Method for manufacturing electrode plates for lead-acid batteries using PEDOT
Coating lead-acid battery grids with PEDOT enhances interfacial adhesion and conductivity, addressing delamination and resistance issues, thereby extending electrode life and improving performance under demanding conditions.
Patent Information
- Application Number
- KR1020250052542
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-04-22
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2045-04-22
AI Technical Summary
Existing lead-acid batteries face issues with interfacial delamination and increased resistance due to repeated expansion and contraction of the active material, leading to decreased conductivity and shortened lifespan, especially under high-temperature or high-power conditions.
Coating the lead grid with poly(3,4-ethylenedioxythiophene) (PEDOT) through electrochemical polymerization to enhance interfacial adhesion and conductivity, utilizing π-π interactions and intermolecular interlocking effects.
Improves electrode lifespan and conductivity by stabilizing the active material, reducing internal resistance, and maintaining output stability under repeated charging and discharging cycles, while being environmentally friendly and compatible with existing manufacturing processes.
Smart Images

Figure 112025045737029-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for manufacturing an electrode plate for a lead-acid battery using PEDOT, and more specifically, to a method for manufacturing an electrode plate for a lead-acid battery using PEDOT (Poly(3,4-ethylenedioxythiophene)), a conductive polymer, to improve interfacial adhesion and electrical characteristics between the grid and the active material of a lead-acid battery. Background Technology
[0003] Lead-acid batteries are a representative secondary battery (electrochemical storage device) that has been commercialized since the late 19th century and is still widely used in various applications such as automotive starter batteries, industrial energy storage devices, and uninterruptible power supplies (UPS).
[0004] This battery is still considered an important energy storage technology due to its advantages, such as a relatively low price, high reliability, and stable power supply capability.
[0005] The basic structure of a lead-acid battery consists of forming electrode plates by coating an active material, such as lead oxide (PbO2) or lead sulfate (PbSO4), onto a grid made of conductive metal, and sealing this together with an aqueous sulfuric acid (H2SO4) electrolyte.
[0006] This structure enables repeated energy storage and release by causing lead-based materials to undergo electrochemical reactions through redox reactions during charging and returning to their original state during discharge.
[0007] However, as charge and discharge cycles are repeated, the active material within the electrode undergoes repeated expansion and contraction, and as a result, delamination is prone to occur at the interface between the grid and the active material.
[0008] In particular, the expansion of microscopic cracks or pores generated within the electrode gradually increases interfacial contact resistance, which hinders current flow and leads to a decrease in battery conductivity and output performance.
[0009] To address these issues, some existing technologies have applied supplementary measures, such as applying an adhesive binder to enhance adhesion between the active material and the grid, or mechanical surface treatment (increasing roughness) to form fine irregularities on the grid surface.
[0010] However, these technologies have the following fundamental limitations.
[0011] First, since binders are generally insulating polymers, they impede conductivity, and due to their low thermal and chemical stability, performance degradation is likely to occur under high-temperature operating conditions.
[0012] Second, while increasing surface roughness can improve mechanical adhesion to some extent, it does not directly contribute to the efficiency of interfacial electron transfer pathways, and its effectiveness tends to decrease during repeated charge-discharge processes.
[0013] Therefore, existing bonding technologies fail to fundamentally resolve issues such as active material delamination, increased internal resistance, and shortened lifespan that occur under high-temperature or high-power conditions, and there are limitations in ensuring long-term electrode stability and electrical reliability.
[0014] Ultimately, the present invention is proposed to solve the aforementioned problems. Prior art literature
[0015] Republic of Korea Published Patent No. 10-2015-0044634 The problem to be solved
[0016] Accordingly, the main objective of the present invention is to simultaneously solve the following technical and functional problems by coating the surface of a lead grid with poly(3,4-ethylenedioxythiophene) (PEDOT), a conductive polymer, through an electrochemical polymerization method.
[0017] First, we aim to provide a dramatic improvement in interfacial bonding strength.
[0018] In other words, PEDOT can simultaneously mechanically and chemically enhance the interfacial adhesion between the lead grid and the active material through π-π interactions and intermolecular interlocking effects.
[0019] This ensures that the active material remains stable without detaching from the interface, even if it expands or contracts during charging and discharging.
[0020] Second, it aims to provide the minimization of resistance in the electrical conduction path.
[0021] In other words, PEDOT inherently possesses excellent electron mobility (conductivity), and when formed on a grid surface, it expands the current flow path, substantially reducing the resistance of the interfacial conduction path.
[0022] This is a key factor in suppressing voltage drop during high-output discharge and improving energy efficiency during charging.
[0023] Third, we aim to simultaneously ensure electrode lifespan and output stability during repeated charging and discharging cycles.
[0024] In other words, the PEDOT coating layer prevents structural detachment of the active material while suppressing the increase in internal resistance, thereby substantially extending electrode life and maintaining output stability.
[0025] This was experimentally proven through results showing that a capacity retention rate of over 110% and structural stability of over 300 cycles were secured in C20 standard charge / discharge tests.
[0026] Ultimately, the objective of the present invention is to provide a high-performance electrode manufacturing technology that overcomes the structural and electrical limitations of existing lead-acid batteries and satisfies long-term durability, high-output capability, and manufacturing process compatibility. means of solving the problem
[0027] In order to achieve the problem that the present invention aims to solve,
[0028] A method for manufacturing an electrode plate for a lead-acid battery using PEDOT according to one embodiment of the present invention is,
[0029] A pretreatment step (S100) of acid-cleaning or ultrasonically cleaning a lead grid;
[0030] Electrochemical polymerization step (S200) of forming a PEDOT coating layer by immersing the grid in an electrolyte solution containing EDOT monomer and electrolyte, and then electrochemically polymerizing under a +1.2V constant potential condition;
[0031] A drying and post-treatment step (S300) in which the grid having the above-mentioned PEDOT coating layer is dried at 60 to 80°C to remove electrolyte residue and provide coating stability;
[0032] The method is characterized by including an active material coating and molding step (S400) in which an active material is applied to the above-mentioned PEDOT-coated grid, and the electrode plate is completed by roll pressing and drying.
[0033] At this time, the above PEDOT coating layer is,
[0034] It is characterized by being formed with a thickness of approximately 100 to 300 nm.
[0035] At this time, the above PEDOT coating layer is,
[0036] It is characterized by performing the function of enhancing interfacial adhesion with the active material through π-π interactions and inter-particle interlocking phenomena.
[0037] At this time, the electrode plate is,
[0038] It is characterized by the conductivity being improved from about 6.2×10⁴ S / m to 6.8×10⁴ S / m and the contact resistance being reduced by about 12% through the PEDOT coating layer. Effects of the invention
[0039] The method for manufacturing an electrode plate for a lead-acid battery using PEDOT according to the present invention provides the following remarkable effects.
[0040] First, it provides an extended electrode lifespan due to improved adhesion.
[0041] That is, the PEDOT polymer layer according to the present invention provides both mechanical bonding force and intermolecular π-π interaction at the interface between the lead grid and the active material, thereby effectively suppressing the detachment phenomenon despite the expansion and contraction stress that occurs during the repeated charging and discharging process of the active material.
[0042] As a result, the active material remains stable without detaching from the electrode plate, ensuring the structural stability of the electrode and significantly extending the charge / discharge cycle life.
[0043] This offers significant advantages in applications requiring long-term stability, such as industrial ESS and UPS systems.
[0044] Second, it provides improved conductivity and enhanced output stability.
[0045] In other words, PEDOT possesses excellent electron mobility due to its inherent conductive polymer properties, which reduces interfacial resistance and substantially lowers the internal electrical resistance of the entire electrode plate.
[0046] As a result, the voltage drop during charging is reduced, and voltage retention characteristics are improved even under high-output discharge conditions, thereby increasing the electrical efficiency of the battery.
[0047] Experimentally, it has been proven that the electrode plate manufactured in the present invention has an approximately 10% improvement in conductivity and a approximately 12% reduction in contact resistance compared to conventional electrodes, which leads to improved output stability and response speed of the entire battery system.
[0048] Third, it provides high compatibility with the manufacturing process.
[0049] In other words, since the PEDOT coating grows directly on the lead grid surface via electrochemical polymerization, it can be easily integrated into existing lead-acid battery manufacturing lines, and additional application is easy without the need for complex equipment modifications.
[0050] In addition, the coating thickness (100 to 300 nm) and polymerization time can be precisely controlled, providing versatility and flexibility that allow for adjustment and application to product families of various specifications.
[0051] This contributes to minimizing process costs and ensuring quality consistency within the lead-acid battery industry.
[0052] Fourth, it ensures eco-friendliness and improves corrosion resistance.
[0053] In other words, PEDOT is a non-toxic and environmentally friendly conductive polymer that can reduce the total amount of chemicals used in electrode manufacturing by replacing or reducing the use of conventional organic binders.
[0054] In addition, the PEDOT layer also plays a role in partially protecting the lead grid surface, thereby suppressing grid damage caused by oxidation and corrosion, and improving the long-term durability and environmental stability of the electrode.
[0055] This can be particularly advantageous for automotive batteries or industrial batteries operating in high-temperature and high-humidity environments.
[0056] As described above, the present invention provides a high-performance lead-acid battery electrode manufacturing technology that simultaneously improves mechanical stability, electrical efficiency, manufacturing compatibility, and environmental friendliness. Brief explanation of the drawing
[0057] FIG. 1 is a flowchart illustrating a method for manufacturing an electrode plate for a lead-acid battery using PEDOT according to an embodiment of the present invention. FIG. 2 is a cross-sectional view schematically illustrating the interface structure of a lead-acid battery electrode plate according to an embodiment of the present invention. FIG. 3 is a schematic cross-sectional view showing a structure in which the PEDOT-based electrode plates of the present invention are stacked in the upper and lower directions. Figure 4 is a schematic diagram structurally illustrating the interfacial bonding mechanism between the PEDOT polymer chain and the active material of the present invention. Figure 5 is a graph visualizing a quantitative comparison of electrode performance indicators based on whether the technology of the present invention is applied. Specific details for implementing the invention
[0058] The following description merely illustrates the principles of the present invention. Therefore, those skilled in the art may invent various devices that embody the principles of the present invention and are included within the concept and scope of the present invention, even though they are not explicitly described or illustrated in this specification.
[0059] Furthermore, all conditional terms and embodiments listed in this specification are, in principle, explicitly intended only for the purpose of enabling an understanding of the concept of the invention and should be understood not as being limited to the embodiments and conditions specifically listed as such.
[0060] A method for manufacturing an electrode plate for a lead-acid battery using PEDOT according to one embodiment of the present invention is,
[0061] It is characterized by improving the adhesion between the grid and the active material and reducing internal resistance by electrochemically polymerizing and coating the surface of a lead-acid battery grid with PEDOT (Poly(3,4-ethylenedioxythiophene)), a conductive polymer.
[0062] At this time, the electrochemical polymerization is performed for at least 10 minutes under a constant potential of +1.2V, and is characterized by having a coating thickness of 100 to 300 nm.
[0063] At this time, the electrolyte is characterized by using an acetonitrile-based solution containing LiClO4 or NaClO4.
[0064] At this time, the electrode plate is manufactured by applying an active material to a PEDOT-coated grid and performing roll pressing and drying processes.
[0065] At this time, it is possible to provide a lead-acid battery including an electrode plate for a lead-acid battery utilizing PEDOT manufactured through the above manufacturing method.
[0066] Meanwhile, the method for manufacturing an electrode plate for a lead-acid battery using PEDOT according to the present invention is,
[0067] A pretreatment step (S100) of acid-cleaning or ultrasonically cleaning a lead grid;
[0068] Electrochemical polymerization step (S200) of forming a PEDOT coating layer by immersing the grid in an electrolyte solution containing EDOT monomer and electrolyte, and then electrochemically polymerizing under a +1.2V constant potential condition;
[0069] A drying and post-treatment step (S300) in which the grid having the above-mentioned PEDOT coating layer is dried at 60 to 80°C to remove electrolyte residue and provide coating stability;
[0070] The method is characterized by including an active material coating and molding step (S400) in which an active material is applied to the above-mentioned PEDOT-coated grid, and the electrode plate is completed by roll pressing and drying.
[0071] At this time, the above PEDOT coating layer is,
[0072] It is characterized by being formed with a thickness of approximately 100 to 300 nm.
[0073] At this time, the above PEDOT coating layer is,
[0074] It is characterized by performing the function of enhancing interfacial adhesion with the active material through π-π interactions and inter-particle interlocking phenomena.
[0075] At this time, the electrode plate is,
[0076] It is characterized by the conductivity being improved from about 6.2×10⁴ S / m to 6.8×10⁴ S / m and the contact resistance being reduced by about 12% through the PEDOT coating layer.
[0077] Hereinafter, a method for manufacturing an electrode plate for a lead-acid battery using PEDOT according to the present invention will be explained in detail through an example.
[0078] FIG. 1 is a flowchart illustrating a method for manufacturing an electrode plate for a lead-acid battery using PEDOT according to an embodiment of the present invention.
[0079] As illustrated in FIG. 1, the method for manufacturing an electrode plate for a lead-acid battery using the above-mentioned PEDOT is as follows:
[0080] A pretreatment step (S100) of acid-cleaning or ultrasonically cleaning a lead grid;
[0081] Electrochemical polymerization step (S200) of forming a PEDOT coating layer by immersing the grid in an electrolyte solution containing EDOT monomer and electrolyte, and then electrochemically polymerizing under a +1.2V constant potential condition;
[0082] A drying and post-treatment step (S300) in which the grid having the above-mentioned PEDOT coating layer is dried at 60 to 80°C to remove electrolyte residue and provide coating stability;
[0083] The method is characterized by including an active material coating and molding step (S400) in which an active material is applied to the above-mentioned PEDOT-coated grid, and the electrode plate is completed by roll pressing and drying.
[0084] To explain in detail, the above pretreatment step (S100) is a step of acid-washing or ultrasonically cleaning the lead grid.
[0085] In other words, the lead grid is used as a conductive support, and surface activation treatment is required for a uniform coating of PEDOT polymer.
[0086] First, place the lead grid in an ultrasonic cleaner and wash it with deionized water for about 5 minutes to remove contaminants and fine dust from the surface.
[0087] Afterwards, acid washing is performed by immersing in a 5% hydrochloric acid (HCl) solution for 3 minutes to remove oxide film and surface impurities.
[0088] Through this process, the contact angle of the grid surface is lowered and hydrophilicity is enhanced, creating an environment where PEDOT monomers can be evenly coated.
[0089] The above electrochemical polymerization step (S200) is a step of forming a PEDOT coating layer by immersing the grid in an electrolyte solution containing EDOT monomer and electrolyte, and then electrochemically polymerizing it under a positive potential of +1.2V.
[0090] That is, the pretreated lead grid is used as the working electrode of an electrochemical cell to induce the polymerization of EDOT monomers.
[0091] At this time, the electrolyte solution consists of an acetonitrile (CH3CN)-based solvent containing 0.02 M EDOT and 40.1 M LiClO.
[0092] At this time, the electrochemical cell is configured in a three-electrode manner, and the counter electrode uses a platinum wire (Pt wire), and the reference electrode uses an Ag / AgCl electrode.
[0093] At this time, the potential control method is the constant potential electropolymerization method, and the reaction is carried out for 10 minutes by applying a voltage of +1.2V.
[0094] In this process, the PEDOT polymer grows uniformly on the lead grid surface, and a coating layer with a thickness of 100 to 300 nm is formed.
[0095] In addition, PEDOT polymers adhere strongly to the grid surface through π-π interactions and electrochemical bonding, providing conductivity and interfacial bonding strength simultaneously.
[0096] Afterwards, the drying and post-treatment step (S300) is a step of drying the grid on which the PEDOT coating layer is formed at 60 to 80°C to remove electrolyte residue and provide coating stability.
[0097] That is, first, air drying is performed at room temperature for about 10 minutes to naturally evaporate volatile solvents such as acetonitrile.
[0098] Afterwards, place in a drying oven at 60 to 80°C for about 1 hour to remove residual electrolytes and stabilize the arrangement of PEDOT polymer chains.
[0099] This step is essential for improving the heat resistance, moisture resistance, and chemical resistance of the PEDOT layer and preventing long-term performance degradation.
[0100] Subsequently, the active material coating and molding step (S400) is a step of applying an active material to a PEDOT-coated grid, and completing the electrode plate by roll pressing and drying.
[0101] In other words, the dried PEDOT-coated grid undergoes a final process of supporting the active material of the lead-acid battery electrode.
[0102] Specifically, the active material is composed in the form of a mixed slurry of PbO2 and PbSO4 and is evenly coated on the grid.
[0103] At this time, after application, the active material is compressed using a 2MPa roll pressing machine so that it adheres strongly to the grid and the PEDOT layer.
[0104] Afterward, the moisture is evaporated through a drying process, and the active material is fixed onto the electrode plate.
[0105] As a result, the completed electrode plate maintains the active material without detachment through the PEDOT layer, and improves structural stability and output characteristics even with repeated charging and discharging.
[0106] FIG. 2 is a cross-sectional view schematically illustrating the interface structure of a lead-acid battery electrode plate according to the present invention, showing a triple structure composed of a grid, a PEDOT coating layer, and an active material layer sequentially from the bottom.
[0107] To explain in detail, the aforementioned Grid is located at the bottom of the drawing and is a grid-shaped section, which is a conductive support made of lead (Pb) or a lead alloy (Pb-Ca-Sn).
[0108] This structure maintains the mechanical strength of the electrode plate while simultaneously serving as a conductor that allows current to flow.
[0109] In this case, the grid is identical to the existing technology, but the technical difference of the present invention is that the surface of the grid is coated with PEDOT.
[0110] In addition, the above PEDOT (coating layer) is an intermediate layer, an area depicted as a dot pattern or a uniform pattern in the drawing, and is a conductive thin film composed of a Poly(3,4-ethylenedioxythiophene) polymer.
[0111] At this time, the PEDOT layer is formed directly on the grid surface by electrochemical polymerization, and is formed very thinly and uniformly with a thickness of about 100 to 300 nm.
[0112] The above-mentioned PEDOT layer performs the following functions.
[0113] First, it provides enhanced adhesion between the grid and the active material.
[0114] Second, it provides an effect of improving conductivity due to improved electron mobility.
[0115] Third, it provides mechanical stability to the electrode structure.
[0116] Also, regarding the active material mentioned above, the part depicted as irregular oval particles at the top of the drawing is a lead-based active material (lead oxide PbO2 or lead sulfate PbSO4, etc.).
[0117] The above active material performs the core function of storing or releasing energy through charge and discharge reactions.
[0118] In the present invention, this active material layer is in direct contact with the PEDOT coating layer, and the adhesion of the active material is increased due to the π-π interaction and surface interference (interlocking effect) of the PEDOT molecules, and has an effect of preventing detachment during repeated charging and discharging.
[0119] Meanwhile, the meaning of interface structure will be explained below.
[0120] Figure 1 above is a drawing that emphasizes the functional interaction between each layer, rather than a simple stacked structure.
[0121] In other words, while conventional methods only achieved indirect adhesion between the grid and the active material through the application of binders or roughness, this structure dramatically improves electrode performance by simultaneously providing conductivity and adhesion through the use of PEDOT.
[0122] In addition, thanks to the flexibility of PEDOT, interfacial delamination is suppressed even with respect to volume changes (expansion / contraction) that occur during charging and discharging.
[0123] In summary, Figure 1 shows the multilayer interface configuration of the Grid-PEDOT-Active material, which is the core structure of the present invention, and visually explains how each layer interacts electrically and mechanically. This interface structure serves as the technical basis for realizing major performance improvements, such as extending electrode life, reducing internal resistance, and enhancing active material retention.
[0124] FIG. 3 is a schematic cross-sectional view showing the structure of the PEDOT-based electrode plates of the present invention stacked in the upper and lower directions, and FIG. 3 visually shows what components the lead-acid battery electrode plates are made of and how the physical and functional relationships between them are established.
[0125] In the case of the above-mentioned electrode plate, the overall structure constitutes a single electrode plate for a lead-acid battery, and is labeled 'Electrode plate' at the top of the drawing.
[0126] The above electrode plate consists of a lower grid, a middle PEDOT coating layer, and an upper active material.
[0127] In this case, the Grid is a part depicted in a grid shape at the bottom of the drawing, and is a metal support composed of lead or a lead alloy (Pb-Ca-Sn).
[0128] The above grid functions as a primary path for transmitting current, along with ensuring the mechanical strength of the electrode plate.
[0129] And, in the case of the above PEDOT coating (coating layer), the dot pattern layer formed thinly on the grid is the PEDOT conductive polymer layer.
[0130] This layer is formed by electrochemically polymerizing EDOT monomers, and has an average thickness of about 100 to 300 nm.
[0131] In addition, the PEDOT coating improves the electrical conductivity of the electrode while simultaneously acting as an electron transport layer that allows the active material to make direct contact.
[0132] In addition, the adhesion to the active material is dramatically improved through the π-π interactions and intermolecular interlocking structure of the PEDOT molecule.
[0133] And, the above active material (active material layer) is the active material, which is the core reactive material of a lead-acid battery.
[0134] The active material is composed of lead-based compounds such as PbO₂ or PbSO₄, and stores and releases energy through charge and discharge reactions.
[0135] These particles come into direct contact with the PEDOT layer, and thanks to the interfacial bonding force provided by PEDOT, they remain stably fixed without easily detaching during charging and discharging.
[0136] Meanwhile, while existing technologies maintained adhesion by adding binders or relying solely on surface roughness, the present invention is differentiated in that PEDOT provides both structural and chemical bonding simultaneously.
[0137] In addition, Figure 3 illustrates the electrical flow and mechanical bonding mechanism within the electrode through an upper and lower stacked structure. In particular, the PEDOT layer functions not merely as a simple buffer but as a conductive interface material and an adhesive medium, which is a structure capable of effectively solving the chronic problems of active material delamination and increased contact resistance in conventional lead-acid batteries.
[0138] And, FIG. 4 is a schematic diagram structurally illustrating the interfacial bonding mechanism between the PEDOT polymer chain and the active material, which is a key technical element of the present invention.
[0139] Figure 4 above visually illustrates electronic interactions (π-π interaction) and mechanical interlocking effects occurring at the molecular level simultaneously.
[0140] Specifically, the chain structure located in the center of the diagram is a PEDOT (Poly(3,4-ethylenedioxythiophene)) polymer.
[0141] In other words, the PEDOT chain is a conductive polymer consisting of repeating benzene rings (hexagonal structure) and thiophene rings (pentagonal, including S), exhibiting excellent electron mobility and high stability.
[0142] This structure has a π-electron cloud and can induce non-covalent bonding (π-π interaction) with adjacent materials.
[0143] In this case, regarding the above π-π interaction, specifically, the "π-π interaction" indicated at the top center of the PEDOT chain refers to the non-covalent electron interaction between PEDOT and the active material.
[0144] That is, a chemically strong adsorbent bond is formed by the interaction between the electron-packed structure present on the surface of the active material (e.g., the bond shell structure within the PbO₂ particle) and the π electrons of the PEDOT chain.
[0145] As a result, the active material adheres to the PEDOT coating layer and remains firmly in place without detaching during charging and discharging.
[0146] Also, to explain the interlocking (mechanical coupling effect), the "active material" is indicated by a dotted oval on both sides of the drawing, and an arrow connected to the PEDOT chain inside is labeled "Interlocking."
[0147] This means that the flexible chain structure of PEDOT forms a structure in which it is partially physically fitted into or encases the micro-irregularities and crevices of the active material particles.
[0148] This physical interlocking serves to structurally fix the active material so that it does not detach even if it expands and contracts during charging and discharging.
[0149] In addition, to explain the complexity of interfacial bonding, it was shown that PEDOT is a foundational structure that goes beyond a simple conductive layer and simultaneously implements two mechanisms—chemical adhesion (π-π interaction) and mechanical fixation (interlocking)—thereby improving the interfacial stability, charge / discharge durability, conductivity, and output stability of the electrode plate.
[0150] In conclusion, Figure 4 structurally explains the fact that the key principle leading to the improvement of the physical properties of the electrode plate is attributed to the molecular structure of PEDOT and the interfacial action mechanism.
[0151] And, Fig. 5 is a graph visualizing a quantitative comparison of electrode performance indicators according to whether the technology of the present invention is applied.
[0152] The left side shows a comparison of electrode conductivity, and the right side shows a comparison of contact resistance.
[0153] The performance improvement effect of the present invention is intuitively explained by showing the case without PEDOT coating (Without PEDOT) and the case with PEDOT coating (With PEDOT) side by side.
[0154] First, regarding Electrode Conductivity, the graph on the left is a comparison of the electrical conductivity of the electrodes.
[0155] Under the 'Without PEDOT' condition, conductivity is shown to be relatively low, while under the 'With PEDOT' condition, conductivity is visualized to be improved by more than 10%.
[0156] In other words, the upward arrow (↑) emphasizes that the application of the PEDOT coating enhances electron mobility, thereby forming a more efficient conduction path.
[0157] This is consistent with the figures measured in actual experiments, for example, as follows.
[0158] - Existing grid: approx. 6.2 × 10⁴ S / m
[0159] - PEDOT coating grid: approx. 6.8 × 10⁴ S / m
[0160] Second, regarding contact resistance, the graph on the right compares the contact resistance between the active material and the grid.
[0161] Under 'Without PEDOT' conditions, contact resistance is relatively high, while under 'With PEDOT' conditions, it shows a significantly reduced value.
[0162] At this time, the downward arrow (↓) highlights that the contact resistance was reduced by about 12% due to the improvement in interfacial bonding strength (π-π interaction and interlocking) by the PEDOT coating.
[0163] In this case, a reduction in contact resistance means that charge and discharge efficiency increases and output loss decreases.
[0164] This drawing serves as a document to demonstrate, based on data, the quantitative performance improvement effect provided by the PEDOT electrochemical polymerization coating to lead-acid battery electrode plates. It goes beyond a simple structural description and visually expresses the technical effect, enabling examiners or technology users to intuitively understand the practical value of the performance improvement.
[0165] Furthermore, drawings serve as key evidence that can be used for comparative analysis with other technologies, and act as a factor that strengthens the inventive step and industrial applicability of a patent.
[0166] In summary, Figure 5 is a technical diagram that demonstrates, through numerical visual data, the fact that the PEDOT technology of the present invention improves conductivity and reduces contact resistance, thereby simultaneously improving the efficiency and lifespan of the battery.
[0167] Meanwhile, Example 1 is a process of PEDOT coating a lead grid.
[0168] That is, the lead grid (thickness 0.8 mm) is ultrasonically cleaned and then acid-washed with a 5% HCl solution for 3 minutes to activate the surface.
[0169] Afterwards, the grid is immersed in an acetonitrile solution containing 0.02M EDOT and 0.1M LiClO4, and then an electrochemical cell is constructed.
[0170] Afterwards, the working electrode (grid), reference electrode (Ag / AgCl), and counter electrode (Pt) are configured and maintained at a constant potential of +1.2V for 10 minutes.
[0171] Afterwards, the coated grid is air-dried at room temperature for 10 minutes, and then dried at 70℃ for 1 hour.
[0172] And, in the case of Example 2, the electrode plate manufacturing and performance comparison are as follows.
[0173] First, an active material (PbO2+PbSO4 mixed slurry) is applied onto a coated grid, and 2 MPa roll pressing is performed.
[0174] Afterward, following drying and molding, charge and discharge tests are conducted under the same conditions as commercial lead-acid batteries.
[0175] Subsequently, as a result of the C20 cycle test, the PEDOT-coated electrode showed a capacity retention rate of over 110% and was confirmed to have minimal structural damage even after 300 cycles.
[0176] Meanwhile, the PEDOT coating layer is,
[0177] It is characterized by being formed with a thickness of approximately 100 to 300 nm.
[0178] Specifically, it is intended to ensure a balance between conductivity and interfacial adhesion.
[0179] In other words, PEDOT is an inherently conductive polymer, and requires a certain thickness to secure electron transport pathways.
[0180] However, if the thickness increases excessively, the internal resistance of the electrode increases and the possibility of mechanical delamination increases.
[0181] The range of 100 to 300 nm set in the present invention effectively supports electron flow and secures interfacial conductivity when the minimum thickness (100 nm) or greater, and allows for the maintenance of mechanical flexibility and adhesion during the active material coating and roll pressing processes when the maximum thickness (300 nm) or less.
[0182] In other words, the above range is the optimal range for ensuring conductivity and mechanical stability.
[0183] In addition, it is intended for the optimization of interface π-π interactions and interlocking.
[0184] That is, the π-electron cloud of PEDOT forms non-covalent bonds (π-π interaction) between the active material particles (PbO2, PbSO4) and molecules, thereby strengthening adhesion.
[0185] In this bonding, the adhesion is weak in layers that are too thin (less than 100 nm) due to insufficient electron distribution, and in layers that are too thick (more than 300 nm), PEDOT itself can hinder physical interference with the active material.
[0186] Therefore, 100 to 300 nm is an effective thickness range in which the molecular chains of PEDOT can mechanically interlock with the surface irregularities of the active material.
[0187] In addition, it is a standard value for ensuring thermal / chemical stability.
[0188] In other words, although PEDOT can deteriorate or oxidize at high temperatures, it has high stability due to the short thermal conduction path at a thickness of 100 to 300 nm.
[0189] In this case, if the process remains within this range during subsequent processes (drying, active material coating), there is almost no deformation, and heat resistance and moisture resistance are maintained.
[0190] In summary, the above range is significant as a critical optimal range that maximizes the conductivity and interfacial adhesion properties of PEDOT while also ensuring mechanical flexibility, manufacturing process applicability, and structural stability.
[0191] According to the present invention, the PEDOT polymer layer according to the present invention provides both mechanical bonding force and intermolecular π-π interaction at the interface between the lead grid and the active material, thereby effectively suppressing the detachment phenomenon despite the expansion and contraction stress that occurs during the repeated charging and discharging process of the active material.
[0192] As a result, the active material remains stable without detaching from the electrode plate, ensuring the structural stability of the electrode and significantly extending the charge / discharge cycle life.
[0193] Those skilled in the art to which the present invention pertains will understand that the present invention, as described above, may be implemented in other specific forms without altering the technical concept or essential features of the invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.
[0194] The scope of the present invention is defined by the claims set forth below rather than by the detailed description above, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of the present invention. Explanation of the symbols
[0195] S100: Preprocessing step S200: Electrochemical polymerization step S300: Drying and post-processing stage S400: Active material coating and molding step
Claims
Claim 1 A method for manufacturing an electrode plate for a lead-acid battery using PEDOT, characterized by electrochemically polymerizing and coating the surface of a lead-acid battery grid with PEDOT (Poly(3,4-ethylenedioxythiophene)), a conductive polymer, thereby improving adhesion between the grid and the active material and reducing internal resistance. Claim 2 A method for manufacturing an electrode plate for a lead-acid battery using PEDOT, characterized in that, in claim 1, the electrochemical polymerization is performed for at least 10 minutes under a constant potential condition of +1.2V, and the coating thickness is 100 to 300 nm. Claim 3 A method for manufacturing an electrode plate for a lead-acid battery using PEDOT, characterized in that, in claim 1, an active material is applied to a PEDOT-coated grid and a roll pressing and drying process is performed to manufacture the electrode plate. Claim 4 A lead-acid battery comprising an electrode plate for a lead-acid battery utilizing PEDOT according to any one of claims 1 to 3. Claim 5 delete
Citation Information
Patent Citations
Hot air heater
JP1994313621A
Lithium secondary battery having excellent stability against overcharge
KR1020130123492A
Negative electrode for secondary battery and secondary battery comprising the same
KR1020170006693A
Electrode for secondary cell and secondary cell including the same
KR1020240025393A
Manufacturing method for electrode plate for lead-acid battery using conductive graphene hydrogel
KR1020250018813A