Separator for Zinc Rechargeable Batteries
A PAN nanofiber mat impregnated with gelatin enhances the performance of zinc secondary batteries by improving porosity and mechanical strength, addressing the limitations of aqueous electrolytes and enhancing lifespan and discharge capacity.
Patent Information
- Application Number
- KR1020240174106
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-11-29
- Filing Date
- 2024-11-28
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-11-28
AI Technical Summary
The lifespan, energy density, and practical universality of zinc secondary batteries are limited by the narrow electrochemical stable potential window of aqueous electrolytes, leading to water consumption and potential explosion risks, as well as corrosion and Zn dendrite formation.
A separator for zinc secondary batteries is developed using a polyacrylonitrile (PAN) nanofiber mat impregnated with gelatin, manufactured through electrospinning, to enhance porosity, breathability, and mechanical strength.
The separator improves lifespan and discharge capacity retention, addressing the limitations of aqueous electrolytes by maintaining ionic conductivity and preventing water consumption and corrosion.
Smart Images

Figure 112024132091679-PAT00026_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a separator for a zinc secondary battery. Background Technology
[0002] Aqueous zinc-ion rechargeable batteries can fundamentally resolve the risks of fire and explosion, enable low-cost implementation, and have low toxicity, leading to active research and development for their application as energy storage rechargeable batteries. The fabrication of zinc-ion rechargeable batteries utilizes zinc metal as the negative electrode active material and manganese dioxide as the positive electrode active material; this system leverages the oxidation / reduction reaction between zinc metal and zinc ions at the negative electrode, and the oxidation / reduction reaction of manganese through the insertion / extraction of zinc ions and hydrogen ions at the positive electrode.
[0003] The problem with zinc secondary batteries (ZIB) is that their lifespan, energy density, and practical universality are limited by the narrow electrochemical stable potential window of water in the aqueous electrolyte, and the theoretical window voltage is only 1.23 V.
[0004] Theoretically, if the anode reaction potential energy level is higher than the lowest unoccupied molecular orbital of the aqueous solvent, water molecules are easily reduced to produce hydrogen molecules through the hydrogen evolution reaction (HER); conversely, if the cathode reaction potential energy level is lower than the highest unoccupied molecular orbital of the aqueous solvent, oxygen molecules are produced through the oxygen evolution reaction (OER). Since these two reactions consume water from the electrolyte, they increase the electrolyte concentration and decrease the ionic conductivity of the electrolyte; furthermore, there is a risk of explosion if hydrogen and oxygen are simultaneously released from the ZIB during charging.
[0005] Meanwhile, if the pH value decreases locally, corrosion occurs on zinc surfaces that are highly reactive with water, and if the electrolyte dissolves on the irregular zinc surface, Zn dendrite is also formed.
[0006] Therefore, host design, coating medification, uniform Zn electrodeposition, and the structural configuration of the anode must be reviewed. The essential components of the aqueous electrolyte are six water molecules and Zn that interact strongly. 2+ Coordination structures exist between ions, and numerous hydrogen bonds are formed between water molecules. As such, zinc coordination structure and hydrogen bonds, which are two important indicators affecting battery performance, can be reconfigured by changing the electrolyte, such as by changing the anion, using a high-concentration electrolyte, or using an organic solvent.
[0007] Therefore, the present invention aims to provide a high-performance zinc secondary battery (ZIB) by developing an electrolyte membrane that serves as the basis for such an electrolyte modification. The problem to be solved
[0008] In this invention, an electrolytic membrane having excellent porosity and breathability and excellent mechanical strength is manufactured using an electrospinning machine. means of solving the problem
[0009] The present invention provides a method for manufacturing a separator for a zinc secondary battery, comprising the steps of: manufacturing a polyacrylonitrile (PAN) nanofiber mat by electrospinning; and impregnating the polyacrylonitrile (PAN) nanofiber mat with a gelatin solution and drying it to manufacture a polyacrylonitrile (PAN) nanofiber mat containing gelatin.
[0010] In addition, the present invention provides a separator for a zinc secondary battery manufactured by the above manufacturing method.
[0011] In addition, the present invention provides a zinc secondary battery comprising the above-mentioned separator. Effects of the invention
[0012] According to the present invention, a separator for a zinc secondary battery can be provided that has excellent porosity and breathability and high mechanical strength, resulting in excellent lifespan characteristics and discharge capacity maintenance characteristics.
[0013] In addition, the present invention can provide a zinc secondary battery having excellent lifespan characteristics and discharge capacity retention characteristics including the separator. Brief explanation of the drawing
[0014] Figure 1 is a photograph of an early electrosprayer. Figure 2 is a photograph of the shape of the radiated material. Figure 3 is a photograph showing the radiation shape according to the radiation speed (left: radiation speed 1.5 ml / hr, right: radiation speed 1.2 ml / hr). Figure 4 is a photograph of the electrospinning condition experiment process (1: Fiber emerging stably from the syringe, 2: Fiber when electrospinning is not working well). Figure 5 is a photograph of a drum-type collector. Figure 6 is a photograph of a syringe holder and a controller. Figure 7 is a photograph of the drum collector and controller. Figure 8 is a photograph of the electrospinning device of the present invention. FIG. 9 is a photograph of an electrospinning device capable of adjusting the width of the present invention to a constant level. Figure 10 is a photograph of the PAN manufacturing process. Figure 11 is a photograph showing the shape of electrospinning according to a change in spinning speed (1: spinning speed 2.1 ml / hr, 2: spinning speed 1.4 ml / hr). Figure 12 is a photograph taken when the radiation rate is 1.45 ml / hr. Figure 13 is a photograph of the shape when the radiation spacing is changed. Figure 14 is a photograph showing the process of an electrospinning condition experiment as the ambient temperature rises. Figure 15 is a photograph of an electrolytic film made of PAN. Figure 16 is a photograph of the PAN electrospinning process in the electrospinning machine of the present invention. Figure 17 is a photograph of a PAN attached to aluminum foil. Figure 18 is a photograph showing the process of a PAN electrolytic film peeling experiment using fiber foil. Figure 19 is a photograph showing the shape of PAN fibers according to changes in collector drum speed. Figure 20 is a photograph of the gelatin manufacturing process. Figure 21 is a photograph of gelatin-impregnated PAN. Figure 22 is a photograph of PAN containing gelatin. Figure 23 is an SEM structure of PAN when impregnated with gelatin (1: PAN before gelatin content, 2: PAN with high gelatin content, 3: PAN with moderate gelatin content) Figure 24 shows the appearance of gelatin-containing PAN when the PAN thickness is varied (Left: when the PAN thickness is thick, Middle: when the PAN thickness is moderate, Right: when the PAN thickness is too thin). Figure 25 shows the cycle life of a cell using a water-soluble electrolyte and a polymer prepared in the present invention. Specific details for implementing the invention
[0015] The present invention will be described in detail below.
[0017] The present invention provides a method for manufacturing a separator for a zinc secondary battery, comprising the steps of: manufacturing a polyacrylonitrile (PAN) nanofiber mat by electrospinning; and impregnating the polyacrylonitrile (PAN) nanofiber mat with a gelatin solution and drying it to manufacture a polyacrylonitrile (PAN) nanofiber mat containing gelatin.
[0018] In one embodiment of the present invention, the gelatin solution may be prepared by mixing and stirring gelatin, potassium persulfate, zinc sulfate, manganese sulfate, and distilled water, and then adding acrylamide and N,N' methylenebisacrylamine in portions.
[0019] In one embodiment of the present invention, the electrospinning may be performed by an electrospinning machine comprising: a syringe portion; a syringe holder that supports the syringe portion and allows free movement in the left-right and forward-backward directions; a regulator connected to the syringe portion to control the amount of solution emitted; and a drum collector that controls the rotational speed.
[0020] The amount of gelatin contained in the above PAN may be 50% to 120% of the weight of the PAN. When gelatin is contained in the PAN within the above range, as shown in FIG. 23, a suitable amount of gelatin exists between the PAN fibers, allowing sufficient pores to be formed.
[0021] The thickness of the PAN may be 50㎛ to 500㎛. As shown in FIG. 24, if the thickness of the PAN exceeds the above range, swelling may occur after drying, and if it is below the above range, the amount of gelatin is relatively too high, so a gelatin film may be formed that completely blocks the pores of the PAN fibers.
[0022] In addition, the present invention provides a separator for a zinc secondary battery manufactured by the above manufacturing method.
[0023] In addition, the present invention provides a zinc secondary battery comprising the above-mentioned separator.
[0025] Hereinafter, the structure of the present invention and the resulting effects are to be explained in more detail through specific embodiments and comparative examples. However, these embodiments are intended to explain the present invention more specifically, and the scope of the present invention is not limited to these embodiments.
[0027] <Example>
[0028] Example 1. Manufacture of an electrospinning machine
[0029] Early electrospinning machines were produced by electrospinning onto a plate-shaped collector, and the extruded sample was made into a shape resembling a cotton ball as shown in Fig. 1, making it difficult to use.
[0030] Therefore, by fabricating a drum-type collector as shown in Fig. 5, it was possible to produce a plate-type sample with the shape shown in Fig. 3, but the width could not be controlled as in Fig. 5, and thus it is a one-time production without any aspect.
[0031] Therefore, the syringe and collector parts were newly manufactured, and mass production feasibility was examined.
[0032] First, to ensure the stability and accurate width of the syringe section, a syringe holder device as shown in Fig. 6 was installed on the syringe section to allow for free movement in the left-right and front-back directions, and a regulator was newly attached to control the amount of solution emitted from the syringe.
[0033] In addition, as shown in Fig. 7, a device capable of controlling the rotational speed by attaching a regulator to the drum collector was also developed and attached.
[0034] The electrospinning device manufactured by combining the newly configured devices as described above is as shown in FIG. 8.
[0035] The above electrospinning machine can independently control the syringe part and the drum collector part, and can move the syringe back and forth to control the width of the electrospinning, and can smoothly control the rotation and reciprocating motion of the drum collector, and thus the shape of the spun material can be controlled in width as shown in FIG. 9.
[0036] That is, the electrospinning device of the present invention can adjust the width to a constant level.
[0038] Example 2. Fabrication of a PAN nanofiber mat by electrospinning
[0039] Conventional electrolytes were made of glass wool, but electrolytes using polymers have high mechanical strength, are easy to fabricate as thin films, and have excellent contact ability with electrodes and electrolytes. However, since general polymers have low ionic conductivity, the present invention fabricated an electrolyte capable of having ionic conductivity.
[0040] Looking at the characteristics of some polymers, it can be seen that they have high ionic conductivity, as shown in Table 1 below.
[0041]
[0043] Production of electrospinning PANs
[0044] 200ml of DMF was added to 20g of PAN, heated to 70℃ in a double-jacketed stirrer, stirred at 200rpm until no air bubbles were removed, and then refrigerated.
[0045] Electrospinning conditions experiment of PAN
[0046] Electrospinning was performed under conditions such as a syringe volume of 10 ml, a voltage of 12 to 15 kV, a distance of 10 to 20 cm between the collector and the syringe, and a spinning rate of 0.5 to 2.0 ml / hr or higher.
[0047] Experiments were conducted with the distance between the collector and the syringe fixed at 15 cm and the voltage at 1.49 kV, while changing the emission rate to 2.1 and 1.4 ml / hr. As shown in Fig. 11, different appearances were observed. When the emission rate was set to 2.1 ml / hr as shown in Fig. 11, the emission pattern appeared constant, and the emission width was maintained in a narrow shape. However, when the emission rate was lowered to 1.4 ml / hr, the emission pattern became unstable. As shown in 2-1 and 2-2 of Fig. 11, the Taylor cone shape, which is the form of the solution in front of the syringe, gradually lengthened. In cases where it stretched out and attached to the collector in the form of a bead, as shown in 2-2 of Fig. 11, it occurred.
[0048] PAN is manufactured for use as an electrolytic membrane, and it is desirable to have a wide width and a uniform thickness. In the case of 1-1 and 1-2 of Fig. 11, the spinning pattern is uniform but the width appears narrow. In the case of 2-1, 2-2, and 2-3 of Fig. 11, the spinning width is wide and good, but since wide beads are attached, it was difficult to manufacture an electrolytic membrane with a uniform thickness and uniform fibers.
[0049] When the electrospinning was performed with the emission distance fixed at 15 cm, the emission voltage at 14.0 kV, and the emission rate at 1.45 ml / hr, the shape of the emitted solution was larger than that of case 1-1 in Fig. 11, but smaller than that of cases 2-1 and 2-2 in Fig. 11. The shape of the emitted Taylor cone was formed as shown in Fig. 12, and the emission width was slightly wider than that of case 1-2 in Fig. 11, but much smaller than that of case 2-3.
[0050] The shape of the Taylor cone in Fig. 12 is a diagram of the initial spinning of the spinning solution (Fig. 12-1) and the final spinning (Fig. 12-3).
[0051] Figure 13 shows the shape when the electrospinning conditions are changed to voltage 15.5 kV, spinning speed 1.0 ml / hr, and spacing 10 cm (Figure 13, 1) and 15 cm (Figure 13, 2).
[0052] As shown in Fig. 13, when the voltage was increased to 15.5 kV, it was better to lower the radiation speed compared to the previous example and set the distance to 15 cm.
[0053] As shown in Figure 14, an experiment on electrospinning conditions was conducted as the ambient temperature increased. To investigate the effect of temperature as the ambient temperature rose to 27℃, the effect of temperature was observed when the radiation shape and the radiation distance at which constant radiation occurred were set to 15cm, the radiation voltage to 14.0kV, and the radiation rate to 1.45ml / hr.
[0054] First, during the preparation of the PAN solution, as the ambient temperature increased, a phenomenon occurred in which dissolution did not occur well, as shown in Figure 14.
[0055] If the solution is not completely dissolved in DMF, the dissolved solution passes through the needle tip during the initial electrospinning, so spinning occurs well as shown in 2-1 of Fig. 14. However, as time progresses, the Taylor cone gradually enlarges as shown in 1-2 of Fig. 14, and as time progresses, it hardens at the needle tip as shown in 3-1 of Fig. 14, resulting in a phenomenon where spinning does not occur as shown in 3-2 of Fig. 14. Therefore, it can be seen that when the weather is hot and the ambient temperature rises, the influence of the ambient temperature must also be considered in addition to the influence of humidity mentioned earlier.
[0056] A high-quality electrolytic film was fabricated by considering the above conditions, such as voltage, radiation rate, ambient temperature, and radiation distance.
[0057] Although varying slightly depending on the ambient temperature, 18 ml of PAN solution was prepared in a 150 x 300 mm area twice under conditions of voltage of 14.7–15 kV, radiation rate of 1.69–1.96 ml / hr, radiation distance of 15 cm, ambient temperature of 26–27℃, and humidity of 50–60% (Fig. 15).
[0058] PAN production in the newly manufactured electrospinning machine
[0059] Electrospinning of a PAN solution was performed under spinning conditions: voltage 14.7 kV, spinning speed 1.8 ml / hr, spinning distance 15 cm, and spinner ambient temperature 26.7 ℃.
[0060] As shown in Fig. 16, it was observed that electrospinning proceeded well to a uniform thickness, but the PAN electrolytic film collected using aluminum foil on the collector drum for PAN recovery could not be peeled off well because the PAN was attached to the aluminum foil as shown in Fig. 17.
[0061] Since it is difficult to peel off a uniformly produced PAN film from the attached foil, an experiment was conducted to purchase a new foil so that it could be easily peeled off.
[0062] This foil is made of fiber, and as a result of conducting an experiment using this fiber foil, peeling was easily possible as shown in Fig. 18.
[0063] The left side of Fig. 18 shows fiber foil being applied to the collector drum, the middle image shows the electrospinning of PAN after the fiber foil is attached, the top right shows the peeling of PAN from aluminum foil, and the bottom right shows the peeling from fiber foil. As shown in the figures above, it was found that when fiber foil is used, the peeling is completely successful.
[0064] Another variable in the spinning conditions is the change in speed of the drum collector. In the present invention, PAN fiber formation was measured according to two speed changes: 180 rpm and 1050 rpm.
[0065] Figure 19 shows the shape when the speed of the collector drum is changed, and it was found that the width is wider and the radiation is smoother when the speed is faster than when it is slow.
[0066] When the speed is too slow, the shape of the extruded surface is relatively rough and the width is small, and when the speed is too fast, it is too dense and compact, which seems to cause problems in accommodating the electrolyte, so when producing PAN fibers with a new electrospinning machine, the speed was set to 500 rpm.
[0067] Since the electrolytic membrane prepared above used PAN dissolved in DMF as the electrospinning solution, the added DMF was removed by drying it in a vacuum dryer at a vacuum level of 0.1 MPa, 60°C, for 6 hours.
[0068] Example 3. Fabrication of a gelatin-containing PAN nanofiber mat
[0069] PAN electrolytic membrane treatment
[0070] In order to use PAN as an electrolyte membrane, ion conduction must be achieved, so gelatin must be prepared and infiltrated into the PAN membrane, and an electrolyte solution must be poured into it to facilitate the movement of electrons.
[0071] gelatin manufacturing
[0072] In order to generate ionic conductivity while dissolving gelatin, potassium persulfate, zinc sulfate, manganese sulfate, etc. must be added to the gelatin and then prepared as a solution.
[0073] 10g of gelatin, 0.075g of potassium persulfate, 5ml / 100ml of 2M ZnSO4 (DI water), 1.51g of MnSO4, and 200ml of DI water were placed in a double-jacketed container and stirred at 80℃ for 1 hour, then lowered to 40℃, and then 15g of acrylamide and 15mg of N,N' methylenebisacrylamine were added in portions to prepare the mixture.
[0074] Figure 20 shows the process of preparing a gelatin solution, where 1 in Figure 20 shows undissolved gelatin particles at the beginning of preparation, and indicates that the gelatin particles have completely dissolved over time.
[0075] Figure 21 is a diagram showing the process of impregnating with gelatin. When PAN is placed in a mold and then dried after impregnating with gelatin, gelatin-impregnated PAN is produced as shown in the figure. The gelatin-containing PAN was cut into a certain size as shown in Figure 22, and the degree of impregnation was measured.
[0076] Amount of gelatin in PAN [Unit: g / cm²] Before injection After injection 0.0039 0.008156 0.004593 0.009706 0.004594 0.01047 0.007288 0.01896 0.0073556 0.02235 0.0076 0.02935 0.007663 0.02423 0.007713 0.02459
[0078] Table 2 summarizes the experimental results to determine how the amount of gelatin injected changes depending on the shape or thickness of the PAN through the weight ratio before and after gelatin injection. In the case of the same thickness, the amount of gelatin was almost the same, indicating no quantitative change in gelatin. Changes in the tissue before and after gelatin injection were observed and are shown in Figure 23.
[0079] Figure 23 is an SEM image of PAN containing gelatin. Figure 23-1 shows the image when no gelatin is contained, which shows that sufficient pores are formed between the PAN fibers because no gelatin is contained. Figure 23-2 shows that there are almost no pores because the gelatin is excessive and covers the PAN fibers. Figure 23-3 shows that there is an appropriate amount of gelatin in the PAN, which forms sufficient pores.
[0080] The thickness of the PAN also affects the gelatin impregnated with it, as shown in Fig. 24. If the PAN thickness is too thick, swelling occurs after drying, and if it is too thin, the amount of gelatin is relatively too large, so a gelatin film is formed that can completely block the pores of the PAN fibers.
[0081] Example 4. Coin cell fabrication and measurement
[0082] - CR2032 Coin cell
[0083] - Electrolyte: 3 M Zn(CF3SO3)2
[0084] - Anode: NVO
[0085] - Cathode: 0.05 mm (t) Zn foil
[0086] - Electrolyte: The gelatin-containing PAN nanofiber mat prepared in Example 3 was used as the electrolyte.
[0087] <Condition>
[0088] - Battery cycler: WBCS 3000 L; WonATech
[0089] - Voltage range: 0.2 - 1.8 V
[0090] - Temperature: 30 ℃
[0091] <Result>
[0092] Figure 25 shows the cycle life of a cell using a water-soluble electrolyte and the polymer developed in this patent.
[0093] A cycle performance test was conducted at a current density of 1Ag-1.
[0094] The cell using water-soluble electrolytes showed a capacity retention rate of 50% or less at 1000th, and at 1400th, the cell was no longer functioning normally.
[0095] On the other hand, the cell produced in the present invention showed a high capacity retention rate of 73.59% even at 2000th.
Claims
Claim 1 A method for manufacturing a separator for a zinc secondary battery, comprising: a step of manufacturing a polyacrylonitrile (PAN) nanofiber mat by electrospinning; and a step of manufacturing a polyacrylonitrile (PAN) nanofiber mat containing gelatin by impregnating the polyacrylonitrile (PAN) nanofiber mat with a gelatin solution and drying it; wherein the gelatin solution is prepared by mixing and stirring gelatin, potassium persulfate, zinc sulfate, manganese sulfate, and distilled water, and then adding acrylamide and N,N' methylenebisacrylamine in portions. Claim 2 delete Claim 3 A method for manufacturing a separator for a zinc secondary battery according to claim 1, wherein the amount of gelatin contained in the PAN is 50% to 120% of the weight of the PAN. Claim 4 A method for manufacturing a separator for a zinc secondary battery according to claim 1, wherein the thickness of the PAN is 50㎛ to 500㎛. Claim 5 A method for manufacturing a separator for a zinc secondary battery according to claim 1, wherein the electrospinning is performed by an electrospinning machine comprising: a syringe part; a syringe holder that supports the syringe part and allows free movement in the left-right and front-back directions; a regulator connected to the syringe part to control the amount of solution emitted; and a drum collector that controls the rotational speed. Claim 6 A separator for a zinc secondary battery manufactured by the method of any one of claims 1, and 3 to 5. Claim 7 A zinc secondary battery comprising the separator of claim 6.
Citation Information
Patent Citations
Battery electrolyte and manufacturing method for the same
KR1020210087845A
Electrospun nanofibrous membrane and producing method therefor
KR102237839B1
Electrospun composite separator for electrochemical devices and applications of same
US20200220219A1
Electrospun composite separator for electrochemical devices and applications of same
WO2020191003A1
Ionic conductive materials for electrochemical generators and methods for producing the same
KR1020190039949A