Coating composition for steel structure and method of using the same

An integrated epoxy-based paint composition for steel coatings addresses the inefficiencies of sequential application by combining intermediate and primer functions, ensuring adhesion and shielding while reducing construction time and costs.

KR103045480B1Active Publication Date: 2026-11-104M CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020260104966
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2026-06-09
Publication Date
2026-11-10
Estimated Expiration
2046-06-09

AI Technical Summary

Technical Problem

Conventional steel coating systems require sequential application of primer, intermediate, and top coats, which are time-consuming and costly, necessitating a new painting method and composition that integrates the intermediate and primer functions into a single layer.

Method used

A low-intermediate integrated epoxy-based paint composition comprising difunctional bisphenol A type epoxy resin, polyfunctional epoxy novolak resin, epoxy functional silane oligomer, reactive diluent, and organic solvent, applied directly to the steel surface without a separate primer layer, forming a thick film with adhesion and shielding properties.

Benefits of technology

The composition maintains film thickness and shielding properties while providing direct adhesion to steel, reducing construction time and material usage by eliminating the need for a separate primer layer, and enhancing corrosion resistance, adhesion, water resistance, and weather resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112026070103441-PAT00001_ABST
    Figure 112026070103441-PAT00001_ABST
Patent Text Reader

Abstract

The present disclosure provides a steel coating composition comprising a main component comprising a difunctional bisphenol A type epoxy resin, a polyfunctional epoxy novolak resin, an epoxy functional silane oligomer, a reactive diluent, and an organic solvent, and a coating method using the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to a composition for coating steel and a coating method using the same. Background Technology

[0002] For steel structures such as bridges, offshore structures, and plant facilities, a coating system using anti-corrosion paint is generally applied to inhibit corrosion and ensure the durability of the structure. Conventional steel coating systems mainly adopt a 3-coating system consisting of a primer layer applied directly to the steel surface to provide adhesion and initial anti-corrosion properties, an intermediate layer to provide thick film shielding and water resistance, and a top layer to provide weather resistance and exterior protection.

[0003] However, the method of applying primer, intermediate, and top coats sequentially has limitations in that the application and drying of each film require significant construction time and cost, thus necessitating the design of a new painting method and paint composition. The problem to be solved

[0004] The present disclosure aims to provide a lower-intermediate integrated epoxy-based paint composition that can be applied directly to the surface of steel without forming a separate lower layer, and can provide both the thick film shielding properties of the intermediate layer and the direct adhesion properties of the lower layer to the steel, as well as a painting method using the same.

[0005] The problems that this disclosure aims to solve are not limited to those described above, and other unmentioned problems will be clearly understood by a person skilled in the art from the description below. means of solving the problem

[0006] One embodiment of the present disclosure may provide a composition for coating steel comprising a main component comprising a difunctional bisphenol A type epoxy resin, a polyfunctional epoxy novolak resin, an epoxy functional silane oligomer, a reactive diluent, and an organic solvent.

[0007] In some embodiments, the epoxy functional silane oligomer may include a structural unit represented by the following chemical formula 1.

[0008] [Chemical Formula 1]

[0009] X-[Si(R 1 )(OR 2 )-O]n-Si(R 3 )(OR 4 )-Y

[0010] (In Chemical Formula 1, R 1 and R 3 Each is independently a C1 to C6 alkyl group or a C1 to C6 alkoxy group, R2 and R4 are each independently a C1 to C4 alkyl group, at least one of X and Y is an organic group comprising an epoxy group, a glycidoxy group, or an epoxycycloalkyl group, and n is an integer from 1 to 20)

[0011] In some embodiments, the content of the epoxy functional silane oligomer may be 0.1% to 5.0% by weight based on the total weight of the main component.

[0012] In some embodiments, the reactive diluent may include an aliphatic glycidyl ether-based reactive diluent.

[0013] One embodiment of the present disclosure may provide a method for coating steel, comprising preparing a steel surface, applying a first composition to the steel surface to form a first coating film, and applying a second composition to the first coating film to form a second coating film, wherein applying the first composition comprises mixing a main component and a curing agent component comprising a difunctional bisphenol A type epoxy resin, a polyfunctional epoxy novolak resin, an epoxy functional silane oligomer, a reactive diluent, and an organic solvent, and applying the mixture directly onto the steel surface. Effects of the invention

[0014] The first integrated low-to-mid-coat epoxy-based composition according to the present disclosure can maintain the film thickness and shielding properties of existing high-solids epoxy-based intermediate materials, while supplementing direct adhesion to the steel surface through a combination of epoxy-functional silane oligomers and polyfunctional epoxy novolak resins. Furthermore, since the first composition according to the present disclosure uses a low content of epoxy-functional silane oligomers, it can suppress the deterioration of storage stability with increasing content of silane-based components and mitigate the increase in viscosity or degradation of function during storage compared to the case where monomeric silanes are used.

[0015] The two-coating paint system according to the present disclosure can secure corrosion resistance, adhesion, water resistance, weather resistance, and appearance of steel structures with a two-coating system of a first composition and a second composition without applying a separate primer layer, thereby reducing the construction period and material usage. Brief explanation of the drawing

[0016] FIG. 1 is a flowchart for explaining a coating method using a steel coating composition according to one embodiment of the present disclosure. Specific details for implementing the invention

[0017] Hereinafter, exemplary embodiments according to the present invention will be described in detail. However, the present invention is not limited or restricted by the exemplary embodiments. Unless otherwise specifically defined, terms used herein may be used in the sense generally understood by a person skilled in the art to which the present invention pertains.

[0018] In this specification, when a part is described as “comprising” a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components. Furthermore, the singular form used in this specification includes the plural form unless specifically stated otherwise.

[0019] In this specification, the term “integrated undercoat and intermediate coat type” may mean that the undercoat and intermediate coat are not formed as separate application steps, but rather that a single coating film can provide direct adhesion to the steel surface, initial corrosion resistance, thick film shielding, and mechanical protection. However, this is not limited to the meaning that the undercoat area and the intermediate coat area are clearly separated within the coating film.

[0020] In this specification, “direct application to steel” or “Direct-To-Metal (DTM)” may mean that a paint composition can be applied directly to a steel surface, for example, a steel surface that has been blasted, ground, washed, or degreased, without a separate primer layer.

[0021] In this specification, “thick film” or “thick film” may mean that the dry film thickness can be formed to about 100 μm or more by a single application.

[0022] In this specification, “VOC content” may refer to the volatile organic compound content of a paint composition, and may be measured, for example, by KS M ISO 11890-2 or a method equivalent thereto.

[0023] Hereinafter, each component of the first composition and the second composition of the present disclosure will be described.

[0024] According to exemplary embodiments, the first composition may be a low-to-medium integrated paint composition applied directly to the surface of a steel material. The first composition may be a two-component composition comprising a main component and a hardener component. In this specification, a “two-component” composition may refer to a composition comprising a first component and a second component that are stored separately in distinct containers during the storage or distribution stage, and wherein the first component and the second component are mixed and applied or cured during the use stage. For example, the two-component composition may be applied by mixing the main component and the hardener component at a predetermined mixing ratio immediately before use, and after mixing, the coating film may be cured by the reaction between the epoxy resin component and the hardener component.

[0025] According to exemplary embodiments, the main component may comprise a difunctional bisphenol A type epoxy resin, a polyfunctional epoxy novolak resin, an epoxy-functional silane oligomer, a reactive diluent, a co-solvent, an anti-corrosion pigment, a extender pigment, and an organic solvent. The curing agent component may comprise an amine-based curing agent. In some embodiments, the curing agent component may comprise a polyamine-based curing agent, a polyamide-based curing agent, a polyamidoamine-based curing agent, a modified alicyclic amine-based curing agent, or a combination thereof.

[0026] According to exemplary embodiments, the difunctional bisphenol A type epoxy resin is used as the main binder of the first composition to form a continuous epoxy film after being applied to the surface of a steel material, and can provide thick film shielding, water resistance, chemical resistance, and mechanical strength.

[0027] In some embodiments, the difunctional bisphenol A type epoxy resin is bisphenol A diglycidyl ether, bisphenol A-epichlorohydrin epoxy resin, 2,2-bis(4-hydroxyphenyl)propane-epichlorohydrin copolymer, diglycidyl ether of bisphenol A, epichlorohydrin-bisphenol A condensate, bisphenol A polyglycidyl ether, 4,4'-(1-methylethylenedene)bisphenol diglycidyl ether, 2,2-bis(4-glycidyloxyphenyl)propane, oxirane 2,2'-[(1-methylethylenedene)bis(4,1-phenyleneoxymethylene)]bis-, a polymer of 4,4'-(1-methylethylenedene)bisphenol and (chloromethyl)oxirane, It may include 2-[[4-[2-[4-(oxiran-2-ylmethoxy)phenyl]propane-2-yl]phenoxy]methyl]oxiran, 4,4'-(propane-2,2-diyl)bis(glycidyloxybenzene), bisphenol A type diglycidyl ether oligomer, bisphenol A epoxy resin condensation polymer, hydrogenated bisphenol A diglycidyl ether, ethoxylated bisphenol A diglycidyl ether, propoxylated bisphenol A diglycidyl ether, alkylated bisphenol A diglycidyl ether, brominated bisphenol A diglycidyl ether, dimeric acid-modified bisphenol A epoxy resin, or a combination thereof.

[0028] In some embodiments, the difunctional bisphenol A type epoxy resin may be included in an amount of 10% to 45% by weight based on the total weight of the main component of the first composition. In some embodiments, the difunctional bisphenol A type epoxy resin may be included in an amount of 20% to 35% by weight based on the total weight of the main component of the first composition. If the content is excessively low, there may be a lack of continuous binder components to form a thick film, which may result in reduced shielding properties, water resistance, or mechanical strength. Conversely, if the content is excessively high, the viscosity of the composition may increase, which may reduce sprayability, atomization, and leveling properties, and may result in unfavorable dispersibility of extender pigments and anti-corrosion pigments.

[0029] According to exemplary embodiments, the multifunctional epoxy novolak resin is an epoxy resin having three or more functional groups, and can complement the crosslinking density, initial structural fixation, water resistance, and shielding properties of the first composition. In addition, when a relatively low content of epoxy functional silane oligomer assists in interfacial bonding between the steel surface and the epoxy matrix, the multifunctional epoxy novolak resin can compensate for the reduction in direct adhesion resulting from the omission of the undercoat layer by highly crosslinking the epoxy network in the region adjacent to the interface.

[0030] In some embodiments, the polyfunctional epoxy novolak resin is a phenol novolak epoxy resin, an epoxy novolak resin, a novolak-type epoxy resin, a phenol-formaldehyde novolak epoxy resin, a polyglycidyl ether of phenol-formaldehyde novolak, a polyfunctional phenol novolak epoxy condensate, a phenol epoxy novolak condensation polymer, a polymer of phenol and formaldehyde glycidyl ether, a polymer of oxirane with 2-(chloromethyl)-·formaldehyde and phenol, a condensation polymer of 2-(chloromethyl)oxirane with formaldehyde and phenol, poly[(phenylglycidyl ether)-co-formaldehyde], a formaldehyde-phenol copolymer polyglycidyl ether, a polyfunctional novolak-type epoxy oligomer, a trifunctional phenol novolak-type polyglycidyl ether, and a high-density cross-linked phenol It may include novolak-type epoxy resin, cresol novolak epoxy resin, epoxy cresol novolak resin (ECN), bisphenol A novolak epoxy resin, hydrogenated phenol novolak epoxy resin, alkyl-modified phenol novolak epoxy resin, or a combination thereof.

[0031] In some embodiments, the multifunctional epoxy novolak resin may be included in an amount of 1% to 20% by weight based on the total weight of the main component of the first composition. In some embodiments, the multifunctional epoxy novolak resin may be included in an amount of 5% to 15% by weight based on the total weight of the main component of the first composition. If the content is excessively low, it is difficult to sufficiently reinforce the interfacial adhesion assisting effect of the low-content silane oligomer, and the effect of suppressing sagging or densifying the film may not be sufficient when applying a thick film in a single application. Conversely, if the content is excessively high, the viscosity of the composition and the brittleness of the film increase, and orange peel, poor leveling, pinholes, or residual internal bubbles may occur when applying by airless spray or air spray.

[0032] According to exemplary embodiments, the epoxy-functional silane oligomer is an oligomer comprising epoxy functional groups and siloxane bonds, which can improve interfacial adhesion between the steel surface and the epoxy-based coating film.

[0033] In some embodiments, the epoxy-functional silane oligomer is an epoxy-functional silane oligomer, an epoxy-functional silane oligomer, an epoxyalkylalkoxysilane oligomer, an epoxy-functional polysiloxane oligomer, an epoxy-functional alkoxysiloxane oligomer, a gamma-glycidoxypropylalkoxysilane linear condensate, a linear co-condensate oligomer of 3-glycidoxypropylmethoxysilane, a cyclic co-condensate oligomer of 3-glycidoxypropylmethoxysilane, a partially condensate oligomer of 3-glycidoxypropylethoxysilane, a 2-(3,4-epoxycyclohexyl)ethylalkoxysilane condensate oligomer, a methoxy-terminated epoxysilane oligomer, an ethoxy-terminated epoxysilane oligomer, an epoxy-functional methylmethoxysiloxane oligomer, an epoxy-functional ethylethoxysiloxane oligomer, an oligomeric organoalkoxysiloxane, It may include alkyl / epoxy co-condensed silane oligomers, phenyl-modified epoxy silane oligomers, aliphatic-modified epoxy polysiloxane oligomers, cycloaliphatic-modified epoxy silane oligomers, or combinations thereof.

[0034] For example, the epoxy functional silane oligomer may include a partially hydrolyzed product, partially condensed product, or combination thereof of 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, or a combination thereof.

[0035] In some embodiments, the epoxy-functional silane oligomer may have a number average molecular weight (Mn) of 500 to 1,500 g / mol in consideration of mobility to the steel interface. In some embodiments, the epoxy-functional silane oligomer may have an oligomer backbone with a silicon number (degree of polymerization) in the range of 2 to 5.

[0036] In some embodiments, the epoxy functional silane oligomer may include a structural unit represented by the following chemical formula 1.

[0037] [Chemical Formula 1]

[0038] X-[Si(R 1 )(OR 2 )-O]n-Si(R 3 )(OR 4 )-Y

[0039] In Chemical Formula 1, R 1 and R 3 Each is independently a C1 to C6 alkyl group or a C1 to C6 alkoxy group, R2 and R4 are independently a C1 to C4 alkyl group, at least one of X and Y is an organic group including an epoxy group, a glycidoxy group or an epoxycycloalkyl group, and n may be an integer from 1 to 20.

[0040] In some embodiments, the number average molecular weight of the epoxy functional silane oligomer may be 500 g / mol to 1,500 g / mol. If the number average molecular weight is excessively low, premature hydrolysis or self-condensation due to trace moisture during storage may occur, similar to monomeric silanes, which may lead to increased viscosity, the formation of gel particles, or reduced adhesion after storage. Conversely, if the number average molecular weight is excessively high, compatibility within the composition may decrease, and wettability or interfacial accessibility to the steel surface may be reduced, resulting in reduced initial adhesion.

[0041] In some embodiments, the epoxy-functional silane oligomer may be included in an amount of 0.1% to 5.0% by weight based on the total weight of the main component of the first composition. In some embodiments, the epoxy-functional silane oligomer may be included in an amount of 1.0% to 2.0% by weight based on the total weight of the main component of the first composition. If the content is excessively low, the direct adhesion to the steel surface and the adhesion retention rate after moisture resistance may not be sufficient under conditions where the undercoat layer is omitted. Conversely, if the content is excessively high, the raw material cost increases, and an increase in viscosity, phase separation, or increased film brittleness may occur during storage, and the appearance of the film may deteriorate due to residual alkoxy groups or reactive groups of the silane component.

[0042] According to exemplary embodiments, the ether-based reactive diluent may be a component that lowers the viscosity of the first composition, reduces the amount of volatile organic solvent used, and improves atomization and leveling properties during spray coating. Since the reactive diluent contains epoxy functional groups and can react with an amine-based curing agent, it may remain in the coating film compared to a general volatile organic solvent.

[0043] In some embodiments, the ether-based reactive diluent may include an aliphatic glycidyl ether-based reactive diluent. In some embodiments, the aliphatic glycidyl ether-based reactive diluent is butyl glycidyl ether, 2-ethylhexyl glycidyl ether, C12-C14 alkyl glycidyl ether, C13-C15 alkyl glycidyl ether, C8-C10 alkyl glycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, o-cresyl glycidyl ether, neopentyl glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, ethylene glycol It may include diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, cyclohexanedimethanol diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, trimethylolpropane triglycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, sorbitol polyglycidyl ether, cardanol glycidyl ether, glycidyl ether derived from cashew nut shell liquid, or a combination thereof.

[0044] In some embodiments, the reactive diluent may be included in an amount of 1% to 15% by weight based on the total weight of the main component of the first composition. In some embodiments, the reactive diluent may be included in an amount of 3% to 8% by weight based on the total weight of the main component of the first composition. If the content is excessively low, it may not sufficiently compensate for the increase in viscosity resulting from the introduction of the polyfunctional epoxy novolak resin, which may lead to reduced spray atomization, leveling properties, and thick film coating properties. Conversely, if the content is excessively high, the crosslinking density, hardness, water resistance, or chemical resistance of the coating film may be reduced, and the adhesion retention rate after moisture resistance may be lowered.

[0045] According to exemplary embodiments, the first composition may further include a glycol ether-based cosolvent. The glycol ether-based cosolvent may be a component that improves compatibility between the epoxy resin, the polyfunctional epoxy novolak resin, the silane oligomer, the pigment, and the organic solvent, and mitigates the excessively rapid drying of the surface during thick film application, thereby suppressing the occurrence of pinholes or craters.

[0046] In some embodiments, the glycol ether-based cosolvent is ethylene glycol monobutyl ether (butyl cellosolve), ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether (butyl carbitol), triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether (PMB), dipropylene glycol monomethyl ether (DPGME), dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, ethylene glycol dimethyl ether, and diethylene glycol dimethyl It may include ether, diethylene glycol methyl ethyl ether, or a combination thereof.

[0047] In some embodiments, the co-solvent may be included in an amount of 2% to 5% by weight based on the total weight of the main component of the first composition. If the content is excessively low, compatibility, leveling properties, and pinhole suppression effects may not be sufficient. Conversely, if the content is excessively high, VOC content may increase, or drying delay, surface adhesion, or deterioration of film properties due to solvent residue may occur.

[0048] According to exemplary embodiments, the main component of the first composition may include an organic solvent. The organic solvent may be a component that controls the miscibility, dispersibility, storage stability, and coating viscosity of the difunctional bisphenol A type epoxy resin, the polyfunctional epoxy novolak resin, the epoxy functional silane oligomer, the reactive diluent, the co-solvent, the anti-corrosion pigment, and the extender pigment.

[0049] In some embodiments, the organic solvent may include an aromatic hydrocarbon solvent, an aliphatic hydrocarbon solvent, a ketone solvent, an ester solvent, an alcohol solvent, or a combination thereof.

[0050] In some embodiments, the organic solvent may include xylene, o-xylene, m-xylene, p-xylene, mixed xylene, ethylbenzene, toluene, solvent naphtha, high-boiling point aromatic hydrocarbon solvent, low-odor aromatic hydrocarbon solvent, mineral spirit, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, acetone, ethyl acetate, butyl acetate, isobutyl acetate, propylene glycol monomethyl ether acetate, ethylene glycol monobutyl ether acetate, n-butanol, isobutanol, isopropanol, diacetone alcohol, or a combination thereof.

[0051] In some embodiments, the organic solvent may include a xylene-based solvent. In some embodiments, the organic solvent may include a mixed xylene comprising xylene, o-xylene, m-xylene, and p-xylene. The xylene-based solvent may be advantageous for controlling spray viscosity and leveling properties required at the painting site, while providing solubility and pigment dispersibility for the epoxy resin component.

[0052] In some embodiments, the organic solvent may be included in an amount of 1% to 25% by weight based on the total weight of the main component of the first composition. If the content of the organic solvent is excessively low, it is difficult to sufficiently compensate for the increase in viscosity resulting from the introduction of the polyfunctional epoxy novolak resin and pigment component, which may lead to a decrease in atomization, leveling properties, or film appearance when applied by airless spray or air spray. Conversely, if the content of the organic solvent is excessively high, the VOC content of the first composition for application increases after mixing, making it difficult to satisfy low VOC conditions, and solvent residue, pinholes, craters, or internal curing non-uniformity may occur when applying a thick film.

[0053] In some embodiments, the main component of the first composition may include a reactive diluent replacing a portion of the organic solvent. The reactive diluent controls the coating viscosity of the first composition together with the organic solvent, and since it can participate in the epoxy network within the coating film during the curing process, it can suppress the increase of volatile organic compounds. In some embodiments, the content of the organic solvent and the reactive diluent may be controlled so that the main component of the first composition has a viscosity suitable for airless spray application, while the VOC content of the first composition for application after mixing is 300 g / L or less.

[0054] According to exemplary embodiments, the anti-corrosion pigment may be a component that compensates for the reduction in initial anti-corrosion properties resulting from the omission of the primer layer. In some embodiments, the anti-corrosion pigment may include a zinc phosphate-based anti-corrosion pigment, aluminum tripolyphosphate, zinc aluminum phosphate, calcium ion-exchange silica, a molybdate-based anti-corrosion pigment, or a combination thereof.

[0055] In some embodiments, the anti-corrosion pigment may be included in an amount of 3% to 20% by weight based on the total weight of the main component of the first composition. If the content is excessively low, it is difficult to sufficiently compensate for the initial anti-corrosion properties resulting from the omission of the undercoat layer, and rust, blistering, or peeling may occur under salt spray or moisture resistance conditions. Conversely, if the content is excessively high, an increase in the viscosity of the composition, a decrease in dispersibility, film brittleness, or an increase in surface roughness may occur.

[0056] According to exemplary embodiments, the extender pigment may be a component that controls the volumetric stability, mechanical strength, sagging inhibition, and shielding properties of the coating film. In some embodiments, the extender pigment may include talc, mica, barium sulfate, calcium carbonate, alumina, silica, titanium dioxide, or a combination thereof.

[0057] According to exemplary embodiments, the curing agent portion of the first composition may include an amine-based curing agent, a curing accelerator, an organic solvent, and an auxiliary solvent. According to exemplary embodiments, the amine-based curing agent may react with an epoxy resin, a polyfunctional epoxy novolak resin, an epoxy-functional silane oligomer, and an aliphatic glycidyl ether-based reactive diluent to form an epoxy-based curing network.

[0058] In some embodiments, the amine-based curing agent may include polyamine, polyamide, polyamidoamine, modified alicyclic amine, amine adduct, phenalcarmine-based curing agent, or a combination thereof.

[0059] In some embodiments, the weight ratio of the epoxy-functional silane oligomer to the polyfunctional epoxy novolak resin may be 1:3 to 1:15. At this weight ratio, the interfacial adhesion assisting effect of the low-content silane oligomer and the high-crosslinking network formation effect of the polyfunctional epoxy novolak resin can be balanced. If the relative content of the polyfunctional epoxy novolak resin is excessively low, the film matrix may not sufficiently support the interfacial anchoring effect of the silane oligomer, and if it is excessively high, an increase in viscosity, poor leveling, or film brittleness may occur.

[0060] In some embodiments, the weight ratio of the polyfunctional epoxy novolak resin to the aliphatic glycidyl ether-based reactive diluent may be 1:0.3 to 1:1.5. At this weight ratio, the increase in crosslinking density by the polyfunctional epoxy novolak resin and the viscosity reduction and VOC reduction effects by the reactive diluent can be balanced.

[0061] In some embodiments, the weight ratio of the volatile aromatic solvent to the aliphatic glycidyl ether-based reactive diluent may be 1:0.5 to 1:3. At this weight ratio, the amount of volatile organic solvent used can be reduced while maintaining coating viscosity, and the VOC content of the first composition can be controlled to 300 g / L or less.

[0062] In some embodiments, the curing accelerator can promote the reaction between the amine-based curing agent and the epoxy group to improve curability at room temperature or low temperature conditions. In some embodiments, the curing accelerator may include 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, triethanolamine, dimethylaminoethanol, or a combination thereof.

[0063] In some embodiments, the curing agent portion of the first composition may further include an organic solvent and an auxiliary solvent. The organic solvent and the auxiliary solvent may control the viscosity of the amine-based curing agent, the miscibility with the main component, the coating viscosity after mixing, and the airless sprayability.

[0064] In some embodiments, the organic solvent included in the curing agent part may include xylene, o-xylene, m-xylene, p-xylene, mixed xylene, ethylbenzene, toluene, solvent naphtha, butyl acetate, isobutyl acetate, methylisobutylketone, cyclohexanone, or a combination thereof. In some embodiments, the auxiliary solvent included in the curing agent part may include isobutanol, n-butanol, 2-methyl-1-propanol, isopropanol, diacetone alcohol, ethylene glycol monobutyl ether, or a combination thereof.

[0065] In some embodiments, the amine-based curing agent may be included in an amount of 60% to 90% by weight based on the total weight of the curing agent portion of the first composition. If the content of the amine-based curing agent is excessively low, the curing reaction of the epoxy group is insufficient, and the water resistance, chemical resistance, direct adhesion to steel, or hardness of the coating film may be reduced. Conversely, if the content of the amine-based curing agent is excessively high, the pot life may be shortened, or coating film brittleness, surface defects, or yellowing may increase.

[0066] In some embodiments, the curing accelerator may be included in an amount of 0.1% to 3% by weight based on the total weight of the curing agent portion of the first composition. In some embodiments, the curing agent portion of the first composition may include 5% to 25% by weight of an organic solvent and 1% to 10% by weight of an auxiliary solvent based on the total weight of the curing agent portion of the first composition.

[0067] In some embodiments, the main component of the first composition and the curing agent may be mixed immediately before use. In some embodiments, the main component of the first composition and the curing agent may be mixed in a weight ratio of 70:30 to 90:10.

[0068] According to exemplary embodiments, the second composition may be a topcoat composition applied on a cured film of the first composition. The second composition may be a two-component composition comprising a main component and a curing agent component.

[0069] The main component of the second composition may include an acrylic polyol resin, an interfacial swelling type mixed solvent, a coloring pigment, a dispersant, an antifoaming agent, a leveling agent, and an organic solvent. In some embodiments, the curing agent component of the second composition may include an aliphatic polyisocyanate curing agent. The second composition may be applied to a cured film of the first composition by mixing the main component and the curing agent component in a predetermined mixing ratio immediately before use, and after mixing, the hydroxyl groups of the acrylic polyol resin and the isocyanate groups of the aliphatic polyisocyanate curing agent may react to form a polyurethane-based topcoat film.

[0070] According to exemplary embodiments, the acrylic polyol resin can serve as the main binder of the second composition to provide weather resistance, gloss retention, color retention, and appearance. The acrylic polyol resin used as the main binder of the second composition according to the present invention can provide excellent atomization and leveling properties without orange-peel defects during spraying, even when the amount of organic solvent used is reduced to satisfy low VOC regulatory conditions, and can ensure weather resistance and gloss retention of the final coating film.

[0071] In some embodiments, the acrylic polyol resin may comprise alkyl (meth)acrylate monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate; hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone-modified hydroxyalkyl (meth)acrylate; and copolymers of one or more known monomers selected from styrene, alpha-methylstyrene, (meth)acrylic acid, itaconic acid, and acrylonitrile, or combinations thereof.

[0072] In some embodiments, the acrylic polyol resin may comprise at least one selected from hydroxyl group-containing acrylic resin, hydroxyethyl methacrylate copolymer acrylic resin, hydroxypropyl methacrylate copolymer acrylic resin, hydroxyethyl acrylate copolymer acrylic resin, methyl methacrylate-butyl acrylate-hydroxyalkyl methacrylate copolymer, styrene-acrylic polyol resin, polyester-modified acrylic polyol resin, silicone-modified acrylic polyol resin, fluorine-modified acrylic polyol resin, high-solids acrylic polyol resin, low-viscosity acrylic polyol resin, aliphatic urethane-modified acrylic polyol resin, caprolactone-modified acrylic polyol resin, alkyl methacrylate-based acrylic polyol resin, alkyl acrylate-based acrylic polyol resin, and hydroxyl group-containing acrylic oligomer.

[0073] In some embodiments, the acrylic polyol resin may have a viscosity of 2,000 cPs to 4,000 cPs at 25°C based on a solid content of 75%. If the viscosity is excessively low, film formation or durability may be insufficient, and if the viscosity is excessively high, spray atomization under low VOC conditions may be reduced, resulting in orange peel or leveling defects.

[0074] In some embodiments, the acrylic polyol resin may be included in an amount of 35% to 60% by weight based on the total weight of the main component of the second composition. In some embodiments, the acrylic polyol resin may be included in an amount of 40% to 55% by weight based on the total weight of the main component of the second composition. If the content is excessively low, the continuity, gloss retention, or weather resistance of the topcoat film may be reduced, and if the content is excessively high, the paint viscosity may increase, thereby reducing sprayability and leveling properties.

[0075] According to exemplary embodiments, the aliphatic polyisocyanate curing agent may be included in the curing agent portion of the second composition. The aliphatic polyisocyanate curing agent may react with the hydroxyl groups of the acrylic polyol resin to form a polyurethane-based cross-linked film. The aliphatic polyisocyanate curing agent exhibits less yellowing compared to an aromatic isocyanate-based curing agent and may be advantageous for ensuring weather resistance, gloss retention, and color retention of the topcoat film.

[0076] In some embodiments, the aliphatic polyisocyanate curing agent may comprise hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (H12MDI), tetramethylxylene diisocyanate (TMXDI), lysine diisocyanate, their isocyanurate trimers, their biuret modified forms, their uretdione dimers, their allophanate modified forms, their oligomeric polyfunctional derivatives, or a blocked polyisocyanate compound capped by one or more blockers selected from methyl ethyl ketoxime (MEKO), diethyl malonate (DEM), 3,5-dimethylpyrazole (DMP), 1,2-pyrazole, triazole, and alcohols, or a combination thereof.

[0077] In some embodiments, the aliphatic polyisocyanate curing agent may comprise at least one selected from hexamethylene diisocyanate isocyanurate trimer, hexamethylene diisocyanate biuret modified agent, hexamethylene diisocyanate allophanate modified agent, isophorone diisocyanate isocyanurate trimer, and 4,4'-dicyclohexylmethane diisocyanate modified agent.

[0078] In some embodiments, the aliphatic polyisocyanate curing agent may have a viscosity of 1,500 cPs or less at 25°C. Within this viscosity range, the second composition may exhibit excellent sprayability even under low VOC conditions. In some embodiments, the aliphatic polyisocyanate curing agent may have a viscosity of 200 cPs to 1,500 cPs at 25°C. If the viscosity is excessively low, the solid content or formability of the topcoat film may be insufficient, and if it is excessively high, the viscosity may increase after mixing with the main component, thereby reducing sprayability or leveling performance.

[0079] According to exemplary embodiments, the interfacial swelling type mixed solvent may be included in the main component of the second composition. The interfacial swelling type mixed solvent may be a component that controls the paintability, leveling properties, and interlayer adhesion to the first coating film of the second composition. The interfacial swelling type mixed solvent can suppress interlayer delamination between the first coating film and the second coating film by supplementing the wettability to the surface of the first coating film and the flatness of the topcoat film.

[0080] In some embodiments, the interfacial swelling type mixed solvent may comprise n-butyl acetate, ethyl acetate, isobutyl acetate, isopropyl acetate, methyl acetate, propylene glycol monomethyl ether acetate (PMA), propylene glycol monoethyl ether acetate, ethyl ether acetate, ethyl 3-ethoxypropionate (EEP), dimethyl adipate, dimethyl glutarate, dimethyl succinate, diethylene glycol monobutyl ether acetate, methyl isobutyl ketone (MIBK), methyl ethyl ketone (MEK), cyclohexanone, diisobutyl ketone, butyl cellosolve acetate, or a combination thereof.

[0081] In some embodiments, the interfacial swelling type mixed solvent may include butyl acetate and propylene glycol monomethyl ether acetate together. In this case, the weight ratio of butyl acetate to propylene glycol monomethyl ether acetate may be 6:4 to 8:2. In the above weight ratio, butyl acetate can complement the sprayability and initial drying properties of the second composition, and propylene glycol monomethyl ether acetate can complement the wettability and leveling properties of the first coating surface. If the relative content of butyl acetate is excessively low, drying may be delayed or surface adhesion may occur, and if it is excessively high, the complementary effect on wettability or interlayer adhesion of the first coating may not be sufficient.

[0082] In some embodiments, the interfacial swelling type mixed solvent may be included in an amount of 20% to 40% by weight based on the total weight of the main component of the second composition. In some embodiments, the interfacial swelling type mixed solvent may be included in an amount of 25% to 35% by weight based on the total weight of the main component of the second composition. If the content is excessively low, the coating viscosity may increase, which may reduce leveling and atomization properties, and if it is excessively high, the VOC content may increase, or the coating film thickness, opacity, or drying properties may decrease.

[0083] According to exemplary embodiments, the coloring pigment may be included in the main part of the second composition. The coloring pigment may provide color, opacity, and appearance of the topcoat film. In some embodiments, the coloring pigment may include at least one selected from rutile titanium dioxide, anatase titanium dioxide, iron oxide red pigment, iron oxide yellow pigment, iron oxide black pigment, carbon black, phthalocyanine blue, phthalocyanine green, chromium oxide green, cobalt blue, ultramarine blue, quinacridone-based pigment, azo-based pigment, and composite inorganic color pigment.

[0084] In some embodiments, the coloring pigment may be included in an amount of 5% to 30% by weight based on the total weight of the main component of the second composition. In some embodiments, the coloring pigment may be included in an amount of 10% to 25% by weight based on the total weight of the main component of the second composition. If the content is excessively low, opacity or color realization may be insufficient, and if it is excessively high, dispersibility, leveling ability, or gloss may be reduced.

[0085] In some embodiments, the main component of the second composition may further include a dispersant, an antifoaming agent, a leveling agent, an ultraviolet absorber, a light stabilizer, or a combination thereof. For example, the dispersant may include a polycarboxylic acid-based wetting dispersant, the antifoaming agent may include a non-silicone-based polymer antifoaming agent or a siloxane-based antifoaming agent, and the leveling agent may include a polyacrylate-based leveling agent. Additionally, the ultraviolet absorber may include a benzotriazole-based ultraviolet absorber, and the light stabilizer may include a hindered amine-based light stabilizer.

[0086] In some embodiments, the main component of the second composition may comprise 0.1% to 1.0% by weight of a dispersant, 0.05% to 0.5% by weight of an antifoaming agent, 0.05% to 0.5% by weight of a leveling agent, 0.1% to 2.0% by weight of an ultraviolet absorber, and 0.1% to 2.0% by weight of a light stabilizer.

[0087] In some embodiments, the VOC content of the second composition may be 300 g / L or less. In some embodiments, the VOC content of the second composition may be 250 g / L or less.

[0088] In some embodiments, the curing agent portion of the second composition may include a curing agent, an organic solvent, and an auxiliary solvent.

[0089] In some embodiments, the curing agent may include an aliphatic polyisocyanate curing agent. The aliphatic polyisocyanate curing agent may be a component that reacts with the hydroxyl groups of the acrylic polyol resin included in the main part of the second composition to form a polyurethane-based topcoat film. In some embodiments, the aliphatic polyisocyanate curing agent may include a hexamethylene diisocyanate isocyanurate trimer, a hexamethylene diisocyanate biuret modified agent, a hexamethylene diisocyanate allophanate modified agent, an isophorone diisocyanate isocyanurate trimer, a 4,4'-dicyclohexylmethane diisocyanate modified agent, or a combination thereof.

[0090] In some embodiments, the aliphatic polyisocyanate curing agent may include a first aliphatic polyisocyanate curing agent and a second aliphatic polyisocyanate curing agent. The first aliphatic polyisocyanate curing agent may include a hexamethylene diisocyanate isocyanurate trimer, and the second aliphatic polyisocyanate curing agent may include a hexamethylene diisocyanate biuret modified agent. For example, the hexamethylene diisocyanate isocyanurate trimer and the hexamethylene diisocyanate biuret modified agent may each have an NCO content of 20% to 23% by weight.

[0091] The organic solvent may be a component that controls the viscosity of the aliphatic polyisocyanate curing agent, the miscibility with the main component, and the coating viscosity. In some embodiments, the organic solvent may include n-butyl acetate, isobutyl acetate, ethyl acetate, propylene glycol monomethyl ether acetate, methyl isobutyl ketone, methyl ethyl ketone, xylene, or a combination thereof. For example, the organic solvent may include n-butyl acetate.

[0092] The above auxiliary solvent may be a component that complements the storage stability of the curing agent part, compatibility with the main part, and sprayability. In some embodiments, the above auxiliary solvent may include propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, butyl cellosolve acetate, or a combination thereof. For example, the above auxiliary solvent may include propylene glycol monomethyl ether acetate.

[0093] In some embodiments, the aliphatic polyisocyanate curing agent may be included in an amount of 60% to 95% by weight based on the total weight of the curing agent portion of the second composition. In some embodiments, the aliphatic polyisocyanate curing agent may be included in an amount of 70% to 90% by weight based on the total weight of the curing agent portion of the second composition.

[0094] In some embodiments, the organic solvent may be included in an amount of 5% to 25% by weight based on the total weight of the curing agent portion of the second composition. In some embodiments, the auxiliary solvent may be included in an amount of 0% to 15% by weight based on the total weight of the curing agent portion of the second composition.

[0095] In some embodiments, the main component and the curing agent component of the second composition may be mixed such that the NCO / OH equivalent ratio is 0.9 to 1.2. In some embodiments, the main component and the curing agent component of the second composition may be mixed such that the NCO / OH equivalent ratio is 1.0. If the NCO / OH equivalent ratio is excessively low, the curing density, weather resistance, or chemical resistance of the topcoat film may be reduced, and if it is excessively high, film brittleness, bubbles, or appearance defects may occur due to residual isocyanate.

[0096] FIG. 1 is a flowchart for explaining a coating method using a steel coating composition according to one embodiment of the present disclosure.

[0097] According to exemplary embodiments, a method for coating a steel structure using the first composition and the second composition may be provided. The coating method may be applied to coating a new steel structure, repair coating of a steel structure from which an existing coating has been removed, or recoating a steel structure in which a portion of an existing coating remains.

[0098] Referring to FIG. 1, the coating method may include the steps of preparing a steel surface, directly applying a first composition to the steel surface to form a first coating film, and applying a second composition on the first coating film to form a second coating film.

[0099] The step of preparing the steel surface (S110) may include removing rust, deteriorated coating, oil, moisture, dust, salt, or foreign substances present on the steel surface. In some embodiments, the step of preparing the steel surface may include blast treatment, polishing treatment, grinding treatment, high-pressure water washing, solvent washing, compressed air cleaning, or a combination thereof. In some embodiments, the steel surface may be a bare metal steel surface. In some embodiments, the steel surface may be a surface for repair painting or repainting in which a bare metal exposed portion and a portion of the existing coating remain together.

[0100] In some embodiments, the step of applying the first composition may include the step of preparing a first composition for application by mixing the main component and the hardener component of the first composition. For example, the main component and the hardener component of the first composition may be mixed in a weight ratio of 80:20. After mixing, the first composition may be applied to the surface of a steel material within a pot life. In some embodiments, the pot life of the first composition at 25°C after mixing may be 2 to 8 hours, preferably 3 to 6 hours.

[0101] In some embodiments, the first composition may be applied directly to the surface of the steel without a separate undercoat or primer layer (S120). That is, the first composition may be a composition for direct application to the steel. The first composition may form a first coating film that integrates the undercoat and intermediate layers, providing both the direct adhesion and initial corrosion resistance of the undercoat layer and the thick film shielding properties of the intermediate layer.

[0102] In some embodiments, the first composition may be applied by an airless spray, an air spray, a roller, a brush, or a combination thereof. In some embodiments, the first composition may be applied by an airless spray method. The airless spray method may be suitable for on-site painting or repainting of large-area steel structures and may be advantageous for forming a thick film by a single application.

[0103] In some embodiments, the first film may be formed with a dry film thickness of 100 μm to 200 μm by a single application. In some embodiments, the first film may be formed with a dry film thickness of 120 μm to 180 μm by a single application. If the dry film thickness is excessively low, the anti-corrosion, shielding, or mechanical protection properties required to simultaneously provide the functions of the undercoat and intermediate layers may not be sufficient. Conversely, if the dry film thickness is excessively high, sagging, pinholes, bubbles, craters, or internal curing non-uniformity may occur.

[0104] In some embodiments, the first film may be cured at room temperature. For example, the first film may be cured for 12 to 48 hours under conditions of 20°C to 25°C and 50% to 60% relative humidity. In some embodiments, the first film may be cured even under low temperature conditions of 10°C to 15°C.

[0105] In some embodiments, the step of applying the second composition may include the step of preparing a second composition for application by mixing the main component and the curing agent component of the second composition. In some embodiments, the main component and the curing agent component of the second composition may be mixed such that the NCO / OH equivalent ratio is 0.9 to 1.2. In some embodiments, the main component and the curing agent component of the second composition may be mixed such that the NCO / OH equivalent ratio is 1.0.

[0106] In some embodiments, the second composition may be applied to the first film after the surface of the first film has dried (S130). In some embodiments, the second composition may be applied within 8 hours to 7 days after the first film is formed. In some embodiments, the second composition may be applied within 24 hours to 72 hours after the first film is formed. If the recoating interval is too short, the solvent or reaction byproduct inside the first film may not be sufficiently discharged, which may result in bubbles or interlayer defects, and if it is too long, the interlayer adhesion with the second film may be reduced due to contamination of the surface of the first film or the progress of curing.

[0107] In some embodiments, the second composition may be applied by an airless spray, an air spray, a roller, a brush, or a combination thereof. In some embodiments, the second film may be formed with a dry film thickness of 40 μm to 75 μm. In some embodiments, the second film may be formed with a dry film thickness of 50 μm to 70 μm.

[0108] In some embodiments, the second coating film may be cured on the first coating film to form a top coating film. The second coating film may provide weather resistance, color retention, gloss retention, and appearance protection.

[0109] In some embodiments, the coating system formed by the coating method may include a first coating formed directly on the surface of the steel and a second coating formed on the first coating. The first coating may provide the functions of a primer and an intermediate layer, and the second coating may provide the functions of a top layer. Accordingly, the coating method may replace a conventional three-coating system including a primer, an intermediate layer, and a top layer with a two-coating system including a first coating and a second coating.

[0110] In some embodiments, the coating system formed by the coating method may have a dry film thickness of the first coating film of 100 μm to 200 μm and a dry film thickness of the second coating film of 40 μm to 75 μm. In some embodiments, the total dry film thickness of the coating system may be 140 μm to 275 μm.

[0111] In some embodiments, the coating system formed by the coating method may have excellent direct adhesion to the steel surface, adhesion retention rate after moisture resistance, rust prevention after salt spray, thick film workability, and interlayer adhesion between the first coating and the second coating.

[0112] In order to aid in understanding the present invention, synthetic and experimental examples including preferred embodiments are presented below; however, these embodiments are merely illustrative of the invention and do not limit the appended claims. It is obvious to those skilled in the art that various changes and modifications to the embodiments are possible within the scope and spirit of the invention, and that such variations and modifications fall within the scope of the appended claims.

[0113] [Synthesizing Example] Preparation of Epoxy Functional Silane Oligomer

[0114] 100 parts by weight of 3-glycidoxypropyltriethoxysilane, 40 to 80 parts by weight of anhydrous ethanol, and 3 to 8 parts by weight of deionized water were introduced into a reactor under a nitrogen atmosphere. Subsequently, 0.05 to 0.3 parts by weight of acetic acid were added as a catalyst, and partial hydrolysis and partial condensation reactions were carried out by stirring at 25°C to 50°C for 2 to 6 hours.

[0115] Samples were taken at regular time intervals during the reaction, and the number average molecular weight was determined using gel permeation chromatography (GPC). The reaction was terminated when the number average molecular weight reached the range of 500 g / mol to 1,500 g / mol. Subsequently, the acid catalyst was removed using a neutralizing agent or an adsorbent, and the low-boiling point component was removed under reduced pressure conditions to obtain epoxy functional silane oligomer S-2.

[0116] The above epoxy functional silane oligomer S-2 contained epoxy functional groups and partially condensed Si-O-Si bonds. The number average molecular weight of S-2 was approximately 950 g / mol.

[0117] Low molecular weight epoxy functional silane oligomer S-3 was prepared using the same method as Synthesis Example 1, except that the amount of deionized water added and the reaction time were reduced in Synthesis Example 1 of epoxy functional silane oligomer S-2. The number average molecular weight of S-3 was less than 300 g / mol, specifically about 280 g / mol.

[0118] High molecular weight epoxy functional silane oligomer S-4 was prepared in the same manner as Synthesis Example 1, except that the amount of deionized water input, the amount of catalyst, and the reaction time were increased in Synthesis Example 1 of epoxy functional silane oligomer S-2. The number average molecular weight of S-4 was greater than 4,000 g / mol, specifically about 4,800 g / mol.

[0119] The components of Table 1 below are used as the main component of the first composition, and Table 2 below shows the composition table of the main component of the first composition according to experimental examples and comparative examples.

[0120] division sign Specific ingredients Difunctional epoxy resin E-1 Bisphenol A diglycidyl ether-based liquid epoxy resin, epoxy equivalent 180 g / eq to 200 g / eq Polyfunctional epoxy resin E-2 Phenol novolak epoxy resin, average number of epoxy functional groups 3 or more, epoxy equivalent 170 g / eq to 230 g / eq Silane component S-1 3-Glycidoxypropyltriethoxysilane Silane component S-2 Epoxy functional silane oligomer of Synthesis Example 1, Mn approx. 950 g / mol Silane component S-3 Low molecular weight epoxy functional silane oligomer of Synthesis Example 2, Mn approx. 280 g / mol Silane component S-4 High molecular weight epoxy functional silane oligomer of Synthesis Example 3, Mn approx. 4,800 g / mol Reactive diluent R-1 C12-C14 alkyl glycidyl ether Public sale C-1 Ethylene glycol monobutyl ether, i.e., butyl cellosolve Anti-corrosion pigment P-1 zinc phosphate Body pigment F-1 A mixture of talc and mica Coloring pigment T-1 Rutile titanium dioxide solvent X-1 Xylene Dispersant A-1 Acid group-containing polymer-based wetting dispersant Antifoamer A-2 Polyether-modified polydimethylsiloxane-based defoamer Leveling agent A-3 Polyacrylate-based leveling agent Anti-settling agent A-4 polyamide wax

[0121] division E-1 E-2 Silane component Silane content R-1 C-1 P-1 F-1 T-1 A-1 X-1 Example 1 30 10 S-2 1.5 5 3 10 25 5 0.5 10 Example 2 30 10 S-2 1 5 3 10 25 5 0.5 10.5 Example 3 30 10 S-2 2 5 3 10 25 5 0.5 9.5 Example 4 30 5 S-2 1.5 5 3 10 25 5 0.5 15 Example 5 30 15 S-2 1.5 5 3 10 25 5 0.5 5 Example 6 30 10 S-2 1.5 3 3 10 25 5 0.5 12 Example 7 30 10 S-2 1.5 8 3 10 25 5 0.5 7 Example 8 30 10 S-3 1.5 5 3 10 25 5 0.5 10 Example 9 30 10 S-4 1.5 5 3 10 25 5 0.5 10 Example 10 30 10 S-2 0.5 5 3 10 25 5 0.5 11 Example 11 30 10 S-2 3 5 3 10 25 5 0.5 8.5 Example 12 30 3 S-2 1.5 5 3 10 25 5 0.5 17 Example 13 30 10 S-2 1.5 12 3 10 25 5 0.5 3 Comparative Example 1 30 0 doesn't exist 0 5 3 10 25 5 0.5 21.5 Comparative Example 2 30 0 S-2 1.5 5 3 10 25 5 0.5 20 Comparative Example 3 30 10 doesn't exist 0 5 3 10 25 5 0.5 11.5 Comparative Example 4 30 10 S-1 1.5 5 3 10 25 5 0.5 10 Comparative Example 5 30 20 S-2 1.5 5 3 10 25 5 0.5 0 Comparative Example 6 30 10 S-2 1.5 0 3 10 25 5 0.5 15

[0122] The components and content according to Table 3 below were used as the curing agent part of the first composition, the components and content according to Table 4 below were used as the main part of the second composition, and the components and content according to Table 5 below were used as the curing agent part of the second composition.

[0123] division Specific ingredients Content, weight% 1st amine-based curing agent Polyamide resin that is a condensation product of dimerized fatty acid and diethylenetriamine, amine value 250 mgKOH / g to 320 mgKOH / g, viscosity at 25°C 3,000 cPs to 8,000 cPs 65 Secondary amine-based curing agent An amine adduct that is a reaction product of isophoronediamine and bisphenol A diglycidyl ether, amine value 300 mgKOH / g to 420 mgKOH / g, viscosity at 25°C 1,000 cPs to 4,000 cPs 20 hardening accelerator 2,4,6-Tris(dimethylaminomethyl)phenol 1 organic solvents Mixed xylene including xylene, o-xylene, m-xylene, and p-xylene 10 auxiliary solvent 2-methyl-1-propanol 4 total 100

[0124] division Specific ingredients Content, weight% acrylic polyol resin Copolymer of methyl methacrylate, n-butyl acrylate, 2-hydroxyethyl methacrylate, and styrene, solid content 75%, hydroxyl group 80 mgKOH / g to 120 mgKOH / g, viscosity at 25°C 2,000 cPs to 4,000 cPs 45 white coloring pigment Rutile titanium dioxide 18 Coloring auxiliary pigment Iron oxide yellow pigment, CI Pigment Yellow 42 2 Dispersant Poly(12-hydroxystearic acid)-based polymer wetting dispersant, acid value 20 mgKOH / g to 80 mgKOH / g 0.5 Antifoamer Polypropylene glycol, number average molecular weight 1,000 g / mol to 3,000 g / mol 0.2 Leveling agent Polyacrylate-based leveling agent that is a copolymer of n-butyl acrylate and 2-ethylhexyl acrylate 0.3 UV absorber 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol 1 light stabilizer Bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate 1 Interfacial swelling type mixed solvent n-butyl acetate 22.4 Interfacial swelling type mixed solvent Propylene glycol monomethyl ether acetate 9.6 total 100

[0125] division Specific ingredients Content, weight% First aliphatic polyisocyanate curing agent Hexamethylene diisocyanate isocyanurate trimer, NCO content 20 wt% to 23 wt%, viscosity at 25°C 1,000 cPs to 3,000 cPs 75 Second aliphatic polyisocyanate curing agent Hexamethylene diisocyanate biuret modified agent, NCO content 20 wt% to 23 wt%, viscosity at 25°C 1,500 cPs to 4,000 cPs 10 organic solvents n-butyl acetate 10 auxiliary solvent Propylene glycol monomethyl ether acetate 5 total 100

[0126] Experimental results according to examples and comparative examples are presented below. Unless otherwise specified, the main component of the first composition was prepared according to the composition of Table 2, and the curing agent component of the first composition was fixed to the composition of Table 3. In addition, the main component and the curing agent component of the second composition were fixed to the compositions of Table 4 and Table 5, respectively.

[0127] The main component and the curing agent component of the first composition were mixed in a weight ratio of 80:20 and used. The main component and the curing agent component of the second composition were mixed so that the NCO / OH (moles of isocyanate groups / moles of hydroxyl groups) equivalent ratio was 1.0 and used.

[0128] [Preparation of specimens for evaluation of coating method]

[0129] SS400 steel plates were used for the steel specimens. The size of the steel specimens was set to 150 mm × 70 mm × 3 mm.

[0130] To simulate new coating conditions, the first steel specimen was blasted or polished to remove rust, oil, dust, and foreign substances, and the surface of the bare steel was exposed. Subsequently, polishing powder, oil, and foreign substances were removed from the surface through compressed air and xylene washing, and the specimen was dried at room temperature.

[0131] To simulate recoating conditions, the second steel specimen was coated with an existing epoxy film, and then a portion of the film was polished to prepare a surface containing a mixture of exposed bare metal and a residual film. Subsequently, polishing powder, oil, and foreign substances were removed from the surface through compressed air and xylene washing, and the specimen was dried at room temperature.

[0132] The main component and the hardener component of the first composition were mixed in a weight ratio of 80:20, and then applied directly to the surface of the steel specimen within 30 minutes of mixing. The first composition was applied directly to the steel surface without a separate undercoat or primer layer. The first composition was applied using an airless spray method, and the dry film thickness of the first coating was formed to be 150 μm. The first coating was cured for 24 hours under conditions of 20°C to 25°C and a relative humidity of 50% to 60%.

[0133] The main component and the curing agent component of the second composition were mixed such that the NCO / OH equivalent ratio was 1.0, and then applied onto the first coating film. The second composition was applied 24 hours after the first coating film was formed. The second composition was applied by a spray method, and the amount of application was adjusted so that the dry film thickness of the second coating film was 60 μm. After the second coating film was formed, the entire coating system was cured for 7 days under conditions of 20°C to 25°C and relative humidity of 50% to 60%, and then the physical properties were evaluated.

[0134] [Evaluation Example 1] Storage Stability Evaluation

[0135] After preparing the main component of the first composition of Examples 1 to 13 and Comparative Examples 1 to 6, respectively, they were filled into sealed metal containers. The filled main component compositions were stored at 40°C for 8 weeks.

[0136] The viscosity before and after storage was measured at 25°C using a Brookfield viscometer. The rate of change in viscosity was calculated by the following Equation 1.

[0137] [Equation 1]

[0138] Viscosity change rate (%) = [(Viscosity after storage - Initial viscosity) / Initial viscosity] × 100

[0139] In addition, the occurrence of gel particles, precipitation, and redispersibility were visually checked after storage. Storage stability was evaluated according to the following criteria and is shown in Table 6 below.

[0140] ○: Viscosity change rate is 20% or less, and no gel particles or redispersion defects are observed

[0141] △: Viscosity change rate exceeding 20% ​​but not exceeding 50%, or microgels or redispersible precipitates observed

[0142] ×: Viscosity change rate exceeding 50%, generation of gel particles, or poor redispersion

[0143] division Viscosity change rate Whether gel particles are generated Sedimentation / Redispersibility Storage stability Example 1 8% doesn't exist Good ○ Example 2 9% doesn't exist Good ○ Example 3 10% doesn't exist Good ○ Example 4 10% doesn't exist Good ○ Example 5 11% doesn't exist Good ○ Example 6 9% doesn't exist Good ○ Example 7 10% doesn't exist Good ○ Example 8 42% Microgel generation commonly △ Example 9 14% doesn't exist Good ○ Example 10 10% doesn't exist Good ○ Example 11 28% Some viscosity also increased commonly △ Example 12 12% doesn't exist Good ○ Example 13 13% doesn't exist Good ○ Comparative Example 1 12% doesn't exist Good ○ Comparative Example 2 16% doesn't exist Good ○ Comparative Example 3 10% doesn't exist Good ○ Comparative Example 4 38% Microgel generation commonly △ Comparative Example 5 18% doesn't exist Good ○ Comparative Example 6 9% doesn't exist Good ○

[0144] Referring to Table 6 above, Comparative Example 4, which used monomeric silane instead of epoxy-functional silane oligomer, showed an increase in the rate of change in viscosity after storage and the formation of a microgel. This is believed to be because monomeric silane has a structure that is prone to early hydrolysis or self-condensation by trace amounts of moisture during storage.

[0145] On the other hand, Examples 1 to 7 containing epoxy-functional silane oligomers maintained a viscosity change rate of 20% or less after storage, and no gel particles or redispersion defects were observed.

[0146] When comparing the examples, Example 8, which used a low molecular weight silane oligomer with a number average molecular weight of about 280 g / mol, showed an increased rate of change in viscosity and a microgel compared to Example 1. In addition, Example 11, which had a silane oligomer content of 3 wt%, showed an increased rate of change in viscosity compared to Examples 1 to 7. From this, it was confirmed that the number average molecular weight and content of the epoxy-functional silane oligomer affect storage stability.

[0147] [Evaluation Example 2] Evaluation of Direct Adhesion to Steel

[0148] After evaluating the storage stability of Evaluation Example 1, the main component and the hardener component of each first composition were mixed in a weight ratio of 80:20. The mixed first composition was applied directly to a blast-treated bare metal steel specimen and cured for 7 days under conditions of 20°C to 25°C and a relative humidity of 50% to 60%.

[0149] Cross-cut adhesion and pull-off adhesion strength were evaluated for the above specimens. Cross-cut adhesion was evaluated using ASTM D3359 or a similar method. Pull-off adhesion strength was evaluated using ASTM D4541 or a similar method.

[0150] After the pull-off test, the failure location was observed and classified into failure at the steel / first coating interface, internal cohesive failure of the first coating, failure at the first coating / second coating interface, or failure of the adhesive. Direct adhesion to the steel was evaluated according to the following criteria and is shown in Table 7 below.

[0151] ◎: Cross-cut 5B, pull-off adhesion strength 5.0 MPa or higher

[0152] ○: Cross-cut 4B or larger, pull-off adhesion strength 3.5 MPa or higher

[0153] △: Cross-cut 3B or larger, or partial interfacial delamination occurs

[0154] ×: Cross-cut 2B or less or peeling occurs at the steel / first coating interface

[0155] division Cross-cut Pull-off adhesion strength Destruction location Adhesion Example 1 5B 5.8 MPa Internal cohesive failure of the first film ◎ Example 2 4B 4.6 MPa Partial cohesive breakdown ○ Example 3 5B 5.6 MPa Internal cohesive failure of the first film ◎ Example 4 4B 4.8 MPa Partial cohesive breakdown ○ Example 5 5B 5.5 MPa Internal cohesive failure of the first film ◎ Example 6 4B 4.8 MPa Partial cohesive breakdown ○ Example 7 5B 5.1 MPa Internal cohesive failure of the first film ◎ Example 8 3B 3.1 MPa Partial steel / first coating interface failure △ Example 9 3B 3.4 MPa Partial steel / first coating interface failure △ Example 10 3B 3.3 MPa Partial steel / first coating interface failure △ Example 11 5B 5.7 MPa Internal cohesive failure of the first film ◎ Example 12 3B 4.0 MPa Partial interface breakdown △ Example 13 3B 3.2 MPa Partial interface breakdown △ Comparative Example 1 2B 2.4 MPa Steel / First Coating Interface Fracture × Comparative Example 2 3B 3.2 MPa Partial steel / first coating interface failure △ Comparative Example 3 3B 3.4 MPa Partial steel / first coating interface failure △ Comparative Example 4 3B 3.0 MPa Steel / First Coating Interface Fracture △ Comparative Example 5 4B 4.2 MPa Partial cohesive breakdown △ Comparative Example 6 4B 3.7 MPa Partial interface breakdown △

[0156] Referring to Table 7 above, Comparative Example 1, which does not contain both polyfunctional epoxy novolak resin and epoxy functional silane oligomer, exhibited failure at the steel / first coating interface and had low pull-off adhesion strength.

[0157] Comparative Example 2, which contains only epoxy-functional silane oligomers and does not contain polyfunctional epoxy novolak resin, and Comparative Example 3, which contains only polyfunctional epoxy novolak resin and does not contain silane components, showed improved adhesion compared to Comparative Example 1, but lower adhesion compared to Example 1. Therefore, it was confirmed that direct adhesion to steel is significantly improved when epoxy-functional silane oligomers and polyfunctional epoxy novolak resins are used in combination.

[0158] When comparing the examples, Examples 1 to 3, in which the content of the epoxy functional silane oligomer was 1.0 wt% to 2.0 wt%, showed superior adhesion compared to Example 10. In addition, Examples 1, 4, and 5, in which the content of the polyfunctional epoxy novolak resin was 5 wt% to 15 wt%, showed superior adhesion compared to Example 12, in which the content of the polyfunctional epoxy novolak resin was 3 wt%.

[0159] Meanwhile, Example 8 using a low molecular weight silane oligomer and Example 9 using a high molecular weight silane oligomer had lower adhesion compared to Example 1, even though they contained epoxy-functional silane oligomers. This is believed to be because if the number average molecular weight of the silane oligomer is excessively low, stability during storage decreases, and if it is excessively high, mobility or wettability to the steel interface decreases.

[0160] [Evaluation Example 3] Evaluation of Thick Film Constructability

[0161] The first composition of each example and comparative example was applied to a vertically positioned steel specimen using an airless spray method. The dry film thickness of the first coating was adjusted to 150 μm. In addition, for Example 1, the dry film thickness was varied to 100 μm, 150 μm, and 200 μm to determine the range of possible thick film application.

[0162] The occurrence of sagging was visually checked after 30 minutes and 24 hours following application. Pinholes and craters were evaluated by counting the number of defects within a 10 cm × 10 cm area. Internal curability was assessed by observing the cross-section of the film after 24 hours of curing to check for any remaining uncured layers or air bubbles.

[0163] Thick film constructability was evaluated according to the following criteria, and the results are shown in Table 8.

[0164] ○: No sagging, 0 to 2 pinholes or craters, and good internal hardenability

[0165] △: Some sagging or defects are observed, but are at an acceptable level for actual use.

[0166] ×: Continuous sagging, more than 10 defects, or occurrence of internal incomplete curing

[0167] division Dry film thickness Sagging Pinhole / Crater Internal hardening Thick film constructability Example 1 100 μm ○ ○ ○ ○ Example 1 150 μm ○ ○ ○ ○ Example 1 200 μm △ ○ ○ △ Example 2 150 μm ○ ○ ○ ○ Example 3 150 μm ○ ○ ○ ○ Example 4 150 μm ○ ○ ○ ○ Example 5 150 μm ○ ○ ○ ○ Example 6 150 μm ○ ○ ○ ○ Example 7 150 μm ○ ○ △ △ Example 8 150 μm △ △ ○ △ Example 9 150 μm ○ △ ○ △ Example 10 150 μm ○ ○ ○ ○ Example 11 150 μm ○ △ ○ △ Example 12 150 μm △ △ ○ △ Example 13 150 μm ○ ○ △ △ Comparative Example 1 150 μm △ △ ○ △ Comparative Example 2 150 μm △ △ ○ △ Comparative Example 3 150 μm ○ △ ○ △ Comparative Example 4 150 μm △ △ ○ △ Comparative Example 5 150 μm × △ ○ × Comparative Example 6 150 μm △ △ ○ △

[0168] Referring to Table 8 above, no sagging, pinholes, or internal curing defects were observed in Example 1 under dry film thicknesses of 100 μm and 150 μm. When the dry film thickness was 200 μm, some sagging was observed, but it was at an acceptable level for actual use. Therefore, it was confirmed that the first composition of the present invention exhibits good workability even under thick film application conditions to integrate the functions of the undercoat and intermediate layers.

[0169] Comparative Example 5 contained an excessive amount of polyfunctional epoxy novolak resin and did not contain an organic solvent, which increased the viscosity of the composition and significantly increased sagging and leveling defects under 150 μm thick film coating conditions. Comparative Example 6 did not contain a reactive diluent, which reduced spray atomization and increased appearance defects.

[0170] When comparing the examples, Examples 1, 4, and 5, which contained 5% to 15% by weight of polyfunctional epoxy novolak resin, had superior thick film workability compared to Example 12, which contained 3% by weight of polyfunctional epoxy novolak resin. In addition, Examples 1, 6, and 7, which contained 3% to 8% by weight of reactive diluent, had superior internal curing properties compared to Example 13, which contained 12% by weight of reactive diluent.

[0171] [Evaluation Example 4] VOC and Coatability Evaluation

[0172] The VOC content was measured for the first composition of each example and comparative example. The VOC content was measured using KS M ISO 11890-2 or a method equivalent thereto.

[0173] In addition, the spray pattern, atomization properties, nozzle clogging, and film appearance were evaluated while applying the first composition using an airless spray method.

[0174] VOC and paintability were evaluated according to the following criteria and are shown in Table 9.

[0175] ○: VOC content is 300 g / L or less, and sprayability is good

[0176] △: VOC content exceeding 300 g / L and not exceeding 350 g / L, or partial deterioration in paintability observed

[0177] ×: VOC content exceeding 350 g / L or poor paintability

[0178] division VOC content Spray paintability Coating exterior evaluation Example 1 265 g / L Good Good ○ Example 2 267 g / L Good Good ○ Example 3 263 g / L Good Good ○ Example 4 282 g / L Good Good ○ Example 5 248 g / L Good Good ○ Example 6 292 g / L Good Good ○ Example 7 248 g / L Good Good ○ Example 8 265 g / L commonly Some defects △ Example 9 265 g / L commonly Some defects △ Example 10 270 g / L Good Good ○ Example 11 255 g / L commonly Some craters △ Example 12 286 g / L commonly Partial sagging △ Example 13 235 g / L Good Good ○ Comparative Example 1 330 g / L commonly Some orange peel △ Comparative Example 2 325 g / L commonly Some orange peel △ Comparative Example 3 268 g / L Good commonly ○ Comparative Example 4 268 g / L commonly Some defects △ Comparative Example 5 220 g / L error Leveling failure × Comparative Example 6 335 g / L commonly Some orange peel △

[0179] Referring to Table 9 above, Comparative Example 6, which does not contain a reactive diluent, had an increased amount of organic solvent to lower the paint viscosity under low VOC conditions, resulting in a VOC content exceeding 300 g / L. In addition, Comparative Example 1, in which both the multifunctional epoxy novolak resin and the silane component were omitted, and Comparative Example 2, in which the multifunctional epoxy novolak resin was omitted, also had a relatively increased amount of organic solvent, resulting in a VOC content exceeding 300 g / L.

[0180] On the other hand, Examples 1 to 7 all had VOC content of 300 g / L or less, and the sprayability and film appearance were also good. Therefore, it was confirmed that the first composition containing a reactive diluent can ensure paintability while reducing the volatile organic solvent content.

[0181] When comparing the examples, Example 6, with a reactive diluent content of 3 wt%, satisfied the regulatory standard with a VOC content of 292 g / L, while Example 7, with a reactive diluent content of 8 wt%, had a lower VOC content. However, when the reactive diluent is increased to 12 wt% as in Example 13, the VOC content may be lower, but as confirmed in Evaluation Examples 3 and 5, it was found that internal curability and adhesion after moisture resistance were reduced.

[0182] [Evaluation Example 5] Evaluation of Rust Resistance and Moisture Resistance

[0183] A first coating film was formed by directly applying the first composition of each example and comparative example to a bare metal steel specimen, and then a two-coating film system was formed by applying the second composition.

[0184] After curing the above coating specimens for 7 days under conditions of 20°C to 25°C and 50% to 60% relative humidity, they were exposed to salt spray tests and moisture resistance tests. The salt spray test was performed for 500 hours in accordance with KS D 9502 or ASTM B117. The moisture resistance test was performed for 500 hours under conditions of 40°C and 95% relative humidity.

[0185] After the test, rust formation, blistering, peeling, and adhesion retention rate were evaluated. The adhesion retention rate was calculated as the ratio of the pull-off adhesion strength after the test to the pull-off adhesion strength before the test.

[0186] Rust resistance and moisture resistance were evaluated according to the following criteria and are shown in Table 10.

[0187] ○: No rust, blisters, or peeling are substantially observed, and the adhesion retention rate is 80% or higher

[0188] △: Localized rust or blisters are observed, but are at an acceptable level for practical use.

[0189] ×: Occurrence of rust, blisters, or peeling over a large area

[0190] division Appearance after salt spray Appearance after moisture Adhesion retention rate evaluation Example 1 No rust or blisters Good 91% ○ Example 2 No rust or blisters Good 86% ○ Example 3 No rust or blisters Good 90% ○ Example 4 No micro-blisters Good 85% ○ Example 5 No rust or blisters Good 89% ○ Example 6 No rust or blisters Good 84% ○ Example 7 No rust micro-blister 82% ○ Example 8 Local blister Partial attachment degradation 70% △ Example 9 Local blister Partial attachment degradation 72% △ Example 10 Fine rust formation Some blisters 73% △ Example 11 No rust Some surface defects 84% △ Example 12 Fine rust formation Some blisters 76% △ Example 13 Local blister Partial peeling 70% △ Comparative Example 1 Localized rust formation Some blisters 58% × Comparative Example 2 Fine rust formation Some blisters 72% △ Comparative Example 3 Fine rust formation Some blisters 75% △ Comparative Example 4 Localized rust formation Some blisters 68% △ Comparative Example 5 Local blister Partial peeling 76% △ Comparative Example 6 Local blister Partial peeling 74% △

[0191] Referring to Table 10 above, Comparative Example 1, which does not contain both polyfunctional epoxy novolak resin and epoxy functional silane oligomer, showed localized rust and blisters after salt spraying, and the adhesion retention rate after moisture resistance was also low.

[0192] Comparative Examples 2 and 3 were improved compared to Comparative Example 1, but the corrosion resistance and moisture resistance retention rates were lower than those of Example 1. This suggests that corrosion resistance and moisture resistance can be more stably secured even under conditions where the primer layer is omitted, when the interfacial adhesion assisting effect of the epoxy-functional silane oligomer and the dense epoxy network formation effect of the polyfunctional epoxy novolak resin work together.

[0193] When comparing the examples, Examples 1 to 7 all showed an adhesion retention rate of 80% or more, and it was confirmed that the adhesion retention rate was relatively high compared to Example 8 using a low molecular weight silane oligomer, Example 9 using a high molecular weight silane oligomer, Example 10 with a silane oligomer content of 0.5 wt%, Example 12 with a multifunctional epoxy novolak resin content of 3 wt%, and Example 13 with a reactive diluent content of 12 wt%.

[0194] [Evaluation Example 6] Evaluation of interlayer adhesion between the first and second coatings

[0195] After forming a first coating film by directly applying the first composition to a steel specimen, the second composition was applied on the first coating film. The second composition was applied at recoating intervals of 8 hours, 24 hours, 72 hours, and 7 days after the formation of the first coating film.

[0196] After forming the second film, the entire film system was cured for 7 days under conditions of 20°C to 25°C and 50% to 60% relative humidity. Subsequently, cross-cut adhesion, pull-off adhesion strength, and failure location were evaluated.

[0197] Interlayer adhesion was evaluated according to the following criteria and is shown in Table 11.

[0198] ○: No peeling at the interface between Coat 1 and Coat 2

[0199] △: Partial delamination of the 1st and 2nd film interfaces

[0200] ×: Major delamination occurs at the interface between the first and second coatings

[0201] division Repainting interval Cross-cut Pull-off adhesion strength Destruction location Interlayer adhesion Example 1 8 hours 4B 4.2 MPa Cohesive failure within some of the first coating ○ Example 1 24 hours 5B 5.3 MPa Internal cohesive failure of the first film ○ Example 1 72 hours 5B 5.1 MPa Internal cohesive failure of the first film ○ Example 1 7 days 4B 4.0 MPa Partial destruction of the first / second film interface △ Comparative Example 1 24 hours 3B 3.0 MPa Breakdown of the first / second film interface △ Comparative Example 3 24 hours 3B 3.2 MPa Partial interface breakdown △ Comparative Example 6 24 hours 3B 3.1 MPa Partial interface breakdown △

[0202] Referring to Table 11 above, the first film of Example 1 had excellent interlayer adhesion with the second composition. In particular, when the second composition was applied at 24 and 72 hours after the formation of the first film, no delamination at the interface between the first film and the second film was observed, and mainly cohesive failure occurred within the first film.

[0203] On the other hand, in Comparative Examples 1, 3, and 6, some interfacial breakdown was observed even under 24-hour recoating conditions. This indicates that if the interfacial structure of the first film itself, film density, or film homogeneity due to the reactive diluent is insufficient, the interlayer adhesion with the second film may also be reduced.

[0204] [Evaluation Example 7] Low-temperature curability evaluation

[0205] Considering on-site construction conditions, curing properties were evaluated for some examples and comparative examples under conditions of 10°C and 60% relative humidity.

[0206] After mixing the main component and the hardener component of the first composition, the mixture was applied directly to a steel specimen. The surface condition was checked visually and by touch after 24 and 48 hours. Cross-cut adhesion was measured after 48 hours.

[0207] Low-temperature curability was evaluated according to the following criteria and is shown in Table 12.

[0208] ○: Touch dry within 48 hours, Cross-cut 4B or higher

[0209] △: Drying delay, but Cross-cut 3B or higher

[0210] ×: Surface adhesion, uncured, or cross-cut 2B or less

[0211] division Surface condition after 24 hours Surface condition after 48 hours Cross-cut Low-temperature curable Example 1 Touch dry Good 5B ○ Example 5 Touch dry Good 5B ○ Example 7 Some adhesive Good 4B ○ Example 8 Some adhesive commonly 3B △ Example 11 Some adhesive commonly 4B △ Example 13 Some adhesive Some adhesive 3B △ Comparative Example 1 Some adhesive Some adhesive 3B △ Comparative Example 5 Some adhesive commonly 4B △ Comparative Example 6 Some adhesive Some adhesive 3B △

[0212] Referring to Table 12 above, Example 1 became tack-dried within 48 hours even under 10°C conditions and demonstrated the adhesion of Cross-cut 5B. Examples 5 and 7 also showed good curing properties for actual use under low-temperature conditions.

[0213] On the other hand, Example 13 had an excessive amount of reactive diluent, so some surface adhesion remained under low-temperature conditions. Comparative Example 6 did not contain a reactive diluent, so the homogeneity of the coating film was reduced under low VOC conditions, and drying and curing properties were unfavorable under low-temperature conditions.

[0214] When comparing the examples, Examples 1, 6, and 7, which contained 3% to 8% by weight of reactive diluent, exhibited superior low-temperature curability and film surface condition compared to Example 13, which contained an excess amount of reactive diluent. Additionally, Example 1, in which the molecular weight of the silane oligomer was within a preferred range, exhibited superior adhesion under low-temperature conditions compared to Example 8, which used a low molecular weight silane oligomer.

[0215] The above descriptions are specific embodiments for carrying out the present disclosure. The present disclosure will include not only the embodiments described above, but also embodiments that can be simply modified or easily modified. Furthermore, the present disclosure will include technologies that can be easily modified and implemented using the embodiments described above. Accordingly, the scope of the present disclosure should not be limited to the embodiments described above, but should be defined by the claims set forth below as well as equivalents to the claims of the present disclosure.

Claims

Claim 1 A steel coating composition comprising a main component including a difunctional bisphenol A type epoxy resin; a polyfunctional epoxy novolak resin; an epoxy-functional silane oligomer; a reactive diluent; and an organic solvent, wherein the epoxy-functional silane oligomer comprises a structural unit represented by the following chemical formula 1. [Chemical Formula 1] X-[Si(R 1 )(OR 2 )-O]n-Si(R 3 )(OR 4 )-Y(In Chemical Formula 1, R 1 and R 3 Each is independently a C1 to C6 alkyl group or a C1 to C6 alkoxy group, and R 2 and R 4 Each is independently a C1 to C4 alkyl group, at least one of X and Y is an organic group comprising an epoxy group, a glycidoxy group, or an epoxycycloalkyl group, and n is an integer from 1 to 20). Claim 2 delete Claim 3 A steel coating composition according to claim 1, wherein the content of the epoxy functional silane oligomer is 0.1% to 5.0% by weight based on the total weight of the main component. Claim 4 In claim 1, the reactive diluent is a steel coating composition comprising an aliphatic glycidyl ether-based reactive diluent. Claim 5 A method for coating steel, comprising: preparing a steel surface; applying a first composition to the steel surface to form a first coating film; and applying a second composition onto the first coating film to form a second coating film; wherein applying the first composition comprises mixing a main component and a curing agent component, each comprising a difunctional bisphenol A type epoxy resin, a polyfunctional epoxy novolak resin, an epoxy functional silane oligomer, a reactive diluent, and an organic solvent, and applying the mixture directly onto the steel surface, wherein the epoxy functional silane oligomer comprises a structural unit represented by the following chemical formula 1. [Chemical Formula 1] X-[Si(R 1 )(OR 2 )-O]n-Si(R 3 )(OR 4 )-Y(In Chemical Formula 1, R 1 and R 3 Each is independently a C1 to C6 alkyl group or a C1 to C6 alkoxy group, and R 2 and R 4 Each is independently a C1 to C4 alkyl group, at least one of X and Y is an organic group comprising an epoxy group, a glycidoxy group, or an epoxycycloalkyl group, and n is an integer from 1 to 20).

Citation Information

Patent Citations

  • Epoxy-containing polysiloxane oligomer compositions, process for making same and uses thereof

    KR1020140116848A

  • Coated steel pipe with heterogeneous epoxy two-layer structure and manufacturing method thereof

    KR102763532B1

  • Two-component compositions based on blends of epoxide compounds

    JP2025530806A

  • Epoxy anticorrosive coating composition

    KR1020240131160A