Polyurethane, abrasive layer, abrasive pad, and abrasive method

A polyurethane layer with carboxyl groups in the molecular structure addresses clogging issues in polishing pads by repelling abrasive particles, ensuring stable and extended polishing performance.

KR103045255B1Active Publication Date: 2026-11-06KURARAY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020227019386
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-13
Filing Date
2020-12-10
Publication Date
2026-11-06
Estimated Expiration
2040-12-10

AI Technical Summary

Technical Problem

Existing polishing pads for semiconductor wafers face issues with clogging due to abrasive particle accumulation, leading to reduced polishing speed, shortened lifespan, and increased likelihood of scratches, particularly in non-woven type pads with uneven structures.

Method used

Incorporating polyurethane with carboxyl groups in the molecular structure to create a polishing layer that generates a negative potential, repelling abrasive particles and preventing clogging, thus stabilizing the polishing process and extending the pad's lifespan.

Benefits of technology

The polyurethane layer with carboxyl groups ensures stable and long-lasting polishing by preventing abrasive particle clogging, reducing scratches, and maintaining polishing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022059947833-PCT00004_ABST
    Figure 112022059947833-PCT00004_ABST
Patent Text Reader

Abstract

The present invention provides a polyurethane capable of suppressing clogging and enabling stable, long-lasting polishing while suppressing the occurrence of scratches, a polishing layer using the same, a polishing pad, and a polishing method. A polyurethane having at least one structural unit derived from a compound having a carboxyl group. Also, a polishing layer, a polishing pad, and a polishing method using the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a novel polyurethane, a polishing layer using the same, a polishing pad, and a polishing method. Background Technology

[0002] Recently, as semiconductor wafers and devices require high integration and multilayer wiring, there is a growing demand for improvements in the basic quality of their materials, such as surface flatness.

[0003] Chemical Mechanical Polishing (CMP) is a polishing method for planarizing the surface of a semiconductor wafer. CMP is a method of polishing a workpiece with high precision using a polishing pad while supplying a slurry containing abrasive particles and a reaction solution to the surface of the workpiece. As for the material constituting the polishing layer of the polishing pad used in this method, for example, polyurethane having a closed-cell structure can be used. Polyurethane having a closed-cell structure is generally manufactured by mold foaming and curing using a two-component curing type polyurethane (e.g., Patent Documents 1 to 4).

[0004] However, in this method, it is difficult to homogenize the reaction and foaming, and there is a limit to the high hardness of the resulting polyurethane, so polishing characteristics such as the flatness of the polished surface and the flattening efficiency are prone to variation. In addition, since the foaming structure consists of independent pores, polishing slurry or polishing debris used in the polishing process tends to enter the pores and clog, causing problems such as reduced polishing speed and shortened pad life.

[0005] Meanwhile, as a polyurethane constituting the polishing layer, a polyurethane resin impregnated and solidified into a nonwoven fabric can be cited (e.g., Patent Documents 5 to 7). Such nonwoven fabric type polishing pads have an uneven structure, pores, and a connecting hole structure derived from the structure of the nonwoven fabric, so the liquid retention of the slurry during polishing is good, making it easy to improve the polishing rate, and also have the characteristic of having good contact with the wafer due to high flexibility. Prior art literature

[0006] Japanese Published Patent Application No. 2000-178374 Japanese Published Patent Application No. 2000-248034 Japanese Published Patent Application No. 2001-89548 Japanese Published Patent Application No. Hei 11-322878 Japanese Published Patent Application No. Hei 11-99479 Japanese Published Patent Application No. 2005-212055 Japanese Published Patent Application No. Hei 3-234475 The problem to be solved

[0007] However, non-woven type polishing pads had a problem in that, while the liquid retention of the slurry was good due to the uneven structure of the non-woven fabric, the hardness and elastic modulus of the polyurethane changed as abrasive particles clogged due to the unevenness, and as a result, scratches on the wafer became more likely to occur. In addition, there was a problem in that the stability of polishing was reduced due to changes in hardness, etc. caused by clogging, and the lifespan of the polishing pad was shortened.

[0008] The present invention is made in consideration of the above-mentioned conventional problems and aims to provide a polyurethane that forms a polishing layer capable of polishing stably for a long life while suppressing the occurrence of scratches by suppressing clogging of the polishing layer, a polishing layer using the same, a polishing pad, and a polishing method. means of solving the problem

[0009] As a result of repeated investigations to solve the above problem, the inventors found that by using a polyurethane having carboxyl groups in its molecular structure in the polishing layer, the carboxyl groups dissociate during polishing, causing the entire polishing layer to change to a negative potential. Consequently, it was discovered that the clogging of abrasive particles can be prevented by the repulsive force between the polishing layer with a negative potential and the abrasive particles with a negative potential, thereby enabling stable polishing with a long lifespan while suppressing the occurrence of scratches, and thus the present invention was completed.

[0010] The present invention is characterized by the following [1] to

[10] .

[0011] [1] Polyurethane having at least one structural unit derived from a compound having a carboxyl group.

[0012] [2] The polyurethane described in [1] comprises at least a structural unit derived from a compound having the above carboxyl group, a structural unit derived from a chain extender, a structural unit derived from a polymeric diol, and a structural unit derived from an organic diisocyanate.

[0013] [3] Polyurethane described in [1] or [2], wherein the amount of structural units derived from the compound having the carboxyl group among the total structural units constituting the polyurethane is 3 to 30 mol%.

[0014] [4] A polishing layer using polyurethane as described in any one of [1] to [3] above.

[0015] [5] The abrasive layer described in [4] is a nonwoven fabric impregnated with the polyurethane and further solidified.

[0016] [6] The abrasive layer described in [4] or [5], wherein the zeta potential of the polyurethane constituting the abrasive layer at pH 7.0 is -10.0 mV or less.

[0017] [7] A polishing layer described in any one of [4] to [6], wherein the above polyurethane is non-foamed.

[0018] [8] A polishing layer described in any one of [4] to [7], wherein the above polyurethane is saturated with water at 50°C and then swells, and the storage modulus measured at 50°C is 50 to 1,200 MPa, and the contact angle with water is 80 degrees or less.

[0019] [9] A polishing pad using the polishing layer described in any one of [4] to [8] above.

[0020]

[10] A polishing method using a polishing layer described in any one of [4] to [8] above,

[0021] A process of fixing a polishing pad having the above-mentioned polishing layer onto a surface plate of a polishing device, and

[0022] A process of holding the workpiece to be polished in the holder of the polishing device so as to face the polishing surface of the polishing layer, and

[0023] A polishing method having a process of polishing a workpiece by supplying a neutral or alkaline polishing slurry between the polishing surface and the workpiece, and sliding the polishing pad and the workpiece relatively. Effects of the invention

[0024] According to the present invention, a polyurethane that forms a polishing layer capable of polishing stably for a long life while suppressing the occurrence of scratches by suppressing clogging of the polishing layer, a polishing layer using the same, a polishing pad, and a polishing method can be provided. Brief explanation of the drawing

[0025] FIG. 1 is a schematic diagram illustrating the carboxyl groups present in the molecular structure of the polyurethane of the present invention having structural units derived from dimethylolpropionic acid. Figure 2 is a schematic diagram illustrating the dissociated state of the carboxyl group in Figure 1. FIG. 3 is a schematic diagram illustrating the polishing method of the present invention. Figure 4 is a photograph showing the types of scratches (evaluation criteria) on the workpiece in the examples and comparative examples. Specific details for implementing the invention

[0026] [Polyurethane]

[0027] The polyurethane of the present invention has at least one structural unit derived from a compound having a carboxyl group.

[0028] According to the present invention, since it has at least one structural unit derived from a compound having a carboxyl group, a carboxyl group is present within the molecular structure of the polyurethane. When this is used as a material for the polishing layer of a polishing pad, the negative potential generated by the dissociation of the carboxyl group and the repulsive force of the negative potential of the abrasive grains make it difficult for clogging of the abrasive grains to occur in the uneven parts of the polishing layer. Therefore, it is possible to suppress the occurrence of scratches caused by clogging and to polish stably for a long life.

[0029] In addition, in the present invention, by adjusting the amount of carboxyl groups present in the molecular structure of the polyurethane, it is possible to impart not only a negative potential to the surface of the polyurethane but also properties such as hydrophilicity.

[0030] The polyurethane of the present invention can be manufactured, for example, by using a compound having a carboxyl group in addition to the raw materials used in the manufacture of general polyurethanes. Specifically, the compound having a carboxyl group may be, for example, dimethylolpropionic acid, and by reacting this with a raw material such as a polymer diol or isocyanate, a polyurethane having a carboxyl group in its molecular structure, as shown in the schematic diagram of FIG. 1, can be obtained. As described above, this carboxyl group can improve the hydrophilicity of the surface of the polyurethane and improve the wettability on the surface of the polyurethane.

[0031] FIG. 2 is a diagram illustrating the dissociated state of the carboxyl groups of the polyurethane in FIG. 1. For the polyurethane of FIG. 1, by applying pH conditions where the carboxyl groups ionize, the carboxyl groups become -COO, as shown in FIG. 2. - and H + Because it dissociates, -COO on the surface of polyurethane - A negative potential originating from can be imparted. Therefore, when the polyurethane of the present invention is used as an abrasive layer, if an alkaline slurry is used, the carboxyl groups dissociate, and -COO - As a result, the zeta potential of the abrasive layer becomes negative. Consequently, the abrasive particles in the alkaline slurry and the polyurethane are repelled by repulsion, making it difficult for the abrasive particles to clog the uneven parts of the abrasive layer, and as a result, the abrasive efficiency is improved.

[0032] The polyurethane of the present invention is not particularly limited as long as it has at least one structural unit derived from a compound having a carboxyl group, and may be a thermoplastic polyurethane or a thermosetting polyurethane, but it is preferred to be a thermoplastic polyurethane in that it can be continuously produced by melt polymerization and can be easily processed into a sheet when used as a polishing layer of a polishing pad.

[0033] In addition, the polyurethane of the present invention can be preferably used not only as a polishing layer of a polishing pad, but also for applications requiring hydrophilicity on the polyurethane surface or modification of electrical properties.

[0034] Hereinafter, a thermoplastic polyurethane is described in detail as an example of the polyurethane of the present invention.

[0035] The thermoplastic polyurethane related to the present invention preferably comprises, for example, structural units derived from a compound having a carboxyl group, structural units derived from a chain extender, structural units derived from a polymeric diol, and structural units derived from an organic diisocyanate, for the sake of ease of manufacture.

[0036] [Compounds having a carboxyl group]

[0037] Specific examples of compounds having a carboxyl group include, for example, diols having a carboxyl group, diamines having a carboxyl group, polymeric diols having a carboxyl group, and derivatives thereof. Specifically, for example, compounds represented by the following general formulas (1) to (3) may be cited.

[0038] [Chemical Formula 1]

[0039]

[0040] (Among Equations (1) to (3), R 1 ~ R 6 Each represents a hydroxyl group or an amino group independently. Additionally, R represents a trivalent hydrocarbon group or an aromatic hydrocarbon group having 1 to 10 carbon atoms that may have substituents, and R' represents a divalent hydrocarbon group having 1 to 10 carbon atoms independently. l, m, and n represent integers from 1 to 10.

[0041] Compounds having such a carboxyl group include dimethylolpropionic acid, dimethylolbutanoic acid, tartaric acid, 2-hydroxypropionic acid, malic acid, 4-hydroxymethylbenzoic acid, etc., in terms of excellent reactivity and ease of availability. Among these, the compound represented by Formula (1) is preferred, and in the compound represented by Formula (1), a compound in which R is a trivalent hydrocarbon group having 1 to 6 carbon atoms is more preferred, and dimethylolpropionic acid and dimethylolbutanoic acid are even more preferred in terms of ensuring the rigidity of the polishing layer while exhibiting the characteristics of the zeta potential.

[0042] [Chain Extender]

[0043] Examples of chain extenders include compounds commonly used in the manufacture of polyurethane (except for compounds having the above-mentioned carboxyl group). Specifically, examples include low molecular weight compounds that do not contain dienophil or diene, which are compounds having a molecular weight of 300 or less and having two or more active hydrogen atoms in the molecule capable of reacting with isocyanate groups.

[0044] As chain extenders, for example, diols such as ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 2,2-diethyl-1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,4-bis(β-hydroxyethoxy)benzene, 1,4-cyclohexanediol, cyclohexanedimethanol (1,4-cyclohexanedimethanol, etc.), bis(β-hydroxyethyl)terephthalate, 1,9-nonanediol, m-xylylene glycol, p-xylylene glycol, diethylene glycol, triethylene glycol, etc.;Ethylenediamine, trimethylenediamine, tetramethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 3-methylpentamethylenediamine, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 1,2-diaminopropane, hydrazine, xylylenediamine, isophoronediamine, piperazine, o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, tolylenediamine, xylenediamine, adipic acid dihydrazide, isophthalic acid dihydrazide, 4,4'-Diaminodiphenylmethane, 4,4'-Diaminodiphenyl ether, 4,4'-Bis(4-aminophenoxy)biphenyl, 4,4'-Bis(3-aminophenoxy)biphenyl, 1,4-Bis(4-aminophenoxy)benzene, 1,3-Bis(4-aminophenoxy)benzene, 1,3-Bis(3-aminophenoxy)benzene, 3,4'-Diaminodiphenyl ether, 4,4'-Diaminodiphenylsulfone, 3,4-Diaminodiphenylsulfone, 3,3'-Diaminodiphenylsulfone, 4,4'-Methylene-Bis(2-chloroaniline), 3,3'-Dimethyl-4,4'-Diaminobiphenyl, 4,4'-Diaminodiphenylsulfide, 2,6-Diaminotoluene, 2,4-Diaminochlorobenzene, Examples include 1,2-diaminoanthraquinone, 1,4-diaminoanthraquinone, 3,3'-diaminobenzophenone, 3,4-diaminobenzophenone, 4,4'-diaminobenzophenone, 4,4'-diaminobibenzyl, 2,2'-diamino-1,1'-vinaphthalene, 1,3-bis(4-aminophenoxy)alkanes, 1,4-bis(4-aminophenoxy)alkanes, 1,5-bis(4-aminophenoxy)alkanes, 1,n-bis(4-aminophenoxy)alkanes (n is 3 to 10), 1,2-bis[2-(4-aminophenoxy)ethoxy]ethane, 9,9-bis(4-aminophenyl)fluorene, 4,4'-diaminobenzanilide, and other diamines. These may be used individually or in combination of two or more types.

[0045] Among these, diols such as 1,4-butanediol and 1,5-pentanediol, and diamines such as hydrazine are preferred in terms of improving the rigidity of the polishing layer.

[0046] When a chain extender is used, the ratio (mol%) of the compound having a carboxyl group to the total amount of the compound having a carboxyl group and the chain extender is appropriately selected according to the purpose, but for example, preferably 5 to 90 mol%, more preferably 10 to 70 mol%, and even more preferably 15 to 60 mol%. By keeping the content ratio of the compound having a carboxyl group within the above range, a negative potential that sufficiently repels the negative potential of the abrasive particles can be imparted to the polyurethane.

[0047] [Polymer Diol]

[0048] Specific examples of polymeric diols include, for instance, polyether diols, polyester diols, and polycarbonate diols. These may be used individually or in combination of two or more types. Among these, polyether diols and polycarbonate diols are preferred from the perspective of ease of availability and excellent reactivity, and polyether diols are more preferred.

[0049] The number average molecular weight of the polymeric diol is preferably 450 to 3,000, more preferably 500 to 2,700, and even more preferably 550 to 2,400. If the number average molecular weight of the polymeric diol is within the above range, it is easy to obtain a polishing layer that maintains required properties such as rigidity, hardness, and hydrophilicity. In addition, the number average molecular weight of the polymeric diol refers to the number average molecular weight calculated based on the hydroxyl value measured in accordance with JIS K 1557-1:2007.

[0050] (Polyetherdiol)

[0051] Specific examples of polyetherdiols include, for instance, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, poly(methyltetramethylene glycol), glycerin-based polyalkylene ether glycol, etc. These may be used individually or in combination of two or more types. Among these, polyethylene glycol and polytetramethylene glycol are preferred.

[0052] (Polyesterdiol)

[0053] In the present invention, a polyester diol may be used. The polyester diol is obtained, for example, by directly esterifying or transesterifying a low molecular weight diol with an ester-forming derivative such as a dicarboxylic acid or its ester or anhydride.

[0054] Specific examples of dicarboxylic acids, their esters, and their anhydrides for producing polyesterdiols include, for example, aliphatic dicarboxylic acids having 2 to 12 carbon atoms, such as oxalic acid, succinic acid, glutaric acid, adipic acid, pimelolic acid, souveric acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, 2-methylsuccinic acid, 2-methyladipoic acid, 3-methyladipoic acid, 3-methylpentanoic acid, 2-methyloctaenoic acid, 3,8-dimethyldecaneic acid, 3,7-dimethyldecaneic acid; aliphatic dicarboxylic acids having 14 to 48 carbon atoms, such as dimerized aliphatic dicarboxylic acids (dimer acids) obtained by dimerizing unsaturated fatty acids by fractional distillation of triglycerides, and their hydrogenated derivatives (hydrogenated dimer acids); Examples include alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and orthophthalic acid. In addition, specific examples of dimer acids and hydrogenated dimer acids include, for example, the trade names "Freepol 1004," "Freepol 1006," "Freepol 1009," and "Freepol 1013" manufactured by Unichema. These may be used individually or in combination of two or more types.

[0055] In addition, specific examples of low molecular weight diols for producing polyester diols include, for example, aliphatic diols such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 2-methyl-1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol; and alicyclic diols such as cyclohexanedimethanol and cyclohexanediol. These may be used individually or in combination of two or more types.

[0056] Among these, a diol having 6 to 12 carbon atoms is preferred, and a diol having 8 to 10 carbon atoms is more preferred.

[0057] (Polycarbonate diol)

[0058] Examples of polycarbonate diols include those obtained by the reaction of a low molecular weight diol with a carbonate compound such as a dialkyl carbonate, an alkylene carbonate, or a diaryl carbonate. Examples of low molecular weight diols for producing polycarbonate diols include the low molecular weight diols exemplified above. In addition, examples of dialkyl carbonates include dimethyl carbonate and diethyl carbonate. In addition, examples of alkylene carbonates include ethylene carbonate. Examples of diaryl carbonates include diphenyl carbonate.

[0059] [Organic Diisocyanate]

[0060] As for the organic diisocyanate, there are no particular restrictions as long as it is an organic diisocyanate commonly used in the manufacture of polyurethane. For example, ethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, dodecamethylene diisocyanate, isophorone diisocyanate, isopropylidene bis(4-cyclohexyl isocyanate), cyclohexylmethane diisocyanate, methylcyclohexane diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethylcaproate, bis(2-isocyanatoethyl)fumarate, bis(2-isocyanatoethyl)carbonate, Aliphatic or alicyclic diisocyanates such as 2-isocyanatoethyl-2,6-diisocyanatohexanoate, cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, bis(2-isocyanatoethyl)-4-cyclohexene; Examples of aromatic diisocyanates include 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, 1,5-naphthylene diisocyanate, 4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatodiphenylmethane, chlorophenylene-2,4-diisocyanate, and tetramethylxylylene diisocyanate. These may be used alone or in combination of two or more.Among these, alicyclic diisocyanates and aromatic diisocyanates are preferred in terms of improving the wear resistance of the obtained abrasive layer, 4,4'-dicyclohexylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, and 2,6-tolylene diisocyanate are more preferred, and 4,4'-diphenylmethane diisocyanate is even more preferred in terms of improving the rigidity of the abrasive layer.

[0061] [Additives]

[0062] The polyurethane of the present invention may, if necessary, contain additives such as crosslinking agents, fillers, crosslinking accelerators, crosslinking aids, softeners, tackifiers, anti-aging agents, foaming agents, processing aids, adhesion agents, inorganic fillers, organic fillers, crystallization nucleating agents, heat stabilizers, weather stabilizers, antistatic agents, colorants, lubricants, flame retardants, flame retardant aids (antimony oxide, etc.), anti-blooming agents, release agents, thickeners, antioxidants, and conductive agents.

[0063] The content ratio of additives in the polyurethane is not particularly limited, but is preferably 50 mass% or less, more preferably 20 mass% or less, and even more preferably 5 mass% or less.

[0064] [Mixing Ratio]

[0065] The mixing ratio of each component can be appropriately adjusted according to the desired characteristics. In the present invention, the amount of structural units derived from compounds having carboxyl groups among the total structural units constituting the polyurethane is preferably 3 to 30 mol%, more preferably 4 to 20 mol%, even more preferably 6 to 15 mol%, and even more preferably 6 to 12 mol%. If the amount of structural units of compounds having carboxyl groups is greater than or equal to the above lower limit, sufficient effects derived from carboxyl groups can be imparted to the polyurethane obtained. That is, since sufficient negative potential derived from carboxyl groups can be imparted to the polyurethane, by using this in a polishing layer, the clogging of the polishing layer can be suppressed by repelling the abrasive particles with negative potentials. Furthermore, if the amount of structural units derived from compounds having carboxyl groups is less than or equal to the above upper limit, it becomes easier to adjust physical properties such as the hardness of the polyurethane to the range described below.

[0066] The amount of isocyanate groups contained in the organic diisocyanate per 1 mole of active hydroxyl groups contained in the compound having a carboxyl group, the polymeric diol, and the chain extender is preferably 0.80 to 1.3 moles, and more preferably 0.90 to 1.2 moles.

[0067] If the ratio of isocyanate groups to 1 mole of active hydroxyl groups is greater than or equal to the lower limit above, the mechanical strength and wear resistance of the thermoplastic polyurethane are improved, and the lifespan of the polishing layer also tends to be longer. On the other hand, if the ratio of isocyanate groups to 1 mole of active hydrogen atoms is less than or equal to the upper limit above, the productivity and storage stability of the thermoplastic polyurethane are improved, and the polishing layer tends to be easier to manufacture.

[0068] <Method for Manufacturing Thermoplastic Polyurethane>

[0069] Thermoplastic polyurethane is obtained by polymerizing the aforementioned raw materials through a urethane reaction using a known prepolymer method or a one-shot method. More specifically, methods include manufacturing by melt polymerization while melt-mixing each of the components described above in a predetermined ratio using a single-screw or multi-screw extruder in the substantially absence of a solvent, or manufacturing by polymerization using a prepolymer method in the presence of a solvent. Furthermore, melt polymerization may be carried out continuously.

[0070] In the present invention, it is preferable to use solution polymerization from the perspective of stably carrying out the production of the polyurethane of the present invention. The concentration of the reaction solution is preferably 10 to 70 mass% from the perspective of reactivity and operability due to viscosity, more preferably 20 to 60 mass%, and even more preferably 20 to 50 mass%.

[0071] The obtained thermoplastic polyurethane is, for example, pelletized and then formed into a sheet-like molded body by various molding methods such as extrusion molding, injection molding, blow molding, and calendering. In particular, a sheet-like molded body of uniform thickness is obtained by extrusion molding using a T-die.

[0072] [Abrasive layer]

[0073] The polishing layer of the present invention utilizes the polyurethane of the present invention. As described above, the polyurethane of the present invention has carboxyl groups within its molecular structure. By using this in the polishing layer, clogging of abrasive particles becomes difficult to occur due to the repulsive force between the negative potential of the carboxyl groups and the negative potential of the abrasive particles; consequently, polishing can be performed stably for a long lifespan while suppressing the occurrence of scratches. More specifically, the slurry used in CMP is an alkaline slurry, and abrasive particles contained in the alkaline slurry typically have a negative zeta potential. In contrast, since the polishing layer of the present invention utilizes a polyurethane having carboxyl groups, when it comes into contact with an alkaline slurry, the carboxyl groups on the surface become -COO - As it dissociates, the zeta potential of the surface of the abrasive layer is lowered to, for example, -10 mV or less. In this case, the abrasive particles exhibiting a negative zeta potential in alkaline conditions and the abrasive layer exhibit electrostatic repulsion, and as a result, the adhesion of abrasive particles to the abrasive layer is prevented, and particularly in nonwoven abrasive layers, the suppression of clogging can be realized, and it is inferred that the occurrence of scratches or defects is reduced.

[0074] In addition, the polishing layer may be either a foamed polyurethane or a non-foamed polyurethane, but it is preferable that it be a non-foamed polyurethane. If the polishing layer is a non-foamed polyurethane, the polishing characteristics are less likely to fluctuate, so stable polishing can be achieved.

[0075] <Composition of the Abrasive Layer>

[0076] The polishing layer of the present invention may be formed by molding polyurethane into a sheet, or by impregnating a nonwoven fabric with the polyurethane of the present invention and further solidifying it. However, since using the polyurethane of the present invention makes it difficult for abrasive particles to enter the irregularities caused by the nonwoven fabric, thereby enabling stable polishing with a long lifespan, a polishing layer formed by impregnating a nonwoven fabric with the polyurethane of the present invention and further solidifying it is preferred.

[0077] In a method for impregnating a nonwoven fabric with polyurethane, first, an organic solution such as an N,N-dimethylformamide solution (DMF solution) is prepared, wherein the concentration of polyurethane is preferably 10 to 50 mass%, more preferably 20 to 40 mass%. Next, this is preferably heated to about 27 to 40°C, and the nonwoven fabric is preferably left standing on it for about 5 to 20 minutes to impregnate it with an organic solvent. Then, the nonwoven fabric is immersed in the organic solution of polyurethane, preferably for 2 to 15 minutes, and the excess organic solution attached to the nonwoven fabric is removed. After that, the polyurethane is solidified by immersing the nonwoven fabric in an aqueous solution having a concentration of organic solvent of 5 to 30 mass% and a temperature of about 27 to 40°C. Next, a nonwoven fabric impregnated with polyurethane can be obtained by washing the nonwoven fabric with an organic solvent, water, etc., as needed, and drying it.

[0078] In addition, the polyurethane solution impregnated into the nonwoven fabric in the present invention may include water-based polyurethane and solvent-based polyurethane. Here, water-based polyurethane refers to a polyurethane that can be dispersed in water or an aqueous solution, and solvent-based polyurethane refers to a polyurethane that can be dissolved in an organic solvent. Among these, solvent-based polyurethane is more preferred in that it improves the degree of freedom in selecting a chain elongator that contributes to the expression of zeta potential.

[0079] <Non-woven fabric>

[0080] There are no particular limitations on the nonwoven fabrics that can be used in the present invention, and examples include nonwoven fabrics made of fibers with polyester resins as the main component, such as nylon, polybutylene terephthalate (PBT), or polyethylene terephthalate (PET). Among these, in the case of polyester fibers, the storage modulus is difficult to fluctuate because it is difficult to absorb during polishing, so the polishing efficiency is stable. For example, in the case of highly absorbent fibers such as nylon fibers, the absorption rate increases during polishing, causing the storage modulus to fluctuate, making the polishing pad prone to deformation and the polishing efficiency prone to deterioration.

[0081] When using polyester fibers, the average staple fiber fineness is preferably 0.01 to 5.0 dtex, and more preferably 0.03 to 1.0 dtex. If the average staple fiber fineness is greater than or equal to the lower limit value, the fibers are less likely to break during dressing, thus preventing scratches caused by detachment. On the other hand, if the average staple fiber fineness is less than or equal to the upper limit value, the load on the object to be polished does not become excessively large, thus preventing scratches.

[0082] <Zeta Potential>

[0083] In terms of effectively suppressing scratches by suppressing clogging of the polishing layer, the zeta potential of the polyurethane constituting the polishing layer at pH 7.0 is preferably -10.0 mV or less, more preferably -50.0 to -12.0 mV, even more preferably -40.0 to -15.0 mV, even more preferably -30.0 to -17.0 mV, and even more preferably -27.0 to -20.0 mV. Since the zeta potential of the polyurethane constituting the polishing layer at pH 7.0 is below the upper limit value, the clogging suppression effect is improved because the polishing layer and the abrasive particles repel each other electrically. On the other hand, since the zeta potential at pH 7.0 is above the lower limit value, the amount of slurry retained on the polishing surface does not become excessively small, allowing for the maintenance of a good polishing speed.

[0084] In addition, in this specification, zeta potential refers to the potential generated on the surface of an electric double layer (sliding surface) by counter ions according to the surface charge of the material when the material comes into contact with a liquid. Specifically, it can be measured using an electrophoretic light scattering device (ELS-Z, manufactured by Otsuka Electronics Co., Ltd.) and a monitor latex (manufactured by Otsuka Electronics Co., Ltd.) dispersed in a 10 mM NaCl aqueous solution adjusted to pH 7.0 with an NaCl aqueous solution.

[0085] Also, the zeta potential of the polyurethane forming the polishing layer at pH 5.0 is, in the same view as above, preferably -5.0 mV or less, more preferably -40.0 to -12.0 mV, even more preferably -35.0 to -15.0 mV, and even more preferably -30.0 to -17.0 mV.

[0086] In addition, the zeta potential of the polyurethane forming the polishing layer at pH 8.0 is, in the same view as above, preferably -15.0 mV or less, more preferably -60.0 to -20.0 mV, even more preferably -50.0 to -25.0 mV, and even more preferably -40.0 to -30.0 mV.

[0087] <Storage Modulus>

[0088] After saturated swelling of the polyurethane constituting the polishing layer with water at 50°C, the storage modulus measured at 50°C is preferably 50 to 1,200 MPa, more preferably 100 to 1,100 MPa, even more preferably 200 to 1,000 MPa, and even more preferably 400 to 1,000 MPa. If the storage modulus at 50°C is above the lower limit value, the polishing layer has appropriate softness, so the polishing speed becomes good. On the other hand, if the storage modulus is below the upper limit value, the occurrence of scratches on the polished surface of the workpiece tends to decrease.

[0089] In addition, the storage modulus can be measured by the method described in the example.

[0090] A polyurethane satisfying the above storage modulus can be obtained, for example, by adjusting the content of nitrogen atoms derived from isocyanate groups in the polyurethane. Specifically, the content of nitrogen atoms derived from isocyanate groups in the polyurethane is preferably 4.5 to 7.6 mass%, more preferably 5.0 to 7.4 mass%, and even more preferably 5.2 to 7.3 mass%.

[0091] <Contact angle with water>

[0092] The contact angle of the polyurethane constituting the polishing layer with water is preferably 80 degrees or less, more preferably 70 degrees or less, even more preferably 60 degrees or less, and even more preferably 49 degrees or less. If the contact angle of the polyurethane with water is lower than the upper limit value above, the hydrophilicity of the polishing surface is improved, so scratches during polishing can be reduced.

[0093] In addition, the contact angle of the polyurethane with water can be measured according to the method described in the example.

[0094] The polyurethane constituting the polishing layer of the present invention preferably has a storage modulus within the above range and a contact angle with water within the above range. Specifically, after saturated swelling the polyurethane constituting the polishing layer with water at 50°C, the storage modulus measured at 50°C is preferably 50 to 1,200 MPa, more preferably 100 to 1,100 MPa, and even more preferably 200 to 1,000 MPa, and the contact angle of the polyurethane constituting the polishing layer with water is preferably 80 degrees or less, more preferably 70 degrees or less, even more preferably 60 degrees or less, and even more preferably 50 degrees or less.

[0095] If both the above storage modulus and the above contact angle with water are within the above range, the polishing uniformity and polishing stability are further improved.

[0096] <Density>

[0097] In the present invention, the polyurethane may be impregnated and solidified into a nonwoven fabric, or it may be formed from a molded sheet of polyurethane. In the case of a molded sheet, the density of the polyurethane is preferably 1.0 g / cm³ or higher, more preferably 1.1 g / cm³ or higher, and even more preferably 1.2 g / cm³ or higher. If the density of the molded body of the thermoplastic polyurethane is greater than or equal to the above lower limit value, it possesses suitable flexibility as an abrasive layer. Furthermore, regarding the thermoplastic polyurethane, non-foamed thermoplastic polyurethane is particularly preferred in that it exhibits excellent abrasive stability due to high rigidity and material homogeneity.

[0098] <Thickness of the polishing layer>

[0099] The shape of the polishing layer of the present invention can be appropriately adjusted, for example, by cutting, slicing, punching, etc., of a sheet-shaped molded body of thermoplastic polyurethane. The thickness of the polishing layer is not particularly limited, but is preferably 0.5 to 5.0 mm, more preferably 1.0 to 3.0 mm, and even more preferably 1.2 to 2.0 mm. If the thickness of the polishing layer is within the above range, productivity and handling are improved, and the stability of the polishing performance is also improved.

[0100] <Hardness of the abrasive layer>

[0101] The hardness of the polishing layer, as measured by JIS K 6253-3:2012, is preferably 60 or higher, more preferably 65 or higher, and preferably 95 or lower, more preferably 90 or lower. If the hardness is above the lower limit value, the following ability of the polishing pad on the surface to be polished is reduced, and flatness is improved. On the other hand, if the hardness is below the upper limit value, it is preferable because it becomes difficult for scratches to occur.

[0102] <Shape of the polished layer>

[0103] It is preferable that concave portions, such as grooves or holes, be formed on the polished surface of the polishing layer in a predetermined pattern of concentric, grid, spiral, or radial shapes by grinding or laser processing. Such concave portions help to uniformly and sufficiently supply slurry to the polishing surface, as well as to discharge polishing debris that causes scratches and prevent wafer breakage caused by adsorption on the polishing layer. For example, when forming grooves in a concentric shape, the spacing between grooves is preferably 1.0 to 50 mm, more preferably 1.5 to 30 mm, and even more preferably 2.0 to 15 mm. In addition, the width of the groove is preferably 0.1 to 3.0 mm, and more preferably 0.2 to 2.0 mm. Furthermore, the depth of the groove is less than the thickness of the polishing layer, preferably 0.2 to 1.8 mm, and more preferably 0.4 to 1.5 mm. In addition, regarding the cross-sectional shape of the groove, shapes such as rectangular, trapezoidal, triangular, and semicircular shapes are appropriately selected depending on the purpose.

[0104] [Grinding Pad]

[0105] The polishing pad of the present invention uses the polishing layer of the present invention. The polishing pad of the present invention may be composed solely of the polishing layer of the present invention, or it may be a laminate in which a cushion layer is laminated on the surface of the polishing layer that is not the polishing surface.

[0106] As for the cushion layer, it is preferable that it be a layer having a hardness lower than that of the polishing layer. When the hardness of the cushion layer is lower than that of the polishing layer, the hard polishing layer follows local irregularities on the surface to be polished, and the cushion layer follows the bending or curvature of the entire substrate to be polished, so polishing with an excellent balance of global flatness (a state in which large irregularities on the wafer substrate are reduced) and local flatness (a state in which local irregularities are reduced) becomes possible.

[0107] Specific examples of materials used as a cushion layer include a composite in which polyurethane is impregnated into a nonwoven fabric (e.g., "Suba 400" (manufactured by Nitta & Haas Co., Ltd.)); rubbers such as natural rubber, nitrile rubber, polybutadiene rubber, and silicone rubber; thermoplastic elastomers such as polyester-based thermoplastic elastomers, polyamide-based thermoplastic elastomers, and fluorine-based thermoplastic elastomers; foamed plastics; and polyurethane. Among these, polyurethane having a foamed structure is particularly preferred because it is easy to obtain the flexibility desired for a cushion layer.

[0108] The thickness of the cushion layer is not particularly limited, but, for example, it is preferably about 0.5 to 5 mm. If the cushion layer is excessively thin, the following effect for bending or curvature of the entire workpiece surface is reduced, and global flatness tends to decrease. On the other hand, if the cushion layer is excessively thick, the entire polishing pad becomes soft, and stable polishing tends to become difficult. When laminating a cushion layer onto a polishing layer, it is preferable that the thickness of the polishing pad be about 0.3 to 5 mm.

[0109] [Polishing Method]

[0110] The polishing method of the present invention uses the polishing layer of the present invention, comprising the steps of: fixing a polishing pad having the polishing layer on a polishing plate of a polishing device; and

[0111] A process of holding the workpiece to be polished in the holder of the polishing device so as to face the polishing surface of the polishing layer, and

[0112] The polishing method has a process of polishing a workpiece by supplying a neutral or alkaline polishing slurry between the polishing surface and the workpiece, and sliding the polishing pad and the workpiece relative to each other.

[0113] According to the polishing method of the present invention, when performing CMP using an alkaline slurry, by improving the repulsive force between the abrasive particles in the slurry and the polishing pad, the clogging of the abrasive particles can be suppressed, thereby extending the lifespan of the polishing pad.

[0114] An embodiment of the polishing method of the present invention when carried out by CMP is explained using FIG. 3.

[0115] In CMP, a CMP device (10) is used, which is equipped with a circular rotary plate (2) shown in FIG. 3, a slurry supply nozzle (3), a holder (4), and a pad conditioner (6). A polishing pad (1) having the polishing layer described above is attached to the surface of the rotary plate (2) using double-sided tape or the like. Also, the holder (4) supports the workpiece (5).

[0116] In the CMP device (10), the rotary plate (2) rotates in the direction indicated by the arrow by a motor not shown. Also, the holder (4) rotates in the direction indicated by the arrow, for example, by a motor not shown within the surface of the rotary plate (2). The pad conditioner (6) also rotates in the direction indicated by the arrow, for example, by a motor not shown within the surface of the rotary plate (2).

[0117] First, while flowing distilled water over the polishing surface of a polishing pad (1) that is fixed to a rotating platen (2) and rotates, a pad conditioner (6) for CMP, which has diamond particles fixed to a carrier surface by nickel electrodeposition or the like, is applied to the polishing surface of the polishing pad (1) to perform conditioning of the polishing surface of the polishing pad (1). Through conditioning, the polishing surface is adjusted to a surface roughness desirable for polishing the surface to be polished. Next, a slurry (7) is supplied from a slurry supply nozzle (3) to the polishing surface of the rotating polishing pad (1). Also, when performing CMP, a lubricant, a coolant, etc. may be used together with the slurry as needed.

[0118] Here, the slurry includes acidic slurries, alkaline slurries, and slurries near neutral, for example, a liquid medium such as water or oil; abrasive particles such as silica, alumina, cerium oxide, zirconium oxide, silicon carbide; and a slurry used in CMP containing oxidizing agents, reducing agents, chelating agents, etc., such as bases, acids, surfactants, and hydrogen peroxide, is preferably used.

[0119] When using the polishing layer of the present invention, it is preferable to perform CMP using a neutral or alkaline slurry to adjust to alkali, preferably using a slurry with a pH of 5.0 to 12.0, more preferably with a pH of 6.0 to 10.0, in order to maintain the repulsion between the abrasive grains and the polishing layer.

[0120] Then, a workpiece (5) that is fixed to a holder (4) and rotated is placed on a polishing pad (1) on which a slurry (7) is evenly spread across the polishing surface of the polishing layer. Then, the polishing process continues until a predetermined flatness is obtained. The finished quality is affected by adjusting the pressure applied during polishing or the speed of the relative movement between the rotating plate (2) and the holder (4).

[0121] Although the polishing conditions are not particularly limited, in order to perform polishing efficiently, it is preferable that the rotational speed of each of the rotary plate and the holder be a low rotation of 300 rpm or less, and that the pressure applied to the workpiece be 150 kPa or less so that scratches do not occur after polishing. During polishing, it is preferable to continuously supply slurry to the polishing surface using a pump or the like. Although the amount of slurry supplied is not particularly limited, it is preferable to supply it so that the polishing surface is always covered with slurry.

[0122] In addition, it is desirable to thoroughly wash the workpiece with flowing water after the polishing is finished, and then dry it by using a spin dryer or the like to remove water droplets attached to the workpiece. In this way, by polishing the workpiece surface with a slurry, a smooth surface can be obtained over the entire surface of the workpiece. Furthermore, the CMP described above can be preferably used for polishing various semiconductor materials such as silicon wafers.

[0123] Examples

[0124] An example of the present invention is described below by way of an example. Furthermore, the scope of the present invention is not limited by the following examples.

[0125] [Example 1]

[0126] A thermoplastic polyurethane having carboxyl groups was prepared by performing solution polymerization using polytetramethylene glycol (PTG850) with a number average molecular weight of 850, dimethylolpropionic acid (DMP) which is a compound having carboxyl groups, 1,4-butanediol (BD), and 4,4'-diphenylmethane diisocyanate (MDI) in a mass ratio of PTG850 : DMP : BD : MDI of 19.9 : 6.0 : 16.0 : 58.1 (molar ratio of DMP to BD is 20 / 80). A thermoplastic polyurethane was obtained by forming a solution of the prepared thermoplastic polyurethane into a cast film and then dehumidifying and drying it at 80°C for 20 hours.

[0127] The obtained thermoplastic polyurethane was evaluated as described below. The results are shown in Table 1.

[0128] [Examples 2–10, Comparative Examples 1–3]

[0129] Polyurethanes of Examples 2 to 10 and Comparative Examples 1 to 3 were prepared in the same manner as Example 1, except that they were made according to the formulations in Table 1. The evaluation described below was performed on the obtained thermoplastic polyurethanes. The results are shown in Table 1.

[0130] In addition, the raw materials listed in Table 1 are as follows.

[0131] BD: 1,4-butanediol

[0132] PD: 1,5-Pentanediol

[0133] DMP: Dimethylolpropionic acid (2,2-bis(hydroxymethyl)propionic acid)

[0134] DMB: Dimethylolbutyric acid (2,2-bis(hydroxymethyl)butyric acid)

[0135] MPD: 3-methyl-1,5-pentanediol

[0136] PTG850: Polytetramethylene glycol with a number average molecular weight of 850.

[0137] PEG600: Polyethylene glycol with a number-average molecular weight of 600.

[0138] PD1000: Polycarbonate diol with a number average molecular weight of 1,000

[0139] MDI: 4,4'-Diphenylmethane diisocyanate

[0140] [Evaluation Method]

[0141] Each evaluation was performed on the thermoplastic polyurethanes obtained in the examples and comparative examples according to the method described below.

[0142] <Measurement of Zeta Potential>

[0143] A molded sheet of thermoplastic polyurethane with a thickness of 0.3 to 0.5 mm was obtained by inserting pellets (5 to 14 g) of each thermoplastic polyurethane prepared in the examples and comparative examples into a Teflon (registered trademark) sheet and then pressing and molding them using a heat press at 200 to 230 ℃.

[0144] Next, the obtained molded sheet was cut into 30 mm × 60 mm pieces, and the surface was cleaned. Then, using an electrophoretic light scattering device (ELS-Z, manufactured by Otsuka Electronics Co., Ltd.), the sample was mounted in a flat-plate measuring cell. Subsequently, the zeta potential was measured using a monitor latex (manufactured by Otsuka Electronics Co., Ltd.) dispersed in a 10 mM NaCl aqueous solution adjusted to pH 5.0, pH 7.0, and pH 8.0, respectively, with an NaOH aqueous solution.

[0145] <Contact Angle with Water>

[0146] For each thermoplastic polyurethane prepared in the examples and comparative examples, a film with a thickness of 300 μm was prepared by a heat press method. Subsequently, the obtained film was left for 3 days under conditions of 20°C and 65% RH, and then, after 15 minutes had passed since water was applied to the surface, the contact angle with water was measured using a DropMaster 500 manufactured by Kyowa Interface Science Co., Ltd.

[0147] <Storage modulus at 50°C after saturated swelling with 50°C water>

[0148] For each thermoplastic polyurethane prepared in the examples and comparative examples, an injection-molded sheet with a width of 5 mm, a length of 30 mm, and a thickness of 2 mm was prepared. Then, the injection-molded sheet was immersed in water at 50°C for 3 days. Subsequently, after removing the injection-molded sheet from the water and wiping off the water from the surface, the storage modulus was determined by measuring the dynamic viscoelasticity ratio at 50°C at a frequency of 11 Hz using a dynamic viscoelasticity measuring device ("DVE Rheospectra", manufactured by Rheology Co., Ltd.).

[0149] <Evaluation of Grinding Pads>

[0150] A polishing pad was manufactured using the polyurethane obtained in the examples and comparative examples, and an evaluation was performed.

[0151] [Manufacture of a fabric containing PET nonwoven fabric and non-porous polyurethane]

[0152] A strand of a sea-island type composite fiber with a sea-island number of 25, comprising polyethylene terephthalate (PET) as the island component and water-soluble thermoplastic PVA as the sea component, with a sea component / island component mass ratio of 25 / 75, was extruded from a melt composite spinning die at 265°C, and the sea-island type composite fiber was spun by cooling while stretching and fineening it. Then, long fiber webs were obtained by continuously collecting and pressing. Next, the long fiber webs were overlapped, needle punching was performed alternately on both sides, and the long fiber webs were bonded together to obtain a three-dimensional bonded body.

[0153] Next, as a non-porous polymer elastomer, a water-based emulsion of polyurethane for fabric was impregnated into a three-dimensional composite by dip-nip and a drying treatment was performed. Then, the water-soluble thermoplastic PVA of the island component was dissolved and removed from the island-type composite fiber by dip-niping the three-dimensional composite in hot water, and by drying, a non-woven fabric (thickness 1.8 mm) of PET fiber (average single fiber fineness 0.05 dtex) having 25 bundles of single fibers and a fabric containing non-porous polyurethane were obtained.

[0154] [Impregnation of Thermoplastic Polyurethane in Examples and Comparative Examples]

[0155] The obtained fabric was cut into 380 mm × 380 mm pieces. Subsequently, the thermoplastic polyurethane obtained in the examples and comparative examples was impregnated into the cut fabrics, respectively.

[0156] Impregnation was performed as follows. A DMF solution with a concentration of 25 mass% of each thermoplastic polyurethane was heated to 30°C, and the fabric was placed thereon for 10 minutes to allow the DMF solution to penetrate. Subsequently, the fabric was immersed in the DMF solution for 5 minutes, after which the fabric was removed, placed on a glass plate, and the surface of the fabric was traced with a doctor knife to remove the attached DMF solution. The same operation was performed on the reverse side.

[0157] Next, an aqueous solution with a DMF concentration of 10 mass% was maintained at 30°C, and the fabric was immersed in it. By leaving it for 30 minutes, the thermoplastic polyurethane of the examples and comparative examples was coagulated, and then the fabric impregnated with the thermoplastic polyurethane was immersed in hot water at 70 to 95°C. Subsequently, the fabric impregnated with the thermoplastic polyurethane was placed on a metal roller, the water was squeezed out, and then it was immersed in hot water again to be washed. This operation was repeated until the DMF concentration in the squeezed water was 0.3 mass% or less. In addition, the concentration of DMF was measured using an Abbe refractometer 1T (Atago Co., Ltd.).

[0158] Next, the washed fabric was placed in a hot air dryer (device name: Safety Oven SPH-202 / Espec Co., Ltd.) and dried at 100°C for 40 minutes. In this way, the fabric for the abrasive pad was obtained.

[0159] [Flattening and Grooving of the Fabric on the Abrasive Pad]

[0160] The surface of the abrasive pad material was buffed with sandpaper (grit #180) to eliminate thickness unevenness and flatten it, and then a grid groove with a groove width of 2.0 mm, a groove depth of 0.5 mm, and a pitch of 15 mm was formed on the abrasive surface of the abrasive pad using a flattening groove processing machine. Then, by cutting the abrasive pad with the formed grid groove into a circle with a diameter of 370 mm, an abrasive pad with a groove with a thickness of 1.5 mm (an abrasive pad consisting only of an abrasive layer) was obtained.

[0161] Next, the obtained polishing pad was polished according to the polishing method of the present invention. Specifically, the obtained polishing pad was mounted on a polishing device "MAT-BC15" manufactured by M·A·T Co., Ltd. Then, using a diamond dresser (#100 - coverage 80%, diameter 19 cm, mass 1 kg) manufactured by Allied Materials Co., Ltd., conditioning of the pad surface was performed for 15 minutes under conditions of a dresser rotation speed of 140 rpm, a platen rotation speed of 100 rpm, while distilled water was flowed at a rate of 150 mL / min. Next, a slurry with a pH of 7.0 to 11 was prepared by diluting a slurry (colloidal silica, slurry concentration 1%) 20 times. Then, under conditions of a platen rotation speed of 100 rpm, a head rotation speed of 99 rpm, and a polishing pressure of 55.1 kPa, a slurry was supplied to the polishing surface of the polishing pad at a rate of 200 mL / min, and a silicon wafer with a diameter of 4 inches having a silicon oxide film with a thickness of 1000 nm on its surface was polished for 60 seconds. After polishing for 60 seconds, the polishing pad was conditioned for 30 seconds. Then, another silicon wafer was polished again, and conditioning was performed for an additional 30 seconds. In this way, 10 silicon wafers were polished.

[0162] Then, the speed was calculated from the weight change of the 10th polished silicon wafer before and after polishing, and the average value was taken as the polishing speed.

[0163] <Change in polishing speed (nm / min), Polishing speed stability (%)>

[0164] A 6-hour long-run test was conducted using each polishing layer, and the change in polishing speed at the later stage of polishing (after 5 hours of polishing) was defined as the "change in polishing speed (nm / min)" based on the value of the polishing speed at the point where the polishing speed stabilized (after 1 hour of polishing). In addition, the ratio of the change after 5 hours of polishing to after 1 hour of polishing was defined as the "polishing speed stability (%)".

[0165] <Appearance Test (Scratch Amount)>

[0166] After polishing, the appearance of the workpiece was observed using a high-intensity halogen lighting device. The presence and number of scratches, abrasions, contamination, and polishing residues were evaluated according to the following evaluation criteria. Additionally, FIG. 4 is a drawing showing the state with scratches, the state with abrasions, and the state with contamination and polishing residues, respectively, and corresponds to “3” to “4” of the following evaluation.

[0167] <Evaluation Criteria>

[0168] [1 : Very good]

[0169] No scratches, abrasions, contamination, or polishing residues are present on more than 90% of the evaluated silicon wafers.

[0170] [2 : Good]

[0171] No scratches, abrasions, contamination, or polishing residues are present on more than 70% but less than 90% of the evaluated silicon wafers.

[0172] [3 : Bad]

[0173] Scratches, abrasions, contamination, and polishing residue are present on more than 50% but less than 70% of the evaluated silicon wafers.

[0174] [4 : Very bad]

[0175] Scratches, abrasions, contamination, or polishing residue are present on more than 70% of the evaluated silicon wafers, or large scratches occur.

[0176] <Clocking (%)>

[0177] After polishing for 6 hours, a cross-section of the polishing pad was photographed, and the ratio of the part where the abrasive grains were clogged and colored brown was defined as the amount of clogging.

[0178]

[0179] As is evident from the results of Table 1, according to the present invention, clogging can be suppressed, and thus a polishing pad that can be polished stably for a long life while suppressing the occurrence of scratches can be provided.

[0180] Also, as is evident from the comparison of Examples 1 to 9 and Example 10 in Table 1, it is more preferable to use polyetherdiol as the polymeric diol in terms of excellent stability and clogging inhibition.

[0181] [Example 11]

[0182] [Manufacture of fabric containing PET nonwoven fabric and non-porous polyurethane]

[0183] A strand of a sea-island type composite fiber with a sea-island number of 25, comprising polyethylene terephthalate (PET) as the sea component and water-soluble thermoplastic PVA as the sea component, with a sea component / sea component mass ratio of 25 / 75, was extruded from a melt composite spinning die at 265°C, and the sea-island type composite fiber was spun by cooling while stretching and slendering it. Then, long fiber webs were obtained by continuously collecting and pressing. Next, the long fiber webs were overlapped, needle punching was performed alternately on both sides, and the long fiber webs were bonded together to obtain a three-dimensional bonded body.

[0184] Next, as a non-porous polymer elastomer, a water-based emulsion of polyurethane for fabric was impregnated into a three-dimensional composite by dip-nip and a drying treatment was performed. Then, the water-soluble thermoplastic PVA of the island component was dissolved and removed from the island-type composite fiber by dip-niping the three-dimensional composite in hot water, and by drying, a non-woven fabric (thickness 1.8 mm) of PET fiber (average single fiber fineness 0.05 dtex) having 25 bundles of single fibers and a fabric containing non-porous polyurethane were obtained.

[0185] [Impregnation of Thermoplastic Polyurethane in Examples and Comparative Examples]

[0186] Next, the obtained nonwoven fabric was impregnated with an aqueous dispersion of cross-linked polyurethane elastomer A adjusted to a solid content concentration of 25 mass%.

[0187] In addition, the aqueous dispersion of crosslinked polyurethane elastomer A is obtained by adding 3 parts by mass of a carbodiimide-based crosslinking agent to 100 parts by mass of an aqueous dispersion of polyurethane, which is obtained by polymerizing a polyol component consisting of 95 parts by mass of an amorphous polycarbonate-based polyol, which is a copolymer polyol of hexamethylene carbonate and pentamethylene carbonate, and 5 parts by mass of 2,2-bis(hydroxymethyl)propionic acid, a chain extender consisting of dimethylolpropionic acid (a diol having a carboxyl group), a polyisocyanate compound consisting of 4,4'-dicyclohexylmethane diisocyanate, and an amine-based chain extender consisting of hydrazine.

[0188] The ratio of the polyol component, polyisocyanate component, and chain extender forming the polyurethane was formulated as polyol component : polyisocyanate component : chain extender = 55 : 40 : 5.

[0189] In addition, regarding the impregnation, the amount of solid content of the aqueous dispersion attached to the mass of the nonwoven fabric was 15 mass%. Then, the polyurethane was solidified by heat-treating the nonwoven fabric impregnated with the aqueous dispersion at 90°C under a 50% RH atmosphere. After that, a cross-linked structure was formed by further heat-treating at 150°C. Then, a fabric for the abrasive pad was obtained by further heat-pressing at 150°C.

[0190] [Flattening and Grooving of the Fabric on the Abrasive Pad]

[0191] The surface of the abrasive pad material was buffed with sandpaper (grit #180) to eliminate thickness unevenness and flatten it, and then a grid groove with a groove width of 2.0 mm, a groove depth of 0.5 mm, and a pitch of 15 mm was formed on the abrasive surface of the abrasive pad using a flattening groove processing machine. Then, by cutting the abrasive pad with the formed grid groove into a circle with a diameter of 370 mm, an abrasive pad with a groove with a thickness of 1.5 mm (an abrasive pad consisting only of an abrasive layer) was obtained.

[0192] The obtained polishing pads were evaluated in the same manner as in Examples 1 to 10. The results are shown in Table 2.

[0193]

[0194] As is evident from the results of Table 2, according to the present invention, even though it is a water-based polyurethane, it can be seen that a polyurethane can be obtained that can be polished stably for a long life while suppressing the occurrence of scratches, just like a solvent-based polyurethane.

Claims

Claim 1 A polishing layer comprising a nonwoven fabric and a solvent-based polyurethane impregnated into the nonwoven fabric, wherein the polyurethane has at least one structural unit derived from a compound having a carboxyl group, and the amount of the structural unit derived from the compound having a carboxyl group among the total structural units constituting the polyurethane is 3 to 30 mol%. Claim 2 A polishing layer according to claim 1, wherein the polyurethane comprises at least a structural unit derived from a compound having a carboxyl group, a structural unit derived from a chain extender, a structural unit derived from a polymeric diol, and a structural unit derived from an organic diisocyanate. Claim 3 delete Claim 4 A polishing layer according to claim 1, wherein the zeta potential of the polyurethane constituting the polishing layer at pH 7.0 is -10.0 mV or less. Claim 5 In claim 1, the abrasive layer, wherein the polyurethane is a non-foamed material. Claim 6 A polishing layer according to claim 1, wherein, with respect to the polyurethane, after saturated swelling with water at 50°C, the storage modulus measured at 50°C is 50 to 1,200 MPa, and the contact angle with water is 80 degrees or less. Claim 7 A polishing pad using the polishing layer described in any one of claims 1, 2, and 4 to 6. Claim 8 A polishing method using a polishing layer described in any one of claims 1, 2 and 4 to 6, comprising the steps of: fixing a polishing pad having the polishing layer on a surface plate of a polishing device; holding a workpiece to be polished in a holder of a polishing device so as to face the polishing surface of the polishing layer; and polishing the workpiece by sliding the polishing pad and the workpiece relatively while supplying a neutral or alkaline polishing slurry between the polishing surface and the workpiece. Claim 9 delete Claim 10 delete

Citation Information

Patent Citations

  • Abrasive composition for metal chemical mechanical polishing

    JP2007287938A

  • Urethane-based prepolymer, polishing pad and preparation method thereof

    KR1020180024096A

  • Polymer body, polishing pad, and method for producing polymer body

    JP2017141393A