-, where, each R C and each R P is independently unsubstituted (C1-C 30)hydrocarbyl or -H, and each R N It is unsubstituted (C1-C 30 It is hydrocarbil.

[0069] The term "-H" refers to a hydrogen radical or hydrogen covalently bonded to another atom. "Hydrogen," H, and "-H" are interchangeable and refer to the same thing unless explicitly stated otherwise.

[0070] term "(C1-C 40 "Hydrocarbyl" refers to a hydrocarbon radical having 1 to 40 carbon atoms, and the term "(C1-C 40 ")hydrocarbylene" means a hydrocarbon deradical having 1 to 40 carbon atoms, wherein each hydrocarbon radical and each hydrocarbon deradical are aromatic or non-aromatic, saturated or unsaturated, straight-chain or branched-chain, cyclic (including monocyclic and polycyclic, fused and non-fused polycyclic including dicyclic; including 3 or more carbon atoms) or acyclic, and are unsubstituted or have one or more R S It is replaced with.

[0071] The term "heterohydrocarbon" refers to a molecule or molecular skeleton in which one or more carbon atoms are replaced by heteroatoms. The term "(C1-C 40 "Heterohydrocarbyl" refers to a heterohydrocarbon radical having 1 to 40 carbon atoms, and the term "(C1-C 40 ")heterohydrocarbylene" refers to a heterohydrocarbon deradical having 1 to 40 carbon atoms, and each heterohydrocarbon has one or more heteroatoms. The radical of the heterohydrocarbylene exists on a carbon atom or a heteroatom, and the deradical of the heterohydrocarbylene exists on (1) one or two carbon atoms, (2) one or two heteroatoms, or (3) a carbon atom and a heteroatom. Each (C1-C 40 )heterohydrocarbyl and (C1-C 40)hetero-hydrocarbylenes are not substituted or (one or more R S It can be substituted with ) and may be aromatic or non-aromatic, saturated or unsaturated, straight or branched, cyclic (including monocyclic and polycyclic, fused and non-fused polycyclic) or noncyclic.

[0072] The term "halogen atom" or "halogen" means a radical of a fluorine atom (F), a chlorine atom (Cl), a bromine atom (Br), or an iodine atom (I). The term "halide" means an anionic form of a halogen atom: fluoride (F-), chloride (Cl-), bromide (Br-), or iodide (I-).

[0073] A method for determining the TGIC width parameter B1 / x of a polymer composition comprising one or more olefinic polymers is also provided; said method comprises the steps described in said SOI. said method may include a combination of two or more embodiments described herein.

[0074] In each embodiment or combination of two or more embodiments described herein, the composition comprises at least 50% by weight, or at least 60% by weight, or at least 70% by weight, or at least 80% by weight, or at least 85% by weight, one or more olefinic polymers based on the weight of the composition, and further comprises at least 50% by weight, or at least 60% by weight, or at least 70% by weight, or at least 80% by weight, or at least 85% by weight, one olefinic polymer, and additionally an ethylene / alpha-olefin copolymer.

[0075] In each embodiment or combination of two or more embodiments described herein, the composition comprises at least 90 wt%, or at least 92 wt%, or at least 94 wt%, or at least 96 wt%, or at least 98 wt%, or at least 99 wt% of one or more olefinic polymers based on the weight of the composition, and further comprises at least 90 wt%, or at least 92 wt%, or at least 94 wt%, or at least 96 wt%, or at least 98 wt%, or at least 99 wt% of one olefinic polymer, and additionally comprises an ethylene / alpha-olefin copolymer.

[0076] In each of the embodiments described herein or a combination of two or more embodiments, the composition comprises only one olefinic polymer. In additional embodiments, the olefinic polymer is an ethylene / alpha-olefin copolymer.

[0077] In each of the embodiments described herein or a combination of two or more embodiments, the support material comprises at least 10 weight%, or at least 20 weight%, or at least 30 weight%, or at least 40 weight%, or at least 50 weight%, or at least 60 weight%, or at least 70 weight%, or at least 80 weight%, or at least 85 weight% of graphite based on the weight of the support material.

[0078] In each of the embodiments described herein or a combination of two or more embodiments, the support material comprises at least 90 weight%, or at least 92 weight%, or at least 94 weight%, or at least 96 weight%, or at least 98 weight%, or at least 99 weight% of graphite based on the weight of the support material.

[0079] definition

[0080] Unless otherwise specified, implied by the context, or customary in the art, all parts and percentages are based on weight, and all test methods are in use as of the filing date of this disclosure.

[0081] As used herein, the term "composition" includes not only the composition but also a mixture of materials including reaction products and decomposition products formed from the material of the composition. Any reaction product or decomposition product is typically present in trace or residual amounts.

[0082] As used herein, the term "polymer" refers to a polymeric compound prepared by polymerizing the same or different types of monomers. Accordingly, the general term polymer includes the terms homopolymer (used to refer to a polymer prepared from only one type of monomer, including the fact that trace impurities may be incorporated into the polymer structure) and copolymer as defined below. Trace impurities, such as catalyst residues, may be incorporated into and / or within the polymer. Typically, the polymer is stabilized by one or more stabilizers in very low amounts ("ppm" amounts).

[0083] As used herein, the term "copolymer" refers to a polymer produced by the polymerization of at least two different types of monomers. Accordingly, the term copolymer includes the term copolymer (used to refer to a polymer produced from two different types of monomers) and polymers produced from more than two different types of monomers.

[0084] As used herein, “olefinic polymer” refers to a polymer that comprises 50% by weight or a majority by weight of an olefin, such as ethylene or propylene, in a polymerized form (based on the weight of the polymer), and may optionally comprise one or more comonomers.

[0085] As used herein, the term "propylene-based polymer" refers to a polymer that comprises a majority weight percent of propylene in a polymerized form (based on the weight of the polymer) and may optionally comprise one or more comonomers.

[0086] As used herein, the term “ethylene-based polymer” refers to a polymer that comprises 50% by weight or a majority by weight of ethylene in a polymerized form (based on the weight of the polymer) and may optionally comprise one or more comonomers.

[0087] The term "ethylene / alpha-olefin copolymer" as used herein refers to a random copolymer comprising 50% by weight or a majority by weight of ethylene and alpha-olefin in a polymerized form (based on the weight of the copolymer).

[0088] The term "ethylene / alpha-olefin copolymer" as used herein refers to a random polymer comprising 50% by weight or a majority amount of ethylene monomer and alpha-olefin as only two monomer types in a polymerized form (based on the weight of the copolymer).

[0089] As used herein, the term "solution polymerization" refers to a polymerization process in which the monomer(s) as well as the prepared polymer are dissolved in a polymerization solvent. In one embodiment, the reactor pressure is 1000 psig or less.

[0090] As used herein, "reaction mixture" refers to a mixture comprising one or more monomer types, a solvent, and a metal complex. Typically, the reaction mixture also comprises one or more co-catalysts and hydrogen (H2).

[0091] As used herein with respect to the polymerization process, the term “total catalytic efficiency (units of 10 ≤ 6 g polymer / g total catalytic metal)” refers to the production rate of the polymer formed during the polymerization process (or polymerization run) (e.g., lb / hour) divided by the total feed rate (e.g., lb / hour) of the catalytic metal (e.g., metal(s) from one or more metal complexes) used during the same polymerization process (or polymerization run). Typically, polymerization is a steady-state process.

[0092] As used herein, the term “silane coupling agent” refers to a compound containing at least one “Si” atom and at least one “-CH2-” group and / or at least one “-CH3” group, and the compound forms a chemical link between two materials; for example, between a polymer and an inorganic material.

[0093] As used herein, the term "solar cell (or photovoltaic cell)" refers to a device that converts solar radiation into electricity. Solar cells typically exist in an array pattern.

[0094] As used herein, the term "solar cell module (or solar panel or solar module)" refers to a photovoltaic panel comprising a solar cell assembly.

[0095] As used herein, the terms “laminar,” “laminar,” and similar terms refer to a process in which a plurality of layered materials are joined together under conditions including heat, pressure, and optional vacuum.

[0096] The terms “comprising,” “including,” “having,” and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether specifically disclosed. To avoid any doubt, any composition claimed through the use of the term “comprising” may include any additional additives, adjuvants, or compounds, whether polymeric or not, unless otherwise stated. In contrast, the term “essentially composed of” excludes any other components, steps, or procedures from any subsequent references, except those not essential to the feasibility. The term “composed of” excludes any components, steps, or procedures that are not specifically described or enumerated.

[0097] List of features of some compositions

[0098] A] A composition comprising an ethylene / alpha-olefin copolymer having the following properties:

[0099] a) Total unsaturation / 1000C ≥ 0.30;

[0100] b) Molecular weight distribution (MWD) ≤ 3.0;

[0101] c) TGIC width parameter B 1 / 4 ≤ 8.0.

[0102] B] A composition according to A, wherein the ethylene / alpha-olefin copolymer has a density of 0.860 g / cc or more, or 0.861 g / cc or more, or 0.862 g / cc or more, or 0.863 g / cc or more, or 0.864 g / cc or more, or 0.865 g / cc or more, or 0.866 g / cc or more, or 0.867 g / cc or more, or 0.868 g / cc or more, or 0.869 g / cc or more, or 0.870 g / cc (1 cc = 1 cm³).

[0103] C] A composition according to A] or B], wherein the ethylene / alpha-olefin copolymer has a density of 0.900 g / cc or less, or 0.890 g / cc or less, or 0.888 g / cc or less, or 0.886 g / cc or less, or 0.885 g / cc or less, or 0.884 g / cc or less, or 0.883 g / cc or less, or 0.882 g / cc or less, or 0.880 g / cc or less, or 0.878 g / cc or less.

[0104] D] A composition in any one of the above A]-C](A] to C], wherein the ethylene / alpha-olefin copolymer has a total unsaturated / 1000C of 0.32 or more, or 0.35 or more, or 0.40 or more, or 0.45 or more, or 0.50 or more, or 0.52 or more, or 0.54 or more, or 0.56 or more.

[0105] E] A composition in any one of A] to D] above, wherein the ethylene / alpha-olefin copolymer has a total unsaturated / 1000C of 1.00 or less, or 0.95 or less, or 0.90 or less, or 0.85 or less, or 0.80 or less, or 0.78 or less, or 0.76 or less, or 0.74 or less, or 0.72 or less, or 0.70 or less.

[0106] F] A composition in any one of A] to E] above, wherein the ethylene / alpha-olefin copolymer further comprises 50% or more, or 52% or more, or 54% or more, or 56% or more, or 58% or more, or 60% or more, or 62% or more of %vinyl.

[0107] G] A composition in any one of A] to F] above, wherein the ethylene / alpha-olefin copolymer further comprises 100% or less, or 95% or less, or 90% or less, or 85% or less, or 80% or less, or 78% or less, or 76% or less, or 74% or less, or 72% or less, or 70% or less, or 68% or less, or 66% or less %vinyl.

[0108] H] In any one of A] to G] above, the ethylene / alpha-olefin copolymer [(vinyl / 1000C)*(Mn)] has a result of 5.0 x 10 3 (g / mol) or more, or 6.0 x 10⁻⁶ 3 (g / mol) or more, or 7.0 x 10⁻⁶ 3 (g / mol) or more, or 7.5 x 10⁻⁶ 3 (g / mol) or more, or 8.0 x 10⁻⁶ 3 (g / mol) or more, or 8.5 x 10⁻⁶ 3 (g / mol) or more, or 9.0 x 10⁻⁶ 3 (g / mol) or more, or 9.5 x 10⁻⁶ 3 (g / mol) or more, or 10 x 10⁻⁶ 3A composition further comprising (g / mol) or more.

[0109] I] In any one of A] to H] above, the ethylene / alpha-olefin copolymer [(vinyl / 1000C)*(Mn)] has a result of 30 x 10 3 (g / mol) or less, or 20 x 10⁻⁶ 3 (g / mol) or less,), or 18 x 10 3 (g / mol) or less, or 16 x 10⁻⁶ 3 (g / mol) or less, or 14 x 10⁻⁶ 3 (g / mol) or less, or 12 x 10⁻⁶ 3 A composition further comprising (g / mol) or less.

[0110] J] A composition further comprising, in any one of A] to I] above, that the ethylene / alpha-olefin copolymer has a ratio of [(vinyl / 1000C) / (vinylidene / 1000C)] of 2.0 or more, or 2.2 or more, or 2.4 or more, or 2.6 or more, or 2.8 or more, or 3.0 or more, or 3.1 or more, or 3.2 or more, or 3.3 or more, or 3.4 or more.

[0111] K] A composition further comprising, in any one of A] to J] above, that the ethylene / alpha-olefin copolymer has a ratio of [(vinyl / 1000C) / (vinylidene / 1000C)] of 6.0 or less, or 5.5 or less, or 5.0 or less, or 4.8 or less, or 4.6 or less, or 4.4 or less, or 4.2 or less, or 4.0 or less, or 3.8 or less.

[0112] L] A composition comprising, in any one of A] to K] above, the ethylene / alpha-olefin copolymer further comprising an amount of (vinyl / 1000C) of 0.30 or more, or 0.32 or more, or 0.34 or more, or 0.36 or more.

[0113] M] A composition comprising, in any one of A] to L] above, the ethylene / alpha-olefin copolymer further comprising an amount of (vinyl / 1000C) of 0.60 or less, or 0.58 or less, or 0.56 or less, or 0.54 or less.

[0114] N] A composition in any one of A] to M] above, wherein the ethylene / alpha-olefin copolymer further comprises an amount of (vinylidene / 1000C) of 0.06 or more, or 0.08 or more, or 0.10 or more.

[0115] O] A composition comprising, in any one of A] to N] above, the ethylene / alpha-olefin copolymer further comprising an amount of (vinylidene / 1000C) of 0.20 or less, or 0.18 or less, or 0.16 or less.

[0116] P] A composition in any one of A] to O] above, wherein the ethylene / alpha-olefin copolymer further comprises a sum of [(vinyl / 1000C) + (vinylidene / 1000C)] of 0.42 or more, or 0.44 or more, or 0.46 or more.

[0117] Q] A composition in any one of A] to P] above, wherein the ethylene / alpha-olefin copolymer further comprises a sum of [(vinyl / 1000C) + (vinylidene / 1000C)] of 0.61 or less, or 0.60 or less, or 0.59 or less.

[0118] R] A composition in any one of A] to Q] above, wherein the ethylene / alpha-olefin copolymer has a melt index (I2) of 2.0 g / 10 min or more, or 4.0 g / 10 min or more, or 6.0 g / 10 min or more, or 8.0 g / 10 min or more, or 10.0 g / 10 min or more, or 12.0 g / 10 min or more, or 14.0 g / 10 min or more, or 15.0 g / 10 min or more.

[0119] S] A composition in any one of A] to R] above, wherein the ethylene / alpha-olefin copolymer has a melt index (I2) of 60 g / 10 min or less, or 50 g / 10 min or less, or 45 g / 10 min or less, or 40 g / 10 min or less, or 38 g / 10 min or less, or 36 g / 10 min or less, or 34 g / 10 min or less, or 32 g / 10 min or less.

[0120] T] A composition in any one of A] to S] above, wherein the ethylene / alpha-olefin copolymer has an I10 / I2 of 5.0 or more, or 5.5 or more, or 6.0 or more, or 6.2 or more, or 6.4 or more, or 6.6 or more, or 6.8 or more, or 7.0 or more, or 7.2 or more, or 7.4 or more, or 7.6 or more.

[0121] U] A composition in any one of A] to T] above, wherein the ethylene / alpha-olefin copolymer has an I10 / I2 of 30.0 or less, or 25.0 or less, or 20.0 or less, or 15.0 or less, or 10.0 or less, or 9.0 or less, or 8.8 or less, or 8.6 or less, or 8.4 or less, or 8.2 or less, or 8.0 or less.

[0122] V] A composition in any one of A] to U] above, wherein the ethylene / alpha-olefin copolymer has a number average molecular weight Mn of 12,000 g / mol or more, or 14,000 g / mol or more, or 16,000 g / mol or more, or 18,000 g / mol or more, or 20,000 g / mol or more, or 22,000 g / mol or more, or 24,000 g / mol or more.

[0123] W] A composition in any one of A] to V] above, wherein the ethylene / alpha-olefin copolymer has a number average molecular weight Mn of 50,000 g / mol or less, or 45,000 g / mol or less, or 40,000 g / mol or less, or 38,000 g / mol or less, or 36,000 g / mol or less, or 34,000 g / mol or less, or 32,000 g / mol or less, or 30,000 g / mol or less.

[0124] X] A composition in any one of A] to W] above, wherein the ethylene / alpha-olefin copolymer has a weight average molecular weight Mw of 38,000 g / mol or more, or 40,000 g / mol or more, or 42,000 g / mol or more, or 44,000 g / mol or more, or 46,000 g / mol or more, or 48,000 g / mol or more, or 50,000 g / mol or more.

[0125] Y] A composition in any one of A] to W] above, wherein the ethylene / alpha-olefin copolymer has a weight average molecular weight Mw of 80,000 g / mol or less, or 75,000 g / mol or less, or 70,000 g / mol or less, or 68,000 g / mol or less, or 66,000 g / mol or less, or 64,000 g / mol or less, or 62,000 g / mol or less, or 60,000 g / mol or less.

[0126] Z] A composition in any one of A] to Y] above, wherein the ethylene / alpha-olefin copolymer has a molecular weight distribution (MWD = Mw / Mn) of 1.6 or more, or 1.7 or more, or 1.8 or more, or 1.9 or more, or 2.0 or more.

[0127] AA] A composition in any one of A] to Z] above, wherein the ethylene / alpha-olefin copolymer has a molecular weight distribution MWD of 2.9 or less, or 2.8 or less, or 2.7 or less, or 2.6 or less, or 2.5 or less, or 2.4 or less, or 2.3 or less, or 2.2 or less.

[0128] BB] In any one of the above A] to AA], in the case of an ethylene / alpha-olefin copolymer, the alpha-olefin is C3-C 20 Alpha-olefins and additionally C3-C 10 A composition that is an alpha-olefin.

[0129] CC] A composition in any one of A] to BB] above, wherein in the case of an ethylene / alpha-olefin copolymer, the alpha-olefin is selected from propylene, 1-butene, 1-pentene, 1-hexene, or 1-octene, further selected from propylene, 1-butene, or 1-octene, further selected from 1-butene or 1-octene, and further selected from 1-octene.

[0130] DD] A composition in which, in any one of A] to CC] above, the ethylene / alpha-olefin copolymer is an ethylene / alpha-olefin copolymer.

[0131] EE] A composition wherein, in any one of A] to DD] above, the ethylene / alpha-olefin copolymer is selected from an ethylene / propylene copolymer, an ethylene / butene copolymer, or an ethylene / octene copolymer, further selected from an ethylene / butene copolymer or an ethylene / octene copolymer, and further selected from an ethylene / octene copolymer.

[0132] FF] A composition comprising, in any one of A] to EE] above, an ethylene / alpha-olefin copolymer in an amount of 50.0 wt% or more, or 55.0 wt% or more, or 60.0 wt% or more, or 65.0 wt% or more, or 70.0 wt% or more, or 75.0 wt% or more, or 80.0 wt% or more, or 85.0 wt% or more, or 90.0 wt% or more, or 92.0 wt% or more, or 94.0 wt% or more, based on the weight of the composition.

[0133] A composition comprising, in any one of A to FF, an ethylene / alpha-olefin copolymer in an amount of 95.0 wt% or more, or 95.5 wt% or more, or 96.0 wt% or more, or 96.5 wt% or more, or 97.0 wt% or more, or 97.5 wt% or more, or 98.0 wt% or more, or 98.1 wt% or more, based on the weight of the composition.

[0134] [HH] A composition comprising, in any one of A] to GG] above, an ethylene / alpha-olefin copolymer in an amount of 100.0 wt% or less, or 99.8 wt% or less, or 99.6 wt% or less, or 99.4 wt% or less, or 99.2 wt% or less, or 99.0 wt% or less, or 98.8 wt% or less, or 98.6 wt% or less, or 98.4 wt% or less, or 98.3 wt% or less, based on the weight of the composition.

[0135] II] A composition further comprising a second ethylene / alpha-olefin copolymer different from the ethylene / alpha-olefin copolymer in any one of A] to HH], wherein in one or more polymer properties, additionally in one or more properties selected from comonomer content, I2, I10 / I2, Mn, Mw, Mz, MWD, or any combination thereof, additionally in one or more properties selected from Mw, Mz, MWD, or any combination thereof.

[0136] JJ] In the above II], the composition wherein the second ethylene / alpha-olefin copolymer has a density of 0.860 to 0.890 g / cc, or 0.865 to 0.888 g / cc, or 0.865 to 0.885 g / cc.

[0137] A composition in which, in any one of the above II to JJ, the second ethylene / alpha-olefin copolymer has a melt index (I2) of 0.5 to 50 g / 10 min, or 1.0 to 20.0 g / 10 min, or 5.0 to 10.0 g / 10 min.

[0138] LL] In any one of the above II to KK], in the case of the second ethylene / alpha-olefin copolymer, the alpha-olefin is C3-C 20 It is an alpha-olefin, and additionally C3-C 10 A composition that is an alpha-olefin.

[0139] [MM] A composition in any one of the above II to LL, wherein in the case of the second ethylene / alpha-olefin copolymer, the alpha-olefin is selected from propylene, 1-butene, 1-pentene, 1-hexene, or 1-octene, is selected from propylene, 1-butene, or 1-octene, is further selected from 1-butene or 1-octene, and is further selected from 1-octene.

[0140] NN] A composition in which, in any one of II] to MM] above, the second ethylene / alpha-olefin copolymer is an ethylene / alpha-olefin copolymer.

[0141] OO] A composition in any one of II] to NN] above, wherein the second ethylene / alpha-olefin copolymer is selected from an ethylene / propylene copolymer, an ethylene / butene copolymer, or an ethylene / octene copolymer, further selected from an ethylene / butene copolymer or an ethylene / octene copolymer, and further selected from an ethylene / octene copolymer.

[0142] PP] In any one of the above A] to OO], TGIC width parameter B 1 / 4 A composition having a value of 7.5 or less, or 7.0 or less, or 6.5 or less, or 6.0 or less, or 5.5 or less, or 5.0 or less, or 4.8 or less, or 4.6 or less, or 4.4 or less, or 4.2 or less, or 4.0 or less, or 3.8 or less.

[0143] QQ] In any one of the above A] to OO], TGIC width parameter B 1 / 4 A composition having a value of 1.5 or more, or 2.0 or more, or 2.2 or more, or 2.4 or more, or 2.6 or more, or 2.8 or more, or 3.0 or more, or 3.2 or more.

[0144] [RR] A composition comprising, in any one of [II] to [QQ] above, a peroxide and a silane coupling agent.

[0145] SS] A composition in which, in any one of A] to RR] above, the weight ratio of the peroxide to the silane coupling agent is 0.5 or more, or 1.0 or more, or 1.5 or more, or 2.0 or more, or 2.5 or more, or 3.0 or more, or 3.5 or more, or 4.0 or more.

[0146] A composition in which, in any one of A to SS, the weight ratio of peroxide to silane coupling agent is 7.0 or less, or 6.5 or less, or 6.0 or less, or 5.5 or less, or 5.0 or less, or 4.5 or less.

[0147] A composition comprising, in any one of the above A]-TT](A to TT), further comprising a crosslinking agent.

[0148] [VV] A composition in which, in the above UU], the crosslinking agent is present in an amount of 0.05 wt% or more, or 0.10 wt% or more, or 0.15 wt% or more, or 0.20 wt% or more, or 0.25 wt% or more, or 0.30 wt% or more, or 0.35 wt% or more, or 0.40 wt% or more, or 0.45 wt% or more, or 0.50 wt% or more, based on the weight of the composition.

[0149] [WW] A composition in which, in the above UU] or VV], the crosslinking agent is present in an amount of 3.00 wt% or less, or 2.50 wt% or less, or 2.00 wt% or less, or 1.50 wt% or less, or 1.00 wt% or less, or 0.80 wt% or less, or 0.70 wt% or less, or 0.60 wt% or less, based on the weight of the composition.

[0150] A composition in which, in any one of the above UU to WW], the weight ratio of peroxide to the preparation is 0.5 or more, or 0.8 or more, or 1.0 or more, or 1.1 or more, or 1.2 or more, or 1.3 or more, or 1.4 or more, or 1.5 or more, or 1.6 or more, or 1.8 or more.

[0151] A composition in which, in any one of [YY] to [XX] above, the weight ratio of peroxide to the preparation is 3.0 or less, or 2.8 or less, or 2.6 or less, or 2.4 or less, or 2.3 or less, or 2.2 or less, or 2.0 or less.

[0152] A composition in which, in any one of [ZZ] to [UU] to [YY], the weight ratio of the preparation to the silane coupling agent is 1.0 or more, or 1.2 or more, or 1.4 or more, or 1.6 or more, or 1.8 or more, or 2.0 or more.

[0153] A3] A composition in which, in any one of the above UU] to ZZ], the weight ratio of the preparation to the silane coupling agent is 3.6 or less, or 3.4 or less, or 3.2 or less, or 3.0 or less, or 2.8 or less, or 2.6 or less, or 2.4 or less.

[0154] B3] A composition comprising, in any one of A] to A3] above, a peroxide in an amount of 0.05 wt% or more, or 0.10 wt% or more, or 0.15 wt% or more, or 0.20 wt% or more, or 0.25 wt% or more, or 0.30 wt% or more, or 0.35 wt% or more, or 0.40 wt% or more, or 0.45 wt% or more, or 0.50 wt% or more, or 0.55 wt% or more, or 0.60 wt% or more, based on the weight of the composition.

[0155] C3] A composition comprising, in any one of A] to B3] above, a peroxide in an amount of 5.00 wt% or less, or 4.50 wt% or less, or 4.00 wt% or less, or 3.50 wt% or less, or 3.00 wt% or less, or 2.50 wt% or less, or 2.00 wt% or less, or 1.50 wt% or less, or 1.00 wt% or less, based on the weight of the composition.

[0156] D3] A composition comprising, in any one of A] to C3] above, a silane coupling agent comprising 0.05 wt% or more, or 0.10 wt% or more, or 0.15 wt% or more, or 0.20 wt% or more based on the weight of the composition.

[0157] E3] A composition comprising a silane coupling agent in any one of A] to D3] above, wherein the silane coupling agent is 3.00 wt% or less, or 2.50 wt% or less, or 2.00 wt% or less, or 1.50 wt% or less, or 1.00 wt% or less, or 0.80 wt% or less, or 0.60 wt% or less, based on the weight of the composition.

[0158] F3] A composition comprising, in any one of A] to E3] above, a copolymer comprising 99.0 wt% or more, or 99.1 wt% or more, or 99.2 wt% or more, or 99.3 wt% or more based on the weight of the composition, a peroxide, and a silane coupling agent.

[0159] G3] A composition comprising, in any one of A] to F3] above, a copolymer in an amount of 100.0 wt% or less, or 99.9 wt% or less, or 99.8 wt% or less, or 99.7 wt% or less, or 99.6 wt% or less, or 99.5 wt% or less based on the weight of the composition, a peroxide, and a silane coupling agent.

[0160] H3] A composition comprising, in any one of A] to G3] above, at least one additive selected from a UV stabilizer, an antioxidant, or a combination thereof.

[0161] I3] A composition in which, in the above H3], at least one additive is present in an amount of 0.01 wt% or more, or 0.02 wt% or more, or 0.03 wt% or more, or 0.04 wt% or more, or 0.06 wt% or more, or 0.08 wt% or more, or 0.10 wt% or more, based on the weight of the composition.

[0162] J3] A composition in which, in the above H3] or I3], at least one additive is present in an amount of 2.00 wt% or less, or 1.50 wt% or less, or 1.00 wt% or less, or 0.80 wt% or less, or 0.60 wt% or less, or 0.40 wt% or less, or 0.20 wt% or less, based on the weight of the composition.

[0163] K3] A crosslinking composition formed from any one of the compositions A to J3.

[0164] L3] A composition having an “MH-ML” value of 5.00 or more, or 5.10 or more, or 5.15 or more, or 5.20 or more, or 5.22 or more, or 5.24 or more, or 5.26 or more, or 5.28 or more in the above K3].

[0165] M3] A composition having a gel content (4 + 12 min) of 84% or more, or 85% or more, or 86% or more in the above K3] or L3].

[0166] N3] An article comprising at least one component formed from any one of the compositions A] to M3] above.

[0167] In O3] N3], an article that is a film, an article that is additionally an extruded film and / or a cast film, an article that is additionally an extruded film.

[0168] In P3] N3], an article that is a solar cell module.

[0169] Q3] A process for forming a solar cell module comprising the step of stacking a solar cell array between two film layers, wherein each film layer is independently formed from any one of the compositions A] to M3].

[0170] R3] A process for forming a solar cell module in which, in the above Q3], each film layer is formed from the same composition.

[0171] S3] A solution polymerization process for producing an ethylene / alpha-olefin / hybrid polymer, comprising the step of polymerizing a reaction mixture comprising ethylene, an alpha-olefin, a solvent, and a metal complex selected from a) below at a reactor temperature of 150°C or higher in a single reactor:

[0172] a) A biphenylphenol metal complex selected from the following structural formula 1 described above in the content of the invention (SOI):

[0173]

[0174] Structural Formula 1.

[0175] T3] In the above S3], for structural formula 1, L is -(CH2) n -, where, n = 2 to 4; -CH2C(R a R b )CH2-, here, R a and R b are independently (C1-C 40 )hydrocarbyl, (C1-C 40 )heterohydrocarbyl, or -H; or -CH2Ge(R D )2CH2- or -CH2Si(R D )2CH2-, where, each R D is independently -H, (C1-C 40 )hydrocarbyl, (C1-C 40 )heterohydrocarbyl, -Si(R C )3, -Ge(R C )3, -P(R P )2, -N(R N )2, -OR C , -SR C , -NO2, -CN, -CF3, R C S(O)-, R C S(O)2-, (R C )2C=N-, R C C(O)O-, R C OC(O)-, R C C(O)N(R N )-, and (R N Selected from a group consisting of )2NC(O)-; and;

[0176] Each R in structural formula 1 C , R P , and R N is independently (C1-C 30 )hydrocarbyl, (C1-C 30 ) Heterohydrocarbyl, or -H, solution polymerization process.

[0177] U3] In the above S3] or T3], in the case of Structural Formula 1, each -Z 1 - and -Z 2 - is -O-, solution polymerization process.

[0178] V3] In any one of the above S3] to U3], in the case of Structural Formula 1, R 1 or R 8 A solution polymerization process selected from at least one radical having chemical formula (II) or a radical having chemical formula (I).

[0179] W3] In any one of the above S3] to V3], in the case of Structural Formula 1, R 1 and R 8 A solution polymerization process that is identical and selected from the group consisting of a radical having chemical formula (I), a radical having chemical formula (II), and a radical having chemical formula (III).

[0180] X3] In any one of the above S3] to W3], in the case of Structural Formula 1, R 1 = R 8 = Solution polymerization process, which is a radical having chemical formula (II).

[0181] Y3] In the above X3], in the case of chemical formula (II) of structural formula 1, R 43 = R 46 = unsubstituted alkyl, and additionally unsubstituted (C1-C 10 A solution polymerization process in which alkyl is additionally unsubstituted (C1-C8) alkyl, additionally unsubstituted (C1-C6) alkyl, additionally unsubstituted (C1-C4) alkyl, and additionally t-butyl.

[0182] Z3] In the above X3] or Y3], in the case of chemical formula (II), R 41 = R 42 = R 44 = R 45 = R 47 = R 48 = H, solution polymerization process.

[0183] A4] In any one of the above S3] to Z3], in the case of Structural Formula 1, L is - CH2C(R a R b )CH2-, here R a and R b are independently (C1-C 40 )hydrocarbyl, (C1-C 40 )heterohydrocarbyl, or -H; or -CH2Ge(R D )2CH2- or -CH2Si(R D )2CH2-, where each R D is independently -H, (C1-C 40 )hydrocarbyl, and (C1-C 40 Selected from the group consisting of )heterohydrocarbyl; phosphorus, solution polymerization process.

[0184] B4] In any one of the above S3] to A4], in the case of Structural Formula 1, L is a solution polymerization process selected from i) to iv) below:

[0185] i) -CH2Si(R a )(R b )CH2- or -CH2Ge(R a )(R b )CH2-, here, R a and R b are independently (C1-C 30 )hydrocarbyl or (C1-C 30 )heterohydrocarbilim;

[0186] ii) 1,3-dimethylpropane-1,3-diyl;

[0187] iii) bis(methylene)cyclohexane-1,2-diyl;

[0188] iii) propane-1,3-diyl; or

[0189] iv) Bhutan-1,4-diil.

[0190] C4] In any one of the above S3] to B4], in the case of Structural Formula 1, L is a solution polymerization process selected from i) to iii) below:

[0191] i) -CH2Si(R a )(R b )CH2-, here, R a and R b are each independently unsubstituted (C1-C 10 )alkyl, additionally unsubstituted (C1-C8) alkyl, additionally unsubstituted (C1-C6) alkyl, additionally unsubstituted (C1-C4) alkyl, and additionally unsubstituted (C1-C3) alkyl;

[0192] ii) 1,3-dimethylpropane-1,3-diyl; or

[0193] iii) bis(methylene)cyclohexane-1,2-diyl.

[0194] D4] A solution polymerization process in any one of S3] to C4] above, wherein in the case of structural formula 1, n = 2, and each X is the same and is an unsubstituted alkyl.

[0195] E4] In the above D4], each X is an unsubstituted (C1-C3) alkyl, additionally an unsubstituted (C1-C2) alkyl, and additionally a methyl, in a solution polymerization process.

[0196] F4] A solution polymerization process in any one of S3] to E4] above, wherein R10 = R15 in the case of structural formula 1.

[0197] G4] A solution polymerization process in any one of S3] to F4] above, wherein in the case of structural formula 1, R10 = R15 = halogen and additionally F.

[0198] H4] A solution polymerization process in any one of S3 to G4, wherein R3 = R6 in the case of structural formula 1.

[0199] I4] A solution polymerization process in any one of S3] to H4] above, wherein in the case of structural formula 1, R3 = R6 = unsubstituted alkyl.

[0200] J4] In any one of the above S3] to I4], in the case of structural formula 1, R3 = R6 = unsubstituted (C1-C 12 )alkyl, and additionally unsubstituted (C1-C 10 A solution polymerization process in which the alkyl is additionally unsubstituted (C2-C8)alkyl, additionally unsubstituted (C4-C8)alkyl, and additionally unsubstituted C8alkyl.

[0201] K4] A solution polymerization process in any one of the above S3 to J4, wherein in the case of structural formula 1, R2 = R4 = R5 = R7 = R9 = R11 = R12 = R13 = R14 = R16 = H.

[0202] L4] A solution polymerization process in any one of S3] to K4] above, wherein in the case of structural formula 1, metal M = Zr.

[0203] M4] In any one of the above S3] to L4], the solution polymerization process, wherein structural formula 1 is selected from the following structural formula (1a) or (1b):

[0204] , or .

[0205] N4] In the above M4], the solution polymerization process in which structural formula 1 is structural formula (1a).

[0206] O4] A solution polymerization process in which, in any one of S3] to N4] above, the reaction mixture further comprises a co-catalyst-1 containing borate and a co-catalyst-2 containing alumonic acid.

[0207] P4] In any one of S3] to O4] above, at a reactor temperature of 155°C or higher, or 160°C or higher, or 165°C or higher, or 170°C or higher, or 175°C or higher, or 180°C or higher, or 185°C or higher, or 186°C or higher, or 187°C, or 188°C or higher, or 189°C or higher, or 190°C or higher, 2.5 x 10 6More than, or 2.6 x 10 6 More than, or 2.8 x 10 6 More than, or 3.0 x 10 6 More than, or 3.2 x 10 6 More than, or 3.4 x 10 6 More than, or 3.6 x 10 6 More than, or 3.7 x 10 6 More than, or 3.8 x 10 6 More than, or 3.9 x 10 6 More than, or 4.0 x 10 6 More than, or 4.1 x 10 6 More than, or 4.2 x 10 6 A solution polymerization process having the total catalytic efficiency of [(gram copolymer) / (gram total catalyst metal)].

[0208] Q4] In any one of the above S3] to P4], at an ethylene / alpha-olefin / hybrid polymer density of 0.860 to 0.900 g / cc, or 0.865 to 0.890 g / cc, or 0.868 to 0.880 g / cc, 2.5 x 10 6 More than, or 2.6 x 10 6 More than, or 2.8 x 10 6 More than, or 3.0 x 10 6 More than, or 3.2 x 10 6 More than, or 3.4 x 10 6 More than, or 3.6 x 10 6 More than, or 3.7 x 10 6 More than, or 3.8 x 10 6 More than, or 3.9 x 10 6 More than, or 4.0 x 10 6 More than, or 4.1 x 10 6 More than, or 4.2 x 10 6 A solution polymerization process having the total catalytic efficiency of [(gram copolymer) / (gram total catalyst metal)].

[0209] R4] A solution polymerization process carried out at a reactor temperature of 155°C or higher, or 160°C or higher, or 165°C or higher, or 170°C or higher, or 175°C or higher, or 180°C or higher, or 185°C or higher, or 186°C or higher, or 187°C, or 188°C or higher, or 189°C or higher, or 190°C or higher, in any one of S3] to Q4] above.

[0210] S4] A solution polymerization process carried out at a reactor temperature of 250°C or lower, or 240°C or lower, or 230°C or lower, or 220°C or lower, or 210°C or lower, or 200°C or lower, in any one of S3] to R4] above.

[0211] T4] A solution polymerization process in any one of S3] to S4], wherein the reactor is selected from a continuous stirred tank reactor, a loop reactor, or a plug flow reactor (or tubular reactor), further selected from a continuous stirred tank reactor or a loop reactor, and further selected from a continuous stirred tank reactor.

[0212] [U4] A solution polymerization process in which, in any one of [S3] to [T4] above, the reaction mixture further comprises hydrogen (H2).

[0213] V4] A composition comprising an ethylene / alpha-olefin copolymer formed by any one of the processes S3 to U4.

[0214] W4] TGIC width parameter B of a polymer composition comprising one or more olefinic polymers 1 / x A method for determining; comprising the steps described in SOI.

[0215] X4] A method for determining the composition in which, in the above W4], the composition comprises one or more olefinic polymers in an amount of 50 wt% or more, or 60 wt% or more, or 70 wt% or more, or 80 wt% or more, or 85 wt% or more, or 90 wt% or more, or 92 wt% or more, or 94 wt% or more, or 96 wt% or more, or 98 wt% or more, or 99 wt% or more based on the weight of the composition.

[0216] Y4] A method for determining, wherein the composition comprises one or more olefinic polymers in an amount of 100% or less by weight, or 99% or less by weight, or 98% or less by weight, or 95% or less by weight, based on the weight of the composition.

[0217] Z4] A method of determination in which, in any one of W4] to Y4], the composition comprises only one olefinic polymer.

[0218] A5] A method of determination in which, in any one of the above Z4], the olefin-based polymer is an ethylene / alpha-olefin copolymer and additionally an ethylene / alpha-olefin copolymer.

[0219] B5] A crystallization method in any one of W4 to A5, wherein the support material comprises graphite in an amount of 10 wt% or more, or 20 wt% or more, or 30 wt% or more, or 40 wt% or more, or 50 wt% or more, or 60 wt% or more, or 70 wt% or more, or 80 wt% or more, or 85 wt% or more, or 90 wt% or more, or 92 wt% or more, or 94 wt% or more, or 96 wt% or more, or 98 wt% or more, or 99 wt% or more, based on the weight of the support material.

[0220] C5] A method of determination in any one of W4 to B5, wherein the support material comprises 100 weight% or more, or 99 weight% or more, or 98 weight% or more, or 95 weight% or more, or 90 weight% or more of graphite based on the weight of the support material.

[0221] D5] A determination method in which, in any one of W4] to C5] above, in the case of step d) of the method, the temperature is increased from 25℃ to 170℃, further from 30℃ to 165℃, and further from 30℃ to 160℃.

[0222] E5] A method for determining, wherein in any one of W4] to D5] above, the HDPE has a weight average molecular weight reported as an MWD of 2.3 to 3.0, or 2.4 to 2.9, or 2.5 to 2.8, and a polyethylene equivalent of 100,000 to 140,000 g / mol, or 105,000 to 135,000 g / mol, or 110,000 to 130,000 g / mol, or 115,000 to 125,000 g / mol.

[0223] F5] A method for determining, wherein in any one of W4] to E5] above, for the B1 / x value, x = 1.5 to 6, additionally x = 2 to 6, additionally x = 3 to 6, additionally x = 4 to 6.

[0224] G5] A method of determination in which, in any one of W4] to F5] above, the support material further comprises a filler.

[0225] Test method

[0226] MDR test

[0227] Curing characteristics were measured according to ASTM D5289 using an Alpha Technologies Moving Die Rheometer (MDR) 2000 E with a 0.5-degree arc. For each composition, approximately 4 g of pellets were loaded onto the MDR. The MDR was run at 150°C for 30 minutes, and "time versus torque" profiles were generated over a defined interval. The following data were used from each MDR run: MH (dNm) or maximum torque applied by the MDR during the 30-minute test interval (which generally corresponds to the torque applied at the 30-minute time point); ML (dNm) or minimum torque applied by the MDR during the 30-minute test interval (which generally corresponds to the torque applied at the start of the test interval); and T90 (time taken to reach 90% of the MH value).

[0228] Gel content test

[0229] Each cured film produced from the lamination process (see Experimental Section) was cut into small pieces of "3 mm x 3 mm (approximately 0.5 g sample, Ws)". Subsequently, the sample was packed in a metal mesh (mesh number 120 and weight Wt1) and placed in a 250 ml glass vial holding 100 ml xylene at room temperature for 24 hours. Afterward, the metal mesh and sample were transferred into a 500 ml flask equipped with a condenser and holding 350 ml xylene. After refluxing in boiling xylene under stirring for 5 hours, the packed sample was removed from the xylene, placed in a vacuum oven, and heated at 120°C under vacuum for 2 hours until the sample reached a constant weight. Finally, the sample was weighed along with the metal mesh for weight Wt2. The gel content was calculated by the following equation: Gel content = [(Wt2 - Wt1) / Ws] * 100%. The xylene used is of AR grade with a purity of 99% or higher, is a mixture of ortho, meta, and para isomers, and may contain ethylbenzene.

[0230] Gel permeation chromatography

[0231] The chromatography system consisted of a PolymerChar GPC-IR (Valencia, Spain) high-temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5). The autosampler oven compartment was set to 160°C, and the column compartment was set to 150°C. The column was a four-arm AGILENT "Mixed A" 30 cm 20-micron linear mixed-bed column. The chromatography solvent was 1,2,4-trichlorobenzene containing 200 ppm butylated hydroxytoluene (BHT). The solvent source was nitrogen sparging. The injection volume used was 200 microliters, and the flow rate was 1.0 milliliter / min.

[0232] Calibration of the GPC column set was performed using 21 polystyrene standards with a narrow molecular weight distribution having molecular weights ranging from 580 to 8,400,000 g / mol, with six "cocktail" mixtures arranged with at least a 10-fold interval between each molecular weight. The standards were purchased from Agilent Technologies. Polystyrene standards were prepared with 0.025 grams in 50 milliliters of solvent for molecular weights greater than 1,000,000, and with 0.05 grams in 50 milliliters of solvent for molecular weights less than 1,000,000. The polystyrene standards were dissolved at 80°C for 30 minutes with gentle stirring. The molecular weight of the polystyrene standard peak was converted to the molecular weight of polyethylene using the following Equation 1 (as described in the literature [Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)]):

[0233] (Equation 1), in the above equation, M is the molecular weight, A has a value of 0.4315, and B is equal to 1.0.

[0234] A fifth-order polynomial was used to match each polyethylene-equivalent correction point. To compensate for column resolution and band-broadening effects, A was slightly adjusted (approximately 0.375 to 0.445) so that linear homopolymer polyethylene standards were obtained at 120,000 Mw.

[0235] The total plate count of the GPC column set was determined using decane (prepared with 0.04 g in 50 ml of TCB and dissolved with gentle stirring for 20 minutes). The number of plates (Equation 2) and symmetry (Equation 3) were measured for a 200 microliter injection according to the following equations:

[0236] (Equation 2), in the above equation, RV is the residence volume in milliliters, the peak width is in milliliters, the maximum peak is the maximum height of the peak, and the ½ height is the height of the peak maximum value;

[0237] (Equation 3), where RV is the retention volume in milliliters, the peak width is in milliliters, the maximum peak is the maximum position of the peak, the 1 / 10 height is the 1 / 10 height of the peak maximum, the back peak refers to the peak tail at a retention volume after the maximum peak, and the forward peak refers to the peak at a retention volume before the maximum peak. The number of stages for the chromatography system must be greater than 18,000, and the symmetry must be between 0.98 and 1.22.

[0238] The sample was prepared semi-automatically using PolymerChar "Instrument Control" software, with a target weight of 2 mg / ml, and a solvent (containing 200 ppm BHT) was added to a pre-nitrogen-sparged diaphragm stopper vial via a PolymerChar high-temperature autosampler. The sample was dissolved at 160°C for 2 hours under "low-speed" shaking.

[0239] Mn (GPC) , Mw (GPC) , and Mz (GPC) The calculation was based on GPC results using the internal IR5 detector (measurement channel) of the PolymerChar GPC-IR chromatograph according to Equations 4 to 6, using PolymerChar GPCOne™ software, baseline-subtracted IR chromatograms at each equally spaced data acquisition point (i), and polyethylene equivalent molecular weights obtained from a narrow standard calibration curve for said point (i) from Equation 1. Equations 4 to 6 are as follows:

[0240]

[0241] To monitor deviations over time, a flow marker (decane) was introduced into each sample via a micropump controlled by a PolymerChar GPC-IR system. Using this flow marker (FM), the pump flow rate (flow rate (nominal)) for each sample was linearly corrected to the RV alignment of each decane peak within the sample (RV(FM sample)) relative to the RV alignment of the decane peak within a narrow standard correction (RV(corrected FM)). Subsequently, any change in the decane marker peak over time is assumed to be associated with a linear shift in the flow rate (flow rate (effective)) over the entire run.

[0242] To ensure the RV measurement of the flow marker peak yields maximum accuracy, the peak of the flow marker concentration chromatogram is applied to a quadratic equation using a least-squares fitting routine. Subsequently, the first derivative of the quadratic equation is used to locate the actual peak position. After calibrating the system based on the flow marker peak, the effective flow (for narrow standard correction) is calculated using Equation 7: Flow (Effective) = Flow (Nominal) * (RV (Corrected FM) / RV (FM Sample)) (Equation 7).

[0243] Processing of flow rate marker peaks was performed using PolymerChar GPCOne™ software. Acceptable flow rate correction ensures that the effective flow rate is within ± 0.7% of the nominal flow rate.

[0244] 1H NMR method

[0245] Sample manufacturingApproximately 130 mg of the sample was prepared by adding it to 3.25 g of "50 / 50 by weight tetrachloroethane-d2 / perchloroethylene containing 0.001 M Cr(AcAc)3" in a NORELL 1001-7, 10 mm, NMR tube. The sample was purged to prevent oxidation by bubbling N2 through the solvent for approximately 5 minutes using a pipette inserted into the tube. Next, the tube was capped, sealed with TEFLON tape, and then immersed overnight at room temperature to promote sample dissolution. During storage, the sample was kept in an N2 purging box before and after preparation to minimize exposure to O2. The sample was heated and vortexed at 115°C to ensure homogeneity.

[0246] Data Acquisition Parameters and Data Analysis . 1 ¹H NMR was performed on a Bruker AVANCE 600 MHz spectrometer equipped with a Bruker high-temperature cryoprobe at a sample temperature of 120 °C. Two experiments were conducted to obtain the spectrum, a control spectrum for quantifying total polymer protons, and a dual pre-saturation experiment that suppresses high-intensity peaks associated with polymer chains and enables a high-sensitivity spectrum for quantifying end groups. The control was run with a ZG pulse, 4 scans, SWH 10,000 Hz, AQ 1.82 s, and D 114 s. The dual pre-saturation experiment was performed with a modified pulse sequence, lc1prf2.zz, TD 32768, 64 scans, DS 2, SWH 9,000 Hz, AQ 1.82 s, D 12 s, D 13The experiment was performed for 12 seconds. Unsaturation measurements were made according to the method described below. The area under resonance from the polymer chains (i.e., CH, CH2, and CH3 within the polymer) was measured from the spectrum (control spectrum) obtained during the first experiment described above. The area under the four major types of unsaturation (i.e., vinyl, vinylene, trisubstituted, and vinylidene) was measured from the spectrum obtained during the second (pre-saturation) experiment described above. The spectra of both were normalized to the area under resonance from the solvent. The moles of each unsaturation were calculated by dividing the area under the unsaturation resonance by the number of protons contributing to that resonance. The moles of carbon within the polymer were calculated by dividing the area under the peak for the polymer chains (i.e., CH, CH2, and CH3 within the polymer) by 2. Subsequently, the total amount of unsaturation was expressed as the relative ratio of the total moles of unsaturation to the moles of carbon within the polymer, expressed as the number of unsaturations per 1,000 carbons.

[0247] Melting index

[0248] The melt index I2 of ethylene-based polymers is measured according to ASTM D-1238, condition 190°C / 2.16 kg (melt index I10 at 190°C / 10.0 kg). I10 / I2 is calculated from the ratio of I10 to I2. The melt flow rate MFR of propylene-based polymers is measured according to ASTM D-1238, condition 230°C / 2.16 kg.

[0249] polymer density

[0250] Polymer density is measured according to ASTM D-792.

[0251] High Temperature Thermal Gradient Interaction Chromatography (HT-TGIC or TGIC) – Determination of TGIC Width Parameters

[0252] TGIC measurements were performed using a commercial crystallization elution fractionation (CEF) instrument (Polymer Char, Spain) (Cong, et al., Macromolecules, 2011, 44 (8), 3062-3072). The CEF instrument is equipped with an IR-5 detector. Graphite was used as the stationary phase in an HT TGIC column (U.S. Patent No. 8,476,076 (Freddy, A. Van Damme et al.); U.S. Patent No. 8,318,896 (Winniford et al.)). A single graphite column (250 x 4.6 mm) was used for separation. Graphite was packed within the column using dry packing followed by wet packing technology (European Patent EP 2714226B1 (Cong et al.) and cited references). Graphite (substantially non-porous with high crystallinity) was obtained from Superior Graphite. The experimental parameters are as follows: top oven / transfer line / needle temperature of 150°C, dissolution temperature of 150°C, dissolution stirring setting of 2, pump stabilization time of 15 seconds, pump flow rate for column washing of 0.500 mL / m, pump flow rate for column loading of 0.300 mL / min, stabilization temperature of 150°C, stabilization time of 2.0 min (pre-, before loading into column), stabilization time of 1.0 min (post-, after loading into column), SF (soluble fraction) time of 5.0 min, cooling rate of 3.00°C / min from 150°C to 30°C, flow rate during cooling process of 0.04 mL / min, heating rate of 2.00°C / min from 30°C to 160°C, isothermal time of 10 min at 160°C, elution flow rate of 0.500 mL / min, and injection loop size of 200 microliters. The flow rate during the cooling process was adjusted according to the length of the graphite column so that all polymer fractions remained on the column at the end of the cooling cycle.

[0253] Samples were prepared by a PolymerChar autosampler at a concentration of 4.0 mg / ml in ODCB (defined below) at 150°C for 120 minutes. Silica Gel 40 (particle size 0.2 to 0.5 mm, catalog number 10181-3, EMD) was dried in a vacuum oven at 160°C. For a CEF instrument equipped with an autosampler with an N2 purging function, Silica Gel 40 was packed into three "300 x 7.5 mm" GPC-sized stainless steel columns, and the Silica Gel 40 columns were installed in the pump inlet of the CEF instrument to dry the ODCB. This "silica gel-dried ODCB" is now referred to as "ODCB".

[0254] TGIC data were processed on the PolymerChar (Spain) "GPC One" software platform. Temperature correction was performed with a mixture of about 2 to 6 mg of eicosan and 14.0 mg of isotactic homopolymer polypropylene iPP (molecular weight Mw reported as 150,000 to 190,000 polyethylene equivalents, and polydispersity (Mw / Mn) of 3.6 to 4.0, wherein the iPP DSC melting temperature was measured to be 158 to 159°C (DSC method described herein below)). 14.0 mg of linear homopolymer polyethylene HDPE (comonomer content of 0, weight average molecular weight (Mw) reported as polyethylene equivalent of 115,000 to 125,000 g / mol, and polydispersity of 2.5 to 2.8) was added to a "10 mL vial" filled with 7.0 mL of ODCB. The dissolution time was 2 hours at 160°C.

[0255] For the correction process, a solution of Eicosan, iPP, and HDPE was used. For an elution temperature in the range of 30°C to 150°C, the process consisted of the following steps.

[0256] 1. A step of extrapolating the dissolution temperature for each isothermal step during dissolution according to the heating rate (described in Fig. 1). The solid line is experimental data. The dotted line is the extrapolation of the dissolution temperature for two isothermal steps.

[0257] 2. Step for calculating the lag volume. The temperature (x-axis) corresponding to the IR measurement channel chromatogram (y-axis) is shifted so that the peak maximum value (y-axis) of eicosan matches the elution temperature of 30.0°C. The lag volume is calculated from the temperature difference (30°C - actual elution temperature of the peak maximum of eicosan) obtained by dividing by the heating rate of the above method and then multiplying by the elution flow rate.

[0258] 3. A step of adjusting each recorded elution temperature to this same delayed volume adjustment.

[0259] 4. A step of linearly changing the heating rate so that the maximum temperature of the eicosan elution peak is maintained at 30.0°C, while the observed HDPE reference has a maximum temperature of the elution peak at 150.0°C. The TGIC chromatogram of the eicosan / iPP / HDPE mixture is shown in Fig. 2.

[0260] At least 20 ethylene octene random copolymers were prepared with a single-site catalyst having an Mw (ethylene equivalent weight average molecular weight) in the range of 36,000 to 150,000 and a polydispersity (MWD) of 2.0 to 2.2. The measured elution peak temperature (Tp) of each ethylene octene copolymer and the octene content (weight%) of the copolymer follow the correlations specified in Fig. 3. The molecular weight distribution is measured according to the reference (Cong et al., Macromolecule, 2011, 44 (8), 3062-3072). The octene content is measured by 13C NMR according to U.S. Patent No. 7,608,668 (Li et al.) and the cited reference.

[0261] Data processing for HT-TGIC polymer samples

[0262] A solvent blank (pure solvent injection) was performed under the same experimental conditions as the polymer sample. Data processing for the polymer sample includes: solvent blank subtraction for each detector channel, temperature extrapolation described in the calibration process, temperature compensation with a delay volume determined from the calibration process, and adjustment of the elution temperature axis to a range of 30°C to 160°C calculated from the heating rate of the calibration.

[0263] The chromatogram (measurement channel of the IR-5 detector) was integrated into the PolymerChar "GPC One" software. A straight baseline was plotted from the visible difference when the peak fell into the flat baseline at the high elution temperature (approximately 0 value in the blank-subtracted chromatogram) and the minimum or flat region of the detector signal on the high-temperature side of the soluble fraction (SF).

[0264] The melting temperature of the homopolymer polypropylene, specified as the HT-TGIC melting point of iPP, is determined using differential scanning calorimetry (DSC). The temperature at the maximum heat flow rate relative to a linear baseline was used as the melting point. The linear baseline consisted of the start of melting (above the glass transition temperature) and the end of melting. The temperature was raised from room temperature to 200°C at a rate of 10°C / min and held at 200°C for 5 minutes; lowered to 0°C at a rate of 10°C / min and held at 0°C for 5 minutes; then the temperature was raised from 0°C to 200°C at a rate of 10°C / min, and data was taken from this second heating cycle.

[0265] Width parameter B for the TGIC profile 1 / x Calculation of

[0266] At this institution, parameter B 1 / x B1 / x was defined from TGIC measurements to quantify the respiration of the comonomer distribution in both the comparative and invention samples (see, for example, Fig. 4). The following procedure describes a method for calculating B1 / x from TGIC measurements.

[0267] 1. Both the test sample and the eicosan / iPP / HDPE mixture are run in the same run queue according to the above TGIC method.

[0268] 2. Generate a TGIC chromatogram (dwi / dT versus elution temperature (T) profile).

[0269] 3. For the test sample, each data point for maximum intensity from 35.0°C to 170.0°C is searched to obtain the maximum height from the TGIC chromatogram (dwi / dTi versus temperature), and the corresponding elution temperature of the TGIC chromatogram at the maximum height is defined as the profile temperature (Tp). If the TGIC chromatogram has multiple peaks (excluding the SF peak) and multiple peaks have exactly the same peak height, the peak at the maximum elution temperature is defined as the profile temperature (Tp). The profile width (@1 / x maximum height) is defined as the temperature difference between the forward and backward temperatures at 1 / x of the maximum height. The forward temperature at 1 / x of the maximum height is searched forward from 35.0°C, while the backward temperature at 1 / x of the maximum peak is searched in the opposite direction from 170.0°C.

[0270] 4. Calculate the peak width of HDPE (peak width@1 / x) at 1 / x of the HDPE peak height from the Eicosan / iPP / HDPE reference (at an elution temperature of 150.0°C) (see Fig. 2).

[0271] 5. Next, B 1 / x is calculated based on the following equation:

[0272]

[0273] TGIC width parameter (e.g., B 1 / 4 ) is an indication of the respiration of the comonomer distribution of the ethylene / alpha-olefin copolymer. B 1 / 4 A smaller value indicates a narrower comonomer distribution. A narrow comonomer distribution (smaller B 1 / x It was found that ) is beneficial to the curing effect of POE in PV encapsulation formulations. TGIC chromatography is an important technique for characterizing comonomer content and its distribution (see Fig. 3). The peak width (°C) at a specific portion of the height of the maximum (mass intensity) peak in the TGIC profile can be used to quantify the respiration of the comonomer distribution. However, the absolute value of the peak width is also a chromatography-related experimental factor (reference [Stregel, et al., "Modern size-exclusion liquid chromatography," Wiley, 2 nd It may be affected by the resin comonomer content.

[0274] In the current case, the comonomer distribution is B to minimize bias from experimental factors and the comonomer content within the polymer. 1 / x It was defined using parameters.

[0275] experiment

[0276] Commercial polymers and additives

[0277] Ethylene / 1-octene random copolymer: density 0.873 g / cc, I2 14 g / 10 min (XUS 38669 polyolefin elastomer from The Dow Chemical Company). This copolymer is indicated as "POE 669" in the table below.

[0278] ENGAGE 8407 polyolefin elastomer, ethylene / 1-octene random copolymer from The Dow Chemical Company: density 0.870 g / cc, I2 30 g / 10 min. Indicated as POE 407 in the table below.

[0279] TBEC: tert-butylperoxy-2-ethylhexyl carbonate; LUPEROX TBEC organic peroxide from Arkema. VMMS: 3-(trimethoxysilyl)propyl-methacrylate; silane coupling agent from Dow Corning. Crosslinking agent: trialyl isocyanurate (TAIC).

[0280] Polymer Synthesis and Properties

[0281] The copolymers were each prepared in a 1-gallon polymerization reactor filled with hydraulic pressure and operating under normal conditions. The catalyst and co-catalyst are listed in Table 1. The solvent, hydrogen, catalyst, and co-catalyst were supplied to the reactor according to the process conditions outlined in Tables 2a through 2c. The solvent was ISOPAR E supplied by the ExxonMobil Chemical Company. The reactor temperature was measured at or near the reactor outlet. The copolymers were isolated and pelletized.

[0282] POE characteristics are summarized in Table 3. Desaturation measurements from 1H NMR are summarized in Table 4. TGIC results are summarized in Table 5.

[0283] [Table 1]

[0284]

[0285] [Table 2a]

[0286]

[0287] [Table 2b]

[0288]

[0289] [Table 2c]

[0290]

[0291] [Table 3]

[0292]

[0293] [Table 4]

[0294]

[0295] [Table 5]

[0296]

[0297] POE peroxide cured formulation

[0298] The POE peroxide curing compositions are shown in Tables 6 and 7. To ensure that the peroxide, the agent, and the silane are well mixed into the formulation, polymer pellets (98.25 wt%) were immersed in a curing additive (1.00 wt% peroxide, 0.50 wt% crosslinking agent, and 0.25% silane coupling agent) in a sealed fluorinated high-density polyethylene container. The immersion (absorption) process was carried out at 50°C for 5 hours until no liquid residue was visible adhering to the container. To ensure that the peroxide, silane, and agent were homogeneously absorbed by the pellets, the container was shaken for 30 seconds every 30 minutes during the absorption process.

[0299] Fabrication of stacked samples

[0300] Crosslinked POE films were prepared using two slightly different manufacturing conditions (A and B below). A PENERGY L036 laminater was used for each preparation.

[0301] A) Sample preparation by lamination process using a glass substrate (Table 6)

[0302] Inside the laminater, approximately 2.5 g of pellet sample, infused with peroxide, silane, and preparation, was placed on a PTFE film (0.24 mm thick) on top of an organic substrate (3 mm thick). A metal frame having a thickness of 1 mm was placed around the sample as a spacer to ensure the cross-linked POE had a thickness of approximately 1 mm. Subsequently, another PTFE film (0.24 mm thick) was placed on top of the sample. Lamination was performed at a set temperature of 150°C. The heating process included the following two steps: Step 1 -- preheating for 4 minutes under vacuum (-100 kPa) without pressure; and Step 2 -- 12 minutes under a pressure of 1 bar. After the lamination cycle, the cross-linked film was removed for further gel measurements.

[0303] B) Sample preparation by additive manufacturing process using a metal substrate (Table 7)

[0304] Inside the laminater, a pellet sample of approximately 2.5 g, infused with peroxide, silane, and preparation, was placed on a PTFE film (0.24 mm thick) on top of a metal substrate (1.8 mm thick). A PTFE frame with a thickness of 0.5 mm was placed around the sample as a spacer to ensure the cross-linked POE had a thickness of approximately 0.5 mm. Subsequently, another PTFE film (0.24 mm thick) was placed on top of the sample. Lamination was performed at a set temperature of 150°C. The heating process included the following two steps: Step 1 -- preheating for 4 minutes under vacuum (-100 kPa) without pressure; and Step 2 -- 10 or 16 minutes under a pressure of 1 bar. After the lamination cycle, the cross-linked film was removed for further gel measurements.

[0305] Adhesion measurement for glass after lamination

[0306] A film (100 mm x 150 mm x 0.5 mm) was prepared by compression molding of formulated resin pellets using a Lab Tech LP-S-50 compression molder under the following conditions: preheating for 4 minutes at 100°C without pressure; and 2 minutes at 100°C and 100 MPa. After molding, the film was placed on a glass substrate (measured at 100 mm x 150 mm x 3 mm) and covered with a polyester backing sheet. Subsequently, the sample was passed through a lamination process (laminator SHUNHONG SH-X-1000) at 150°C under the following conditions: preheating for 4 minutes under vacuum (-100 kPa) without pressure; and 16 minutes at a pressure of 1 bar.

[0307] After lamination, the laminated film and backing sheet were further cut and divided into three pieces, each having a width of 1 inch and a length of 150 mm. A 180° peel test was performed on the three specimens by pulling the laminated film and backing sheet from a glass substrate using an INSTRON 5565. The average of the three results was recorded.

[0308] Summary of Results

[0309] During the production process of PV encapsulant films, the processability of the formulated material is limited by the shear heating of the polymer during the extrusion process. Since peroxides in the PV encapsulant film formulation decompose at temperatures above 110°C and crosslink the POE, the RPM and resin extrusion speed may not exceed the threshold range that allows the resin melting temperature to sufficiently exceed 110°C. It is known that POE with a higher melt index (i.e., POE with lower viscosity) can have improved processability or throughput within the extruder due to lower viscosity and reduced shear heating. In this case, both the comparative and inventive samples were selected to have a relatively high melt index to ensure excellent processability of the formulation. However, in the case of high melt index resins, the crosslinked film typically has a relatively low degree of curing. Consequently, it is very important to improve the curing effect for these high melt index resins.

[0310] To compare the curing between POEs with different levels of unsaturation, the curing effect of formulations containing POEs with similar melt index / processability, density, MWD, and comonomer distribution was tested (see Table 6). In this invention, Example 1 was compared with Comparative Example 1 (POE with a melt index of approximately 14 dg / min), and Example 2 was compared with Comparative Example 2 (POE with a melt index of approximately 30 dg / min). The compositions of the present invention containing high unsaturated POE clearly exhibited an improved (higher) MDR torque change (MH-ML) and a higher gel content after vacuum lamination of "4 + 12 mins".

[0311] The results in Table 7 compare the curing effects of encapsulating film formulations formed from the mentioned POE. Films formed from the compositions of the present invention (POE with a narrow MWD and narrow comonomer distribution in addition to high unsaturation) yield optimal curing performance with improved MDR torque change (MH-ML) and higher gel content after "4 + 10 min" vacuum lamination and "4 + 16 min" vacuum lamination. It is also worth noting that the compositions of the present invention (containing POE with a higher fraction of vinyl groups relative to total unsaturation, a higher vinyl / vinylidene ratio, and a narrower comonomer distribution) have excellent adhesion to glass.

[0312] [Table 6]

[0313]

[0314] [Table 7]

[0315]

Claims

Claim 1 A polymer composition comprising an ethylene / alpha-olefin copolymer having the following characteristics: a) total unsaturation / 1000C ≥ 0.30; b) molecular weight distribution (MWD) ≤ 3.0; c) TGIC broadness parameter B 1 / 4 ≤ 8.0 where the polymer composition further comprises a peroxide, a silane coupling agent, and a crosslinking coagent, and TGIC width parameter B 1 / 4 A polymer composition obtained by a method comprising the following steps: a) dissolving the polymer composition in an organic solvent to form a polymer solution; b) injecting at least a portion of the polymer solution onto a column comprising a support material comprising graphite; c) cooling the support material at a rate of 0.1°C / min or higher; d) increasing the temperature of the support material to elute the polymer(s) of the polymer composition; e) generating a "dwi / dT versus temperature" profile; f) calculating the width of the profile at 1 / x of the maximum height for the maximum height of the profile (dwi / dT versus temperature), wherein x = 4; g) determining the temperature (Tp) at the maximum height of the profile; h) of the HDPE peak height from an eicosan / iPP / HDPE reference. 1 / x Peak width of HDPE (at an elution temperature of 150.0℃) Peak width @ 1 / x A step for calculating ), wherein the reference is analyzed by the TGIC according to steps a) to g); step i) based on the following equation B 1 / x Step to calculate: . Claim 2 A polymer composition according to claim 1, wherein the ethylene / alpha-olefin copolymer has a density of 0.860 g / cc or more. Claim 3 A polymer composition according to claim 1 or 2, wherein the ethylene / alpha-olefin copolymer has a density of 0.900 g / cc or less. Claim 4 In claim 1 or 2, the copolymer has a result of [(vinyl / 1000C)*(Mn)] of 5 x 10 3 A polymer composition further comprising (g / mol) or more. Claim 5 A polymer composition according to claim 1 or 2, further comprising a copolymer having a ratio of [(vinyl / 1000C) / (vinylidene / 1000C)] of 2.0 or higher. Claim 6 An article comprising at least one component formed from the composition of claim 1 or 2. Claim 7 delete Claim 8 delete Claim 9 delete Claim 10 delete Claim 11 delete Claim 12 delete Claim 13 delete Claim 14 delete Claim 15 delete

Citation Information

Patent Citations

  • Encapsulating material for solar cell and solar cell module

    EP2993704A1

  • Production process of olefin polymerization catalyst and olefin polymer

    US20120264889A1

  • Catalyst system for multi-block copolymer formation

    WO2018170208A1

  • Ethylene / alpha-olefin copolymer and method for preparing same

    WO2019212307A1

  • Bis-biphenylphenoxy catalysts for the polymerization of low molecular weight ethylene-based polymers

    JP2017522425A