Pellicle frame and pellicle
A lightweight pellicle frame with specific material properties and design features addresses the issues of wrinkle prevention and weight in EUV lithography, enhancing processability and yield.
Patent Information
- Application Number
- KR1020240182725
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-10-10
- Filing Date
- 2024-12-10
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2038-06-28
AI Technical Summary
Conventional pellicles used in EUV lithography fail to prevent wrinkles, peeling, or cracking during the formation of fine patterns of 10 nm or less, and are not lightweight enough for high-throughput EUV exposure technology.
A pellicle frame made of a metal or alloy with a linear expansion coefficient of 10 × 10⁻⁶ (1/K) or less and a density of 4.6 g/cm³ or less, featuring a thickness of less than 2.5 mm and side holes for ventilation, is used to minimize frame expansion and weight.
The solution effectively prevents pellicle film damage and ensures high processability, allowing for larger ventilation areas and reduced weight, suitable for EUV exposure technology.
Smart Images

Figure 112024136875000-PAT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a lithography pellicle used as a dust film when manufacturing semiconductor devices such as LSIs and ultra-LSIs, printed circuit boards, liquid crystal displays, etc. Background Technology
[0002] When manufacturing semiconductor devices such as LSIs and ultra-LSIs, or liquid crystal displays, light is irradiated onto a semiconductor wafer or a liquid crystal substrate to create a pattern. However, if dust is attached to the photomask or reticle used at this time (hereinafter referred to simply as "photomask"), there was a problem in that the dimensions, quality, and appearance of the resulting product were compromised, such as the edges of the pattern becoming rough and the substrate becoming black and contaminated.
[0003] For this reason, pattern fabrication is typically carried out in a cleanroom, but it is still difficult to keep the photomask clean. Therefore, exposure is performed after attaching a pellicle as a dust barrier to the surface of the photomask. In this case, since foreign substances do not adhere directly to the surface of the photomask but adhere to the pellicle film, if the focus is set on the pattern of the photomask during lithography, the foreign substances on the pellicle film are irrelevant to the transfer.
[0004] Generally, a transparent pellicle film made of nitrocellulose, cellulose acetate, fluoropolymer, etc., which transmits light well, is bonded by applying a solvent of the pellicle film to the upper surface of a pellicle frame made of aluminum, stainless steel, polyethylene, etc., and then air-drying it (see Patent Document 1), or by bonding it with an adhesive such as acrylic resin or epoxy resin (see Patent Documents 2 and 3). In addition, on the lower surface of the pellicle frame, an adhesive layer made of polybutene resin, polyvinyl acetate resin, acrylic resin, silicone resin, etc., for attachment to a photomask, and a release layer (separator) for protecting the adhesive layer are formed.
[0005] In addition, when such a pellicle is mounted on the surface of a photomask and a photoresist film formed on a semiconductor wafer or a liquid crystal substrate is exposed through the photomask, foreign substances such as dust adhere to the surface of the pellicle and do not adhere directly to the surface of the photomask. Therefore, if light for exposure is irradiated so that the focus is positioned on the pattern formed on the photomask, it is possible to avoid the influence of foreign substances such as dust.
[0006] However, recently, semiconductor devices and liquid crystal displays have been becoming increasingly highly integrated and miniaturized. Currently, technology for forming fine patterns of about 32 nm on photoresist films is also being commercialized. Patterns of about 32 nm can be achieved using improved technologies using conventional excimer lasers, such as immersion exposure technology, in which a liquid such as ultrapure water is filled between a semiconductor wafer or liquid crystal substrate and a projection lens, and an argon fluoride (ArF) excimer laser is used to expose the photoresist film, or double exposure.
[0007] However, next-generation semiconductor devices and liquid crystal displays require the formation of even finer patterns of 10 nm or less, and it is already impossible to meet this requirement by improving conventional exposure technology using excimer lasers.
[0008] Therefore, as a method for forming patterns of 10 nm or less, EUV lithography technology using EUV (Extreme Ultra Violet) light with a wavelength of 13.5 nm is considered a promising option. When forming fine patterns of 10 nm or less on a photoresist film using this EUV lithography technology, it is necessary to solve technical challenges such as which light source to use, which photoresist to use, and which pellicle to use. Among these technical challenges, development is underway regarding new light sources and new photoresist materials, and various proposals are being made.
[0009] Regarding pellicles that determine the yield of semiconductor devices or liquid crystal displays, for example, Patent Document 3 describes a silicon film with a thickness of 0.1 to 2.0 μm that is transparent and does not cause optical deformation as a pellicle film used in EUV lithography, but there are still unresolved problems in its actual application, which is a major obstacle to the commercialization of EUV exposure technology.
[0010] Conventionally, regarding the material of the pellicle frame constituting the pellicle, in the case of exposure using i-ray (wavelength 365 nm), krypton fluoride (KrF) excimer laser light (wavelength 248 nm), and argon fluoride (ArF) excimer laser light (wavelength 193 nm), it is selected considering only its rigidity and processability, and typically aluminum, stainless steel, polyethylene, etc. are used.
[0011] Meanwhile, regarding the material of the photomask, quartz glass is commonly used, and for the pellicle film, a transparent film according to the light source is used, such as nitrocellulose, cellulose acetate, or fluoropolymer for i-line, KrF, or ArF, and silicon for EUV.
[0012] However, when using EUV lithography technology to form fine patterns of 10 nm or less on a photoresist film, if a conventional pellicle is used, wrinkles may form in the pellicle film, or the pellicle film may peel off from the pellicle frame, tear, or crack.
[0013] In Patent Document 4, it was found that the occurrence of film wrinkling or breakage of the pellicle film is caused by the expansion and deformation of the pellicle frame that may occur due to the temperature rise caused by light energy during exposure, and the linear expansion coefficient 10 × 10 -6 It has been proposed to use a material with a kJ or less (1 / K) for the frame.
[0014] However, materials such as Si, SiO2, SiC, and SiN, which have low coefficients of thermal expansion, are soft and difficult to process. In particular, EUV pellicles need to have a height of 2.5 mm or less because the pellicle placement space within the EUV exposure device is small.
[0015] In addition, typically, the side of the pellicle frame of a pellicle is formed with a jig hole used for handling or peeling the pellicle from a photomask, or a vent to alleviate the pressure difference between the inside and outside of the pellicle. Furthermore, since the inside of the exposure apparatus is under vacuum in EUV lithography, EUV pellicles must withstand pressure changes from atmospheric pressure to vacuum, and thus the vents of the EUV pellicle are required to be large in area.
[0016] For example, when the thickness of the pellicle frame of an EUV pellicle is reduced to less than 2.5 mm, but a hole with a diameter of 1 mm is to be formed on the side of the pellicle frame made of materials such as Si, SiO2, SiC, and SiN, the thickness of the pellicle frame near the hole may decrease, and there is a high possibility that the pellicle frame will be damaged during the processing of the hole or the peeling of the pellicle. If a large area of the vent is required, the possibility of damage increases even further.
[0017] Therefore, it is also worth considering using metals such as Invar as materials with a low coefficient of thermal expansion. Metals and alloys are easy to process and do not break even if holes are formed in the sides of the pellicle frame.
[0018] However, it is desirable for the width of the pellicle frame to be as small as possible to take a wide exposure area, and conventionally, it was about 2 mm. However, in the case of EUV pellicles, it was found that the width of the pellicle frame is limited by the pellicle film, so it is necessary to make it large, about 3 to 4 mm.
[0019] In addition, recently, in order to improve the throughput of EUV manufacturing, faster movement of the mask stage is required, and the total weight of the pellicle is required to be 15 g or less.
[0020] However, when the width is increased from 2 mm to 4 mm, the volume of the pellicle frame increases by about 2 times, and even at 3 mm, it increases by about 1.5 times. It was found that this makes the pellicle frame made of Invar excessively heavy. Prior art literature
[0021] Japanese Patent Publication No. Sho 58-219023, Specification of U.S. Patent No. 4861402, Japanese Patent Publication No. Sho 63-27707, Japanese Patent Publication No. 2016-200616 The problem to be solved
[0022] The present invention is made in consideration of the above circumstances and aims to provide a pellicle frame that is lightweight and has a low risk of breakage, and a pellicle using the same, which can effectively prevent wrinkles from forming on the pellicle film, peeling off from the pellicle frame, tearing, or cracking when a fine pattern of 10 nm or less is formed on a photoresist film using EUV exposure technology. means of solving the problem
[0023] The inventors provide a pellicle frame on a frame having an upper surface forming a pellicle film and a lower surface facing a photomask, wherein the coefficient of linear expansion is 10 × 10 -6 By using a metal or alloy with a density of 4.6 g / cm³ or less and a density of 1 / K or less, it was discovered that it is optimal for the latest EUV lithography technology because it does not cause wrinkles or damage to the pellicle film and is also lightweight, thereby achieving the present invention.
[0024] Accordingly, the present invention provides the following pellicle frame and pellicle.
[0025] 1. The coefficient of linear expansion is 10 × 10 -6 A pellicle frame characterized by being made of a metal or alloy having a density of (1 / K) or less and a density of 4.6 g / cm³ or less.
[0026] 2. A pellicle frame described in 1, wherein the metal or alloy is titanium or a titanium alloy.
[0027] 3. A pellicle frame as described in 1 or 2 with a thickness of less than 2.5 mm.
[0028] 4. A pellicle frame described in any one of 1 to 3, having one or more holes formed on the side.
[0029] 5. A pellicle characterized by including a pellicle frame described in any one of 1 to 4 as a component. Effects of the invention
[0030] According to the pellicle frame and pellicle of the present invention, even if the temperature of the pellicle frame rises due to light energy from exposure, the expansion and deformation of the pellicle frame can be suppressed to a small extent, thereby preventing wrinkles or damage to the pellicle film. Furthermore, since the pellicle frame and pellicle of the present invention have excellent processability, an improvement in yield can be expected, and the area of the ventilation portion can be made large. Moreover, because there is a low risk of damage during pellicle peeling and the pellicle is lightweight, it can be applied to the latest EUV exposure technology. Brief explanation of the drawing
[0031] FIG. 1 is a schematic diagram (example) showing one embodiment of the pellicle frame of the present invention, (A) is a view from the bottom side, (B) is a view from the outer side of the long side, and (C) is a view from the outer side of the short side. FIG. 2 is a schematic diagram showing another embodiment of the pellicle frame of the present invention, (A) is a view from the bottom side, (B) is a view from the outer side of the long side, and (C) is a view from the outer side of the short side. Specific details for implementing the invention
[0032] The pellicle frame of the present invention typically has an upper surface forming a pellicle film and a lower surface facing a photomask. In addition, its shape is a frame shape corresponding to the shape of the photomask on which the pellicle is mounted. Generally, it is a rectangular (rectangular or square) frame shape.
[0033] The pellicle frame has an upper surface for forming a pellicle film and a lower surface facing the photomask when mounting the photomask; typically, a pellicle film is formed on the upper surface by interposing an adhesive or the like, and an adhesive or the like is formed on the lower surface for mounting the pellicle to the photomask, but is not limited thereto.
[0034] The dimensions of the pellicle frame are not specifically limited, but since the height of the EUV pellicle is limited to 2.5 mm or less, the thickness of the EUV pellicle frame is smaller than that and less than 2.5 mm. In practice, considering the thickness of the pellicle film or mask adhesive, it is preferable that it be 2.0 mm or less, and more preferable that it be 1.6 mm or less.
[0035] In addition, in order to fully perform its function as a pellicle, a height of at least 1.5 mm is required. Then, considering the thickness of the pellicle frame for EUV, it is desirable that the thickness be at least 1.0 mm, taking into account the thickness of the pellicle film or mask adhesive.
[0036] In addition, typically, a jig hole used for handling or peeling the pellicle from the photomask, or a vent to alleviate the pressure difference inside and outside the pellicle, is formed on the side of the pellicle frame. Furthermore, since the inside of the exposure apparatus is under vacuum in EUV lithography, the EUV pellicle must withstand pressure changes from atmospheric pressure to vacuum, and it is desirable for the vent of the EUV pellicle to be as large an area as possible.
[0037] Accordingly, it is desirable to form holes on the sides of the pellicle frame, and the size of the jig holes or ventilation holes is such that the length in the thickness direction of the frame (diameter in the case of a circular shape) is 0.5 to 1.0 mm. There are no restrictions on the shape of the holes, and they may be circular or square. Also, typically, the jig holes are holes that do not penetrate from the outer surface to the inner surface, and the ventilation holes are holes that penetrate from the outer surface to the inner surface.
[0038] When forming a hole on the side of a pellicle frame, a margin of at least 0.2 mm is required around the machined hole to maintain processing constraints or the strength of the frame. If a jig hole or a ventilation hole is to be formed with a size of 1.0 mm or more in the length of the frame thickness direction, it is preferable that the frame thickness be 1.4 mm or more.
[0039] Typically, the dimensions of the EUV pellicle frame are such that the length of the long side is 145 to 152 mm, the length of the short side is 113 to 120 mm, the thickness is 1.0 to 2.0 mm, and the width is 3.0 to 4.0 mm. In addition, the volume of the pellicle frame is preferably 3.2 cm³ or less, and more preferably 2.6 cm³ or less.
[0040] In the present invention, the material of the pellicle frame has a linear expansion coefficient of 10 × 10 -6 (1 / K) or less, and also use a metal or alloy with a density of 5 g / cm³ or less.
[0041] In the present invention, by using a metal or alloy as the material for the pellicle frame, a hole can be formed on the side with a margin of 0.2 mm. For example, a hole with a diameter of 1.0 mm is formed on the side of a pellicle frame with a thickness of 1.5 mm. At this time, the upper and lower margins of the hole are 0.25 mm.
[0042] Furthermore, when forming holes in a pellicle frame made of a brittle material such as a silicon single crystal, a margin of at least 0.5 mm around the hole is required. Consequently, only holes up to a diameter of 0.5 mm can be formed on the side of a pellicle frame with a thickness of 1.5 mm. Under these conditions, in addition to the risk of the ventilation area of the EUV pellicle becoming insufficient, it is necessary to increase the number of holes to ensure secure retention or peeling from a 0.5 mm diameter jig hole, which also leads to a decrease in yield. Moreover, even with a margin of 0.5 mm, there is a high probability of breakage when large forces are applied, such as during peeling.
[0043] In the present invention, the linear expansion coefficient of the material of the pellicle frame is 10 × 10 -6(1 / K) or less, and if within this range, the expansion and deformation of the pellicle frame that may occur due to the temperature rise caused by light energy during exposure can be sufficiently suppressed to a small extent, thereby resolving the issue without causing wrinkles or damage to the pellicle film.
[0044] In addition, in the present invention, the density of the metal or alloy that is the pellicle frame material is 4.6 g / cm³ or less. Within this density range, it becomes possible to make the weight 15 g or less for a pellicle frame with a volume of 3.2 cm³ or less. However, if the volume of the pellicle frame exceeds 2.6 cm³, it is necessary to make the weight of the pellicle film or mask adhesive other than the pellicle frame 3 g or less. Accordingly, it is preferable that the volume of the pellicle frame be 2.6 cm³ or less, and the density is more preferably 4.5 g / cm³ or less.
[0045] Examples of such metals or alloys include titanium and titanium alloys such as Ti-V-Al alloys and Ti-V-Cr-Sn-Al alloys, and it is desirable to use these.
[0046] In the pellicle of the present invention, a pellicle film is formed on the upper surface of the pellicle frame by interposing an adhesive or a pressure-sensitive adhesive. There are no restrictions on the material of the pressure-sensitive adhesive or adhesive, and known materials may be used. For example, the pellicle film may be bonded by applying a solvent and then air-drying, or adhesives or pressure-sensitive adhesives such as acrylic resin, silicone resin, or epoxy resin may be used.
[0047] In addition, there are no restrictions on the material of the pellicle film, but it is desirable that it has high transmittance and high light resistance at the wavelength of the exposure light source. For example, for excimer lasers, amorphous fluoropolymers can be used. Examples of amorphous fluoropolymers include Cytop [manufactured by Asahi Glass Co., Ltd.: trade name], Teflon (registered trademark) AF [manufactured by DuPont Corporation: trade name], etc.
[0048] In addition, for EUV lithography, ultra-thin silicon films or carbon films composed of single-crystal silicon, polycrystalline silicon, or amorphous silicon are used. The pellicle film may be provided with a protective film such as SiC, SiO2, Si3N4, SiON, Y2O3, YN, Mo, Ru, and Rh.
[0049] Additionally, an adhesive for mounting to a photomask is formed on the bottom surface of the pellicle frame. As for the mask adhesive, known materials may be used, and adhesives composed of polybutene resin, polyvinyl acetate resin, SEBS (poly(styrene-ethylene-butadiene-styrene)) resin, acrylic resin, silicone resin, etc. may be used. In particular, adhesives composed of acrylic resin and silicone resin are preferred.
[0050] The application of the pellicle film adhesive and mask adhesive can be carried out, for example, by dip, spray, brush application, or by a dispensing device, but application using a dispensing device is preferable in terms of stability, workability, yield, etc.
[0051] In addition, the adhesive or bonding agent is generally formed along the entire circumference of the cross-section of the pellicle frame in the perimeter direction, with a width equal to or less than the width of the pellicle frame.
[0052] In addition, if the viscosity of the pellicle film adhesive and the mask adhesive is high and it is difficult to apply them using an application device, aromatic solvents such as toluene and xylene, aliphatic solvents such as hexane, octane, isooctane, and isoparaffin, ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone, ester solvents such as ethyl acetate and butyl acetate, ether solvents such as diisopropyl ether and 1,4-dioxane, or a mixture of these solvents may be added as needed.
[0053] A release layer (separator) to protect the adhesive may be attached to the bottom surface of the mask adhesive. The material of the release layer is not particularly limited, but, for example, polyethylene terephthalate (PET), polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), polyethylene (PE), polycarbonate (PC), polyvinyl chloride (PVC), polypropylene (PP), etc. may be used. In addition, if necessary, a release agent such as a silicone-based release agent or a fluorine-based release agent may be applied to the surface of the release layer.
[0054] If a hole is formed penetrating from the outer surface to the inner surface of the pellicle frame, a dust removal filter may be formed for the purpose of removing particles. The filter may be installed inside the hole, or it may be installed on the side to cover the opening of the hole.
[0055] In addition, in the pellicle frame for EUV, it is preferable that the total area of the openings of the ventilation holes be 5 mm² or more, and more preferable that it be 10 mm² or more. The ventilation holes may, for example, be made to penetrate from the outer surface toward the inner surface so that a concave portion is formed on the bottom surface.
[0056] Here, FIGS. 1 and 2 illustrate an example of a pellicle (1) comprising a pellicle frame (2) of the present invention as a component. A pellicle film (3) is attached and installed on the upper surface of the pellicle frame (2) by an adhesive (5). Additionally, an adhesive (4) for mounting to a photomask (not specifically shown) is formed on the lower surface of the pellicle frame (2). Also, in the drawings, reference numeral 6 is a ventilation hole, and unlike FIG. 1, the pellicle frame of FIG. 2 is formed such that a ventilation hole forms a concave portion (6) on the lower surface. Additionally, reference numeral 7 indicates a jig hole formed to peel the pellicle from the photomask using a jig.
[0057] Examples
[0058] The present invention will be specifically described below by presenting examples and comparative examples, but the present invention is not limited to the following examples.
[0059] [Example 1]
[0060] Titanium (Coefficient of linear expansion: 8.4 × 10⁻⁶ -6 A pellicle frame (outer dimensions 150 mm × 118 mm × 1.5 mm, frame width 3.0 mm) was manufactured using (1 / K), density: 4.5 g / cm³).
[0061] On the outer side of the long side of the pellicle frame, a jig hole with a diameter of 1 mm × a depth of 1.2 mm was formed at 2 points located 52 mm away from the center of the side in the corner direction. Additionally, through holes were formed at 6 points located 10 mm, 30 mm, and 65 mm away from the center of the long side in the corner direction, and at 4 points located 10 mm and 30 mm away from the center of the short side in the corner direction.
[0062] After cleaning and drying the pellicle frame with a neutral detergent and pure water, a silicone adhesive (X-40-3264 manufactured by Shin-Etsu Chemical Co., Ltd.) was applied to the top and bottom surfaces of the frame over the entire perimeter.
[0063] After that, the pellicle frame was heated at 90°C for 12 hours to cure the adhesive on the upper and lower cross-sections. Subsequently, an ultra-thin silicone film was pressed onto the adhesive formed on the upper surface of the frame as a pellicle film to complete the pellicle.
[0064] Here, the volume of the pellicle frame is about 2.4 cm³, and the total weight of the pellicle film and the adhesive is about 3.1 g.
[0065] [Example 2]
[0066] As a material for the pellicle frame, Ti-Al6-V4 titanium alloy, an alloy of titanium, aluminum, and vanadium (coefficient of linear expansion: 8.8 × 10⁻⁶ -6(1 / K), density: 4.4 g / cm³) was used. Except for that, the pellicle was prepared in the same way as in Example 1.
[0067] [Comparative Example 1]
[0068] As the material for the pellicle frame, quartz glass (SiO2) (coefficient of linear expansion: 0.5 × 10⁻⁶ -6 (1 / K), density: 2.2 g / cm³) was used. Except for that, the pellicle was prepared in the same way as in Example 1.
[0069] Here, when forming jig holes or through holes in the pellicle frame, 7 out of 10 were damaged. Also, after the heat cycle test described later, when attempting to peel the pellicle from the quartz substrate using a peeling jig, the jig holes were damaged.
[0070] [Comparative Example 2]
[0071] As a material for the pellicle frame, silicon nitride (Si3N4) (coefficient of linear expansion: 2.8 × 10⁻⁶ -6 (1 / K), density: 3.2 g / cm³) was used. Except for that, the pellicle was prepared in the same way as in Example 1.
[0072] Here, when forming jig holes or through holes in the pellicle frame, 9 out of 10 were damaged. Also, after the heat cycle test described later, when attempting to peel the pellicle from the quartz substrate using a peeling jig, the jig holes were damaged.
[0073] [Comparative Example 3]
[0074] As a material for the pellicle frame, Invar (Fe-Ni36) (coefficient of linear expansion: 1.5 × 10⁻⁶ -6 (1 / K), density: 8.1 g / cm³) was used. Except for that, the pellicle was prepared in the same way as in Example 1.
[0075] [Comparative Example 4]
[0076] As the material for the pellicle frame, aluminum (Al) (coefficient of linear expansion: 23 × 10⁻⁶ -6 (1 / K), density: 2.7 g / cm³) was used. Except for that, the pellicle was prepared in the same way as in Example 1.
[0077] Heat cycle tests as described below were performed on the pellicles prepared in Examples 1 and 2 and Comparative Examples 1 to 4. Table 1 shows the processability of each material as a pellicle frame, the heat cycle test results, the weight of the pellicle, and the overall evaluation results of each pellicle.
[0078] [Heat Cycle Test]
[0079] The pellicle attached to the quartz substrate was heated in an oven at 200°C and left to stand for 24 hours, and then left to stand at room temperature for an additional 24 hours. This cycle was repeated 5 times. Afterward, the condition of the pellicle was visually inspected.
[0080]
[0081] According to the results of Table 1, the pellicles of Examples 1 and 2 showed good processability in the heat cycle test results, and the pellicle weight could be kept below 15 g.
[0082] Meanwhile, the pellicles of Comparative Examples 1 and 2 had problems with processability and it was difficult to form holes in the side portions.
[0083] The pellicle of Comparative Example 3 showed good processability as a result of the heat cycle test, but it cannot be applied to EUV lithography because the weight of the pellicle exceeds 15 g.
[0084] The pellicle frame of Comparative Example 4 showed large expansion of the pellicle frame due to the heat cycle test, and cracks occurred in the pellicle film. Explanation of the symbols
[0085] 1 : Pellicle 2 : Pellicle Frame 3 : Pellicle 4 : Photomask adhesive 5: Pellicle film adhesive 6 : Ventilation holes 7 : Jig ball
Claims
Claim 1 As a pellicle frame, the coefficient of linear expansion is 10 × 10 -6 A pellicle frame characterized by being made of a metal or alloy having a density of 4.6 g / cm³ or less and having one or more holes formed on the side, and having a margin of the diameter of the holes relative to the thickness of the pellicle frame of 0.2 to 0.25 mm. Claim 2 A pellicle frame characterized by using titanium or a titanium alloy as a material, having one or more holes formed on the side, and having a margin of the diameter of the holes relative to the thickness of the pellicle frame of 0.2 to 0.25 mm. Claim 3 In claim 2, the coefficient of linear expansion is 10 × 10 -6 A pellicle frame made of titanium or a titanium alloy having a density of (1 / K) or less and a density of 4.6 g / cm³ or less. Claim 4 A pellicle frame according to claim 2 or 3, wherein the titanium alloy is a Ti-V-Al alloy or a Ti-V-Cr-Sn-Al alloy. Claim 5 A pellicle frame having a thickness of less than 2.5 mm, according to claim 1 or 2. Claim 6 delete Claim 7 A pellicle frame having a width of 3 to 4 mm in claim 1 or 2. Claim 8 A pellicle frame having a volume of 3.2 cm³ or less, according to claim 1 or 2. Claim 9 A pellicle frame according to claim 1 or 2, having ventilation holes and a total opening area of 5 mm² or more. Claim 10 A pellicle frame for EUV exposure according to claim 1 or 2. Claim 11 A pellicle characterized by including a pellicle frame and a pellicle membrane as components as described in claim 1 or 2. Claim 12 In claim 11, a pellicle having a height of 2.5 mm or less. Claim 13 In claim 11, a pellicle for EUV lithography. Claim 14 A photomask with a pellicle attached thereto, wherein the pellicle described in claim 11 is formed on the photomask. Claim 15 In claim 14, a photomask with a pellicle attached for EUV exposure. Claim 16 An exposure method characterized by using a photomask attached with a pellicle as described in claim 14. Claim 17 In claim 16, the exposure method wherein the exposure is EUV exposure. Claim 18 A method for manufacturing a semiconductor device characterized by exposing using a photomask attached to a pellicle as described in claim 14. Claim 19 In claim 18, a method for manufacturing a semiconductor device in which the exposure is EUV exposure. Claim 20 A method for manufacturing a liquid crystal display characterized by exposing using a photomask attached to a pellicle as described in claim 14. Claim 21 A method for manufacturing a liquid crystal display in which the exposure is EUV exposure, in claim 20.
Citation Information
Patent Citations
An EUV pellicle frame and an EUV pellicle using it
KR1020160120225A
Pellicle for EUV
KR1020170045714A
Pellicle frame
JP2009025559A
Pellicle
JP2016191902A
Pellicle film, pellicle frame, and pellicle and method for producing same
KR1020170070146A