Transparent conductive film

A transparent conductive film with a krypton-containing light-transmitting layer addresses the slow etching issue, ensuring high etching rates and improved manufacturing efficiency.

KR103045258B1Active Publication Date: 2026-11-06NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020227030817
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-02
Filing Date
2021-03-18
Publication Date
2026-11-06
Estimated Expiration
2041-03-18

AI Technical Summary

Technical Problem

The etching speed of the light-transmitting conductive layer in conventional transparent conductive films is slow, which hampers the efficiency of device manufacturing processes.

Method used

A transparent conductive film comprising a transparent substrate and a light-transmitting conductive layer containing krypton, with specific resistivity, hole mobility, and carrier density ratios, enabling a high etching rate.

Benefits of technology

The film achieves a high etching rate in the light-transmitting conductive layer, enhancing manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022093415853-PCT00002_ABST
    Figure 112022093415853-PCT00002_ABST
Patent Text Reader

Abstract

The transparent conductive film (X) of the present invention comprises a transparent substrate (10) and a light-transmitting conductive layer (20) in this order in the thickness direction (D). The light-transmitting conductive layer (20) contains krypton and has a resistivity of less than 2.8×10-4 Ω·cm. The light-transmitting conductive layer (20) has a hole mobility μ (cm2 / V·s) and a carrier density n×10¹⁹ (cm⁻³), and the ratio of n to μ is 4 or greater.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a transparent conductive film. Background Technology

[0002] Conventionally, a transparent conductive film is known to have a transparent substrate film and a transparent conductive layer (light-transmitting conductive layer) arranged sequentially in the thickness direction. The light-transmitting conductive layer is used as a conductive film for patterning transparent electrodes in various devices such as liquid crystal displays, touch panels, and optical sensors. The light-transmitting conductive layer is formed, for example, by depositing a conductive oxide on a substrate film by a sputtering method. In the sputtering method, conventionally, an inert gas such as argon is used as a sputtering gas to collide with a target (a material supply for depositing film) and eject atoms from the target surface. Technology regarding such a transparent conductive film is described, for example, in Patent Document 1 below. Prior art literature

[0003] Japanese Patent Publication No. 2017-71850 The problem to be solved

[0004] The light-transmitting conductive layer of a transparent conductive film is patterned by an etching process involving a predetermined etching mask for the light-transmitting conductive layer. However, the transparent conductive film of Patent Document 1 has a problem in that the etching speed in the etching process for the light-transmitting conductive layer is slow. The slow etching speed of the light-transmitting conductive layer in the transparent conductive film is undesirable from the perspective of the efficiency of the device manufacturing process in which the transparent conductive film is used.

[0005] The present invention provides a transparent conductive film suitable for realizing a high etching rate in a light-transmitting conductive layer. means of solving the problem

[0006] The present invention [1] comprises a transparent substrate and a light-transmitting conductive layer in this order in the thickness direction, wherein the light-transmitting conductive layer contains krypton and is 2.8×10 -4 The light-transmitting conductive layer has a resistivity of less than Ω·cm, and the light-transmitting conductive layer has a hole mobility μ (cm²). 2 / V·s) and carrier density n×10 19 (cm -3 It includes a transparent conductive film having ) and a ratio of n to μ of 4 or more.

[0007] The present invention [2] comprises a transparent conductive film described in [1], wherein the light-transmitting conductive layer contains an indium-containing conductive oxide.

[0008] The present invention [3] has a hole mobility of 5 cm 2 / V·s or more 40 cm 2 It includes a transparent conductive film described in [1] or [2] above, which is less than or equal to / V·s.

[0009] The present invention [4] has a carrier density of 100×10 19 cm -3 170×10 19 cm -3 It includes a transparent conductive film described in any one of [1] to [3] above.

[0010] The present invention [5] includes a transparent conductive film described in any one of [1] to [4], wherein the light-transmitting conductive layer is patterned.

[0011] The present invention [6] has a light-transmitting conductive layer, which is 2.2×10 -4 It includes a transparent conductive film described in any one of [1] to [5] above, having a resistivity of less than Ω·cm. Effects of the invention

[0012] The transparent conductive film of the present invention comprises a light-transmitting conductive layer containing krypton and also 2.8 × 10⁻⁶ -4It has a resistivity of less than Ω·cm. In addition, in the transparent conductive film of the present invention, the hole mobility μ (cm²) of the light-transmitting conductive layer 2 / V·s) and carrier density n×10 19 (cm -3 In this case, the ratio of n to μ is 4 or greater. Therefore, the transparent conductive film of the present invention is suitable for realizing a high etching rate in a light-transmitting conductive layer. Brief explanation of the drawing

[0013] FIG. 1 is a schematic cross-sectional view of one embodiment of the transparent conductive film of the present invention. FIG. 2 illustrates a method for manufacturing a transparent conductive film as shown in FIG. 1. FIG. 2A illustrates a process for preparing a resin film, FIG. 2B illustrates a process for forming a functional layer on a resin film, FIG. 2C illustrates a process for forming a light-transmitting conductive layer on a functional layer, and FIG. 2D illustrates a process for crystallizing a light-transmitting conductive layer. FIG. 3 shows a case in which a light-transmitting conductive layer is patterned in the transparent conductive film shown in FIG. 1. Figure 4 is a graph showing the relationship between the amount of oxygen introduced when forming a light-transmitting conductive layer by sputtering and the resistivity of the formed light-transmitting conductive layer. Specific details for implementing the invention

[0014] FIG. 1 is a schematic cross-sectional view of a transparent conductive film (X), which is an embodiment of the transparent conductive film of the present invention. The transparent conductive film (X) comprises a transparent substrate (10) and a light-transmitting conductive layer (20) in this order, facing one side in the thickness direction (D). The transparent conductive film (X) has a shape that widens in a direction orthogonal to the thickness direction (D) (plane direction). The light-transmitting conductive film (X) is an element provided in a touch sensor device, a light-diffusing element, a photoelectric conversion element, a heat wire control member, an antenna member, an electromagnetic shield member, a lighting device, an image display device, etc.

[0015] In this embodiment, the transparent substrate (10) is provided with a resin film (11) and a functional layer (12) in this order toward one side of the thickness direction (D). The transparent substrate (10) has a shape that widens in a direction perpendicular to the thickness direction (D) (plane direction).

[0016] The resin film (11) is a transparent resin film having flexibility. Examples of materials for the resin film (11) include polyester resin, polyolefin resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin, and polystyrene resin. Examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of polyolefin resins include polyethylene, polypropylene, and cycloolefin polymer (COP). Examples of acrylic resins include polymethacrylate. As for the material of the resin film (11), polyolefin resin is preferably used, and more preferably COP is used, for example, in terms of transparency and strength.

[0017] The surface of the functional layer (12) in the resin film (11) may be surface modified. Examples of surface modification treatments include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.

[0018] The thickness of the resin film (11) is preferably 1 μm or more, more preferably 10 μm or more, and even more preferably 30 μm or more. The thickness of the resin film (11) is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 75 μm or less. These configurations regarding the thickness of the resin film (11) are suitable for ensuring the handling properties of the transparent conductive film (X).

[0019] The total light transmittance (JIS K 7375-2008) of the resin film (11) is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. This configuration is suitable for ensuring the transparency required for the transparent conductive film (X) when the transparent conductive film (X) is provided in a touch sensor device, a light-diffusing element, a photoelectric conversion element, a heat-controlling member, an antenna member, an electromagnetic shield member, a lighting device, and an image display device, etc. The total light transmittance of the resin film (11) is, for example, 100% or less.

[0020] In this embodiment, the functional layer (12) is located on one side in the thickness direction (D) of the resin film (11). Also, in this embodiment, the functional layer (12) is a hard coat layer to make it difficult for scratches to form on the exposed surface (upper surface in FIG. 1) of the light-transmitting conductive layer (20).

[0021] The hard coat layer is a cured product of a curable resin composition. Examples of resins contained in the curable resin composition include polyester resin, acrylic resin, urethane resin, amide resin, silicone resin, epoxy resin, and melamine resin. Additionally, examples of the curable resin composition include a UV-curing type resin composition and a thermosetting type resin composition. In order to help improve the manufacturing efficiency of the transparent conductive film (X) because it can be cured without high-temperature heating, the UV-curing type resin composition is preferably used as the curable resin composition. Specifically, as an example of the UV-curing type resin composition, the composition for forming a hard coat layer described in Japanese Patent Publication No. 2016-179686 may be used.

[0022] The surface of the light-transmitting conductive layer (20) in the functional layer (12) may be surface modified. Examples of surface modification treatments include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.

[0023] The thickness of the functional layer (12) as a hard coat layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more. Such a configuration is suitable for exhibiting sufficient abrasion resistance in the light-transmitting conductive layer (20). From the perspective of ensuring the transparency of the functional layer (12), the thickness of the functional layer (12) as a hard coat layer is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less.

[0024] The thickness of the transparent substrate (10) is preferably 1 μm or more, more preferably 10 μm or more, even more preferably 15 μm or more, and particularly preferably 30 μm or more. The thickness of the transparent substrate (10) is preferably 310 μm or less, more preferably 210 μm or less, even more preferably 110 μm or less, and particularly preferably 80 μm or less. These configurations regarding the thickness of the transparent substrate (10) are suitable for ensuring the handling properties of the transparent conductive film (X).

[0025] The total light transmittance (JIS K 7375-2008) of the transparent substrate (10) is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. This configuration is suitable for ensuring the transparency required for the transparent conductive film (X) when the transparent conductive film (X) is provided in a touch sensor device, a light-diffusing element, a photoelectric conversion element, a heat-controlling member, an antenna member, an electromagnetic shield member, a lighting device, and an image display device, etc. The total light transmittance of the transparent substrate (10) is, for example, 100% or less.

[0026] In this embodiment, the light-transmitting conductive layer (20) is located on one side of the thickness direction (D) of the transparent substrate (10). The light-transmitting conductive layer (20) is a crystalline film that combines light transmittance and conductivity.

[0027] The light-transmitting conductive layer (20) is a layer formed of a light-transmitting conductive material. The light-transmitting conductive material contains, for example, a conductive oxide as a main component.

[0028] Examples of conductive oxides include metal oxides containing at least one metal or metalloid selected from the group consisting of In, Sn, Zn, Ga, Sb, Ti, Si, Zr, Mg, Al, Au, Ag, Cu, Pd, and W. Specifically, examples of conductive oxides include indium-containing conductive oxides and antimony-containing conductive oxides. Examples of indium-containing conductive oxides include indium-tin composite oxide (ITO), indium-zinc composite oxide (IZO), indium-gallium composite oxide (IGO), and indium-gallium-zinc composite oxide (IGZO). Examples of antimony-containing conductive oxides include antimony-tin composite oxide (ATO). In terms of realizing high transparency and good conductivity, indium-containing conductive oxides are preferably used as conductive oxides, and more preferably, ITO is used. This ITO may contain metals or metalloids other than In and Sn in an amount less than the respective content of In and Sn.

[0029] When ITO is used as a conductive oxide, the ratio of the tin oxide content to the total content of indium oxide (In2O3) and tin oxide (SnO2) in the light-transmitting conductive layer (20) (tin oxide content ratio) is preferably 1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, and particularly preferably 7 mass% or more. Such a composition is suitable for ensuring the durability of the light-transmitting conductive layer (20). Also, from the perspective of obtaining a light-transmitting conductive layer (20) that is prone to crystallization by heating, the tin oxide content ratio is preferably 15 mass% or less, more preferably 13 mass% or less, and even more preferably 12 mass% or less. The above tin oxide content ratio can be obtained from the XPS spectrum measured by X-ray Photoelectron Spectroscopy on the object to be measured.

[0030] The tin oxide content ratio in the light-transmitting conductive layer (20) does not need to be uniform in the thickness direction (D). For example, the light-transmitting conductive layer (20) may include a first layer with a relatively high tin oxide content ratio and a second layer with a relatively low tin oxide content ratio in this order from the transparent substrate (10) side. The tin oxide content ratio in the first layer is preferably 5 mass% or more, more preferably 8 mass% or more. The tin oxide content ratio in the first layer is preferably 15 mass% or less, more preferably 13 mass% or less. The tin oxide content ratio in the second layer is preferably 0.5 mass% or more, more preferably 2 mass% or more. The tin oxide content ratio in the second layer is preferably 8 mass% or less, more preferably 5 mass% or less. The ratio of the thickness of the first layer to the thickness of the light-transmitting conductive layer (20) is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more. Also, the ratio of the thickness of the second layer to the thickness of the light-transmitting conductive layer (20) is preferably 50% or less, more preferably 40% or less, and even more preferably 30% or less.

[0031] The light-transmitting conductive layer (20) contains krypton (Kr) as a noble gas atom. In this embodiment, the noble gas atom in the light-transmitting conductive layer (20) originates from the noble gas atom used as a sputtering gas in the sputtering method described later. In this embodiment, the light-transmitting conductive layer (20) is a film (sputter film) formed by the sputtering method.

[0032] A configuration in which the light-transmitting conductive layer (20) contains Kr is suitable for realizing low resistance in the light-transmitting conductive layer (20). In addition, the configuration is suitable for realizing a high etching rate when the light-transmitting conductive layer (20) is etched, for example, for patterning. The presence of Kr in the light-transmitting conductive layer (20) is identified, for example, by fluorescent X-ray analysis, which will be described later with respect to the examples.

[0033] The content ratio of Kr in the light-transmitting conductive layer (20) is, for example, 0.5 atomic% or less throughout the thickness direction (D), preferably 0.3 atomic% or less, and more preferably 0.2 atomic% or less. This composition is suitable for realizing good crystal growth and forming large crystal grains when crystallizing an amorphous light-transmitting conductive layer (the light-transmitting conductive layer (20') described later) by heating during the manufacturing process of a transparent conductive film (X), and thus is suitable for obtaining a low-resistance light-transmitting conductive layer (20) (the larger the crystal grains in the light-transmitting conductive layer (20), the lower the resistance of the light-transmitting conductive layer (20)). Also, the content ratio of Kr in the light-transmitting conductive layer (20) is, for example, 0.0001 atomic% or more throughout the thickness direction (D).

[0034] The Kr content ratio in the light-transmitting conductive layer (20) does not have to be uniform in the thickness direction (D). For example, in the thickness direction (D), the Kr content ratio may increase or decrease as it moves further away from the transparent substrate (10). Alternatively, in the thickness direction (D), a portion region where the Kr content ratio increases as it moves further away from the transparent substrate (10) may be located on the side of the transparent substrate (10), and a portion region where the Kr content ratio decreases as it moves further away from the transparent substrate (10) may be located on the opposite side of the transparent substrate (10). Alternatively, in the thickness direction (D), a portion region where the Kr content ratio decreases as it moves further away from the transparent substrate (10) may be located on the side of the transparent substrate (10), and a portion region where the Kr content ratio increases as it moves further away from the transparent substrate (10) may be located on the opposite side of the transparent substrate (10).

[0035] It is preferable that the light-transmitting conductive layer (20) contains only Kr as a noble gas atom. Such a configuration is desirable from the perspective of realizing low resistance in the light-transmitting conductive layer (20). In addition, the configuration is desirable from the perspective of realizing a high etching rate when the light-transmitting conductive layer (20) is etched, for example, for patterning.

[0036] When the light-transmitting conductive layer (20) contains noble gas atoms other than Kr, noble gas atoms other than Kr may include, for example, argon (Ar) and xenon (Xe). From the perspective of reducing the manufacturing cost of the transparent conductive film (X), the light-transmitting conductive layer (20) preferably does not contain Xe.

[0037] The content ratio of noble gas atoms (containing Kr) in the light-transmitting conductive layer (20) is, for example, 0.5 atomic% or less, preferably 0.3 atomic% or less, and more preferably 0.2 atomic% or less throughout the thickness direction (D). This configuration is suitable for realizing good crystal growth and forming large crystal grains when crystallizing an amorphous light-transmitting conductive layer by heating to form a light-transmitting conductive layer (20) during the manufacturing process of a transparent conductive film (X), and thus is suitable for obtaining a low-resistance light-transmitting conductive layer (20). In addition, the content ratio of noble gas atoms in the light-transmitting conductive layer (20) is, for example, 0.0001 atomic% or more throughout the thickness direction (D).

[0038] The thickness of the light-transmitting conductive layer (20) is, for example, 10 nm or more, preferably 25 nm or more, more preferably 30 nm or more, even more preferably 35 nm or more, and particularly preferably 40 nm or more. Such a configuration is suitable for achieving low resistance of the light-transmitting conductive layer (20). In addition, the thickness of the light-transmitting conductive layer (20) is, for example, 1000 nm or less, preferably less than 300 nm, more preferably 250 nm or less, even more preferably 200 nm or less, even more preferably 160 nm or less, particularly preferably less than 150 nm, and most preferably 148 nm or less. Such a configuration is suitable for reducing the compressive residual stress of the light-transmitting conductive layer (20) and suppressing bending of the transparent conductive film (X).

[0039] The total light transmittance (JIS K 7375-2008) of the light-transmitting conductive layer (20) is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring transparency in the light-transmitting conductive layer (20). In addition, the total light transmittance of the light-transmitting conductive layer (20) is, for example, 100% or less.

[0040] The surface resistance of the light-transmitting conductive layer (20) is, for example, 200 Ω / □ or less, preferably 70 Ω / □ or less, more preferably 55 Ω / □ or less, even more preferably 50 Ω / □ or less, and particularly preferably 45 Ω / □ or less. The surface resistance of the light-transmitting conductive layer (20) is, for example, 1 Ω / □ or more. These configurations regarding surface resistance are suitable for ensuring the low resistance required of the light-transmitting conductive layer (20) when a transparent conductive film (X) is provided in a touch sensor device, a light-diffusing element, a photoelectric conversion element, a heat wire control member, an antenna member, an electromagnetic shield member, a lighting device, and an image display device, etc. The surface resistance can be measured by the four-terminal method in accordance with JIS K 7194.

[0041] The resistivity of the light-transmitting conductive layer (20) is 2.8×10 -4 Less than Ω·cm, preferably 2.2×10 -4 Ω·cm or less, more preferably 2×10⁻⁶ -4 Ω·cm or less, more preferably 1.8×10⁻⁶ -4 Ω·cm or less, particularly preferably 1.7×10⁻⁶ -4 It is Ω·cm or less. The resistivity of the light-transmitting conductive layer (20) is, for example, 0.1×10⁻⁶ -4The resistivity is greater than or equal to Ω·cm. These configurations regarding resistivity are suitable for ensuring low resistivity required for a light-transmitting conductive layer (20) when a transparent conductive film (X) is provided in a touch sensor device, a light-diffusing element, a photoelectric conversion element, a heat wire control member, an antenna member, an electromagnetic shield member, a lighting device, and an image display device, etc. Resistivity can be obtained by multiplying the surface resistance by the thickness.

[0042] The hole mobility in the light-transmitting conductive layer (20) is preferably 5 cm 2 / V·s or more, more preferably 10 cm 2 / V·s or more, more preferably 20 cm 2 It is greater than / V·s. The hole mobility of the light-transmitting conductive layer (20) is preferably 40 cm 2 / V·s or less, more preferably 35 cm 2 / V·s or less, more preferably 30 cm 2 The hole mobility is less than or equal to / V·s. The hole mobility can be adjusted, for example, by adjusting the Kr content ratio in the light-transmitting conductive layer (20), and by adjusting various conditions when sputtering the amorphous light-transmitting conductive layer (the light-transmitting conductive layer (20') described later) which is converted into the light-transmitting conductive layer (20) by heating. Such conditions include, for example, the temperature of the substrate (transparent substrate (10) in this embodiment) on which the amorphous light-transmitting conductive layer is deposited, or the sputter output of the substrate side (transparent substrate (10) side in this embodiment). In addition, the hole mobility can also be adjusted by adjusting the surface characteristics (surface characteristics of the functional layer (12) in this embodiment), such as the surface shape of the substrate on which the amorphous light-transmitting conductive layer is deposited.

[0043] The carrier density in the light-transmitting conductive layer (20) is preferably 100×10 19 cm -3 Ideally, 120×10 19cm -3 That is all. The carrier density in the light-transmitting conductive layer (20) is preferably 170×10 19 cm -3 Below, more preferably 150×10 19 cm -3 The following describes how the carrier density can be adjusted, for example, by adjusting the Kr content ratio in the light-transmitting conductive layer (20), and by adjusting various conditions when sputtering the amorphous light-transmitting conductive layer (the light-transmitting conductive layer (20') described later) which is converted into the light-transmitting conductive layer (20) by heating. Examples of such conditions include the temperature of the substrate (transparent substrate (10) in this embodiment) on which the amorphous light-transmitting conductive layer is deposited, and the amount of oxygen introduced into the deposition chamber. Additionally, the carrier density can also be adjusted by adjusting the surface properties of the substrate on which the amorphous light-transmitting conductive layer is deposited (surface properties of the functional layer (12) in this embodiment).

[0044] The hole mobility of the light-transmitting conductive layer (20) is μ (cm 2 / V·s), and also, the carrier density of the light-transmitting conductive layer (20) is n×10 19 cm -3 In this case, the ratio of n to μ (n / μ) is 4 or more, preferably 4.2 or more, more preferably 4.4 or more, even more preferably 5 or more, and particularly preferably 6 or more. Such a configuration is suitable for realizing a high etching rate in the light-transmitting conductive layer (20). From the perspective of achieving a high etching rate and low resistance in the light-transmitting conductive layer (20), the ratio of n to μ is, for example, 20 or less, preferably 10 or less, and more preferably less than 6.2.

[0045] Whether the light-transmitting conductive layer is crystalline can be determined, for example, as follows. First, the light-transmitting conductive layer (in the case of a transparent conductive film (X), the light-transmitting conductive layer (20) on the transparent substrate (10)) is immersed in hydrochloric acid with a concentration of 5 mass% at 20°C for 15 minutes. Next, the light-transmitting conductive layer is washed with water and then dried. Next, the resistance (inter-terminal resistance) between a pair of terminals separated by a distance of 15 mm is measured on the exposed surface of the light-transmitting conductive layer (in the case of a transparent conductive film (X), the surface opposite to the transparent substrate (10) in the light-transmitting conductive layer (20)). In this measurement, if the inter-terminal resistance is 10 kΩ or less, the light-transmitting conductive layer is crystalline.

[0046] A transparent conductive film (X) is manufactured, for example, as follows.

[0047] First, prepare a resin film (11) as shown in Fig. 2A.

[0048] Next, as shown in FIG. 2B, a functional layer (12) is formed on one side in the thickness direction (D) of the resin film (11). By forming the functional layer (12) on the resin film (11), a transparent substrate (10) is manufactured.

[0049] The functional layer (12) described above as a hard coat layer can be formed by applying a curable resin composition onto a resin film (11) to form a coating film, and then curing the coating film. If the curable resin composition contains a UV-curable resin, the coating film is cured by UV irradiation. If the curable resin composition contains a thermosetting resin, the coating film is cured by heating.

[0050] The exposed surface of the functional layer (12) formed on the resin film (11) is surface modified as needed. When plasma treatment is used as the surface modification treatment, argon gas is used as an inert gas. In addition, the discharge power in the plasma treatment is, for example, 100 W or more, and also, for example, 500 W or less.

[0051] Next, as shown in FIG. 2C, an amorphous light-transmitting conductive layer (20') is formed on a transparent substrate (10) (film formation process). Specifically, the amorphous light-transmitting conductive layer (20') is formed by forming a material on a functional layer (12) in the transparent substrate (10) by a sputtering method. The light-transmitting conductive layer (20') is an amorphous film that combines light transmittance and conductivity (the light-transmitting conductive layer (20') is converted into a crystalline light-transmitting conductive layer (20) by heating in the crystallization process described later).

[0052] In the sputtering method, it is preferable to use a sputtering device capable of performing a film deposition process in a roll-to-roll manner. In the manufacture of a transparent conductive film (X), when using a roll-to-roll sputtering device, a transparent substrate (10) in the shape of a long rod is driven from a dispensing roll to a winding roll equipped with the device, and a material is deposited on the transparent substrate (10) to form a light-transmitting conductive layer (20'). Furthermore, in the sputtering method, a sputtering device equipped with a single film deposition chamber may be used, or a sputtering device equipped with a plurality of film deposition chambers arranged in sequence along the driving path of the transparent substrate (10) may be used (in the case of forming a light-transmitting conductive layer (20') including the first layer and the second layer described above, a sputtering device equipped with two or more film deposition chambers is used).

[0053] In the sputtering method, specifically, a sputtering gas (inert gas) is introduced into the film deposition chamber under vacuum conditions, and a negative voltage is applied to a target placed on the cathode inside the film deposition chamber. This generates a glow discharge to ionize gas atoms, and the gas ions are collided with the target surface at high speed, causing the target material to be ejected from the target surface, and the ejected target material is deposited on the functional layer (12) in the transparent substrate (10).

[0054] As the material of the target placed on the cathode in the film-forming chamber, the conductive oxide described above with respect to the light-transmitting conductive layer (20) is used, preferably an indium-containing conductive oxide is used, and more preferably ITO is used. When ITO is used, the ratio of the tin oxide content to the total content of tin oxide and indium oxide in the ITO is preferably 1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, particularly preferably 7 mass% or more, and also preferably 15 mass% or less, more preferably 13 mass% or less, and even more preferably 12 mass% or less.

[0055] The sputtering method is preferably a reactive sputtering method. In the reactive sputtering method, a reactive gas is introduced into the film formation chamber in addition to the sputtering gas.

[0056] When forming a light-transmitting conductive layer (20') containing Kr across the entire thickness direction (D), the gas introduced into the film formation chamber contains Kr as a sputtering gas and oxygen as a reactive gas. The sputtering gas may contain an inert gas other than Kr. Examples of inert gases other than Kr include noble gas atoms other than Kr. Examples of noble gas atoms include Ar and Xe. When the sputtering gas contains an inert gas other than Kr, the content ratio is preferably 5 volume% or less, more preferably 3 volume% or less.

[0057] In the reactive sputtering method, the ratio of the amount of oxygen introduced to the total amount of sputtering gas and oxygen introduced into the film deposition chamber is, for example, 0.1 flow% or more, and also, for example, 5 flow% or less.

[0058] The atmospheric pressure inside the membrane chamber during the membrane formation (sputter membrane formation) by the sputtering method is, for example, 0.02 Pa or higher, and also, for example, 1 Pa or lower.

[0059] The temperature of the transparent substrate (10) during the sputtering film is, for example, 100°C or lower, preferably 50°C or lower, more preferably 30°C or lower, and also, for example, -20°C or higher, preferably -10°C or higher, more preferably -7°C or higher.

[0060] Power sources for applying voltage to the target may include, for example, DC power, AC power, MF power, and RF power. DC power and RF power may be used in combination. The discharge voltage during sputter film deposition is, for example, 200 V or higher, and also, for example, 400 V or lower.

[0061] In the present manufacturing method, next, as shown in FIG. 2D, the light-transmitting conductive layer (20) is converted from amorphous to crystalline by heating (crystallization process). For example, an infrared heater and an oven may be used as means of heating. The heating temperature is, for example, 100°C or higher, and preferably 120°C or higher, from the perspective of securing a high crystallization rate. The heating temperature is, for example, 200°C or lower, and preferably 180°C or lower, more preferably 170°C or lower, and even more preferably 165°C or lower, from the perspective of suppressing the effect of heating on the transparent substrate (10). The heating time is, for example, 6 hours or less, preferably 200 minutes or less, more preferably 150 minutes or less, and even more preferably 90 minutes or less, and also, for example, 1 minute or more, preferably 5 minutes or more.

[0062] As described above, a transparent conductive film (X) is manufactured.

[0063] The light-transmitting conductive layer (20) in the transparent conductive film (X) may be patterned as schematically shown in FIG. 3. The light-transmitting conductive layer (20) can be patterned by etching the light-transmitting conductive layer (20) through a predetermined etching mask. The patterning of the light-transmitting conductive layer (20) may be performed before the crystallization process described above, or after the crystallization process. The patterned light-transmitting conductive layer (20) functions, for example, as a wiring pattern.

[0064] As described above, the transparent conductive film (X) has a light-transmitting conductive layer (20) on a transparent substrate (10) that contains krypton and is also 2.8×10 -4 It has a resistivity of less than Ω·cm. In addition, the hole mobility of the light-transmitting conductive layer is μ (cm²). 2 Let / V·s) and also set the carrier density to n×10 19(cm -3 In the case where ), the ratio of n to μ (n / μ) is 4 or more, preferably 4.2 or more, more preferably 4.4 or more, even more preferably 5 or more, and particularly preferably 6 or more.

[0065] Such a configuration in the transparent conductive film (X) is suitable for realizing a high etching rate in the light-transmitting conductive layer (20). Specifically, it is as shown in the examples and comparative examples described below.

[0066] In the transparent conductive film (X), the functional layer (12) may be an adhesion enhancing layer for realizing high adhesion of the light-transmitting conductive layer (20) to the transparent substrate (10). A configuration in which the functional layer (12) is an adhesion enhancing layer is suitable for securing adhesion between the transparent substrate (10) and the light-transmitting conductive layer (20).

[0067] The functional layer (12) may be an index-matching layer for adjusting the reflectance of the surface (one side in the thickness direction (D)) of the transparent substrate (10). A configuration in which the functional layer (12) is an index-matching layer is suitable for making it difficult to see the pattern shape of the light-transmitting conductive layer (20) when the light-transmitting conductive layer (20) on the transparent substrate (10) is patterned.

[0068] The functional layer (12) may be a peeling functional layer that enables the light-transmitting conductive layer (20) to be practically peeled off from a transparent substrate (10). A configuration in which the functional layer (12) is a peeling functional layer is suitable for peeling off the light-transmitting conductive layer (20) from a transparent substrate (10) and transferring the light-transmitting conductive layer (20) to another component.

[0069] The functional layer (12) may be a composite layer in which a plurality of layers are connected in the thickness direction (D). The composite layer preferably comprises two or more layers selected from the group consisting of a hard coat layer, an adhesion enhancing layer, a refractive index adjusting layer, and a peeling functional layer. This configuration is suitable for complexly expressing the functions described above for each selected layer in the functional layer (12). In one preferred embodiment, the functional layer (12) is provided with the adhesion enhancing layer, the hard coat layer, and the refractive index adjusting layer in this order facing one side of the thickness direction (D) on the resin film (11). In another preferred embodiment, the functional layer (12) is provided with the peeling functional layer, the hard coat layer, and the refractive index adjusting layer in this order facing one side of the thickness direction (D) on the resin film (11).

[0070] A transparent conductive film (X) is laminated to an article and, if necessary, used in a patterned state. The transparent conductive film (X) is laminated to an article, for example, with an adhesive functional layer interposed therein.

[0071] Examples of articles include elements, components, and devices. That is, examples of articles to which a transparent conductive film is attached include elements with a transparent conductive film attached, components with a transparent conductive film attached, and devices with a transparent conductive film attached.

[0072] Examples of devices include light-diffusing devices and photoelectric conversion devices. Examples of light-diffusing devices include current-driven light-diffusing devices and electric field-driven light-diffusing devices. Examples of current-driven light-diffusing devices include electrochromic (EC) light-diffusing devices. Examples of electric field-driven light-diffusing devices include PDLC (polymer dispersed liquid crystal) light-diffusing devices, PNLC (polymer network liquid crystal) light-diffusing devices, and SPD (suspended particle device) light-diffusing devices. Examples of photoelectric conversion devices include solar cells. Examples of solar cells include organic thin-film solar cells and dye-sensitized solar cells. Examples of components include electromagnetic shielding components, heat wire control components, heater components, and antenna components. Examples of devices include touch sensor devices, lighting devices, and image display devices.

[0073] The article with the transparent conductive film attached is suitable for realizing a high etching rate in the light-transmitting conductive layer (20) of the transparent conductive film (X) it has, and is therefore suitable for realizing high manufacturing efficiency.

[0074] Examples of the adhesive functional layers described above include adhesive layers and bonding layers. As for the material of the adhesive functional layer, any material that is transparent and exhibits an adhesive function may be used without particular limitation. The adhesive functional layer is preferably formed from a resin. Examples of resins include acrylic resin, silicone resin, polyester resin, polyurethane resin, polyamide resin, polyvinyl ether resin, vinyl acetate / vinyl chloride copolymer, modified polyolefin resin, epoxy resin, fluoropolymer, natural rubber, and synthetic rubber. Acrylic resin is preferred as the resin in terms of exhibiting adhesive properties such as cohesiveness, adhesion, and appropriate wettability, having excellent transparency, and having excellent weather resistance and heat resistance.

[0075] In the fixing functional layer (resin forming the fixing functional layer), a corrosion inhibitor may be added to inhibit corrosion of the light-transmitting conductive layer (20). In the fixing functional layer (resin forming the fixing functional layer), a migration inhibitor (e.g., a material disclosed in Japanese Patent Publication No. 2015-022397) may be added to inhibit migration of the light-transmitting conductive layer (20). In addition, in the fixing functional layer (resin forming the fixing functional layer), an ultraviolet absorber may be added to inhibit deterioration of the article during outdoor use. Examples of ultraviolet absorbers include benzophenone compounds, benzotriazole compounds, salicylic acid compounds, oxalate anilide compounds, cyanoacrylate compounds, and triazine compounds.

[0076] In addition, when a transparent substrate (10) of a transparent conductive film (X) is fixed to an article via a fixing functional layer, a light-transmitting conductive layer (20) (including the light-transmitting conductive layer (20) after patterning) in the transparent conductive film (X) is exposed. In such a case, a cover layer may be placed on the exposed surface of the light-transmitting conductive layer (20). The cover layer is a layer that covers the light-transmitting conductive layer (20), and can improve the reliability of the light-transmitting conductive layer (20) and suppress functional deterioration caused by scratches on the light-transmitting conductive layer (20). Such a cover layer is preferably formed of a dielectric material, and more preferably formed of a composite material of a resin and an inorganic material. As for the resin, for example, the resin mentioned above with respect to the fixing functional layer may be cited. As for the inorganic material, for example, inorganic oxides and fluorides may be cited. Examples of inorganic oxides include silicon oxide, titanium oxide, niobium oxide, aluminum oxide, zirconium dioxide, and calcium oxide. Examples of fluorides include magnesium fluoride. In addition, the above-mentioned corrosion inhibitor, migration inhibitor, and ultraviolet absorber may be incorporated into the cover layer (a mixture of resin and inorganic material).

[0077] Examples

[0078] The present invention will be described in detail below by presenting examples. The present invention is not limited to examples. In addition, specific numerical values ​​such as the mixing amount (content), physical property value, and parameter described below may be replaced with upper limits (numerical values ​​defined as “less than” or “less than”) or lower limits (numerical values ​​defined as “greater than” or “exceeds”) of the mixing amount (content), physical property value, and parameter, etc., corresponding to those described in the “form for carrying out the invention” described above.

[0079] [Example 1]

[0080] A UV-curable resin composition containing acrylic resin was applied to one side of a long cycloolefin polymer (COP) film (product name "Zeonora", thickness 40 μm, manufactured by Zeon Co., Ltd.) as a transparent resin film to form a coating film. Next, the coating film was cured by UV irradiation to form a hard coat layer (thickness 1 μm). Next, a UV-curable resin composition (composite resin composition containing zirconia particles) for forming a refractive index adjusting layer was applied to the hard coat layer to form a coating film. Next, the coating film was cured by UV irradiation to form a refractive index adjusting layer (thickness 90 nm, refractive index 1.62) on the hard coat layer. In this way, a transparent substrate having a resin film, a hard coat layer, and a refractive index adjusting layer in this order was manufactured.

[0081] Next, an amorphous light-transmitting conductive layer with a thickness of 66 nm was formed on a hard coat layer on a transparent substrate by a reactive sputtering method (film deposition process). For the reactive sputtering method, a sputter film deposition apparatus (DC magnetron sputtering apparatus) capable of performing the film deposition process in a roll-to-roll manner was used. The conditions for sputter film deposition in this embodiment are as follows.

[0082] As the target, a sintered body of indium oxide and tin oxide (tin oxide concentration of 10 mass%) was used. A DC power source was used to apply voltage to the target. The horizontal magnetic field strength on the target was set to 90 mT. The film deposition temperature (the temperature of the transparent substrate on which the light-transmitting conductive layer is laminated) was set to 20 ℃. In addition, the achievable vacuum level in the film deposition chamber equipped with the device was 0.8 × 10⁻⁶ -4After vacuuming the deposition chamber to Pa, Kr was introduced as a sputtering gas and oxygen as a reactive gas into the deposition chamber, thereby setting the atmospheric pressure inside the chamber to 0.2 Pa. The ratio of the amount of oxygen introduced to the total amount of Kr and oxygen introduced into the deposition chamber is approximately 2 flow%, and as shown in Fig. 4, the amount of oxygen introduced falls within the region R of the resistivity-oxygen introduction curve, such that the resistivity of the formed film is 6.9 × 10⁻⁶. -4 It was adjusted to Ω·cm. The resistivity-oxygen introduction curve shown in Fig. 4 can be prepared by first investigating the dependence of the resistivity of the light-transmitting conductive layer on the amount of oxygen introduced when the light-transmitting conductive layer is formed by reactive sputtering under conditions other than the amount of oxygen introduced as above.

[0083] Next, the light-transmitting conductive layer on the transparent substrate was crystallized by heating in a hot air oven (crystallization process). In this process, the heating temperature was set to 130°C and the heating time was set to 1.5 hours.

[0084] As described above, the transparent conductive film of Example 1 was prepared. The light-transmitting conductive layer (thickness 66 nm, crystalline) of the transparent conductive film of Example 1 is composed of a single Kr-containing ITO layer.

[0085] [Examples 2, 3 and Comparative Example 1]

[0086] Each of the transparent conductive films of Examples 2, 3 and Comparative Example 1 was prepared in the same manner as the transparent conductive film of Example 1, except for the following.

[0087] In the film deposition process, the thickness of the light-transmitting conductive layer formed is 56 nm (Example 2), 41 nm (Example 3), or 43 nm (Comparative Example 1) instead of 66 nm, and the resistivity of the formed film is 6.9 × 10⁻⁶. -4 7.4×10⁻⁶ instead of Ω·cm -4Ω·cm (Example 2), 7.2×10 -4 Ω·cm (Example 3) or 7.5×10 -4 The amount of oxygen introduced was adjusted to Ω·cm (Comparative Example 1).

[0088] The light-transmitting conductive layer (crystalline) of each transparent conductive film of Examples 2, 3 and Comparative Example 1 is composed of a single Kr-containing ITO layer.

[0089] [Comparative Example 2]

[0090] A transparent conductive film of Comparative Example 2 was prepared in the same manner as the transparent conductive film of Example 1, except for the following.

[0091] In the film deposition process, Ar was used instead of Kr as the sputtering gas, the film deposition pressure was set to 0.4 Pa instead of 0.2 Pa, and the resistivity of the formed film is 6.5×10⁻⁶ -4 7.0×10⁻⁶ instead of Ω·cm -4 The amount of oxygen introduced has been adjusted to Ω·cm.

[0092] The light-transmitting conductive layer (thickness 70 nm, crystalline) of the transparent conductive film of Comparative Example 2 is composed of a single Ar-containing ITO layer.

[0093] [Comparative Example 3]

[0094] A transparent conductive film of Comparative Example 3 was prepared in the same manner as the transparent conductive film of Example 1, except for the following.

[0095] In the film deposition process, a first sputter film deposition process for forming a first layer (thickness 26 nm) on a transparent substrate and a second sputter film deposition process for forming a second layer (thickness 4 nm) on the first layer are carried out sequentially.

[0096] The conditions for the first sputter film deposition in this comparative example are as follows. A sintered body of indium oxide and tin oxide (tin oxide concentration of 10 mass%) was used as the target. A DC power source was used for applying voltage to the target. The horizontal magnetic field strength on the target was set to 90 mT. The film deposition temperature was set to 20 ℃. In addition, the achievable vacuum level in the first film deposition chamber equipped with the apparatus was 0.8 × 10⁻⁶ -4 After vacuuming the first deposition chamber until the pressure reached Pa, Ar was introduced into the first deposition chamber as a sputtering gas and oxygen as a reactive gas, and the atmospheric pressure inside the deposition chamber was set to 0.4 Pa. The amount of oxygen introduced into the deposition chamber was such that the resistivity of the formed film was 6.2 × 10⁻⁶. -4 It was adjusted to Ω·cm.

[0097] The conditions for the second sputtering film deposition in this comparative example are as follows. As the target, a sintered body of indium oxide and tin oxide (tin oxide concentration of 3 mass%) was used. The achievable vacuum level in the second film deposition chamber equipped with the apparatus is 0.8 × 10⁻⁶ -4 After vacuuming the second film-forming chamber until it reached Pa, Ar as a sputtering gas and oxygen as a reactive gas were introduced into the second film-forming chamber, and the atmospheric pressure inside the chamber was set to 0.2 Pa. In this comparative example, other conditions of the second sputter film formation are the same as those of the first sputter film formation.

[0098] The light-transmitting conductive layer (thickness 30 nm, crystalline) of the transparent conductive film of Comparative Example 3 has a first layer (thickness 26 nm) consisting of an Ar-containing ITO layer and a second layer (thickness 4 nm) consisting of an Ar-containing ITO layer in order from the transparent substrate side.

[0099] [Comparative Example 4]

[0100] A transparent conductive film of Comparative Example 4 was prepared in the same manner as the transparent conductive film of Example 1, except for the following.

[0101] In the film deposition process, Ar was used instead of Kr as the sputtering gas, and the resistivity of the formed film is 6.5 × 10⁻⁶ -4 Instead of Ω·cm, 3.1×10 -4 The amount of oxygen introduced is adjusted to Ω·cm, and the thickness of the formed light-transmitting conductive layer is 83 nm instead of 66 nm.

[0102] The light-transmitting conductive layer (thickness 83 nm, crystalline) of the transparent conductive film of Comparative Example 4 is composed of a single Ar-containing ITO layer.

[0103] <Thickness of the light-transmitting conductive layer>

[0104] The thickness of the light-transmitting conductive layer in each transparent conductive film of Examples 1 to 3 and Comparative Examples 1 to 4 was measured by FE-TEM observation. Specifically, first, samples for cross-sectional observation of each light-transmitting conductive layer in Examples 1 to 3 and Comparative Examples 1 to 4 were prepared by the FIB microsampling method. For the FIB microsampling method, a FIB device (product name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the thickness of the light-transmitting conductive layer in the cross-sectional observation samples was measured by FE-TEM observation. For FE-TEM observation, a FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.

[0105] The thickness of the first layer of the light-transmitting conductive layer in Comparative Example 3 was measured by preparing a sample for cross-sectional observation from an intermediate product before forming the second layer on the first layer, and by observing the sample using FE-TEM. The thickness of the second layer of the light-transmitting conductive layer in Comparative Example 3 was obtained by subtracting the thickness of the first layer from the total thickness of the light-transmitting conductive layer in Comparative Example 3.

[0106] Resistivity

[0107] For each transparent conductive film of Examples 1 to 3 and Comparative Examples 1 to 4, the resistivity of the light-transmitting conductive layer was investigated. Specifically, the surface resistance of the light-transmitting conductive layer was measured by the four-terminal method in accordance with JIS K 7194 (1994), and the resistivity (Ω·cm) was calculated by multiplying the surface resistance value by the thickness of the light-transmitting conductive layer. The results are shown in Table 1.

[0108] <Hole Mobility and Carrier Density>

[0109] For each transparent conductive film of Examples 1 to 3 and Comparative Examples 1 to 4, the hole mobility and carrier density of the light-transmitting conductive layer were measured. A Hall effect measurement system (product name "HL5500PC", manufactured by Bio-Rad) was used for these measurements. The hole mobility μ (cm²) obtained from these measurements 2 / V·s) and carrier density n×10 19 (cm -3 The values ​​of ) are shown in Table 1. In addition, Table 1 also shows the ratio of n to μ (n / μ).

[0110] <Etching Speed>

[0111] For each transparent conductive film of Examples 1 to 3 and Comparative Examples 1 to 4, the etching rate of the light-transmitting conductive layer was investigated. Specifically, for the transparent conductive film, one cycle was repeated in which the following first step, second step, and third step were performed in this order (in the third step, one cycle was repeated until it was determined that the etching was completed based on the criteria described below).

[0112] In the first step, the transparent conductive film was immersed in hydrochloric acid with a concentration of 7 mass%. The immersion temperature was set to 35°C. The immersion time was set to 15 seconds. In the second step, the transparent conductive film was washed with water and subsequently dried. In the third step, the resistance between a pair of terminals separated by a distance of 15 mm (inter-terminal resistance) was measured on the exposed surface of the light-transmitting conductive layer of the transparent conductive film using a surface resistance tester. If the measured inter-terminal resistance exceeded 50 kΩ or was impossible to measure, it was determined that etching was completed in the first step of the cycle to which the third step belonged. The etching rate (seconds / nm) was calculated by dividing the cumulative immersion time (etching time) of multiple first steps over multiple cycles by the thickness of the light-transmitting conductive layer. The values ​​are shown in Table 1.

[0113] <Confirmation of Kr atoms in the light-transmitting conductive layer>

[0114] It was confirmed as follows that each transparent conductive layer in Examples 1 to 3 and Comparative Example 1 contains Kr atoms. First, using a scanning fluorescence X-ray analyzer (product name "ZSX Primus IV", manufactured by Rigaku Co., Ltd.), fluorescence X-ray analysis measurements were repeated five times under the following measurement conditions, and the average value of each scanning angle was calculated to create an X-ray spectrum. In the created X-ray spectrum, it was confirmed that the light-transmitting conductive layer contains Kr atoms by confirming that a peak appears near a scanning angle of 28.2°.

[0115] <Measurement Conditions>

[0116] Spectrum ; Kr-KA

[0117] Measured diameter: 30 mm

[0118] Atmosphere: Vacuum

[0119] Target: Rh

[0120] Tube voltage: 50 kV

[0121] Tube current: 60 mA

[0122] Primary filter: Ni40

[0123] Scan angle (deg): 27.0 ~ 29.5

[0124] Step (deg): 0.020

[0125] Speed ​​(deg / min): 0.75

[0126] Attenuator : 1 / 1

[0127] Slit : S2

[0128] Spectroscopic crystal: LiF (200)

[0129] Detector: SC

[0130] PHA : 100-300

[0131]

[0132] [evaluation]

[0133] In each of the transparent conductive films of Examples 1 to 3, the light-transmitting conductive layer contains Kr, and the value of n / μ described above in the light-transmitting conductive layer is 4 or higher. In each of the transparent conductive films of Examples 1 to 3, a higher etching rate in the light-transmitting conductive layer is realized compared to the transparent conductive film of Comparative Example 1 (where the value of n / μ is less than 4) and each of the transparent conductive films of Comparative Examples 2 to 4 (where the light-transmitting conductive layer does not contain Kr).

[0134] In addition, each transparent conductive film of Examples 1 to 3 (the light-transmitting conductive layer contains Kr) has a lower resistivity of the light-transmitting conductive layer than each transparent conductive film of Comparative Examples 2 to 4 (the light-transmitting conductive layer does not contain Kr). Each transparent conductive film of Examples 2 and 3 (the light-transmitting conductive layer contains Kr, and also the value of n / μ is 4 or higher) has a particularly low resistivity of the light-transmitting conductive layer and is lower than that of the transparent conductive film of Comparative Example 1 (the light-transmitting conductive layer contains Kr, but the value of n / μ is less than 4).

[0135] Industrial applicability

[0136] The transparent conductive film of the present invention can be used as a supply material for a conductive film for patterning a transparent electrode in various devices, such as, for example, a liquid crystal display, a touch panel, and a light sensor. Explanation of the symbols

[0137] X : Transparent conductive film D: Thickness direction 10 : Transparent material 11: Resin film 12: Functional layer 20: Light-transmitting conductive layer

Claims

Claim 1 A transparent substrate and a light-transmitting conductive layer are provided in this order in the thickness direction, and the light-transmitting conductive layer is crystalline, contains krypton, and has a thickness of 2.8 × 10⁻⁶ -4 The light-transmitting conductive layer has a resistivity of less than Ω·cm, and the light-transmitting conductive layer has a hole mobility μ (cm²). 2 / V·s) and carrier density n×10 19 (cm -3 A transparent conductive film having ) and a ratio of n to μ of 4.4 or greater and 20 or less. Claim 2 In claim 1, the light-transmitting conductive layer comprises a transparent conductive film containing an indium-containing conductive oxide. Claim 3 In claim 1 or 2, the hole mobility is 5 cm 2 / V·s or more 40 cm 2 Transparent conductive film with / V·s or less. Claim 4 In claim 1 or 2, the carrier density is 100×10 19 cm -3 170×10 19 cm -3 Lee Ha-in, transparent conductive film. Claim 5 A transparent conductive film according to claim 1 or 2, wherein the light-transmitting conductive layer is patterned. Claim 6 In claim 1 or 2, the light-transmitting conductive layer is 2.2×10 -4 A transparent conductive film having a resistivity of less than Ω·cm.

Citation Information

Patent Citations

  • Transparent conductive film and method for producing same

    KR1020170008196A

  • Transparent conductive film and manufacturing method therefor

    US20130280554A1

  • Organic light-emitting device

    WO2016088378A1

  • Manufacture of transparent conductive film

    JP1993334924A