Method and apparatus for joining different materials

Laser-based bonding of dissimilar materials, enhanced by surface treatment, addresses bonding strength and appearance issues, offering strong and deformity-free joins with improved process efficiency.

KR103045764B1Active Publication Date: 2026-11-06LG CHEM LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020210113531
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-26
Publication Date
2026-11-06
Estimated Expiration
2041-08-26

AI Technical Summary

Technical Problem

Existing methods for joining dissimilar materials such as metal and resin face challenges with bonding strength, appearance quality, and process complexity, including defects, insufficient bonding, and deformation issues.

Method used

A method involving laser irradiation on the outer surface of a metal member to melt and bond a resin member, with optional surface treatment of the metal member to create irregularities or micro-protrusions, enhancing bonding strength and appearance quality.

Benefits of technology

Secures strong, consistent bonding between dissimilar materials with improved processability and appearance quality, reducing the need for additional fastening components and minimizing deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112021099043181-PAT00001_ABST
    Figure 112021099043181-PAT00001_ABST
Patent Text Reader

Abstract

The present invention discloses a method for joining dissimilar materials having excellent bonding strength and appearance quality. A method for joining dissimilar materials according to one aspect of the present invention comprises the steps of: preparing a resin member and a metal member; laminating the resin member and the metal member; and irradiating a laser onto the outer surface of the metal member laminated in the lamination step to join the resin member and the metal member.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to bonding technology, and more specifically, to a method and apparatus for bonding dissimilar materials using a laser. Background Technology

[0002] Typically, there are many cases where it is necessary to join dissimilar materials, such as metal and resin materials. In particular, the use and joining of such dissimilar materials are widely employed to achieve product weight reduction and material cost savings while securing a certain level of mechanical strength. However, there are aspects where joining is not easy when using such dissimilar materials.

[0003] A typical method for joining such dissimilar materials involves the use of adhesives, such as acrylic or urethane-based adhesives. However, this method of joining using adhesives carries a high risk of defects occurring during the application or curing process, and is also significantly affected by factors such as the operator's skill level. Furthermore, this method presents the problem of insufficient bonding strength.

[0004] Accordingly, to increase bonding strength, a hybrid bonding method is sometimes used, which secures bonding force by utilizing additional fastening components such as bolts in addition to adhesives. However, this hybrid bonding method increases the number of work processes and carries a risk of breakage during the bolting process. Furthermore, there is a need to secure bolting space within the product, and there are also issues regarding reduced appearance quality.

[0005] In addition, as another example of a bonding method for dissimilar materials, ultrasonic bonding technology can be cited. However, in the case of such ultrasonic bonding technology, it is difficult to secure sufficient bonding strength, and problems may arise regarding the appearance quality of the bonded part. Furthermore, in the case of ultrasonic bonding technology, a horn and anvil are used, and there is a high possibility that the resin will be constricted in the horn or anvil. As background technology, the invention disclosed in Korean Patent Publication No. 10-2018-0036574 (April 9, 2018) is known. The problem to be solved

[0006] Accordingly, the present invention was devised to solve the above-mentioned problems and aims to provide a method and apparatus for joining dissimilar materials with excellent bonding strength and appearance quality.

[0007] Other objects and advantages of the present invention may be understood from the following description and will become more clearly apparent from the embodiments of the present invention. Furthermore, it will be readily apparent that the objects and advantages of the present invention can be realized by the means and combinations thereof set forth in the claims. means of solving the problem

[0008] A method for joining heterogeneous materials according to one aspect of the present invention for achieving the above-mentioned purpose comprises the steps of: preparing a resin member and a metal member; laminating the resin member and the metal member; and irradiating a laser onto the outer surface of the metal member laminated in the lamination step to join the resin member and the metal member.

[0009] Here, the bonding step can be performed such that the resin member is melted by heat conducted through the metal member and bonded to the surface of the metal member.

[0010] In addition, the heterogeneous material joining method according to the present invention may further include a step of surface treating the joining surface of the metal member so as to form irregularities on the joining surface of the metal member prior to the lamination step.

[0011] In addition, the surface treatment step may be performed in such a way that two or more surface treatment lines in different directions intersect.

[0012] Additionally, the surface treatment step may be performed to form one or more of a groove and a burr on the bonding surface of the metal member.

[0013] In addition, the surface treatment step may be performed to form micro-protrusions of 1 µm or less in size on the bonding surface of the metal member.

[0014] In addition, the metal member prepared in the above preparation step may contain aluminum.

[0015] In addition, the metal member prepared in the above preparation step may have a ten-point average roughness of 6 µm or less.

[0016] In addition, the metal member prepared in the above preparation step may have a reflectance of 20% to 70% with respect to a light source with a wavelength of 900 nm to 1100 nm.

[0017] In addition, a heterogeneous material bonding device according to another aspect of the present invention for achieving the above-mentioned purpose comprises: a lamination unit configured to laminate a resin member and a metal member; and a bonding unit configured to bond the resin member and the metal member by irradiating a laser onto the outer surface of the metal member laminated by the lamination unit. Effects of the invention

[0018] According to one aspect of the present invention, sufficient bonding strength can be secured when bonding dissimilar materials, particularly resin and metal. Therefore, an appropriate combination of resin material and metal material is possible, which can be advantageous for weight reduction or cost reduction.

[0019] Furthermore, according to one aspect of the present invention, superior bonding strength can be secured compared to bonding methods using adhesives or ultrasound.

[0020] In addition, according to one aspect of the present invention, consistency of bonding strength can be easily ensured.

[0021] In addition, according to one aspect of the present invention, the deformation of the exterior is not significant, so the exterior quality of the product can be excellent.

[0022] Furthermore, according to one aspect of the present invention, a laser may be irradiated onto a metal member instead of a resin member. Therefore, the resin member does not need to be limited to a material or shape that allows for the transmission of the laser. Accordingly, in this case, the expandability of the type or shape of the resin member can be increased.

[0023] In particular, the present invention provides a bonding technology between dissimilar materials having excellent processability and bonding properties for structures or materials that are structurally difficult to fuse, such as vehicle parts, such as component structures of ADAS (Advanced Driver Assistance Systems) modules or camera component structures.

[0024] In addition, the present invention can achieve various additional effects in various embodiments, and such effects are described in each embodiment, or detailed descriptions of effects that can be clearly understood by those skilled in the art from the configuration are omitted. Brief explanation of the drawing

[0025] The following drawings attached to this specification illustrate preferred embodiments of the present invention and serve to further enhance understanding of the technical concept of the present invention together with the detailed description of the invention provided below; therefore, the present invention should not be interpreted as being limited only to the matters described in such drawings. FIG. 1 is a flowchart schematically illustrating a heterogeneous material joining method according to one embodiment of the present invention. FIG. 2 is a perspective view schematically showing a bonding configuration between dissimilar materials according to one embodiment of the present invention. Figure 3 is a cross-sectional view along the line A1-A1' of Figure 2. FIG. 4 is a flowchart schematically illustrating the configuration of a heterogeneous material joining method according to another embodiment of the present invention. FIG. 5 is a diagram schematically showing the surface treatment configuration of a metal member according to one embodiment of the present invention. FIG. 6 is a diagram illustrating an example of a surface-treated configuration of a metal member in a heterogeneous material joining method according to another embodiment of the present invention. FIG. 7 is a diagram illustrating an example of a surface-treated configuration of a metal member in a heterogeneous material joining method according to another embodiment of the present invention. FIG. 8 is a block diagram schematically showing the configuration of a heterogeneous material joining device according to one embodiment of the present invention. FIG. 9 is a graph showing a comparison of bonding strengths for various embodiments and comparative examples of the present invention. FIG. 10 is a table showing the results of bonding strength measurements according to various other embodiments of the present invention. Figure 11 is a graph illustrating the measurement results of Figure 10. FIG. 12 is a cross-sectional image showing an enlarged view of the configuration in which the bonding surface of the metal plate before fusion is surface-treated in Example 5 of the present invention. FIG. 13 is an enlarged cross-sectional image showing the configuration in which the bonding surface of the metal plate before fusion is surface-treated in Example 12 of the present invention. FIGS. 14 and 15 are cross-sectional images showing an enlarged view of the bonded surface after fusion for embodiments 5 and 6 of the present invention. FIG. 16 is a cross-sectional image showing an enlarged view of the bonding surface after fusion for Example 12 of the present invention. FIGS. 17 and 18 are graphs showing a comparison of the reflectance and absorption of the metal material of Example 4 of the present invention and the metal material of Example 8. FIG. 19 is a partial enlarged image of the configuration in which the surface-treated joint surface of the metal plate before fusion in Example 8 of the present invention is viewed from the front. FIG. 20 is a partial enlarged image of the configuration in which the surface-treated joint surface of the metal plate before fusion in Example 4 of the present invention is viewed from the front. FIG. 21 is a graph showing a relative comparison of bonding strengths according to various embodiments of the present invention. Specific details for implementing the invention

[0026] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. Prior to this, terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, and should be interpreted in a meaning and concept consistent with the technical spirit of the present invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0027] Therefore, the embodiments described in this specification and the configurations illustrated in the drawings are merely the most preferred embodiments of the present invention and do not represent all of the technical ideas of the present invention; thus, it should be understood that various equivalents and modifications that can replace them may exist at the time of filing this application.

[0028] In this specification, terms indicating directions such as up, down, left, right, front, and back may be used; however, these terms indicate relative positions and are used merely for convenience of explanation, and it is obvious to those skilled in the art that they may vary depending on the position of the object or the position of the observer.

[0030] FIG. 1 is a flowchart schematically illustrating a heterogeneous material joining method according to one embodiment of the present invention.

[0031] Referring to FIG. 1, the heterogeneous material joining method according to the present invention includes a preparation step (S110), a stacking step (S120), and a joining step (S130).

[0032] The above preparation step (S110) is a step of preparing heterogeneous materials to be bonded. In particular, in the case of the present invention, a resin member and a metal member may be used as heterogeneous materials. Accordingly, the above preparation step (S110) may be a step of preparing a resin member and a metal member. For example, in the preparation step (S110), a resin plate (plastic plate) and a metal plate may be prepared as bonding targets. However, the present invention is not necessarily limited to such forms of heterogeneous materials.

[0033] The above lamination step (S120) is a step of laminating heterogeneous materials to be bonded. In particular, in the case of the present invention, in this lamination step (S120), a resin member and a metal member can be laminated together. For example, in the lamination step (S120), a resin member and a metal member can be laminated in an up-and-down direction.

[0034] In the above lamination step (S120), the dissimilar materials may come into contact with each other in a surface contact form such that the surfaces of the dissimilar materials come into contact with each other. For example, in the lamination step (S120), the resin plate and the metal plate may be laminated so that an overlapping portion is formed by at least partially making surface contact in the vertical direction. In particular, when the resin plate is located at the bottom and the metal plate is located at the top, the resin plate and the metal plate may be partially laminated together in a form where a portion of the upper surface of the resin plate and a portion of the lower surface of the metal plate come into contact with each other, thereby forming an overlapping portion.

[0035] The bonding step (S130) is a step of bonding the heterogeneous materials prepared and laminated in steps S110 and S120. In particular, in the case of the present invention, since a resin member and a metal member may be used as heterogeneous materials, the bonding step (S130) in this case may be a step of bonding the resin member and the metal member to each other. This bonding step (S130) will be explained in more detail with reference to FIGS. 2 and FIGS. 3.

[0036] FIG. 2 is a perspective view schematically showing a bonding configuration between dissimilar materials according to one embodiment of the present invention, and FIG. 3 is a cross-sectional view along the line A1-A1' of FIG. 2.

[0037] Referring to FIGS. 2 and 3, the bonding step (S130) may involve irradiating a laser, as indicated by L, to bond dissimilar materials, specifically a resin member, as indicated by P, and a metal member, as indicated by M. Furthermore, in the bonding step (S130), the laser (L) may be irradiated onto the outer surface of the metal member (M). Here, the outer surface of the metal member (M) may be interpreted as the surface opposite to the bonding surface that is bonded to the resin member (P) in the metal member (M).

[0038] For example, as illustrated in FIGS. 2 and 3, when a resin plate (P) is positioned at the bottom and a metal plate (M) is positioned at the top and joined together, the joining surface of the metal plate (M) can be said to be the bottom surface and the outer surface the top surface. In this case, a laser (L) can be irradiated onto the top surface of the metal plate (M). Additionally, in step S130, the laser (L) can be irradiated while moving horizontally along the top surface of the metal plate (M) as indicated by arrow A2 in FIG. 2.

[0039] In such a bonding configuration, the bond can be formed at the interface between the resin member and the metal member. For example, in the case of the embodiment of FIGS. 2 and FIGS. 3, the bond formed by laser irradiation can be formed as a welded part at the interface between the metal plate (M) and the resin plate (P), that is, the lower surface of the metal plate and the upper surface of the resin plate, as indicated by the part marked W.

[0040] As another example, in a case where a resin plate is positioned on the left and a metal plate on the right and are joined together, the outer surface of the metal plate is the right surface. In this case, a laser can be irradiated onto the right surface of the metal plate from the right to the left. In this case, a joint can be formed on the left surface of the metal plate.

[0041] According to this embodiment of the present invention, excellent bonding strength can be secured for the joining of dissimilar materials. Furthermore, according to this embodiment of the present invention, there is no need to perform additional joining configurations such as bolting. Therefore, excellent processability and economic efficiency regarding the joining of dissimilar materials can be achieved. Moreover, in the case of the present invention, watertightness or sealing performance can be improved due to the excellent bonding strength.

[0042] In addition, according to the above embodiment of the present invention, it can be said that the laser is irradiated to the metal side rather than the resin side. Also, the bonding portion may be formed on the bonding surface of the metal member.

[0043] Therefore, in this case, a laser-based bonding process can be implemented without being significantly affected by the shape or type of the resin member. In particular, according to the above embodiment, bonding can be performed with respect to the resin member without significant consideration of the laser transmission characteristics. That is, according to the above configuration of the present invention, since the laser does not need to pass through the resin member, the resin member does not need to be limited to a material capable of transmitting the laser above a certain level. Furthermore, if a laser is irradiated from the side of the resin member, and the transmittance of the resin member does not exceed a certain level, the laser output needs to be increased to ensure sufficient bonding. However, even in this case, not only may high bonding performance not be secured, but the surface of the resin member to which the laser is irradiated may also be damaged or deformed. However, according to the above embodiment of the present invention, since the laser is not irradiated from the side of the resin member, such limitations or problems may not occur. Therefore, the resin member to which the bonding method according to the present invention is applied may include various resin materials known at the time of filing the present invention.

[0044] In addition, according to the above embodiment, since the laser does not need to pass through the resin member, bonding can be performed regardless of the thickness of the resin member. In particular, in the above embodiment, there is no need to make the thickness of the resin member thin below a certain level.

[0045] In addition, according to the above embodiment, significant deformation may not occur in the appearance of the product, particularly in the appearance of the resin side. Therefore, in this case, excellent appearance quality can be ensured for a product that includes a configuration of mutual bonding between dissimilar materials.

[0046] Unlike the present invention, in the case of a bonding method using ultrasound, the bonding strength is weaker compared to a bonding method using a laser such as the present invention, and a problem may occur where the resin layer is constricted by a horn or anvil. Furthermore, such resin constriction can deform the outer surface of the resin layer. However, according to the present invention, problems such as deformation caused by such resin constriction may not occur.

[0047] The bonding step (S130) above can be performed in a manner such that the resin member (P) is melted and bonded to the surface of the metal member (M). At this time, the melting of the resin member can be achieved by heat conducted through the metal member. That is, in the bonding step (S130), a laser can be applied to the metal member side to supply heat to the metal member. Then, the heat supplied in this way can move from the outer surface of the metal member to the bonding surface side of the metal member by a heat conduction method. Here, since the resin member exists in a state of contact with the bonding surface side of the metal member, the resin member can be heated by the heat conducted from the metal member and at least partially melted. Then, the resin member melted in this way is attached to the bonding surface of the metal member, and the fusion of the resin member and the metal member can be achieved.

[0048] For example, in the embodiment of FIG. 3, a metal member (M) and a resin member (P) are sequentially stacked from top to bottom, and a laser can be irradiated from the upper side of the metal member (M) toward the metal member (M). At this time, heat from the laser can be conducted from the upper surface to the lower surface through the metal member (M). Then, the heat conducted in this way can melt the upper surface, which is the bonding surface of the resin member (P), to form a fused portion.

[0049] In this regard, the bonding of the resin member and the metal member can be said to be achieved by a thermal conduction fusion method.

[0050] Meanwhile, the laser (joining laser) irradiated in the joining step (S130) may have a wavelength range of 350 nm to 1200 nm. Additionally, the laser irradiated in the joining step (S130) may have a line energy of 60 J / mm to 300 J / mm. Here, line energy may refer to the energy used when irradiating once with a laser in a single line pattern. In particular, the laser irradiated in the joining step (S130) may have a line energy of 85 J / mm to 150 J / mm.

[0051] FIG. 4 is a flowchart schematically illustrating the configuration of a heterogeneous material joining method according to another embodiment of the present invention.

[0052] Referring to FIG. 4, the heterogeneous material joining method according to the present invention may further include a surface treatment step (S220) in addition to the preparation step (S210), stacking step (S230), and joining step (S240) as described in FIG. 1. Since the preparation step (S210), stacking step (S230), and joining step (S240) of FIG. 4 can be said to be similar to the preparation step (S110), stacking step (S120), and joining step (S130) of FIG. 1, a detailed description thereof is omitted.

[0053] The surface treatment step (S220) added in FIG. 4 can be performed prior to the lamination step (S230) of the resin member and the metal member. The surface treatment step (S220) can be described as a step of surface treating the bonding surface of the metal member. In particular, this surface treatment step (S220) can cause irregularities to be formed on the bonding surface of the metal member.

[0054] According to this embodiment of the present invention, irregularities are formed on the bonding surface of a metal member, thereby enabling better fusion between a resin member and a metal member during fusion by heat conduction. In particular, in the case of the above embodiment, a molten resin member can be inserted into and bonded to the irregularities of the metal member formed by surface treatment. Accordingly, the fusion strength between the resin member and the metal member can be further improved.

[0055] The above surface treatment step (S220) may be performed by irradiating a laser (surface treatment laser) onto the bonding surface of a metal member. In particular, such irradiation of the surface treatment laser may be performed in a manner where two or more surface treatment lines in different directions intersect. This will be explained in more detail with reference to FIG. 5.

[0056] FIG. 5 is a diagram schematically showing the surface treatment configuration of a metal member according to one embodiment of the present invention.

[0057] Referring to FIG. 5, for the performance of the surface treatment step (S220), a laser (surface treatment laser) may be irradiated onto at least one surface of a metal member, particularly a surface bonded to a resin member. For example, as indicated by D1 in FIG. 5, the surface treatment laser may be applied while moving in a horizontal direction (X-axis direction) along the surface (bonding surface) of the metal member. At this time, the surface treatment laser may be irradiated in a form having a plurality of straight line patterns. Additionally, as indicated by D2 in FIG. 5, the surface treatment laser may be applied while moving in a vertical direction (Y-axis direction) along the surface (bonding surface) of the metal member. At this time, the surface treatment laser may be irradiated in a form having a predetermined pattern due to surface treatment lines (laser lines) in two intersecting directions (horizontal direction and vertical direction). Furthermore, the surface treatment laser may be irradiated to form a mesh-shaped surface treatment pattern. In particular, a laser for surface treatment can form a square mesh pattern by having surface treatment lines in different directions orthogonal to each other.

[0058] In addition, the surface treatment laser can form mesh patterns of various shapes other than squares, such as pentagons or hexagons, by having surface treatment lines in different directions intersect (contact) each other to form vertices.

[0059] In addition, the laser for surface treatment may form a surface treatment pattern by forming multiple folded lines, such as zigzag lines, rather than straight lines, in a form where these lines do not intersect each other but extend parallel to one another.

[0060] According to this embodiment of the present invention, surface treatment can be performed on the bonding surface of a metal member by irradiating a laser in the form of a plurality of straight lines, particularly in the form of a mesh. And, due to this surface treatment, irregularities suitable for fusion can be formed on the bonding surface of the metal member. Accordingly, fusion between the metal member and the resin member can be achieved more smoothly. In particular, when the surface treatment pattern of the metal member is performed in the form of a mesh, the surface area or specific surface area on the bonding surface of the metal member can be further increased. Therefore, in this case, more heat can be conducted from the metal member to the resin member, and as a result, fusion of the resin member to the metal member can be achieved more effectively.

[0061] Meanwhile, a laser for surface treatment can be applied to the surface of a metal member in various specifications and methods. In particular, the laser for surface treatment can be applied in various specifications and methods depending on the type and shape of the metal member or resin member, and the shape or area of ​​the joint. For example, the laser for surface treatment may have a wavelength of 1064 nm (nanometer), a speed of 300 mm / s, an output of 36 W, and a frequency of 70 kHz. In addition, the laser for surface treatment may be irradiated several times, for example four times, on the same line (groove), and may have a spot delay of 0.1 ms.

[0062] FIG. 6 is a diagram illustrating an example of a surface-treated configuration of a metal member in a heterogeneous material joining method according to another embodiment of the present invention. For example, FIG. 6 can be described as an enlarged view of a partial configuration of a cross-section along the line A3-A3' of FIG. 5.

[0063] Referring to FIG. 6, the bonding surface of the metal member is shown positioned at the top, and this bonding surface is surface-treated. Furthermore, the surface treatment of the bonding surface of the metal member can be performed through irradiation with a surface treatment laser, as previously described. When the bonding surface of the metal member is surface-treated in this manner, irregularities may be formed on the bonding surface of the metal member. In particular, the surface treatment step may be performed in a manner that forms one or more of grooves and burrs on the bonding surface of the metal member.

[0064] More specifically, when a surface treatment laser is irradiated onto the surface of a metal member, a concave groove may be formed at the irradiated location, as indicated by G in FIG. 6. And, a burr may be formed around this groove (G), as indicated by B.

[0065] In this way, when a groove (G) and / or burr (B) is formed on the bonding surface of the metal member by surface treatment, fusion with the resin member can be achieved more effectively. In particular, when bonding the metal member and the resin member, the molten resin member is inserted into the space formed by the groove (G) and / or burr (B), thereby further improving the bonding strength between the metal member and the resin member.

[0066] In particular, the surface treatment step (S220) can achieve improved fusion strength by appropriately adjusting the shape, location, size, etc. of the groove (G) and / or burr (B) formed on the surface of the metal member.

[0067] For example, the surface treatment step (S220) can be performed such that the depth of the groove is 100 μm (micrometer) to 200 μm. Here, the depth of the groove can be the part indicated as C1 in FIG. 6. That is, the depth of the groove can be the straight-line length from the surface of the metal member to the inner end of the groove. In particular, the surface treatment step (S220) can be performed such that the depth of the groove is 110 μm or more, more than 130 μm or more, and more than 150 μm or more.

[0068] Additionally, the surface treatment step (S220) can be performed such that the height of the burr is 10 μm to 70 μm. Here, the height of the burr can be defined as the straight-line length from the surface of the metal member to the highest height of the burr, as indicated by C2 in FIG. 6. In particular, the surface treatment step (S220) can be performed such that the height of the burr is 30 μm or more, more than 40 μm or more, and more than 50 μm or more.

[0069] Additionally, the surface treatment step (S220) can be performed such that the groove entrance width is 20 μm to 60 μm. Here, the groove entrance width can be understood to mean the length of the entrance side for a single groove, as indicated by the part labeled C3 in FIG. 6. Furthermore, the surface treatment step (S220) can be performed such that the groove entrance width is 30 μm or more and 55 μm or less, particularly 40 μm or more and 50 μm or less.

[0070] In addition, the surface treatment step (S220) can be performed such that the pitch between the grooves is 100 μm to 200 μm. Here, the pitch between the grooves can be defined as the straight distance between the inner ends of the grooves, as indicated by C4 in FIG. 6. In particular, the surface treatment step (S220) can be performed such that the pitch between the grooves is 140 μm or more and 180 μm or less, and furthermore, 160 μm or more and 170 μm or less.

[0071] Additionally, the surface treatment step (S220) can be performed such that the sum of the groove depth and the burr height is 120 µm or more. Here, the sum of the groove depth and the burr height can be the value indicated as C1+C2 in FIG. 6. In particular, the surface treatment step (S220) can be performed such that the sum of the groove depth and the burr height is 130 µm or more, more than 140 µm or more, and more than 150 µm or more.

[0072] Meanwhile, the various numerical values ​​for the grooves or burrs described above may be applied as absolute values ​​for all grooves or burrs, or as average values ​​for all grooves or burrs. In addition, the shape, size, location, etc., of the grooves or burrs described above may be determined by various specifications of the surface treatment laser, such as the irradiation type, output, time, and speed.

[0073] In particular, as described in the embodiment of FIG. 5 above, when a laser is irradiated in a mesh-shaped pattern during the surface treatment step (S220), the grooves and / or burrs can be formed in a mesh shape.

[0074] In addition, the surface treatment step (S220) may be performed so as to form micro-protrusions on the bonding surface of the metal member. This will be explained in more detail with reference to FIG. 7.

[0075] FIG. 7 is a diagram illustrating an example of a surface-treated configuration of a metal member in a heterogeneous material joining method according to another embodiment of the present invention. For example, FIG. 7 can be described as a diagram showing all or part of the A4 portion of FIG. 6 in enlargement.

[0076] Referring to FIG. 7 in conjunction with FIG. 6, micro-protrusions can be formed on the bonding surface of a metal member through a surface treatment step (S220), such as the part indicated by F. Here, the micro-protrusions (F) can be said to have a size of tens of nanometers (nm), that is, a size of 1 μm or less. The size of these micro-protrusions (F) can be described as a straight-line distance from one end to the other end, as indicated by C5 in FIG. 7. Furthermore, if the micro-protrusions (F) are viewed as particles protruding from the surface of the metal member, the size of the micro-protrusions (F) can be expressed as a particle diameter. In particular, the micro-protrusions (F) can have a size of 100 nm or less, a size of 80 nm or less, or an even smaller size of 50 nm or less. Additionally, in FIG. 7, for convenience of illustration, the size and shape of a plurality of micro-protrusions are all depicted as identical; however, at least some, particularly a significant number, of the plurality of micro-protrusions may be formed with different sizes and shapes.

[0077] Furthermore, when a groove is formed on the bonding surface of the metal member through the surface treatment step (S220), micro-protrusions of tens of nanometers in size can be formed on the surface between the grooves.

[0078] According to this configuration of the present invention, the welding strength between the metal member and the resin member can be further improved by forming micro-protrusions on the bonding surface of the metal member through the surface treatment step (S220). In particular, the surface area or specific surface area on the bonding surface of the metal member can be increased due to the micro-protrusions formed on the bonding surface of the metal member. Furthermore, this increase in surface area, etc., can allow more heat to be conducted from the metal member to the resin member. Therefore, even if the same welding laser is applied, the welding efficiency can be further increased. In addition, in this case, the welding area between the metal member and the resin member can also be increased due to the micro-protrusions, so it can be said that the welding strength is further improved in this aspect as well.

[0079] As previously explained, a heterogeneous material joining method according to one aspect of the present invention joins a metal member and a resin member, wherein a laser is irradiated from the metal member side to fuse the metal member and the resin member by a thermal conduction fusion method. At this time, employing a suitable metal member can further enhance the effects of the present invention. For example, by preparing a suitable type of metal material as a metal member in the preparation step (S210), it becomes possible to form grooves, burrs, micro-protrusions, etc. suitable for fusion in the surface treatment step (S220), thereby further enhancing the fusion effect in the joining step (S240).

[0080] In particular, the above preparation steps (S110, S210) may prepare a metal member containing aluminum. That is, the heterogeneous material joining method according to the present invention can be applied to joining a metal member containing aluminum and a resin member. Furthermore, in the above preparation steps (S110, S210), an aluminum alloy may be prepared as the metal member.

[0081] In this way, in the case of a metal member containing aluminum, the thermal conduction fusion method with a resin member according to the above embodiment of the present invention can be performed more smoothly. Furthermore, in the case of a metal member containing aluminum, the laser-based bonding step (S130, S240) and / or the laser-based surface treatment step (S220) described above can be performed more effectively. In particular, according to the heterogeneous material bonding method of the present invention, a laser is irradiated onto the metal member side, and heat is transferred to the resin member side by thermal conduction, so that the resin member can be fused to the metal member. With respect to this bonding method, when a material containing aluminum is used as the metal member, it can be performed more effectively.

[0082] In addition, the above preparation step (S110, S210) can prepare a metal member having a ten-point average roughness (Rz) of 6 μm or less. Furthermore, even if the metal member is the same in terms of being an aluminum alloy, the bonding performance may vary depending on this surface roughness. In particular, the metal member prepared in the preparation step (S110, S210) may have a ten-point average roughness (Rz) of 3 μm or less, even smaller than 2 μm or less, and even smaller than 1 μm or less. For example, in the above preparation step (S110, S210), a metal member having a ten-point average roughness (Rz) of 0.6 μm or less, such as 0.51 μm, may be prepared.

[0083] Additionally, the preparation step (S110, S210) may prepare a metal member having a centerline average roughness (Ra), which is another form of surface roughness, of 1 μm or less. In particular, the preparation step (S110, S210) may adopt and prepare a metal member having a ten-point average roughness (Rz) of 0.7 μm or less, even smaller than 0.5 μm or less, and even smaller than 0.3 μm or less. For example, in the preparation step (S110, S210), a metal member having a centerline average roughness (Ra) of 0.2 μm or less, such as 0.13 μm, may be prepared.

[0084] In the case of a metal member having such surface roughness, the welding performance by laser can be improved by reducing scattering and reflection during laser irradiation.

[0085] Additionally, the preparation step (S110, S210) may prepare a metal member having an emissivity of 0.1 to 0.95 with respect to a laser light source with a wavelength of 900 nm to 1100 nm. In particular, the metal member prepared in the preparation step (S110, S210) may be configured to have an emissivity of 0.2 or more, more than 0.3 or more, and more than 0.4 or more with respect to a laser light source with a wavelength of 900 nm to 1000 nm at room temperature. For example, in the preparation step (S110, S210), an aluminum alloy having an emissivity of 0.5 to 0.8 with respect to a laser light source with a wavelength of 900 nm to 1000 nm may be adopted and prepared as the metal member in the S110 step. As a more specific example, in the preparation step (S110, S210), a metal member having an emissivity of 0.6 to 0.7, such as 0.62, with respect to a laser light source of 915 nm wavelength may be prepared.

[0086] Additionally, the preparation step (S110, S210) may prepare a metal member having a reflectance of 20 to 70 as a percentage with respect to a laser light source with a wavelength of 900 nm to 1100 nm. In particular, the metal member prepared in the preparation step (S110, S210) may be configured to have a reflectance of 55 or less, less than 50 or less, and less than 45 or less with respect to a laser light source with a wavelength of 900 nm to 1100 nm incident perpendicularly to the surface. In particular, the preparation step (S110, S210) may prepare a metal member having a reflectance of 25% to 40% with respect to a laser light source with a wavelength of 900 nm to 1100 nm. For example, in the preparation steps (S110, S210), an aluminum alloy having a ten-point average roughness (Rz) of 0.51 μm and a centerline average roughness (Ra) of 0.13 μm with respect to a laser light source of 915 nm wavelength, and a reflectance of 25% to 35%, such as 30.5%, may be adopted as a metal member in step S110 and prepared.

[0087] In addition, the preparation step (S110, S210) may prepare a metal member having an absorbance of 0.1 to 0.6 with respect to a light source with a wavelength of 900 nm to 1100 nm. In particular, the metal member prepared in the preparation step (S110, S210) may be configured to have an absorbance of 0.2 or more, more than 0.3 or more, and more than 0.4 or more with respect to a laser light source with a wavelength of 900 nm to 1100 nm. For example, in the preparation step (S110, S210), an aluminum alloy having a ten-point average roughness (Rz) of 0.51 μm, a centerline average roughness (Ra) of 0.13 μm, and an absorbance of 0.5 or more, such as 0.52, with respect to a laser light source with a wavelength of 915 nm may be adopted and prepared as a metal member.

[0088] When a metal member as described above is prepared in the preparation step (S110, S210) and bonded with a resin member, excellent processability and bonding properties for bonding can be secured.

[0089] Meanwhile, in the bonding step (S130, S240), a pressing operation of the laminate may be performed together during the process of irradiating a laser onto the outer surface of the metal member, or after the laser irradiation. For example, in the embodiment of FIG. 2, when bonding is performed by irradiating a laser (L) onto the upper surface of the metal member while the metal member (M) is laminated on top of the resin member (P), pressing may be performed together in the direction indicated by J. Such pressing may be performed, for instance, by a jig. When such a pressing process is performed together, the bonding process, particularly bonding by fusion, can be carried out more smoothly.

[0090] The heterogeneous material joining device according to the present invention may be configured to perform at least some of the processes of the heterogeneous material joining method according to the present invention described above.

[0091] FIG. 8 is a block diagram schematically showing the configuration of a heterogeneous material joining device according to one embodiment of the present invention.

[0092] Referring to FIG. 8, the heterogeneous material bonding device according to the present invention includes a stacking unit (100) and a bonding unit (200).

[0093] The above-described lamination unit (100) may be configured to perform lamination steps (S120, S230) in the heterogeneous material bonding method according to the present invention described above. That is, the lamination unit (100) may be configured to laminate a resin member and a metal member.

[0094] In particular, the stacking unit (100) may be provided with a seating portion (110) and a transfer portion (120) as shown in the drawing. Here, the seating portion (110) is a component provided to allow the bonding target, namely a resin member and a metal member, to be seated. For example, the seating portion (110) may be configured so that the resin member and the metal member are seated on the upper part. And, the transfer portion (120) is a component provided to transfer the resin member and the metal member to the seating portion (110). For example, the transfer portion (120) may be configured in the form of a conveyor belt. At this time, the seating portion (110) and the transfer portion (120) may be implemented as a single integrated device.

[0095] The bonding unit (200) may be configured to perform bonding steps (S130, S240) in the heterogeneous material bonding method according to the present invention described above. That is, the bonding unit (200) may be configured to bond a resin member and a metal member by irradiating a laser onto the outer surface of a metal member stacked by the stacking unit (100). To this end, the bonding unit (200) may be provided with a bonding laser application unit (210). Additionally, the bonding unit (200) may further be provided with a jig unit (220). This jig unit (220) may be configured to press the stack of the metal member and the resin member in the stacking direction when a bonding laser is applied by the bonding laser application unit (210), or after the bonding laser is applied.

[0096] The bonding unit (200) may be configured such that heat supplied by applying a laser is conducted through a metal member, and the resin member is melted by this heat conduction so that the resin member is bonded to the surface of the metal member.

[0097] In addition, the heterogeneous material joining device according to the present invention may further include a surface treatment unit (300) as shown in FIG. 8. The surface treatment unit (300) may be configured to perform a surface treatment step (S220) in the heterogeneous material joining method according to the present invention described above. That is, the surface treatment unit (300) may be configured to surface treat the joining surface of a metal member so that irregularities can be formed on the joining surface of the metal member prior to the lamination operation by the lamination unit (100).

[0098] In particular, the surface treatment unit (300) may include a laser application unit (310) for surface treatment. Here, the laser application unit (310) for surface treatment may apply a laser for surface treatment to the bonding surface of a metal member. At this time, the laser application unit (310) for surface treatment and the laser application unit (210) for bonding may be implemented as a single laser application device.

[0099] The surface treatment unit (300) may be configured such that the irregularities formed on the bonding surface of the metal member have a predetermined pattern. In particular, the surface treatment unit (300) may irradiate a laser for surface treatment so that two or more surface treatment lines in different directions intersect. For example, the surface treatment unit (300) may apply a laser for surface treatment to the bonding surface of the metal member so that the irregularities have a square mesh-shaped pattern, as shown in FIG. 5.

[0100] Additionally, the surface treatment unit (300) may be configured to form one or more of grooves and burrs on the bonding surface of a metal member. In particular, such grooves or burrs may be formed by applying a laser by a laser application unit (310) for surface treatment.

[0101] In addition, the surface treatment unit (300) may be configured to form fine protrusions of 1 µm or less on the bonding surface of a metal member.

[0102] Additionally, the lamination unit (100) can laminate a metal member containing aluminum, such as an aluminum alloy, and a resin member. And, the bonding unit (200) can be configured to bond the aluminum-containing metal member and the resin member.

[0103] In addition, the metal member laminated and bonded by the lamination unit (100) and the bonding unit (200) may have a ten-point average roughness of 6 μm or less. In addition, the metal member laminated and bonded by the lamination unit (100) and the bonding unit (200) may have a reflectance of 20% to 70% with respect to a laser light source with a wavelength of 900 nm to 1100 nm.

[0104] For such a heterogeneous material joining device, various descriptions of the heterogeneous material joining method described earlier may be applied identically or similarly. Therefore, a more specific description of such a heterogeneous material joining device is omitted.

[0106] Hereinafter, the present invention will be described in more detail by citing various embodiments to explain it more clearly. However, embodiments according to the present invention may be modified in various different forms, and the scope of the present invention should not be interpreted as being limited to the embodiments described below. The embodiments of the present invention are provided to more completely explain the present invention to those with average knowledge in the art.

[0108] (Examples 1 to 3)

[0109] A resin plate (EU5300) having a length of 60 mm, a width of 25 mm, and a thickness of 1.5 mm, and a metal plate (Al5052) having a length of 100 mm, a width of 25 mm, and a thickness of 1 mm were prepared. At this time, a surface treatment laser was applied to one surface of the metal plate to form a mesh-shaped pattern as shown in Fig. 5. At this time, the surface treatment laser was applied four times repeatedly using a laser marking device with a wavelength of 1064 nm, a speed of 300 mm / s, an output of 36 W, and a frequency of 70 kHz, and the spot delay was set to 0.1 ms.

[0110] Regarding the resin plate and metal plate prepared in this manner, the surface-treated portion of the metal plate was laminated in the thickness direction so as to be in contact with the resin plate. Then, by applying a bonding laser 7 to 9 times to the outer surface of the metal plate using a laser welding device, the resin plate and the metal plate were bonded by a thermal conduction fusion method, thereby preparing samples of Examples 1 to 3. At this time, the bonding laser was applied at an output of 500 W and a speed of 40 mm / s (12.5 J / mm) for each application. That is, in the case of Example 1, the bonding laser was applied 7 times, and a line energy of 87.5 J / mm (2.5 J / mm × 7) was applied; in the case of Example 2, the bonding laser was applied 8 times, and a line energy of 100 J / mm was applied; and in the case of Example 3, the bonding laser was applied 9 times, and a line energy of 112.5 J / mm was applied.

[0112] (Comparative Example 1)

[0113] A resin plate and a metal plate identical to those in Example 1 were prepared, but the laser was applied to the resin plate side rather than the metal plate side. That is, in the case of Comparative Example 1, a specimen was prepared in a form generally identical to that of Example 1, but unlike Example 1, the bonding laser was attempted to pass through the resin plate and reach the bonding site to prepare the sample of Comparative Example 1. At this time, the applied energy of the bonding laser was performed in the same manner as in Example 1.

[0115] (Comparative Example 2)

[0116] A resin plate and a metal plate identical to those in Example 1 were prepared, but the bonding was performed using an ultrasonic welding method instead of a laser welding method. At this time, an ultrasonic device from Emerson was used, and a sample of Comparative Example 2 was prepared by applying vibration in a transverse direction, which is orthogonal to the stacking direction of the specimen. Here, the ultrasound was applied at a frequency of 30 kHz and 100% output while applying a pressure of 350 psi for 10 seconds.

[0118] (Comparative Example 3)

[0119] A sample of Comparative Example 3 was prepared by preparing the specimen and performing ultrasonic welding under conditions similar to Comparative Example 2, except that the direction of vibration application was the longitudinal direction, which is the same as the stacking direction of the specimen.

[0121] Tensile tests were performed on the samples of Examples 1 to 3 and Comparative Examples 1 to 3, respectively, and are shown in FIG. 9. That is, FIG. 9 is a graph showing a comparison of the bonding strengths of various embodiments and comparative examples of the present invention. At this time, the bonding strength was measured using a tensile testing device from Zwick using a tensile mode measurement method.

[0122] Referring to FIG. 9, it can be seen that Examples 1 to 3, which utilize the laser thermal conduction welding method according to the present invention, all exhibit a bonding strength close to 20 MPa. On the other hand, Comparative Example 3 exhibits a bonding strength of less than 5 MPa. Furthermore, in Comparative Example 3, surface deformation occurred due to the horn or anvil. Therefore, it can be seen that the appearance quality is inferior compared to Examples 1 to 3, in which almost no surface deformation occurred.

[0123] Meanwhile, Comparative Examples 1 and 2 are not illustrated in FIG. 9. This is because, in the case of Comparative Examples 1 and 2, fusion itself did not occur between the resin plate and the metal plate. Furthermore, even with a laser-based fusion method as in Comparative Example 1, fusion did not occur when the laser was applied from the resin plate side, unlike in the embodiment of the present invention. Additionally, in the case of Comparative Example 2, when the direction of vibration applied by ultrasound was transverse, a part of the resin plate was constricted by the horn or anvil, and fusion between the resin plate and the metal plate did not occur.

[0124] Therefore, based on these comparison results, it can be seen that when heterogeneously joining a resin plate and a metal plate, the joining technology according to the present invention is superior to the ultrasonic welding technology or laser transmission welding technology of the comparative example.

[0126] (Examples 4 to 7)

[0127] Samples were prepared in a manner and form generally similar to Example 1, but with only the number of times the bonding laser was applied differing from Example 1. Specifically, after a resin plate (EU5300) was laminated against the surface of a surface-treated metal plate (Al5052), samples of Examples 4 to 7 were prepared by applying a bonding laser 12, 14, 16, and 18 times to the outer surface of the metal plate. That is, in the case of Example 4, 12 lasers were applied, and it can be said that 150 J / mm of energy was applied, and in the case of Example 5, 14 lasers were applied, and 175 J / mm of energy was applied. In addition, in the case of Example 6, 16 lasers were applied, and 200 J / mm of energy was applied, and in the case of Example 7, 18 lasers were applied, and 225 J / mm of energy was applied. Meanwhile, for Examples 4 to 7, three or four samples were prepared for each example.

[0129] (Examples 8 to 12)

[0130] Samples were prepared in a manner and form generally similar to Examples 4 to 7, but the type of metal plate was changed from Al5052 to ADC12. That is, several metal plates (ADC12) and several resin plates (EU5300) were prepared, and surface treatment was performed on the bonding surface of each metal plate in the same manner as in Examples 1 or 4. Then, after manufacturing a plurality of laminates in which the metal plates (ADC12) were laminated with the resin plates (EU5300), a bonding laser was applied to the metal plate (ADC12) side of each laminate. At this time, the specifications of the bonding laser were the same as in Example 4, but the number of times the bonding laser was applied was set to 7, 8, 9, 10, and 12, and samples of Examples 8 to 12 were prepared. That is, in the case of Example 8, it can be said that 7 laser pulses were applied and 87.5 J / mm of energy was applied, and in the case of Example 9, 8 laser pulses were applied and 100 J / mm of energy was applied. In addition, in the case of Example 10, 9 laser pulses were applied and 112.5 J / mm of energy was applied, and in the case of Example 11, 10 laser pulses were applied and 125 J / mm of energy was applied. Furthermore, in the case of Example 12, 12 laser pulses were applied and 150 J / mm of energy was applied. Also, in the case of Examples 8 to 12, 3 or 4 samples were prepared for each example.

[0132] For the samples of Examples 4 to 12, tensile tests were conducted in the same manner as in FIG. 9, and the results are shown in FIG. 10 and FIG. 11. Specifically, FIG. 10 is a table showing the results of bonding strength measurements according to various other embodiments of the present invention, and FIG. 11 is a graph illustrating the measurement results of FIG. 10. In particular, the tensile test results for each embodiment are shown as tensile force (N) in the table of FIG. 10, and the tensile strength (Tensile shear) (MPa) for each embodiment is shown in the graph of FIG. 11.

[0133] Referring to FIGS. 10 and 11, first, in the case of Example 4, a bonding strength of around 20 MPa is shown. Furthermore, in the case of Examples 5 to 7, a bonding strength of generally 20 MPa or higher is shown. In addition, in the case of Examples 6 and 7, a bonding strength in the range of 18 MPa to 66 MPa is shown.

[0134] In particular, Examples 8 to 12 show a bonding strength higher than 43 MPa. Furthermore, Example 11 shows a bonding strength in the range of 58 MPa to 69 MPa.

[0135] Referring to the measurement results of FIGS. 10 and FIGS. 11, it can be seen that in Examples 4 to 12 according to the present invention, and furthermore in Examples 5 to 12, bonding between dissimilar materials (metal and resin) is achieved with a bonding strength higher than 20 MPa. In particular, in Examples 8 to 12, in which ADC12 material is applied as the metal member, it can be seen that the bonding strength is significantly improved compared to Examples 4 to 7, in which Al5052 material is applied as the metal member. Considering that the bonding strength of general structural adhesives is generally less than 20 MPa, the bonding strength according to the present invention can be said to be very high compared to adhesives.

[0136] Furthermore, in the case of Examples 8 to 12, the bonding strength was improved even though the applied energy of the bonding laser was lower than that of Examples 4 to 7. Therefore, according to Examples 8 to 12, the energy efficiency for fusion can be said to be high. In addition, compared to Examples 4 to 7, the variation in fusion strength between samples in Examples 8 to 12 is not large.

[0137] In addition, regarding the cases where the sample was damaged in a separated form at the interface between the metal plate and the resin plate during the tensile test for Examples 4 to 12, this is indicated by shading in FIG. 10. In such cases where the interface is separated, the bonding performance can be considered relatively low. On the other hand, the parts not indicated by shading in FIG. 10 can be interpreted as meaning that the bonding was successful, as the sample was damaged in a fractured form at the base material (metal plate or resin) during the tensile test.

[0138] Looking at the results in Fig. 10 from this perspective, it can be seen that in all of Examples 4 to 7, interfacial separation occurred in some or all of the samples. On the other hand, in Examples 8 to 12, interfacial separation did not occur in any of the samples, and all showed results where the base material fractured. Therefore, even based on this aspect, it can be seen that the bonding effect in Examples 8 to 12 is superior to that in Examples 4 to 7.

[0139] Meanwhile, the thermal conductivity of the ADC12 material used as the metal member in Examples 8 to 12 is approximately 92 W / mK, which is lower than the thermal conductivity of the Al5052 material used as the metal member in Examples 4 to 7, which is 138 W / mK. However, the emissivity of the ADC12 material is about 0.62 at a light source with a wavelength of about 1000 nm, which is much higher than the emissivity of the Al5052 material, which is 0.2. Therefore, due to this difference in emissivity, it can be presumed that the bonding strength of Examples 8 to 12 is superior to that of Examples 4 to 7.

[0140] In addition, Examples 8 to 12 can be said to secure superior bonding strength due to the surface treatment characteristics of the metal material compared to Examples 4 to 7. This will be explained in more detail with reference to FIGS. 12 to 16. The images and numerical values ​​related to FIGS. 12 to 16 were captured and measured using a 3D Profiler Microscope. For reference, the images in FIGS. 12 to 16 are shown with the bonding surface of the metal plate positioned at the top.

[0141] First, FIG. 12 is an enlarged cross-sectional image showing the configuration in which the bonding surface of the metal plate before fusion is surface-treated in Example 5, and FIG. 13 is an enlarged cross-sectional image showing the configuration in which the bonding surface of the metal plate before fusion is surface-treated in Example 12. These configurations of FIG. 12 and FIG. 13 may be considered as examples of cross-sectional configurations along the line A3-A3' in FIG. 5.

[0142] Looking at the images in Figures 12 and 13, it can be seen that even though the surface treatment was performed in the same way, the shape of the grooves or burrs is different.

[0143] First, the measurement results for the groove and burr formed in the embodiment of FIG. 12 are as follows.

[0144] Groove entrance width: 26 um,

[0145] Groove depth: 105 um,

[0146] Burr height: 26 um,

[0147] Pitch (spacing) between grooves: 160 um.

[0148] And, the measurement results for the groove and burr formed in the embodiment of FIG. 13 are as follows.

[0149] Groove entrance width: 46 um,

[0150] Groove depth: 160 um,

[0151] Burr height: 58 um,

[0152] Pitch between grooves: 164 um.

[0154] Looking at the shapes and measurement results of FIGS. 12 and 13, it can be seen that in the case of Example 12 (Fig. 13), the groove entrance width is wider, the groove depth is deeper, and the burr height is higher than in Example 5 (Fig. 12). Furthermore, it can be presumed that these results are due to the fact that the metal material (ADC12) used in Example 12 has a relatively higher emissivity or absorption rate compared to the metal material (Al5052) used in Example 4, so energy absorption for the laser is well achieved during surface treatment.

[0155] In addition, such differences in surface treatment results can be said to lead to differences in bonding strength as previously described in FIGS. 10 and 11. This will be explained further with reference to FIGS. 14 to 16.

[0156] FIGS. 14 and 15 are magnified cross-sectional images of the bonded surface after fusion for Examples 5 and 6, and FIG. 16 is a magnified cross-sectional image of the bonded surface after fusion for Example 12. These images of FIGS. 14 to 16 were captured using a 3D Profiler Microscope.

[0157] First, referring to FIG. 14 related to Example 5, it is observed that at the bonding interface between the resin plate (upper position) and the metal plate (lower position), as indicated by A5, the resin is not sufficiently pressed into the groove side of the metal plate. Then, in the case of FIG. 15 related to Example 6, in which the energy of the fusion laser is relatively increased, it is observed that the resin is relatively well pressed into the bonding interface, as indicated by A6, compared to FIG. 14.

[0158] In contrast, referring to FIG. 16 related to Example 12, it can be seen that resin indentation was performed very well at the bonding interface between the resin plate and the metal plate, as indicated by the part labeled A7. Furthermore, in the case of Example 12, the applied energy was 150 J / mm, which is much smaller than 175 J / mm of Example 5 or 200 J / mm of Example 6. Therefore, in the case of Example 12, even though a lower fusion energy was applied compared to Examples 6 and 7, the bonding strength was actually improved.

[0159] Furthermore, if resin intrusion into the groove side of the metal plate is not sufficiently achieved as shown in FIG. 14, interfacial separation may occur during the tensile test, as previously explained with respect to Example 5 of FIG. 10. On the other hand, if resin intrusion into the groove side of the metal plate is sufficiently achieved as shown in FIG. 16, interfacial separation does not occur during the tensile test and the base material fractures, as previously explained with respect to Example 12 of FIG. 10.

[0160] In addition, by referring to these measurement results, it can be seen that in the case of a metal material (ADC12) such as Example 12, compared to a metal material (Al5052) such as Example 5 or 6, the groove size is formed relatively larger even with the same type of surface treatment, and less energy is required to penetrate the resin into the groove side of the metal.

[0162] Meanwhile, regarding the metal plate (Al5052) used in Example 4 and the metal plate (ADC12) used in Example 8, the surface roughness was measured under the same processing conditions using a 3D Profiler Microscope in a roughness measurement mode, and the following results were obtained.

[0163] Centerline average roughness (Ra) of the metal plate in Example 4: 0.79 µm

[0164] Centerline average roughness (Ra) of the metal plate in Example 8: 0.13 µm

[0165] Ten-point average roughness (Rz) of the metal plate in Example 4: 3.62 μm

[0166] Ten-point average roughness (Rz) of the metal plate in Example 8: 0.51 μm

[0167] Looking at these surface roughness measurement results, it can be said that the metal plate (Al5052) of Example 4 has a roughness approximately 7 times greater than that of the metal plate (ADC12) of Example 8. Furthermore, due to this difference in roughness, Example 4 may cause relatively more scattering and reflection with respect to the laser source (greater than 915 nm) used during laser irradiation for bonding compared to Example 8.

[0168] Therefore, in terms of such surface roughness as well, it can be well understood that the results examined above, namely the bonding strength of the samples of Examples 8 to 12, are superior to the bonding strength of the samples of Examples 4 to 7.

[0170] In addition, FIGS. 17 and 18 are graphs comparing the reflectance and absorbance of the metal material of Example 4 and the metal material of Example 8. These reflectances and absorbances were measured using a UV-VIS Spectrometer in reflectance measurement mode and absorption measurement mode.

[0171] First, referring to FIG. 17, the reflectance of the metal material (Al5052) of Example 4 gradually increases as the wavelength of the light source increases. More specifically, the metal material of Example 4 exhibits a reflectance of approximately 30% to 70% in the wavelength range of 300 nm to 1200 nm. On the other hand, the metal material (ADC12) of Example 8 maintains a reflectance of approximately 30% even as the wavelength of the light source increases. That is, the metal material of Example 8 exhibits a reflectance of approximately 30% in the wavelength range of 300 nm to 1200 nm. As a more specific example, regarding a wavelength of 915 nm, Example 4 exhibits a reflectance of 56.79%, while Example 8 exhibits a reflectance of 30.5%.

[0172] Next, referring to FIG. 18, as the wavelength of the light source increases, the absorbance of the metal material (Al5052) of Example 4 gradually decreases. More specifically, the metal material of Example 4 exhibits an absorbance of approximately 0.1 to 0.5 in the wavelength range of 300 nm to 1200 nm. On the other hand, the metal material of Example 8 (ADC12) maintains an absorbance of approximately 0.5 even as the wavelength of the light source increases. That is, the metal material of Example 8 exhibits an absorbance of approximately 0.5 in the wavelength range of 300 nm to 1200 nm. As a more specific example, regarding a wavelength of 915 nm, Example 4 exhibits an absorbance of 0.19, while Example 8 exhibits an absorbance of 0.52.

[0173] Even by referring to the optical property measurement results of FIGS. 17 and FIGS. 18, it can be seen that the metal material (ADC12) of Example 8 is more advantageous for energy absorption compared to the metal material (Al5052) of Example 4. In particular, the metal material of Example 4 can be said to have optical properties that are approximately 66% higher in terms of reflectance and approximately 63% lower in terms of absorption compared to the metal material of Example 8.

[0174] Therefore, due to such surface roughness and optical properties, the metal material (ADC12) of Examples 8 to 12 can be said to achieve a superior bonding effect in the present invention compared to the metal material (Al5052) of Examples 4 to 7. In particular, such surface roughness or optical properties can be said to be properties related to the opposite side of the metal surface to which the laser is applied, that is, the bonding surface of the metal, rather than the bonding surface. For example, when a metal plate is laminated on top of a resin plate, the bonding laser is irradiated onto the upper surface of the metal plate, and such surface roughness or optical properties on the upper surface of the metal plate may affect the bonding strength between the metal plate and the resin plate.

[0176] FIG. 19 is a partial enlarged image of the surface-treated configuration of the bonding surface of the metal plate before fusion in Example 8, viewed from the front, and FIG. 20 is a partial enlarged image of the surface-treated configuration of the bonding surface of the metal plate before fusion in Example 4, viewed from the front.

[0177] Such images and related measurements were performed using a scanning electron microscope (FIB-SEM).

[0178] First, referring to FIG. 19, the metal material (ADC12) of Example 8 was subjected to surface treatment as described above, and the height of the burr was measured to be 42.48 μm, the total height of the groove and the burr was 163.42 μm, and the average pitch (spacing) between the grooves (patterns) was 177.06 μm.

[0179] In particular, referring to the embodiment of FIG. 19, specifically the 50,000x magnified view on the far right, it can be seen that a large number of micro-protrusions at the level of tens of nanometers are formed on the surface-treated bonding surface of the metal plate. In particular, many of these micro-protrusions were observed in the spaces between the grooves formed in a mesh pattern.

[0180] On the other hand, referring to FIG. 20, when surface treatment was performed on the metal material (Al5052) of Example 4 in the same manner as in Example 8, the height of the burr was measured to be 30.76 μm, the total height of the groove and the burr was 83.37 μm, and the average pitch (spacing) between the grooves (patterns) was 150.62 μm.

[0181] In particular, in the case of Fig. 20, even when referring to the drawing magnified up to 50,000 times, no micro-protrusions of the tens of nanometer level as in Fig. 19 were observed on the surface-treated bonding surface of the metal plate.

[0182] As such, unlike Example 4, in the case of Example 8, numerous micro-protrusions of 100 μm or less were formed. This can be attributed, in part, to the fact that the metal used in Example 8 absorbed more laser energy during surface treatment than the metal used in Example 4, and was subsequently melted and cooled at a higher temperature. Additionally, this result can be attributed to the fact that in the case of Example 4, compared to Example 8, the metal tended to cool and solidify relatively slowly after melting during the surface treatment process.

[0183] Meanwhile, as such, in the case of Example 8, unlike Example 4, since many micro-protrusions at the level of tens of nanometers are formed on the bonding surface of the metal member, the surface area or specific surface area can be increased. And, such an increase in surface area increases the thermal conductivity efficiency, which can ultimately lead to a result of increasing the fusion efficiency with the same energy.

[0185] (Examples 13 to 17)

[0186] A sample was prepared in which a metal plate (ADC12) and a resin plate (EU5300) were joined in a manner generally identical to that of Example 12, except that the mesh-shaped surface treatment conditions for the metal plate (ADC12) before fusion (bonding) were treated slightly differently. That is, for each example, only the surface treatment conditions described below were performed differently, and all other processes were performed in the same manner as in Example 12.

[0187] First, in the case of Example 13, the depth of the groove (pattern) was increased by 30% compared to Example 12. That is, in the case of Example 13, the groove depth of the mesh pattern was approximately 208 μm, which is approximately 30% higher than the groove depth of 160 μm in Example 12.

[0188] In addition, in the case of Example 14, the depth of the groove (pattern) was reduced by 30% compared to Example 12. That is, in the case of Example 14, the groove depth of the mesh pattern was approximately 112 μm, which is approximately 30% lower than the groove depth of 160 μm in Example 12.

[0189] In addition, in the case of Example 15, the groove (pattern) inlet width was increased by 20% compared to Example 12. That is, in the case of Example 15, the groove inlet width of the mesh pattern was approximately 55.2 μm, which is approximately 20% higher than the groove inlet width of 46 μm in Example 12.

[0190] In addition, in the case of Example 16, the groove (pattern) entrance width was reduced by 20% compared to Example 12. That is, in the case of Example 16, the groove entrance width of the mesh pattern was approximately 36.8 μm, which is approximately 20% lower than the groove entrance width of 46 μm in Example 12.

[0191] In addition, in the case of Example 17, the spacing between patterns (pitch) was doubled compared to Example 12. That is, in the case of Example 17, the spacing between patterns was approximately 320 μm, which is approximately double the spacing between patterns of 164 μm in Example 12.

[0193] (Examples 18 to 22)

[0194] Samples were prepared in a manner generally identical to that of the preceding Examples 12 to 16, except that the surface treatment conditions for the metal plate (ADC12) were changed from a square mesh form to a line form. That is, in the case of Examples 18 to 22, the grooves on the surface of the metal plate were formed in a parallel form rather than a form in which multiple lines are orthogonal. In other words, for each example, other details were performed in the same manner as the preceding examples, except for the matters described below.

[0195] First, in the case of Example 18, a pattern (groove) was formed in a line shape rather than a mesh shape during surface treatment, and the fusion conditions or other surface treatment conditions, such as the depth or width of the groove and the spacing between patterns, were performed in a manner generally identical to that of Example 12 to prepare a sample.

[0196] In addition, in the case of Example 19, a pattern (groove) was formed in a line shape rather than a mesh shape during surface treatment, and the fusion conditions or other surface treatment conditions, such as the depth or width of the groove and the spacing between patterns, were performed in a manner generally identical to that of Example 13 to prepare the sample.

[0197] In addition, in the case of Example 20, a pattern (groove) was formed in a line shape rather than a mesh shape during surface treatment, and the fusion conditions or other surface treatment conditions, such as the depth or width of the groove and the spacing between patterns, were performed in a manner generally identical to that of Example 14 to prepare the sample.

[0198] In addition, in the case of Example 21, a pattern (groove) was formed in a line shape rather than a mesh shape during surface treatment, and the fusion conditions or other surface treatment conditions, such as the depth or width of the groove and the spacing between patterns, were performed in a manner generally identical to that of Example 15 to prepare the sample.

[0199] In addition, in the case of Example 22, a pattern (groove) was formed in a line shape rather than a mesh shape during surface treatment, and the fusion conditions or other surface treatment conditions, such as the depth or width of the groove and the spacing between patterns, were performed in a manner generally identical to that of Example 16 to prepare the sample.

[0200] In addition, for Examples 13 to 22 prepared in this manner and Example 12 described above, the bonding strength was measured in the same manner as described above, and the results are shown in FIG. 21 from a relative perspective. That is, FIG. 21 is a graph showing a relative comparison of bonding strengths according to various embodiments of the present invention. In particular, FIG. 21 shows the bonding strengths of other embodiments as relative ratios with the bonding strength of Example 18 set as the reference (100%) (horizontal axis).

[0201] Referring to FIG. 21, it can be seen that the bonding strength of Examples 12 to 16, in which grooves are formed in a mesh pattern, is higher than the bonding strength of Examples 18 to 22, in which grooves are formed in a line pattern. In particular, in the case of Example 12, the bonding strength can be seen to be significantly higher than that of Examples 18 to 22.

[0202] Therefore, according to these comparison results, it can be seen that when grooves are formed in a polygonal mesh pattern during surface treatment, superior bonding strength can be achieved compared to when grooves are formed in a line pattern. This can be understood as being due to the fact that when grooves are formed in a mesh pattern, the surface area or specific surface area increases, thereby increasing thermal conductivity efficiency, and more grooves or burrs that can be fused with the molten resin are formed.

[0203] Furthermore, among Examples 12 to 17, in which grooves are all formed with a mesh pattern, the bonding strength of Example 12 can be said to be relatively higher than that of the other Examples 13 to 17. Even with the same mesh pattern, the bonding strength can vary depending on the depth, width, and spacing of the pattern (groove); however, in the case of Example 12, it can be judged that it has a relatively appropriately formed pattern depth, width, and spacing. Therefore, in this regard, it can be said that the appropriate design of the depth, width, and spacing of the pattern (groove) during surface treatment is also important for improving the bonding strength.

[0205] As described above, although the present invention has been explained by limited embodiments and drawings, the present invention is not limited thereto, and it is obvious that various modifications and variations are possible within the scope of the technical spirit of the present invention and the equivalent scope of the claims described below by those skilled in the art to which the present invention belongs. Explanation of the symbols

[0206] M: Metal member P: Resin absence L: Laser W: Joint G: Groove B: Bur F: Micro-protrusions 100: Stacking unit 110: Seating section, 120: Transfer section 200: Joining unit 210: Laser application unit for bonding, 220: Jig unit 300: Surface treatment unit 310: Laser application unit for surface treatment

Claims

Claim 1 A method for bonding heterogeneous materials comprising: a step of preparing a resin member and a metal member; a step of surface treating the bonding surface of the metal member so as to form irregularities on the bonding surface of the metal member; a step of laminating the resin member and the metal member; and a step of bonding the resin member and the metal member by irradiating a laser onto the outer surface of the metal member laminated in the lamination step; wherein the metal member prepared in the preparation step has an emissivity of 0.5 to 0.8 and a reflectivity of 25% to 40% with respect to a light source with a wavelength of 900 nm to 1100 nm, and the surface treatment step is characterized by forming a micro-protrusion of 1 μm or less on the bonding surface of the metal member. Claim 2 A method for joining dissimilar materials according to claim 1, wherein the joining step is characterized by melting the resin member by heat conducted through the metal member and joining it to the surface of the metal member. Claim 3 delete Claim 4 A heterogeneous material joining method according to claim 1, wherein the surface treatment step is performed in a manner in which two or more surface treatment lines of different directions intersect. Claim 5 A method for joining dissimilar materials according to claim 1, wherein the surface treatment step is characterized by forming one or more of a groove and a burr on the joining surface of the metal member. Claim 6 delete Claim 7 A method for joining dissimilar materials according to claim 1, wherein the metal member prepared in the preparation step contains aluminum. Claim 8 A method for joining dissimilar materials according to claim 1, wherein the metal member prepared in the preparation step has a ten-point average roughness of 6 µm or less. Claim 9 delete Claim 10 A heterogeneous material bonding device comprising: a stacking unit configured to stack a resin member and a metal member; a bonding unit configured to bond the resin member and the metal member by irradiating a laser onto the outer surface of the metal member stacked by the stacking unit; and a surface treatment unit configured to surface treat the bonding surface of the metal member so that irregularities can be formed on the bonding surface of the metal member prior to the stacking operation by the stacking unit; wherein the metal member prepared in the preparation step has an emissivity of 0.5 to 0.8 and a reflectivity of 25% to 40% with respect to a light source with a wavelength of 900 nm to 1100 nm, and the surface treatment unit includes forming a micro-protrusion of 1 μm or less on the bonding surface of the metal member.

Citation Information

Patent Citations

  • Composite of aluminum alloy and resin and method for manufacturing the same

    JP2012232583A

  • Different material joint body and method for manufacturing the same

    KR1020180036574A

  • Method for manufacturing different material joint body and different material joint body

    KR1020200036363A